Amino-modified colloidal silica
Amino group-modified colloidal silica with controlled particle size and pH ensures stable dispersibility and high-speed polishing by minimizing aggregation and coupling agent inhibition, addressing the aggregation and polishing speed issues in CMP processes.
Patent Information
- Application Number
- JP2025174692
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-10-16
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-05-30
AI Technical Summary
Amino group-modified colloidal silica used in chemical mechanical polishing (CMP) for semiconductor wafers tends to aggregate over time, leading to increased surface roughness and reduced polishing speed due to unreacted aminosilane coupling agents binding to the surface.
Amino group-modified colloidal silica with specific particle size, concentration, and pH control, minimizing particle aggregation and unreacted coupling agent content, ensuring stable dispersibility and high polishing speed.
The solution provides stable dispersibility over time and enables high-speed formation of a highly flat polished surface for semiconductor wafers by suppressing particle aggregation and coupling agent inhibition.
Smart Images

Figure 0007954792000001 
Figure 0007954792000002 
Figure 0007954792000003
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to amino group-modified colloidal silica.
BACKGROUND ART
[0002] In semiconductor manufacturing processes, a semiconductor wafer is held by a member called a carrier, and the semiconductor wafer is polished and flattened by bringing the wafer into contact with a polishing pad and rotating them while flowing a slurry containing chemicals, abrasive grains, and the like.
[0003] In the above polishing method, chemical mechanical polishing (CMP), which utilizes the chemical polishing action of chemicals and the mechanical polishing action of abrasive grains, has also come to be used.
[0004] In chemical mechanical polishing (CMP), there is a growing demand for polishing abrasive grains that can provide a polished surface with further reduced surface roughness of the semiconductor wafer to be polished.
[0005] Under such circumstances, colloidal silica particles, that is, colloidal silica (silica sol), have come to be used as abrasive grains for polishing semiconductor wafers.
[0006] However, colloidal silica tends to cause silica particles to aggregate with each other to form aggregated particles particularly when stored for a long period of time, so that when used as abrasive grains for polishing semiconductor wafers, the polished surface roughness increases, making it difficult to obtain a flat polished surface. For this reason, amino group-modified colloidal silica, which is obtained by modifying colloidal silica with an aminosilane coupling agent (a silane coupling agent having an amino group), has been proposed in order to suppress aggregation of silica particles and exhibit stable dispersibility over a long period of time (see Patent Document 1, International Publication No. 2018 / 061656 pamphlet).
PRIOR ART DOCUMENTS
[0007] [Patent Document 1] International Publication No. 2018 / 061656 Brochure [Disclosure of the Invention] [Problems that the invention aims to solve]
[0008] According to Patent Document 1, amino group-modified colloidal silica in which the formation of aggregated particles is suppressed can be obtained by manufacturing while maintaining a pH higher than the isoelectric point.
[0009] However, after diligent investigation by the present inventors, it was found that the amino group-modified colloidal silica obtained by the method described in Patent Document 1 contains a large amount of unreacted aminosilane coupling agent (used when modifying the amino group) remaining in the solvent. Further investigation by the present inventors revealed that when chemical mechanical polishing is performed using amino group-modified colloidal silica obtained by the method described in Patent Document 1 as polishing grains, it becomes difficult to obtain a sufficient polishing speed, possibly because the unreacted aminosilane coupling agent binds to the surface of the object to be polished, thereby inhibiting polishing.
[0010] Under these circumstances, the present invention aims to provide an amino group-modified colloidal silica that suppresses the generation of aggregated particles and exhibits stable dispersibility over a long period of time, while also being capable of forming a highly flat polished surface at high speed even when used for polishing semiconductor wafers. [Means for solving the problem]
[0011] In order to solve the above technical problems, the inventors conducted diligent research and found that the above problems could be solved by specific amino group-modified colloidal silica, and based on this finding, the present invention was completed.
[0012] In other words, the present invention is (1) The Si concentration in the solvent is 150 ppm by mass or less. Contains amino group-modified silica particles in which the coarse particle content of 0.2 μm or larger is 10,000,000 particles / mL or less when the silica particle concentration is 1% by mass. amino group-modified colloidal silica characterized by, (2) The Si concentration in the solvent is 150 ppm by mass or less. Contains amino group-modified silica particles with an average secondary particle diameter of 10-150 nm. amino group-modified colloidal silica characterized by This provides... [Effects of the Invention]
[0013] According to the present invention, it is possible to provide an amino group-modified colloidal silica that suppresses the formation of aggregated particles and exhibits stable dispersibility over a long period of time, while also being able to form a highly flat polished surface at high speed even when used for polishing semiconductor wafers. [Modes for carrying out the invention]
[0014] First, let me explain the amino group-modified colloidal silica according to the present invention.
[0015] The amino group-modified colloidal silica according to the present invention includes amino group-modified silica particles in which amino groups are immobilized on silica particles constituting colloidal silica. Suitable amino-group modified colloidal silica according to the present invention includes amino-group modified silica particles in which an aminosilane compound (a silane compound having an amino group) is chemically bonded to silica particles constituting colloidal silica.
[0016] Examples of the above-mentioned aminosilane compounds include various aminosilane coupling agents.
[0017] Examples of the aminosilane coupling agent include one or more selected from 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 4-amino-3,3-dimethylbutyltriethoxysilane, N-methylaminopropyltrimethoxysilane, (N,N-dimethyl-3-aminopropyl)trimethoxysilane, 2-(4-pyridylethyl)triethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, and the like, and one or more selected from 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane are suitable.
[0018] In the amino group-modified colloidal silica according to the present invention, by using the above aminosilane coupling agent as the aminosilane compound, a Si-O-Si bond is formed with the colloidal silica through a hydrolysis reaction and a dehydration condensation reaction, so that the surface of the silica particles constituting the colloidal silica can be subjected to amino group modification (amino groups are immobilized).
[0019] As described above, the amino group-modified colloidal silica constituting the amino group-modified colloidal silica according to the present invention is a dispersion in a solvent of amino group-modified silica particles in which amino groups (-NH2) are immobilized on the silica particles constituting the colloidal silica, and thus the amino group-modified silica particles have the basic structure derived from the silica particles constituting the colloidal silica.
[0020] In the present application documents, that the amino group-modified colloidal silica contains amino group-modified silica particles modified with amino groups is confirmed by X-ray photoelectron spectroscopy (XPS) described below. The measurement sample is centrifuged under conditions of 77000G, 5°C for 90 minutes. The obtained precipitate is dried at 60°C for 12 hours, then the obtained solid is ground in a mortar using a pestle, and dried under reduced pressure at 60°C under a gauge pressure of -0.1 MPa or lower for 2 hours to prepare a dry powder. Using the dried powder, the presence or absence of amino groups on the surface of the silica particles was confirmed by X-ray photoelectron spectroscopy under the following conditions. Measuring instrument: AXIS-NOVA manufactured by Shimadzu Corporation Irradiation X-ray: Al-Kα (15kV, 10mA) Analytical X-ray spot diameter: 300 × 700 μm
[0021] As will be described later, one method for preparing colloidal silica is to stir tetramethoxysilane (Si(OCH3)4), for example, in an organic solvent containing water, to hydrolyze and dehydrate it, forming a dimer. This dimer then polymerizes (oligomerizes) to form spherical silica primary particles in the solvent. Colloidal silica is formed when these spherical silica primary particles are dispersed in the solvent. Furthermore, the colloidal silica described above includes not only primary silica particles but also secondary silica particles formed by the association of these primary silica particles, and these secondary silica particles are dispersed in the solvent together with the primary silica particles. The amino group-modified colloidal silica according to the present invention corresponds to a material containing amino group-modified silica particles in which amino groups are immobilized on silica particles dispersed in the above colloidal silica.
[0022] The average primary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is not particularly limited, but is preferably 5 nm or more and 120 nm or less.
[0023] The average primary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is preferably 120 nm or less, more preferably 110 nm or less, and even more preferably 100 nm or less.
[0024] Because the average primary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is less than or equal to the above value (upper limit), when polishing is performed using the amino-modified colloidal silica according to the present invention, a polished surface with superior flatness can be formed.
[0025] The average primary particle size of the amino group-modified silica particles contained in the amino group-modified colloidal silica according to the present invention is preferably 5 nm or more, more preferably 6 nm or more, and even more preferably 7 nm or more.
[0026] Because the average primary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is equal to or greater than the above value (lower limit), particle aggregation is less likely to occur when polishing is performed using the amino-modified colloidal silica according to the present invention, making it possible to easily form a polished surface with superior flatness.
[0027] In this application, the average primary particle size of amino-modified silica particles contained in amino-modified colloidal silica refers to the value measured by the BET method described below. Specifically, first, amino group-modified colloidal silica is pre-dried on a hot plate at 150°C, then heat-treated at 800°C for 1 hour to prepare a sample for measurement. The specific surface area (BET specific surface area) S is then measured using the obtained sample by the BET method. For nearly perfectly spherical particles, the average primary particle diameter (nm) of amino-modified silica particles is given by the following formula: Average primary particle diameter (nm) of amino group-modified silica particles = 6000 / (BET specific surface area S (m²) 2 / g) x true density (g / cm 3 )) This can be determined by the following formula, where the true density of silica particles is 2.2 g / cm³. 3 Based on this, the average primary particle size (nm) of amino group-modified silica particles is given by the following formula Average primary particle diameter (nm) of amino group-modified silica particles = 2727 / specific surface area (m²) 2 / g) This can be determined by [method].
[0028] As described above, since amino group-modified colloidal silica includes amino group-modified silica particles in which amino groups are fixed to the silica particles constituting colloidal silica, in this application, the average primary particle diameter of the amino group-modified silica particles contained in the amino group-modified colloidal silica (average diameter of the amino group-modified silica primary particles) shall be defined as the value calculated by the method described above based on the true density of the silica particles.
[0029] The amino-modified colloidal silica according to the present invention includes amino-modified silica secondary particles formed by the association of amino-modified silica primary particles. The amino group-modified silica secondary particles contained in the amino group-modified colloidal silica according to the present invention, together with the amino group-modified silica primary particles contained in the amino group-modified colloidal silica according to the present invention, constitute the main particles of the amino group-modified silica, and are distinct from the coarse particles (described later) formed by the aggregation of the above-mentioned amino group-modified silica secondary particles and aminosilane coupling agents.
[0030] The average secondary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is preferably 10 to 150 nm, more preferably 15 to 140 nm, and even more preferably 20 to 130 nm.
[0031] Because the average secondary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica according to the present invention is within the above value range, when polishing is performed using the amino-modified colloidal silica according to the present invention, a polished surface with superior flatness can be formed.
[0032] In this application, the average secondary particle diameter of the amino-modified silica particles contained in the amino-modified colloidal silica refers to the value measured by the dynamic light scattering method described below. Specifically, first, a 0.3% by mass citric acid aqueous solution is added to the amino group-modified colloidal silica, which will be used as the measurement sample, to uniformly dilute it to a silica particle concentration of 0.8% by mass, and the resulting diluted solution is used as the measurement sample. Using the above-mentioned sample for measurement, the average particle diameter measured by dynamic light scattering using the zeta potential, particle size, and molecular weight measurement system "ELSZ-2000S" manufactured by Otsuka Electronics Co., Ltd. is defined as the average secondary particle diameter of the amino group-modified silica particles.
[0033] The amino-modified colloidal silica according to the present invention preferably has an average secondary particle diameter increase rate of 5.0% or less for the amino-modified silica particles constituting the amino-modified colloidal silica, more preferably 4.5% or less, and even more preferably 4.0% or less.
[0034] <Method for calculating the increase rate of average secondary particle diameter> The silica particle concentration in the amino-modified colloidal silica is adjusted to 10% by mass. The sample with the adjusted silica particle concentration is placed in a fluororesin container, sealed, and stored at 25°C for 48 hours. The average secondary particle diameter of amino-modified silica particles in amino-modified colloidal silica before and after storage of the above sample was measured using the method described above, and the rate of increase in the average secondary particle diameter was calculated using the following formula. Increase rate of average secondary particle diameter (%) = {(Average secondary particle diameter of amino-modified silica particles after 48 hours of storage - Average secondary particle diameter of amino-modified silica particles before storage) / Average secondary particle diameter of amino-modified silica particles before storage} × 100
[0035] In this application, the rate of increase in the average secondary particle size of the amino group-modified silica particles constituting the amino group-modified colloidal silica serves as an indicator of the ease with which the amino group-modified silica particles constituting the amino group-modified colloidal silica aggregate. The amino-modified colloidal silica according to the present invention suppresses aggregation of the amino-modified silica particles constituting the amino-modified colloidal silica by having an increase rate of the average secondary particle diameter of the amino-modified silica particles constituting the amino-modified colloidal silica that is below a predetermined value, thereby easily exhibiting stable dispersibility over a long period of time.
[0036] In the amino-modified colloidal silica according to the present invention, the content of coarse particles with a particle size of 0.2 μm or more contained in the amino-modified silica particles is preferably 10,000,000 particles / mL or less, more preferably 9,800,000 particles / mL or less, and even more preferably 9,600,000 particles / mL or less, when the silica particle concentration (in the amino-modified colloidal silica) is 1% by mass.
[0037] In the amino-modified colloidal silica according to the present invention, the content of coarse particles with a particle size of 0.2 μm or more contained in the amino-modified silica particles is less than or equal to the above value (upper limit) when the silica particle concentration in the amino-modified colloidal silica is 1% by mass. Therefore, when performing chemical mechanical polishing (CMP) using the amino-modified colloidal silica according to the present invention, surface roughness caused by the presence of coarse particles is suppressed, and a highly flat polished surface can be easily formed.
[0038] In the amino-modified colloidal silica according to the present invention, there is no particular lower limit to the content of coarse particles with a particle size of 0.2 μm or larger contained in the amino-modified silica particles. However, in the amino-modified colloidal silica according to the present invention, the content of coarse particles with a particle size of 0.2 μm or larger contained in the amino-modified silica particles can be 1,000 particles / mL or more when the silica particle concentration is 1% by mass, and it is preferable that it be 0 particles / mL or more.
[0039] The amino-modified colloidal silica according to the present invention has a suppressed content of coarse particles with a particle size of 0.2 μm or larger. Therefore, when performing chemical mechanical polishing (CMP) using the amino-modified colloidal silica according to the present invention, a highly flat polished surface can be easily formed at a high polishing speed.
[0040] In this application, the content of coarse particles with a particle size of 0.2 μm or larger in the amino-modified silica particles constituting the amino-modified colloidal silica refers to the value measured by the particle size distribution method using the counting method described below. <Method for measuring the content of coarse particles with a particle size of 0.2 μm or larger in amino group-modified silica particles> The amino group-modified colloidal silica to be measured is diluted with ultrapure water until the silica particle concentration reaches 1.0% by mass. The resulting diluted solution was used as the measurement sample, and the number of coarse particles with a particle size of 0.2 μm or larger was measured using an Accusizer FX-nano manufactured by Particle Sizing System Inc. under the following measurement conditions. <System Setup> ·Stirred Vessel Volume: 13.22 mL ·Sample Loop Volume: 0.52 mL ·Autodilution delay time : 3 sec. ·Normal Speed Flow Rate: 15 mL / min <Sensor Setup Menu> ·FX-Nano HG Minimum Size: 0.15μm ·FX-Nano HG Maximum Size: 0.27μm ·FX-Nano HG Collection Time: 60sec. ·HG Starting Concentration : 8000♯ / mL
[0041] The pH of the amino-modified colloidal silica according to the present invention is preferably 8.50 to 9.50.
[0042] The pH of the amino-modified colloidal silica according to the present invention is preferably 8.50 or higher, more preferably 8.52 or higher, and even more preferably 8.54 or higher. By having a pH of the amino-modified colloidal silica according to the present invention equal to or greater than the above value (lower limit), the dispersion stability of the amino-modified silica particles constituting the amino-modified colloidal silica according to the present invention is easily improved, making it less likely for the amino-modified silica particles to aggregate during storage or polishing of the amino-modified colloidal silica according to the present invention, and allowing for the easy formation of a highly flat polished surface when used as an abrasive grain.
[0043] Furthermore, the pH of the amino-modified colloidal silica according to the present invention is preferably 9.50 or less, more preferably 9.48 or less, and even more preferably 9.46 or less. By having a pH of the amino-modified colloidal silica according to the present invention below the above value (upper limit), the long-term dispersion stability of the amino-modified silica particles is improved while suppressing their solubility, making it easier for them to exhibit excellent polishing properties when used as a polishing abrasive grains, and allowing for the easy formation of a highly flat polished surface.
[0044] In this application, pH refers to the value measured by a pH meter F-2000PI (manufactured by Horiba, Ltd.) equipped with a pH electrode 9615S-10D (manufactured by Horiba, Ltd.).
[0045] The content of amino group-modified silica particles in the amino group-modified colloidal silica according to the present invention is not particularly limited, but is preferably 1% by mass or more and 50% by mass or less.
[0046] The content of amino group-modified silica particles in the amino group-modified colloidal silica according to the present invention is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more.
[0047] By ensuring that the content of amino-modified silica particles in the amino-modified colloidal silica according to the present invention is equal to or greater than the above value (lower limit), the polishing performance when the amino-modified colloidal silica dispersion according to the present invention is used as an abrasive is further improved.
[0048] The content of amino group-modified silica particles in the amino group-modified colloidal silica according to the present invention is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. By keeping the content of amino-modified silica particles in the amino-modified colloidal silica according to the present invention below the above value (upper limit), the dispersion stability of the amino-modified silica particles can be further improved.
[0049] In this application, the content of amino group-modified silica particles in the amino group-modified colloidal silica according to the present invention refers to the value measured by the following measurement method. In other words, it refers to the value calculated using the following formula, where 10.0 g of amino-modified colloidal silica is dried on a hot plate at 150°C, then heated at 800°C for 1 hour to remove moisture, and the resulting amount of solids is denoted as Wg. Content (mass%) of amino-modified silica particles in amino-modified colloidal silica = (W / 10.0) × 100 The silica particle content mentioned above corresponds to the total content of amino-modified primary silica particles, amino-modified secondary silica particles, and coarse particles in the amino-modified colloidal silica.
[0050] The amino group-modified colloidal silica according to the present invention has a Si concentration of 150 ppm by mass or less in the solvent.
[0051] The amino group-modified colloidal silica according to the present invention has a Si concentration in the solvent of 150 ppm by mass or less, preferably 145 ppm by mass or less, more preferably 140 ppm by mass or less, and even more preferably 135 ppm by mass or less.
[0052] In the amino group-modified colloidal silica according to the present invention, the Si concentration in the solvent serves as an indicator of the amount of unreacted aminosilane coupling agent remaining in the solvent. The amino group-modified colloidal silica according to the present invention has a Si concentration in the solvent that is below the above value (upper limit), thereby limiting the amount of unreacted aminosilane coupling agent remaining in the solvent and suppressing the bonding reaction between the unreacted aminosilane coupling agent and the surface of the object to be polished. Therefore, when polishing is performed using the amino group-modified colloidal silica according to the present invention as a polishing abrasive grain, it is possible to form a highly flat polished surface at high speed while suppressing polishing inhibition caused by unreacted aminosilane coupling agents.
[0053] In the amino group-modified colloidal silica according to the present invention, the lower limit of the Si concentration in the solvent is not particularly limited, and a lower concentration is preferable. However, the content of the amino group-modified colloidal silica according to the present invention may be, for example, 1 ppm by mass or more, 5 ppm by mass or more, or 10 ppm by mass or more.
[0054] As described above, the inventors have found that when polishing a semiconductor wafer using amino group-modified colloidal silica, unreacted aminosilane coupling agents used to modify the amino groups (-NH2) remain in the solvent. These aminosilane coupling agents react with the semiconductor wafer surface and inhibit the polishing process, making it difficult to obtain a sufficient polishing rate. In contrast, in the amino group-modified colloidal silica according to the present invention, the Si concentration in the solvent is limited to a predetermined value or less, so even when polishing semiconductor wafers, high-speed polishing can be performed to form a highly flat polished surface.
[0055] In this application, the Si concentration in the solvent of the amino group-modified colloidal silica refers to the silicon atom concentration calculated by the following method.
[0056] The amino-modified colloidal silica to be measured is centrifuged at 77,000 G, 5°C, and for 90 minutes. The Si concentration (silicon atom concentration) in the obtained supernatant is measured using an inductively coupled plasma atomic emission spectroscopy (ICP-AES) instrument (Thermo Fisher IRIS intrepid II) with an absolute calibration curve.
[0057] Furthermore, the presence of residual aminosilane coupling agents in the solvent of the amino group-modified colloidal silica according to the present invention can be confirmed by liquid chromatography-mass spectrometry (LC-MS).
[0058] The amino group-modified colloidal silica according to the present invention may contain metal impurities.
[0059] In the amino group-modified colloidal silica according to the present invention, the above-mentioned metal impurities can be one or more selected from sodium, potassium, iron, aluminum, calcium, magnesium, titanium, nickel, chromium, copper, zinc, lead, silver, manganese, cobalt, and the like.
[0060] In the amino group-modified colloidal silica according to the present invention, the total content of metal impurities is preferably 1 ppm by mass or less. Because the total content of metal impurities is 1 ppm by mass or less, the amino group-modified colloidal silica according to the present invention can be suitably used as an abrasive grain for polishing electronic materials such as semiconductor wafers.
[0061] In this application, the metal impurity content refers to the value measured using an atomic absorption spectrometer.
[0062] The amino group-modified colloidal silica according to the present invention can be suitably prepared by the manufacturing method described later.
[0063] According to the present invention, it is possible to provide an amino group-modified colloidal silica that suppresses the formation of aggregated particles and exhibits stable dispersibility over a long period of time, while also being able to form a highly flat polished surface at high speed even when used for polishing semiconductor wafers.
[0064] Next, a preferred method for producing amino group-modified colloidal silica according to the present invention will be described. A preferred method for producing amino group-modified colloidal silica according to the present invention is: A method for producing amino group-modified colloidal silica according to the present invention, A contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion is then used. (i) A first pH control step in which the pH is adjusted to be 8.00 or less while maintaining the zeta potential at -20.0 mV or less, (ii) The method is characterized by sequentially performing a second pH control step in which a base is added to the adjusted solution obtained in the first pH control step to adjust the pH to 8.50 to 9.50.
[0065] <Contact liquid obtained by contacting colloidal silica with an aminosilane coupling agent dispersion> In a preferred method for producing amino group-modified colloidal silica according to the present invention, the colloidal silica used as a raw material (raw colloidal silica) can be appropriately selected from colloidal silica having desired properties produced by known production methods. For example, colloidal silica having desired properties produced by the sol-gel method can be cited.
[0066] In the preferred method for producing amino group-modified colloidal silica according to the present invention, if the colloidal silica used as a raw material is colloidal silica produced by the sol-gel method, it can be suitably used because it contains a low amount of metal impurities that are diffusible into semiconductors and corrosive ions such as chloride ions.
[0067] In a preferred method for producing amino group-modified colloidal silica according to the present invention, when colloidal silica produced by the sol-gel method is used as the colloidal silica raw material, conventionally known methods can be used to produce the colloidal silica. Specifically, it can be produced by using one or more hydrolyzable silicon compounds (for example, alkoxysilanes or their derivatives) as raw materials and carrying out a hydrolysis-condensation reaction.
[0068] The silicon compound mentioned above is the one shown in the following general formula (1) Si(OR)4(1) (In the above general formula (1), the R group is an alkyl group having 1 to 8 carbon atoms.) Examples of tetraalkoxysilanes or their derivatives can be given.
[0069] In a silicon compound or derivative represented by general formula (1), the R group is an alkyl group having 1 to 8 carbon atoms, and preferably an alkyl group having 1 to 4 carbon atoms.
[0070] In silicon compounds or derivatives represented by general formula (1), the R group can be one or more selected from, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, and an octyl group, with one or more selected from a methyl group, an ethyl group, a propyl group, an isopropyl group, and a butyl group being preferred.
[0071] Preferred silicon compounds represented by general formula (1) are tetramethoxysilane, in which the R group is a methyl group; tetraethoxysilane, in which the R group is an ethyl group; or tetraisopropoxysilane, in which the R group is an isopropyl group. Furthermore, examples of derivatives of silicon compounds represented by general formula (1) include low-condensation products obtained by partially hydrolyzing the silicon compound (tetraalkoxysilane) represented by general formula (1). As the silicon compound or derivative represented by general formula (1), tetramethoxysilane is preferred because it is easy to control the hydrolysis rate, easy to obtain fine silica particles, and leaves little unreacted residue.
[0072] Silicon compounds represented by general formula (1) or their derivatives undergo hydrolysis and condensation in the reaction solvent to form colloidal silica.
[0073] Examples of dispersion solvents (reaction solvents) used when silicon compounds or derivatives represented by general formula (1) undergo hydrolysis and condensation include water or organic solvents containing water. The above organic solvents include one or more selected from hydrophilic organic solvents such as methanol, ethanol, isopropanol, n-butanol, t-butanol, pentanol, alcohols such as ethylene glycol, propylene glycol, and 1,4-butanediol, and ketones such as acetone and methyl ethyl ketone. Among these organic solvents, it is particularly preferable to use alcohols such as methanol, ethanol, and isopropanol. From the viewpoint of post-treatment of the reaction solvent, it is even more preferable to use alcohols having the same alkyl group as the alkyl group (R group) of the silicon compound used as a starting material (for example, methanol for tetramethoxysilane).
[0074] The amount of the above organic solvent used is not particularly limited, but it is preferable to use 5 moles or more and 50 moles or less per mole of the silicon compound or its derivative represented by general formula (1). If the amount of organic solvent used is less than 5 moles per mole of the silicon compound or its derivative represented by general formula (1), compatibility with the silicon compound represented by general formula (1) may be poor. If the amount used exceeds 50 moles per mole of the silicon compound or its derivative represented by general formula (1), the manufacturing efficiency may decrease.
[0075] The amount of water added to the silicon compound or its derivative represented by general formula (1) is not particularly limited and should be any amount required for the hydrolysis of the silicon compound represented by general formula (1). Preferably, it is about 2 to 200 moles per mole of the silicon compound or its derivative represented by general formula (1). Furthermore, when an organic solvent containing water is added to a silicon compound or its derivative represented by general formula (1), the amount of water mixed in the organic solvent greatly affects the particle size of the colloidal silica formed. By relatively increasing the amount of water added relative to the amount of organic solvent added, the particle size of the resulting colloidal silica can be made relatively larger, and by relatively decreasing the amount of water added relative to the amount of organic solvent added, the particle size of the resulting colloidal silica can be made relatively smaller. In this way, the particle size of the resulting colloidal silica can be arbitrarily adjusted by changing the mixing ratio of water and organic solvent.
[0076] For the hydrolysis condensation reaction of silicon compounds to obtain colloidal silica, it is preferable to adjust the reaction solvent to be alkaline in the presence of a basic catalyst. Through the above adjustments, the reaction solvent is preferably controlled to a pH above 8.00 and below 11.00, more preferably between 8.50 and 10.50, allowing for the rapid formation of colloidal silica.
[0077] As for the basic catalyst mentioned above, from the viewpoint of preventing contamination with impurities, one or more selected from organic amines and ammonia are preferred, and one or more selected from ethylenediamine, diethylenetriamine, triethylenetetraamine, 3-ethoxypropylamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide are particularly preferred.
[0078] To hydrolyze and condense a silicon compound in a reaction solvent, the silicon compound represented by general formula (1) or a derivative thereof is added to a solvent containing water, and the mixture is stirred at a temperature of typically 0°C to 100°C, preferably 0°C to 50°C.
[0079] By stirring a silicon compound in a water-containing solvent, hydrolysis and dehydration condensation reactions proceed of the silicon compound or its derivative represented by general formula (1). First, the silicon compound or its derivative represented by general formula (1) undergoes dehydration condensation to form a dimer, and this dimer undergoes polymerization (oligomerization) to form spherical silica primary particles in the solvent, thereby obtaining colloidal silica in which silica primary particles are dispersed in the solvent. The colloidal silica described above also contains secondary particles (silica secondary particles) formed by the association of primary silica particles. Colloidal silica with uniform silica particle size can be obtained by hydrolyzing and condensing a silicon compound while stirring it in a water-containing solvent.
[0080] The colloidal silica obtained by the above hydrolysis-condensation reaction (sol-gel method) can be used as a raw material colloidal silica in the manufacturing method according to the present invention by adjusting its concentration as appropriate.
[0081] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the colloidal silica used as a raw material includes an aqueous medium that serves as a solvent. The aqueous medium mentioned above may be the dispersion solvent used during the preparation of colloidal silica, or it may be one that was added separately after the preparation of the colloidal silica used as the raw material. Furthermore, examples of aqueous media include those similar to the dispersion solvent used during the preparation of colloidal silica.
[0082] In the preferred method for producing amino group-modified colloidal silica according to the present invention, the colloidal silica used as a raw material is preferably pH greater than 8.00 and 11.00 or less, and more preferably pH greater than 8.50 and 10.50 or less.
[0083] Furthermore, in the preferred method for producing amino group-modified colloidal silica according to the present invention, the colloidal silica used as a raw material is preferably one in which the average secondary particle diameter of the silica particles is 150 nm or less, more preferably 145 nm or less, and even more preferably 140 nm or less.
[0084] In a preferred method for producing amino-modified colloidal silica according to the present invention, the average secondary particle diameter of the silica particles constituting the colloidal silica used as a raw material is less than or equal to the above value (upper limit), so that when the amino-modified colloidal silica obtained by the production method according to the present invention is polished, a polished surface with superior flatness can be formed.
[0085] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the average secondary particle diameter of the silica particles constituting the colloidal silica used as a raw material is preferably 10 nm or more, more preferably 12 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.
[0086] Because the average secondary particle diameter of the silica particles constituting the colloidal silica is greater than or equal to the above value (lower limit), when polishing is performed using the amino group-modified colloidal silica obtained by the manufacturing method according to the present invention, aggregation of silica particles is less likely to occur, thus enabling the formation of a polished surface with superior flatness.
[0087] Furthermore, in this application, the average secondary particle diameter of the silica particles constituting colloidal silica can be measured using the same method as described above for measuring the average secondary particle diameter of silica particles in amino group-modified colloidal silica.
[0088] In the preferred method for producing amino group-modified colloidal silica according to the present invention, the colloidal silica used as a raw material is preferably such that the content of coarse particles with a particle size of 0.2 μm or more contained in the silica particles is 10,000,000 particles / mL or less, more preferably 9,800,000 particles / mL or less, and even more preferably 9,600,000 particles / mL or less, when the silica particle concentration is 1% by mass.
[0089] In the amino-modified colloidal silica according to the present invention, the content of coarse particles with a particle size of 0.2 μm or larger in the silica particles constituting the colloidal silica used as a raw material is less than or equal to the above value (upper limit) when the silica particle concentration is 1% by mass. Therefore, when performing chemical mechanical polishing (CMP) using the amino-modified colloidal silica obtained by the manufacturing method according to the present invention, surface roughness caused by the presence of coarse particles is suppressed, and a highly flat polished surface can be easily formed.
[0090] In the preferred method for producing amino-modified colloidal silica according to the present invention, there is no particular lower limit to the content of coarse particles with a particle size of 0.2 μm or larger in the silica particles constituting the colloidal silica used as a raw material. However, the content of coarse particles with a particle size of 0.2 μm or larger in the silica particles constituting the colloidal silica can be 1,000 particles / mL or more when the silica particle concentration is 1% by mass, and is preferably 0 particles / mL or more.
[0091] Furthermore, in this application, the content of coarse particles with a particle size of 0.2 μm or larger contained in the silica particles constituting the colloidal silica used as a raw material can be measured by the same method as the method for measuring the content of coarse particles with a particle size of 0.2 μm or larger contained in the amino group-modified silica particles constituting the amino group-modified colloidal silica described above.
[0092] In a preferred method for producing amino group-modified colloidal silica according to the present invention, a contact solution obtained by contacting the above-mentioned colloidal silica, which is a raw material, with an aminosilane coupling agent dispersion is used.
[0093] In the preferred method for producing amino group-modified colloidal silica according to the present invention, the details of the aminosilane coupling agent are as described in the description of amino group-modified colloidal silica according to the present invention.
[0094] In the preferred method for producing amino group-modified colloidal silica according to the present invention, the content of the aminosilane coupling agent in the aminosilane coupling agent dispersion is preferably 0.5 to 30.0% by mass, more preferably 1.0 to 28.0% by mass, and even more preferably 1.5 to 26.0% by mass.
[0095] In a preferred method for producing amino group-modified colloidal silica according to the present invention, by having the content ratio of the aminosilane coupling agent in the aminosilane coupling agent dispersion within the above range, the uneven distribution of the aminosilane coupling agent in the dispersion can be suppressed, and when in contact with colloidal silica, high miscibility can be achieved. It can be brought into sufficient contact with silica particles.
[0096] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the dispersion solvent (reaction solvent) used in the aminosilane coupling agent dispersion is water or an organic solvent containing water. The above organic solvents include one or more selected from hydrophilic organic solvents such as methanol, ethanol, isopropanol, n-butanol, t-butanol, pentanol, alcohols such as ethylene glycol, propylene glycol, and 1,4-butanediol, and ketones such as acetone and methyl ethyl ketone. Among these organic solvents, it is particularly preferable to use alcohols such as methanol, ethanol, and isopropanol.
[0097] The amount of the above aminosilane coupling agent in contact with 1 g of colloidal silica (per g of silica particles contained in colloidal silica), calculated on a solid content basis, is preferably 5 μmol to 150 μmol, more preferably 10 μmol to 145 μmol, and even more preferably 15 μmol to 140 μmol.
[0098] In a preferred method for producing amino group-modified colloidal silica according to the present invention, by having the contact amount of the aminosilane coupling agent within the above range, the surface of the silica particles can be sufficiently cationized by the amino groups, and amino group-modified colloidal silica that exhibits excellent performance when used as an abrasive grain can be easily prepared.
[0099] In a preferred method for producing amino group-modified colloidal silica according to the present invention, when contacting the colloidal silica raw material with an aminosilane coupling agent dispersion, it is preferable to contact them under temperature conditions of 5°C to 60°C, 6 to 59°C, and more preferably 7 to 58°C.
[0100] In a preferred method for producing amino group-modified colloidal silica according to the present invention, by contacting a colloidal silica dispersion with an aminosilane coupling agent under the above temperature conditions, the rapid progression of hydrolysis and condensation polymerization of the aminosilane coupling agent can be suppressed, and the generation of aggregated particles can be easily suppressed.
[0101] The contact time (reaction time) when performing the above contact treatment is not particularly limited, but it is preferably 5 minutes to 3 hours, more preferably 7 minutes to 2 hours, and even more preferably 9 minutes to 1 hour. The pH during the above contact treatment is not particularly limited, but a pH of 7.00 to 11.00 is preferred.
[0102] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the method of contacting the colloidal silica with the aminosilane coupling agent dispersion is not particularly limited, and for example, a method of dropping the aminosilane coupling agent dispersion onto the colloidal silica can be given.
[0103] A preferred method for producing amino group-modified colloidal silica according to the present invention, comprising colloidal silica and an aminosilane coupling agent dispersion. The contact solution obtained by bringing the two into contact has a pH of typically 8.10 to 11.00, with 8.30 to 10.50 being suitable, and 8.50 to 10.00 being more suitable.
[0104] <First pH control process> In a preferred method for producing amino group-modified colloidal silica according to the present invention, a first pH control step is performed on the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion, in which (i) the pH is adjusted to 8.00 or less while maintaining the zeta potential at -20.0 mV or less.
[0105] In a preferred method for producing amino group-modified colloidal silica according to the present invention, in the first pH control step, the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion is adjusted to have a pH of 8.00 or less, preferably to have a pH of 7.96 or less, and more preferably to have a pH of 7.92 or less.
[0106] In a preferred method for producing amino group-modified colloidal silica according to the present invention, in the first pH control step, the pH of the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion is adjusted to be less than or equal to the above value (upper limit). In a preferred method for producing amino group-modified colloidal silica according to the present invention, the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion usually has a pH greater than 8.00. Therefore, the first pH control step corresponds to a step of lowering the pH of the contact solution to a predetermined range. In a preferred method for producing amino group-modified colloidal silica according to the present invention, by adjusting the pH of the contact solution as described above in the first pH control step, the solubility of the aminosilane coupling agent in the contact solution can be suppressed (the solubility of the aminosilane coupling agent in the solvent can be reduced), and the reactivity of the aminosilane coupling agent with respect to the silica particles constituting the colloidal silica can be improved. As a result, the amount of aminosilane coupling agent remaining in the solvent can be reduced, and even when the resulting amino-modified colloidal silica is used as an abrasive grain, polishing inhibition caused by the bonding between the unreacted aminosilane coupling agent remaining in the solvent and the surface of the object being polished can be effectively suppressed.
[0107] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the pH adjustment of the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion in the first pH control step is performed while maintaining the zeta potential at -20.0 mV or less, preferably at -20.2 mV or less, and more preferably at -20.4 mV or less.
[0108] Zeta potential is the potential difference that occurs at the interface between a solid and a liquid when they are in relative motion. As the absolute value of the zeta potential increases, the repulsion between particles becomes stronger and the stability of the particles increases. As the absolute value of the zeta potential approaches zero, the particles become more prone to agglomeration. In a preferred method for producing amino-modified colloidal silica according to the present invention, by controlling the zeta potential as described above in the first pH control step, the dispersion stability of the amino-modified silica particles constituting the amino-modified colloidal silica can be improved, and its aggregation can be effectively suppressed.
[0109] In a preferred method for producing amino group-modified colloidal silica according to the present invention, If the pH of the contact solution is lowered too much during the first pH control step, the dispersion stability of the amino group-modified silica particles constituting the amino group-modified colloidal silica decreases, making it difficult to suppress their aggregation. A preferred method for producing amino-modified colloidal silica according to the present invention allows for easy maintenance of the dispersion stability of amino-modified silica particles in the contact solution during the first pH control step by defining the zeta potential in the first pH control step as described above, instead of defining the lower limit of the pH of the adjustment solution obtained in the first pH control step.
[0110] In this application, the zeta potential refers to the value obtained when the silica particle concentration in the sample is diluted with a 10 mM sodium chloride aqueous solution to 1% by mass, and the resulting diluted solution is measured using a zeta potential, particle size, and molecular weight measurement system (ELS-Z, manufactured by Otsuka Electronics Co., Ltd.).
[0111] In a preferred method for producing amino group-modified colloidal silica according to the present invention, the method for controlling pH in the first pH control step is not particularly limited. As described above, in a preferred method for producing amino group-modified colloidal silica according to the present invention, the contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion usually has a pH greater than 8.0, and often contains a dispersion medium such as alcohol in addition to water. Therefore, one method is to adjust the pH by replacing the dispersion medium such as alcohol in the obtained reaction solution with water.
[0112] The method of replacing the dispersion medium with water is not particularly limited. For example, one method is to heat the reaction solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion, and add a fixed amount of water dropwise while distilling off the dispersion medium such as alcohol.
[0113] <Second pH control process> In a preferred method for producing amino group-modified colloidal silica according to the present invention, (ii) a second pH control step is performed in which a base is added to the adjusted solution obtained in the first pH control step to adjust the pH to 8.50 to 9.50.
[0114] In the preferred method for producing amino group-modified colloidal silica according to the present invention, in the second pH control step, a base is added to the adjusted solution obtained in the first pH control step to adjust the pH to 8.50 to 9.50, preferably to 8.52 to 9.48, and more preferably to 8.54 to 9.46.
[0115] In the preferred method for producing amino group-modified colloidal silica according to the present invention, the base used in the second pH control step is preferably one or more selected from organic amines and ammonia, from the viewpoint of preventing contamination with impurities, and is more preferably one or more selected from ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide.
[0116] In a preferred method for producing amino-modified colloidal silica according to the present invention, in the second pH control step, a base is added to the adjusted solution obtained in the first pH control step to raise the pH to 8.50 to 9.50. This improves the dispersion stability of the amino-modified silica particles constituting the amino-modified colloidal silica, thereby easily improving its long-term storage stability while suppressing aggregation.
[0117] Details of the amino group-modified colloidal silica obtained by the preferred manufacturing method described above are as stated in the description of the amino group-modified colloidal silica according to the present invention.
[0118] As detailed above, it is possible to provide a method for producing amino group-modified colloidal silica that suppresses the formation of aggregated particles, exhibits stable dispersibility over a long period of time, and can form a highly flat polished surface at high speed even when used for polishing semiconductor wafers. [Examples]
[0119] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited in any way by the following examples.
[0120] (Example 1) (1) Preparation process for colloidal silica (silica sol) A mother liquor (water concentration 17.4% by mass, ammonia concentration 0.97% by mass) was prepared by mixing 2253 g of pure water, 527 g of 28% by mass aqueous ammonia, and 12391 g of methanol. Next, a starting material solution containing 1522 g of tetramethoxysilane (TMOS) and 413 g of methanol was injected into the mother liquor at a constant rate over 25 minutes while maintaining the liquid temperature in the reaction system at 20°C, to prepare a silica sol reaction solution with water and methanol as dispersion media. A portion of the obtained silica sol reaction solution was placed in a flask under atmospheric pressure. The flask was heated to remove the solvent by distillation, and the remaining silica sol reaction solution was added dropwise to the flask, maintaining a constant volume of the reaction solution in the flask. This concentrated silica sol solution (average secondary particle size of silica particles: 68 nm, pH: 9.41) was obtained by concentrating the silica particles to a concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion (1) To 800 g of the silica sol concentrate obtained in step (1), a mixture of 14.4 g of methanol and 1.6 g of 3-aminopropyltrimethoxysilane (methanol concentration 90% by mass) was added dropwise over 10 minutes while maintaining the liquid temperature at 30°C to obtain a reaction solution (zeta potential -51.5 mV). Specifically, a reaction solution (pH 9.61) was obtained by contacting 1 part by mass of aminosilane coupling agent per 100 parts by mass of colloidal silica (per 100 parts by mass of silica particles contained in the colloidal silica) under the above conditions. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.42, zeta potential -32.0 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.10, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.05, a Si concentration of 87 ppm by mass in the solvent, an average secondary particle diameter of 68 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of 7,754,231 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0121] (Example 2) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1100 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.92, zeta potential -41.2 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.05, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.03, a Si concentration of 90 ppm by mass in the solvent, an average secondary particle diameter of 68 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, which was 6,259,124 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0122] (Example 3) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1800 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 6.87, zeta potential -20.5 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.19, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.16, a Si concentration of 84 ppm by mass in the solvent, an average secondary particle diameter of 67 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of which 8,238,512 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0123] (Example 4) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.54, zeta potential -30.5 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 8.62, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 8.61, a Si concentration of 72 ppm by mass in the solvent, an average secondary particle diameter of 67 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of 8,072,412 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0124] (Example 5) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.48, zeta potential -31.2 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.44, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.41, a Si concentration of 115 ppm by mass in the solvent, an average secondary particle diameter of 69 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, which was 5,489,239 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0125] (Example 6) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion (1) To 800 g of the silica sol concentrate obtained in step (1), a mixture of 14.4 g of methanol and 1.6 g of 3-aminopropyltriethoxysilane (methanol concentration 90% by mass) was added dropwise over 10 minutes while maintaining the liquid temperature at 30°C to obtain a reaction solution (zeta potential -53.2 mV). Specifically, a reaction solution (pH 9.53) was obtained by contacting 1 part by mass of aminosilane coupling agent per 100 parts by mass of colloidal silica (per 100 parts by mass of silica particles contained in the colloidal silica) under the above conditions. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.31, zeta potential -35.1 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.12, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.10, a Si concentration of 80 ppm by mass in the solvent, an average secondary particle diameter of 68 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, resulting in 6,817,240 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0126] (Example 7) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion (1) To 800 g of the silica sol concentrate obtained in step (1), a mixture of 14.4 g of methanol and 1.6 g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (methanol concentration 90% by mass) was added dropwise over 10 minutes while maintaining the liquid temperature at 30°C to obtain a reaction solution (zeta potential -49.2 mV). Specifically, a reaction solution (pH 9.72) was obtained by contacting 1 part by mass of aminosilane coupling agent per 100 parts by mass of colloidal silica (per 100 parts by mass of silica particles contained in the colloidal silica) under the above conditions. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.51, zeta potential -28.7 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.08, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.04, a Si concentration of 85 ppm by mass in the solvent, an average secondary particle diameter of 67 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of 7,701,856 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0127] (Comparative Example 1) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate was obtained with a silica particle concentration of 20% by mass. Subsequently, the obtained silica sol concentrate was heated to remove the solvent by distillation, while pure water was added dropwise to the flask, maintaining a constant volume of liquid inside the flask. When the temperature at the top of the flask reached 100°C or higher and the pH was 8.00 or lower, the addition of pure water was stopped, yielding a silica sol with a silica particle concentration of 20% by mass (average secondary particle diameter of silica particles: 68 nm, pH: 7.72). (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion (1) To 800 g of silica sol obtained in step (1), a mixture of 14.4 g of methanol and 1.6 g of 3-aminopropyltrimethoxysilane (methanol concentration 90% by mass) was added dropwise over 10 minutes while maintaining the liquid temperature at 30°C to obtain a reaction solution (zeta potential -34.2 mV). Specifically, a reaction solution (pH 8.21) was obtained by contacting 1 part by mass of aminosilane coupling agent per 100 parts by mass of colloidal silica (per 100 parts by mass of silica particles contained in the colloidal silica) under the above conditions. (3) pH control process (2) The reaction solution obtained in step (2) was heated to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.37, and the solution was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.35, a Si concentration of 285 ppm by mass in the solvent, an average secondary particle diameter of 67 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, resulting in 8,659,112 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0128] (Comparative Example 2) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 800 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 8.58, zeta potential -44.5 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.35, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.31, a Si concentration of 185 ppm by mass in the solvent, an average secondary particle diameter of 69 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of 7,681,922 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0129] (Comparative Example 3) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 2100 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 6.32, zeta potential -7.8 mV). (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 9.29, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.26, a Si concentration of 89 ppm by mass in the solvent, an average secondary particle diameter of 72 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, which was 43,456,912 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0130] (Comparative Example 4) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 parts by mass of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.57, zeta potential -30.4 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 8.21, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 8.20, a Si concentration of 65 ppm by mass in the solvent, an average secondary particle diameter of 71 nm for the amino-modified silica particles, and a content of coarse particles with a particle size of 0.2 μm or larger, when the silica particle concentration was 1% by mass, of 29,105,261 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0131] (Comparative Example 5) (1) Preparation process for colloidal silica (silica sol) By performing the same procedure as in step (1) of Example 1, a silica sol concentrate (average secondary particle diameter of silica particles 68 nm, pH 9.41) was obtained with a silica particle concentration of 20% by mass. (2) Contact process between colloidal silica (silica sol) and aminosilane coupling agent dispersion A reaction solution (pH 9.61, zeta potential -51.5mV) was obtained by performing the same procedure as in step (2) of Example 1. (3) First pH control process (2) The reaction solution obtained in step (2) was placed in a flask under atmospheric pressure, and while heating the flask to remove the solvent by distillation, 1300 g of pure water was added dropwise to the flask, replacing the solvent with water while maintaining a constant volume of the reaction solution in the flask, to obtain a silica aqueous dispersion (pH 7.61, zeta potential -33.1 mV). Throughout the entire process of replacing the solvent with water, the zeta potential in the reaction solution was maintained at -20.0 mV or lower. (4) Second pH control process (3) The silica aqueous dispersion obtained in step (3) was cooled to 70°C, then 28% by mass aqueous ammonia was added to raise the pH to 10.02, and the liquid was then held at a temperature of 70°C for 24 hours to obtain the desired product. The resulting solution was confirmed to contain silica particles with amino groups fixed to their surface, i.e., it was amino-modified colloidal silica. The above-mentioned amino-modified colloidal silica had a pH of 9.98, a Si concentration of 221 ppm by mass in the solvent, an average secondary particle diameter of 73 nm for the amino-modified silica particles, and a coarse particle content of 0.2 μm or larger when the silica particle concentration was 1% by mass, resulting in 38,120,412 particles / mL. The above manufacturing conditions are shown in Table 1, and the physical properties of the obtained amino-modified colloidal silica are shown in Table 2.
[0132] The dispersion stability of the amino group-modified silica particles constituting the amino group-modified colloidal silica obtained in each of the above examples and comparative examples was evaluated by the following method. The results are shown in Table 2. <Method for evaluating dispersion stability> The rate of increase in the average secondary particle size of amino-modified silica particles in the amino-modified colloidal silica obtained in each of the above examples or comparative examples was calculated using the method described above. Furthermore, regarding dispersion stability, if the increase rate of the average secondary particle size exceeds 5.0%, the dispersion stability is evaluated as poor due to the progression of aggregation of amino group-modified silica particles. If the increase rate of the secondary particle size is 5.0% or less, the dispersion stability of the amino group-modified silica particles is evaluated as good.
[0133] The amino group-modified colloidal silica obtained in each of the above examples and comparative examples was used as abrasive grains, and the surface roughness of the polished surface was evaluated by the following method. The results are shown in Table 2.
[0134] <Method for evaluating polishing speed and polished surface roughness> To the amino group-modified colloidal silica obtained in each example and comparative example, ultrapure water was added to dilute it to a silica particle concentration of 3.0% by mass, and an abrasive composition was prepared. Using the obtained polishing composition, a 3 cm square silicon wafer with a silicon oxide film deposited on its surface was polished under the following conditions. (polishing conditions) Polishing machine: NF-300CMP, manufactured by Nanofactor Co., Ltd. Polishing pad: Manufactured by Nitta DuPont, IC1000TMPad Slurry supply rate: 50 mL / min Head rotation speed: 32 rpm Platen rotation speed: 32 rpm Polishing pressure: 4 psi Polishing time: 2 min
[0135] (Method for measuring polishing speed) The film thickness of the silicon wafer before and after polishing under the above polishing conditions was measured using an optical interferometry film thickness analyzer (Ava Spec-2048, manufactured by Avantes), and the polishing speed was calculated from the difference in thickness and the polishing time. When calculating the polishing speed using the method described above, a polishing speed of 70 Å / min or higher was judged to be good, and a polishing speed of less than 70 Å / min was judged to be poor.
[0136] (Method for measuring surface roughness) The surface roughness of the polished silicon wafer, after polishing under the above conditions, was measured using an atomic force microscope under the following conditions. Atomic force microscope: Shimadzu Corporation SPM-9700HT Cantilever: OLYMPUS MICRO CANTILEVER OMCL-AC240TS-R3 Observation mode: Dynamic Scanning area: 3.0 μm square Scanning speed: 1.00Hz Number of fields of view observed: Five arbitrary fields of view were observed per polished wafer (observation area per field of view: 3 μm × 3 μm). In five observation fields (5 fields) on the wafer polished surface, the root mean square roughness x was measured for each. i The (nm) is measured, and the root mean square roughness x in the five fields is calculated using the following formula. i The arithmetic mean of (nm) was defined as the polished surface roughness Rms(nm). TIFF0007954792000001.tif26170 When the polished surface roughness Rms was measured using the method described above, polishing performance was judged to be good if the polished surface roughness Rms was 10.0 nm or less, and poor if the polished surface roughness was greater than 10.0 nm.
[0137] [Table 1]
[0138] [Table 2]
[0139] As shown in Table 1, in Examples 1 to 7, amino group-modified colloidal silica was prepared by sequentially applying the following steps to a contact solution obtained by contacting colloidal silica with an aminosilane coupling agent dispersion: (i) a first pH control step in which the pH is adjusted to 8.00 or less while maintaining the zeta potential at -20.0 mV or less, and (ii) a second pH control step in which a base is added to the adjusted solution obtained in the first pH control step to adjust the pH to 8.50 to 9.50.
[0140] Therefore, as shown in Table 2, the amino group-modified colloidal silica obtained in Examples 1 to 7 has a Si concentration of 150 ppm by mass or less in the solvent, and the amount of coarse particles with a particle size of 0.2 μm or more contained in the amino group-modified silica particles is 10,000,000 particles / mL or less when the silica particle concentration is 1% by mass, or it contains amino group-modified silica particles with a Si concentration of 150 ppm by mass or less in the solvent and an average secondary particle diameter of 10 to 150 nm. In this case, as shown in Table 2, the amino group-modified colloidal silica obtained in Examples 1 to 7 exhibits a low rate of increase in the average secondary particle diameter of the amino group-modified silica particles, suppresses the formation of aggregated particles, and provides stable dispersibility over a long period of time. Furthermore, when used for polishing semiconductor wafers, it can form a highly flat polished surface at high speed.
[0141] On the other hand, as shown in Table 1, in Comparative Examples 1 to 5, the first pH control step was not performed during the preparation of the amino group-modified colloidal silica (Comparative Example 1), or the pH and zeta potential in the first pH control step were outside the specified range (Comparative Examples 2 and 3), or the pH in the second pH control step was outside the specified range (Comparative Examples 4 and 5). Therefore, as shown in Table 2, the amino group-modified colloidal silica obtained in Comparative Examples 1 to 5 had Si concentrations in the solvent exceeding a predetermined value (Comparative Examples 1, 2, and 5), or contained in amino group-modified silica particles with a particle size of 0.2 μm or larger exceeding a predetermined value (Comparative Examples 3 to 5), or the average secondary particle diameter of the amino group-modified silica particles was outside the predetermined range (Comparative Examples 3 to 5). In this case, as shown in Table 2, the amino group-modified colloidal silica obtained in Comparative Examples 1 to 5 exhibited a high rate of increase in the average secondary particle size of the amino group-modified silica particles, making it impossible to maintain stable dispersibility over a long period of time (Comparative Examples 4 and 5). Furthermore, when used for polishing semiconductor wafers, it was not possible to form a polished surface at high speed (Comparative Examples 1, 2, and 5), nor was it possible to form a highly flat polished surface (Comparative Examples 3 to 5). [Industrial applicability]
[0142] According to the present invention, it is possible to provide an amino group-modified colloidal silica that suppresses the formation of aggregated particles and exhibits stable dispersibility over a long period of time, while also being able to form a highly flat polished surface at high speed even when used for polishing semiconductor wafers.
Claims
1. The Si concentration in the solvent is 150 ppm by mass or less. Contains amino group-modified silica particles in which the coarse particle content of 0.2 μm or larger is 10,000,000 particles / mL or less when the silica particle concentration is 1% by mass. A colloidal silica characterized by its amino group modification.
2. The Si concentration in the solvent is 150 ppm by mass or less. Contains amino group-modified silica particles with an average secondary particle diameter of 10 to 150 nm. A colloidal silica characterized by its amino group modification.
Citation Information
Patent Citations
Method of producing polishing composition
JP2022179329A
Method for producing inorganic particle-containing slurry and zirconia particle-containing slurry
JP2023147153A
JPP7678242B
Method for producing cationically modified silica and cationically modified silica dispersion
WO2017170660A1
Method for producing cationically modified silica, cationically modified silica dispersion, method for producing polishing composition using cationically modified silica, and polishing composition using cationically modified silica
WO2018061656A1