Liners for cardboard and corrugated cardboard
The paperboard composition with specific pulp and drying agent ratios minimizes creasing cracks, enhancing structural integrity and printability for corrugated cardboard applications.
Patent Information
- Application Number
- JP2026109224
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-06-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-06-22
AI Technical Summary
Conventional corrugated cardboard liners are prone to creasing cracks during folding, which compromises their structural integrity and aesthetic quality.
A paperboard composition comprising a surface layer, one or more middle layers, and a back layer, with specific pulp and drying agent content ratios, including 20% or more hardwood kraft pulp, varying paper strength agent contents across layers, and a total basis weight of 290 g/m², to minimize creasing cracks.
The paperboard exhibits reduced creasing cracks, enhanced specific burst strength, and improved printability, making it suitable for use as a corrugated cardboard liner.
Smart Images

Figure 0007954852000001 
Figure 0007954852000002 
Figure 0007954852000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to paperboard, particularly paperboard suitable for corrugated cardboard liners, box making, and laminated paper. [Background technology]
[0002] Corrugated cardboard is manufactured by laminating a liner to one or both sides of a corrugated core using a corrugator. Corrugated cardboard is lightweight and inexpensive, so it is used to pack a variety of goods. When corrugated cardboard is processed into so-called corrugated boxes for packing goods, creasing (damage lines arising from creasing lines (shallow grooves) made in the base paper) may occur on the outer surface of the fold during this folding process. It is preferable that corrugated cardboard does not develop crease lines. For example, Patent Document 1 describes a corrugated cardboard comprising at least a surface layer, a front middle layer, a back middle layer, and a back layer, having 4 to 6 layers in total, wherein the surface layer contains 50 to 100% by mass of unbleached softwood kraft pulp, the front middle layer and the back middle layer contain 95% by mass or less of recycled corrugated cardboard pulp, and the back layer contains less than 90% by mass of recycled corrugated cardboard pulp, all layers contain an internal sizing agent, the total internal sizing agent content is 0.2 to 1.0 parts by mass per 100 parts by mass of total pulp, and the total basis weight is 330 g / m². 2 The above results show that the Cobb water absorption of the surface and back layers at a measurement time of 2 minutes was 5 g / m². 2 More than 50g / m 2 The absolute value of the difference in Cobb water absorption between the surface layer and the back layer is 10 g / m². 2 The following high-basis-weight cardboard is proposed, which is less prone to cracking along the crease lines when folded and offers excellent print quality. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2024-90387 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The cardboard described in Patent Document 1 can prevent cracking along the crease lines compared to conventional cardboard, but further prevention of cracking along the crease lines is required. The present invention aims to provide cardboard that is less prone to cracking along the crease lines when folded. [Means for solving the problem]
[0005] The means to solve the above problems are as follows: 1. It has a surface layer, one or more middle layers, and a back layer. It contains 20% or more by mass of hardwood kraft pulp relative to the total pulp mass. The content of internally added drying agent relative to the pulp in each layer is lowest in at least one of the middle layers. The content of the internally added drying agent in the pulp of the surface layer is smaller than the content of the internally added drying agent in the pulp of the back layer. Total basis weight: 290 g / m² 2 That's all. Cardboard characterized by having a creasing rate of 30% or less. 2. The cardboard according to 1, characterized in that the average water filtration rate of the pulp in each layer is 350 mlCSF or more. 3. The paperboard according to 1. or 2., characterized in that the content of internally added drying force agent relative to the pulp in each layer is highest in the back layer. 4. The surface layer contains 50% to 100% by mass of softwood kraft pulp relative to the pulp mass. The cardboard according to any one of claims 1 to 3, characterized in that the backing layer contains 40% to 100% by mass of hardwood kraft pulp relative to the pulp mass. 5. The paperboard according to any one of 1 to 4, characterized in that the recycled paper pulp content relative to the pulp mass of the surface layer is 1% by mass or less. 6. The paperboard according to any one of 1 to 5, characterized in that the content of internally added drying force agent relative to the pulp in each layer satisfies the following conditions. The paper strength agent content of the back layer > the paper strength agent content of the front layer ≥ the paper strength agent content of the middle layer with the lowest paper strength agent content. 7. A corrugated cardboard liner characterized by having a cardboard sheet as described in any of 1 to 6. [Effects of the Invention]
[0006] The paperboard of the present invention is less prone to cracking along the crease lines when folded. Because the paperboard of the present invention is less prone to cracking along the crease lines, it can be suitably used as a liner for corrugated cardboard. [Modes for carrying out the invention]
[0007] The paperboard of the present invention has a surface layer, one or more intermediate layers, and a back layer. It contains 20% or more by mass of hardwood kraft pulp relative to the total pulp mass. The content of internally added drying agent relative to the pulp in each layer is lowest in at least one of the middle layers. The content of the internally added drying agent in the pulp of the surface layer is smaller than the content of the internally added drying agent in the pulp of the back layer. Total basis weight: 290 g / m² 2 That's all. The rate of splitting is 30% or less. In this specification, the notation "A~B" (where A and B are numerical values) refers to a numerical range that includes both ends of that range.
[0008] The paperboard of the present invention is composed of a surface layer, one or more intermediate layers, and a back layer, with the surface layer and back layer being the outermost layers. The paperboard of the present invention has three or more layers, and the number of intermediate layers can be appropriately set according to the required basis weight, etc. The back layer is the bottom surface during papermaking and is the layer formed when raw materials are first supplied to the wire part in a multi-layer papermaking machine, while the surface layer is the opposite side of the back layer, i.e., the top surface during papermaking and is the layer formed when raw materials are last supplied to the wire part in a multi-layer papermaking machine.
[0009] The paperboard of the present invention contains 20% or more by mass of hardwood kraft pulp relative to the total pulp mass. Although the mechanism is unknown, paperboard that satisfies this hardwood kraft pulp content exhibits excellent specific burst strength, cushioning properties, and printability. In addition to hardwood kraft pulp, the paperboard of the present invention may also contain various pulps derived from wood fibers, such as softwood kraft pulp, recycled paper pulp, ground wood pulp (GP), refiner ground pulp (RGP), chemical pulp (CP), thermomechanical pulp (TMP), and chemothermetic pulp (CTMP), as well as non-wood pulps obtained from kenaf, bagasse, bamboo, hemp, straw, etc. Both unbleached kraft pulp (LUKP / NUKP) and bleached kraft pulp (LBKP / NBKP) can be used as hardwood kraft pulp and softwood kraft pulp. However, for applications where whiteness is not required, unbleached kraft pulp is preferable because it has superior strength and can be produced with less energy because it does not require a bleaching process. In the paperboard of the present invention, the average water filtration rate (Canadian standard water filtration rate) of the pulp used in each layer is not particularly limited, but from the viewpoint of preventing cracking along the crease, strength, and printability, it is preferably 350 ml CSF or more and 600 ml CSF or less, more preferably 400 ml CSF or more, and even more preferably 450 ml CSF or more.
[0010] The content of hardwood kraft pulp relative to the total pulp mass of the paperboard of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, and even more preferably 70% by mass or more, from the viewpoint of specific burst strength, scratch resistance, cushioning, printability, and improvement of paper strength by the addition of internally added drying force agents. In the paperboard of the present invention, the content ratio of softwood kraft pulp relative to the total pulp mass is preferably 5 mass% or more, more preferably 7 mass% or more, and still more preferably 10 mass% or more. Further, the content ratio of softwood kraft pulp relative to the total pulp mass is preferably 30 mass% or less, more preferably 25 mass% or less, and still more preferably 20 mass% or less.
[0011] From the viewpoint of cost reduction, the paperboard of the present invention preferably uses inexpensive waste paper pulp. As the waste paper pulp, it is possible to use one type or a mixture of two or more selected from: waste paper pulp obtained by disintegrating unprinted waste paper such as corrugated board waste paper, high-grade white waste paper, special white waste paper, medium white waste paper, and white broke; pulp (DIP) obtained by disintegrating and then deinking printed waste paper on high-quality paper, high-quality coated paper, medium-quality paper, medium-quality coated paper, and low-grade paper, handwritten waste paper, papers such as discarded confidential documents, magazine waste paper, and newspaper waste paper. Among these, waste paper pulp derived from corrugated board waste paper (hereinafter referred to as corrugated board waste paper pulp) and magazine waste paper are preferred from the viewpoints of cost and strength development.
[0012] In the paperboard of the present invention, the content ratio of waste paper pulp relative to the total pulp mass is not particularly limited, and may be, for example, 0.1 mass% or more and 70 mass% or less. The lower the content ratio of waste paper pulp, the higher the specific burst strength, scratch resistance, cushioning property, printability and the like can be maintained. Therefore, from the viewpoints of specific burst strength, scratch resistance, cushioning property, printability and the like, the content ratio of waste paper pulp relative to the total pulp mass is preferably 60 mass% or less, more preferably 50 mass% or less, still more preferably 40 mass% or less, even more preferably 30 mass% or less, even more preferably 10 mass% or less, and even more preferably 5 mass% or less. On the other hand, since waste paper pulp is inexpensive, the cost decreases as its content ratio increases. Therefore, from the viewpoint of cost, the content ratio of waste paper pulp relative to the total pulp mass is preferably 0.1 mass% or more, more preferably 1 mass% or more, still more preferably 5 mass% or more, even more preferably 10 mass% or more, and even more preferably 15 mass% or more.
[0013] It is preferable that the surface layer contains 50 mass% or more and 100 mass% or less of softwood kraft pulp relative to the pulp contained in the surface layer. Thereby, the burst strength and scratch resistance are improved, and crease crack prevention, cushioning properties, and printability are also improved. The content of this softwood kraft pulp in the surface layer is more preferably 60 mass% or more, further preferably 80 mass% or more, still more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 100 mass%. The surface layer preferably has a waste paper pulp content of 1 mass% or less relative to the pulp mass. Waste paper pulp is generally blended into paperboard due to its low cost, but it reduces strength and scratch resistance. In addition, waste paper pulp is hard due to advanced fiber hornification, and tends to induce crease cracks in the surface layer when the surface layer is folded outward. The content of waste paper pulp is more preferably 0.5 mass% or less, further preferably 0.3 mass% or less, still more preferably 0.1 mass% or less, and most preferably 0 mass% (not contained).
[0014] The surface layer may contain pulps other than softwood kraft pulp and waste paper pulp, for example, hardwood kraft pulp, but among the pulps used, the total proportion of softwood kraft pulp and hardwood kraft pulp is preferably the highest, and the proportion of softwood kraft pulp is more preferably the highest. The total of softwood kraft pulp and hardwood kraft pulp is preferably 60 mass% or more, more preferably 80 mass% or more, further preferably 90 mass% or more, still more preferably 95 mass% or more, and most preferably 100 mass%. Virgin pulps such as softwood kraft pulp and hardwood kraft pulp have flexible fibers, so blending them improves the strength of the paper itself, and can more effectively prevent crease cracks in the surface layer even when the surface layer is folded outward.
[0015] The backing layer preferably contains 40% to 100% by mass of hardwood kraft pulp relative to the pulp it contains, in order to provide cushioning, printability, specific burst strength, and to suppress deterioration of strength and form when a high amount of internally added drying force agent is used. The hardwood kraft pulp content is more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass. Regarding the backing layer, the recycled paper pulp content relative to the pulp contained in the backing layer is preferably 10% to 50% by mass from the viewpoint of balancing cost and strength, and from the viewpoint of specific bursting strength, it is preferably 5% or less by mass, more preferably 3% or less by mass, even more preferably 1% or less by mass, even more preferably 0.5% or less by mass, and most preferably 0% by mass (not included). The backing layer may contain pulps other than hardwood kraft pulp and recycled paper pulp, but it is preferable that hardwood kraft pulp accounts for the highest proportion of the pulps used.
[0016] The paperboard of the present invention only needs to contain 20% by mass or more of hardwood kraft pulp relative to the total pulp mass contained in the paperboard, and as long as this condition is satisfied, the pulp constituting the middle layer is not particularly limited. The middle layer may contain one or more types of pulps derived from wood fibers, such as softwood kraft pulp, hardwood kraft pulp, recycled paper pulp, crushed wood pulp (GP), refiner ground pulp (RGP), chemical pulp (CP), thermomechanical pulp (TMP), chemothermetic pulp (CTMP), and non-wood pulps obtained from kenaf, bagasse, bamboo, hemp, straw, etc. In terms of cushioning and printability, the content of hardwood kraft pulp relative to the pulp in the middle layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 75% by mass or more. The middle layer is less prone to collapse when internally added drying strength agents are added, and the reduction in strength is minimal. Therefore, the content of softwood kraft pulp in the middle layer relative to the pulp is preferably 29% by mass or less, and more preferably 25% by mass or less. Furthermore, the content of recycled paper pulp in the middle layer relative to the pulp is preferably 5% by mass or more and 50% by mass or less, from the standpoint of balancing cost and strength. If there are two or more intermediate layers, the pulp composition of each intermediate layer may be the same or different.
[0017] The paperboard of the present invention has a ratio of internally added dry paper strength agent to the pulp in the surface layer, one or more middle layers, and back layer (hereinafter also referred to as the paper strength agent content), with at least one middle layer having the lowest ratio, and the paper strength agent content of the surface layer being lower than that of the back layer. Because the paper strength agent content of each layer of the present invention satisfies this relationship, buckling is more likely to occur in the middle layer during folding, and by breaking the middle layer first, it is possible to prevent the occurrence of crease line cracking in the surface layer. Furthermore, because the paper strength agent content of at least one middle layer is the lowest, it has excellent cushioning properties and printability. As the internally added drying strength agent, one or more types of those used in the papermaking field, such as polyacrylamide (PAM) or modified starch, can be used without particular restriction. However, it is preferable to use a polyacrylamide type because it has a high paper strength-enhancing effect. Any type of polyacrylamide can be used, including anionic, cationic, or amphoteric types. Furthermore, the composition of the internally added drying strength agent in each layer may be the same or different.
[0018] The paper strength agent content of each layer in the paperboard of the present invention is not particularly limited as long as the above conditions are satisfied, but it is preferable that the paper strength agent content of each layer be 0.01% by mass or more and 3.0% by mass or less. The paper strength agent content of the middle layer, which has the lowest paper strength agent content, is preferably 0.01% by mass or more and 1.0% by mass or less, more preferably 0.8% by mass or less, even more preferably 0.6% by mass or less, even more preferably 0.4% by mass or less, even more preferably 0.2% by mass or less, even more preferably 0.15% by mass or less, even more preferably 0.12% by mass or less, and also more preferably 0.03% by mass or more, and even more preferably 0.05% by mass or more.
[0019] The paper strength agent content of the surface layer is smaller than that of the back layer. The difference between the paper strength agent content of the back layer and the paper strength agent content of the surface layer (back layer - surface layer) is preferably 0.1% by mass or more and 1% by mass or less, more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more. The paper strength agent content in the surface layer is preferably 0.01% by mass or more and 2.9% by mass or less. As the paper strength agent content in the surface layer decreases, flexibility and cushioning are imparted, and the prevention of line cracking and printability are improved, so 2.5% by mass or less is more preferable, 2.0% by mass or less is even more preferable, 1.5% by mass or less is even more preferable, 1.0% by mass or less is even more preferable, 0.8% by mass or less is even more preferable, and 0.6% by mass or less is even more preferable. On the other hand, if it is too low, the strength may decrease too much, so 0.1% by mass or more is more preferable, and 0.2% by mass or more is even more preferable.
[0020] The paper strength agent content in the backing layer is preferably 0.02% by mass or more and 3.0% by mass or less, more preferably 2.5% by mass or less, even more preferably 2.0% by mass or less, even more preferably 1.5% by mass or less, and even more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more.
[0021] In the middle layer, at least one layer has the lowest paper strength agent content among all layers. If there are two or more middle layers, from the viewpoint of preventing cracking along the crease lines, the middle layer with the lowest paper strength agent content is preferably a middle layer that is farther from the surface layer, and more preferably a middle layer that is closest to the back layer. Note that there may be two or more layers with the lowest paper strength agent content. That is, among the paper strength agent content of each layer, the lowest paper strength agent content may be in two or more middle layers, or the lowest paper strength agent content may be in one or more middle layers and the surface layer. However, in the paperboard of the present invention, since the paper strength agent content of the back layer is greater than that of the surface layer, the paper strength agent content of the back layer is greater than the lowest paper strength agent content of the middle layer.
[0022] It is preferable that the backing layer has the highest paper strength agent content among all the layers. It is also possible for two or more layers to have the highest paper strength agent content. Paperboard with the highest paper strength agent content in the backing layer exhibits improved strength as paperboard, such as specific burst strength, and also improves print quality because the backing layer acts as a support layer during printing. Furthermore, the paper strength agent content in each layer preferably satisfies the following conditions. The paper strength agent content of the back layer > the paper strength agent content of the front layer ≥ the paper strength agent content of the middle layer with the lowest paper strength agent content.
[0023] In the paperboard of the present invention, it is preferable that the surface layer, one or more intermediate layers, and back layer all contain a sizing agent, in order to maintain strength in a high-humidity environment. Examples of sizing agents include rosin-based sizing agents, rosin emulsion-based sizing agents, α-carboxymethyl saturated fatty acids, neutral rosin-based sizing agents, alkyl ketene dimers (AKD), alkenyl succinic anhydride (ASA), cationic polymer-based sizing agents, etc., and one or more of these can be used. Among these, rosin-based sizing agents and rosin emulsion-based sizing agents are preferred because they do not easily soil the paper machine and have excellent operability. The sizing agent content in each layer is preferably 0.2% by mass or more, more preferably 0.25% by mass or more, and even more preferably 0.3% by mass or more, relative to the pulp mass, from the viewpoint of maintaining strength in a high-humidity environment. There is no particular upper limit to the sizing agent content, but it is approximately 1.0% by mass relative to the pulp mass. Even if the sizing agent is added in amounts exceeding 1.0% by mass relative to the pulp mass, the effect of maintaining strength in a high-humidity environment is almost saturated and hardly improves, and it becomes costly. In the paperboard of the present invention, the type and content of the sizing agent in each paper layer may be the same or different.
[0024] The paperboard of the present invention may contain internal additives such as aluminum sulfate, aluminum chloride, sodium aluminate, basic aluminum compounds, water-soluble aluminum compounds, polyvalent metal compounds, and silica sol, to the extent that it does not affect the quality. The type and content of internal additives in each paper layer of the paperboard of the present invention may be the same or different. However, it is preferable that the content of the internally added wet paper strength enhancer relative to the pulp mass of the paperboard of the present invention is less than 0.1% by mass. If the content of the internally added wet paper strength enhancer is 0.1% by mass or more, the disintegrability decreases, which may reduce its recyclability as waste paper or recycled paper.
[0025] Furthermore, known fillers may be added to each paper layer of the paperboard of the present invention as needed. Examples of fillers include inorganic fillers such as kaolin, calcined kaolin, delaminated kaolin, clay, calcined clay, delaminated clay, illite, heavy calcium carbonate, light calcium carbonate, light calcium carbonate-silica composite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon dioxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, and zinc hydroxide, as well as organic fillers such as urea-formaldehyde resin, polystyrene resin, and phenolic resin. One or more of these can be used. The filler content in each paper layer of the paperboard of the present invention may be the same or different.
[0026] The paperboard of the present invention may have a coating layer on its surface for purposes such as improving the strength of the paperboard and imparting printability. Depending on the purpose, the coating layer may contain one or more of known surface treatment chemicals such as external paper strength agents (hereinafter also referred to as surface paper strength agents), surface sizing agents, water repellents, pigments, binder resins, anti-slip agents, preservatives, defoamers, viscosity modifiers, and creasing crack inhibitors. From the viewpoint of strength improvement, the paperboard of the present invention preferably has a coating layer containing a surface paper strength agent. As the surface paper strength agent, polyacrylamide-based, polyvinyl alcohol-based, starch-based materials such as oxidized starch, cationized starch and amphoteric starch, and cellulose-based materials such as carboxymethyl cellulose can be used, among which polyacrylamide-based materials are preferred. The coating amount of the surface paper strength agent is 0.05 g / m 2 or more, more preferably 0.1 g / m 2 or more. Further, for the purpose of improving weather resistance, the coating layer preferably contains a surface sizing agent and a water repellent. Examples of the surface sizing agent include those similar to the aforementioned internal sizing agents, and examples of the water repellent include fluorine-based resins, polyamide-based resins, and wax emulsions.
[0027] The paperboard of the present invention has a total basis weight of 290 g / m 2 or more. The higher the basis weight of paperboard, the greater the elongation on the outer side during bending, making creasing cracks more likely to occur. However, since the paperboard of the present invention is less prone to creasing cracks, it can have a high basis weight. The total basis weight of the paperboard of the present invention is preferably 300 g / m 2 or more, more preferably 350 g / m 2 or more, even more preferably 400 g / m 2 or more, and the upper limit thereof can be, for example, 800 g / m 2 or less.
[0028] The ratio of the basis weight of the surface layer to the total basis weight is preferably 10 mass% or more and 30 mass% or less, more preferably 11 mass% or more and 29 mass% or less, and even more preferably 12 mass% or more and 25 mass% or less, from the viewpoint of burst strength. The ratio of the basis weight of all intermediate layers to the total basis weight is preferably 30% to 50% by mass, and more preferably 35% to 45% by mass, from the viewpoint of preventing cracking along the grid lines. If there are two or more intermediate layers, the basis weight ratio of each intermediate layer may be the same or different. From the viewpoint of bursting strength, the ratio of the basis weight of the backing layer to the total basis weight is preferably 30% to 50% by mass, more preferably 31% to 48% by mass, and even more preferably 32% to 45% by mass. In the present invention, from the viewpoint of bursting strength, it is preferable that the basis weight of the backing layer of the paperboard is greater than that of the fronting layer. It is preferable that the basis weight ratio of the backing layer is 1% by mass or more greater than the basis weight ratio of the fronting layer, and more preferably 5% by mass or more greater.
[0029] The paperboard of the present invention has a creasing rate of 30% or less when evaluated under controlled humidity conditions of 23°C and 50%. This creasing rate is more preferably 1% to 27%, even more preferably 24% or less, even more preferably 21% or less, even more preferably 18% or less, even more preferably 15% or less, even more preferably 13% or less, even more preferably 11% or less, and even more preferably 9% or less.
[0030] The cardboard of the present invention preferably has an IBT interlaminar strength of 20 N·cm or more and 30 N·cm or less, as measured in accordance with JAPAN TAPPI No. 18-2:2000. In cardboard, a strong IBT interlaminar strength is considered desirable, but cardboard with an IBT interlaminar strength of 30 N·cm or less is more prone to inward buckling during folding, which can prevent the occurrence of creasing cracks on the surface. This IBT interlaminar strength is more preferably 29 N·cm or less, even more preferably 28 N·cm or less, even more preferably 27 N·cm or less, even more preferably 26 N·cm or less, and even more preferably 25 N·cm or less.
[0031] The paperboard of the present invention can be suitably used, for example, as a liner for corrugated cardboard, core paper, paperboard for paper containers, paperboard for box making, paperboard for laminated paper, etc. Because the paperboard of the present invention can suppress cracking along the crease lines, it can be particularly suitably used as a liner for corrugated cardboard.
[0032] The paperboard according to the present invention has three or more paper layers, and known manufacturing (papermaking) methods and papermaking machines, such as those using a combination papermaking machine that combines a long wire papermaking machine, a twin wire papermaking machine, a cylinder papermaking machine, a gap former, a hybrid former (on-top former), etc., can be selected. Furthermore, the pH during papermaking can be in the acidic range (acidic papermaking), the pseudo-neutral range (pseudo-neutral papermaking), the neutral range (neutral papermaking), or the alkaline range (alkaline papermaking), and an alkaline agent may be applied to the surface of the paper layers after papermaking in the acidic range.
[0033] In the paperboard of the present invention, since the composition of raw materials such as pulp differs for each layer, a paper stock is prepared according to each layer and then the paper is made. When making the paperboard of the present invention, it is preferable to use a shaking device in the wire section. A shaking device is a device that slides the breast roll of the wire section in a direction perpendicular to the flow direction of the paper stock (also called the machine width direction). By using a shaking device, the basis weight is made uniform (the form is improved), so the number of thin areas compared to other parts that become the starting point of breakage is reduced, and the bursting strength is improved.
[0034] Furthermore, the strength of the paperboard can be improved by adjusting the papermaking conditions of each layer. For example, by setting the J / W ratio (=J / W × 100), which is the ratio of the velocity (J) of the jet liquid (pulp) injected from the headbox to the velocity (W) of the wire, to less than 100%, the jet liquid is pulled by the wire, allowing the pulp to be oriented in the papermaking direction (flow direction). Paperboard in which the pulp is oriented in the longitudinal direction (longitudinal direction) tends to have improved specific burst strength. The J / W ratio is preferably 81% to 99%, and more preferably 84% to 98%. In addition, strength can be improved by changing the basis weight distribution of each layer to increase the basis weight of the surface and / or back layer, or by adjusting the paper strength agent content of each layer to make the paper strength agent content in the surface and / or back layer higher than in the middle layer.
[0035] The manufacturing (papermaking) method and papermaking machine after the wire section are not particularly limited, as long as they do not impair the required strength and production efficiency of the paperboard, and those used in ordinary papermaking machines can be used. The type of press used in the press section of the paper machine is not particularly limited, but any known press device can be used, such as a straight-through press, reverse press, inbar press, twin-bar press, pickup press, UniPress, TriNip press, TriVent press, shoe press, or mini-shoe press. The press conditions are also not particularly limited and can be set appropriately within the normal operating range. However, since increasing the press time makes it easier for hydrogen bonds to form between fibers and improves the strength of the paperboard, it is preferable to manufacture at a low speed within a range that does not impair production efficiency.
[0036] The type of dryer (drying apparatus) in the dryer section process of a paper machine is not particularly limited as long as production efficiency and paperboard strength are not impaired, and known drying apparatuses used in ordinary paper machines, such as a hot air drying system and a multi-cylinder cylinder drying system, can be used. The number of installed drying apparatuses may be one, or two or more including a pre-dryer and an after-dryer may be installed. The drying conditions are also not particularly limited, and can be appropriately set within the normal operation range.
[0037] When a coating layer is provided, a coating liquid containing surface treatment chemicals such as a surface paper strength agent, a surface sizing agent, and a water repellent is applied after paper making. The method for applying the coating liquid is not particularly limited, and known apparatuses such as a two-roll size press, a gate roll coater, a sym-sizer, and a spray can be appropriately used. The calendering step may be bypassed, or the treatment may be performed within the normal operation range. [Examples]
[0038] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not limited only to the following Examples. The paperboards obtained in the following Examples and Comparative Examples were measured by the following methods. The results are shown in Tables 1 to 3. <Pulp freeness> Measured in accordance with JIS P 8121-2:2012. <Basis weight> Measured in accordance with JIS P 8124:2011. <Paper thickness> Measured in accordance with JIS P 8118:2014. <Density> Calculated from the basis weight and the thickness.
[0039] <IBT interlayer strength> Measured in accordance with JAPAN TAPPI No.18-2:2000. <Creasing crack rate (23°C, 50%)> A 5cm square sheet of cardboard sample, conditioned to 23℃ and 50% humidity, was folded in half using a screw servo press (Muto Design Co., Ltd., MSV-10-200S) at a speed of 175mm / min, a pressure of 5.0kN, and a pressing time of 0.3s, with the surface facing outwards and the fold line oriented in the CD direction of the cardboard. The length of the cracked area on the surface of the sample was then measured and divided by the total sample length (5cm) to determine the creasing rate. <Burst strength, specific burst strength> Measurements and calculations were performed in accordance with JIS P 8131:2009. <Print Glossiness> A solid cyan print (size: 2cm high x 3cm wide) was applied to the surface of the prepared cardboard using a flexographic printing press (IGT Testing Systems Co., Ltd., Printability Tester F1). In accordance with JIS Z 8741, the glossiness of the solid cyan printed area after flexographic printing (at a light incidence angle of 75 degrees) was measured using a gloss meter (True GLOSS GM-26PRO, manufactured by Murakami Color Technology Laboratory). Under these conditions, a glossiness of 12.5% or higher is considered desirable after printing. <Print density> One day after flexographic printing as described above, the post-print density was measured using a spectrophotometer (eXact, manufactured by X-Rite). <White area percentage> For the flexographic printed samples described above, a 3.5cm x 15cm print sample image was captured using an Epson GT-X830 printer. The image was then binarized using Media Cybernetics' Image Pro image analysis software, and the number of pixels in the white areas (print defects) was measured by adjusting the threshold.
[0040] • Examples, comparative examples Tables 1-3 show the pulp used for each layer. For mechanical processing of the pulp, a double conifer was used for the surface layer, and a double disc refiner was used for the middle and back layers. The average filtration efficiency (CSF) at the outlets of the double conifer and double disc refiner is shown in each table as the average filtration efficiency (CSF) immediately after mechanical processing. For each layer, a paper strength enhancer (PAM) and a sizing agent (rosin-based) were added to the pulp in the mass percentages shown in each table to create the paper stock. The pulp for each layer was assembled using a multi-layer papermaking machine, and the J / W ratio for the surface layer, middle layer (2 layers), and back layer was set to 90%. In the wire section, a shaking device was activated during the back layer formation to obtain the paperboard.
[0041] [Table 1]
[0042] [Table 2]
[0043] [Table 3]
[0044] ·result The cardboard obtained in the embodiment of the present invention had a low rate of creasing and was less prone to cracking along the creasing lines. Furthermore, it possessed practical bursting strength and printability.
Claims
1. It has a surface layer, one or more middle layers, and a back layer. The average filtration efficiency of the pulp in each layer is 350 ml CSF or higher. It contains 20% or more by mass of hardwood kraft pulp relative to the total pulp mass. The content of internally added drying agent relative to the pulp in each layer is lowest in at least one of the middle layers. The content of the internally added drying agent in the pulp of the surface layer is smaller than the content of the internally added drying agent in the pulp of the back layer. Total basis weight: 290 g / m² 2 That's all. Cardboard characterized by having a creasing rate of 30% or less.
2. The paperboard according to claim 1, characterized in that the content of internally added drying force agent relative to the pulp in each layer is highest in the back layer.
3. The aforementioned surface layer contains 50% to 100% by mass of softwood kraft pulp relative to the total pulp mass. The cardboard according to claim 1, characterized in that the backing layer contains 40% to 100% by mass of hardwood kraft pulp relative to the pulp mass.
4. The paperboard according to claim 1, characterized in that the recycled paper pulp content relative to the pulp mass of the surface layer is 1% by mass or less.
5. The paperboard according to claim 1, characterized in that the content of internally added drying force agent relative to the pulp in each layer satisfies the following conditions. The paper strength agent content of the back layer > the paper strength agent content of the front layer ≥ the paper strength agent content of the middle layer with the lowest paper strength agent content.
6. A corrugated cardboard liner characterized by having the cardboard described in any one of claims 1 to 5.
Citation Information
Patent Citations
Cardboard
JP2024090387A
Liner for corrugated cardboard
JP2024129342A
JPP7323113B
Liner for cardboard and manufacturing method of liner for cardboard
WO2020241417A1