Phosphor powder and light-emitting device
By adjusting the particle size distribution and composition of europium-activated β-type sialon phosphors, the challenges of enhancing brightness and reducing chromaticity variation in light-emitting devices are addressed, leading to improved performance.
Patent Information
- Application Number
- JP2025510450
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-03-13
AI Technical Summary
Existing light-emitting devices using europium-activated β-type sialon phosphors face challenges in achieving both sufficient brightness (total luminous flux) and reducing chromaticity variation simultaneously.
Adjusting the 50% cumulative diameter (D50) and span value ((D90-D10)/D50) of the phosphor powder within specific numerical ranges to improve total luminous flux and reduce chromaticity variation, using a composition represented by Si12-aAlaO bN16-b:Eu x, where a, b, and x are within defined limits, and controlling particle sizes through calcination and grinding processes.
The solution enhances the total luminous flux and minimizes chromaticity variation in light-emitting devices by optimizing the particle size distribution and composition of the phosphor powder, resulting in improved performance.
Smart Images

Figure 0007954804000003 
Figure 0007954804000001 
Figure 0007954804000002
Abstract
Description
[Technical Field]
[0001] This disclosure relates to phosphor powder and light-emitting devices. [Background technology]
[0002] Europium-activated β-type sialon phosphors (also known as "europium-activated β-type sialon phosphors") are known as phosphors used in light-emitting devices such as LED packages. Studies are underway to improve the performance of light-emitting devices by controlling the particle shape and other characteristics of the phosphors used in these devices.
[0003] For example, Patent Document 1 contains the general formula: Eu a Si b Al c O d N e A group of divalent europium-attached active oxynitride green-emitting phosphor particles, which are substantially represented by the formula (wherein 0.005≦a≦0.4, b+c=12, and d+e=16), is disclosed, wherein 60% or more of the phosphor particles consist of phosphor particles (1) whose major axis divided by minor axis is greater than 1.0 and less than or equal to 3.0, and it is also stated that the median diameter of the above group of phosphor particles may be in the range of 6 to 20 μm. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] International Publication No. 2009 / 008250 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] A light-emitting device is required to have sufficient brightness (total luminous flux), while also being required to have small chromaticity variation. However, according to studies by the present inventors, it is difficult to achieve both improvement in total luminous flux and reduction in chromaticity variation in a light-emitting device using a phosphor powder containing a europium-activated β-type sialon phosphor.
[0006] Accordingly, the present disclosure aims to provide a phosphor powder capable of improving the total luminous flux of a light-emitting device and reducing chromaticity variation. [MEANS FOR SOLVING THE PROBLEMS]
[0007] As a result of intensive studies, the present inventors have found that the total luminous flux of a light-emitting device can be improved and chromaticity variation can be reduced by respectively adjusting the 50% cumulative diameter in the volume-based cumulative particle size distribution of the phosphor powder and the span value ((D90-D10) / D50) indicating the relationship among the 10% cumulative diameter, the 50% cumulative diameter, and the 90% cumulative diameter to fall within specific numerical ranges.
[0008] The present disclosure provides the following [1] to [3]. [1] A phosphor powder comprising particles of a europium-activated β-type sialon phosphor, where D10, D50, and D90 are respectively defined as a 10% cumulative diameter, a 50% cumulative diameter, and a 90% cumulative diameter in a volume-based cumulative particle size distribution, D50 is more than 20.0 μm and 30.0 μm or less, and (D90-D10) / D50 is less than 1.10. [2] The phosphor powder according to [1], wherein the europium-activated β-type sialon phosphor has a composition represented by the following general formula (1). Si 12-a Al a O b N 16-b :Eu x ... (1) [In general formula (1), a, b, and x each represent a numerical value satisfying 0<a≦3, 0<b≦3, and 0<x≦0.1.] [3] A light-emitting device comprising: a light-emitting element that emits primary light; and a wavelength converter that absorbs part of the primary light and emits secondary light having a longer wavelength than the wavelength of the primary light, The light-emitting device, wherein the wavelength converter comprises the phosphor powder according to [1] or [2]. [Advantageous Effects of Invention]
[0009] According to the present disclosure, it is possible to provide a phosphor powder that can improve the total luminous flux of a light-emitting device and reduce variation in chromaticity. [Brief Description of the Drawings]
[0010] [Figure 1] Figure 1 is a schematic cross-sectional view showing an example of the light-emitting device. [Mode for Carrying Out the Invention]
[0011] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are illustrative for describing the present disclosure, and are not intended to limit the present disclosure to the following contents.
[0012] Unless otherwise specified, the materials exemplified in the present specification may be used singly or in combination of two or more thereof.
[0013] One embodiment of the phosphor powder is a phosphor powder comprising particles of a europium-activated β-type sialon phosphor, wherein when the 10% cumulative diameter, 50% cumulative diameter, and 90% cumulative diameter in the volume-based cumulative particle size distribution are defined as D10, D50, and D90 respectively, D50 is more than 20.0 μm and 30.0 μm or less, and (D90-D10) / D50 is less than 1.10.
[0014] The europium-activated β-sialon phosphor particles are particulate europium-activated β-sialon phosphor. The europium-activated β-sialon phosphor particles may contain, as a main crystal, a crystal having the same crystal structure as β-sialon, or may consist of a crystal having the same crystal structure as β-sialon. The europium-activated β-sialon phosphor particles may contain a heterogeneous phase within a range that does not impair the gist of the present disclosure.
[0015] The europium-activated β-sialon phosphor may have a composition represented by the following general formula (1). Si 12-a Al a O b N 16-b :Eu x … (1) [In general formula (1), a, b, and x each represent a numerical value satisfying 0<a≦3, 0<b≦3, and 0<x≦0.1.]
[0016] In the above general formula (1), a may be 0.005 or more, 0.01 or more, 0.1 or more, or 0.2 or more, and may be 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, or 0.4 or less. Further, b may be 0.005 or more, 0.01 or more, 0.1 or more, or 0.2 or more, and may be 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, or 0.4 or less. a and b may be different from each other, or may be equal. x may be 0.005 or more, or 0.01 or more, and may be 0.08 or less, 0.06 or less, or 0.05 or less. a, b, and x in the general formula (1) can be adjusted by adjusting the composition and composition ratio of the raw materials.
[0017] In the composition of the above europium-activated β-sialon phosphor, the contents of nitrogen atoms (N) and oxygen atoms (O) can be quantified by an oxygen-nitrogen analyzer, and the contents of europium (Eu), silicon (Si), and aluminum (Al) can be confirmed by performing quantitative elemental analysis using an ICP emission spectrometer.
[0018] The 10% cumulative particle size (D10) in the volume-based cumulative particle size distribution of the above-mentioned phosphor powder may be 5.0 μm or more, 8.0 μm or more, 10.0 μm or more, 12.0 μm or more, 14.0 μm or more, 15.0 μm or more, or 16.0 μm or more, from the viewpoint of further improving the total luminous flux of the light-emitting device and suppressing light scattering on the particle surface of the phosphor powder. From the viewpoint of reducing the amount (mass) of phosphor powder used in the light-emitting device, it may be 20.0 μm or less, 19.0 μm or less, 18.0 μm or less, or 17.0 μm or less. When D10 is below the above upper limit, the specific surface area of the phosphor powder can be increased, making it possible to obtain light of the desired color with a smaller amount of phosphor powder when used in a light-emitting device.
[0019] The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the above-mentioned phosphor powder is greater than 20.0 μm and less than or equal to 30.0 μm. From the viewpoint of further improving the total luminous flux of the light-emitting device and suppressing light scattering on the particle surface of the phosphor powder, the D50 of the above-mentioned phosphor powder may be 21.0 μm or more, 22.0 μm or more, 23.0 μm or more, 24.0 μm or more, 25.0 μm or more, 25.5 μm or more, or 25.8 μm or more. Furthermore, from the viewpoint of reducing the amount (mass) of phosphor powder used in the light-emitting device, the D50 of the above-mentioned phosphor powder may be 29.0 μm or less, 28.5 μm or less, 28.0 μm or less, 27.5 μm or less, 27.0 μm or less, or 26.5 μm or less. When D50 is below the above upper limit, the specific surface area of the phosphor powder can be increased, making it possible to obtain light of the desired color with a smaller amount of phosphor powder when used in a light-emitting device. The D50 of the phosphor powder can be adjusted within the above range, for example, 25.0 to 30.0 μm or 25.5 to 30.0 μm.
[0020] The 90% cumulative diameter (D90) in the volume-based cumulative particle size distribution of the above-mentioned phosphor powder may be 23.0 μm or more, 25.0 μm or more, 28.0 μm or more, 30.0 μm or more, 32.0 μm or more, 35.0 μm or more, 38.0 μm or more, 40.0 μm or more, or 41.0 μm or more, from the viewpoint of further improving the total luminous flux of the light-emitting device and suppressing light scattering on the particle surface of the phosphor powder. From the viewpoint of reducing the amount (mass) of phosphor powder used in the light-emitting device, it may be 50.0 μm or less, 48.0 μm or less, 46.0 μm or less, or 44.0 μm or less. When D90 is below the above upper limit, the specific surface area of the phosphor powder can be increased, making it possible to obtain light of the desired color with a smaller amount of phosphor powder when used in a light-emitting device.
[0021] In this specification, the 10% cumulative diameter (D10), 50% cumulative diameter (D50), and 90% cumulative diameter (D90) in the volume-based cumulative particle size distribution of the above-mentioned phosphor powder refer to the particle diameters at which the cumulative value from the smallest particle size in the volume-based particle size distribution curve, measured by laser diffraction-scattering, reaches 10%, 50%, and 90% of the total, respectively. Specifically, D10, D50, and D90 can be determined by the operations described in the examples of this specification. Note that D50 is also called the median diameter and refers to the average particle size of the target particles. D10, D50, and D90 can be controlled, for example, by adjusting conditions such as the heating temperature and heating time when manufacturing the above-mentioned phosphor powder.
[0022] The (D90-D10) / D50 (span value) of the above-mentioned phosphor powder is less than 1.10. The span value of the above-mentioned phosphor powder may be 1.05 or less, 1.00 or less, 0.99 or less, or 0.98 or less. By setting the span value to be below the above upper limit, the variation in the chromaticity of the light-emitting device can be further reduced. In addition, the span value of the above-mentioned phosphor powder may be, for example, 0.10 or more, or 0.50 or more.
[0023] The above-mentioned phosphor powder has a relatively large average particle size while suppressing the span value to a range of less than 1.1. When manufacturing a light-emitting device, the above-mentioned phosphor powder may have, for example, a D50 of 25 to 30 μm and a span value of 0.10 to 1.05, a D50 of 25 to 30 μm and a span value of 0.60 to 1.05, or a D50 of 25 to 30 μm and a span value of 0.90 to 1.05.
[0024] The above-mentioned phosphor powder is excited by excitation light (light with a shorter wavelength than the light emitted by the phosphor powder) and emits fluorescence. The emission peak wavelength of the above-mentioned phosphor powder may be, for example, 540 nm or higher, or 550 nm or lower.
[0025] The chromaticity X of the above-mentioned phosphor powder may be, for example, 0.350 or higher, 0.360 or higher, or 0.370 or higher, and may be 0.400 or lower, 0.390 or lower, or 0.380 or lower. The chromaticity X of the above-mentioned phosphor powder can be adjusted within the above range, for example, 0.350 to 0.400, or 0.360 to 0.390.
[0026] The chromaticity Y of the above-mentioned phosphor powder may be, for example, 0.580 or higher, 0.590 or higher, or 0.600 or higher, and may be 0.630 or lower, 0.620 or lower, 0.615 or lower, or 0.610 or lower. The chromaticity Y of the above-mentioned phosphor powder can be adjusted within the above range, for example, 0.580 to 0.630, or 0.590 to 0.620.
[0027] The chromaticity X and chromaticity Y of the phosphor powder are calculated from data in the wavelength range of 465 to 780 nm of the fluorescence spectrum of the phosphor powder, in accordance with JIS Z8724:2015, as the x-value (chromaticity X) and y-value (chromaticity Y) of the CIE chromaticity coordinates in the XYZ color system specified in JIS Z8781-3:2016.
[0028] An example of a method for producing phosphor powder containing particles of europium-activated β-type sialon phosphor is a calcination step of obtaining a calcined product from a raw material composition containing a silicon source, an aluminum source, a europium source, and a nucleating agent, wherein at least one of the silicon source, the aluminum source, and the europium source is included as a nitride, by one or more heat treatments; and a grinding step of grinding the calcined product to obtain a powder. In the grinding step, the powder is ground so that the D50 of the obtained powder is greater than 20.0 μm and less than or equal to 30.0 μm, and (D90-D10) / D50 is less than 1.10.
[0029] The raw material composition contains a compound having an element that constitutes europium-activated β-type sialon, and contains at least a silicon source, an aluminum source, and a europium source. In the raw material composition, at least one of the silicon source, aluminum source, and europium source is a nitride. Since the nitride contains nitrogen, which is a constituent element of europium-activated β-type sialon, it is also a nitrogen source. A silicon source means a compound or element with silicon as a constituent element. An aluminum source means a compound or element with aluminum as a constituent element. A europium source means a compound or element with europium as a constituent element. In this specification, a compound with silicon as a constituent element is also called a silicon compound, a compound with aluminum as a constituent element is also called an aluminum compound, and a compound with europium as a constituent element is also called a europium compound. The silicon compound, aluminum compound, and europium compound may each be a nitride, oxide, oxynitride, hydroxide, or halide.
[0030] Examples of silicon compounds include silicon nitride (Si3N4) and silicon dioxide (SiO2). When silicon nitride powder is used as the silicon compound, it is preferable to use silicon nitride powder with a high α fraction. The α fraction of silicon nitride powder may be, for example, 80% by mass or more, 90% by mass or more, or 95% by mass or more. When the α fraction of silicon nitride powder is within the above range, primary particle growth can be promoted. It is preferable to use silicon nitride powder with a low oxygen content. The oxygen content of silicon nitride powder may be, for example, 3% by mass or less, 2% by mass or less, 1.5% by mass or less, or 1.3% by mass or less, based on the total mass of silicon nitride powder. When the oxygen content of silicon nitride powder is within the above range, the occurrence of defects in the crystals of β-type sialon and the main crystal phase of europium-activated β-type sialon phosphor can be suppressed.
[0031] Examples of aluminum compounds include aluminum nitride (AlN), aluminum oxide (Al2O3), and aluminum hydroxide (Al(OH)3). When using aluminum nitride powder as the aluminum compound, it is preferable to use aluminum nitride powder with a low oxygen content. The oxygen content of the aluminum nitride powder may be, for example, 3% by mass or less, 2% by mass or less, 1.5% by mass or less, or 1.0% by mass or less, based on the total mass of the aluminum nitride powder.
[0032] Examples of europium compounds include europium oxide, europium nitride, and europium halides. Examples of europium halides include europium fluoride, europium chloride, europium bromide, and europium iodide. Europium compounds preferably contain europium oxide. The valency of europium in the europium compound may be divalent or trivalent.
[0033] The nucleating agent may include, for example, β-type sialon, europium-activated β-type sialon, etc. By adding a nucleating agent and adjusting the amount of nucleating agent added, it is possible to promote the growth of europium-activated β-type sialon phosphor particles. Then, by increasing the particle size of the calcined product and performing the grinding process in the grinding step described later, the particle size can be adjusted to a predetermined span value while maintaining a predetermined average particle size. The europium-activated β-type sialon used as the nucleating agent may be prepared separately and can be obtained, for example, by the preparation method having the calcination step described above. The particle size (D50) of the nucleating agent may be, for example, 10 μm or more, or 15 μm or more, and may be less than 45 μm. The particle size of the nucleating agent can be determined by the same method as the D50 of the phosphor powder described above.
[0034] The raw material composition can be prepared by weighing and mixing each compound. The mixing may be done using either a dry or wet mixing method. A dry mixing method may involve mixing each component using, for example, a V-type mixer. A wet mixing method may involve preparing a solution or slurry by adding a solvent or dispersion medium such as water, mixing the components, and then removing the solvent or dispersion medium.
[0035] The heating temperature in the firing process may be, for example, 1800-2500°C, 1800-2400°C, 1850-2100°C, 1900-2100°C, 1900-2050°C, or 1920-2050°C. By setting the heating temperature in the firing process to 1800°C or higher, grain growth of the main crystal phase of β-type sialon and europium-activated β-type sialon phosphor can be promoted, and the amount of europium solid solution can be made more sufficient. By setting the heating temperature in the firing process to 2500°C or lower, the decomposition of the β-type sialon crystals and the main crystal phase of europium-activated β-type sialon phosphor can be sufficiently suppressed.
[0036] While a longer heating time in the firing process is preferable from the viewpoint of promoting the primary particle growth of the main crystal phase of β-type sialon and europium-activated β-type sialon phosphor, excessively long heating times reduce production efficiency. Therefore, the heating time may be, for example, 1 to 30 hours, 3 to 25 hours, or 5 to 20 hours.
[0037] The heating of the raw material composition in the firing process may be carried out, for example, under a nitrogen atmosphere. Heating under conditions of high nitrogen partial pressure can suppress the decomposition of silicon nitride at high temperatures. Furthermore, processing at high temperatures can promote particle growth. The heating of the raw material composition in the firing process may also be carried out, for example, under pressure. The pressure (absolute pressure) in this case may be, for example, 0.01 to 200 MPa, 0.02 to 200 MPa, 0.05 to 200 MPa, 0.1 to 100 MPa, 0.5 to 100 MPa, 0.5 to 50 MPa, 0.5 to 10 MPa, or 0.5 to 1 MPa.
[0038] The calcined product obtained by the calcination process may contain a solid solution having β-type sialon crystals, in which an element that serves as a luminescence center is solid-dissolved in a portion of the crystals, and which itself may emit fluorescence. In other words, the calcined product may contain europium-activated β-type sialon phosphor.
[0039] For the grinding process, for example, a jet grinder can be used. The grinding of the calcined material is carried out in two or more stages. Dividing the grinding process into two or more stages makes it easier to adjust the particle size, such as by suppressing over-grinding. The number of grinding stages can be two or more, but it may also be three or more. For example, the number of grinding stages may be five or less. In this specification, "grinding" also includes "decomposition".
[0040] Each grinding cycle may be carried out under conditions where the air pressure is 0.2 MPa or higher, or 0.4 MPa or higher. Each grinding cycle may be carried out under conditions where the air pressure is 0.8 MPa or lower, or 0.6 MPa or lower. Each grinding cycle may be carried out under conditions where the air pressure is, for example, 0.2 to 0.8 MPa. In addition, each grinding cycle may be carried out under conditions where the feed rate of the fired material is 1.0 kg / h or higher, 2.0 kg / h or higher, or 2.5 kg / h or higher. Each grinding cycle may be carried out under conditions where the feed rate of the fired material is 10.0 kg / h or lower, 5.0 kg / h or lower, or 3.5 kg / h or lower. Each grinding cycle may be carried out under conditions where the feed rate of the fired material is 1.0 to 10.0 kg / h. Multiple grinding cycles may all be carried out under the same conditions, or they may be carried out under different conditions.
[0041] The above manufacturing method may further include, in addition to the firing and grinding steps, an annealing step in which the fired material is heated at a temperature lower than the heating temperature in the firing step to obtain an annealed product. The fired material heated in the annealing step may be the fired material after the grinding step (in other words, the ground fired material). When the above manufacturing method includes an annealing step, the luminescence efficiency of the produced phosphor powder can be further improved. Furthermore, since strains and defects in β-type sialon can be removed by rearranging the elements, transparency can also be improved. Note that a different phase may occur in the annealing step, but this can be removed by treatment with acid, as described later.
[0042] The annealing process can be carried out in an atmosphere selected from the group consisting of, for example, an atmosphere of an inert gas, a reducing gas, a mixture thereof, and a non-oxidizing atmosphere. Examples of inert gases include noble gases (such as argon gas) and nitrogen gas. Examples of reducing gases include hydrogen gas, carbon monoxide gas, hydrocarbon gases, and ammonia gas. Examples of mixed gases include a mixture of the above-mentioned inert gas and reducing gas. The non-oxidizing atmosphere is preferably a non-oxidizing atmosphere other than pure nitrogen, such as a vacuum. The annealing process is preferably carried out in a hydrogen gas atmosphere or an argon atmosphere.
[0043] The annealing process may be carried out under either atmospheric pressure or pressurized conditions. The heat treatment temperature in the annealing process is not particularly limited, but is preferably 1100 to 1700°C, more preferably 1100 to 1650°C, and even more preferably 1200 to 1600°C.
[0044] The heating time in the annealing process may be, for example, 1 to 20 hours, 3 to 15 hours, or 5 to 10 hours.
[0045] In the annealing process, other components may be added to the calcined material before heating it. That is, the calcined material may be heated as a mixture of the calcined material and other components. Examples of other components include compounds whose constituent elements are the elements that make up europium-activated β-type sialon phosphor (at least one element selected from the group consisting of silicon, aluminum, europium, oxygen, and nitrogen).
[0046] Examples of compounds whose constituent elements are the elements that make up europium-activated β-type sialon phosphors include the silicon compounds (such as silicon dioxide), aluminum compounds (such as aluminum oxide), and europium compounds (such as europium oxide and europium fluoride) mentioned above.
[0047] The above manufacturing method may further include a step of treating the annealed product with at least one of an acid and an alkali, a classification step of adjusting the particle size of the calcined product or annealed product (including the annealed product after treatment with at least one of an acid and an alkali), and so on.
[0048] The process of treating the annealed material with acid is called the acid treatment process, and the process of treating the annealed material with alkali is called the alkali treatment process. The acid treatment process or alkali treatment process makes it possible to, for example, reduce the crystal defect density in the phosphors contained in the annealed material, remove silicon present on the surface of solid solutions generated by the thermal decomposition of β-type sialon, and remove AlN polytypoids, which are pseudopolymorphs of aluminum nitride (AlN) produced as by-products during the preparation of the calcined product. Furthermore, if other components are added in the annealing process, it is possible to remove other phases other than the europium-activated β-sialon phosphors that originate from the added components. The acid may include, for example, hydrofluoric acid, nitric acid, hydrochloric acid, etc. The acid may be a mixed acid of hydrofluoric acid and nitric acid. The alkali may include, for example, sodium hydroxide, etc.
[0049] The classification process may be carried out by either a wet classification method or a dry classification method. Examples of wet classification include elutriation classification, in which the calcined or annealed product is added to a solvent such as a mixed solvent containing deionized water and a dispersant (e.g., sodium hexametaphosphate), or a mixed solvent containing deionized water and ammonia water, stirred, and then allowed to stand, separating the fine particles with small particle sizes from the supernatant liquid.
[0050] The above-mentioned phosphor powder may be used alone or in combination with other phosphor powders. The phosphor powder of this disclosure, which contains particles of europium-activated β-type sialon phosphor, also exhibits excellent excitation light absorption when dispersed in a cured resin, and can therefore be used, for example, in light-emitting devices such as LED packages.
[0051] One embodiment of the light-emitting device comprises a light-emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than the wavelength of the primary light. The wavelength converter contains the above-mentioned phosphor powder. The light-emitting element and the wavelength converter may be sealed with a sealing resin or the like.
[0052] Figure 1 is a schematic cross-sectional view showing an example of a light-emitting device. The light-emitting device shown in Figure 1 is an example of an optoelectronic device classified as a surface-mount type. The light-emitting device 100 comprises a substrate 10, a light-emitting element 40 electrically connected to a metal layer 20 of the substrate 10, a reflective portion 30 provided on the surface of the substrate 10 so as to surround the light-emitting element 40, and a transparent sealing resin 60 that fills the recess formed by the substrate 10 and the reflective portion 30 and seals the light-emitting element 40. The transparent sealing resin 60 contains phosphor powder 52 containing the aforementioned europium-activated β-type sialon phosphor particles and other phosphor powders 54 dispersed within it.
[0053] The substrate 10 has a metal layer 20 on a portion of its surface, and the metal layer 20 is an electrode that is electrically connected to the light-emitting element 40 placed on the surface of the substrate 10. The light-emitting element 40 is die-bonded to either the anode side or the cathode side of the metal layer 20 and is electrically connected to the metal layer 20 via a die-bonding material 42. The light-emitting element 40 is also electrically connected to either the anode side or the cathode side of the metal layer 20 via a bonding wire 44.
[0054] The reflective section 30 is filled with a transparent sealing resin 60 for sealing the light-emitting element 40, and reflects the light (excitation light) emitted from the light-emitting element 40, as well as the fluorescence emitted from the phosphor powder 52 and other phosphor powders 54 in response to that light, to the surface side of the light-emitting device 100.
[0055] The light-emitting element 40 may emit light (primary light, excitation light) capable of exciting at least one of the phosphor powder 52 and other phosphor powders 54. The light-emitting element 40 may be, for example, a near-ultraviolet light-emitting diode (near-ultraviolet LED), an ultraviolet light-emitting diode (ultraviolet LED), or a blue light-emitting diode (blue LED). Multiple light-emitting elements 40 may be provided.
[0056] The light-emitting device 100 includes other phosphor powders 54 in addition to the phosphor powder 52 described above. The other phosphor powders 54 may include, for example, phosphors other than the europium-activated β-type sialon phosphor described above (red phosphor, yellow phosphor, green phosphor, blue phosphor, etc.). In another example, the light-emitting device 100 may contain only phosphor powder 52 containing particles of europium-activated β-type sialon phosphor as the phosphor powder.
[0057] Examples of transparent sealing resins 60 include silicone resin, epoxy resin, polyvinyl resin, polyethylene, polypropylene, and polyester.
[0058] In the above example, the light-emitting device was described using an example of an optoelectronic device classified as a surface-mount type, but the light-emitting device is not limited to this. The light-emitting device may be, for example, an analytical light source, a signaling device, or a backlight for liquid crystal displays and liquid crystal panels.
[0059] Although several embodiments have been described above, this disclosure is not limited in any way to the embodiments described above. Furthermore, the descriptions of the embodiments described above are applicable to each other. [Examples]
[0060] The contents of this disclosure will be described in more detail below with reference to examples and comparative examples. However, this disclosure is not limited to the examples described below.
[0061] In the following examples and comparative examples, the following raw materials were used: α-type silicon nitride powder (manufactured by UBE Corporation, product name "UBE Silicon Nitride SN-E10", oxygen content based on the total mass of silicon nitride powder: 1.0% by mass), aluminum nitride powder (manufactured by Tokuyama Corporation, product name "Aluminum Nitride Powder E Grade", oxygen content based on the total mass of aluminum nitride powder: 0.8% by mass), aluminum oxide powder (manufactured by Daimyo Chemical Industry Co., Ltd., product name "Low-Temperature Sinterable Alumina TM-DAR"), and europium(III) oxide powder (manufactured by Shin-Etsu Chemical Co., Ltd., product name "Europium Oxide Fine Powder RU Type").
[0062] [Production of nuclear agents] Using a micro-type V-type mixer (manufactured by Tsutsui Chemical Instruments Co., Ltd., S-3 type), 95.20% by mass of α-type silicon nitride powder, 2.88% by mass of aluminum nitride powder, 0.92% by mass of aluminum oxide powder, and 1.00% by mass of europium oxide powder were mixed. The resulting mixture was passed through a sieve with a mesh size of 250 μm to remove aggregates and obtain the first raw material composition. The mixing ratio of each component here is calculated from the ratio of silicon to aluminum (Si / Al ratio) in the first raw material composition, and the general formula for β-type SiAlON is: Si 12-a Al a O b N 16-b This design ensures that the values of a and b in the equation are a=b=0.5.
[0063] 200 g of the obtained first raw material composition was filled into a cylindrical boron nitride container with a lid, measuring 10 cm in inner diameter and 10 cm in height. This container was then placed in an electric furnace with a carbon heater and subjected to a heat treatment at 1950°C for 10 hours in a pressurized nitrogen atmosphere at 0.8 MPa to obtain the first calcined product. This first calcined product was crushed once using a supersonic jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd., product name "Supersonic Jet Pulverizer PJM-80SP") under conditions of an air pressure of 0.5 MPa and a supply rate of the first calcined product of 3.0 kg / h. The crushed first calcined product was passed through a nylon sieve with a mesh size of 45 μm to obtain β-type Sialon powder (D50: approximately 16 μm) to be used as a nucleating agent.
[0064] [Manufacturing of fluorescent powders] <Example 1> Using a micro-type V-type mixer (manufactured by Tsutsui Chemical Instruments Co., Ltd., S-3 type), 93.29% by mass of α-type silicon nitride powder, 2.82% by mass of aluminum nitride powder, 0.91% by mass of aluminum oxide powder, 0.98% by mass of europium oxide powder, and 2.00% by mass of the nucleating agent (β-type sialon powder) prepared by the method described above were mixed. The resulting mixture was passed through a sieve with a mesh size of 250 μm to remove aggregates and obtain a second raw material composition.
[0065] 200 g of the obtained second raw material composition was filled into a cylindrical boron nitride container with a lid, measuring 10 cm in inner diameter and 10 cm in height. This container was then placed in an electric furnace with a carbon heater and subjected to a heat treatment (calcination process) at 1950°C for 10 hours in a pressurized nitrogen atmosphere at 0.8 MPa to obtain a second calcined product. This second calcined product was pulverized twice using a supersonic jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd., product name "Supersonic Jet Pulverizer PJM-80SP") under conditions of an air pressure of 0.5 MPa and a supply rate of 3.0 kg / h for the second calcined product. After that, it was passed through a nylon sieve with a mesh size of 45 μm to obtain calcined powder.
[0066] 20 g of the obtained calcined powder was packed into a cylindrical boron nitride container with a lid, measuring 5 cm in inner diameter and 3.5 cm in height. This container was then placed in an electric furnace with a carbon heater and heated at 1500°C for 8 hours in an argon atmosphere at atmospheric pressure to obtain an annealed product. The annealed product was added to a mixed acid of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass) (a mixture of hydrofluoric acid and nitric acid in a 1:1 volume ratio). The resulting mixture was stirred at 75°C for 30 minutes to perform acid treatment. After acid treatment, stirring was stopped to allow the powder to settle, and the supernatant and the fine particles contained in the supernatant were removed. Decantation was then repeated until the pH of the solution was 5 or higher and the supernatant was clear. Decantation was performed by calculating the sedimentation time of the phosphor powder using Stokes' formula, setting it to remove fine particles with a particle size of 7 μm or less, and removing the supernatant above a predetermined height after a predetermined time had elapsed from the start of sedimentation. An aqueous solution of ion-exchanged water mixed with 0.05% by mass of sodium hexametaphosphate was used as the dispersion medium. The powder obtained as a precipitate was recovered by filtration and dried to obtain a dried powder. Analysis of the dried powder using an oxygen-nitrogen analyzer and an ICP emission spectrometer revealed that the dried powder contained Si 11.7 Al 0.3 O 0.3 N 15.7 :EU 0.03 It was confirmed that it had the following composition. This dried powder was used as the phosphor powder for Example 1.
[0067] <Examples 2-4 and Comparative Examples 1-3> Except for changing the amounts of each component in the second raw material composition and the number of times the second calcined product was pulverized as shown in Table 1 below, the phosphor powders of Examples 2-4 and Comparative Examples 1-3 were obtained in the same manner as in Example 1. Analysis using an oxygen-nitrogen analyzer and an ICP emission spectrometer showed that the phosphor powders of Examples 2-4 and Comparative Examples 1-3 were Si 12-a Al a O b N 16-b :EU x It was confirmed that the composition has the following properties: (0.25≦a≦0.35, 0.25≦b≦0.35, 0.02≦x≦0.04).
[0068] [Table 1]
[0069] [evaluation] The following evaluations were performed on the manufactured phosphor powder. The results are shown in Table 2.
[0070] <10% cumulative diameter (D10), 50% cumulative diameter (D50), and 90% cumulative diameter (D90)> The particle size distribution of each phosphor powder was measured in accordance with the method for measuring particle size distribution by laser diffraction and scattering described in JIS R 1629:1997 "Method for measuring particle size distribution of fine ceramic raw materials by laser diffraction and scattering". Specifically, first, 0.03 g of the phosphor powder to be measured was added to 100 mL of deionized water containing 0.05 mass% sodium hexametaphosphate, and the sample was dispersed for 3 minutes using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd., product name "Ultrasonic Homogenizer US-150E", Amplitude: 100%, oscillation frequency: 19.5 KHz, tip size: φ20, amplitude: 32 ± 2 μm) to prepare the measurement sample. Then, the particle size was measured using a particle size distribution analyzer (manufactured by Microtrac-Bell Co., Ltd., product name "Microtrac MT3300EX II"). From the obtained particle size distribution, D10, D50, and D90 were determined. Furthermore, based on the determined values of D10, D50, and D90, (D90-D10) / D50 (span value) was calculated.
[0071] <Emission peak intensity and emission peak wavelength> The phosphor powder to be measured was packed into a concave cell so that its surface was smooth, and then attached to the opening of an integrating sphere. Monochromatic light spectrally separated to a wavelength of 455 nm from a Xe lamp, which was the light source, was introduced into the integrating sphere using an optical fiber as excitation light. This excitation light was irradiated onto the phosphor powder to be measured, and the fluorescence spectrum was measured. A spectrophotometer (Otsuka Electronics Co., Ltd., product name "MCPD-7000") was used for the measurement. In the obtained fluorescence spectrum data, the wavelength showing the highest intensity in the range of 465 nm to 800 nm was determined as the emission peak wavelength. Furthermore, the relative value of the emission intensity value at this emission peak wavelength, with respect to the emission intensity value at the emission peak wavelength determined for the phosphor powder of Comparative Example 1, was calculated as the emission peak intensity (%).
[0072] <Chromaticity> From the fluorescence spectrum data measured using the method described above, in the wavelength range of 465 to 780 nm, the CIE chromaticity coordinates x-value (chromaticity X) and y-value (chromaticity Y) in the XYZ color system specified in JIS Z8781-3:2016 were calculated in accordance with JIS Z8724:2015.
[0073] Furthermore, when the emission peak wavelength, chromaticity X, and chromaticity Y were measured for a standard sample of β-type Sialon phosphor (NIMS Standard Green lot No. NSG1301, manufactured by Sialon Corporation) using the measurement method described above, the peak wavelength was 543 nm, chromaticity X was 0.356, and chromaticity Y was 0.624.
[0074] The measured values for emission peak wavelength, chromaticity X, and chromaticity Y may fluctuate if the manufacturer of the measuring device, the manufacturing lot number, etc., changes. Therefore, the values measured by the measurement method described in this specification should be adopted as the various measured values. However, if the manufacturer of the measuring device, the manufacturing lot number, etc., are changed, the measured values can also be corrected using the measured values from the standard sample of β-type sialon phosphor described above as reference values.
[0075] <Relative value of the total luminous flux of the light-emitting device> First, the light-emitting devices (LED packages) of Examples 1-4 and Comparative Examples 1-3 were manufactured using the phosphor powders of Examples 1-4 and Comparative Examples 1-3, respectively. The phosphor powder and silicone resin (manufactured by Toray Dow Corning Ltd., product name "OE6656") were weighed out so that the phosphor powder accounted for 2% by mass, based on the total amount of phosphor powder and silicone resin, and mixed using a rotation-and-revolution type mixer (manufactured by Thinky Co., Ltd., product name "Awatori Rentaro (registered trademark) ARE-310"). Next, the LED was placed at the bottom of the concave package body, and after wire bonding the LED to the electrodes on the substrate, the above-mentioned mixture of phosphor powder and silicone resin was injected from a microsyringe to mount the LED. Subsequently, the resin was cured at 120°C, and then post-cured at 110°C for 10 hours to seal and obtain the light-emitting device. The LED used had an emission peak wavelength of 448 nm and a chip size of 1.0 mm × 0.5 mm. Furthermore, the amount of phosphorescent powder, based on the total amount of phosphorescent powder and silicone resin, was changed to 4% by mass, 8% by mass, and 16% by mass, and other parameters were kept the same to obtain light-emitting devices. Using the above method, four types of light-emitting devices with different phosphorescent powder contents were manufactured for each example and comparative example.
[0076] The total luminous flux and chromaticity Y of the fabricated light-emitting devices were measured using a total luminous flux measuring instrument (a device manufactured by Otsuka Electronics Co., Ltd., combining a 500 mm diameter integrating hemisphere and a spectrophotometer (product name "MCPD-9800")). To compare the results of the light-emitting devices of each example and comparative example, the relative values of the total luminous flux were determined as follows. First, for each example and comparative example, a graph was created with chromaticity Y on the horizontal axis and total luminous flux on the vertical axis based on the measurement results of the four types of light-emitting devices, and an approximation curve was obtained. Based on the relationship of this approximation curve, the total luminous flux when chromaticity Y = 0.230 was calculated. Next, the total luminous flux values of the light-emitting devices of each example and comparative example were calculated as the relative values (%) of the total luminous flux of the light-emitting devices, with the total luminous flux value of the light-emitting device of Comparative Example 1 set to 100.0%.
[0077] <Variation in chromaticity Y of the light-emitting device> The concentration of the phosphor powder was fixed at 8% by mass, and 20 light-emitting devices for each example and comparative example were prepared using the method described above. The chromaticity Y of each prepared light-emitting device was measured using the method described above, and the standard deviation of the chromaticity Y of each light-emitting device was determined for each of Examples 1-4 and Comparative Examples 1-3. Furthermore, the relative value (%) of the standard deviation of the standard deviation of each example and comparative example was calculated as the variability of the chromaticity Y of the light-emitting devices, with the standard deviation of the chromaticity Y of the light-emitting device of Comparative Example 1 set to 100%.
[0078] [Table 2] [Explanation of Symbols]
[0079] 10...Substrate, 20...Metal layer, 30...Reflective part, 40...Light-emitting element, 42...Die bond material, 44...Bonding wire, 52...Phosphorescent powder containing europium-activated β-type sialon phosphor particles, 54...Other phosphorescent powders, 60...Transparent sealing resin, 100...Light-emitting device.
Claims
1. A phosphor powder containing particles of europium-activated β-type sialon phosphor, When the cumulative particle size distribution based on volume is defined as D10, D50, and D90 for the 10% cumulative diameter, 50% cumulative diameter, and 90% cumulative diameter, respectively, D10 is 5.0 μm or larger, D50 is greater than 20.0 μm and less than or equal to 30.0 μm. D90 is 50.0 μm or less. (D90 - D10) / D50 is less than 1.10, The volume-based cumulative particle size distribution is obtained by adding 0.03 g of the phosphor powder to 100 mL of deionized water containing 0.05% by mass of sodium hexametaphosphate, dispersing it for 3 minutes using an ultrasonic homogenizer (oscillation frequency: 19.5 kHz, tip size: φ20, amplitude: 32 ± 2 μm), preparing a measurement sample, and then measuring the particle size using a particle size distribution analyzer. The europium-activated β-type sialon phosphor is a phosphor powder having a composition represented by the following general formula (1). Si 12-a Al a O b N 16-b : Eu x … (1) [In general formula (1), a, b, and x represent numerical values that satisfy 0.2 ≤ a ≤ 0.4, 0.2 ≤ b ≤ 0.4, and 0.01 ≤ x ≤ 0.05, respectively.]
2. A light-emitting device comprising a light-emitting element that emits primary light, and a wavelength converter that absorbs a portion of the primary light and emits secondary light having a wavelength longer than the wavelength of the primary light, A light-emitting device comprising the wavelength converter containing the phosphor powder described in claim 1.
Citation Information
Patent Citations
β-TYPE SIALON PHOSPHOR AND LIGHT-EMITTING DEVICE
JP2020084177A
Group of phosphor particles, and light-emitting device using the same
WO2009008250A1
Phosphor and light emitting device
WO2017122800A1
Α-sialon fluorescent body and light-emitting device
WO2019188630A1
Β-sialon fluorescent body and light-emitting device
WO2019188631A1