Nanomembrane, electronic device containing the same, and method for manufacturing the nanomembrane.

A polyimide fiber nanomembrane with anisotropic properties addresses the issues of durability and dust collection efficiency, ensuring high efficiency and reduced membrane fractures while maintaining sound transmission.

JP7954827B2Active Publication Date: 2026-11-20KOLON INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2025538548
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-12-15
Filing Date
2023-12-21
Publication Date
2026-11-20
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

Existing nanomembranes used in electronic devices suffer from insufficient dust collection efficiency and durability, leading to membrane tearing and a decline in air permeability or sound transmission, despite attempts to enhance durability with reinforcing materials.

Method used

A nanomembrane composed of polyimide fibers with specific anisotropy, porosity, and air permeability, produced through electrospinning and uniaxial orientation, achieving high dust collection efficiency and durability without compromising air permeability or sound transmission.

Benefits of technology

The nanomembrane exhibits a dust collection efficiency of 95% or more, with improved tensile strength in the machine direction, reducing membrane fractures during manufacturing and maintaining sound transmission loss below 5 dB/pa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954827000003
    Figure 0007954827000003
  • Figure 0007954827000004
    Figure 0007954827000004
  • Figure 0007954827000005
    Figure 0007954827000005
Patent Text Reader

Abstract

The present invention provides a nanomembrane formed of polyimide fibers having an average diameter of 0.1 to 15 μm and a porosity of 50 to 90%, wherein the nanomembrane has an anisotropy between the strength in the machine direction (MD) and the strength in the transverse direction (TD) (MD strength / TD strength) of 2 to 11, a ratio of the number of fiber strands in the machine direction to the number of fiber strands in the transverse direction (MD fiber strands / TD fiber strands) of 1.5 to 10, and an air permeability of the nanomembrane of 50 to 200 cm 3 / cm 2 The nanomembrane has a dust collection efficiency of 95% or more as measured by the following method, a nanomembrane assembly and an electronic device including the same, and a method for manufacturing the nanomembrane. [Measurement method] Dust size: 1 μm; Air flow rate: 32 L / min; Measurement area: 100 cm 2 Measure according to AFT8130.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a nanomembrane with excellent dust collection efficiency and durability, an electronic device containing the same, and a method for manufacturing the nanomembrane. [Background technology]

[0002] Recently, electronic devices include, for example, communication devices such as smartphones. They are becoming smaller, more integrated, and more power-efficient.

[0003] Communication devices such as smartphones incorporate microelectronic systems (MEMS), and within these MEMS are various electronic components. Therefore, a wide range of research has been continuously conducted on encapsulation materials to prevent these electronic components from being contaminated by external pollutants.

[0004] However, the sealing materials that have been successfully commercialized to date still suffer from insufficient dust collection efficiency and durability, resulting in damage such as membrane tearing due to tension during the nanomembrane manufacturing process, and a decline in quality.

[0005] To address these problems, attempts have been made to add small amounts of reinforcing materials, such as inorganic particles, to the membrane or to increase the density of the pores. However, these attempts have limitations, as they result in loss of air permeability or sound transmission.

[0006] As a result, there is still a demand for nanomembranes with improved durability without a decrease in air permeability or sound transmission loss. [Overview of the project] [Problems that the invention aims to solve]

[0007] The present invention provides a nanomembrane with excellent dust collection efficiency and durability, an electronic device containing the same, and a method for manufacturing the nanomembrane. [Means for solving the problem]

[0008] A nanomembrane formed of polyimide fibers on one side, having a porosity of 50 to 90%, wherein the anisotropy between the machine direction (MD) strength and the transverse direction (TD) strength (MD strength / TD strength) is 2 to 11, the ratio of the number of fibrous strands in the machine direction to the number of fibrous strands in the transverse direction (number of MD fibrous strands / number of TD fibrous strands) is 1.5 to 10, and the air permeability of the nanomembrane is 50 to 200 cm². 3 The nanomembrane is provided with a dust collection efficiency of 95% or more, as measured by the following method.

[0009] [Measurement method] Dust size: 1 μm; Air flux: 32 l / min; Measurement area: 100 cm² 2 Measured using AFT8130.

[0010] According to one example, the sound transmission loss of the nanomembrane can be less than 5 dB / pa based on a 94 dB standard.

[0011] According to one example, the polyimide fiber may include polyimide, polyamideimide, polyetherimide, or a combination thereof.

[0012] According to one example, the thermal shrinkage rate of the nanomembrane at 300°C may be 1% or less.

[0013] According to one example, the weight loss rate of the nanomembrane at 300°C may be 1% by weight or less.

[0014] In other aspects, a nanomembrane assembly is provided, comprising a substrate; the nanomembrane; and an adhesive layer interposed between the substrate and the nanomembrane.

[0015] According to another aspect, an electronic device comprising the aforementioned nanomembrane is provided.

[0016] Further, according to another aspect, there is provided a method for producing a nanomembrane, comprising: an electrospinning step of electrospinning a polyamic acid solution to produce a precursor, wherein the ratio of the winding speed in the machine direction (MD) to the reciprocating speed in the traverse direction (TD) (MD winding speed / TD reciprocating speed) in the electrospinning step is adjusted to produce an anisotropic precursor; a processing step of adjusting the density and thickness of the precursor; a converting step of determining the form of the precursor; and a step of applying tension to the converted precursor in the MD direction to imidize it into a uniaxially oriented form to obtain a nanomembrane, wherein air is blown in the direction in which the precursor is discharged, the value of the MD winding speed / TD reciprocating speed is 2 to 10, and the nanomembrane has a dust collection efficiency of 95% or more as measured by the measurement method described below.

[0017] [Measurement Method] Dust size: 1 μm; Air flow rate: 32 L / min; Measurement area: 100 cm 2 Measurement is performed using AFT8130

[0018] According to one embodiment, the step of imidizing into the uniaxially oriented form can be carried out by applying a tension of 20 N to 100 N in the machine direction to the converted precursor. [Advantageous Effects of the Invention]

[0019] In the case of unilateral nanomembranes, a polyamic acid solution is electrospun at a specific temperature, for example, 70°C. An anisotropic precursor is obtained by adjusting the ratio of the winding speed in the machine direction (MD) to the reciprocating speed in the traverse direction (TD) (MD winding speed / TD reciprocating speed). After processing and converting such a precursor, tension is applied in the MD direction to imidize it into a uniaxial orientation. This results in a ratio of the number of fibers in the machine direction to the number of fibers in the traverse direction to 1.5 to 10. The resulting unique porosity structure improves the tensile strength in the MD direction, suppresses breakage during the roll-to-roll process, and improves processability. [Brief explanation of the drawing]

[0020] [Figure 1] This is a schematic diagram of a nanomembrane assembly according to one embodiment of the present invention. [Figure 2] This is a photograph taken from above of a nanomembrane assembly manufactured according to one embodiment of the present invention. [Figure 3] These are photographs showing the results of fiber arrangement experiments on the nanomembranes produced in Example 1 and Comparative Example 2. [Modes for carrying out the invention]

[0021] In the following, "top" or "above" can include not only things that are directly above and in contact with the object, but also things that are above but not in contact with the object. Singular expressions include multiple expressions unless the context clearly indicates otherwise. Furthermore, when a part "contains" a component, this means, unless otherwise stated, that it may contain other components rather than excluding them.

[0022] The use of the term "above" and similar referential terms may be singular or plural. Unless there is a clear indication of the order of the steps constituting the method, these steps may be performed in any order, and are not necessarily limited to the order in which they are stated.

[0023] As used herein, the terms “comprise,” “comprising,” “formed,” “has,” “having,” or any other variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, product, or apparatus that includes a list of elements is not necessarily limited to such elements alone, but may also include other elements that are not explicitly listed or that are inherent in such process, method, product, or apparatus. Furthermore, unless clearly stated otherwise, “or” means inclusive or not exclusive.

[0024] All use of example or illustrative terms is solely for the purpose of detailing the technical idea and is not limited by such example or illustrative terms unless otherwise specified by the claims.

[0025] Figure 1 is a schematic diagram of a nanomembrane assembly (10) containing a nanomembrane (100), and Figure 2 is a photograph of a group of such nanomembrane assemblies (10) taken from above.

[0026] Referring to Figure 1, the nanomembrane assembly (10) includes a nanomembrane (100), an adhesive layer (110) arranged on one surface of the nanomembrane along the frame of the nanomembrane, and a substrate (120) arranged on the adhesive layer.

[0027] The nanomembrane assembly (10) can be manufactured by arranging an adhesive film, in which an adhesive layer (110) is placed on a substrate (120), on one surface along the periphery of the nanomembrane (100).

[0028] The portion of the nanomembrane assembly (10) where the adhesive film is not placed constitutes a dustproof section (B). The dustproof section (B) allows air to pass through but substantially prevents dust particles of a few micrometers from passing through, and also has oil-repellent properties that substantially prevent moisture from passing through. Therefore, when such a nanomembrane assembly is applied to a microelectronic system (MEMS), it is possible to prevent the performance of the MEMS from degrading due to the influx of foreign substances such as saliva and dust.

[0029] The adhesive layer (110) can be made of a known adhesive capable of firmly maintaining adhesion between the nanomembrane (100) and the MEMS subsequently applied. Examples of such adhesives include epoxy adhesives, urethane adhesives, acrylic adhesives, thermosetting adhesives, and petroleum resin adhesives.

[0030] For example, the adhesive layer (110) may include a thermosetting adhesive.

[0031] The substrate (120) may be a release film. The release film acts as a carrier for placing the adhesive film on the nanomembrane (100) and prevents contamination of the adhesive layer until the nanomembrane assembly (10) is applied to an acoustic element such as a MEMS.

[0032] The substrate (120) can be selected from known films that are easily peeled off from the adhesive layer (110).

[0033] The nanomembrane (100) may be a nanomembrane formed of polyimide fibers having an average diameter of 0.1 to 15 μm.

[0034] The polyimide fiber refers to a polymer containing imide bonds in its main chain, and may include polyimide, polyamideimide, polyetherimide, or a combination thereof.

[0035] According to one example, the polyimide fiber can be produced by electrospinning a solution containing a polyimide precursor to produce a precursor, then processing and converting the precursor, and finally heating it to imide it.

[0036] Polyamic acid can be used as the polyimide precursor.

[0037] The aforementioned cingipolyamic acid solution can be prepared by dissolving a diamine monomer and a dianehydride monomer in a solvent.

[0038] The diamine monomer may be one or more selected from the group consisting of 4,4'-oxydianiline (ODA), 1,3-bis(4-aminophenoxy)benzene (RODA), p-phenylene diamine (p-PDA), and o-phenylene diamine (o-PDA). Preferably, it may be 4,4'-oxydianiline (ODA), p-phenylene diamine (p-PDA), o-phenylene diamine (o-PDA), or a mixture thereof.

[0039] The dianehydride monomer may be one or more selected from the group consisting of pyromellyrtic dianhydride (PMDA), 3,3',4,4'-benzophenonetracarboxylic dianhydride (BTDA), 4,4'-oxydiphthalicanhydride (ODPA), 3,4,3',4'-biphenyltetracarboxylic dianhydride (BPDA), and bis(3,4-dicarboxyphenyl)dimethylsilane dianhydride (SiDA).

[0040] The solvent may be one or more selected from the group consisting of m-cresol, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), acetone, diethyl acetate, tetrahydrofuran (THF), chloroform, and γ-butyrolactone.

[0041] The solid content of the polyamic acid solution may be 5 to 30% by weight, and the solution viscosity may be 100 to 500 poise. For example, the solid content of the polyamic acid solution may be 10 to 20% by weight, and the solution viscosity may be 200 to 300 poise. The solution viscosity can be measured at a temperature of 23°C using the KSMISO2555 method. The solid content and solution viscosity may affect the quality and thickness of the resulting fibers, but if the solid content and solution viscosity are satisfied, polyimide fibers of 0.1 to 15 μm can be obtained.

[0042] The aforementioned electrospinning step is a step in which a polyamic acid solution is electrospinned to produce a precursor. In order to disperse the precursor during the electrospinning step, air can be blown in the direction from which the precursor is discharged. The direction of the air can be adjusted at various angles relative to the direction from which the precursor is discharged in order to disperse the precursor.

[0043] During electrospinning, a polyamic acid solution is spun from the nozzle to produce a precursor, and the precursor is dispersed by the electrostatic force generated between the spun precursors. At this time, air can be blown towards the precursor at a predetermined angle to disperse the precursor over a wider area. Due to the air pressure, the precursor is dispersed and accumulates over a wider area. In this process, the solvent contained in the precursor is removed.

[0044] In this invention, by blowing air toward the precursor, the precursor can be dispersed over a wider area, and the resulting nanomembrane (100) has large diameter pores and high air permeability.

[0045] Furthermore, high-temperature air can be injected horizontally to sufficiently remove the solvent during the electrospinning stage, and by adjusting the temperature and amount of this horizontally injected air and the air used to disperse the precursor, the pore size, porosity, and physical properties of the nanomembrane (100) can be finely controlled.

[0046] Furthermore, in the electrospinning step described above, when the spinning solution is discharged through a nozzle, an anisotropic precursor can be produced by adjusting the ratio of the machine direction (MD) winding speed to the traverse direction (TD) reciprocating speed (MD winding speed / TD reciprocating speed). By producing an anisotropic precursor, an improvement in mechanical strength in a specific direction can be expected.

[0047] For example, the value of MD winding speed / TD reciprocating speed can be 2 to 10 days, 3 to 9, 4 to 8, or 5 to 7 days, but any range that falls within the aforementioned range may be included.

[0048] The discharge rate in the electrospinning stage may be 0.5 to 8 ml / min, for example, 1 to 7 ml / min, 2 to 6 ml / min, or 3 to 5 ml / min. By adjusting the discharge rate in the electrospinning stage to within the above range, a sufficient amount of fibers can be discharged and accumulated from the collector, allowing the solvent to evaporate and build up to form a membrane, which in turn can increase the dust collection efficiency.

[0049] A certain electric field may be applied between the nozzle and the collector to produce a nanomembrane having nanofibers of a certain thickness. The strength of the electric field can be between 3 and 80 kV. When the strength of the electric field is within this range, a constant amount of spinning solution can be continuously discharged, enabling the production of a nanofiber web of uniform thickness. On the other hand, if the strength of the electric field is too low, for example less than 3 kV, the spinning solution may not be discharged smoothly, causing nozzle clogging. If the strength of the electric field is too high, for example exceeding 80 kV, the scattered fiber solvent may not be completely removed before reaching the collector, making it difficult to obtain nano-sized fibers.

[0050] The precursor, which consists of nanofibers, can be formed by arranging the fibers in a specific direction in a collector, or by bonding randomly arranged fibers. For example, the precursor can have a structure formed by bonding in the form of a nonwoven fabric.

[0051] After the polyamic acid solution is electrospun to form a precursor, a processing step follows to adjust the density and thickness of the precursor.

[0052] The aforementioned processing step involves adjusting the density and thickness of the precursor accumulated during the electrospinning stage, and can be performed through a two-stage continuous calender. The processing step is carried out at a temperature of 20 to 100°C and a load of 20 to 200 kgf / cm². 2 This can be carried out by applying pressure. For example, the processing step may be performed at a temperature of 30 to 80°C and a pressure of 30 to 150 kgf / cm². 2 This can be carried out by applying pressure. By performing the above processing steps within the aforementioned temperature and pressure range, there is no sound transmission loss due to void destruction caused by excessive density increase, resulting in excellent durability.

[0053] Following the processing stage, which adjusts the density and thickness of the precursor, a converting stage follows, which determines the shape of the precursor.

[0054] The converting steps described above may include slitting to obtain a product of a desired width, lateral cutting such as guillotining to obtain a product of a desired length, and, for example, flatbed or rotary die cutting to obtain a product of a desired shape.

[0055] The precursor that has undergone the above-mentioned converting step can then undergo a step in which tension is applied in the mechanical direction (MD) to imidize it into a uniaxial orientation in order to obtain a nanomembrane.

[0056] The converted precursor can be imidized to form strong bonds between fibers.

[0057] The aforementioned imidation can be carried out by thermal imidation, chemical imidation, or a combination thereof.

[0058] For example, the thermal imidation step can be carried out by heating the converted precursor at a temperature of 200°C to 500°C for 10 to 30 minutes. When the thermal imidation step is carried out within the above range, a polyimide nanomembrane with the desired properties can be obtained without the destruction or thermal shrinkage of the polyimide nanomembrane.

[0059] For example, the chemical imidation step can be carried out by contacting the converted precursor with a solvent such as an acid anhydride like acetic anhydride, or a tertiary amine like pyridine.

[0060] The polyimide nanomembrane that has undergone the aforementioned imidation process can have an imidation rate of 90% or more. An imidation rate of 90% or more allows for excellent heat resistance and durability, enabling it to withstand high temperatures of 280°C or higher.

[0061] Furthermore, the imidization process can be carried out by applying tension in the mechanical direction to imidize the material in a uniaxial orientation, thereby achieving excellent mechanical strength. For example, the step of imidizing the material in a uniaxial orientation can be performed by applying a tension of 20N to 100N in the mechanical direction to the converted precursor.

[0062] By applying tension in the machine direction, fiber orientation and imidation bond formation are densely established in the machine direction, and the ratio of the number of fiber reinforcing fibers in the machine direction to the number of fiber reinforcing fibers in the width direction (i.e., the machine transverse direction) (number of MD fiber reinforcing fibers / number of TD fiber reinforcing fibers) is deformed to 1.5 to 10, for example, 2 to 9 or 2.5 to 8, thereby improving strength in the machine direction and suppressing fracture in the machine direction.

[0063] Furthermore, the anisotropy between the strength in the machine direction (MD) and the strength in the transverse direction (TD) (MD strength / TD strength) can be 2 to 11, for example, 2.5 to 9 or 3 to 8.

[0064] Not only that, through the aforementioned imidization step, the effect of improving dust collection efficiency and durability is achieved without reducing sound transmission loss and air permeability.

[0065] In addition, the polyimide nanomembrane that has undergone the aforementioned imidization step may have a porosity of 50 to 90%. For example, the porosity of the polyimide nanomembrane may be 60 to 90%, 70 to 90%, or 60 to 80%.

[0066] The polyimide nanomembrane that has undergone the aforementioned imidization step may have a dust collection efficiency of 95% or more as measured by the following measurement method. For example, the dust collection efficiency of the polyimide nanomembrane may be 96% or more, 97% or more, 98% or more, or 99% or more.

[0067] [Measurement Method] Dust size: 1 μm; Air flow rate: 32 L / min; Measurement area: 100 cm 2 Measured with AFT8130

[0068] The polyimide nanomembrane produced as described above may have the following physical property values.

[0069] The polyimide nanomembrane may have a thickness of 0.5 to 20 μm.

[0070] The air permeability of the nanomembrane may be 50 to 200 cm 3 / cm 2 / sec. For example, the air permeability of the nanomembrane may be 100 to 195 cm 3 / cm 2 / sec, or 110 to 190 cm 3 / cm 2 / sec.

[0071] The basis weight of the nanomembrane may be 0.1 to 10 g / m 2It is possible that the unit weight of the nanomembrane is 1 to 5 g / m². 2 , or 1 to 3 g / m 2 It is possible.

[0072] The thermal shrinkage rate of the aforementioned nanomembrane may be 1% or less at 300°C.

[0073] The weight loss rate of the nanomembrane at 300°C may be 1% by weight or less.

[0074] The sound transmission loss of the nanomembrane may be less than 5 dB / pa based on a 94 dB standard. For example, the sound transmission loss of the nanomembrane may be 4 dB / pa or less based on a 94 dB standard.

[0075] Figure 3 is a photograph showing the surfaces of the nanomembrane of Example 1 (left) and the nanomembrane of Comparative Example 2 (right). Referring to Figure 3, it can be seen that the nanomembrane of Example 1 was manufactured by applying tension during the imidation process and undergoing uniaxial orientation heat treatment, resulting in a higher ratio of the mechanical direction to the width direction of the fiber strands. The nanomembrane of Comparative Example 2 was manufactured through tensionless heat treatment during the imidation process, and it was confirmed that the ratio of the orientation in the width direction to the mechanical direction in the fiber strands was almost identical.

[0076] Conventionally, in the process of imparting anisotropy to polyimide nanomembranes, membrane fracture due to tension in a specific direction was a problem. However, in one embodiment of the present invention, the ratio of the MD winding speed to the TD reciprocating speed is adjusted during the electrospinning process of the spinning solution, and uniaxial orientation imidation is promoted in the MD direction, resulting in a significant improvement in tensile strength in the MD direction. As a result, a polyimide nanomembrane with significantly improved tensile strength in the MD direction was obtained during the manufacturing process.

[0077] A nanomembrane assembly according to one embodiment of the present invention can be used in a variety of electronic devices, including MEMS such as mobile phones, electronic pads, microphones, and speakers. [Examples]

[0078] The present invention will be described in more detail below through specific examples, and the present invention is not limited to the following examples.

[0079] <Example 1> A 5 L polyamic acid solution was prepared with a solid content of 11% by weight and a solution viscosity of 250 poise (KSMISO2555, 23°C).

[0080] After transferring the manufactured polyamic acid solution to a solution tank, it was supplied via a metering gear pump to a spinning chamber consisting of 20 nozzles to which a high voltage of 60kV was applied, and a precursor was manufactured by electrospinning. During this process, the discharge rate was 4ml / min, the ratio of the distance between the nozzle and the accumulation plate to the distance to the nozzle tip was 1.2, and 70°C air was blown in the direction from which the precursor was discharged to disperse it. At this time, the winding speed in the MD direction and the reciprocating speed in the TD direction of the precursor were adjusted as shown in Table 1 below. Subsequently, the precursor was processed by applying a linear pressure of 100kgf / cm using a two-stage continuous calender maintained at a temperature of 65°C while being transported in a roll-to-roll manner. After a conversion process, it was processed to a thickness of 5μm and a unit weight of 3g / m². 2 A converted precursor was manufactured. Subsequently, when the converted precursor was transported in a roll-to-roll manner, the precursor was imidized for 20 minutes in a continuous heat treatment furnace maintained at a temperature of 400°C while applying a tension of 50N in the machine direction, resulting in a final thickness of 3 μm and a unit weight of 1.5 g / m². 2 We manufactured polyimide nanomembranes.

[0081] <Examples 2 to 7> The reaction conditions were modified as shown in Table 1 below, and an oil-repellent nanomembrane was produced using the same method as in Example 1.

[0082] <Comparative Example 1> A 5 L polyamic acid solution was prepared with a solid content of 11% by weight and a solution viscosity of 250 poise (KSMISO2555, 23°C).

[0083] After transferring the manufactured polyamic acid solution to a solution tank, it was supplied via a metering gear pump to a spinning chamber consisting of 20 nozzles to which a high voltage of 60kV was applied, and a precursor was manufactured by electrospinning. The discharge rate was 4ml / min, the ratio of the distance between the nozzle and the accumulation plate to the distance to the nozzle tip was 1.2, and 70°C air was blown in the direction from which the precursor was discharged to disperse the precursor. During this process, the ratio of the winding speed in the MD direction to the reciprocating speed in the TD direction of the precursor was adjusted as shown in Table 1. Subsequently, the precursor was processed by applying a linear pressure of 100kgf / cm using a two-stage continuous calender maintained at a temperature of 65°C while being transported in a roll-to-roll manner. After a converting process, the resulting material had a thickness of 5μm and a unit weight of 3g / m². 2 Converted precursors were manufactured. For roll-to-roll transport of the converted precursors, the precursors were imidized for 20 minutes in a continuous heat treatment furnace maintained at 300°C while applying a tension of 10N in the machine direction, resulting in a final thickness of 3μm and a unit weight of 2g / m². 2 We manufactured polyimide nanomembranes.

[0084] <Comparative Example 2> A 5 L polyamic acid solution was prepared with a solid content of 11% by weight and a solution viscosity of 250 poise (KSMISO2555, 23°C).

[0085] After transferring the manufactured polyamic acid solution to a solution tank, it was supplied via a metering gear pump to a spinning chamber consisting of 20 nozzles to which a high voltage of 60kV was applied, and a precursor was manufactured by electrospinning. At this time, the discharge rate was 3 ml / min, the ratio of the distance between the nozzle and the accumulation plate to the distance to the nozzle tip was 1.2, and 70°C air was blown in the direction in which the precursor was discharged to disperse the precursor. At this time, the ratio of the winding speed in the MD direction to the reciprocating speed in the TD direction of the precursor was 3.0. Subsequently, while the precursor was transferred in a roll-to-roll manner, it was processed by applying a linear pressure of 100 kgf / cm using a two-stage continuous calender maintained at a temperature of 65°C, and after a converting process, it was obtained with a thickness of 4 μm and a unit weight of 3 g / m 2 A converted precursor was manufactured. The converted precursor was then imidized for 20 minutes in a continuous heat treatment furnace maintained at a temperature of 400°C while being transported under tension-free conditions in a roll-to-roll manner, resulting in a final product with a thickness of 3 μm and a unit weight of 2.5 g / m². 2 We manufactured polyimide nanomembranes.

[0086] <Comparative Examples 3 to 5> The reaction conditions were modified as shown in Table 1 below, and an oil-repellent nanomembrane was produced using the same method as in Comparative Example 1.

[0087] <Comparative Example 6> Polyvinylidene difluoride (PVDF) was dissolved in dimethylformamide (DMF) solvent to prepare 5 L of an electrospinning solution with a solid content of 15% by weight and a solution viscosity of 250 poise (KS MISO 2555, 23°C).

[0088] After transferring the manufactured electrospinning solution to a solution tank, it was supplied via a metering gear pump to a spinning chamber consisting of 20 nozzles to which a high voltage of 60kV was applied, and electrospinned to produce PVDF nanomembranes. The discharge rate was 4 ml / min, the ratio of the distance between the nozzle and the integrating plate to the distance to the nozzle tip was 1.2, and the ratio of the winding speed in the MD direction to the reciprocating speed in the TD direction was 0.9. The final result was a nanomembrane with a thickness of 4 μm and a unit weight of 2 g / m². 2 We manufactured polyvinylidene fluoride nanomembranes.

[0089] [Table 1]

[0090] <Evaluation of nanomembranes> The unit weight, thickness, porosity, air permeability, average pore size, tensile strength (MD), tensile strength (TD), roll-to-roll stability, sound transmission loss, dust collection efficiency, thermal shrinkage rate, and weight loss rate of the nanomembranes of Examples 1 to 7 and Comparative Examples 1 to 6 were measured using the method described below, and the results are shown in Table 2.

[0091] (1) Unit weight: KSK0514 or ASTM D3776 (2) Thickness: KSK0506 or KSK ISO 9073-2, ISO 4593

[0092] (3) Porosity: Calculated as the ratio of air volume to total volume of the nanofiber membrane based on Formula 1 below (total volume is calculated by manufacturing a rectangular or circular sample and measuring its width, length, and thickness, while air volume is calculated by measuring the mass of the sample and then subtracting the polymer volume, which is calculated inversely from the density, from the total volume).

[0093] [Formula 1] Porosity (%) = [1 - (A / B)] × 100 = {1 - [(C / D) / B]} × 100

[0094] In Equation 1, A is the density of the nanomembrane, B is the density of the nanomembrane polymer, C is the weight of the nanomembrane, and D is the volume of the nanomembrane.

[0095] (4) Air permeability: ASTM D737, area 38 cm² 2 (cm) Measured under constant pressure conditions of 125 Pa 3 / cm 2 It is possible to convert ( / sec) to CFM (Cubic Feet per Minute) using a conversion factor of 0.508016, and the unit is ft. 3 / ft 2 It is / min(CFM).

[0096] (5) Mean pore diameter: Using a capillary flow porometer (CFP) as specified in ASTM F316, the mean pore size and pore size distribution were measured from the diameter of the limiting pore, which is the pore size in the narrowest section.

[0097] (6) Intensity: The ASTMD882 was applied, and the MD (machine direction) and TD (transverse direction) were measured 10 times each. The average value was obtained by excluding the maximum and minimum values.

[0098] (7) Anisotropy of intensity: Calculate the ratio of the MD / TD values ​​of the intensity.

[0099] (8) Observation of fiber arrangement: Each sample was prepared, and an SEM image was taken of the sample using an FE-SEM (JSM-7900F, JEOL) at a magnification of 2500x with the machine direction as the reference.

[0100] (9) Ratio of fibrous muscle fibers: In the aforementioned SEM image, the ratio (MD / TD) of the number of fibrous muscle fibers in the MD direction to the number of fibrous muscle fibers in the TD direction was calculated. The criteria for determining the MD direction were fibers within a 30° range to the left and right of the machine direction as the reference axis. TD refers to all fibers other than those in the MD direction.

[0101] (10) Sound transmission loss: The degree of sound loss was evaluated by checking the change in microphone sensitivity within the speaker frequency range (100~20,000Hz) and measuring the sensitivity of the MEMS that recognizes microphone sensitivity with and without attaching the nanomembrane assembly.

[0102] (11) Dust collection efficiency: Dust size 1 μm, airflow velocity 32 l / min, and measurement area 100 cm² 2 Then, the measurement is performed using the AFT8130.

[0103] (12) Heat shrinkage rate (%): After heat treatment in an oven at 300°C ± 2°C for 30 ± 2 minutes, the change in length is measured after being left for 24 hours at a temperature of 23°C ± 2°C and a humidity of 50% ± 5% (relative humidity).

[0104] (13) Weight loss rate: Each sample was prepared at 0.5 g, and heat was applied to the sample using a TGA analyzer (Thermoplus EVOII TG8120, Rigaku) ​​under nitrogen conditions at a rate of 20 °C / min, increasing the temperature from room temperature to 800 °C, and the resulting weight change was measured.

[0105] [Table 2]

[0106] As shown in Table 2 above, in Examples 1 to 7, the nanomembrane has a fiber-to-muscle ratio of 1.5 or more, and by applying tension during the imidization process and undergoing a uniaxial orientation heat treatment process, it can be confirmed that it has excellent strength that prevents fracture in the MD or TD direction during an anisotropic roll-to-roll process.

[0107] On the other hand, in Comparative Example 1, where the ratio of fiber reinforcing strands is 1.1, and in Comparative Example 2, where the ratio of fiber reinforcing strands is 0.9 and the uniaxial orientation heat treatment process is not included, it can be confirmed that fracture occurs in the MD direction or in the MD and TD directions during the roll-to-roll process.

[0108] Furthermore, in Comparative Example 3, which has an anisotropy of strength (MD strength / TD strength) of 26.1, fracture occurred in the TD direction, confirming that the dust collection efficiency was very low.

[0109] Furthermore, in Comparative Example 4, which has a strength anisotropy (MD strength / TD strength) of 0.1, it can be confirmed that fracture occurs in the MD direction during the roll-to-roll process.

[0110] Furthermore, in Comparative Example 5, where the MD / TD speed ratio is 15, it can be confirmed that fracture occurs in the TD direction during the roll-to-roll process.

[0111] On the other hand, Comparative Example 6, manufactured using PVDF, was found to have significantly higher sound transmission loss, thermal shrinkage rate, and weight loss rate compared to Examples 1 to 7, which were manufactured using polyamic acid. [Industrial applicability]

[0112] The present invention provides a nanomembrane in which tensile strength in the MD direction is improved due to a unique pore structure, and fracture is suppressed during the roll-to-roll process, thereby improving processability.

Claims

1. A nanomembrane formed from polyimide fibers with a porosity of 50 to 90%, The nanomembrane has an anisotropy (MD intensity / TD intensity) of 2 to 11 between its machine direction (MD) intensity and its transverse direction (TD) intensity. The nanomembrane has a ratio of the number of fibrous fibers in the mechanical direction to the number of fibrous fibers in the width direction (number of MD fibrous fibers / number of TD fibrous fibers) of 1.5 to 10. The air permeability of the aforementioned nanomembrane is 50 to 200 cm². 3 / cm 2 / sec, The aforementioned nanomembrane has a dust collection efficiency of 95% or more, as measured by the following method: [Measurement method] Dust size: 1 μm; Airflow velocity: 32 l / min; Measurement area: 100 cm² 2 Measurements are taken using the AFT8130.

2. The nanomembrane according to claim 1, wherein the sound transmission loss of the nanomembrane is less than 5 dB / pa based on 94 dB.

3. The nanomembrane according to claim 1, wherein the polyimide fiber comprises polyimide, polyamideimide, polyetherimide, or a combination thereof.

4. The nanomembrane according to claim 1, wherein the thermal shrinkage rate of the nanomembrane at 300°C is 1% or less.

5. The nanomembrane according to claim 1, wherein the weight loss rate of the nanomembrane at 300°C is 1% by weight or less.

6. Base material; A nanomembrane according to any one of claims 1 to 5; and An adhesive layer interposed between the substrate and the nanomembrane; Nanomembrane assembly containing

7. An electronic device comprising a nanomembrane according to any one of claims 1 to 5.

8. An electrospinning step to produce a precursor by electrospinning a polyamic acid solution, wherein the ratio of the machine direction (MD) winding speed to the travel direction (TD) reciprocating speed (MD winding speed / TD reciprocating speed) in the electrospinning step is adjusted to produce an anisotropic precursor; A processing step to adjust the density and thickness of the precursor, A converting step in which the shape of the precursor is determined, and The converted precursor is imidized to a uniaxial orientation by applying tension in the MD direction to obtain a nanomembrane, During the electrospinning stage described above, air is blown in the direction from which the precursor is discharged. The value of the MD winding speed / TD reciprocating speed is between 2 and 10. The nanomembrane is characterized in that it has a dust collection efficiency of 95% or more, as measured by the following method, and the method for manufacturing a nanomembrane. [Measurement method] Dust size: 1 μm; Airflow velocity: 32 l / min; Measurement area: 100 cm² 2 Measurements are taken using the AFT8130.

9. The method for producing a nanomembrane according to claim 8, wherein the step of imidizing to a uniaxial orientation is carried out by applying a tension of 20 N to 100 N in the mechanical direction to the converted precursor.

Citation Information

Patent Citations

  • Method for manufacturing polymer electrolyte reinforced membrane andpolymer electrolyte reinforced membrane

    KR1020130078153A

  • Elastic nonwoven made from thermoset fibers

    US20150108063A1

  • NANO membrane, NANO membrane assembly, and method for manufacturing NANO membrane