Coated white cardboard
A two-layered calcium carbonate structure in coated white cardboard addresses uneven whiteness and dust issues, enhancing printability and appearance while maintaining environmental and cost efficiency, using recycled pulp and optional colorants.
Patent Information
- Application Number
- JP2026551827
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2025-06-13
- Filing Date
- 2026-06-04
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-06-04
AI Technical Summary
The increasing use of recycled pulp in coated white cardboard leads to issues such as uneven whiteness, visible dust, and foreign matter, while excessive pigment coating can cause cracking, and high-opaque pigments like kaolin are costly and ineffective in enhancing whiteness.
A coated white paperboard with two pigment coating layers, using calcium carbonate with different average particle diameters in each layer, and incorporating recycled pulp to maintain environmental impact and cost efficiency, with optional blue and/or purple colorants for improved appearance.
The solution provides coated white cardboard with good appearance and printability, including ink drying properties, despite using high recycled pulp content, by optimizing calcium carbonate particle sizes and layering structure.
Smart Images

Figure 0007954867000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to coated white cardboard having a pigment coating layer. [Background technology]
[0002] The base paper for coated white cardboard is typically manufactured using a multi-layer process. The top layer often uses expensive bleached chemical pulp with high whiteness, while the sub- and middle layers often use inexpensive deinked and undeinked recycled paper pulp, which has lower whiteness compared to bleached chemical pulp. Bleached chemical pulp is used for the top layer to suppress unevenness in whiteness on the surface of coated white cardboard and to make foreign matter such as dust contained in recycled paper pulp less visible from the surface. Recycled paper pulp is used for the sub- and middle layers for environmental reasons and cost reduction.
[0003] In recent years, due to increasing demands for environmental protection and cost reduction, the use of recycled pulp in the base paper of coated white cardboard has been increasing. Consequently, problems such as uneven whiteness and visible dust and other foreign matter on the surface of coated white cardboard are becoming more prevalent. Furthermore, increasing the use of recycled pulp tends to lower the whiteness of the base cardboard before coating.
[0004] To address these challenges, techniques have been proposed to improve the coverage of the base paper by increasing the amount of pigment coating layer applied, to remove foreign matter such as dust and residual substances from recycled paper pulp and reduce the number of dust particles to below a specific value (Patent Document 1), and to use a large amount of highly opaque pigments such as kaolin (Patent Document 2). [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2020-133015 [Patent Document 2] Japanese Patent Application Publication No. 6-166991 [Overview of the Initiative] Problem to be Solved by the Invention
[0006] However, if the coating amount is excessively increased, problems such as easy cracking of the coating layer may occur. In addition, the technique for enhancing the removal of foreign matter such as dust and residual substances in Patent Document 1 has a problem that the yield of waste paper pulp deteriorates as the treatment is intensified. Furthermore, pigments with high hiding power such as kaolin used in Patent Document 2 are expensive and thus disadvantageous in terms of cost. Moreover, since pigments such as kaolin have low whiteness of the pigment itself, the effect of increasing the whiteness of the pigment coating layer is insignificant even if the decrease in whiteness derived from the base paper can be suppressed.
[0007] Accordingly, an object of the present invention is to provide a coated white paperboard that has both printability such as ink drying property and good appearance, even when using a base paper with an increased blending ratio of low-whiteness waste paper and reduced environmental load. Means for Solving the Problem
[0008] As a result of intensive studies to achieve the above object, the present inventors have completed the present invention by providing two pigment coating layers on the surface of a base paper containing waste paper pulp, and using calcium carbonate having different average particle diameters in each layer.
[0009] The present invention provides the following. (1) A coated white paperboard having a white paper glossiness of 50% or less, which has two pigment coating layers on at least the surface layer side of a multilayer base paper having a surface layer, a lower surface layer, a middle layer and a back layer, wherein all layers of the multilayer base paper contain waste paper pulp, and among the pigment coating layers, the precoat layer adjacent to the base paper contains 80 parts by weight or more of calcium carbonate having an average particle diameter of more than 1.2 μm in 100 parts by weight of the pigment contained in the precoat layer, and among the pigment coating layers, the topcoat layer provided on the outer side contains 80 parts by weight or more of calcium carbonate having an average particle diameter of 1.2 μm or less in 100 parts by weight of the pigment contained in the topcoat layer. (2) The coated white paperboard according to (1), wherein the surface layer contains 50% by weight or more of deinked waste paper pulp in 100% by weight of pulp. (3) The coated white cardboard according to (1), wherein the surface layer and / or subsurface layer contains 1 to 30% by weight of calcium carbonate relative to 100% by weight of the pulp in each layer. (4) The coated white cardboard according to (1) or (2), wherein the top coat layer contains a blue and / or purple colorant. (5) b measured with a light source including ultraviolet light in accordance with JIS P 8150 * Coated white cardboard according to (1) or (2), wherein the value is 0 or less. (6) The coated white cardboard according to (1) or (2), wherein both the top coat layer and the pre coat layer contain 12 parts by weight or less of latex per 100 parts by weight of pigment contained in each layer. [Effects of the Invention]
[0010] According to the present invention, even when using a base paper with a reduced environmental impact due to a higher proportion of recycled paper with low whiteness, it is possible to provide coated white cardboard that combines printability such as ink drying properties with a good appearance. [Modes for carrying out the invention]
[0011] The present invention will now be described in detail. In this invention, "~" includes the endpoints. That is, "X~Y" includes the values X and Y at both ends.
[0012] The coated white cardboard of the present invention is a coated white cardboard with a white gloss of 50% or less, having two pigment coating layers on at least the surface side of a multilayer base paper having a surface layer, a subsurface layer, a middle layer, and a back layer, wherein all layers of the multilayer base paper contain recycled pulp, and of the pigment coating layers, the pre-coat layer provided on the surface of the surface layer contains 80 parts by weight or more of calcium carbonate with an average particle size of more than 1.2 μm in 100 parts by weight of pigment contained in the pre-coat layer, and of the pigment coating layers, the topcoat layer provided on the surface of the pre-coat layer contains 80 parts by weight or more of calcium carbonate with an average particle size of 1.2 μm or less in 100 parts by weight of pigment contained in the topcoat layer.
[0013] (Coated white cardboard) The coated white cardboard of the present invention has at least two pigment coating layers on the surface side of a multilayer base paper having a surface layer, a subsurface layer, a middle layer, and a back layer.
[0014] (base paper) The base paper is typically a thick cardboard consisting of a multilayer base paper structure of 2 to 9 layers. In the present invention, from the viewpoint of obtaining high basis weight and paper thickness, and from the viewpoint of imparting various functionalities to each layer, a multilayer base paper structure having a surface layer, a subsurface layer, a middle layer, and a back layer is adopted, and the middle layer may consist of two or more layers.
[0015] In the coated white cardboard of the present invention, the base paper is preferably made by multi-layering four or more pulp layers (paper layers) consisting of a surface layer, a subsurface layer, a middle layer, and a back layer. The number of layers in the base paper is four or more, preferably six or more and ten or less. The outermost paper layers of the base paper are called the surface layer and the back layer, the second layer from the surface layer toward the back layer is called the subsurface layer, and the inner layer adjacent to the subsurface layer is called the middle layer. The middle layer may be one layer or a multi-layered layer of two or more. The base paper used in the present invention may also have a subsurface layer adjacent to the back layer between the middle layer and the back layer.
[0016] The base paper used in the present invention can be any paper commonly used for coated white cardboard, but from the viewpoint of reducing environmental impact and costs, all layers of the multilayer base paper contain recycled pulp, preferably containing 90% or more by weight of recycled pulp in 100% by weight of pulp, and more preferably containing 100% by weight of recycled pulp.
[0017] The recycled paper pulp can be either deinked recycled paper pulp (DIP), from which ink and dust have been removed, or undeinked recycled paper pulp. Newspaper pulp, magazine pulp, and corrugated cardboard pulp can be used as recycled paper pulp, but from an environmental perspective, it is preferable to use recycled paper pulp, and it is especially preferable to have a high proportion of recycled paper pulp in the middle layer, which has little impact on the appearance.
[0018] The base paper used in this invention can, for example, use recycled paper pulp with high whiteness for the surface layer and recycled paper pulp with lower whiteness than the surface layer for the layers other than the surface layer, or it is possible to use the same type of recycled paper pulp for all layers and layer them. Furthermore, from the viewpoint of obtaining coated white cardboard that has a good appearance and excellent ink drying properties, it is preferable that the surface layer contains 50% or more by weight of deinked recycled paper pulp (DIP) in 100% by weight of the pulp contained in the surface layer, and preferably 70% or more by weight, but from the viewpoint of aesthetics, it is more preferable to use only deinked recycled paper pulp. As the recycled paper pulp, it is preferable to use recycled newspaper with relatively high whiteness.
[0019] To suppress the decrease in whiteness of coated white cardboard caused by the use of recycled paper pulp in the surface and / or subsurface layers, it is preferable to improve the pulp whiteness by adding fresh calcium carbonate. As for the calcium carbonate, it is preferable to add light calcium carbonate, which has a more uniform particle size and a higher specific scattering coefficient compared to heavy calcium carbonate. The average particle size of calcium carbonate is not particularly limited, but is preferably 0.1 to 1.5 μm, and the BET specific surface area is 1 to 20 m². 2 / g is preferred. The amount added is preferably 1 to 30% by weight, and more preferably 1 to 10% by weight, relative to 100% by weight of pulp in each layer. Magazine waste pulp has a lower whiteness than newspaper waste pulp, which is a factor that reduces the whiteness of coated white cardboard, so it is preferable to add light calcium carbonate to the layer containing magazine waste pulp, and from the viewpoint of aesthetics such as surface strength and whiteness, it is more preferable to use deinked newspaper waste pulp in the surface layer and magazine waste pulp with light calcium carbonate added in the subsurface layer. Furthermore, when using undeinked magazine waste pulp in the subsurface layer, it is preferable to use magazine waste pulp that has been thoroughly washed to improve its whiteness.
[0020] The whiteness of each layer of the base paper is preferably 65% or more for the surface layer, and more preferably 70% or more. For the subsurface layer, it is preferably 50% or more, and more preferably 60% or more. The whiteness of the middle and back layers is not particularly limited because it has little effect on the whiteness of the coated side of the coated white cardboard, but it is preferably 45% or more from the viewpoint of the overall aesthetics of the coated white cardboard.
[0021] The layers of multilayer paper may contain chemical pulp in addition to recycled paper pulp. Furthermore, in addition to chemical pulp, mechanical pulp such as thermomechanical pulp and pressure-ground wood pulp; semi-chemical pulp such as chemical thermomechanical pulp; waste paper; paper sludge, etc., may also be included. The pulp used may be a mixture of one type of pulp or a mixture of several types, as long as it contains recycled paper pulp. The pulp composition may also be varied for each layer.
[0022] Examples of chemical pulps include bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood kraft pulp (NUKP), and sulfite pulp.
[0023] In addition to the calcium carbonate and ash content brought in from recycled paper raw materials mentioned above, the base paper in this invention may also contain fillers. The fillers are not particularly limited, but for example, inorganic fillers such as clay, calcined clay, diatomaceous earth, talc, kaolin, calcined kaolin, delaminated kaolin, heavy calcium carbonate, light calcium carbonate, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon dioxide, amorphous silica, calcium sulfite, gypsum, white carbon, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, recycled inorganic particles from papermaking sludge and deinking floss, organic fillers such as urea-formaldehyde resin, polystyrene resin, vinyl chloride resin, melamine resin, phenolic resin, and plastic micro-hollow particles, and fillers contained in recycled paper or broken paper can be used individually or in combination of two or more as appropriate.
[0024] Furthermore, flocculants, paper strength enhancers, and sizing agents can be used in the base paper layer according to the desired quality. In addition, yield enhancers, water filtration enhancers, and defoaming agents can be used as appropriate to improve operability during papermaking.
[0025] The papermaking method for the base paper used in the present invention is not particularly limited and can be carried out using a wire mesh paper machine including a top wire, an on-top former, a gap former, a round wire mesh paper machine, a paperboard paper machine that uses both a wire mesh paper machine and a round wire mesh paper machine, a Yankee dryer machine, or a hybrid paper machine combining these. The pH during papermaking can be acidic, neutral, or alkaline. In the case of multi-layer papermaking, the pH during papermaking of each layer may be the same or different for each layer. The papermaking speed is not particularly limited. The basis weight of the base paper in the coated white paperboard of the present invention is usually 150 to 650 g / m². 2 It is to that extent. Furthermore, when manufacturing the coated white cardboard of the present invention, the base paper may be smoothed beforehand using an online soft calendar, an online chilled calendar, or the like, before forming the pigment coating layer.
[0026] In the present invention, the method for drying the base paper is not limited. For example, various methods such as steam heating cylinders, heated hot air dryers, gas heater dryers, electric heater dryers, and infrared heater dryers can be used alone or in combination.
[0027] (Pigment coating layer) The coated white cardboard of the present invention has at least two pigment coating layers on the surface side of a multilayer base paper. Depending on the application, the coated white cardboard of the present invention may also have an additional pigment coating layer on the back side. In the present invention, the pigment coating layer adjacent to the base paper is also called the undercoat pigment coating layer (or "precoat layer"), and the coating liquid that forms the undercoat pigment coating layer is also called the undercoat pigment coating liquid. Furthermore, the pigment coating layer provided on the outside, that is, the pigment coating layer provided on the surface of the undercoat pigment coating layer, is also called the topcoat pigment coating layer (or "topcoat layer"), and the coating liquid that forms the topcoat pigment coating layer is also called the topcoat pigment coating liquid.
[0028] (Pre-coat layer) (Pigment) In the present invention, the precoat layer (undercoat pigment coating layer, sometimes abbreviated as "precoat layer") contains, from the viewpoint of whiteness, 80 parts by weight or more of calcium carbonate (hereinafter also referred to as "first calcium carbonate") with an average particle diameter of more than 1.2 μm per 100 parts by weight of pigment contained in the precoat layer, preferably 90 parts by weight or more, and more preferably all 100 parts by weight is said to be the first calcium carbonate. In this specification, the average particle diameter is the 50% volume average particle diameter. In other words, the average particle diameter is the cumulative 50% particle diameter when the volume-based particle diameter distribution is determined. In the present invention, the average particle diameter is measured by laser diffraction and can be measured using a Malvern Mastersizer 3000 or the like. The upper limit of the average particle diameter of the first calcium carbonate is preferably 6.0 μm or less, and more preferably 2.0 μm or less. The lower limit of the average particle diameter of the first calcium carbonate is greater than 1.2 μm, and preferably 1.3 μm or more. Examples of the first calcium carbonate include heavy calcium carbonate and light calcium carbonate. In this invention, the pigment such as the first calcium carbonate is sometimes referred to as a "white pigment" to distinguish it from the pigments used as colored colorants described later. By setting the average particle size within the above range, the calcium carbonate can more easily cover the irregularities of the base paper, thereby improving the smoothness of the paper after pre-coating. As a result, the smoothness and unevenness after the topcoat layer coating can be reduced, improving the aesthetic appeal. Furthermore, by setting the blending ratio within the above range, coated white cardboard with high whiteness and excellent aesthetic appeal can be obtained.
[0029] As a white pigment other than the first calcium carbonate, pigments commonly used in the field can be used. Examples include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate and light calcium carbonate not included in the first calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, and satin white, as well as organic pigments such as dense, hollow, and core-shell types. Multiple types of these pigments may be used in combination, but it is preferable to use a small amount of yellowish pigments such as kaolin and clay, as this may reduce the whiteness.
[0030] (glue) In the present invention, the precoat layer usually contains an adhesive (binder), and the type of adhesive is not particularly limited; adhesives conventionally used for coated paper can be used. Specifically, examples include various copolymers (latexes) such as styrene-butadiene, styrene-acrylic, ethylene-vinyl acetate, butadiene-methyl methacrylate, vinyl acetate-butyl acrylate, and acrylonitrile-butadiene-styrene, as well as synthetic adhesives such as polyvinyl alcohol, maleic anhydride copolymer, and acrylic acid-methyl methacrylate copolymer; proteins such as casein, soy protein, and synthetic protein; starches such as oxidized starch, cationized starch, urea phosphate esterified starch, hydroxyethyl etherified starch, and dextrin; and cellulose derivatives such as carboxymethylcellulose, hydroxyethylcellulose, hydroxymethylcellulose, and nanocellulose. One or more of these adhesives can be appropriately selected and used. In order to achieve a balance of various strengths such as crack resistance and surface strength, the coated white cardboard of the present invention preferably uses starch, styrene-butadiene copolymer, and acrylonitrile-butadiene-styrene copolymer individually or in combination of two or more of them.
[0031] (Top coat layer) (Pigment) In the present invention, the topcoat layer (topcoat pigment coating layer, sometimes abbreviated as "top layer") contains, from the viewpoint of whiteness, 80 parts by weight or more of calcium carbonate (hereinafter also referred to as "second calcium carbonate") with an average particle diameter of 1.2 μm or less per 100 parts by weight of pigment contained in the topcoat layer, preferably 90 parts by weight or more, and more preferably all 100 parts by weight is said to be Examples of the second calcium carbonate include heavy calcium carbonate and light calcium carbonate, which can be used individually or in combination. In this invention, the pigment such as the second calcium carbonate is sometimes referred to as a "white pigment" to distinguish it from the pigments used as colored colorants described later.
[0032] As a white pigment other than the second calcium carbonate, pigments commonly used in the field can be used. Examples include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate and light calcium carbonate not included in the second calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, and satin white, as well as organic pigments such as dense, hollow, and core-shell types. Multiple types of these pigments may be used in combination, but it is preferable to use a small amount of yellowish pigments such as kaolin and clay, as this may reduce the whiteness.
[0033] (glue) In the present invention, the topcoat layer typically contains an adhesive (binder), and the type of adhesive is not particularly limited; adhesives conventionally used for coated paper can be used. Specifically, adhesives that can be used in the precoat layer as described above can be used.
[0034] From the viewpoint of aesthetics, the coated white cardboard of the present invention may contain a blue and / or purple colorant in the top coat layer that appears white to the naked eye.
[0035] (Colorants) In this invention, "colorant" refers to a colored dye or pigment other than white. A dye is an organic pigment that selectively absorbs or reflects visible light to obtain a specific color, and which can be used to dye fibers, pigments, etc., by an appropriate dyeing method, and is soluble in solvents (such as water or organic solvents). A pigment is a white or colored powder that is insoluble, sparingly soluble, or dispersed in water, oil, or organic solvents, and can be inorganic or organic. In this invention, either inorganic or organic pigments are acceptable.
[0036] (color materials / dyes) Examples of blue dyes include TOA Blue A-TMR(L) (manufactured by Toa Chemical Co., Ltd.), and examples of purple dyes include Kayafect Violet (manufactured by Nippon Kayaku Co., Ltd.).
[0037] Dyes can be classified into types such as direct dyes, acid dyes, basic dyes, vat dyes, disperse dyes, and reactive dyes. However, direct dyes, basic dyes, and vat dyes are commonly used for cellulose fibers. Direct dyes bond to the material being dyed through hydrogen bonds, van der Waals forces, etc., while basic dyes bond to the material being dyed through Coulomb forces between ions, hydrogen bonds, van der Waals forces, etc. Examples of direct dyes include azo dyes derived from ditidine and dianisidine. Examples of basic dyes include azo dyes, diphenyl and triphenylmethane dyes, azine dyes, oxazine dyes, and thiazine dyes. Vat dyes are classified into indigo / thioindigo, anthraquinone, and phthalocyanine types.
[0038] (Colorants / Pigments) Examples of blue pigments include DC Blue GAN (Dainichi Seika Kogyo Co., Ltd.), and examples of purple pigments include DC-VIOLET 3RAN (Dainichi Seika Kogyo Co., Ltd.).
[0039] Both inorganic and organic pigments can be used as blue and purple pigments. Specific examples of blue pigments include ultramarine, azurite, prosomyx blue, ultramarine, smalt, cobalt blue (cobalt aluminate), cerulean blue (cobalt stainate), cobalt-chromium blue, cobalt-aluminum-silicon oxide, cobalt-zinc-silicon oxide, manganese blue, and phthalocyanine. Specific examples of purple pigments include inorganic pigments such as cobalt violet (cobalt arsenate, cobalt phosphate, cobalt-lithium-cobalt phosphate, hydrated ammonium cobalt phosphate, cobalt borate, etc.), purple ultramarine, iron oxide violet, manganese violet, and mineral violet, as well as organic pigments such as indigoid, quinacridone, oxazine, anthraquinone, carbonium, and xanthene.
[0040] As the colorant used in the pigment coating layer, it is preferable to use a blue and / or purple colorant. In the present invention, from the viewpoint of having excellent lightfastness and preventing discoloration and staining of the paper over time, it is preferable to mainly use pigments as the colorant for the pigment coating layer.
[0041] In the present invention, the pigment coating layer may use blue or purple colorants alone, or in combination. However, from the viewpoint of aesthetics, it is preferable to use blue and purple colorants in combination. Furthermore, the pigment coating layer may contain colorants other than blue and purple, such as red or yellow, as needed.
[0042] In the present invention, the amount of colorant in the pigment coating layer is not particularly limited, but the total amount of colorant in the pigment coating layer is less than the amount of colorant in 1 m of coated white cardboard. 2The amount is 0.5 to 15.0 mg per serving. It is preferable that the amount be 9.0 to 12.0 mg, and more preferably 9.0 to 12.0 mg.
[0043] In the present invention, the pigment coating layer is formed by coating one or both sides of a base paper with a pigment coating solution prepared by mixing necessary components such as a pigment containing calcium carbonate and an adhesive with water using a conventional mixing means such as a mixer.
[0044] (Pigment coating solution) In the present invention, the mixing ratio of pigment and adhesive in the pigment coating liquid that forms each coating layer is appropriately adjusted within a range in which the desired pigment coating liquid can be obtained. Typically, the solid content ratio is preferably 5 to 30 parts by weight of adhesive per 100 parts by weight of pigment, and more preferably 8 to 20 parts by weight. If the amount is less than 5 parts by weight, the strength of the pigment coating layer will be weak, leading to problems such as insufficient printing surface strength and powder shedding. If the amount is more than 30 parts by weight, problems such as deterioration of ink absorption during printing will occur.
[0045] Furthermore, in the present invention, both the topcoat layer and the precoat layer preferably contain 12 parts by weight or less of latex per 100 parts by weight of pigment contained in each layer, more preferably 3 to 10 parts by weight, and even more preferably 4 to 9 parts by weight. If the amount of latex is too high, the ink drying performance may decrease. In addition, it is preferable that the ratio of latex content in the topcoat layer to the precoat layer be topcoat layer > precoat layer. The topcoat layer contains a large amount of second calcium carbonate, which has a small particle size and high binder requirements, and contributes greatly to the surface strength. Therefore, by increasing the latex content in the topcoat layer, a coated white cardboard with higher strength can be obtained.
[0046] In the pigment coating liquid for forming the pigment coating layer of the present invention, in addition to the pigment, the adhesive, and the colorant used as necessary, various auxiliaries that are usually blended in pigments for coated paper, such as caustic agents, dispersants, preservatives, viscosity improvers, water retention agents, defoamers, water resistance agents, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, printability improvers, lubricants, fluorescent dyes, and metal salts, can be appropriately used.
[0047] The solid content concentration of the pigment coating liquid is preferably 55% by weight or more, more preferably 60% by weight or more. If the solid content is lower than 55% by weight, the quality of the coated white paperboard may deteriorate due to excessive penetration of the pigment coating liquid into the base paper. On the other hand, the upper limit of the solid content concentration is not particularly limited, but in consideration of liquid feeding properties and the like, it is preferably 70% by weight or less, more preferably 65% by weight or less.
[0048] (Coating Method) The coating method for forming the pigment coating layer is not particularly limited, and various conventional coating apparatuses such as a blade coater, a rod coater, an air knife coater, a roll coater, and a curtain coater can be used. Among them, the coating method using a blade coater or a rod coater is preferable because it can increase the density of the pigment coating layer and obtain a pigment coating layer excellent in light-shielding properties and aesthetic properties. The rod coater may also be referred to as a bar coater or a bar blade coater.
[0049] In the present invention, the coating amount of the pigment coating layer is, in terms of dry weight per one side, 10 to 50 g / m in total for all layers 2 is preferable, and 10 to 40 g / m 2 is more preferable, and 15 to 30 g / m 2 is even more preferable. If the total coating amount of all layers is less than 10 g / m 2 , the pigment coating layer becomes thin, and sufficient whiteness of the coated white paperboard may not be obtained. On the other hand, if the total coating amount of all layers exceeds 50 g / m 2 , the operability such as drying property in the drying step may be deteriorated, or it may cause printing unevenness due to binder migration. In this invention, the amount of undercoat pigment coating layer and the amount of topcoat pigment coating layer are not particularly limited, but the total amount of undercoat pigment coating layer per side by dry weight should be 5 to 25 g / m². 2 The topcoat pigment coating layer is 5-25 g / m². 2 It is preferable that the application amount of the undercoat pigment coating layer and the topcoat pigment coating layer be 5 g / m² each. 2 If the amount is less than the recommended amount, the base paper coating may be insufficient, resulting in a poor surface finish when the topcoat is applied. On the other hand, if the coating amount is too high, operability decreases, such as reduced drying performance during the drying process, and there is a tendency for cracking of the pigment coating layer to occur more easily. Furthermore, it is preferable that the amount of the base pigment coating layer > the amount of the topcoat pigment coating layer. By increasing the amount of the base pigment coating layer, the unevenness of the base paper can be made uniform, resulting in a good surface finish when the topcoat pigment coating layer is applied.
[0050] The coated white cardboard of the present invention is manufactured by applying a pigment coating layer to a base paper and then going through a normal drying process, but may be smoothed by a surface treatment process or the like as needed. In a preferred embodiment, the moisture content of the coated white cardboard after manufacture is adjusted to about 3 to 10% by weight, more preferably 4 to 8% by weight. For the smoothing process, a smoothing apparatus such as a normal supercalender, gloss calender, soft calender, hot calender, or shoe calender can be used. The smoothing apparatus is used as appropriate on-machine or off-machine, and the form of the pressurizing device, the number of pressurizing nips, heating, etc., are also adjusted as appropriate.
[0051] The coated white cardboard of the present invention may have a clear coating layer applied to the base paper and / or the coated paper after the pigment coating layer has been applied, for purposes such as suppressing the penetration of the binder in the coating solution into the base paper and / or improving surface strength, and suppressing curling. The clear coating layer may be applied to only one side, and it is preferable to apply it only to the back side. The clear coating solution may contain conventionally known and used binders, and various auxiliary agents that are normally added to clear coating solutions, such as viscosity modifiers, water retention agents, defoaming agents, water-resistant agents, fluorescent dyes, colorants, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts. The type of binder is not particularly limited, but it is preferable to include starches such as raw starch, oxidized starch, esterified starch, cationized starch, and automodified starch produced in a paper mill by thermochemical or enzymatic modification using acetylated tapioca starch as raw materials; modified starches such as aldehyde starch and hydroxyethylated starch; various copolymers such as styrene-butadiene, styrene-acrylic, ethylene-vinyl acetate, butadiene-methyl methacrylate, and vinyl acetate-butyl acrylate; synthetic adhesives such as polyvinyl alcohol, maleic anhydride copolymer, and acrylic acid-methyl methacrylate copolymer; proteins such as casein, soy protein, and synthetic protein; and it is more preferable to include polyvinyl alcohol. From the viewpoint of improving paper strength, it is even more preferable to apply a clear coating liquid containing both polyvinyl alcohol and polyacrylamide, and from the viewpoint of surface strength of the backing layer and curl suppression, the solid content ratio of polyvinyl alcohol to polyacrylamide is preferably 5:1 to 1:5, and more preferably 3:1 to 1:3. In this specification, "clear coating liquid" refers to a coating liquid that does not contain pigments such as white pigments, and "clear coating layer" refers to a coating layer obtained by applying the clear coating liquid. The coating method may be the method of providing the pigment coating layer as described above, or calender sizing may be performed using a calendering machine.
[0052] (Glossiness of white paper) The coated surface of the coated white cardboard of the present invention has a white paper gloss of 60% or less, preferably 20-50%, from the viewpoint of readability of the printed text. White paper gloss is an index indicating the degree of gloss on white paper, and in the present invention, it is the specular gloss at an angle of 75° to the normal of the paper surface, measured according to JIS P 8142. White paper gloss can be adjusted by the calendering linear pressure, coating amount, moisture content, papermaking speed, etc.
[0053] (Basic weight) The coated white cardboard of the present invention has a basis weight of 150 to 1000 g / m², as measured in accordance with JIS P 8124, from the viewpoint of strength and processability. 2 Preferably, 200-600 g / m 2 This is more preferable. If the basis weight is too high compared to the above upper limit, there is a risk of deterioration in drying efficiency during manufacturing, and if it is too low compared to the above lower limit, there is a risk of insufficient strength and paper thickness necessary for use as cardboard.
[0054] (paper thickness) The coated white cardboard of the present invention preferably has a paper thickness of 200 to 1000 μm, and more preferably 250 to 900 μm, as measured in accordance with JIS P 8118, from the viewpoint of strength and workability. If the paper thickness is too large compared to the above upper limit, workability such as bending may decrease, and if it is too small compared to the above lower limit, the strength may be insufficient.
[0055] (density) The density of the coated white cardboard of the present invention is 0.5 to 1.0 g / m², from the viewpoint of print strength and aesthetic appeal during printing. 3 Preferably, 0.7~0.9 g / m 3 This is more preferable. If the density is too high compared to the upper limit above, the paper will have poor cushioning properties and may result in misprints during gravure printing. If it is too low compared to the lower limit above, it may result in paper peeling due to reduced print strength.
[0056] (Oken type smoothness) The Wangken smoothness of the coated surface of the coated white cardboard of the present invention is preferably 50 seconds or more, more preferably 80 seconds or more, and even more preferably 100 seconds or more, from the viewpoint of image resolution when printed. A higher smoothness value indicates a smoother surface. The upper limit of the Wangken smoothness of the coated surface can be 500 seconds or less, 400 seconds or less, or 300 seconds or less, from the viewpoint of preventing soiling due to friction of printed materials and preventing cargo shifting during transportation. The Wangken smoothness of the coated surface can be adjusted by changing the calendar line pressure or the pigment composition (e.g., increased use of kaolin, use of pigments with small particle size).
[0057] (ISO whiteness) The ISO whiteness (hereinafter also simply referred to as "whiteness") of the coated layer surface of the coated white cardboard of the present invention is 60% or higher, more preferably 65% or higher, and even more preferably 70% or higher. The upper limit of the whiteness is approximately 90% or lower. If the whiteness is too low compared to the lower limit, the aesthetic appeal may be inferior. In the present invention, the ISO whiteness is the whiteness measured in accordance with JIS P8148. The coated white cardboard of the present invention can have its whiteness achieved by the pigment in the pigment coating layer further enhanced by adding calcium carbonate to the recycled paper pulp in the surface layer and / or subsurface layer. Since the whiteness of the surface of the pigment coating layer is affected by the whiteness of the base paper, even when using pulp with low whiteness, such as deinked pulp, recycled magazine paper, or recycled corrugated cardboard pulp, in the surface, subsurface, and middle layers, adding fresh calcium carbonate can improve the whiteness of the recycled paper pulp layer, and consequently improve the whiteness when measured from the pigment coating surface of the coated white cardboard.
[0058] (hue) The surface of the coating layer of the coated white cardboard of the present invention was measured using a light source including ultraviolet light according to JIS P 8150 in terms of hue measurement, and b * The value is preferably 0 or less, more preferably adjusted to -5 to -0.5, and even more preferably adjusted to -4 to -1. *As long as the value is within the above range, even if the ISO whiteness score is low due to the inclusion of a large amount of recycled paper in the base paper, it is possible to produce coated white cardboard that is easily perceived as white by the eye.
[0059] a of the coated white cardboard of the present invention, measured under the same conditions as above. * The value does not significantly contribute to the apparent whiteness of the coated white cardboard and is therefore not particularly limited, but is usually preferred to be -2 to 2, and more preferably -1 to 1. Also, L measured under the same conditions as above. * The value is not particularly limited, but is usually preferably 80 to 95, and more preferably 85 to 90.
[0060] (Application) The coated white cardboard of the present invention possesses both excellent ink-drying properties and whiteness, and because it has a pigment coating layer, it also has excellent printability. Therefore, although not particularly limited, it is suitable for use in packaging for food and clothing. [Examples]
[0061] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to these examples. In each example and comparative example, unless otherwise specified, "parts" refers to "parts by weight" and "%" refers to "% by weight".
[0062] (Example 1) (base paper) This pulp is made from 100% by weight of deinked recycled paper pulp (ash content 1.6%, whiteness 72%) derived from recycled newspapers and magazines, with 2.2% of light calcium carbonate 1 (average particle size: 2.84 μm) added as filler, resulting in a basis weight of 35.22 g / m². 2 The surface layer (1st layer, ash content 3.8%, whiteness 72.2%) is prepared by adding 7.7% light calcium carbonate 1 as a filler to 100% by weight of un-deinked recycled paper pulp 1 (ash content 10%, whiteness 56%) made from recycled magazine paper, resulting in a basis weight of 38.16 g / m². 2 The lower surface layer (second layer, 17.7% ash content, 56.5% whiteness) is made using 100% by weight of un-deinked recycled paper pulp 2 (20.5% ash content, 54.5% whiteness) derived from recycled magazine paper, resulting in a basis weight of 181.99 g / m².2 The middle layer (3rd to 6th layers), basis weight 38.16 g / m² 2 The back layer (7th layer) is made by papermaking, then assembled, pressed, and dried to produce a paper with 7 layers and a basis weight of 293.5 g / m². 2 The base paper was obtained. Furthermore, the ash content and whiteness of un-deinked recycled paper pulp 1 and 2, which were made from magazine waste paper, were adjusted by varying the degree of washing.
[0063] (Topcoat pigment coating liquid) A pigment slurry was prepared consisting of 100 parts by weight of heavy calcium carbonate 1 (FMT-97, manufactured by Fimatec Co., Ltd., average particle size: 1.04 μm) on a solid content basis. Then, a slurry was prepared by adding 10 parts by weight of styrene-butadiene copolymer latex (manufactured by Asahi Kasei Corporation, B1443) and 3 parts by weight of starch as adhesives to 100 parts by weight of pigment (solid content). To this slurry, 1.5 parts by weight of a printability improver (Sumirez Resin SPI-102A, manufactured by Taoka Chemical Industry Co., Ltd.), and 0.05% of a blue colorant (DC Blue GAN, manufactured by Dainichi Seika Kogyo Co., Ltd.) and 0.06% of a purple colorant (DC Violet 3RAN, manufactured by Dainichi Seika Kogyo Co., Ltd.) were added as colorants. Water was then added to obtain a topcoat pigment coating solution 1 with a solid content concentration of 60%. The amount of colorant added is the amount added relative to 100 parts by weight of pigment (solid content) in the pigment slurry.
[0064] (Primer pigment coating liquid) To 100 parts by weight of heavy calcium carbonate 2 (FMT-90, manufactured by Fimatec Co., Ltd., average particle size: 1.60 μm) on a solid content basis, 8 parts by weight of acrylonitrile butadiene styrene latex (NB-201, manufactured by ENEOS Material Co., Ltd.) and 3 parts by weight of starch were added as adhesives, and water was further added to obtain a primer pigment coating solution with a solid content concentration of 60%.
[0065] (Coated white cardboard) The surface layer of the base paper is coated with primer pigment solution 1 using a rod coater, with a dry weight of 11.8 g / m² per side. 2After coating and drying, the topcoat pigment coating liquid 1 is applied using a rod coater, with a coating amount of 9.7 g / m² per side by dry weight. 2 The paper was coated and dried to achieve the desired finish. Afterward, it was smoothed using a calender. Furthermore, a clear coating of a surface strengthening agent with a solid content of 3% was applied to the back surface of the pigment-coated white cardboard. The amount of clear coating applied was 0.5 g / m² by dry weight. 2 The surface paper strength agent used is polyvinyl alcohol (PVA) and polyacrylamide (PAM) in a 1:1 weight ratio, with a basis weight of 315.5 g / m². 2 Coated white cardboard 1 was manufactured. The thickness of the obtained coated white cardboard 1 was 389 μm.
[0066] (Example 2) (base paper) Except for changing the layer ratios of the surface layer, subsurface layer, middle layer, and back layer that make up the base paper to the ratios shown in Table 1, the basis weight was 297.4 g / m², similar to Example 1. 2 I obtained the original paper.
[0067] (Topcoat pigment coating liquid) A topcoat pigment coating solution 2 was obtained in the same manner as in Example 1, except that the amount of printability improver (Sumirez Resin SPI-102A, manufactured by Taoka Chemical Industries, Ltd.) was changed to 1.0 part by weight.
[0068] (Coated white cardboard) Using the base paper obtained as described above, the coating amount of primer pigment coating solution 1 was set to 10.3 g / m². 2 The application amount of topcoat pigment coating liquid 2 is 8.4 g / m². 2 Except for the change made, the procedure was the same as in Example 1, with a basis weight of 316.6 g / m². 2 Coated white cardboard 2 with a paper thickness of 382 μm was manufactured.
[0069] (Example 3) (base paper) Using 100% by weight of un-deinked recycled paper pulp 1 (ash content 10%, whiteness 56%) made from recycled magazine paper, the basis weight is 40.88 g / m². 2The surface layer (first layer) is made using 100% by weight of un-deinked recycled paper pulp 2 (ash content 20.5%, whiteness 54.5%) derived from recycled magazine paper, with a basis weight of 52.56 g / m². 2 The lower layer (second layer) of the surface, and basis weight 157.67 g / m² 2 The middle layer (3rd to 5th layer) uses pulp with 100% un-de-inked recycled paper pulp 1, resulting in a basis weight of 40.88 g / m². 2 Each of the back layers (6th layer) is made by papermaking, then assembled, pressed, and dried to produce a paper with 6 layers and a basis weight of 292.0 g / m². 2 I obtained the original paper.
[0070] (Topcoat pigment coating liquid) A topcoat pigment coating solution 3 was obtained in the same manner as in Example 1, except that the amount of styrene-butadiene copolymer latex used as an adhesive was changed to 8 parts by weight, the amount of starch to 2 parts by weight, and no coloring agent was used.
[0071] (Primer pigment coating liquid) A primer pigment coating solution 2 was obtained in the same manner as in Example 1, except that the amount of acrylonitrile butadiene styrene latex (NB-201) added as an adhesive was changed to 6 parts by weight per 100 parts by weight of heavy calcium carbonate 2 in terms of solid content.
[0072] (Coated white cardboard) Using the base paper obtained as described above, the coating amount of the undercoat pigment coating solution 2 was set to 12.4 g / m². 2 The application amount of topcoat pigment coating liquid 3 is 10.1 g / m². 2 Except for the above, the procedure was the same as in Example 1, with a basis weight of 315.0 g / m². 2 Coated white cardboard 3 with a paper thickness of 378 μm was manufactured.
[0073] (Example 4) Coated white cardboard 4 was manufactured in the same manner as in Example 1, except that light calcium carbonate was not added as a filler to the surface layer (first layer).
[0074] (Example 5) Coated white cardboard 5 was manufactured in the same manner as in Example 1, except that light calcium carbonate was not added as a filler to the subsurface layer (second layer).
[0075] (Comparative Example 1) (base paper) The only differences from Example 1 were that the pulp used in the top layer (1st layer) was changed to 100% by weight chemical pulp (1% ash content, 88% whiteness), the pulp used in the subtop layer (2nd layer) was changed to 100% by weight deinked recycled paper pulp (1.6% ash content, 72% whiteness) made from recycled newspaper and magazine paper (without the addition of fillers), and the layer ratios of each layer constituting the base paper were changed to the ratios listed in Table 1. The basis weight was 291.6 g / m². 2 I obtained the original paper.
[0076] (Topcoat pigment coating liquid) A pigment slurry was prepared containing 5 parts by weight of titanium dioxide (Typake PFC503, manufactured by Ishihara Sangyo Co., Ltd., average particle size: 0.25 μm) on a solid content basis and 95 parts by weight of heavy calcium carbonate 1 on a solid content basis. Then, a slurry was prepared by adding 15 parts by weight of styrene-butadiene copolymer latex (B1443) as an adhesive to 100 parts by weight of pigment (solid content). To this slurry, 1.5 parts by weight of a printability improver (Sumirez Resin SPI-102A, manufactured by Taoka Chemical Industry Co., Ltd.) and 0.006% of a purple coloring agent (DC Violet 3RAN, manufactured by Dainichi Seika Kogyo Co., Ltd.) were added as a coloring agent (colorant), and water was further added to obtain a topcoat pigment coating solution 4 with a solid content concentration of 60%. Note that the amount of coloring agent added is the amount added per 100 parts by weight of pigment (solid content) in the pigment slurry.
[0077] (Primer pigment coating liquid) A primer pigment coating solution 3 was obtained in the same manner as in Example 1, except that the amount of acrylonitrile butadiene styrene latex (NB-201) added as an adhesive was changed to 14 parts by weight and the amount of starch added to 1 part by weight, with respect to 100 parts by weight of heavy calcium carbonate 2 in terms of solid content.
[0078] (Coated white cardboard) The surface layer of the base paper is coated with primer pigment solution 3 using a rod coater, with a dry weight of 12.5 g / m² per side. 2 After coating and drying, the topcoat pigment coating liquid 4 is applied using a blade coater, with a coating amount of 10.2 g / m² per side by dry weight. 2 The paper was coated and dried to achieve the desired finish. Afterward, it was smoothed using a calender. Furthermore, a clear coating of a surface strengthening agent with a solid content of 3% was applied to the back surface of the pigment-coated white cardboard. The amount of clear coating applied was 0.5 g / m² by dry weight. 2 The surface paper strength agent used is polyvinyl alcohol (PVA) and polyacrylamide (PAM) in a 1:1 weight ratio, with a basis weight of 314.8 g / m². 2 Coated white cardboard 6 was manufactured. The thickness of the obtained coated white cardboard 6 was 377 μm.
[0079] (Comparative Example 2) (base paper) 100% by weight chemical pulp (1% ash content, 88% whiteness) with 2.2% light calcium carbonate 1 added as filler, resulting in a basis weight of 35.48 g / m². 2 The surface layer (1st layer, ash content 3.2%, whiteness 88.2%) is made by adding 4.4% light calcium carbonate 1 as a filler to 100% by weight of deinked recycled paper pulp (ash content 1.6%, whiteness 72%) made from recycled newspaper and magazine paper, resulting in a basis weight of 35.48 g / m². 2 The lower surface layer (second layer, 6.0% ash content, 88.3% whiteness) is made using 100% by weight of un-deinked recycled paper pulp 2 (20.5% ash content, 54.5% whiteness) derived from recycled magazine paper, resulting in a basis weight of 186.26 g / m². 2 The middle layer (3rd to 6th layers), basis weight 38.43 g / m² 2 The back layer (7th layer) is made by papermaking, then assembled, pressed, and dried to produce a paper with 7 layers and a basis weight of 295.7 g / m². 2 I obtained the original paper.
[0080] (Topcoat pigment coating liquid) A pigment slurry was prepared containing 60 parts by weight of kaolin (Thiele, Kaofine, average particle size: 0.3 μm) on a solid content basis, 5 parts by weight of titanium dioxide (Ishihara Sangyo Co., Ltd., Typake PFC503, average particle size: 0.25 μm) on a solid content basis, 25 parts by weight of heavy calcium carbonate 1 on a solid content basis, and 10 parts by weight of light calcium carbonate 2 (Okutama Kogyo Co., Ltd., Tamapar 221F, average particle size: 0.41 μm) on a solid content basis. Then, a slurry was prepared by adding 15 parts by weight of styrene-butadiene copolymer latex (B1443) as an adhesive to 100 parts by weight of the pigment (solid content). To this slurry, 1.5 parts by weight of a printability improver (Taoka Chemical Industry Co., Ltd., Sumirez Resin SPI-102A) and a blue coloring agent (Dainichi Seika Kogyo Co., Ltd., DC Blue) were added as colorants. 0.01% of GAN and 0.02% of a purple coloring agent (manufactured by Dainichi Seika Kogyo Co., Ltd., DC Violet 3RAN) were added, and then water was added to obtain a topcoat pigment coating solution 5 with a solid content concentration of 60%. The amount of coloring agent added is the amount added per 100 parts by weight of the pigment (solid content) in the pigment slurry.
[0081] (Coated white cardboard) The same undercoat pigment coating solution 3 obtained in Comparative Example 1 was applied to the surface of the base paper using a rod coater, with a dry weight coating amount of 12.0 g / m² per side. 2 After coating and drying, the topcoat pigment coating liquid 5 is applied using a blade coater, with a coating amount of 9.8 g / m² per side by dry weight. 2 The paper was coated and dried to achieve the desired finish. Afterward, it was smoothed using a calender. Furthermore, a clear coating of a surface strengthening agent with a solid content of 3% was applied to the back surface of the pigment-coated white cardboard. The amount of clear coating applied was 0.5 g / m² by dry weight. 2 The surface paper strength agent used is polyvinyl alcohol (PVA) and polyacrylamide (PAM) in a 1:1 weight ratio, with a basis weight of 318.0 g / m². 2 Coated white cardboard 7 was manufactured. The thickness of the obtained coated white cardboard 7 was 380 μm.
[0082] (Evaluation method) The coated white cardboard produced in the examples and comparative examples was evaluated using the following method. The results are shown in Table 1. Basis weight: Measured in accordance with JIS P 8124. Paper thickness: Measured in accordance with JIS P 8118. Density: Determined from basis weight and paper thickness in accordance with JIS P 8118. White paper glossiness: Measured on the front side of the paper according to JIS P 8142. Wang Ken-type smoothness: In accordance with JIS P8155:2010, the front side of the paper was measured using a digital Wang Ken-type air permeability and smoothness tester (manufactured by Asahi Seiko Co., Ltd.). ISO whiteness: Measured on the front side of the paper in accordance with JIS P 8148. Hue: Measured on the front side of the paper using a light source including ultraviolet light, in accordance with JIS P 8150.
[0083] Average particle size: The average particle size of heavy calcium carbonate and light calcium carbonate was measured under the following conditions according to the measuring device's manual. Equipment: Malvern Mastersizer 3000 Measurement conditions: Calcium Carbonate CaCO3 (calcite) (Particle refractive index: 1.655, Particle absorptivity: 0.01)
[0084] Pulp Ash Content and Whiteness: A pulp sample weighing 5g dry, thoroughly washed, was disintegrated and dewatered using a Buchner funnel on a 16cm round filter paper. A hand-making plate was placed on the sheet surface, and several sheets of thick filter paper were placed in between and stacked. This was pressed in a sheet press at 18.6kgf for 5 minutes (first press). The thick filter paper placed in between was replaced with dry thick filter paper, and the sheet was pressed again at 18.6kgf for 2 minutes (second press). With the hand-making plate still attached, it was tension-dried in a forced-air dryer at 50°C for 1 hour. Whiteness was measured according to JIS P 8148, and ash content according to JIS P 8251.
[0085] Ink drying properties: Using a Roland 4-color single-sided sheet-fed printing press (R304) with sheet-fed process inks manufactured by Toyo Ink Mfg. Ltd., printing was performed at a rate of 8000 sheets / hour with solid ink densities (black / blue / magenta / yellow) = 1.85 / 1.60 / 1.50 / 1.40. After 1 hour, the solid ink area of the printed surface was placed on top of a blank sheet of paper and nipped using an RI-II type printing test machine. The ink density transferred to the blank paper was visually evaluated. The evaluation was performed using the following 5-point scale. 5 (excellent: low concentration) -1 (poor: high concentration)
[0086] Texture: Coated white cardboard was visually inspected from the front side, and the unevenness of whiteness and overall whiteness were evaluated according to the following criteria. 5: High whiteness with no unevenness in white, and a very good texture. 4: Relatively high whiteness with minimal white unevenness, resulting in a good texture. 3: Good texture, although the whiteness or unevenness of the whiteness is slightly inferior. 2: Low whiteness or noticeable white unevenness, resulting in a slightly inferior texture. 1: Low whiteness, noticeable unevenness in whiteness, and inferior texture.
[0087] Cost: The manufacturing cost of coated white cardboard was evaluated on a scale of 5 (excellent: low cost) to 1 (poor: high cost).
[0088] [Table 1]
[0089] Table 1 shows that even with base paper made entirely of recycled paper pulp or deinked recycled paper pulp, coatings with excellent ink-drying properties and whiteness can be achieved by adding two pigment coating layers containing a high amount of calcium carbonate. Furthermore, a comparison of Examples 1 and 2 with Example 3 shows that coatings with higher whiteness can be obtained by using deinked recycled paper pulp in the surface layer and incorporating blue and / or purple colorants in the top layer. A comparison of Example 1 with Example 5 shows that coatings with higher whiteness can be obtained by adding calcium carbonate to the subsurface layer using recycled paper with low whiteness. On the other hand, a comparison of Example 1 with Example 4 shows that even when calcium carbonate is not added to the surface layer, adding calcium carbonate to the subsurface layer does not reduce the whiteness of the coatings. From the above comparison of Examples 1, 4, and 5, it was found that adding filler (calcium carbonate) to the subsurface layer with low pulp whiteness is effective for improving the whiteness of coatings.
Claims
1. A coated white cardboard having a white gloss of 50% or less, having two pigment coating layers on at least the surface side of a multilayer base paper having a surface layer, subsurface layer, middle layer, and back layer, The entire layer of the aforementioned multilayer base paper contains recycled paper pulp. Of the pigment coating layers, the pre-coat layer adjacent to the base paper contains 80 parts by weight or more of calcium carbonate with an average particle size of 1.2 μm or more in 100 parts by weight of pigment contained in the pre-coat layer. Coated white cardboard in which a topcoat layer provided on the outside of the pigment coating layer contains 80 parts by weight or more of calcium carbonate with an average particle size of 1.2 μm or less in 100 parts by weight of pigment contained in the topcoat layer.
2. The coated white cardboard according to claim 1, wherein the surface layer contains 50% by weight or more of deinked recycled paper pulp in 100% by weight of pulp.
3. The coated white cardboard according to claim 1, wherein the surface layer and / or subsurface layer contains 1 to 30% by weight of calcium carbonate relative to 100% by weight of the pulp in each layer.
4. The coated white cardboard according to claim 1 or 2, wherein the top coat layer contains a blue and / or purple colorant.
5. b measured with a light source including ultraviolet light in accordance with JIS P 8150 * Coated white cardboard according to claim 1 or 2, wherein the value is 0 or less.
6. The coated white cardboard according to claim 1 or 2, wherein both the topcoat layer and the precoat layer contain 12 parts by weight or less of latex with respect to 100 parts by weight of pigment contained in each layer.
Citation Information
Patent Citations
High solid concentration coating composition
JP1985059192A
Copolymer latex for coating paper
JP1994101196A
Two layer-coated paper board
JP1994166991A
Matte coated paper for printing
JP2008106406A
White paperboard and coated white paperboard
JP2020133015A