Method for simultaneously manufacturing multiple SiC single crystal substrates

By heat-treating SiC single crystals with a controlled temperature gradient in a firing furnace, the method addresses defects in SiC substrates, enabling efficient production of high-quality multiple SiC single crystal substrates with reduced warpage and dislocations.

JP7954858B2Active Publication Date: 2026-11-20NGK CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2026522610
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-07-29
Filing Date
2025-03-12
Publication Date
2026-11-20
Estimated Expiration
2045-03-12

AI Technical Summary

Technical Problem

Existing methods for manufacturing SiC single crystal substrates face challenges in reducing defects such as basal plane dislocations and warpage, particularly when growing multiple substrates simultaneously, and there is a need for improved productivity while maintaining quality.

Method used

A method involving heat-treating a SiC single crystal and a SiC mixed powder layer containing a liquid phase formation aid in a firing furnace with a controlled temperature gradient, allowing multiple SiC single crystal substrates to be grown with low warpage, low basal plane dislocation density, and large crystal growth thickness.

Benefits of technology

The method enables the simultaneous production of multiple SiC single crystal substrates with reduced warpage, low basal plane dislocation density, and increased crystal growth thickness, enhancing productivity and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954858000004
    Figure 0007954858000004
  • Figure 0007954858000005
    Figure 0007954858000005
  • Figure 0007954858000006
    Figure 0007954858000006
Patent Text Reader

Abstract

Provided is a method capable of simultaneously producing multiple sheets of an SiC single crystal substrate having a small amount of warpage, a low basal plane dislocation density, and a large crystal growth thickness. This method involves: a step for preparing a plurality of containers; a step for arranging, in each of the containers, an SiC single crystal as a seed crystal and SiC powder mixture containing SiC powder and a liquid phase generation aid so as to form an SiC powder mixture layer in which the SiC powder mixture is in contact with at least one plane of the SiC single crystal, wherein the liquid phase generation aid contains an oxide; a step for arranging the containers so as to be aligned with each other in the horizontal direction and / or the vertical direction in a firing furnace; and a step for heating the inside of the firing furnace so as to form a temperature gradient in which the temperature is increased or decreased from an upper portion toward a lower portion to subject the containers containing the seed crystal and the SiC powder mixture to heat treatment at an average furnace temperature of 2240-2560°C, thereby growing the SiC single crystal on the seed crystal.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a method for simultaneously producing a plurality of SiC single crystal substrates.

BACKGROUND ART

[0002] SiC (silicon carbide) has attracted attention as a wide bandgap material capable of controlling high voltage and high power with low loss. Particularly in recent years, power semiconductor devices using SiC materials (SiC power devices) are superior to those using Si semiconductors in miniaturization, low power consumption and high efficiency, and thus their use in various applications is expected. For example, by adopting SiC power devices, it is possible to reduce the size and improve the efficiency of converters, inverters, on-board chargers and the like for electric vehicles (EVs) and plug-in hybrid electric vehicles (PHEVs).

[0003] When manufacturing SiC power devices, a nitrogen-doped low-resistance SiC wafer is used as a base substrate. Low-resistance SiC wafers can generally be produced by a method called the sublimation recrystallization method, but a large thermal gradient is generated in the production furnace, so that thermal strain tends to occur in the crystal, resulting in a problem of high crystal defect density. In addition, when defects, particularly basal plane dislocations called device-killer defects, exist in the SiC wafer, there is a problem that the electric resistance increases during device operation and the device characteristics deteriorate. As methods for reducing defects in wafers, the RAF (Repeated A-Face) method and the solution growth method are known. However, the RAF method has difficulties in increasing the diameter and is high in cost, and the solution growth method has problems such as easy occurrence of inclusions in crystals.

[0004] As another example of a manufacturing method that reduces defects, Patent Document 1 (Japanese Patent No. 4069508) discloses a method for manufacturing a SiC single crystal with a blocked micropipe, characterized by embedding a SiC single crystal in SiC powder and heat-treating it. Furthermore, Patent Document 2 (Japanese Patent No. 7339434) discloses a method for manufacturing a SiC single crystal substrate, which includes the steps of placing a SiC single crystal as a seed crystal and a SiC powder layer in a container in contact with each other, and placing the container in an effective heating zone within a firing furnace, controlled to a temperature range of ±50°C of a set temperature, and performing heat treatment to grow a SiC single crystal on the seed crystal. This manufacturing method is said to be able to produce a SiC single crystal substrate with a low basal plane dislocation density and low warpage because the heat treatment is performed with a smaller temperature gradient. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Patent No. 4069508 [Patent Document 2] Patent No. 7339434 [Overview of the Initiative]

[0006] As mentioned above, although various methods have been considered to reduce defects (dislocations) in SiC single-crystal substrates, further improvements are needed. For example, while Patent Document 1 addresses the reduction of micropipes, it does not involve growing new SiC single crystals on SiC single crystals embedded in SiC powder, and therefore has the problem of not reducing dislocations other than micropipes. Also, while Patent Document 2 can reduce the basal plane dislocation density, it is unclear whether it is possible to grow crystals on multiple substrates simultaneously, and there is no mention of the thickness of the resulting SiC single-crystal substrates. In this regard, in order to improve productivity, it is desirable to be able to grow crystals on a large number of SiC single-crystal substrates while maintaining quality.

[0007] The present inventors have now discovered that by heat-treating a SiC single crystal as a seed crystal and a SiC mixed powder layer containing a liquid phase generation aid in a firing furnace with a predetermined temperature gradient while the two are in contact with each other, it is possible to simultaneously manufacture multiple SiC single crystal substrates with low warping, low basal plane dislocation density, and large crystal growth thickness.

[0008] Therefore, the object of the present invention is to provide a method for simultaneously manufacturing multiple SiC single crystal substrates with small warpage, low basal plane dislocation density, and large crystal growth thickness.

[0009] The following aspects are provided according to this disclosure. [Aspect 1] A method for simultaneously manufacturing multiple SiC single crystal substrates, The process of preparing multiple containers, A step of arranging in each of the plurality of containers a SiC single crystal as a seed crystal and a SiC mixed powder containing SiC powder and a liquid phase formation aid, such that the SiC mixed powder forms a SiC mixed powder layer in contact with at least one surface of the SiC single crystal, wherein the liquid phase formation aid contains an oxide, The process of arranging the plurality of containers in a firing furnace so that they are aligned horizontally and / or vertically to each other, The process involves heating the inside of the firing furnace to form a temperature gradient from top to bottom, where the temperature increases or decreases from top to bottom, and performing heat treatment on the multiple containers containing the seed crystal and the SiC mixed powder at an average furnace temperature of 2240 to 2560°C, thereby growing a SiC single crystal on the seed crystal. Methods that include... [Aspect 2] The method according to embodiment 1, wherein the oxide contains a rare earth element. [Aspect 3] The method according to embodiment 1 or 2, wherein the content of the oxide is 0.5 to 33.0% by weight relative to the content of the SiC powder. [Aspect 4] The method according to any one of embodiments 1 to 3, wherein the average temperature inside the furnace for the heat treatment is 2370 to 2515°C. [Aspect 5] The method according to any one of embodiments 1 to 4, wherein the temperature gradient is 0.01 to 0.40°C / mm. [Aspect 6] The method according to any one of embodiments 1 to 5, wherein a temperature gradient is provided so that the side of the container closer to the seed crystal is at a lower temperature than the side of the container closer to the SiC mixed powder layer, and heat treatment is performed. [Aspect 7] The method according to any one of embodiments 1 to 6, wherein the number of containers is 2 to 80. [Aspect 8] The method according to any one of embodiments 2 to 7, wherein the rare earth element includes at least one selected from the group consisting of Gd, Sm, La, Nd, Y, and Ce. [Aspect 9] The method according to any one of embodiments 1 to 8, wherein a dense body having a relative density of 90% or more is disposed on the bottom surface and / or top surface (excluding the surface in contact with the seed crystal) of the SiC mixed powder layer. [Aspect 10] The method according to any one of embodiments 1 to 9, wherein a dense body with a relative density of 90% or more is arranged on the outer edge of the SiC mixed powder layer. [Aspect 11] The method according to any one of embodiments 1 to 10, wherein a dense material with a relative density of 90% or more is disposed on the bottom surface and / or top surface (excluding the surface in contact with the seed crystal) of the SiC mixed powder layer, and a dense material with a relative density of 90% or more is disposed on the outer edge of the SiC mixed powder layer. [Aspect 12] The method according to any one of embodiments 1 to 11, wherein the firing furnace is equipped with an upper heater at the top of the firing furnace and a lower heater at the bottom of the firing furnace, and during the heat treatment, the upper heater and the lower heater are set to different temperatures to produce the temperature gradient and the average temperature inside the furnace. [Brief explanation of the drawing]

[0010] [Figure 1] This is a schematic cross-sectional view showing one configuration of the arrangement of the SiC mixed powder layer and seed crystals within a container. [Figure 2]FIG. 2 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer and the seed crystal in the container. [Figure 3] FIG. 3 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer and the seed crystal in the container. [Figure 4] FIG. 4 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer and the seed crystal in the container. [Figure 5] FIG. 5 is a schematic cross-sectional view showing one embodiment of the arrangement of the SiC mixed powder layer, the seed crystal and the dense body in the container. [Figure 6] FIG. 6 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer, the seed crystal and the dense body in the container. [Figure 7] FIG. 7 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer, the seed crystal and the dense body in the container. [Figure 8] FIG. 8 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer, the seed crystal and the dense body in the container. [Figure 9] FIG. 9 is a schematic cross-sectional view showing another embodiment of the arrangement of the SiC mixed powder layer, the seed crystal and the dense body in the container. [Figure 10] FIG. 10 is a schematic cross-sectional view showing the configuration of a firing furnace used for crystal growth. [Figure 11] FIG. 11 is a top view of the SiC single crystal substrate 20 for explaining the method for measuring the amount of warpage of the SiC single crystal substrate 20. [Figure 12] FIG. 12 is a schematic cross-sectional view of the SiC single crystal substrate 20 for explaining the method for measuring the amount of warpage of the SiC single crystal substrate 20. [Figure 13] FIG. 13 is a schematic cross-sectional view of the SiC single crystal substrate 20 for explaining the method for measuring the amount of warpage of the SiC single crystal substrate 20. [Mode for Carrying Out the Invention]

[0011] Manufacturing method for SiC single crystal substrates The present invention relates to a method for simultaneously manufacturing multiple SiC single crystal substrates. In this manufacturing method, first, multiple containers are prepared. Then, in each of the multiple containers, a SiC single crystal as a seed crystal and a SiC mixed powder containing SiC powder and a liquid phase formation aid are arranged such that the SiC mixed powder forms a SiC mixed powder layer in contact with at least one face of the SiC single crystal. The liquid phase formation aid contains an oxide. Next, the multiple containers are arranged in a firing furnace so as to be aligned horizontally and / or vertically with respect to each other. Finally, the inside of the firing furnace is heated to form a temperature gradient from top to bottom, and the multiple containers containing the seed crystal and SiC mixed powder are heat-treated at an average furnace temperature of 2240 to 2560°C. This causes the SiC single crystal to grow on the seed crystal. In this way, by heat-treating a SiC single crystal as a seed crystal and a SiC mixed powder layer containing a liquid phase generation aid in a firing furnace with a predetermined temperature gradient while they are in contact with each other, it is possible to simultaneously manufacture multiple SiC single crystal substrates with small warpage, low basal plane dislocation density, and large crystal growth thickness.

[0012] As mentioned above, although various methods have been considered to reduce defects (dislocations) in SiC single-crystal substrates, further improvements are needed. For example, while Patent Document 1 addresses the reduction of micropipes, it does not involve growing new SiC single crystals on SiC single crystals embedded in SiC powder, and therefore has the problem of not reducing dislocations other than micropipes. Also, while Patent Document 2 can reduce the basal plane dislocation density, it is unclear whether it is possible to grow crystals on multiple substrates simultaneously, and there is no mention of the thickness of the resulting SiC single-crystal substrates. In this regard, in order to improve productivity, it is desirable to be able to grow crystals on a large number of SiC single-crystal substrates while maintaining quality. According to the present invention, these problems are conveniently resolved. Specifically, the crystal growth thickness is 50 μm or more, the warpage is 40 μm or less, and the basal plane dislocation density is 100 cm². -2 Multiple SiC single-crystal substrates can be manufactured simultaneously.

[0013] (1) Prepare the container Since the present invention is a method for simultaneously manufacturing multiple SiC single crystal substrates, first, multiple containers for holding seed crystals and SiC mixed powder are prepared. The material of the containers is not particularly limited as long as it does not sublimate or melt at the furnace temperature during heat treatment, but graphite or SiC is preferable. The inner and outer walls of the containers may also be coated. Examples of coating materials include SiC, TiC, TaC, NbC, WC, etc. The shape of the containers is not particularly limited, but as shown in Figure 1, it is preferable to have a container body 2a with an open top and an internal space capable of accommodating seed crystals 4 and SiC mixed powder layers 6, and a container lid 2b that fits into the open top of the container body 2a.

[0014] (2) Arrangement of SiC mixed powder and seed crystal Next, in each of the multiple containers 2, a SiC single crystal as a seed crystal 4 and a SiC mixed powder containing SiC powder and a liquid phase generation aid are arranged such that the SiC mixed powder forms a SiC mixed powder layer 6 in contact with at least one face of the SiC single crystal. The seed crystal 4 is typically composed of a SiC single crystal and has a crystal growth surface. The polymorph (polytype), off-angle and polarity of the SiC single crystal, as well as the type and concentration of dopants that may be included in the SiC single crystal, are not particularly limited, but the polymorph is preferably 4H, 6H, or 3C. Alternatively, a SiC single crystal deposited on a Si substrate may be used as the seed crystal 4. The crystal growth surface on the SiC single crystal as the seed crystal 4 may be the Si face or the C face, or both the Si face and the C face may be present. The diameter of the seed crystal 4 is not particularly limited, but may be 100 mm (4 inches), 150 mm (6 inches), or 200 mm (8 inches).

[0015] The SiC mixed powder layer 6 typically refers to the SiC mixed powder spread in layers within the container 2. The SiC mixed powder is preferably prepared by uniformly mixing the SiC powder and a liquid phase generating agent. This mixing method is not particularly limited as long as the SiC powder and the liquid phase generating agent are uniformly mixed; for example, ball mill mixing or mixer mixing may be used. Furthermore, a dispersant or the like may be added during the mixing of the SiC powder and the liquid phase generating agent to suppress aggregation, etc.

[0016] The SiC powder can be either α-SiC or β-SiC, as long as it serves as a SiC source during crystal growth. There are no particular limitations on the particle size or purity of the SiC powder; any commercially available powder can be used. However, in order to produce a high-purity SiC single crystal substrate, it is desirable that the SiC powder itself be of high purity.

[0017] The liquid phase generating aid is an aid that generates a liquid phase in the heat treatment described later (especially near the crystal growth temperature (e.g., the average temperature inside the furnace)), and it has the function of dissolving SiC particles (SiC powder) by melting itself and generating a liquid phase. The liquid phase generating aid contains an oxide. The oxide contained in the liquid phase generating aid preferably contains a metal element (i.e., in the form of a metal oxide), and more preferably contains a rare earth element. Preferred examples of rare earth elements include Gd, Sm, La, Nd, Y, Ce, and combinations thereof, and more preferably Gd, Sm, La, and combinations thereof. Preferred examples of metal elements other than rare earth elements include Al and Nb. The oxide contained in the liquid phase generating aid may also contain elements other than metal elements, and a preferred example of such an element is Si.

[0018] The oxide content in the liquid phase generating aid is preferably 0.5 to 37.0% by weight, more preferably 0.5 to 33.0% by weight, even more preferably 1.0 to 25.0% by weight, particularly preferably 2.0 to 17.0% by weight, and most preferably 4.0 to 10.0% by weight, relative to the SiC powder content (which is used as the basis for 100% by weight).

[0019] As shown in Figures 1-4, the SiC mixed powder is arranged to form a SiC mixed powder layer 6 that is in contact with at least one surface of a SiC single crystal acting as a seed crystal 4. That is, as long as the seed crystal 4 and the SiC mixed powder layer 6 are in contact with each other, their arrangement is not particularly limited. For example, as shown in Figure 1, the seed crystal 4 may be placed on the inner bottom surface of the container 2 and the SiC mixed powder layer 6 may be placed on top of it, or the seed crystal 4 may be embedded in the SiC mixed powder layer 6 inside the container 2 as shown in Figure 2. Alternatively, as shown in Figure 3, the seed crystal 4 may be placed on the upper surface of the SiC mixed powder layer 6 placed on the inner bottom surface of the container 2. Furthermore, multiple seed crystals 4 may be placed inside one container 2 as long as the seed crystal 4 and the SiC mixed powder layer 6 are in contact. In addition, as shown in Figure 4, as long as the seed crystal 4 and the SiC mixed powder layer 6 are in contact, a lateral space may be provided so that the sides (outer edges) of the seed crystal 4 and the SiC mixed powder layer 6 are not in contact with the inner wall of the container 2. The method for filling container 2 with the SiC mixed powder is not particularly limited and can be carried out by known methods such as press filling or vibration filling.

[0020] As shown in Figures 5-7, a dense body 8 may be placed on the bottom and / or top surface of the SiC mixed powder layer 6 (excluding the surface in contact with the seed crystal 4). By placing the dense body 8 in this way, it is possible to prevent impurities from entering from the inner bottom surface of the container 2 and / or the container lid 2b, and to grow a higher purity SiC single crystal. For example, if the seed crystal 4 is not placed on the top surface of the SiC mixed powder layer 6, the dense body 8 may be placed on the top surface of the SiC mixed powder layer 6 as shown in Figure 5. If the seed crystal 4 is not placed on the inner bottom surface of the container 2, the dense body 8 may be placed between the SiC mixed powder layer 6 and the inner bottom surface of the container 2 as shown in Figure 6. If the seed crystal 4 is embedded in the SiC mixed powder layer 6, the dense body 8 may be placed on the top surface of the SiC mixed powder layer 6 and / or between the SiC mixed powder layer 6 and the inner bottom surface of the container 2 as shown in Figure 7.

[0021] As shown in Figures 8 and 9, a dense body 8 may be arranged around the outer edge of the SiC mixed powder layer 6. By arranging the dense body 8 in this way, impurities can be prevented from entering from the side of the container 2, and a higher purity SiC single crystal can be grown. For example, as shown in Figure 8, the dense body 8 may be arranged between the outer edge of the SiC mixed powder layer 6 and the inner wall of the container 2. In this case, it is preferable that the dense body 8 is in contact with at least the outer edge of the SiC mixed powder layer 6. In particular, as shown in Figure 9, it is preferable that the dense body 8 is arranged on the bottom surface and / or top surface of the SiC mixed powder layer 6 (excluding the surface in contact with the seed crystal 4), and that the dense body 8 is arranged around the outer edge of the SiC mixed powder layer 6.

[0022] The dense body 8 is preferably a solid with a relative density of 90% or more, more preferably 95% or more, and even more preferably 99% or more. The higher the relative density, the more effectively impurities can be prevented from entering. The relative density can be determined, for example, by dividing the bulk density of the dense body measured by the Archimedes method by the theoretical density of the dense body and multiplying the result by 100. The dense body 8 is not particularly limited as long as it does not sublimate or melt at the furnace temperature during heat treatment and does not react with SiC. Examples of materials for such a dense body 8 include polycrystalline carbides such as TiC, TaC, NbC, and WC, and nitrides such as Si3N4 and TiN. The shape of the dense body 8 is not particularly limited, but it is preferably layered.

[0023] (3) Placement of multiple containers inside the firing furnace As described above, a plurality of containers 2, each containing a SiC mixed powder layer 6, a seed crystal 4, and optionally a dense body 8, are arranged in a firing furnace 10 so as to be aligned horizontally and / or vertically to one another. From the viewpoint of improving productivity, it is desirable to have a large number of containers 2 arranged in the firing furnace 10. Therefore, it is preferable that the number of containers 2 be 2 or more, more preferably 2 to 80, even more preferably 15 to 80, and particularly preferably 50 to 80, for example, 2 to 15 or 15 to 50. More specifically, when a plurality of containers 2 are arranged vertically (for example, stacked), the number of containers 2 arranged vertically is preferably 2 to 30, more preferably 5 to 30, even more preferably 10 to 30, and particularly preferably 20 to 30, for example, 2 to 5, 5 to 10, or 10 to 20. When multiple containers 2 are arranged horizontally, individually and / or as a set of vertically arranged containers 2, the number of containers 2 and / or sets arranged horizontally is preferably 2 to 10, more preferably 4 to 10, even more preferably 6 to 10, and particularly preferably 8 to 10, for example, 2 to 4, 4 to 6, or 6 to 8. The firing furnace 10 preferably includes an upper heater 12 located at the top of the firing furnace 10, a lower heater 14 located at the bottom of the firing furnace 10, a base 16 for placing the multiple containers 2, and a gas pipe 18 for supplying gas G into the firing furnace 10, as shown in Figure 10. With this configuration, in the subsequent heat treatment process, a temperature gradient can be effectively formed inside the firing furnace 10, where the temperature increases or decreases from top to bottom.

[0024] (4) Heat treatment After placing multiple containers 2 inside the firing furnace 10, the furnace 10 is heated to form a temperature gradient from top to bottom, where the temperature increases or decreases from top to bottom. The multiple containers 2 containing the seed crystals 4 and the SiC mixed powder layer 6 are then heat-treated at an average furnace temperature of 2240 to 2560°C, thereby growing SiC single crystals on the seed crystals 4. At this time, as shown in Figure 10, it is preferable that the firing furnace 10 is equipped with an upper heater 12 at the top and a lower heater 14 at the bottom, and that the upper heater 12 and the lower heater 14 are set to different temperatures during heat treatment to produce the above temperature gradient and average furnace temperature. When heating to form a temperature gradient from top to bottom, the lower heater 14 should be set to a higher temperature than the upper heater 12. Conversely, if heating is required to create a temperature gradient where the temperature decreases from the top to the bottom of the firing furnace 10, the set temperature of the lower heater 14 should be lower than the set temperature of the upper heater 12.

[0025] It is preferable to place the container 2 in the effective heating zone of the firing furnace 10. Here, "effective heating zone" refers to "the charging area in a heat treatment apparatus that can keep a metal product within a temperature tolerance range according to the purpose of heat treatment," as defined by JIS B 6905:1995. The effective heating zone temperature of the firing furnace 10 can be controlled by adjusting the heater output of the upper heater 12 and lower heater 14 provided in the firing furnace 10. This makes it possible to vary the upper and lower temperatures of the heating area in the firing furnace 10 and create a unidirectional temperature gradient within the firing furnace 10.

[0026] The temperature gradient is preferably 0.01 to 0.40°C / mm, more preferably 0.05 to 0.30°C / mm, and even more preferably 0.08 to 0.14°C / mm. It is also preferable to perform the heat treatment with a temperature gradient such that the side of the container 2 closer to the seed crystal 4 is at a lower temperature than the side of the container 2 closer to the SiC mixed powder layer 6. For example, when heating to form a temperature gradient in which the temperature increases from the top to the bottom of the firing furnace 10, the seed crystal 4 should be placed on the SiC mixed powder layer 6 inside the container 2. Conversely, when heating to form a temperature gradient in which the temperature decreases from the top to the bottom of the firing furnace 10, the SiC mixed powder layer 6 should be placed on the seed crystal 4 inside the container 2.

[0027] The average furnace temperature for heat treatment is 2240 to 2560°C, preferably 2370 to 2515°C, more preferably 2390 to 2480°C, and even more preferably 2410 to 2450°C. The average furnace temperature can be determined as the average of the highest and lowest temperatures in the effective heating zone within the firing furnace 10. Typically, the ambient temperature near the bottom and near the top of the effective heating zone within the firing furnace 10 can be measured, and the average of these ambient temperatures can be adopted as the average furnace temperature. The holding time at the above average furnace temperature is not particularly limited, as the longer the holding time, the thicker the SiC single crystal can be grown, so the holding time can be set according to the desired thickness. The heat treatment may be performed under atmospheric pressure or under pressure, such as in a hot press.

[0028] The firing furnace 10 used for heat treatment is not particularly limited as long as SiC crystal growth occurs on the seed crystal 4, and may be any known firing furnace such as a resistance furnace, arc furnace, or induction furnace. The atmosphere inside the firing furnace 10 during firing is preferably a vacuum, nitrogen, an inert gas, or a mixture of nitrogen and an inert gas. The material and resistivity of the heaters 12 and 14 are not particularly limited, but it is desirable that they be made of graphite.

[0029] (5) Polishing After growing a SiC single crystal on the seed crystal 4 in this manner, it is preferable to polish the surface of the SiC single crystal. For example, a desired SiC single crystal substrate can be obtained by polishing with diamond abrasive grains followed by chemical mechanical polishing (CMP). [Examples]

[0030] The present invention will be further described in detail by the following examples. However, the present invention is not limited to the following examples.

[0031] Example 1 (1) Preparation of SiC mixed powder Commercially available β-SiC powder (volume-based D50 particle size: 65.0 μm) and an oxide (Gd2O3) (volume-based D50 particle size: 5.0 μm), which is a liquid phase formation aid, were weighed so that the oxide content relative to the SiC powder content was 8.1% by weight. These were then placed in a polypropylene container along with pebbles and water. After placing the polypropylene container on a pot stand, the container was rotated at a speed of 50 rpm to mix the raw materials. The slurry obtained by mixing the raw materials was dried in a dryer and recovered to obtain a SiC mixed powder.

[0032] (2) Arrangement of SiC mixed powder and SiC single crystal The SiC mixed powder obtained in (1) above was filled into a graphite container and tapped to level the SiC mixed powder so that the outermost layer was visually flat. A commercially available SiC single crystal substrate (4H-SiC, 150 mm (6 inches) in diameter, 4° off-angle, 0.35 mm thick) was placed on the SiC mixed powder so that only the Si side of the seed crystal was in contact with the powder. The graphite container was closed with a graphite lid to form a graphite sheath. Several such graphite sheaths (a total of four in this example) were prepared.

[0033] (3) Placement of multiple graphite stalks inside the resistance furnace Two of the graphite pods prepared in (2) above were placed vertically within the effective heating zone of the firing furnace (resistance furnace) via 5 mm thick graphite spacers, and then two of these were placed horizontally. This resulted in a total of four graphite pods being placed inside the furnace.

[0034] (4) Heat treatment By adjusting the heater output, a temperature gradient of 0.11°C / mm was created inside the firing furnace, with the temperature increasing from top to bottom. The furnace was then heated in an argon atmosphere at an average temperature of 2430°C for 20 hours, thereby heat-treating all the graphite sacs. As a result, SiC single-crystal substrates were obtained, in which SiC single crystals were grown on seed crystals inside all the graphite sacs.

[0035] (5) Measurement of crystal growth thickness of SiC single crystal substrate The thickness of 25 arbitrary locations on the SiC single crystal substrate obtained in (4) above was measured with a micrometer, and the arithmetic mean was calculated. Similarly, the thickness of the seed crystal was also calculated at the time of (2) above. Then, the crystal growth thickness (μm) was calculated by subtracting the arithmetic mean of the seed crystal thickness from the arithmetic mean of the SiC single crystal substrate thickness. It was confirmed that the crystal growth thickness of all four SiC single crystal substrates was 100 μm or more.

[0036] Of all the SiC single crystal substrates whose crystal growth thickness was determined using the method described above, the SiC single crystal substrate with the smallest crystal growth thickness was evaluated according to the evaluation criteria shown below. The results are shown in Table 3. <Evaluation Criteria> - Evaluation A: The SiC single crystal substrate with the smallest crystal growth thickness has a crystal growth thickness of 100 μm or more. - Evaluation B: The SiC single crystal substrate with the smallest crystal growth thickness has a crystal growth thickness of 50 μm or more and less than 100 μm. - Evaluation C: The SiC single crystal substrate with the smallest crystal growth thickness has a crystal growth thickness of less than 50 μm.

[0037] (6) Polishing The obtained SiC single crystals were polished using diamond abrasives, and then finished with chemical mechanical polishing (CMP).

[0038] (7) Measurement of warpage of SiC single crystal substrate The amount of warpage was measured on the polished surface of all the SiC single crystal substrates obtained in (6) above using a high-precision laser measuring instrument (LT-9010M manufactured by Keyence Corporation). As shown in Figure 11, in the planar view of the surface of the SiC single crystal substrate 20 (SiC single crystal 30), two mutually orthogonal lines X and Y were drawn passing through point G, which is the centroid of the planar view. Two points A and B were defined on line X, 70 mm away from point G, and two points C and D were defined on line Y, 70 mm away from point G. Next, as shown in Figure 12, point P on the curve AB between points A and B on the surface of the SiC single crystal substrate 20 (SiC single crystal 30) was determined such that the longest line segment was obtained by extending a line segment perpendicular to line segment AB from any point on the curve AB (for example, in Figure 12, any point on the curve AB could be point P or point O, but the longest line segment obtained by extending a line segment perpendicular to line segment AB from each of these points is the one extended from point P). The distance between line segment AB and point P was then defined as the amount of curvature α. Furthermore, as shown in Figure 13, point R on the curve CD between points C and D on the surface of the SiC single crystal substrate 20 (SiC single crystal 30) was determined such that the longest distance of a line segment extended perpendicular to the line segment CD was obtained from any point on the curve CD (for example, in Figure 13, any point on the curve CD could be point R or point O, but the longest line segment extended perpendicular to the line segment CD from each of these points is the one extended from point R). The distance between the line segment CD and point R was defined as the warp amount β. The average of these warps α and β was defined as the warp amount of the SiC single crystal substrate.

[0039] Of all the SiC single crystal substrates whose warpage was determined using the method described above, the one with the largest warpage was graded according to the evaluation criteria shown below. The results are shown in Table 3. <Evaluation Criteria> - Evaluation A: The warpage of the SiC single crystal substrate with the greatest warpage is 30 μm or less. - Evaluation B: The SiC single crystal substrate with the greatest warpage has a warpage of more than 30 μm but is 40 μm or less. - Evaluation C: The SiC single crystal substrate with the greatest warpage has a warpage exceeding 40 μm.

[0040] (8) Measurement of basal plane dislocation density of SiC single crystal substrate All the SiC single crystal substrates obtained in (6) above were placed in a nickel crucible together with the KOH crystal. This crucible was etched in an electric furnace at 500°C for 10 minutes. After etching, the sample (SiC single crystal substrate) was cleaned, and its surface was observed with an optical microscope to determine the types of defects from the shape of the pits. Of these, the number of basal plane dislocations was measured, and the number of basal plane dislocations (number of) was measured over the area (cm²) of the observation region. 2 By dividing by ), the basal plane dislocation density (cm -2 The total number of basal dislocations was calculated by taking 100 field images of a 2.8 mm x 3.6 mm field of view at 20x magnification for any location on the sample surface. This total was then used to calculate the total area of ​​the 100 field images, which is 10.1 cm². 2 The basal dislocation density was calculated by dividing by [a certain factor].

[0041] Of all the SiC single crystal substrates for which the basal plane dislocation density was determined using the method described above, the SiC single crystal substrate with the highest basal plane dislocation density was evaluated according to the evaluation criteria shown below. The results are shown in Table 3. <Evaluation Criteria> - Evaluation A: The SiC single crystal substrate with the highest basal plane dislocation density has a basal plane dislocation density of 80 cm⁻¹. -2 below - Evaluation B: The SiC single crystal substrate with the highest basal plane dislocation density has a basal plane dislocation density of 80 cm⁻¹. -2 Over 100cm -2 below - Evaluation C: The SiC single crystal substrate with the highest basal plane dislocation density has a basal plane dislocation density of 100 cm². -2 exceed

[0042] Example 2 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 16.2% by weight; (ii) in (2) above, a dense polycrystalline TaC body (relative density of 90% or more) was placed at the bottom and outer edge of the graphite container; (iii) in (3) above, three graphite sheaths were placed horizontally and five vertically in the firing furnace; and (iv) in (4) above, a temperature gradient of 0.17°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2445°C.

[0043] Example 3 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 32.4% by weight; (ii) in (2) above, a dense polycrystalline TaC body (relative density of 90% or more) was placed on the outer edge of the graphite container; (iii) in (3) above, three graphite sheaths were placed horizontally and 25 vertically inside the firing furnace; and (iv) in (4) above, a temperature gradient of 0.06°C / mm was formed inside the firing furnace so that the temperature increased from top to bottom, and the furnace was heated at an average temperature of 2490°C.

[0044] Example 4 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 4.1% by weight; (ii) in (3) above, 10 graphite scabbards were placed horizontally and 5 vertically in the firing furnace; and (iii) in (4) above, a temperature gradient of 0.28°C / mm was formed inside the firing furnace so that the temperature increased from top to bottom, and the furnace was heated at an average temperature of 2450°C. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0045] Example 5 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 2.0% by weight; (ii) in (2) above, a dense polycrystalline TaC body (relative density of 90% or more) was placed at the bottom of a graphite container; (iii) in (3) above, two graphite sheaths were placed horizontally and 30 vertically in the firing furnace; and (iv) in (4) above, a temperature gradient of 0.01°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2508°C.

[0046] Example 6 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 1.0% by weight; (ii) in (2) above, a dense polycrystalline TaC body (relative density of 90% or more) was placed at the bottom of a graphite container; (iii) in (3) above, seven graphite sheaths were arranged horizontally and ten graphite sheaths vertically in the firing furnace; and (iv) in (4) above, a temperature gradient of 0.12°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2445°C.

[0047] Example 7 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 0.8% by weight; (ii) in (2) above, a TaC polycrystalline dense body (relative density of 90% or more) was placed at the bottom of a graphite container; (iii) in (3) above, one graphite sheath was placed horizontally and two graphite sheaths vertically in the firing furnace; and (iv) in (4) above, a temperature gradient of 0.14°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2375°C.

[0048] Example 8 Except for the following, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1: (i) in (1) above, the oxide content relative to the SiC powder content was set to 24.3% by weight; (ii) in (2) above, a dense polycrystalline TaC body (relative density of 90% or more) was placed at the bottom and outer edge of the graphite container; (iii) in (3) above, two graphite sheaths were placed horizontally and one vertically in the firing furnace; and (iv) in (4) above, a temperature gradient of 0.21°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2463°C.

[0049] Example 9 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, and SiC mixed powder was filled on top of it. (ii) In (4) above, the inside of the firing furnace was heated to create a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0050] Example 10 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, and a TaC polycrystalline dense material (relative density of 90% or more) was placed around the outer edge of the graphite container, then SiC mixed powder was filled on top of it, and then another TaC polycrystalline dense material (relative density of 90% or more) was placed on top of the powder layer. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was manufactured and evaluated in the same manner as in Example 2. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0051] Example 11 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, and a dense polycrystalline TaC body (relative density of 90% or more) was placed around the outer edge of the graphite container, and then SiC mixed powder was filled on top of it. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 3. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0052] Example 12 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, and SiC mixed powder was filled on top of it. (ii) In (4) above, the inside of the firing furnace was heated to create a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 4. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0053] Example 13 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, SiC mixed powder was packed on top of it, and a TaC polycrystalline dense material (relative density of 90% or more) was placed on top of the powder layer. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 5. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0054] Example 14 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, SiC mixed powder was packed on top of it, and a TaC polycrystalline dense material (relative density of 90% or more) was placed on top of the powder layer. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 6. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0055] Example 15 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, SiC mixed powder was packed on top of it, and a TaC polycrystalline dense material (relative density of 90% or more) was placed on top of the powder layer. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 7. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0056] Example 16 (i) In (2) above, a commercially available SiC single crystal substrate to be used as a seed crystal was placed at the bottom of a graphite container with the Si surface of the substrate facing upward, and a TaC polycrystalline dense material (relative density of 90% or more) was placed around the outer edge of the graphite container, then SiC mixed powder was filled on top of it, and then another TaC polycrystalline dense material (relative density of 90% or more) was placed on top of the powder layer. (ii) In (4) above, the inside of the firing furnace was heated to form a temperature gradient from top to bottom, except that the SiC single crystal substrate was manufactured and evaluated in the same manner as in Example 8. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0057] Example 17 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1, except that Sm2O3 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0058] Example 18 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1, except that La2O3 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0059] Example 19 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1, except that Nd2O3 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0060] Example 20 Except for (i) using Y2O3 as the oxide liquid phase formation aid in (1) above, and (ii) placing a dense polycrystalline TaC body (relative density of 90% or more) at the bottom of a graphite container in (2) above, the SiC single crystal substrate was prepared and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0061] Example 21 Except for (i) using CeO2 as the oxide for the liquid phase formation aid in (1) above, and (ii) placing a dense polycrystalline TaC body (relative density of 90% or more) at the bottom of a graphite container in (2) above, the SiC single crystal substrate was prepared and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0062] Example 22 In (2) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1, except that the SiC mixed powder was filled into a graphite container to about half its capacity, the powder was leveled, a commercially available SiC single crystal substrate to serve as a seed crystal was placed on top of the powder, and then the seed crystal was embedded by adding more SiC mixed powder to the substrate. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0063] Example 23 Except for (i) using Sm2O3 as the oxide for the liquid phase formation aid in (1) above, and (ii) placing a dense polycrystalline TaC body (relative density of 90% or more) at the bottom of the graphite container and on the upper surface of the powder layer in (2) above, the SiC single crystal substrate was prepared and evaluated in the same manner as in Example 22. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0064] Example 24 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 4, except that Al2O3 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0065] Example 25 Except for (i) using Al2O3 as the oxide for the liquid phase formation aid in (1) above, and (ii) further placing a dense polycrystalline TaC body (relative density of 90% or more) on the outer edge of the graphite container in (2) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 7. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0066] Example 26 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 5, except that Al2O3 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0067] Example 27 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 4, except that Nb2O5 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0068] Example 28 Except for (i) using Nb2O5 as the oxide for the liquid phase formation aid in (1) above, and (ii) further placing a dense polycrystalline body of TaC (relative density of 90% or more) on the outer edge of the graphite container in (2) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 7. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0069] Example 29 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 5, except that Nb2O5 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0070] Example 30 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 4, except that SiO2 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0071] Example 31 Except for (i) using SiO2 as the oxide for the liquid phase formation aid in (1) above, and (ii) further placing a dense polycrystalline TaC body (relative density of 90% or more) on the outer edge of the graphite container in (2) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 7. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0072] Example 32 In (1) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 5, except that SiO2 was used as the oxide for the liquid phase formation aid. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0073] Example 33 (comparison) In (4) above, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1, except that a temperature gradient was not formed (i.e., the temperature of the upper and lower parts of the effective heating zone was made approximately the same) and the furnace was heated at an average temperature of 2450°C. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0074] Example 34 In (4) above, a temperature gradient of 0.36°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2450°C. Except for these differences, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0075] Example 35 In (1) above, the SiC single crystal substrate was prepared and evaluated in the same manner as in Example 1, except that the oxide content relative to the SiC powder content was set to 36.5% by weight. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0076] Example 36 In (4) above, a temperature gradient of 0.06°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2550°C. Except for these differences, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0077] Example 37 (comparison) In (1) above, the SiC single crystal substrate was prepared and evaluated in the same manner as in Example 1, except that a liquid phase formation aid was not added, i.e., commercially available β-SiC powder (volume-based D50 particle size: 65.0 μm) was used instead of SiC mixed powder. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0078] Example 38 In (4) above, a temperature gradient of 0.28°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2250°C. Except for these differences, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0079] Example 39 (comparison) In (4) above, a temperature gradient of 0.14°C / mm was formed inside the firing furnace so that the temperature increased from the top to the bottom, and the furnace was heated at an average temperature of 2225°C. Except for these differences, the SiC single crystal substrate was fabricated and evaluated in the same manner as in Example 1. The evaluation results for the crystal growth thickness, warpage, and basal plane dislocation density of the obtained substrate are shown in Table 3.

[0080] [Table 1]

[0081] [Table 2]

[0082] [Table 3]

[0083] From the results of Examples 1-32, 34-36, and 38, it was found that by heat-treating a SiC single crystal as a seed crystal and a SiC mixed powder layer containing a liquid phase formation aid in a firing furnace with a predetermined temperature gradient (preferably in the effective heating zone) while they are in contact with each other, it is possible to simultaneously produce multiple SiC single crystal substrates with small warpage, low basal plane dislocation density, and large crystal growth thickness, although the reason for this is unknown. On the other hand, from the results of Examples 33, 37, and 39 (comparison), it was found that high-quality SiC single crystal substrates cannot be obtained if a temperature gradient is not formed, if a liquid phase formation aid is not added, or if the average temperature inside the furnace is not controlled. [Explanation of Symbols]

[0084] 2 containers 2a Container body 2b Container lid 4 seed crystals 6 SiC mixed powder layer 8 Dense body 10. Firing furnace 12. Top heater 14. Lower heater 16 bases 18 Gas pipes 20 SiC single crystal substrates 30 SiC single crystals G Gas

Claims

1. A method for simultaneously manufacturing multiple SiC single crystal substrates, The process of preparing multiple containers, A step of arranging in each of the plurality of containers a SiC single crystal as a seed crystal, and a SiC mixed powder containing SiC powder and a liquid phase formation aid, such that the SiC mixed powder forms a SiC mixed powder layer in contact with at least one surface of the SiC single crystal, wherein the liquid phase formation aid contains an oxide, The steps include arranging the plurality of containers in a firing furnace so that they are aligned horizontally and / or vertically to each other, The process involves heating the inside of the firing furnace to form a temperature gradient from top to bottom, where the temperature increases or decreases from top to bottom, and performing heat treatment on the plurality of containers containing the seed crystal and the SiC mixed powder at an average furnace temperature of 2240 to 2560°C, thereby growing a SiC single crystal on the seed crystal. Includes, The temperature gradient is 0.01 to 0.40°C / mm. A method of performing heat treatment by providing a temperature gradient such that the side of the container closer to the seed crystal is at a lower temperature than the side of the container closer to the SiC mixed powder layer.

2. The method according to claim 1, wherein the oxide contains a rare earth element.

3. The method according to claim 1 or 2, wherein the content of the oxide is 0.5 to 33.0% by weight relative to the content of the SiC powder.

4. The method according to claim 1 or 2, wherein the average temperature inside the furnace for the heat treatment is 2370 to 2515°C.

5. The method according to claim 1 or 2, wherein the number of containers is 2 to 80.

6. The method according to claim 2, wherein the rare earth element comprises at least one selected from the group consisting of Gd, Sm, La, Nd, Y, and Ce.

7. The method according to claim 1 or 2, wherein a dense body having a relative density of 90% or more is disposed on the bottom surface and / or top surface (excluding the surface in contact with the seed crystal) of the SiC mixed powder layer.

8. The method according to claim 1 or 2, wherein a dense body with a relative density of 90% or more is disposed on the outer edge of the SiC mixed powder layer.

9. The method according to claim 1 or 2, wherein a dense material having a relative density of 90% or more is disposed on the bottom surface and / or top surface (excluding the surface in contact with the seed crystal) of the SiC mixed powder layer, and a dense material having a relative density of 90% or more is disposed on the outer edge of the SiC mixed powder layer.

10. The method according to claim 1 or 2, wherein the firing furnace is provided with an upper heater at the top of the firing furnace and a lower heater at the bottom of the firing furnace, and during the heat treatment, the upper heater and the lower heater are set to different temperatures to produce the temperature gradient and the average temperature inside the furnace.

Citation Information

Patent Citations

  • Method for growing SiC crystal by low-temperature solution method

    CN116145258A

  • METHOD OF PRODUCING SiC SINGLE CRYSTAL

    JP2004323293A

  • METHOD FOR MANUFACTURING SINGLE CRYSTAL SiC FILM

    JP2009155140A

  • METHOD OF PRODUCING SiC SINGLE CRYSTAL

    JP2012046384A

  • Method for producing silicon carbide single crystal

    JP4069508B2