Plastic container coating technology

The PECVD-based gradient coating for plastic containers addresses the issue of porosity and hydrolysis in existing coatings by forming a non-porous, thin-film structure with alternating oxide and organic layers, ensuring effective barrier performance and chemical resistance for corrosive media storage.

JP7954880B2Active Publication Date: 2026-11-24IONKRAFT GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024552361
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-02-27
Publication Date
2026-11-24
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

Existing plastic container coatings are unsuitable for storing corrosive media due to porosity and susceptibility to hydrolysis, leading to damage and contamination, and current methods are costly, environmentally harmful, or lack sufficient barrier properties.

Method used

A gradient coating technology using PECVD with controlled process conditions to form a non-porous, thin-film structure composed of alternating oxide and organic layers, preventing island growth and ensuring high barrier performance and chemical resistance.

Benefits of technology

The gradient coating provides a uniform, non-porous barrier that effectively prevents gas permeation and protects against corrosive media, maintaining integrity over time, even in alkaline solutions, while being environmentally friendly and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954880000007
    Figure 0007954880000007
  • Figure 0007954880000008
    Figure 0007954880000008
  • Figure 0007954880000009
    Figure 0007954880000009
Patent Text Reader

Abstract

The present invention relates to the field of plastic coating by plasma enhanced chemical vapor deposition (PECVD). In particular, the present invention can be used to coat recyclable plastic containers for storing aggressive chemicals with a stable migration barrier. A method and coating are disclosed. The method can deposit a coating from a process gas mixture of at least one precursor and a reactive gas, where the process gas mixture is excited to form a plasma. By adjusting the reactive gas content in the process gas mixture and varying the excitation energy per unit mass, a gradient coat can be deposited on a plastic substrate to form a chemically resistant migration barrier.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to the field of plastic coating by plasma-enhanced chemical vapor deposition (PECVD).

[0002] In industry, plastic containers such as bottles and canisters are used to store various liquids. The properties of the plastic affect not only the manufacturing cost of the container but also the material's suitability for storing each medium.

[0003] The suitability of the material depends particularly on the permeability of the plastic to various gases (e.g., oxygen from ambient air), solvents, aromatic compounds, dyes, or other substances, and on the plastic's resistance to the storage medium (e.g., acidic or alkaline media).

[0004] To safely store a medium, such as an alkaline solution, it must be protected from permeation and loss of substances from the environment. The contents of the container must not be contaminated with the environment. However, depending on the properties of the container material, gases and other substances may diffuse (permeate) through the container walls. The barrier performance of the container material indicates how well the container or storage medium is protected against permeation.

[0005] Furthermore, the medium itself must not leak from the container, nor should it damage the container. The container material must withstand the long-term storage of the medium and ensure sufficient storage safety. In particular, when storing chemicals, many of which are classified as hazardous materials, high resistance requirements are placed on the container material.

[0006] In principle, manufacturing containers from plastic, for example by extrusion blow molding, is a common method in industry because it allows for cost-effective production and plastic containers are easy to store. However, conventional technology does not yet know of a cost-effective plastic that simultaneously provides sufficient barrier properties and resistance to corrosive media, particularly alkaline or acidic media.

[0007] Therefore, in prior art, plastics and special composite plastics that are expensive to manufacture or difficult to transport and store are often not used for storing corrosive media.

[0008] Containers manufactured by co-extrusion blow molding are often used, and their walls are composed of multiple layers of different plastics. Mixtures of rigid polyethylene (HD-PE), polyamide (PA), and / or ethylene-vinyl alcohol copolymer (EVOH) are frequently used. HD-PE has high resistance to acids, alkalis, and oils, but is highly permeable to certain substances, so EVOH and / or PA are used instead. Such composite plastic packaging is not environmentally friendly because only single-material solutions are sustainable and recyclable.

[0009] Aside from using multi-material solutions for non-recyclable plastics, the only options for plastic barrier finishes are fluorination or plasma coating. In fluorination, containers are placed in a vacuum chamber and exposed to a fluorine gas mixture in the absence of air. Due to its high reactivity, fluorine partially replaces hydrogen atoms on the material surface. However, this only creates an adsorption barrier and can only prevent the migration of a medium such as a solvent. Furthermore, fluorine is toxic and highly corrosive, making this technology unattractive and costly. In addition, there is growing research suggesting that fluorinated plastics have adverse effects on the environment and health.

[0010] On the other hand, plasma polymer coatings are not only low-cost, but can also be manufactured using harmless chemicals and require only small amounts of energy and materials. PECVD can be used to manufacture fluorine-free, silicon-based barrier coatings that can function as passive barriers preventing the migration of any substance. Therefore, these coatings are suitable, for example, as solvent barriers, barriers to prevent the migration of contaminants from recycled plastics to fillers, or gas barriers against oxygen, hydrogen, or carbon dioxide, opening up a wide range of possible applications.

[0011] German Patent Application Publication No. 3632748 describes a low-pressure PEVCD coating process for hollow bodies that is now widely used in industry. First, the entire vacuum chamber, along with the bottle to be coated, is evacuated to the required working pressure. Next, a process gas is introduced into the bottle and excited with microwaves to generate a plasma. The plasma ignites inside the bottle, allowing for the formation of a barrier coating.

[0012] Plasma polymer coatings are not only low-cost but also environmentally friendly, as they require less energy and materials for manufacturing and do not use solvents or other harmful chemicals compared to competing permeability reduction processes. This is especially true for low-pressure plasma processes, as these processes create a sealed reaction space and minimize the use of process gases.

[0013] Silicon oxide (SiOx) barrier coatings, as known from prior art, are extremely susceptible to hydrolysis and will decompose even upon contact with fillers whose pH is slightly above 7.

[0014] German Patent Application Publication No. 102006048658 discloses a multilayer composite coating comprising an SiOx barrier layer and an organosilicon passivation layer.

[0015] A drawback of such multilayer composite coatings, where layers are built successively (often in separate process steps), is that, due to the layer growth mechanism typical of PECVD processes, defects and pores in the lower layers propagate as defects in subsequent coatings, resulting in such layer systems always exhibiting continuous porosity.

[0016] Such PECVD processes for depositing gas-impermeable barrier layers and protective passivation layers on plastic containers (so-called composite coatings) are currently used primarily in the beverage industry.

[0017] For certain fillings that require high mechanical stability, high barrier performance against gases and solvents, and high resistance to acidic and alkaline media, such as corrosive alkaline chemicals, known composite coatings are unsuitable or at least require optimization.

[0018] The growth processes of various layers in a composite coating create pores on the coating surface. In particular, these pores create gaps in the passivation layer, through which the underlying barrier layer is exposed to corrosive media. Pores can especially be caused by the growth of so-called islands during coating deposition. Island growth hinders the formation of a uniform layer.

[0019] Layer growth in PECVD is a complex process overall, largely characterized by the interplay of dynamics and thermodynamics. At the start of the coating process in PECVD, layer-forming particles are accelerated toward the substrate surface. After collision, these particles are reflected from the surface if their kinetic energy is too low. If their kinetic energy is sufficiently high, these particles are adsorbed as adsorbed atoms. Such adsorbed atoms diffuse across the substrate surface until they desorb again or condense with other adsorbed atoms to form nuclei and find their final positions in the coating. The surface energy of the surface being coated greatly contributes to the mobility of the adsorbed atoms and, consequently, the type of layer growth. Uniform layer growth is preferred when the surface energies of the coating material and the substrate are similar.

[0020] In particular, island growth occurs when the surface energy of the substrate is lower than that of the layer being formed, resulting in less interaction between the substrate and the adsorbed atoms than between the particles. In this case, the layered material preferably grows in three-dimensional islands. In this growth mode, condensation of atoms on the substrate is initially not thermodynamically favored, so that a closed layer is only formed during island growth as layer growth proceeds and the islands grow together.

[0021] Furthermore, depending on the type of plasma process and reactor, the number of collisions that occur in the reactive plasma before the reactive particles reach the substrate varies. If the number of collisions is small, only a small amount of reaction occurs in the gas phase, so the deposition rate decreases. If particles and radicals undergo many collisions and reactions before reaching the substrate, volume polymerization can occur, in which case oligomers are already formed in the gas phase. The larger the particles, the lower the probability of surface diffusion, so that island growth occurs more frequently and the layer is closed later because the islands must first grow together.

[0022] This island growth results in a granular surface structure, which then leads to nanoscale pores at the grain boundaries of the coalescing islands. When several grain boundaries come together, pores are formed. The lateral extent of the pores is in the range of a few nanometers. This means that these layer defects are much larger than, for example, molecular oxygen or ions in alkaline solutions, and therefore represent weak points in the layer system.

[0023] If such pores are present in the underlying SiOx layer (barrier layer), nucleation increases here, so that agglomerates are formed here, with the result that these layer defects continue into any subsequent protective layer (passivation layer) that may be present.

[0024] Experiments have shown that numerous nanoscale pores are always formed in SiOx layers deposited on plastic layers or organosilicon adhesion-promoting layers, and these can be detected by electrochemical methods such as cyclic voltammetry and electrochemical impedance spectroscopy.

[0025] This can be explained in particular by differences in the surface energy and chemical composition of the materials, as well as by the increase in volume polymerization. When the existing pores were measured after further application of an organosilicon passivation layer on the SiOx layer, it was found that this additional coating hardly reduced the number of nanoscale pores.

[0026] Therefore, when composite coatings known from prior art are used, exposure to chemically corrosive media leads to system damage due to pores and defects. This can reach the hydrolyzable barrier layer beneath the passivation layer through continuous pores and begin to decompose it. This leads to penetration of the protective layer and damage to the entire system. Consequently, this layer system is unsuitable for industrial storage of chemicals.

[0027] One approach to solving such problems in composite coatings is the use of so-called gradient coatings, in which the chemical composition gradually changes along the layer thickness between organic materials (passivation or adhesion promotion) and oxides (migration barriers). In contrast to composite coatings consisting of several (micro)layers of significantly different materials, gradient coatings have a continuous gradient of material composition along the thickness of the coating.

[0028] Gradient coatings are known from other technical fields, for example, as a scratch-resistant layer for plastic eyeglass lenses.

[0029] From European Patent Application Publication No. 0718418, it is known that PECVD gradient coatings can be produced with otherwise constant parameters by using plasma pulsation parameters. However, these parameters are only suitable for the deposition of scratch-resistant layers, for example, where the same gas composition can be used throughout the layer deposition process because significant differences in chemical composition are not required.

[0030] German Patent Application Publication No. 4238279 discloses a further coating process for manufacturing a scratch-resistant coating.

[0031] European Patent No. 2630273 discloses a plasma treatment method for a workpiece, in which pulsed microwave energy is used to ignite a plasma and the ratio of the switch-on phase period to the switch-off phase period is changed. The ratio of the switch-on time to the switch-off time is initially increased and then decreased again during the coating process in order to initially decrease the carbon content in the barrier layer and then increase it again.

[0032] German Patent No. 19732217 discloses a plasma coating for photovoltaic semiconductor devices using a gradient coating in which the coating properties gradually change by varying plasma parameters and gas supply. The gradient coating includes a diffusion barrier layer, an elastic polymer protective layer zone, and a scratch-resistant surface layer. The film formation is carried out in a microwave plasma. This process is not suitable for producing the required layer properties on plastic substrates for plastic containers for corrosive media such as chemicals. In particular, it does not show how and on what process parameters the plasma power should be controlled to form the desired gradient coating.

[0033] A PICVD process using pulsed microwave plasma for pharmaceutical packaging is known from German Patent Application Publication No. 10139305, but it does not include a sufficient passivation layer.

[0034] International Publication No. 01 / 94448 discloses a beverage bottle coating with improved gas permeability barrier, thin wall thickness, and excellent recyclability. The coating is proposed to have an organic component-containing SiOxCyHz base layer and a barrier layer applied thereon. In one embodiment, a continuous layer structure is disclosed in which the composition changes from SiOxCyHz on the substrate surface to SiOx on the outside of the coating. Such coatings do not have sufficient resistance to chemically corrosive media (e.g., caustic soda).

[0035] U.S. Patent Application Publication 2009 / 148633 discloses a plasma CVD coating for plastic bottles having a high-carbon adhesive layer, a low-carbon intermediate barrier layer, and a high-carbon surface protective layer. While this technology can be used to manufacture coatings for beverage bottles, the coating can withstand the effects of the weak alkalinity of mineral water (pH 7.3), but will be damaged when exposed to more corrosive media.

[0036] Known processes are insufficient to produce non-porous gradient coatings that can cover a wide range of chemical compositions, from highly oxided (SiOx) for barriers to organosilicon (SiOCH) for corrosion protection.

[0037] In particular, simply changing the pulse ratio is not sufficient to achieve the desired bandwidth between the barrier effect and passivation effect in a continuous gradient coating while simultaneously ensuring the growth of a uniform, non-porous coating.

[0038] Referring to the solution known from European Patent No. 2630273, the present invention enables the deposition of a gradient coating more advantageously, and in this deposition, it is not necessarily required to first increase and then decrease the pulse parameters, particularly the ratio of switch-on time to switch-off time. Rather, research has shown that precisely controlling the energy density in the plasma according to the gas composition has a significant impact on the coating properties. For example, by controlling the energy supply, the absolute duration of the pulse, and / or the gas composition, it is possible to control the energy density in the plasma by keeping the ratio of switch-on time to switch-off time of the pulse constant, at least initially.

[0039] Gradient coatings, such as scratch-resistant coatings, known from prior art, are also unsuitable due to their mechanical properties. Scratch-resistant layers with a thickness exceeding 1 μm, often exceeding 2-3 μm, tend to crack or break at stressed points under mechanical stress, thus compromising their chemical protective effect.

[0040] Further development of the gradient coating deposition process, which had already been developed in the 1990s, was limited by the long reaction time of approximately 0.5 seconds for commercially available mass flow controllers. It was impossible to form a non-porous gradient coating with a gradient resolution of several nanometers using the technologies available at the time.

[0041] Therefore, the object of this invention is to demonstrate improved coating technology for plastic containers.

[0042] It was found that specific process conditions and coating characteristics are necessary to form a chemical-resistant coating with good barrier performance.

[0043] In order to achieve sufficiently high chemical resistance for storing chemical substances, it is preferable to produce a high-carbon-content organosilicon coating by retaining methyl groups from the precursor.

[0044] Plasma polymer layers (e.g., silicon oxide barrier layers) deposited from organosilicon precursors consist of silicon, carbon, hydrogen, oxygen, and / or nitrogen. The typical resistance of such layers to alkaline media is due to the significant difference in electronegativity between, for example, oxygen / nitrogen and silicon, which is primarily because ions in solution break bonds with high partial charge shifts. The more inorganic and oxide layers there are, the more positive partial charges there are on carbon atoms, and especially silicon atoms. Since the electronegativity difference between silicon and oxygen is greater than that between silicon and carbon, silicon has the largest positive partial charge, making these bonds, and consequently the often used SiOx barrier layers, particularly susceptible to damage.

[0045] The research revealed that, within a narrow process window of energy density, gas composition, process pressure, and temperature in the plasma, it is possible to retain the methyl groups contained in precursor molecules, such as hexamethyldisiloxane (HMDSO), in the plasma, preventing volume polymerization and thus incorporating them into the layers. Considering the structural formula and bond energy of the HMDSO molecule, PECVD of HMDSO in plasma first cleaves the methyl groups, and then the hydrogens. Typically, these groups are fragmented in the plasma, react with other particles to form volatile components, and leave the reaction space without participating in layer formation.

[0046] By retaining the methyl group, the stability of the layer can be enhanced through the mechanism of steric shielding. Sterishielding refers to the spatial shielding of weak bonds by substituents that fill adjacent spaces. In organic chemistry, a substituent is an atomic group (organyl group or other group) that replaces a hydrogen atom in a molecule (in this case, the methyl group).

[0047] Therefore, the use of oxygen as a reactive gas in the deposition of chemical-resistant passivation layers should be limited or even avoided. However, the addition of a large amount of oxygen is absolutely necessary to create the oxide SiOx layer (barrier layer). Consequently, it is insufficient to produce both functional layers solely by controlling the energy introduced during the process (e.g., by the pulse parameters of plasma excitation).

[0048] This invention relates to both coatings and methods for manufacturing coatings.

[0049] A first aspect of the present invention is the use of a gradient coating, formed by PECVD and having at least one oxidatively characterized barrier zone and an organically characterized passivation zone, for coating plastic containers for corrosive media (e.g., alkalis).

[0050] A gradient coating consists of numerous nanolayers with a resolution of several nanometers (up to 1 nanometer), and the material composition of each nanolayer gradually changes. Along the layer thickness, the material composition gradually changes from organic to oxide, or vice versa. Within a single nanolayer, the material composition of the layer is substantially uniform. The material composition of individual nanolayers is determined by process control of the PECVD process.

[0051] The barrier zone is characterized by oxidation and provides high barrier performance that prevents gas permeation through the container wall. Preferably, the barrier zone has a high concentration of Si-O-Si compound.

[0052] The passivation zone is organically characterized and provides high resistance to corrosive media, particularly alkaline media. The passivation zone is preferably located on top of the barrier zone to protect the barrier zone from environmental influences, especially corrosive media within the container. Preferably, the passivation zone has a high concentration of organic compounds, preferably CH3 and / or CH2 compounds, and a low concentration of oxide compounds, particularly low concentrations of Si-OH and Si-O-Si compounds.

[0053] Depending on the type of plastic substrate to which the coating is applied, it is advantageous to form an organically characterized adhesive zone between the plastic substrate and the oxide-based barrier zone.

[0054] Typically, polyolefins are coated with a bonding zone. However, some plastics, such as PET, can be made without this bonding zone.

[0055] In the first embodiment, the gradient coat includes at least one oxide-based barrier zone and an organic passivation zone (2-zone layer). In a further embodiment, the gradient coat includes an organic adhesive zone, an oxide-based barrier zone, and an organic passivation zone (3-zone layer).

[0056] Different zones gradually merge with each other. Each zone forms a continuous gradient coat with smooth transitions between zones. Each zone preferably has an oxide or organic center located either in the central region of the zone or in the edge region of the zone, depending on whether it is an edge zone of the gradient coat or a zone within the gradient coat. In certain embodiments, the coating may include multiple gradient coats. A gradient coat may also include multiple zones of the same type (passivation zones, barrier zones, or bonding zones).

[0057] A particular advantage of gradient coatings over composite coatings is that gradient coatings can be formed particularly uniformly, i.e., non-porous and with low residual stress. During the deposition of individual nanolayers, chemically similar nanolayers constantly combine, which prevents island growth.

[0058] The gradually fusing zones can be separated from each other in various ways. Preferably, each zone is separated by the proportion of organic compounds or oxide compounds. The gradient coat consists of numerous (approximately 80-1000) nanolayers with a thickness of several nanometers. If oxide compounds are predominant in a nanolayer, this nanolayer can be assigned as a barrier zone. If organic compounds are predominant in a nanolayer, this nanolayer can be assigned as a passivation zone or an adhesion zone.

[0059] A further aspect of the present invention involves varying the concentration of a reactive gas, preferably oxygen, used during the formation of the gradient coat in order to achieve a sufficiently strong gradient between the oxide barrier zone and the organic passivation or adhesion zone.

[0060] To form a gradient coating using the PECVD process, a process gas mixture is supplied to a pre-evacuated reaction space where the plastic substrate is placed. The process gas mixture includes one or more silicon-containing precursors, preferably hexamethyldisiloxane (HMDSO) and / or hexamethyldisilazane (HMDSN). The process gas mixture also includes at least one or more reactive gases, preferably oxygen, intermittently. In certain embodiments, further auxiliary gases, such as noble gases, may be added.

[0061] The composition of the process gas mixture, i.e., the mixing ratio, is preferably dynamically adjustable by a mass flow control device. In particular, the reactive gas mass flow rate, the precursor mass flow rate, and the ratio of the two mass flow rates to each other can be adjusted. In certain embodiments, multiple precursors and / or reactive gases can be used. In these cases, the ratio of the individual precursor mass flow rates to each other can also be controlled. Preferably, the ratio of the reactive gas mass flow rate to the precursor mass flow rate is adjusted.

[0062] The reactive gas content C can be expressed in particular by the following formula:

number

[0063] C: Reactive gas content RGF: Reactive Gas Mass Flow Rate PGF: Precursor mass flow rate.

[0064] The precursor mass flow rate can be obtained from the sum of multiple precursor mass flow rates.

[0065] Increasing the amount of reactive gas, particularly oxygen, added to the process, i.e., increasing the reactive gas content C, leads to a greater degree of fragmentation of silicon-containing monomers and a greater increase in oxidation of the film layer. This oxidation of the layer, in turn, correlates with the barrier effect and hydrolysis stability of the layer.

[0066] By controlling the reactive gas content, preferably the oxygen content, the material composition and, consequently, the function of the deposited nanolayer can be controlled over a wider range. In this way, a high barrier effect and strong passivation can be achieved in a uniform, i.e., non-porous layer structure.

[0067] A further aspect of the present invention involves controlling the excitation energy during the formation of a gradient coat, particularly in relation to the process gas involved in the reaction. Specifically, the excitation energy is controlled on a unit mass basis according to the composition of the process gas mixture. By precisely adjusting the excitation energy per unit mass, volume polymerization can be prevented, thereby preventing the formation of pores.

[0068] In plasma-assisted chemical vapor deposition (CVM), a process gas mixture is excited by an energy source to form a plasma. A magnetron is preferably used as the energy source. Excitation is preferably performed by microwaves. Preferably, the plasma is excited in a pulsed manner. Pulsed excitation prevents the plastic substrate from being overheated by the plasma.

[0069] Plasma excitation supplies energy to the reaction of the process gas. Excitation energy per unit mass represents the energy supplied to the reaction per unit mass of particles. By specifically adjusting the energy supplied per unit mass of particles, particularly uniform layers can be achieved.

[0070] It has been found that a completely poreless layer can be formed by controlling the excitation energy supplied to the reaction according to the process gas mixture. Preferably, the excitation energy per unit mass in each zone of the gradient coat is set to a specific process window according to the content of each reactive gas.

[0071] To calculate the excitation energy per unit mass, it is advantageous to correct the mass flow rate of the process gas involved in the reaction using a correction factor that takes into account the reactivity of the reactive gas. The correction factor for oxygen is K=0.6, and the correction factor for nitrogen is K=0.5.

[0072] The excitation energy per unit mass, also known as energy density, can be expressed by the following equation:

number

[0073] E: Excitation energy (energy density) per unit mass [J / kg] P p :Average pulse power [J / s] F c Corrected process gas flow rate [kg / s] P: Power [J / s] t on :Pulse-on time [s] t off :Pulse off time [s] PGF: Precursor mass flow rate [kg / s] RGF: Reactive gas mass flow rate [kg / s].

[0074] In a preferred embodiment, a relatively high excitation energy per unit mass, preferably 400 kJ / kg ≤ E ≤ 2700 kJ / kg, and particularly preferably 1800 kJ / kg ≤ E ≤ 2200 kJ / kg, is supplied to form a barrier zone with a relatively high reactive gas content, preferably 25 ≤ C ≤ 250, and particularly preferably 50 ≤ C ≤ 100.

[0075] For film deposition in the passivation zone, a relatively low to moderate excitation energy per unit mass, preferably 30 kJ / kg ≤ E ≤ 1700 kJ / kg, and particularly preferably 500 kJ / kg ≤ E ≤ 800 kJ / kg, is supplied with a relatively low reactive gas content, preferably 0 ≤ C ≤ 20, and particularly preferably 0 ≤ C ≤ 10.

[0076] For film formation in any adhesive zone, a relatively low excitation energy per unit mass, preferably 20 kJ / kg ≤ E ≤ 200 kJ / kg, and particularly preferably 30 kJ / kg ≤ E ≤ 140 kJ / kg, is supplied with a relatively low to moderate reactive gas content, preferably 0 ≤ C ≤ 50, and particularly preferably 0 ≤ C ≤ 30.

[0077] The interval limits listed herein are disclosed both individually and in combination, and contribute to the technical effects of the present invention. Accordingly, the lower or upper limits of each interval are also disclosed independently and explicitly.

[0078] A further aspect of the present invention involves forming a gradient coating, particularly individual zones, that are sufficiently thin. Advantageously, the total thickness of the coating is less than 1000 nanometers. Preferably, the coating thickness is up to 500 nanometers.

[0079] Thin coatings have low layer stress. The lower the layer stress, the lower the risk of cracking or failure of the coating under mechanical stress. In contrast to the relatively thick gradient coatings in the field of scratch-resistant coatings (e.g., for eyeglass lenses), the field of plastic containers has relatively high requirements in terms of mechanical load-bearing capacity. Thin-walled plastic containers are generally soft. The containers may deform during storage or transport (e.g., due to impact or stacking). Such deformation must be prevented from leading to damage to the coating. Thin coatings with a thickness of less than 1000 nanometers, preferably less than 500 nanometers, have been found to be particularly suitable for plastic containers, especially for storing corrosive media.

[0080] The zones formed in the gradient coating also preferably have a thickness optimized for their function and / or the coating formation process.

[0081] The thickness of any bonding zone is preferably a maximum of 10 nanometers. The bonding zone is preferably thinner than the barrier zone or passivation zone. Such a thin bonding zone is sufficient to protect the plastic substrate from the effects of oxidative degradation of the oxygen-rich plasma used for barrier zone deposition. Increasing the thickness of the bonding zone may increase pore formation during subsequent barrier zone deposition. Therefore, a thin bonding zone with a maximum thickness of 10 nanometers is advantageous for uniform layer formation. Such a thin bonding zone forms the most homogeneous possible base for subsequent barrier zone deposition.

[0082] The barrier zone preferably has a maximum thickness of 100 nanometers. This thin barrier zone is sufficient to form a adequate transition barrier. At the same time, uniform layer growth is possible. Preferably, the barrier zone is thinner than the passivation zone. A thin barrier zone is advantageous for crack-free layer growth.

[0083] Highly oxidized layers grow with inherent layer stresses. On the other hand, organically characterized passivation layers grow with almost no layer stress, and can therefore be made thicker.

[0084] The passivation zone has a preferred thickness of up to 800 nanometers. Since the passivation zone must ensure adequate protection of the barrier zone against the effects of the corrosive medium within the container, the passivation zone can be thicker than the barrier zone.

[0085] The coating can consist of one or more gradient coats. To enhance the protective effect, the gradient coat structure described above can be repeated in multiple consecutive gradient coats. In the zones located at the edges of the coating, the center of the organic or oxide material is usually at the outer edge, i.e., facing the medium or substrate. In the zones located inside the gradient coat, the center of the oxide or organic material is usually in the center.

[0086] In contrast to composite coatings, which apply different types of layers sequentially, gradient coatings always have chemically similar surfaces, thus promoting layer growth and preventing pore formation in coalescing islands.

[0087] By adjusting the gas flow rate, i.e., the composition of the process gas mixture, the required chemical configuration of the barrier and passivation zones can be set. By precisely controlling the energy introduced per molecule according to the process gas mixture, volume polymerization can be further prevented, thereby preventing large oligomers from participating in layer formation and creating pores.

[0088] Therefore, the method according to the present invention can be used to produce a layer that has high barrier performance against gases and other permeable substances, while also having high stability against corrosive media and other environmental influences because the upper layer is chemically stable and non-porous.

[0089] Depending on the surface quality, volume, and weight of the container, polyethylene containers coated with a gradient coating can achieve a barrier effect of 50 to 2000 times in terms of oxygen permeability. Furthermore, the gradient coating retains its resistance and barrier properties even after long-term storage in highly alkaline NaOH solutions or similar corrosive chemicals. This means that gradient coatings can be used to make packaging made from classic packaging plastics such as PE and PET suitable for storing sensitive chemicals.

[0090] It is conceivable that other suitable metalloids or metals may be used in place of silicon in the present invention. The present invention is not limited to silicon-based starting materials or coatings. Other (semi)metallic monomers may be used in place of, or in addition to, the preferred precursors HMDSO and HMDSN. Furthermore, other reactive gases, such as nitrogen, may be used in place of, or in addition to, oxygen. This disclosure also includes embodiments in which alternatives mentioned herein or known to those skilled in the art of PECVD are used in place of the preferred process gases.

[0091] Further advantageous embodiments are described below with reference to the drawings.

[0092] The present invention is illustrated schematically and illustratively in the drawings. [Brief explanation of the drawing]

[0093] [Figure 1] This is a diagram showing the structure of the reactor. [Figure 2] This diagram shows the structure of a gradient court (3-zone court). [Figure 3] This figure shows the structure of a coating having multiple gradient coats. [Figure 4] This figure shows the favorable transitions of process parameters C and E during the deposition of the gradient layer. [Figure 5] This figure shows the FT-IR spectra at the center of the adhesion zone (EH) and barrier zone (WB). [Figure 6] This figure shows the FT-IR spectrum at the center of the passivation zone.

[0094] Figure 1 shows a schematic structure of the reactor (300). The reactor (300) includes a process chamber (301). A substrate (100) is placed inside the process chamber (301). A reaction space (302) is formed inside or on the plastic substrate (100). The reaction space (302) can be evacuated by a pump (310). In the illustrated embodiment, the reaction space is formed inside a container (100), thereby covering the inside of the plastic container (100), for example, a canister.

[0095] A process gas mixture (PGM) is supplied to the reaction space (302) through a line. The reactor comprises a gas supply unit (320) and one or more gas flow control devices (321), preferably a mass flow control device. The process gas mixture (PGM) consists of one or more process gases (PG1, PG2, RG), and their mixing ratio is controllable.

[0096] In a preferred embodiment, two precursors are used. The first precursor (PG1) is preferably HMDSN. The second precursor (PG2) is preferably HDMSO.

[0097] In particular, one or more precursors (PG1, PG2) can be used in specific zones of the gradient coat. It is especially advantageous to use (mainly) HMDSO as the first precursor for deposition of the adhesion zone (201) and / or passivation zone (203). Alternatively or additionally, it is especially advantageous to use (mainly) HMDSN as the second precursor for deposition of the barrier zone (202).

[0098] In particular, at the transition zone between two zones of the gradient coat, two or more precursors can be mixed at least temporarily.

[0099] The precursor gas mass flow rate is preferably the sum of the mass flow rates of multiple precursors. For chemically similar precursors (e.g., HMDSN and HMDSO), the individual precursor mass flow rates in the process gas mixture can be combined to obtain a calculated precursor gas mass flow rate for determining the excitation energy per unit mass. In some embodiments, it may be useful to weight the individual gas mass flow rates with coefficients.

[0100] Preferably, oxygen is used as the reactive gas (RG). Alternatively or additionally, nitrogen may be used as the (further) reactive gas (RG).

[0101] In the reaction space (302), the process gas mixture (PGM) is excited by an energy source (350). A magnetron is preferably used as the energy source (350). The plasma is preferably excited by pulsed microwaves (351). Alternatively or additionally, an ICP plasma may be used.

[0102] The coating (200) is deposited on a plastic container (100) from a process gas mixture excited by a plasma (352).

[0103] The process chamber (301) may comprise one or more reaction spaces (302). The reaction spaces (302) may occupy the entire process chamber or only a portion of it. In particular, the reaction spaces (302) may be formed inside a plastic container (100). Preferably, the container is sealed. Alternatively or additionally, further reaction spaces may be formed, for example, outside the container.

[0104] The reactor (300) may also comprise multiple process chambers (301) each having one or more reaction spaces (302).

[0105] Depending on the structure of the coating (200), the size of the substrate (100), and the process control, the coating (200) is preferably deposited over a period of about 5 to 60 seconds. For particularly large containers, the process may take longer. During the deposition process, at least one gradient coat is deposited.

[0106] The mixing ratio of the process gas mixture (PGM) is changed during the process. In particular, the mass flow ratio of the precursors (PG1, PG2) and / or the reactive gas (RG) is changed. By changing the process gas, the material composition of the coating (200) is affected.

[0107] The favorable progression of process parameters is shown in Figure 4.

[0108] Preferably, the reactive gas content (C) and / or excitation energy per unit mass (E) between the adhesion zone (201) and the barrier zone (202) are gradually increased along the layer construction direction (x).

[0109] Alternatively or additionally, the reactive gas content (C) and / or excitation energy per unit mass (E) between the barrier zone (202) and the passivation zone (203) are gradually reduced along the layer construction direction (x).

[0110] The changes in reactive gas content (C) and excitation energy per unit mass (E) are preferably uniform, and in particular, stepless.

[0111] Particularly advantageous is that the excitation energy (E) is controlled according to the composition of the process gas mixture (PGM), and especially according to the mass flow rate of the precursor gas and / or the mass flow rate of the reactive gas.

[0112] Several options are available to those skilled in the art for controlling the excitation energy per unit mass. In particular, the average pulse power can be set. Advantageously, the power and / or pulse parameters of the energy source are controlled. It is particularly advantageous to calculate a set value for the excitation energy (E) per unit mass and control or adjust it with one or more operational variables, such as the (nominal) power supply, pulse-on time, pulse-off time, or pulse rate, in a selection or combination.

[0113] Figure 2 shows the schematic structure of a coating (200) having a gradient coat (200') as a three-zone layer. The coating (200) is deposited on a plastic substrate (100). The deposition of the coating, i.e., the construction of the nanolayer (L), is carried out along the layer construction direction (x).

[0114] The appropriate coating thickness (d) is preferably in the range of 80 to 1000 nanometers. The plastic substrate (100) is several orders of magnitude thicker. The typical wall thickness of plastic containers is in the range of millimeters. Therefore, the plastic substrate is shown broken for general expressibility.

[0115] In the three-zone layer (Figure 2), an organically characterized adhesive zone (201) is first deposited on the substrate (100). Next, an oxidatively characterized barrier zone (202) is deposited on the adhesive zone (201), where these zones are smoothly fused together. An organically characterized passivation zone (203) is deposited on the barrier zone (202).

[0116] In the case of a two-zone layer, the barrier zone (202) can also be deposited directly onto the substrate.

[0117] The gradient coating (200') includes at least a barrier zone (202) and a passivation zone (203). The passivation zone (203) is located between the environmental surface (211) of the coating (200) and the barrier zone (202). The passivation zone (203) protects the barrier zone (202). The passivation zone is resistant to the effects of an erosive medium (M).

[0118] The coating (200) forms a migration barrier, or diffusion barrier, for ambient gas (A) that may diffuse through the plastic substrate (100). The permeation path is blocked by forming one or more barrier zones (202). The oxide-based barrier zones (202) act as migration barriers.

[0119] The gradient coating (200') is constructed from numerous nanolayers (L) during the deposition process. The material composition of each nanolayer (L) gradually changes along the layer construction direction (x).

[0120] The gradient (G) schematically shows the gradual progression of the material composition of the gradient coat.

[0121] Each zone, namely the adhesive zone (201), barrier zone (202), and passivation zone (203), can be described based on their material composition and the proportion of specific bonding types. The center of each zone can be considered representative of the gradually changing composition within that particular zone. Each center (S1, S2, S3) of a given zone can be considered a specific nanolayer (L) at the extreme of a specific characteristic curve, e.g., a gradient (G), along the layer construction direction (x).

[0122] The chemical structure of a gradient coating is defined by its poles (centers), particularly local or global maxima or minimum, at which the maximum coating properties for each coating type are set, and process control is adjusted from there to achieve the next limit. The chemical structures at the poles (S1, S2, S3) are described in detail below. Table 1 shows the preferred elemental composition of the layers at the poles, as determined by X-ray photoelectron spectroscopy (XPS).

[0123] [Table 1]

[0124] Fourier transform infrared spectroscopy (FT-IR) is used to further characterize the chemical structures of various zones, particularly the centers of each zone. Table 2 lists the vibrational modes important for evaluating FTIR measurements.

[0125] [Table 2]

[0126] In Table 2, prefixes are s = contraction; b = bending; r = oscillation; and subscripts are sym = symmetry.

[0127] Figures 5 and 6 illustrate the FT-IR spectra of the poles of each zone. The parameter W is in cm. -1 The wavenumber is shown, and the dimensionless parameter X represents the absorbance.

[0128] Figure 5 shows the FT-IR spectra at the center of the HMDSO-based adhesion-promoting zone (EH) and the center of the HMDSN-based barrier zone (WB).

[0129] The coating at the extreme end of the barrier zone (WB) (see center S2 in Figure 2) exhibits a very prominent Si-O-Si network structure (440 cm²). -1 and 1070cm -1) is shown. 900-1,300 cm -1 broadband peak can be primarily assigned to the three asymmetric Si-O stretching vibrations of Si-O-Si compounds. 1135 cm -1 peak nearby can be assigned to Si-O-Si cage structures with a bond angle of approximately 150°. Network structures with a bond angle of approximately 144° are associated with 1070 cm -1 peak nearby. If the structures have bond angles less than 144°, suboxides are considered to be present in the network (1010-1030 cm -1 ). 839 cm -1 peak is characteristic of stretching and rocking vibrations of methyl groups and indicates that, at the focus of the adhesion-promoting zone (EH), a higher retention of these functional groups from the monomer is achieved compared to the barrier zone (WB), which imparts organic characteristics to this zone.

[0130] The intensity and exact peak position of the Si-O-Si network peaks provide information about the degree of crosslinking of the layer. The higher the maximum peak position, the higher the degree of Si-O-Si crosslinking. Such peak shifts can be clearly seen by comparing the two spectra. The barrier zone (WB) is a highly crosslinked coating with a pronounced Si-O-Si network structure, with little C and C-H bonding.

[0131] Figure 6 shows an exemplary FT-IR spectrum at the center of the passivation zone. This figure shows the FT-IR spectrum of an HMDSO-based passivation zone (EP).

[0132] Similar to the spectrum of the adhesion zone (EH) in Figure 5, three particularly prominent peaks can be observed in the spectrum of the passivation zone in Figure 6. 700-900 cm -1 peak in the nearby range consists of a superposition of a series of individual peaks. The peak at a wavenumber of 1070 cm -1 is also due to the stretching vibrations of the Si-O-Si network. 1257 cm -1The peak is characteristic of the symmetric stretching vibration of the methyl group.

[0133] The chemical structure of each zone is extremely important, particularly with respect to the barrier performance of the barrier zone and the hydrolysis stability of the passivation zone.

[0134] Therefore, a structural parameter V was introduced to characterize the chemical structure of each zone. This parameter represents the ratio of the area below the peaks (Gaussian curve) measured by FT-IR, and each peak can be clearly assigned to either a CH3 group or a Si-O group (the peak assignments are shown in Table 2).

[0135]

number

[0136] V: Structural parameter [-] A: W=1376cm -1 Absorbance X[-] B:W = 1257cm -1 Absorbance X[-] E:W=839cm -1 Absorbance X[-] C:W=440cm -1 , 1010cm -1 ~1035cm -1 , 1070cm -1 Absorbance X[-] D:W = 930cm -1 Absorbance X[-] at this point.

[0137] Regarding the chemical structure, the barrier performance of the barrier zone is mainly determined by the degree of crosslinking and oxidation of the layers. At the extreme end of the barrier zone (WB), a favorable range of V < 0.2, and especially a favorable range of V < 0.05, was determined.

[0138] The chemical resistance of the passivation zone can be explained by considering the electronegativity of the elements contained in the coating material, and this electronegativity can be used to evaluate the local partial charge shift of the bond. The greater the difference in electronegativity between the bonding partners, the more strongly the bonding electrons are localized at the bonding partner with the higher electronegativity. As a result, this element experiences an electron boost.

[0139] Of the bonds present in the layer, the oxygen in Si-O in particular experiences the greatest electron boost. As a result, the oxygen is negative (δ - ), the silicon is positive (δ + ) carries a partial charge. As a result, silicon is electron deficient. As a result, negatively charged ions in solution attack the silicon bonded to oxygen due to its positive partial charge. Si-CH3 bonds, in turn, have a low partial charge. As a result, this layer is nucleophilically attacked by ions such as Si-O. This results in Si-OH bonds under bond cleavage of the Si-O-Si bond. As a result, the introduction of anionic end groups creates more and more gaps in the Si-O network. Weak bonds are sterically shielded by CH3 groups, which can significantly delay or completely stop the reaction. The greater the ratio of CH3 groups to Si-O, the more the progression of layer degradation can be delayed. The greater V, the greater the durability of the coating. Preferably, in order to be able to provide the required protective properties, at least one structural parameter V>0.20, particularly advantageously V>0.35, is achieved at the extreme of the passivation zone.

[0140] In order to deposit an advantageous adhesion-promoting layer, a structural parameter V of 0.1<V<0.3 is achieved at the extreme of the adhesion-promoting zone (EH).

[0141] The structural parameter V can be used to determine the center and / or functional zones of the oxide or organic material in the gradient coat. For example, in Figure 2, a schematic curve of the structural parameter V(x) is plotted along the layer construction direction x. The limits (S1, S2, S3) of the structural parameter V(x) can be used to determine the center of the gradient coat and the individual functional zones of the gradient coat.

[0142] The center of each oxide or organic material within a zone can be located at the edge or in the center of the zone, depending on the layer structure. Transitions between zones are fluid.

[0143] The zones are preferably determined by their material composition. The material composition of each nanolayer determines the function of the layer zone.

[0144] Various types of analysis can be used to demarcate zones (201, 202, 203) and, for example, to determine thicknesses (d1, d2, d3). For instance, the material composition of individual nanolayers can be determined by SIMS (Secondary Ion Mass Spectrometry) or even nanoSIMS. By bombarding the surface with ions, layers can be removed and analyzed with nanometer resolution.

[0145] To determine the zone thickness, the structural parameter V or elemental composition of the nanolayer along the layer construction direction can be determined. If organic compounds are predominant, this location can be assigned to a passivation zone or an adhesion zone. If oxide compounds are predominant, this location can be assigned to a barrier zone.

[0146] The material composition of two adjacent nanolayers (L) is always similar. This similarity in the materials of individual nanolayers (L) is advantageous for uniform layer growth.

[0147] The advantage of the stepped structure of the gradient coating zones is that each nanolayer (L) finds a chemically similar base during deposition. The chemical properties of the nanolayers change only gradually. This prevents the growth of islands.

[0148] Figure 3 shows an exemplary structure of a coating (200) having multiple gradient coats (200', 200'', 200''''). The structure of the gradient coats or individual zones can be repeated along the layering direction. Preferably, the zones between two consecutive gradient coats (200', 200'') also gradually fuse with each other.

[0149] The multilayer structure of gradient coatings can be particularly advantageous for enhancing transition barriers and / or chemical resistance, i.e., protection of the barrier zones. However, alternatively or additionally, it is also possible to maintain low thicknesses in individual zones, which is advantageous for uniform layer growth and the mechanical properties of the coating (e.g., low layer stress).

[0150] In embodiments not shown in particular, the coating (200) may also include a gradient coat (200''') having only one barrier zone (202) and one passivation zone (203). In particular, with PET substrates, the adhesive zone (201) can be omitted.

[0151] In the case of a two-zone layer (200''), the barrier zone (202) is preferably located directly on the plastic substrate (100) or on an intermediate gradient coat (200', 200''). In the case of a two-zone layer, the barrier zone (202) may have oxide centers located at the edges of the zone.

[0152] Figure 4 shows the favorable transition of reactive gas content (C) or excitation energy per unit mass (E) during film formation of a gradient coat (200') having an adhesion zone (201), a barrier zone (202), and a passivation zone (203).

[0153] In particular, process variables C and E can each be controlled or adjusted within a specific process window (W).

[0154] The adhesive zone (201) is deposited with a low to moderate reactive gas content (C). In an advantageous embodiment, at least a small amount of oxygen is added at the start of the process. The surface of the plastic substrate (210) is activated by the resulting oxygen-rich plasma. In this way, prior surface activation of the substrate (100) can be omitted, thereby shortening the process time. Surface activation improves the adhesion of the coating (200) to the substrate surface.

[0155] The adhesive zone (201) protects the sensitive plastic substrate (100), particularly polyolefins, from the oxide-based barrier zone (202). In this respect, the adhesive zone (201) has a protective effect on the plastic substrate.

[0156] Stepwise changes in the reactive gas content (C) and / or excitation energy per unit mass (E) control the gradient (G) of the material composition of the deposited layer and promote the growth of a uniform, non-porous layer.

[0157] At certain stages of the film deposition process, the proportion of (at least one) reactive gas (RG) in the process gas mixture can be between 0% and 100%. It may be appropriate to use a very high reactive gas content (C), preferably 50 ≤ C ≤ 100, to deposit strongly oxidized regions. Alternatively or additionally, it may be advantageous to use a low reactive gas content (C) or no reactive gas at all in the organic regions of the gradient coat.

[0158] In particularly advantageous embodiments, the plasma excitation energy (E) is controlled according to the current process gas composition. It is especially advantageous to keep the energy introduced per unit mass of particles within a constant range and to adapt this range to varying reactive gas content.

[0159] By varying the reactive gas content, a wide range of material compositions between oxide and organic components in the gradient coating can be achieved. As a result, particularly strong barrier and passivation effects can be achieved, thereby providing sufficient migration barriers and chemical resistance against corrosive media containers.

[0160] By adjusting the excitation energy (E) per unit mass, excitation and, consequently, the reaction can be kept within an optimal range for uniform layer growth (even with significant changes in gas composition). This means that volume polymerization can be avoided, which in turn enables the formation of non-porous layers.

[0161] Individual features of the embodiments described, illustrated, or claimed herein can also be combined with each other. Each feature can be substituted or supplemented by individual features of other embodiments. [Explanation of Symbols]

[0162] 100 Plastic base material 200 Coating 200' Gradient Coat 201 Contact Zone 202 Barrier Zone 203 Passivation Zone 210 Base material surface, base material surface 211 Environmental aspects S1 Mainly organic matter S2 oxide center S3 Mainly organic matter 300 reactors 301 Process Chamber 302 Reaction Space 310 pump 320 Gas Supply Department 321 Gas flow control device 350 Energy source, magnetron 351 Microwave 352 Plasma PGM process gas mixture PG precursor, polysiloxane PG1 (first) precursor, HMDSN PG2 (second) precursor, HMDSO RG Reactive gas, oxygen A Ambient gas C Reactive gas content E Excitation energy per unit mass Fc-corrected process gas flow rate G gradient K correction factor L nanolayer M medium P power supply r resolution RGF Reactive Gas Mass Flow Rate PGF precursor gas mass flow rate ton pulse-on time toff pulse off time W Process window x layer construction direction

Claims

1. A method for producing a coating (200) for forming a chemical migration barrier on a plastic substrate (100), particularly on a plastic container, by plasma-enhanced chemical vapor deposition (PECVD), comprising: supplying a process gas mixture (PGM) to a reaction space (302); and exciting it with excitation energy (E) by an energy source (350) to form a plasma (352), wherein the process gas mixture (PGM) comprises one or more precursors (PG), or one or more precursors (PG) and 1 A gradient coat (200') having an adjustable composition of one or more reactive gases (RG), wherein the process gas mixture (PGM) comprises one or more silicon-containing precursors (PG, PG1, PG2), particularly organosilicon compounds, siloxanes, silazanes or silanes, and the reactive gas (RG) comprises oxygen and / or nitrogen, and having an adhesion zone (201), a barrier zone (202) and a passivation zone (203), or a barrier zone (202) and a passivation zone (20 3) A method for forming a gradient coat (200'') having the above on a substrate (100), wherein the formation of the gradient coat (200'', 200'') is controlled by changing the reactive gas content (C) in the process gas mixture (PGM), the excitation energy (E) is controlled on a unit mass basis according to the precursor gas mass flow rate and the reactive gas mass flow rate, and the excitation energy (E) per unit mass is gradually reduced for the formation of an organically characterized passivation zone (203) on an oxidatively characterized barrier zone (202), the gradient coat is composed of a number of nanolayers having a thickness of several nanometers, the oxidatively characterized barrier zone (202) is a nanolayer in which oxide compounds predominate over organic compounds, and the organically characterized passivation zone (203) is a nanolayer in which organic compounds predominate over oxide compounds.

2. The method according to claim 1, wherein the process gas mixture (PGM) comprises hexamethyldisiloxane (HMDSO) and / or hexamethyldisilazane (HMDSN).

3. The method according to claim 1 or 2, wherein one or more pulse parameters of the energy source (350), particularly the ratio of the pulse-on time to the pulse-off time of the excitation pulse, are kept at least temporarily constant during the deposition of the gradient coat, particularly during the deposition of the adhesion zone (201) and / or the barrier zone (202).

4. The method according to claim 1 or 2, wherein the reactive gas content (C) and / or the excitation energy per unit mass (E) are gradually increased along the layer construction direction (x) between the adhesive zone (201) and the barrier zone (202).

5. The method according to claim 1 or 2, wherein the reactive gas content (C) is gradually reduced along the layer construction direction (x) between the barrier zone (202) and the passivation zone (203).

6. The method according to claim 1 or 2, wherein the excitation energy (E) is adjusted according to the mass of particles involved in the film formation reaction.

7. The method according to claim 1 or 2, wherein the plasma is excited by pulsed microwaves (351).

8. The method according to claim 1 or 2, for which the plasma excitation power source (P) and / or pulse parameters, in particular the pulse-on time (ton) and / or the pulse-off time (toff), pulse rate, or pulse ratio are controlled for the change in excitation energy (E).

9. The method according to claim 1 or 2, wherein, during the film formation of the barrier zone (202), the reactive gas content (C) is 25 ≤ C ≤ 250 or 50 ≤ C ≤ 100, and / or the excitation energy (E) per unit mass is 400 kJ / kg ≤ E ≤ 2700 kJ / kg or 1800 kJ / kg ≤ E ≤ 2200 kJ / kg.

10. The method according to claim 1 or 2, wherein, during the film formation in the passivation zone (203), the reactive gas content (C) is 0 ≤ C ≤ 20 or 0 ≤ C ≤ 10, and / or the excitation energy (E) per unit mass is 30 kJ / kg ≤ E ≤ 1700 kJ / kg or 500 kJ / kg ≤ E ≤ 800 kJ / kg.

11. The method according to claim 1 or 2, wherein during film formation of the adhesive zone (201), the reactive gas content (C) is 0 ≤ C ≤ 50 or 0 ≤ C ≤ 30, and / or the excitation energy (E) per unit mass is 20 kJ / kg ≤ E ≤ 200 kJ / kg or 30 kJ / kg ≤ E ≤ 140 kJ / kg.

12. The method according to claim 1 or 2, wherein one of hexamethyldisilazane (HMDSN), hexamethyldisiloxane (HMDSO), and hexamethyldisilazane (HMDSN) is used as a precursor (PG1) for forming the barrier zone (202).

13. The method according to claim 1 or 2, wherein one of hexamethyldisilazane (HMDSN), hexamethyldisiloxane (HMDSO), and hexamethyldisiloxane (HMDSO) is used as a precursor (PG2) for forming the adhesive zone (201) and / or the passivation zone (203).

14. A coating for a plastic substrate (100) for forming a chemical migration barrier, particularly for plastic containers, wherein the coating (200) comprises one or more gradient coats (200', 200'', 200''''), and at least one of the gradient coats is an organosilicon compound (SiO₂) formed from one or more silicon-containing precursors, particularly siloxanes, silazanes, or silanes. x C y H z ) comprising, at least one gradient coat comprising at least one oxidatively characterized barrier zone (202) and an organically characterized passivation zone (203), wherein the gradient coat is composed of numerous nanolayers having a thickness of several nanometers, the oxidatively characterized barrier zone (202) is a nanolayer in which oxide compounds predominate over organic compounds, the organically characterized passivation zone (203) is a nanolayer in which organic compounds predominate over oxide compounds, the chemical composition of the gradient coat gradually changes along the layer construction direction (x) starting from the substrate surface (210) of the coating, and changes from at least one barrier zone (202) to the passivation zone (203), where the chemical structure of the gradient coat is determined by a structural parameter V measurable using Fourier transform infrared spectroscopy (FT-IR): [Math 1] Here, A:W=1376cm -1 absorbance B:W=1257cm -1 absorbance E: W = 839 cm -1 absorbance C: W = 440 cm -1 , 1010 cm -1 to 1035 cm -1 , 1070 cm -1 absorbance at D:W = 930cm -1 absorbance A coating characterized in that the structural parameter V at the maximum point (S3) in the passivation zone (203) is V > 0.

2.

15. The coating according to claim 14, wherein the gradient coat (200') further comprises at least one organically characterized adhesive zone (201) between the barrier zone (202) and the substrate surface (210).

16. The coating according to claim 14 or 15, wherein the thickness (d1) of the adhesive zone (201) is a maximum of 10 nanometers.

17. The coating according to claim 14, wherein the thickness (d) of the coating (200) and / or the thickness (d) of the at least one gradient coat (200', 200'', 200'''') is less than 1,000 nanometers or less than 500 nanometers.

18. The coating according to claim 14, wherein the thickness (d2) of the barrier zone (202) is less than 100 nanometers, less than 60 nanometers, or less than 40 nanometers.

19. The coating according to claim 14, wherein the thickness (d3) of the passivation zone (203) is at least 20 nanometers, or at least 200 nanometers and / or up to 800 nanometers.

20. The coating according to claim 14, wherein the chemical structure of the gradient coat (200) is constructed from a plurality of nanolayers (L, L') along the layer construction direction (x) with a resolution (r) of less than 50 nanometers, less than 10 nanometers, or 1 to 5 nanometers.

21. Each individual nanolayer (L, L') has a different elemental composition and / or organic compound, particularly organosilicon compounds (SiO2). x C y H z ) and oxide compounds, especially silicon oxide compounds (SiO x The coating according to claim 20, having the composition of ).

22. The coating according to claim 14, wherein the structural parameter V at the extreme portion (S2) of the barrier zone (201) is smaller than the structural parameter V at the extreme portion (S3) of the passivation zone (203).

23. The coating according to claim 14, wherein the structural parameter V in the extreme portion (S2) of the barrier zone (201) is V < 0.2 or V < 0.

05.

24. The coating according to claim 14, wherein the structural parameter V in the extreme portion (S3) of the passivation zone (203) is V > 0.

35.

25. The coating according to claim 14, wherein the structural parameter V at the extreme portion (S1) of the adhesive zone (201) is 0.1 < V < 0.

3.

26. A plastic container having the coating described in claim 14.

Citation Information

Patent Citations

  • Multifunctional encapsulation layer structure for photovoltaic semiconductor components and method for their production

    DE19732217C2

  • Process for the production of a graded layer

    EP0718418A1

  • Method for producing silicon-containing film