Battery cells, batteries and electrical devices
By using a hydrophilic polymer to form an elastic porous sustained-release electrolyte within the electrode assembly, the battery cell addresses electrolyte leakage issues, enhancing reliability and cycle performance.
Patent Information
- Application Number
- JP2025536917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Battery cell performance, particularly in terms of operational reliability and cycle life, is inadequate for the expanding range of applications, primarily due to issues with electrolyte leakage leading to dendrite formation and short circuits.
Incorporating a hydrophilic polymer into the electrode assembly to form an elastic porous sustained-release electrolyte, which absorbs and traps free electrolyte, reducing the risk of short circuits and enhancing conductivity.
The solution improves battery cell reliability and cycle performance by minimizing electrolyte leakage and maintaining high conductivity through the formation of an aggregated electrolyte.
Smart Images

Figure 0007954824000062 
Figure 0007954824000063 
Figure 0007954824000064
Abstract
Description
[Technical Field]
[0001] This application relates to the field of batteries, and more specifically to battery cells, batteries, and electrical devices. [Background technology]
[0002] Battery cells, possessing characteristics such as high capacity and long lifespan, are widely applied in electronic devices such as mobile phones, laptops, electric scooters, electric vehicles, electric airplanes, electric boats, electric toy cars, electric toy boats, electric toy airplanes, and power tools.
[0003] As the range of battery applications expands, the demands on battery cell performance are also becoming increasingly stringent. Despite the need to improve battery cell performance, their operational reliability and cycle life remain relatively low. [Overview of the Initiative]
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery cell, a battery, and an electrical device.
[0005] A first aspect of the present invention relates to a battery cell comprising an electrode assembly including a first electrode piece, a second electrode piece, and a separator, and an electrolyte, wherein the polarities of the first electrode piece and the second electrode piece are opposite, the separator is placed between the first electrode piece and the second electrode piece, at least one of the first electrode piece, the second electrode piece, and the separator comprises a hydrophilic polymer, and the battery cell satisfies the following formula:
number
[0006] p1 represents the porosity of the first pole segment,
[0007] v1 is the total volume of the first pole segment in units of μm. 3 Represented by,
[0008] p2 represents the porosity of the second pole segment,
[0009] v2 is the total volume of the second pole segment in units of μm. 3 Represented by,
[0010] p3 represents the porosity of the separator.
[0011] v3 defines the total volume of the separator in units of μm. 3 Represented by,
[0012] The present invention provides a battery cell in which y represents the mass of the free electrolyte in the battery cell, expressed in units of grams.
[0013] In this way, when the embodiments of the present invention satisfy the range of the above formula, the hydrophilic polymer has a relatively good affinity for the electrolyte, and the electrolyte can rapidly diffuse between the molecular chains of the hydrophilic polymer and be encapsulated by the molecular chains, swelling and adsorption to obtain an elastic porous sustained-release electrolyte. The sustained-release electrolyte can absorb the free electrolyte in the battery cell, reducing the presence of the free electrolyte. Since the free electrolyte is trapped, the risk of the free electrolyte being pushed out is reduced, thereby reducing the risk of short circuits between the positive and negative electrode pieces caused by dendrite formation, and improving the reliability and cycle performance of the battery cell. Furthermore, the absorbed free electrolyte forms a new aggregated electrolyte with the elastic porous sustained-release electrolyte, ensuring that the electrolyte has relatively high conductivity, thereby improving the electrical performance of the battery cell.
[0014] In some embodiments, the battery cell satisfies the following equation:
number
number
[0015] In this way, when the embodiment of the present invention is given by the above formula, it is possible to further improve both the reliability of the battery cell and its cycle performance.
[0016] In some embodiments, the battery cell also satisfies the following equation:
number
number
number
[0017] m1 represents the mass of the electrode assembly before drying, expressed in units of g.
[0018] m2 represents the dried mass of the electrode assembly in grams.
[0019] In this way, when the embodiment of the present invention is given by the above formula, it is possible to further improve both the reliability of the battery cell and its cycle performance.
[0020] In some embodiments, the amount of free electrolyte per unit volume of a battery cell is b, with units of mg / Ah, where 0 ≤ b ≤ 1400, selectively 0.1 ≤ b ≤ 1000, and more selectively 0.3 ≤ b ≤ 800.
[0021] In this way, when the embodiment of the present invention is given by the above formula, it is possible to further improve both the reliability of the battery cell and its cycle performance.
[0022] In some embodiments, the first pole piece includes a current collector and an active material layer provided on at least one surface of the current collector, the active material layer comprising a hydrophilic polymer and active material particles, the hydrophilic polymer distributed on the surface of the active material particles and / or there being multiple active material particles with pores between adjacent active material particles, the hydrophilic polymer distributed in the pores between the active material particles.
[0023] In this way, the embodiments of the present application can improve the liquid retention capacity of the first electrode sheet by disposing the lyophilic polymer on the first electrode sheet, and can further achieve both improvement of the use reliability and cycle performance of the battery cell.
[0024] In some embodiments, the separator includes a substrate and a coating disposed on at least one surface of the substrate, the lyophilic polymer is distributed in the pores of the substrate, and / or the lyophilic polymer is distributed within the coating, and / or the lyophilic polymer is disposed on the surface of the coating away from the substrate.
[0025] In this way, the embodiments of the present application can improve the liquid retention capacity of the separator by disposing the lyophilic polymer on the separator, and can further achieve both improvement of the use reliability and cycle performance of the battery cell.
[0026] In some embodiments, the lyophilic polymer comprises a fluoropolymer, the crystallinity of the fluoropolymer measured by differential scanning calorimetry is Xc1, 0<Xc1≤30%, and the melting temperature of the fluoropolymer is T m1 , the unit of which is °C, 0<T m1 ≤140.
[0027] In some embodiments, the glass transition temperature of the fluoropolymer is T g1 , the unit of which is °C, -150≤T g1 ≤60.
[0028] In some embodiments, the fluoropolymer comprises at least one of the structural units represented by formula (AI) to the structural unit represented by formula (AIII), [Chemical Formula]
[0029] In formula (AI) and formula (AII), R 11 , R 12 , R 13 and R 14each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and R 11 , R 12 , R 13 and R 14 at least one of them contains a fluorine atom, and when substituted, the substituent includes one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom, ##STR##
[0030] In formula (AIII), R 15 represents a single bond, a substituted or unsubstituted C1-C3 alkyl group, and when substituted, the substituent includes one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom, p is a positive integer selected from 1 to 3, and n is a positive integer selected from 1000 to 30000.
[0031] In some embodiments, the lyophilic polymer includes an ether-based polymer, wherein the ether-based polymer is fabricated into a sheet-like structure, and the sheet-like structure is subjected to a dynamic frequency sweep test at (T m2 +20)°C to obtain an elastic modulus G'-energy dissipation modulus G'' curve, the slope of the elastic modulus G'-energy dissipation modulus G'' curve is K1, 1<K1<∞, T m2 °C represents the melting temperature of the ether-based polymer, optionally, 1<K1≦100, and further optionally, 1<K1≦10.
[0032] In some embodiments, the ether-based polymer comprises a structural unit represented by formula (BI) and / or a structural unit represented by formula (BII), ##STR##
[0033] In formula (BI), R 21 and R 22 each independently include a hydrogen atom, a substituted or unsubstituted C1~C3 alkyl group, or a substituted or unsubstituted C1~C3 alkoxy group, and R 23 includes a substituted or unsubstituted C1~C5 alkylene group,
Chemical Formula
[0034] In formula (BII), R 24 to R 27 each independently include a hydrogen atom, a substituted or unsubstituted C1~C3 alkyl group, a substituted or unsubstituted C1~C3 alkoxy group, or an ether group, and at least one of R 24 to R 27 includes a substituted or unsubstituted C1~C3 alkoxy group or an ether group.
[0035] In some embodiments, the substituent may include one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom.
[0036] In some embodiments, the lyophilic polymer includes an ester-based polymer, where the ester-based polymer is fabricated into a sheet-like structure, and the sheet-like structure is subjected to a dynamic frequency sweep test at (T m3 +20)°C to obtain an elastic modulus G'-energy dissipation modulus G'' curve, the slope of the elastic modulus G'-energy dissipation modulus G'' curve is K2, 1<K2<∞, T m3 °C represents the melting temperature of the ester-based polymer, optionally 1<K2≦100, and further optionally 1<K2≦10.
[0037] In some embodiments, the ester-based polymer includes the structural unit represented by formula (CI) and / or the structural unit represented by formula (CII),
Chemical Formula
[0038] In equation (CI), R 31 , R 32 and R 33 Each independently contains a hydrogen atom or a substituted or unsubstituted C1-C8 alkyl group, R 34 This includes a substituted or unsubstituted C1-C8 alkyl group, or a substituted or unsubstituted C1-C8 hydroxyalkyl group. [ka]
[0039] In equation (CII), R 35 It contains substituted or unsubstituted C2-C6 methylene groups, and selectively, R 35 Each of these independently contains a substituted or unsubstituted C2-C4 methylene group.
[0040] In some embodiments, the substituent may include one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom.
[0041] In some embodiments, the hydrophilic polymer includes an aldehyde ketone polymer, where the aldehyde ketone polymer is produced into a sheet-like structure, and the sheet-like structure is (T m4 The elastic modulus G'-energy consumption coefficient G'' curve was obtained by dynamic frequency scanning testing at +20°C, and the slope of the elastic modulus G'-energy consumption coefficient G'' curve is K3, 0.8≦K3<∞, T m4 °C represents the melting temperature of the aldehyde ketone polymer, selectively defined as 0.8 ≤ K3 ≤ 100, and even more selectively defined as 0.8 ≤ K3 ≤ 10.
[0042] In some embodiments, the aldehyde ketone polymer comprises a structural unit represented by formula (DI) and / or a structural unit represented by formula (DII), [ka]
[0043] In equation (DI), R 41 It contains single bonds, substituted or unsubstituted C1-C6 methylene groups, R 42 It contains a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group, [ka]
[0044] In equation (DII), R 43 ~R 46 Each of these independently comprises a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 hydroxyalkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and r and s are each independently selected integers from 0 to 5, and at least one of r and s is selected from positive integers.
[0045] In some embodiments, the substituent may include one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom.
[0046] In some embodiments, the molecular weight of the hydrophilic polymer is 1.2 × 10⁻⁶. 5 g / mol ~ 1 × 10 6 It is g / mol.
[0047] A second aspect of the present application further provides a battery comprising a battery cell described in any one embodiment of the first aspect of the present application.
[0048] A third aspect of the present application further provides an electrical device including a battery as described in the embodiment of the second aspect of the present application. [Brief explanation of the drawing]
[0049] To more clearly explain the technical concept in the embodiments of this application, the drawings necessary for the embodiments of this application are briefly described below. Clearly, the drawings described below represent only a few embodiments of this application, and those skilled in the art can obtain further drawings based on these drawings without requiring any creative effort.
[0050] [Figure 1] This is a schematic diagram of one embodiment of the battery cell according to the present invention.
[0051] [Figure 2] Figure 1 is a schematic exploded view of an embodiment of the battery cell.
[0052] [Figure 3] This is a schematic diagram of one embodiment of the battery module according to the present invention.
[0053] [Figure 4] This is a schematic diagram of one embodiment of the battery pack according to the present invention.
[0054] [Figure 5] Figure 4 is a schematic exploded view of an embodiment of the battery pack shown.
[0055] [Figure 6] This is a schematic diagram of one embodiment of an electrical device that includes a battery cell as a power source according to the present application.
[0056] Drawings are not always drawn to scale.
[0057] The following is an explanation of the drawing symbols.
[0058] 1. Battery pack, 2. Upper case, 3. Lower case, 4. Battery module,
[0059] 5. Battery cell, 51. Casing, 52. Electrode assembly,
[0060] 53. Cover plate,
[0061] 6. Electrical equipment. [Modes for carrying out the invention]
[0062] The following describes in detail embodiments specifically disclosing the battery cell, battery, and electrical device relating to the present application. However, unnecessary details may be omitted. For example, detailed explanations of well-known matters and redundant explanations of structures that are actually the same may be omitted. This is to avoid making the following explanation unnecessarily long and to make it easily understandable to those skilled in the art. The drawings and the following explanation are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the topics described in the claims.
[0063] The “range” disclosed in this application is limited in the form of a lower limit and an upper limit, and a given range is limited by selecting one lower limit and one upper limit, which define the boundary of a particular range. The range thus limited may or may not include the endpoints, and any combination is possible, that is, any lower limit can be combined with any upper limit to form a range. For example, if the ranges 60-120 and 80-110 are listed for a particular parameter, it is understood that the ranges 60-110 and 80-120 can also be assumed. Furthermore, if 1 and 2 are listed as the minimum range values and 3, 4, and 5 are listed as the maximum range values, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 can all be assumed. In this application, unless otherwise specified, the numerical range “a-b” represents an abbreviated expression for any combination of real numbers a-b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 to 5" have already been listed in this specification, and "0 to 5" is simply an abbreviated representation of combinations of these numbers. Also, when a parameter is described as an integer ≥ 2, it is equivalent to disclosing that this parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0064] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions. Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical solutions.
[0065] Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably in order. For example, if a method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, if a method mentioned may further include step (c), it means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), and so on.
[0066] Unless otherwise specified, the terms "include" and "inclusive" as used in this application may be open or closed. For example, "include" and "inclusive" may further include or include other components not listed, or they may include or include only the listed components.
[0067] Unless otherwise specified, the term “or” is inclusive in this application. For example, the phrase “A or B” means “A, B, or both A and B.” More specifically, any one of the following conditions satisfies “A or B”: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or both A and B are true (or exist).
[0068] In this application, the terms "multiple" and "multiple types" refer to two or more types.
[0069] Unless otherwise specified, the terms used in this application have the meanings generally understood by those skilled in the art.
[0070] Unless otherwise stated, the numerical values of each parameter referred to herein can be measured by various measurement methods commonly used in the art, for example, by testing according to the methods described in the embodiments of this application.
[0071] The term "alkyl group" includes both linear and branched alkyl groups. For example, an alkyl group may be a C1-C5 alkyl group, a C1-C4 alkyl group, a C1-C3 alkyl group, or a C1-C2 alkyl group. In some embodiments, the alkyl group includes methyl, ethyl, propyl, isopropyl, butyl, and isobutyl groups. Furthermore, the alkyl group may be optionally substituted. If substituted, the substituent includes a fluorine atom.
[0072] The term "alkoxy group" refers to an alkyl group bonded to an oxygen atom via a single bond. For example, the alkoxy group may be a C1-C5 alkoxy group, a C1-C3 alkoxy group, or a C1-C2 alkoxy group. In some embodiments, the alkoxy group may include a methoxy group, an ethoxy group, or a propoxy group. Furthermore, the alkoxy group may be optionally substituted.
[0073] The term "halogen atom" refers to atoms such as fluorine, chlorine, and bromine.
[0074] The term "hydrogen" refers to 1H (hydrogen, H), 2H (deuterium, D), or 3H (tritium, T). In each example, "hydrogen" may also be 1H (hydrogen, H).
[0075] The battery cell comprises an electrode assembly including a positive electrode piece, a negative electrode piece, and a separator, and an electrolyte. The separator is placed between the positive and negative electrode pieces and primarily serves to prevent short circuits between them, while simultaneously allowing active ions to pass freely and form a circuit.
[0076] When the electrolyte is immersed in the electrode assembly, active ions can move from the positive electrode piece to the negative electrode piece via the separator. However, during the battery cell's use process, the volume of the electrode assembly may change (e.g., expand) due to the insertion or removal of active ions. The electrolyte immersed in the electrode assembly is continuously pushed out, and not all of the pushed-out electrolyte can be reabsorbed into the electrode assembly. This increases the risk of metal deposition and dendrite formation due to insufficient liquid in the electrode assembly. As the dendrites grow, they can break through the separator, causing a short circuit between the positive and negative electrode pieces, which can degrade the battery cell's reliability and cycle performance.
[0077] In view of the above problems, the present invention provides a battery cell that can improve the reliability of a battery cell by adding a hydrophilic polymer to an electrode assembly, which can pack the electrolyte between the molecular chains of the polymer after contact with and mixing with the free electrolyte to form an aggregated electrolyte, thereby ensuring the electrical performance of the battery cell. The present invention will now be described in detail.
[0078] battery cell
[0079] In a first aspect, the present invention provides a battery cell comprising an electrode assembly including a first electrode piece, a second electrode piece, and a separator, and an electrolyte, wherein the polarities of the first electrode piece and the second electrode piece are opposite, the separator is placed between the first electrode piece and the second electrode piece, and at least one of the first electrode piece, the second electrode piece, and the separator comprises a hydrophilic polymer.
[0080] The aforementioned battery cell satisfies the following equation:
number
[0081] p1 represents the porosity of the first pole piece,
[0082] v1 is the total volume of the first pole piece in units of μm3 Represented by,
[0083] p2 represents the porosity of the second pole piece,
[0084] v2 is the total volume of the second pole piece in units of μm 3 Represented by,
[0085] p3 represents the porosity of the separator,
[0086] v3 is the total volume of the separator in units of μm 3 Represented by,
[0087] y represents the mass of the free electrolyte in the battery cell, expressed in units of g.
[0088] In the embodiments of this application, the porosity p has a meaning known in the art and can be detected using instruments and methods known in the art. For example, it can be obtained by gas displacement.
number
[0089]
number
number
[0090] In the embodiments of this application, the total volume v has a meaning known in the art and can be detected using instruments and methods known in the art. For example, the length, width, and height of the sample can be measured using a ruler, and the total volume can be calculated by multiplying the three values.
[0091] In the embodiments of this application, after the electrolyte is injected into the battery cell, the electrolyte mainly exists in the following several forms: firstly, it is adsorbed onto the electrode pieces and / or separator; secondly, it forms an aggregated electrolyte with the hydrophilic polymer; and thirdly, it exists as a liquid and is free within the battery cell. y represents the mass of the electrolyte in the third state, i.e., the mass of the free electrolyte. The mass of the free electrolyte can be measured by the following method: Take out a new battery cell, discharge it completely to a 0% SOC charge state, make a hole with a diameter of φ5~8 mm at a local location in the battery cell, place the battery cell with the hole facing downwards directly above a container so that the free electrolyte inside the battery cell drips into the container below, leave the battery cell in this state for 3h~5h so that all of the free electrolyte inside drips into the container, and then measure the volume of the electrolyte in the container to obtain y. In the embodiments of this application, a new battery cell may be a battery cell that has just been shipped from the factory (a battery cell that has not undergone any charge-discharge cycles since its formation), or a battery cell that has been installed in an electrical device and has had fewer than 10 cycles.
[0092]
number
[0093] When the embodiments of the present application satisfy the range of the above formula, the hydrophilic polymer has a relatively good affinity for the electrolyte, and the electrolyte can rapidly diffuse between the molecular chains of the hydrophilic polymer and be encapsulated by the molecular chains, swelling and adsorption to obtain an elastic porous sustained-release electrolyte. The sustained-release electrolyte can absorb the free electrolyte in the battery cell, reducing the presence of the free electrolyte, and since the free electrolyte is trapped, the risk of the free electrolyte being pushed out is reduced, thereby reducing the risk of short circuits between the positive and negative electrode pieces caused by dendrite formation, improving the reliability and cycle performance of the battery cell. Furthermore, the absorbed free electrolyte forms a new aggregated electrolyte with the elastic porous sustained-release electrolyte, ensuring that the electrolyte has relatively high conductivity, thereby improving the electrical performance of the battery cell.
[0094] Therefore, the embodiment of the present application is
number
number
number
[0095] for example,
number
[0096] These are 0%, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.012%, 0.014%, 0.016%, 0.018%, 0.02%, 0.022%, 0.024%, 0.0 26%, 0.028%, 0.03%, 0.032%, 0.034%, 0.036%, 0.038%, 0.04%, 0.042%, 0.044%, 0.046%, 0.048%, 0.05%, 0.052%, 0.054%, 0.056%, 0.058%, 0.06%, 0.062% , 0.064%, 0.066%, 0.068%, 0.07%, 0.072%, 0.074%, 0.076%, 0.078%, 0.08%, 0.082%, 0.084%, 0.086%, 0.088%, 0.09%, 0.092%, 0.094%, 0.096%, 0.098%, 0 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.60%, 0.65%, 0.70%, 0.75%, 0.80%, 0.85%, 0.90%, 0.95%, 1.00%, 1.10%, 1.20%, 1.30%, 1.40%, 1.50%, 1.60%, 1.70%, 1.80%, 1.90%, 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, 2.80%, 2.90%, 3.00%, 3.10%, 3.20%, 3.30% 3.40%, 3.50%, 3.60%, 3.70%, 3.80%, 3.90%, 4.00%, 4.10%, 4.20%, 4.30%, 4.40%, 4.50%, 4.60%, 4.70%, 4.80%, 4.90%, 5.00%, 5.10%, 5.20%, 5.30%, 5.40 %, 5.50%, 5.60%, 5.70%, 5.80%, 5.90%, 6.00%, 6.10%, 6.20%, 6.30%, 6.40%, 6.50%, 6.60%, 6.70%, 6.80%, 6.90%, 7.00%, 7.10%, 7.20%, 7.30%, 7.40%, 7.5 0%, 7.60%, 7.70%, 7.80%, 7.90%, 8.00%, 8.10%, 8.20%, 8.30%, 8.40%, 8.50%, 8.60%, 8.70%, 8.80%, 8.90%, 9.00%, 9.10%, 9.20%, 9.30%, 9.40%, 9.50%, 9.60%, 9.70%, 9.80%, 9.90%, 10%, 10.10%, 10.20%, 10.30%, 10.40%, 10.50%, 10.60%, 10.70%, 10.80%, 10.90%, 11.00%, 11.10%, 11.20%, 11.30%, 11.40%, 11.5 0%, 11.60%, 11.70%, 11.80%, 11.90%, 12.00%, 12.10%, 12.20%, 12.30%, 12.40%, 12.50%, 12.60%, 12.70%, 12.80%, 12.90%, 13.00%, 13.10%, 13.20%, 13.30% The range may be 13.40%, 13.50%, 13.60%, 13.70%, 13.80%, 13.90%, 14.00%, 14.10%, 14.20%, 14.30%, 14.40%, 14.50%, 14.60%, 14.70%, 14.80%, 14.90%, 15.00%, 15.50%, 16.00%, 16.50%, 17.00%, 17.50%, 18.00%, 18.50%, 19.00%, 19.50%, 20.00%, 20.50%, 21.00%, 21.50%, 22.00%, 22.50%, 23.00%, or any two of the above values.
[0097] In some embodiments, the battery cell also satisfies the following equation:
number
[0098] m1 represents the mass of the electrode assembly before drying, expressed in grams. This mass is obtained by disassembling the battery cell, removing the electrode assembly, and allowing it to stand for 3 to 5 hours to drain the free electrolyte from within the electrode assembly.
[0099] m2 represents the mass of the electrode assembly after drying, expressed in grams. The mass after drying represents the mass of the electrode assembly obtained after drying and removing the electrolyte adsorbed on the electrode assembly. For example, if an electrode assembly is placed in a drying box and dried at 60°C to 95°C for 24 to 48 hours, then immersed in dimethyl carbonate (DMC) solvent, and then placed in a drying box again and dried at 60°C to 95°C for 24 to 48 hours, the resulting electrode assembly is considered the dried electrode assembly.
[0100] m2-m1 represents the mass of electrolyte adsorbed onto the electrode assembly, and y+m2-m1 represents the sum of the mass of free electrolyte and the mass of electrolyte adsorbed onto the electrode assembly, which can be considered the total amount of electrolyte in the battery cell.
[0101]
number
[0102] The embodiments of this application are within the range of the above formula.
number
number
number
number
[0103] In some embodiments, the amount of free electrolyte per unit volume of a battery cell is b, with units of mg / Ah, and 0 ≤ b ≤ 1400. When the amount of free electrolyte b per unit volume of a battery cell satisfies the above range, the reliability and cycle performance of the battery cell can be further improved.
[0104] Selectively, 0.1 ≤ b ≤ 1000, and more selectively, 0.3 ≤ b ≤ 800. Exemplary examples include the amount of free electrolyte per unit volume of a battery cell: 0 mg / Ah, 0.001 mg / Ah, 0.002 mg / Ah, 0.003 mg / Ah, 0.004 mg / Ah, 0.005 mg / Ah, 0.006 mg / Ah, 0.007 mg / Ah, 0.008 mg / Ah, 0.009 mg / Ah, 0.01 mg / Ah, 0.02 mg / Ah, 0.0 3mg / Ah, 0.04mg / Ah, 0.05mg / Ah, 0.06mg / Ah, 0.07mg / Ah, 0.08mg / Ah, 0.09mg / Ah, 0.1mg / Ah, 0 .2mg / Ah, 0.3mg / Ah, 0.5mg / Ah, 1.0mg / Ah, 5.0mg / Ah, 10.0mg / Ah, 20.0mg / Ah, 50.0mg / Ah, 80. 0mg / Ah, 100mg / Ah, 120mg / Ah, 150mg / Ah, 180mg / Ah, 200mg / Ah, 220mg / Ah, 250mg / Ah, 300mg / A h, 350mg / Ah, 400mg / Ah, 450mg / Ah, 500mg / Ah, 550mg / Ah, 600mg / Ah, 650mg / Ah, 700mg / Ah, 750 The range may be mg / Ah, 800 mg / Ah, 850 mg / Ah, 900 mg / Ah, 950 mg / Ah, 1000 mg / Ah, 1050 mg / Ah, 1100 mg / Ah, 1150 mg / Ah, 1200 mg / Ah, 1250 mg / Ah, 1300 mg / Ah, 1350 mg / Ah, 1400 mg / Ah, or any two of the above values.
[0105] In the embodiments of this application, b is equal to y / x, where x is the nominal capacity of the battery cell in units of Ah, and y is the mass of the free electrolyte as described above.
[0106] In embodiments of the present application, x can be detected using methods and equipment known in the art. For example, it is the product of the total amount of current that can be output and the discharge time when a battery cell is fully charged and discharged to a cutoff voltage at a constant current and voltage of 0.33C.
[0107] In some embodiments, the battery cell is charged to a 100% charged state (SOC) after a linear frequency sweep vibration test, a hole is made in the battery cell, the hole is placed at the lowest point in the vertical direction, and the mass of electrolyte that flows out of the battery cell is recorded as M1, where 0 ≤ M1 ≤ 6 g, and selectively, M1 is 0 g.
[0108] Here,
[0109] The vibration direction of the linear frequency sweep vibration test described above is a single vertical vibration.
[0110] The vibration frequency of the linear frequency sweep vibration test described above is 10 Hz to 55 Hz.
[0111] The maximum acceleration in the linear frequency sweep vibration test was 30 m / s².
[0112] The number of frequency sweep cycles in the linear frequency sweep vibration test described above was 10.
[0113] The vibration duration of the linear frequency sweep vibration test described above is 3 hours.
[0114] In related technologies, battery cells may vibrate due to external forces during the usage process, and the electrolyte located within the electrode assembly may detach from the electrode assembly due to vibration, forming free electrolyte. On the other hand, leakage of free electrolyte from within the battery cell can corrode the battery cell and lead to risks such as battery cell failure. In contrast, the embodiments of the present invention can effectively collect and discharge the electrolyte within the battery cell by placing the battery cell still and vibrating it, thereby more accurately determining whether there is electrolyte flowing between the battery cell casing and the electrode assembly, and determining the content of free electrolyte. When the battery cell of the embodiments of the present invention satisfies the above conditions, the content of free electrolyte within the battery cell is extremely low, and furthermore, the battery cell basically contains no free electrolyte, thereby significantly improving the reliability and cycle performance of the battery cell.
[0115] For example, M1 is 0, 0.05g, 0.10g, 0.15g, 0.20g, 0.25g, 0.3g, 0.35g, 0.4g, 0.45g, 0.5g, 0.55g, 0.60g, 0.65g, 0.70g, 0.75g, 0.80g, 0.85g, 0.90g, 0.95g, 1.00g, 1.10g, 1.20g, 1.30g, 1.40g, 1.50g, 1.60g, 1.70g, 1.80g, 1.90g, 2.00g, 2.10g, 2.20g g, 2.30g, 2.40g, 2.50g, 2.60g, 2.70g, 2.80g, 2.90g, 3.00g, 3.10g, 3.20g, 3.30g, 3.40g, 3.50g, 3.60g, 3.70g, 3.80g, 3.90g, 4.00g, 4.10g, 4.20g, 4.30g, 4.40g, 4.50g, 4.60g, 4.70g, 4.80g, 4.90g, 5.00g, 6.00g, or any two of the above values. M1 being 0g means that the amount of free electrolyte is 0, i.e., the battery cell has essentially no free electrolyte inside after the linear frequency sweep vibration test.
[0116] In some embodiments, after the linear frequency sweep vibration test, the battery cell's casing is removed, the electrode assembly is taken out, and after a pressure test, the volume of electrolyte flowing out of the electrode assembly is recorded as M2 (by suspending a pressure device and placing a weighing balance and electrolyte collection container at the bottom). The condition is 0 ≤ M2 ≤ 0.6 g, and selectively, M2 is 0 g. Here,
[0117] The pressing direction in the aforementioned pressing test is perpendicular to the thickness direction of the electrode assembly.
[0118] The degree of pressure in the aforementioned pressure test was a pressing force of 0.35 MPa.
[0119] In related technologies, battery cells may be subjected to external forces during the usage process. The electrolyte located within the electrode assembly may detach from the electrode assembly due to the pressure, forming free electrolyte. On the other hand, leakage of free electrolyte from within the battery cell can corrode the battery cell and lead to risks such as battery cell failure. Embodiments of the present invention allow for effective pressure testing of the battery cell to expel the electrolyte from within the battery cell. This enables a more accurate determination of whether there is electrolyte flowing between the battery cell casing and the electrode assembly, and thus allows for the determination of the free electrolyte content. When the battery cell of the embodiment of the present invention satisfies the above conditions, the free electrolyte content within the battery cell is extremely low, and furthermore, the battery cell basically contains no free electrolyte, thereby significantly improving the reliability and cycle performance of the battery cell.
[0120] For example, M2 is 0, 0.05 mg, 0.10 mg, 0.15 mg, 0.20 mg, 0.25 mg, 0.3 mg, 0.35 mg, 0.4 mg, 0.45 mg, 0.5 mg, 0.55 mg, 0.60 mg, 0.65 mg, 0.70 mg, 0.75 mg, 0.80 mg, 0.85 mg, 0.90 mg, 0.95 mg, 1.00 mg, 1.10 mg, 1.20 mg, 1.30 mg, 1.40 mg, 1.50 mg, 1.60 mg, 1.70 mg, 1.80 mg, 1.90 mg, 2.00 mg, 2.10 mg, 2.20 mg, 2.30 mg, 2.40 mg , 2.50mg, 2.60mg, 2.70mg, 2.80mg, 2.90mg, 3.00mg, 3.10mg, 3.20mg, 3.30mg, 3.40mg, 3.50mg, 3.60mg, 3.70mg, 3.80mg, 3.90mg, 4.00mg, 4.10mg, 4.2 0mg, 4.30mg, 4.40mg, 4.50mg, 4.60mg, 4.70mg, 4.80mg, 4.90mg, 5.00mg, 10.00mg, 20.00mg, 30.00mg, 40.00mg, 50.00mg, 60.00mg, 70.00mg, 80.00mg , 90.00mg, 100.00mg, 110.00mg, 120.00mg, 130.00mg, 140.00mg, 150.00mg, 160.00mg, 170.00mg, 180.00mg, 190.00mg, 200.00mg, 210.00mg, 220.00 mg, 230.00mg, 240.00mg, 250.00mg, 260.00mg, 270.00mg, 280.00mg, 290.00mg, 300.00mg, 310.00mg, 320.00mg, 330.00mg, 340.00mg, 350.00mg, 360 The range may be 0.00mg, 370.00mg, 380.00mg, 390.00mg, 400.00mg, 410.00mg, 420.00mg, 430.00mg, 440.00mg, 450.00mg, 460.00mg, 470.00mg, 480.00mg, 490.00mg, 500.00mg, 510.00mg, 520.00mg, 530.00mg, 540.00mg, 550.00mg, 560.00mg, 570.00mg, 580.00mg, 590.00mg, 600.00mg, or any two of the above values.A value of 0g for M2 indicates that the amount of free electrolyte is 0, meaning that the battery cell essentially contains no free electrolyte after the pressure test.
[0121] In this application, the pressure test may be performed after the linear frequency sweep vibration test; that is, the battery cell is first subjected to a linear frequency sweep vibration test, then to a pressure test, and the M2 value is measured, and if 0 ≤ M2 ≤ 0.5g, selectively, M2 is 0g.
[0122] In some embodiments, a voltage of 200V is supplied to the battery cell to form a circuit for 4h, and the absolute value of the temperature change of the battery cell is ≤ 4°C.
[0123] For example, by connecting the negative terminal and outer casing of the battery cell to a voltage of 200V to form a current circuit, the temperature fluctuation range of the battery cell within 4 hours is 4°C or less, and there are no failure behaviors such as fire or explosion. In particular, when the free electrolyte y=0, the temperature fluctuation range is relatively small, and the reliability of the battery cell is greatly improved.
[0124] In some embodiments, the electrode pieces include a hydrophilic polymer, specifically, the first electrode piece includes a current collector and an active material layer provided on at least one surface of the current collector, the active material layer including a hydrophilic polymer and active material particles. The hydrophilic polymer may be provided only on the first electrode piece, or only on the second electrode piece, or the hydrophilic polymer may be provided on both the first and second electrode pieces. The first electrode piece may be a positive electrode piece and correspondingly the second electrode piece may be a negative electrode piece, or the first electrode piece may be a negative electrode piece and correspondingly the second electrode piece may be a positive electrode piece.
[0125] As one example, the hydrophilic polymer is distributed on the surface of the active material particles. The active material particles and adhesives are solidified in a film layer on the surface of the current collector, and the hydrophilic polymer is placed on the surface of the film layer away from the current collector. By placing it in this manner, the electrolyte can rapidly diffuse between the molecular chains of the hydrophilic polymer and be encapsulated by the molecular chains, forming a gel-like substance on the surface of the active material particles, which adheres to the surface of the active material particles and provides a protective effect against them. In this way, the active material particles are closely bound to the electrolyte, improving the solid-liquid interface performance, reducing sub-reactions between the active material particles and the electrolyte, and improving the reliability and electrical properties (e.g., cycle performance and storage performance) of the battery cell.
[0126] Specifically, the manufacturing process for the polarity fragments is:
[0127] Adding active material particles to a solvent to produce an active slurry,
[0128] The activated slurry is applied to the surface of the current collector and solidified into a film layer after drying.
[0129] This includes placing a hydrophilic polymer on the surface of a film layer to form polar flakes.
[0130] In some other examples, the active material particles are multiple, with pores between adjacent active material particles, and the hydrophilic polymer is distributed in the pores between the active material particles. This arrangement can improve the liquid storage capacity of the active material layer, i.e., its ability to contain the electrolyte, thereby improving the reliability and electrical properties of the battery cell.
[0131] Specifically, the manufacturing process of one embodiment of the polarity is as follows:
[0132] Dispersing a hydrophilic polymer in a solvent to form a mixed system,
[0133] The process involves adding active material particles to the aforementioned mixed system to produce a slurry,
[0134] The method includes applying the slurry to the surface of a current collector and allowing it to dry and solidify into electrode pieces.
[0135] Specifically, the manufacturing process for another embodiment of the polarity is as follows:
[0136] The process involves dispersing a hydrophilic polymer and active material particles in a solvent to produce a slurry,
[0137] The method includes applying the slurry to the surface of a current collector and allowing it to dry and solidify into electrode pieces.
[0138] As some further examples, the hydrophilic polymer is distributed on the surface of the active material particles, and the hydrophilic polymer is distributed in the pores between the active material particles.
[0139] Specifically, the manufacturing process of one embodiment of the polarity is as follows:
[0140] The process involves dispersing a hydrophilic polymer and active material particles in a solvent to produce a slurry,
[0141] The slurry is applied to the surface of the current collector and solidified into a film layer after drying.
[0142] This includes placing a hydrophilic polymer on the surface of a film layer to form polar flakes.
[0143] In some other embodiments, the separator comprises a hydrophilic polymer, and specifically, the separator may comprise a substrate, and optionally, the separator may further comprise a coating applied to at least one surface of the substrate.
[0144] As some examples, the substrate is generally a porous structure having pores, and the hydrophilic polymer may be distributed in the pores of the substrate.
[0145] As some other examples, the hydrophilic polymer may be distributed within the coating.
[0146] As some further examples, the hydrophilic polymer may be placed on a surface of the coating that is separated from the substrate.
[0147] The specific distribution location of the hydrophilic polymer may be any one of the three types described above, any two of the three types, or a combination of the three types of locations described above.
[0148]
[0149] In some further embodiments, the hydrophilic polymer may be placed on the electrode pieces and separators, with specific placement locations as described above, and their explanation is omitted here.
[0150]
[0151] In some embodiments, the hydrophilic polymer may include one or more of the following: fluorinated polymers, ether polymers, ester polymers, and ketone aldehyde polymers.
[0152] [Fluorine-based polymers]
[0153] In some embodiments, the hydrophilic polymer includes a fluorinated polymer, and the crystallinity of the fluoropolymer, as measured by differential scanning calorimetry, is X C1 %, 0 <X C1 The value is ≤30, and the melting temperature of the fluoropolymer is T m1 The unit is °C, 0 <T m1 The value is ≤ 140.
[0154] Crystallization refers to the process by which atoms, ions, or molecules in a material are arranged according to a certain spatial order, forming an orderly structure. The conformation of a polymer during crystallization is determined by two factors: intramolecular and intermolecular forces, with intermolecular forces influencing the stacking density between molecular chains. Crystallinity X C1The percentage (%) is used to characterize the crystallinity of a material and can be measured by differential scanning calorimetry (DSC). Specifically, the test step involves taking 0.5g to 0.8g of sample, placing the sample in a crucible, heating and cooling the sample in a nitrogen atmosphere, and measuring the material's inherent T2C at a heating rate of 10°C / min. g1 Starting from an initial temperature 20°C lower, the material's inherent T m1 Up to a cutoff temperature 20°C higher, the actual glass transition temperature T of the material is determined according to the endothermic and endothermic peak values or transition points of the material in the process. g1 and melting temperature T m1 These will be decided.
[0155] In this way, fluoropolymers have relatively low crystallinity and melting temperatures, tend to have loose molecular chain arrangements, relatively small inter-chain forces, adjacent molecular chains easily open, and achieve movement of chain segments through intermolecular internal rotation, forming a relatively flexible molecular chain structure. Furthermore, the fluoropolymer and the electrolyte in the battery cell can form a gel-like substance, improving the reliability and cycle performance of the battery cell.
[0156] For example, the degree of crystallinity X of a fluoropolymer measured by differential scanning calorimetry. C1 The percentage may be a range consisting of 5%, 10%, 15%, 20%, 25%, 30%, or any two of the above values.
[0157] For example, the melting temperature of the fluoropolymer may be in the range of 10°C, 20°C, 50°C, 70°C, 90°C, 100°C, 120°C, 140°C, or any two of the above values.
[0158] In some embodiments, the glass transition temperature of the fluoropolymer is T g1 The unit is °C, -150 ≤ T g1 The value is ≤60.
[0159] The glass transition temperature is the temperature at which a polymer chain segment transitions from frozen to moving. The glass transition temperature has a certain effect on the flexibility of the polymer molecular chains; the lower the glass transition temperature, the greater the flexibility of the polymer molecular chains at room temperature, and the higher the glass transition temperature, the less flexible the molecular chains are at room temperature. The glass transition temperature can be measured by differential scanning calorimetry (DSC). A relatively low glass transition temperature of a polymer results in greater flexibility of the chain segments of the molecular chains, and adjacent molecular chains are more likely to open. Exemplarily, the glass transition temperature of a fluoropolymer may be in the range of -150°C, -120°C, -100°C, -80°C, -60°C, -30°C, 0°C, 30°C, 60°C, or any two of the above values.
[0160] In some embodiments, the fluoropolymer comprises at least one of the structural units represented by formula (AI) to formula (AIII), [ka]
[0161] In equations (AI) and (AII), R 11 , R 12 , R 13 and R 14 Each independently contains a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and R 11 , R 12 , R 13 and R 14 At least one of these atoms contains a fluorine atom, and if substituted, the substituent may contain one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom.
[0162] In equation (AIII), R 15includes a single bond, a substituted or unsubstituted C1-C3 alkyl group; when substituted, the substituent may include one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom. p is a positive integer selected from 1 to 3. n is a positive integer selected from 1000 to 30000.
[0163] In some embodiments, R 11 , R 12 , R 13 and R 14 each independently include a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C2 alkyl group, or a substituted or unsubstituted C1-C2 alkoxy group, and further optionally, R 11 , R 12 , R 13 and R 14 each independently include a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, a fluoromethyl group, a methoxy group, or a perfluoromethoxy group.
[0164] In some embodiments, the fluoropolymer includes at least one of the structural units represented by formula (AI-1) to the structural unit represented by formula (AI-11),
Chemical Formula
[0165] In some embodiments, the fluoropolymer includes at least one of the structural units represented by formula (AII-1) to the structural unit represented by formula (AII-5),
Chemical Formula
[0166] In some embodiments, the fluoropolymer includes at least one of the structural units represented by formula (AIII-1) to the structural unit represented by formula (AIII-3),
Chemical Formula
[0167] Exemplary examples include one or more of the following fluoropolymers: polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene copolymer (FEP), perfluoroalkoxy polymer (PFA), perfluoropolyether (PFPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE), and perfluoro(1-butenyl vinyl ether) polymer (CYTOP).
[0168] Selectively, the fluoropolymer includes one or more of the following: polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene copolymer (FEP), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE).
[0169] The above fluoropolymer may be one or more monomers derived from fluorocyclohexane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene. Selectively, the above fluoropolymer may be at least two monomers derived from fluorocyclohexane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene.
[0170] The monomers used in the above-mentioned fluoropolymers are all short-chain monomers, which help in polymerization to form linear or short-branched structures. These types of structures have a relatively low degree of entanglement, which helps improve the flexibility of the molecular chains, allowing the molecular chains to stretch sufficiently in the electrolyte. In this way, the interfacial performance of the active material can be further improved.
[0171] In some embodiments, n is a positive integer selected from 5000 to 20000, and / or the molecular weight of the hydrophilic polymer is 2 × 10⁻⁶. 5 g / mol ~ 1.5 × 10 6 The concentration is g / mol. When the molecular weight of the polymer is within the above range, it is possible to ensure that the polymer exhibits a certain degree of solubility in the electrolyte while simultaneously being difficult to completely dissolve and disperse by the electrolyte. This helps to control the distribution and dispersion of the polymer on the surface of the active material, and further improves the flexibility between the molecular chains of the polymer. The forces between the molecular chains are relatively weak, which helps solvent molecules in the electrolyte to open the molecular chains and enter between them, as well as be enveloped by the molecular chains. In this way, it helps active ions enter the active material through the solvent, enabling smooth and rapid movement of active ions.
[0172] When the molecular weight of a hydrophilic polymer is within the above range, it is possible to ensure that the polymer exhibits a certain degree of solubility in the electrolyte while simultaneously being difficult to completely dissolve and disperse by the electrolyte. This helps to control the distribution and dispersion of the polymer on the surface of the active material, and further improves the flexibility between the polymer's molecular chains. The forces between the molecular chains are relatively weak, which helps solvent molecules in the electrolyte to open the molecular chains, enter between them, and be enveloped by the molecular chains. In this way, it helps active ions enter the active material through the solvent, enabling smooth and rapid movement of active ions. For example, the molecular weight of the polymer is 2 × 10⁻⁶. 5 g / mol, 5 × 10 5 g / mol, 8 × 10 5 g / mol, 1 × 10⁻⁶ 6 g / mol, 1.5 × 10 6It may be g / mol or a range consisting of any two of the above values.
[0173] [Ether-based polymers]
[0174] In some embodiments, the hydrophilic polymer includes an ether-based polymer, the ether-based polymer is manufactured into a sheet-like structure, and the sheet-like structure is (T m2 The elastic modulus G'-energy consumption coefficient G'' curve was obtained by dynamic frequency scanning test at +20°C, and the slope of the elastic modulus G'-energy consumption coefficient G'' curve was K1, 1 <K1<∞であり、T m2 °C represents the melting temperature of ether-based polymers.
[0175] Specifically, the manufacturing process for the sheet-like structure is as follows: The ether-based polymer is vacuum-dried at 80°C for 12 hours. The dried ether-based polymer is hot-pressed in a flat vulcanizing apparatus to form a thin sheet, and the hot-press temperature is set to (T m2 Set the temperature to +20°C, roll to a thickness of 1-2 mm, roll for 2 minutes, and use a pressure of 8 MPa. After 2 minutes of rolling, remove the sample and cold roll it in another vulcanizing apparatus of the same type, using a cold rolling pressure of 10 MPa. A fixed-size polymer disc (sheet-like structure) can be obtained using a circular die with a diameter of 25 mm. Exemplarily, the sheet-like structure may be a disc with a thickness of 1-2 mm and a diameter of 25 mm, and samples may be prepared according to the sample specifications required by the test equipment.
[0176] Based on the conclusions of classical linear viscoelasticity, for polymers, especially linear polymers, the elastic modulus G'-energy consumption coefficient G'' curve in the terminal region (the interval approaching the maximum angular velocity) fits the frequency dependence, and the longest chain of the polymer influences its viscoelastic behavior.
[0177] The specific steps of the dynamic frequency scanning test are as follows. A TA-AR2000EX rotational rheometer (TA Instruments, USA) is used to conduct the dynamic frequency scanning test, with the diameter of the parallel plate set to 25 mm and the thickness set to 0.9 mm. To ensure the test is performed in the linear viscoelastic region, the strain during the dynamic frequency scanning test is set to 2%, and the test temperature is T m2 +20°C, and the frequency scanning range of the test is set to 500 rad / s ≤ ω 2 ≤ 0.05 rad / s, to acquire data at the lowest possible frequency.
[0178] The dynamic frequency scanning test can characterize the degree of molecular chain entanglement in the solid phase molten (molten state) state. Compared with linear structures or short branched chain structures, long branched structures, network structures and low crosslinking structures have a higher degree of entanglement, showing a deviation from linear terminal behavior, and ether-based polymers exhibit solid phase behavior. When the ether-based polymer of the present application satisfies the above range, the entangled state of molecular chains can be further reduced, which is favorable for the diffusion of solvent molecules in the electrolyte between molecular chains, and the ether-based polymer still maintains a certain entangled state of molecular chains, forms a gel-like substance with the electrolyte, and can improve the cycle performance and storage performance of the battery cell.
[0179] In some embodiments, 1 < K1 ≤ 100, and optionally 1 < K1 ≤ 10. Exemplarily, K1 may be 0.8, 0.9, 1, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or a range consisting of any two of the above values.
[0180] In some embodiments, the glass transition temperature of the ether-based polymer is T g2 , its unit is °C, -100 ≤ T g2 ≤ 50, and optionally -80 ≤ T g2 ≤ 30. Exemplarily, the glass transition temperature of the ether-based polymer may be -100°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or a range consisting of any two of the above values.
[0181] In some embodiments, the ether-based polymer comprises a structural unit represented by formula (BI),
Chemical Formula
[0182] In formula (BI), R 21 and R 22 each independently include a hydrogen atom, a substituted or unsubstituted C1 to C3 alkyl group, or a substituted or unsubstituted C1 to C3 alkoxy group, and R 23 includes a substituted or unsubstituted C1 to C5 methylene group, and optionally, R 21 and R 22 each independently include a hydrogen atom, a substituted or unsubstituted C1 to C2 alkyl group, and / or R 23 includes a single bond, a substituted or unsubstituted C1 to C4 methylene group.
[0183] In some examples, the substituent may include one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom.
[0184] Exemplarily, the ether-based polymer comprises at least one of the structural unit represented by formula (BI-1) to the structural unit represented by formula (BI-8),
Chemical Formula
[0185] In some embodiments, the ether-based polymer comprises a structural unit represented by formula (BII),
Chemical Formula
[0186] In formula (BII), R 24 to R 27each independently represents a hydrogen atom, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 alkoxy group or an ether group, and R 24 -R 27 at least one of them contains a substituted or unsubstituted C1-C3 alkoxy group or an ether group.
[0187] Optionally, R 24 -R 27 each independently represents a hydrogen atom, a substituted or unsubstituted C1-C2 alkyl group, a substituted or unsubstituted C1-C2 alkoxy group or an ether group, and R 24 -R 27 at least one of them contains a substituted or unsubstituted C1-C2 alkoxy group or an ether group.
[0188] In some embodiments, the ether-based polymer includes at least one of the structural units represented by formula (BII-1) to the structural unit represented by formula (BII-7), [Chemical Formula]
[0189] The monomer used in the above ether-based polymer is a polycyclic structure, for example, a structure with 6 or fewer membered rings or a short-chain monomer, which facilitates polymerization to form a high content of -O- structure. This type of structure has a relatively low degree of entanglement, which helps to improve the flexibility of the molecular chain. The molecular chain can be fully extended in the electrolyte, easily forming a gel substance with the electrolyte, and improving the cycle performance and storage performance of the battery cell.
[0190] The above polymers are only examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymer may be obtained by copolymerizing the above structural groups with other types of structural groups (for example, olefin-based structural units, acrylonitrile-based structural units, etc.).
[0191] When the above group is substituted, the substituent may include one or more of the following: nitrile group (-CN), nitro group, sulfonic acid group, sulfonyl group, amide, carboxyl group, ester group, and halogen atom. Making the substituent a high-pressure resistant substituent is advantageous for stabilizing the polymer structure. The halogen atom may include fluorine atom, chlorine atom, bromine atom, etc.
[0192] In some embodiments, n is a positive integer selected from 1500 to 25000.
[0193] Selectively, n is a positive integer chosen from 3000 to 18000.
[0194] In some embodiments, the molecular weight of the polymer is 1.2 × 10⁻⁶ 5 g / mol ~ 1.0 × 10 6 It is g / mol.
[0195] For example, the molecular weight of the polymer is 1.2 × 10⁻⁶. 5 g / mol, 2 × 10⁻⁶ 5 g / mol, 5 × 10 5 g / mol, 8 × 10 5 g / mol, 1 × 10⁻⁶ 6 It may be g / mol or a range consisting of any two of the above values.
[0196] [Ester polymers]
[0197] In some embodiments, the hydrophilic polymer includes an ester polymer, wherein the ester polymer is manufactured into a sheet-like structure, and the sheet-like structure is (T m3 The elastic modulus G'-energy consumption coefficient G'' curve was obtained by dynamic frequency scanning test at +20°C, and the slope of the elastic modulus G'-energy consumption coefficient G'' curve was K2, 1 <K2<∞であり、T m3 °C represents the melting temperature of ester polymers.
[0198] When the ester-based polymer of the present application satisfies the above range, the entanglement state of molecular chains can be further reduced, which is advantageous for the diffusion of solvent molecules in the electrolyte between molecular chains, and the ether-based polymer still maintains a certain entanglement state of molecular chains, can form a gel-like substance with the electrolyte, and improve the cycle performance and storage performance of the battery cell.
[0199] In some embodiments, 1<K2≤100, optionally 1<K2≤10.
[0200] Illustratively, K2 may be 1.01, 1.1, 1.2, 1.5, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or a range consisting of any two of the above values.
[0201] In some embodiments, the glass transition temperature of the ester-based polymer is T g3 , the unit of which is °C, -100≤T g3 ≤50, optionally -80≤T g3 ≤30.
[0202] Illustratively, the glass transition temperature of the ester-based polymer may be -100°C, -90°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or a range consisting of any two of the above values.
[0203] In some embodiments, the ester-based polymer comprises a structural unit represented by formula (CI), [Chemical Formula]
[0204] In formula (CI), R 31 , R 32 and R 33 each independently comprise a hydrogen atom, or a substituted or unsubstituted C1~C8 alkyl group, R 34 comprises a substituted or unsubstituted C1~C8 alkyl group, or a substituted or unsubstituted C1~C8 hydroxyalkyl group, optionally, R34 This includes substituted or unsubstituted C1-C6 alkyl groups, or substituted or unsubstituted C1-C6 hydroxyalkyl groups.
[0205] Selectively, R 31 R includes a hydrogen atom or a substituted or unsubstituted methyl group. 32 and R 33 Each of them independently contains a hydrogen atom, R 34 This includes substituted or unsubstituted C1-C4 alkyl groups, or substituted or unsubstituted C1-C4 hydroxyalkyl groups.
[0206] For example, the ester polymer comprises at least one of the structural units represented by formula (CI-1) to formula (CI-15), [ka] [ka]
[0207] In some embodiments, the ester polymer comprises a structural unit represented by formula (CII), [ka]
[0208] In equation (CII), R 35 It contains substituted or unsubstituted C2-C6 methylene groups, and selectively, R 35 Each of these independently contains a substituted or unsubstituted C2-C4 methylene group.
[0209] For example, the ester polymer comprises at least one of the structural units represented by formula (CII-1) to formula (CII-5), [ka]
[0210] The molecular chains of the above-mentioned ester polymers have a relatively low degree of entanglement, which helps to improve the flexibility of the molecular chains. The molecular chains can stretch sufficiently in the electrolyte and readily form a gel-like substance with the electrolyte.
[0211] The polymers described above are merely examples of structural groups of the main molecular chain. In embodiments of the present application, polymers may be obtained by copolymerizing the above structural groups with other types of structural groups (for example, olefin-based structural units, acrylonitrile-based structural units, functional monomers such as maleic anhydride, etc.).
[0212] In some embodiments, the substituent may include one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom.
[0213] In some embodiments, n is a positive integer selected from 800 to 20000.
[0214] Selectively, n is a positive integer chosen from 1000 to 15000.
[0215] In some embodiments, the molecular weight of the polymer is 1.2 × 10⁻⁶ 5 g / mol ~ 1.0 × 10 6 It is g / mol.
[0216] For example, the molecular weight of the polymer is 1.2 × 10⁻⁶. 5 g / mol, 2 × 10⁻⁶ 5 g / mol, 5 × 10 5 g / mol, 8 × 10 5 g / mol, 1 × 10⁻⁶ 6 g / mol, 1.5 × 10 6 It may be g / mol or a range consisting of any two of the above values.
[0217] [Ketone aldehyde polymers]
[0218] In some embodiments, the hydrophilic polymer comprises an aldehyde ketone polymer, wherein the aldehyde ketone polymer is manufactured into a sheet-like structure, and the sheet-like structure is (T m4 A dynamic frequency scanning test at +20°C yielded an elastic modulus G'-energy consumption coefficient G'' curve, and the slope of the elastic modulus G'-energy consumption coefficient G'' curve was K3, 0.8 ≤ K3 < ∞, and T m4 °C represents the melting temperature of the aldehyde ketone polymer.
[0219] In some embodiments, 0.8 ≤ K3 ≤ 100, and selectively, 0.8 ≤ K3 ≤ 10.
[0220] For example, K3 may be a range consisting of 0.8, 0.9, 1, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or any two of the above values.
[0221] In some embodiments, the glass transition temperature of the aldehyde ketone polymer is T g4 The unit is °C, -100 ≤ T g4 ≤ 50, and selectively, -80 ≤ T g4 The value is ≤30.
[0222] For example, the glass transition temperature of an aldehyde ketone polymer may be in the range of -100°C, -90°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or any two of the above values.
[0223] In some embodiments, the aldehyde ketone polymer comprises a structural unit represented by formula (DI), [ka]
[0224] In equation (DI), R 41 It contains single bonds, substituted or unsubstituted C1-C6 methylene groups, R 42It contains a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group,
[0225] Selectively, R 41 It contains single bonds, substituted or unsubstituted C1-C2 methylene groups,
[0226] Selectively, R 42 It contains a hydrogen atom and a substituted or unsubstituted C1-C3 alkyl group.
[0227] In the embodiments of this application, a single bond indicates that there is no group and the atoms on both sides of the group are bonded by a single bond, for example, R 41 The fact that it is a single bond is R 41 This indicates that the carbon atoms on both sides are bonded in the form of a single bond.
[0228] For example, the aldehyde ketone polymer comprises at least one of the structural units represented by formula (DI-1) to formula (DI-6), [ka]
[0229] For example, the aldehyde ketone polymer comprises the structural unit shown in formula (DII), [ka]
[0230] In equation (DII), R 43 ~R 46 Each independently comprises a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 hydroxyalkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and r and s are each independently selected integers from 0 to 5, and at least one of r and s is selected from positive integers, selectively R 43 ~R 46Each of these independently comprises a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C2 hydroxyalkyl group, or a substituted or unsubstituted C1-C2 alkoxy group.
[0231] In some embodiments, the aldehyde ketone polymer comprises at least one of the structural units represented by formula (DII-1) to formula (DII-4), [ka]
[0232] The molecular chains of the above-mentioned aldehyde ketone polymers have a relatively low degree of entanglement, which helps to improve the flexibility of the molecular chains. The molecular chains can stretch sufficiently in the electrolyte and readily form a gel-like substance with the electrolyte.
[0233] The above polymers are merely examples of structural groups of the main molecular chain, and in embodiments of the present application, the polymer may be obtained by copolymerizing the above structural groups with other types of structural groups (e.g., olefin-based structural units, enol-based structural units, acrylonitrile-based structural units, etc.).
[0234] In some embodiments, the substituent may include one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom.
[0235] In some embodiments, n is a positive integer selected from 500 to 15000.
[0236] Selectively, n is a positive integer chosen from 500 to 10000.
[0237] In some embodiments, the molecular weight of the polymer is 1.2 × 10⁻⁶ 5 g / mol ~ 1.0 × 10 6 It is g / mol.
[0238] For example, the molecular weight of the polymer is 1.2 × 10⁻⁶. 5 g / mol, 2 × 10⁻⁶ 5 g / mol, 5 × 10 5 g / mol, 8 × 10 5 g / mol, 1 × 10⁻⁶ 6 g / mol, 1.0 × 10 6 It may be g / mol or a range consisting of any two of the above values.
[0239] Embodiments of the present invention can further improve the reliability and cycle performance of battery cells if the hydrophilic polymer further satisfies one or more of the following conditions.
[0240] In some embodiments, the hydrophilic polymer is added to a first solvent at 70°C to form a polymer system, the polymer system is allowed to stand at 70°C for 8 hours, and then at 25°C for 24 hours or more, and after two-step standing treatments, the polymer system portion is converted into a gel-like substance by swelling and adsorption, and then the polymer system is filtered through a 200-mesh filter to leave the first substance. The mass of the hydrophilic polymer is n, in units of g, and the mass of the first substance is m, in units of g, and the polymer and the first substance have a ratio of 5 ≤ m / n ≤ 1000, selectively 10 ≤ m / n ≤ 1000, and even more selectively 10 ≤ m / n ≤ 50. Exemplarily, m / n may be in the range of 5, 10, 20, 25, 28, 30, 32, 35, 40, 50, 80, 100, 200, 500, 1000, or any two of the above values.
[0241] For example, based on the mass of the polymer system, the ratio of the mass content of the hydrophilic polymer to the mass content of the first solvent is in the range of 1:100 to 1:10, for example, 3:50.
[0242] For example, the first solvent may be the same as or similar to the solvent of the electrolyte, and the first solvent may include a carbonate-based solvent. For example, the carbonate-based solvent includes cyclic carbonate solvents and / or linear carbonate solvents.
[0243] Examples of cyclic carbonate solvents include one or more of the following: ethylene carbonate (EC), vinylidene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), vinylethylene carbonate (VEC), and dioctyl carbonate (CC).
[0244] Examples of linear carbonate solvents include one or more of the following: dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), diphenyl carbonate (DPC), methyl allyl carbonate (MAC), and polycarbonate (PC).
[0245] Selectively, the first solvent may also contain lithium salts and electrolyte additives, such as lithium lithium hexafluorophosphate, vinylidene carbonate VC, fluorovinylidene carbonate FEC, and the like.
[0246] In this application, m / n is also called the precipitation value and characterizes the ability to convert the gel-like substance into a hydrophilic polymer and solvent.
[0247] The first substance mainly comprises a gel-like substance formed from a hydrophilic polymer and a first solvent, and in this gel-like substance, the molecular structure of the polymer remains essentially unchanged.
[0248] In some embodiments, in order to remove the first solvent from the first substance, the first substance is dried at 80°C for 12 hours, and the main component of the dried first substance is the aforementioned hydrophilic polymer, as determined by infrared spectroscopy (IR detection) or nuclear magnetic resonance NMR testing.
[0249] The relevant parameters of the hydrophilic polymer in the embodiments of this application can be detected using the following method.
[0250] The groups of the hydrophilic polymer in the embodiments of this application can be detected using infrared spectroscopy (IR). Specifically, the hydrophilic polymer is tested using a Thermo Nicolet Nexus 670 attenuated total reflectance Fourier transform infrared spectrometer (FTIR-ATR), and then tested according to the GB / T6040-2002 standard, with a test range of 600-4000 cm⁻¹ by the ATR method. -1 , reproducibility ±2cm -1 , resolution 4cm -1 The transmission depth is 0.2 to 0.6 μm.
[0251] The structure of the hydrophilic polymer according to the embodiments of this application can be tested using nuclear magnetic resonance NMR. Specifically, 1H NMR and 13C NMR are performed using a Varian Mercury Plus-400 nuclear magnetic resonance spectrometer, with a test temperature of 20°C, TMS as the internal standard, CDCl3 as the solvent, and a proton resonance frequency of 400 MHz.
[0252] The polymer cell type of the hydrophilic polymer in the embodiment of this application (suitable for cells with a relatively small proportion of polymer) can be tested by decomposition-gas chromatography-mass spectrometry. The specific test steps are as follows: A 0.5 mg sample is accurately weighed and placed in a sample cup, fixed to an injection rod, and placed in a decomposition apparatus attached near the GC (gas chromatography) inlet. After the temperature of the decomposition apparatus reaches the set temperature, the injection button is pressed, and the sample cup is rapidly dropped into the center of the decomposition furnace by free fall. In an inert gas N2 atmosphere, the volatile components are instantly vaporized, carried to a gas chromatography column by a carrier gas, separated, and finally detected by a flame ionization detector (FID) or mass spectrometer (MS), thereby obtaining a gas chromatogram or total ion flow diagram.
[0253] The molecular weight of the hydrophilic polymer in the embodiments of this application has a meaning known in the art and can be measured using instruments and methods commonly used in the art, and can be tested using gel permeation chromatography (GPC). The specific test steps are as follows: weigh an appropriate amount of the sample to be measured (the sample concentration may be such that a light-shielding degree of 8% to 12% is ensured), add 20 ml of deionized water, and simultaneously irradiate with ultraviolet light for 5 minutes (53 kHz / 120 W) to confirm that the sample is completely dispersed, and then measure the sample according to the GB / T19077-2016 / ISO13320:2009 standard.
[0254] Alternatively, the test is performed using a multi-angle laser scattering instrument (MALLS). Specifically, a system combining a GPC and a Dawn Heleos II multi-angle laser scattering instrument, an Optilab T-rEX refractive index (RI) detector, and a Visco Star II viscometer (Wyatt Technology Corporation, USA) is used. The test is performed using tetrahydrofuran as the mobile phase at a flow rate of 1.0 ml / min and 30°C, and the SEC-SAMLL data is processed using the commercially available software ASTRA6 to obtain molecular weight parameters.
[0255] [Positive electrode piece]
[0256] The positive electrode piece includes a positive electrode current collector and a positive electrode active material layer, which is installed on the positive electrode current collector and contains a positive electrode active material and a hydrophilic polymer.
[0257] For example, a positive electrode current collector has two opposing surfaces in the thickness direction of itself, and the positive electrode active material layer is installed on one or both of the two opposing surfaces of the positive electrode current collector.
[0258] The positive electrode active material layer includes positive electrode active materials known in the art for use in battery cells. For example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphate compounds, lithium-containing transition metal oxides, sodium-containing phosphate compounds, and sodium-containing transition metal oxides.
[0259] For example, the general formula for olivine-type phosphate active materials (lithium-containing phosphate compounds) is Li x A y Me a M b P 1-c X c Y z Here, 0≦x≦1.3, 0≦y≦1.3, and 0.9≦x+y≦1.3, 0.9≦a≦1.5, 0≦b≦0.5, and 0.9≦a+b≦1.5, 0≦c≦0.5, and 3≦z≦5, where A includes one or more of Na, K, and Mg; Me includes one or more of Mn, Fe, Co, and Ni; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; and Y includes one or more of O and F. Specifically, the olivine-type phosphate active material includes one or more of the following: LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4.
[0260] Examples include lithium transition metal oxides (layered materials, e.g., ternary, lithium nickelate / sodium, lithium cobaltate / sodium, lithium manganate / sodium, lithium-rich layered and rock salt phase layered materials). The general formula for layered cathode active materials is Li x A y Ni a Co b Mn c M (1-a-b-c) Y zHere, 0≦x≦2.1, 0≦y≦2.1, and 0.9≦x+y≦2.1, 0≦a≦1, 0≦b≦1, 0≦c≦1, and 0.1≦a+b+c≦1, 1.8≦z≦3.5, A includes one or more of Na, K, and Mg, M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Fe, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce, and Y includes one or more of O and F. Selectively, y=0. Specifically, the layered positive electrode active material is lithium cobaltate LCO, lithium nickelate LNO, lithium manganeseate LMO, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) and LiNi 0.5 Co 0.2 Mn 0.3 It may contain one or more of O2 (NCM523) and NCA.
[0261] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. Examples of metal foils include aluminum foil or aluminum alloy foil. The composite current collector may include a polymer material substrate and a metal material layer formed on at least one surface of the polymer material substrate. For example, the metal material may be a combination of one or more selected from aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, and the polymer material substrate may be a combination of one or more selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0262] In some embodiments, the positive electrode active material layer also selectively includes a positive electrode conductive agent. The present application is not particularly limited to the type of positive electrode conductive agent, and for example, the positive electrode conductive agent may be a combination of one or more selected from superconducting carbon, conductive carbon black, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is 5% or less based on the total mass of the positive electrode active material layer.
[0263] In some embodiments, the positive electrode active material layer also selectively includes a positive electrode adhesive. The present application is not particularly limited to the type of positive electrode adhesive, and for example, the positive electrode adhesive may be a combination of one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene ternpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic ester resins. In some embodiments, the mass percentage of the positive electrode adhesive is 5% or less based on the total mass of the positive electrode active material layer. The crystallinity of the positive electrode adhesive is higher than that of the fluoropolymer of the present application. The melting temperature of the positive electrode adhesive is higher than that of the fluoropolymer of the present application.
[0264] The positive electrode active material layer is generally formed by coating a positive electrode slurry onto a positive electrode current collector, drying, and cold rolling. The positive electrode slurry is generally formed by dispersing a positive electrode active material, a hydrophilic polymer, a selectively conductive agent, a selectively adhesive, and any other components in a solvent and stirring uniformly. The solvent may, but is not limited to, N-methylpyrrolidone (NMP). Naturally, the production of the positive electrode piece is not limited to the above method, and the aforementioned production methods may be used.
[0265] [Negative electrode piece]
[0266] In some embodiments, the negative electrode piece includes a negative electrode current collector and a negative electrode active material layer comprising a negative electrode active material, which is provided on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode active material layer is provided on one or both of the two opposing surfaces of the negative electrode current collector.
[0267] The anode active material may be an anode active material known in the art used in battery cells. For example, the anode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, lithium metal, sodium metal, and lithium alloys. The silicon-based material may include at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy materials. The tin-based material may include at least one of elemental tin, tin oxide, and tin alloy materials.
[0268] In some embodiments, the negative electrode active material layer also selectively includes a negative electrode conductive agent. The present application is not particularly limited to the type of the negative electrode conductive agent, and for example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5% based on the total mass of the negative electrode active material layer.
[0269] In some embodiments, the negative electrode active material layer also selectively includes a negative electrode adhesive. The present application is not particularly limited to the type of negative electrode adhesive, and for example, the negative electrode adhesive may include at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, aqueous acrylic acid resin (e.g., polyacrylate PAA, polymethacrylate PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode adhesive is ≤5% based on the total mass of the negative electrode active material layer.
[0270] In some embodiments, the negative electrode active material layer also selectively includes other additives. For example, the other additives may include thickeners such as sodium carboxymethylcellulose (CMC) or PTC thermistor material. In some embodiments, the mass percentage of the other additives is ≤2% based on the total mass of the negative electrode active material layer.
[0271] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. Copper foil may be used as an example of a metal foil. The composite current collector may include a polymer material substrate and a metal material layer formed on at least one surface of the polymer material substrate. For example, the metal material may include at least one of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. For example, the polymer material substrate may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0272] The negative electrode active material layer is generally formed by applying a negative electrode slurry to a negative electrode current collector, drying, and cold rolling. The negative electrode slurry is generally formed by dispersing a negative electrode active material, a hydrophilic polymer, selectively a conductive agent, selectively an adhesive, and selectively other auxiliary agents in a solvent and stirring uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water. Naturally, the production of the negative electrode piece is not limited to the above method, and the aforementioned production methods may be used.
[0273] The negative electrode piece does not exclude any other additional functional layers other than the negative electrode active material layer. For example, in certain embodiments, the negative electrode piece described in this application further includes a conductive primer (e.g., consisting of a conductive agent and an adhesive) sandwiched between the negative electrode current collector and the negative electrode active material layer and placed on the surface of the negative electrode current collector. In some other embodiments, the negative electrode piece described in this application further includes a protective layer covering the surface of the negative electrode active material layer.
[0274] [Separator]
[0275] The separator includes a substrate and a coating applied to at least one surface of the substrate.
[0276] As some examples, the substrate is generally a porous structure having pores, and the hydrophilic polymer may be distributed in the pores of the substrate.
[0277] As some other examples, the hydrophilic polymer may be distributed within the coating.
[0278] As some further examples, the hydrophilic polymer may be placed on a surface of the coating that is separated from the substrate.
[0279] The specific distribution location of the hydrophilic polymer may be any one of the three types described above, any two of the three types, or a combination of the three types of locations described above.
[0280] The embodiments of this application are not particularly limited in terms of the material of the substrate, and any known substrate having good chemical and mechanical stability can be selected, such as glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The substrate may be a single-layer film or a multilayer composite film. If the substrate is a multilayer composite film, the materials of each layer may be the same or different. The substrate generally has a porous structure with pores, and the hydrophilic polymer may be distributed in the pores of the substrate.
[0281] In some embodiments, the coating may further contain a filler. Furthermore, the filler may contain at least one of inorganic particles and organic particles. The hydrophilic polymer may be distributed within the coating.
[0282] In some embodiments, the hydrophilic polymer may be placed on a surface of the coating that is separated from the substrate.
[0283] In some embodiments, the decomposition temperature of the filler may be 200°C or higher. In this way, the filler can have good thermal stability and be resistant to decomposition, and the heat resistance of the separator can be further improved.
[0284] Inorganic particles have the characteristics of high thermal stability and resistance to decomposition. Selectively, the inorganic particles include at least one of the following: inorganic particles having a dielectric constant of 5 or more, inorganic particles having ionic conductivity but not storing ions, and inorganic particles capable of electrochemical reactions.
[0285] Selectively, the inorganic particles having a dielectric constant of 5 or more include boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, aluminum magnesium silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate Pb(Zr,Ti)O3 (abbreviated as PZT), and Pb 1-m La m Zr 1-n Ti n O3 (abbreviated as PLZT, 0 <m<1、0<n<1)、Pb(Mg3Nb 2 / 3 The material comprises O3-PbTiO3 (abbreviated as PMN-PT) and at least one of the respective modified inorganic particles. Selectively, the modification method for each inorganic particle may be chemical modification and / or physical modification. The chemical modification method includes coupling agent modification (e.g., use of silane coupling agents, titanate ester coupling agents, etc.), surfactant modification, polymer graft modification, etc. The physical modification method may include mechanical force dispersion, ultrasonic dispersion, high-energy treatment, etc. The modification treatment can reduce the aggregation of inorganic particles, thereby forming a more stable and uniform spatial network structure with nanocellulose. Furthermore, by selecting coupling agents, surfactants, or polymer-modified inorganic particles having specific functional groups, it is possible to improve the immersion properties of the coating in the electrolyte and improve the adhesive strength between the coating and the substrate.
[0286] Selectively, the inorganic particles that have the aforementioned ion conductivity but do not store ions are Li3PO4, lithium titanium phosphate Li x1 Ti y1 (PO4)3, Lithium Aluminum Titanium Phosphate x2 Al y2 Ti z1 (PO4)3(LiAlTiP) x3O y3 type glass, lithium lanthanum titanate Li x4 La y4 TiO3, lithium germanium thiophosphate Li x5 Ge y5 P z2 S w , lithium nitride Li x6 N y6 , SiS2 type glass Li x7 Si y7 S z3 and P2S5 type glass Li x8 P y8 S z4 includes at least one of them, where 0<x1<2, 0<y1<3, 0<x2<2, 0<y2<1, 0<z1<3, 0<x3<4, 0<y3<13, 0<x4<2, 0<y4<3, 0<x5<4, 0<y5<1, 0<z2<1, 0<w<5, 0<x6<4, 0<y6<2, 0<x7<3, 0<y7<2, 0<z3<4, 0<x8<3, 0<y8<3, 0<z4<7. In this way, the ion transmission characteristics of the separator can be further improved.
[0287] Organic particles have the properties of high thermal stability and being difficult to decompose, so they can improve the heat resistance of the separator. At the same time, when the internal temperature of the battery cell reaches the melting point of the organic particles due to overcharge abuse, thermal abuse or the like, the organic particles melt, are sucked into the micropores of the substrate by capillary action, close the pores and function to cut off the circuit, which helps to ensure high safety performance of the battery cell.
[0288] In some embodiments, the organic particles include, but are not limited to, at least one of polyethylene particles, polypropylene particles, polystyrene particles, melamine resin particles, phenolic resin particles, polyester particles (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), polyimide particles, polyamide-imide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, polyaryletherketone particles, and copolymers of butyl acrylate and ethyl methacrylate (e.g., crosslinked polymers of butyl acrylate and ethyl methacrylate).
[0289] In some embodiments, the coating further comprises an adhesive. The present application is not particularly limited to the type of adhesive, and any known material having good tackiness can be selected. For example, the adhesive comprises at least one of aqueous acrylic resins (e.g., acrylic acid, methacrylic acid, homopolymers of sodium acrylate monomers, or copolymers with other comonomers), polyvinyl alcohol, isobutylene-maleic anhydride copolymer, and polyacrylamide.
[0290] Selectively, the content of the adhesive in the coating is less than 30% based on the mass of the coating.
[0291] [Electrolyte]
[0292] In the charging and discharging process of a battery cell, active ions repeatedly insert into and remove from the positive and negative electrode pieces, and the electrolyte plays a role in conducting these active ions between the positive and negative electrode pieces. This invention is not particularly limited to the type of electrolyte and can be selected according to actual requirements.
[0293] The electrolyte solution comprises an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not specifically limited and can be selected according to actual requirements.
[0294] If the battery cell according to this application is a lithium-ion battery, the electrolyte salt may, for example, include at least one of the following: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonimide (LiFSI), lithium bistrifluoromethanesulfonimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).
[0295] If the battery cell according to this application is a sodium-ion battery, the electrolyte salt may, for example, include at least one of the following: lithium sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bisfluorosulfonimide (NaFSI), sodium bistrifluoromethanesulfonimide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalate borate (NaDFOB), sodium dioxalate borate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorodioxalate phosphate (NaDFOP), and sodium tetrafluorooxalate phosphate (NaTFOP), but is not limited to these.
[0296] For example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).
[0297] In some embodiments, the electrolyte also selectively includes additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and further, additives that can improve specific performance of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high-temperature performance of the battery, and additives that improve the low-temperature power performance of the battery.
[0298] In some embodiments, the positive electrode piece, the separator, and the negative electrode piece can be manufactured into an electrode assembly by a winding process and / or a lamination process.
[0299] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to enclose the electrode assembly and the electrolyte.
[0300] In some embodiments, the outer packaging of the battery cell may be a rigid casing, such as a rigid plastic casing, an aluminum casing, or a steel casing. The outer packaging of the battery cell may also be a soft pack, such as a bag-type soft pack. The material of the soft pack may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0301] In some embodiments, the positive electrode piece, separator, and negative electrode piece can be manufactured into an electrode assembly by a winding process or a lamination process.
[0302] The present invention is not particularly limited to the shape of the battery cell, and it may be cylindrical, prismatic, or any other shape. Figure 1 shows an example of a prismatic battery cell 5.
[0303] In some embodiments, as shown in Figures 1 and 2, the outer packaging may include a casing 51 and a cover plate 53. Here, the casing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates surrounding each other to form a housing cavity. The casing 51 has an opening that communicates with the housing cavity, and the cover plate 53 is used to cover the opening and seal the housing cavity. The positive electrode piece, negative electrode piece and separator can be formed into an electrode assembly 52 by a winding process or a lamination process. The electrode assembly 52 is sealed in the housing cavity. The electrolyte is immersed in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 may be one or more and can be adjusted as needed.
[0304] The method for manufacturing the battery cell according to the present invention is known. In some embodiments, a battery cell can be formed by assembling a positive electrode, a separator, a negative electrode, and an electrolyte. For example, the positive electrode, separator, and negative electrode can be formed into an electrode assembly by a winding or lamination process, the electrode assembly can be placed in an outer package, the electrolyte can be injected after drying, and a battery cell can be obtained by processes such as vacuum sealing, standing, chemical conversion, and shaping.
[0305] In some embodiments of the present invention, a battery module can be assembled using the battery cell according to the present invention, and the number of battery cells included in the battery module may be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.
[0306] Figure 3 is a schematic diagram of an example battery module 4. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged according to any other method. Furthermore, the multiple battery cells 5 can be fixed in place by fastening members.
[0307] Selectively, the battery module 4 may further include an outer casing having a housing space, in which a plurality of battery cells 5 are housed.
[0308] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.
[0309] Both the battery module 4 and the battery pack can be specific examples of the battery of this application.
[0310] Figures 4 and 5 are schematic diagrams of an example battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a battery case and a plurality of battery modules 4 installed inside the battery case. The battery case includes an upper case 2 and a lower case 3, the upper case 2 being used to cover the lower case 3 and to form a sealed space for housing the battery modules 4. The plurality of battery modules 4 can be arranged inside the battery case in any manner.
[0311] Electrical equipment
[0312] In a second embodiment, the present application provides an electrical device comprising at least one of the battery cells, battery modules, and battery packs relating to the present application. The battery cells, battery modules, and battery packs may be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may be, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. In some embodiments, the battery cell includes a liquid injection port for injecting electrolyte, and when the battery cell is applied to an electrical device, the liquid injection port is located at the bottom along the vertical direction of the battery cell. Even when the amount of free electrolyte in the battery cell is very small, or even nonexistent, and the liquid injection port is located at the bottom along the vertical direction of the battery cell, the reliability of the battery cell can be improved, and thereby the reliability of the electrical device can be improved.
[0313] An electrical device can be equipped with a battery cell, battery module, or battery pack, depending on its usage needs. Figure 6 is a schematic diagram of an example electrical device. This electrical device 6 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density needs of this electrical device, a battery pack 1 or a battery module can be used. Another example of an electrical device may be a mobile phone, a tablet PC, or a laptop computer. These electrical devices generally require thinness and lightness, and can use battery cells as a power source.
[0314] Examples
[0315] Examples of the present application are described below. The examples described below are illustrative and are for interpretive purposes only and should not be considered as limitations thereon. Unless otherwise specified in the examples, the techniques or conditions described are to be followed in accordance with the techniques or conditions described in the literature in the art or in accordance with product specifications. Unless otherwise specified, the reagents or equipment used are all common commercially available products.
[0316] Example 1: Manufacturing of a lithium-ion battery
[0317] (1) Manufacturing of positive electrode pieces:
[0318] A 12μm thick aluminum foil was used as the positive electrode current collector.
[0319] LiNi, a hydrophilic polymer and cathode active material. 0.8 Co 0.1 Mn 0.1O2 (NCM811), the conductive agent carbon black, and the adhesive polyvinylidene fluoride (PVDF) were added to N-methylpyrrolidone (NMP) and mixed to produce a positive electrode slurry. The mass ratio of the hydrophilic polymer, NCM811, conductive carbon black, PVDF, and N-methylpyrrolidone (NMP) in the positive electrode slurry was 0.5:96.8:2.2:0.5. The positive electrode slurry was applied to aluminum foil current collectors, dried at 85°C, cold-rolled, then trimmed, cut, and slit, and finally dried under vacuum conditions at 85°C for 4 hours to produce positive electrode pieces.
[0320] (2) Manufacturing of the negative electrode piece:
[0321] A copper foil with a thickness of 8 μm was manufactured as the negative electrode current collector.
[0322] A hydrophilic polymer, artificial graphite (anode active material), carbon black (conductive agent), styrene-butadiene rubber (SBR) (adhesive), and sodium carboxymethylcellulose (CMC) (thickener) were added to deionized water in a weight ratio of 2.5:94.9:2:0.5:0.1 and mixed uniformly to produce anode slurry. The anode slurry was applied to copper foil current collectors, dried at 85°C, then cold-rolled, trimmed, cut, and slit, followed by drying at 120°C under vacuum conditions for 12 hours to produce anode pieces.
[0323] (3) Manufacturing of electrolyte:
[0324] In an environment with a water content of less than 10 ppm, ethylene carbonate (EC) and ethyl methyl carbonate (EMC), which are non-aqueous organic solvents, were mixed in a volume ratio of 3:7 to obtain an electrolyte solvent. Then, the lithium salt LiPF6 was mixed with the resulting solvent to prepare an electrolyte with a lithium salt concentration of 1 mol / L.
[0325] (4) Manufacturing of lithium-ion batteries:
[0326] A 16 μm polyethylene film (PE) was used as the substrate for the separator, and a polymer coating was applied to the surface of the substrate. The mass content of the polymer coating was 85%:15% for conventional vinylidene fluoride (PVDF) and styrene-butadiene rubber (SBR), which is used as an adhesive.
[0327] The positive electrode piece, separator, and negative electrode piece are stacked in order, with the separator interposed between the positive and negative electrode pieces to provide separation. Next, the assembly is wound up to obtain an electrode assembly. The electrode assembly is placed in an outer package, dried, and then an electrolyte is injected. A lithium-ion battery is obtained through processes such as vacuum sealing, standing, chemical formation, and shaping.
[0328] Comparative Example 1
[0329] A lithium-ion battery was manufactured using a method similar to that of Example 1, the only difference from Example 1 being that a hydrophilic polymer was not added to the positive electrode slurry of Comparative Example 1, nor was a hydrophilic polymer added to the negative electrode slurry.
[0330] Examples 2-1 to 2-6
[0331] A lithium-ion battery was manufactured using a method similar to that of Example 1, the difference being that in Examples 2-1 to 2-6, at least one of the following was adjusted: the total pore volume of the positive electrode piece, the total pore volume of the negative electrode piece, the amount of hydrophilic polymer added to the positive electrode slurry, and the amount of hydrophilic polymer added to the negative electrode slurry.
[0332] Examples 3-1 to 3-4
[0333] A lithium-ion battery was manufactured using a method similar to that of Example 1, the only difference being that Examples 3-1 to 3-4 involved adjusting the type of hydrophilic polymer.
[0334] Examples 4-1 to 4-3
[0335] A lithium-ion battery was manufactured using a method similar to that of Example 1. The difference from Example 1 is that Examples 4-1 to 4-3 adjust the setting position of the hydrophilic polymer, in which Example 4-3 had a mass content of 80% polycarbosilane PCS, a mass content of 10% hydrophilic polymer, and a mass content of 10% adhesive.
[0336] The data for the examples and comparative examples are shown in Table 1.
[0337] Test section
[0338] 1. Lithium-ion battery cycle performance test
[0339] The lithium-ion batteries manufactured in the examples and comparative examples were charged at a rate of 1C at 25±2℃ and discharged at a rate of 1C. A full charge-discharge cycle test was performed until the capacity of the secondary battery decreased to 80% of its initial capacity, at which point the test was stopped and the number of cycles was recorded.
[0340] 2. Liquid leakage insulation test of lithium-ion battery modules
[0341] The lithium-ion batteries manufactured in the examples and comparative examples were charged to 100% SOC at 25±2℃ with 0.5C (i.e., a current at 0.5 times the capacity rate) and left to stand for 1 hour. To simulate a battery core liquid leakage scenario, a small hole with a diameter of 2 mm was drilled in the bottom of the battery core. Twelve battery cores were connected in series, with one end of the module connected to the module's negative electrode and the other end half-overlapping / overlapping with the end plate. An external voltage of 200V was connected and observed for 1 hour (the short circuit was disconnected if a fire occurred) to check for the presence or absence of a fire due to insulation failure and the time of the fire.
[0342] [Table 1] [Table 2] [Table 3]
[0343] In Table 1, VDF represents vinylidene fluoride, HFP represents hexafluoropropylene, and TFE represents tetrafluoroethylene. 80%VDF+15%HFP+5%TFE indicates that the total mass of all monomers is 80% VDF, 15% HFP, and 5% TFE.
[0344] The nominal capacity x of the batteries in the comparative example and the example is 151 Ah.
[0345] [Table 4]
[0346] As can be seen from Tables 1 and 2, in Comparative Example 1, no hydrophilic polymer was added to the positive and negative electrode pieces. During the lithium-ion battery cycle process, the volume of the lithium-ion battery changes, which can cause the electrolyte in the electrode assembly to be pushed out, potentially leading to a liquid shortage problem. This increases the risk of lithium dendrite formation and reduces the reliability and cycle performance of the lithium-ion battery.
[0347] The embodiments of this invention can improve the reliability and cycle performance of lithium-ion batteries by adding a hydrophilic polymer, which can form an aggregated electrolyte with the electrolyte to improve liquid retention capacity, to at least one of the positive electrode piece, negative electrode piece, and separator.
[0348] While the present application has been described with reference to preferred embodiments, various improvements can be made thereto without departing from the scope of the application, and components therein can be replaced with equivalents. In particular, each technical feature mentioned in each embodiment can be combined in any manner, provided that there is no structural inconsistency. The present application is not limited to the specific embodiments disclosed herein, but includes all technical concepts included in the claims.
Claims
1. A battery cell comprising an electrode assembly including a first electrode piece, a second electrode piece, and a separator, and an electrolyte, wherein the polarities of the first electrode piece and the second electrode piece are opposite, the separator is placed between the first electrode piece and the second electrode piece, and at least one of the first electrode piece, the second electrode piece, and the separator comprises a hydrophilic polymer. The aforementioned hydrophilic polymer includes one or more types of fluoropolymers, ether polymers, ester polymers, and aldehyde ketone polymers. The degree of crystallinity Xc1 of the fluoropolymer, as measured by differential scanning calorimetry, is 0 < Xc1 ≤ 30%, and the melting temperature Tm1 of the fluoropolymer, in °C, is 0 < Tm1 ≤ 140. The ether-based polymer is manufactured into a sheet-like structure, and the sheet-like structure manufactured from the ether-based polymer is subjected to a dynamic frequency scanning test at (T m2 + 20)°C to obtain an elastic modulus G' - energy consumption coefficient G'' curve, where the slope K1 of the elastic modulus G' - energy consumption coefficient G'' curve is 1 < K1 < ∞, and T m2 represents the melting temperature of the ether-based polymer in °C. The ester-based polymer is manufactured into a sheet-like structure, and the sheet-like structure manufactured from the ester-based polymer is subjected to a dynamic frequency scanning test at (T m3 + 20)°C to obtain an elastic modulus G' - energy consumption coefficient G'' curve, where the slope K2 of the elastic modulus G' - energy consumption coefficient G'' curve is 1 < K2 < ∞, and T m3 represents the melting temperature of the ester-based polymer in °C. The aldehyde ketone polymer is manufactured into a sheet-like structure, and the sheet-like structure manufactured from the aldehyde ketone polymer is subjected to a dynamic frequency scanning test at (T m4 + 20) °C to obtain an elastic modulus G' - energy consumption coefficient G'' curve, where the slope K3 of the elastic modulus G' - energy consumption coefficient G'' curve is 0.8 ≤ K3 < ∞, and T m4 represents the melting temperature of the aldehyde ketone polymer in °C. The aforementioned battery cell satisfies the following equation: [Math 1] p1 represents the porosity of the first pole piece, v1 represents the total volume of the first pole piece in units of mL. p2 represents the porosity of the second pole piece, v2 represents the total volume of the second electrode piece in units of mL. p3 represents the porosity of the separator, v3 represents the total volume of the separator in units of mL. y represents the mass of the free electrolyte in the battery cell, expressed in units of g. Battery cell. 【Request Item 2】 【Number 2】 The battery cell according to claim 1.
3. The aforementioned battery cell also satisfies the following equation: [Math 3] I understand 1 This represents the mass of the electrode assembly before drying, expressed in units of g. I understand 2 This represents the dried mass of the electrode assembly in units of g. The battery cell according to claim 1.
4. The amount of free electrolyte per unit volume of the aforementioned battery cell is b, its unit is mg / Ah, and 0 ≤ b ≤ 1400. The battery cell according to claim 1.
5. The first pole piece includes a current collector and an active material layer provided on at least one surface of the current collector, wherein the active material layer includes the hydrophilic polymer and active material particles. The hydrophilic polymer is distributed on the surface of the active material particles, and / or The active material particles are plurality, and there are pores between adjacent active material particles, and the hydrophilic polymer is distributed in the pores between the active material particles. The battery cell according to claim 1.
6. The separator includes a substrate and a coating applied to at least one surface of the substrate. The hydrophilic polymer is distributed in the pores of the substrate, and / or The hydrophilic polymer is distributed within the coating and / or The hydrophilic polymer is placed on the surface of the coating that is separated from the substrate. The battery cell according to claim 1.
7. The aforementioned hydrophilic polymer includes a fluoropolymer. The battery cell according to claim 1.
8. The glass transition temperature T g1 of the aforementioned fluoropolymer is in °C, and -150 ≤ T g1 ≤ 60 The battery cell according to claim 7.
9. The fluoropolymer comprises at least one of the structural units represented by formula (AI) to formula (AIII), 【Chemistry 1】 In formula (AI) and formula (AII), R 11 , R 12 , R 13 and R 14 each independently include a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and R 11 , R 12 , R 13 and R 14 at least one of which comprises a fluorine atom, and when substituted, the substituent comprises one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxy group, an ester group, and a halogen atom, 【Chemistry 2】 In equation (AIII), R 15 It contains a single bond, a substituted or unsubstituted C1-C3 alkyl group, and if substituted, the substituent includes one or more of the following: a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide, a carboxyl group, an ester group, or a halogen atom, and p is a positive integer selected from 1 to 3, and n is a positive integer selected from 1000 to 30000. The battery cell according to claim 7.
10. The aforementioned hydrophilic polymer includes an ether-based polymer. The battery cell according to claim 1.
11. The ether-based polymer comprises the structural unit shown in formula (BI) and / or the structural unit shown in formula (BII), 【Transformation 3】 In equation (BI), R 21 and R 22 Each independently comprises a hydrogen atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, R 23 It contains substituted or unsubstituted C1-C5 alkylene groups, 【Chemistry 4】 In equation (BII), R 24 ~R 27 Each independently comprises a hydrogen atom, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 alkoxy group, or an ether group, and R 24 ~R 27 At least one of them includes a substituted or unsubstituted C1-C3 alkoxy group or ether group. The battery cell according to claim 10.
12. The aforementioned hydrophilic polymer includes an ester-based polymer. The battery cell according to claim 1.
13. The ester polymer comprises a structural unit represented by formula (CI) and / or a structural unit represented by formula (CII), 【Transformation 5】 In formula (CI), R 31 , R 32 and R 33 Each independently contains a hydrogen atom or a substituted or unsubstituted C1-C8 alkyl group, R 34 This includes a substituted or unsubstituted C1-C8 alkyl group, or a substituted or unsubstituted C1-C8 hydroxyalkyl group. 【Transformation 6】 In equation (CII), R 35 This includes substituted or unsubstituted C2-C6 methylene groups. The battery cell according to claim 12.
14. The aforementioned hydrophilic polymer includes an aldehyde ketone polymer. The battery cell according to claim 1.
15. The aldehyde ketone polymer comprises a structural unit represented by formula (DI) and / or a structural unit represented by formula (DII), 【Transformation 7】 In equation (DI), R 41 It contains single bonds, substituted or unsubstituted C1-C6 methylene groups, R 42 It contains a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group, 【Transformation 8】 In equation (DII), R 43 ~R 46 Each independently comprises a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 hydroxyalkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and r and s are each independently selected integers from 0 to 5, and at least one of r and s is selected from positive integers. The battery cell according to claim 14.
16. The molecular weight of the aforementioned hydrophilic polymer is 1.2 × 10⁻⁶. 5 g / mol ~ 1 × 10 6 It is g / mol. The battery cell according to claim 1.
17. A battery cell according to any one of claims 1 to 16, battery.
18. A battery including the one described in claim 17, Electrical device.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2008071731A
Nonaqueous electrolyte secondary battery
JP2010113804A
Lithium ion secondary battery
JP2013084454A