Coating solution and film formation method

A solvent mixture of cyclic ether and ester solvents with N-alkylmaleimide polymers addresses gelation and residual solvent issues, enabling stable, low-temperature film formation without chlorine-based solvents.

JP7954897B2Active Publication Date: 2026-11-24TOSOH CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022155430
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-27
Filing Date
2022-09-28
Publication Date
2026-11-24
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Existing coating solutions using N-alkylmaleimide polymers face issues with gelation when stored at room temperature and require high-temperature drying to reduce residual solvent content, while chlorine-based solvents pose health and environmental risks.

Method used

A coating solution comprising a solvent mixture of cyclic ether and ester solvents, specifically 1,3-dioxolane and methyl acetate, is used with an N-alkylmaleimide polymer, allowing for low-temperature drying to prevent gelation and minimize residual solvent.

Benefits of technology

The solution effectively suppresses gelation and reduces residual solvent content in the film, ensuring stable storage and low-temperature drying without using harmful chlorine-based solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954897000001
    Figure 0007954897000001
  • Figure 0007954897000002
    Figure 0007954897000002
  • Figure 0007954897000003
    Figure 0007954897000003
Patent Text Reader

Abstract

To provide a coating liquid that can suppress gelation without using a chlorine-based solvent, and when formed into a film, can be dried at a low temperature and yield a film of small amount of residual solvent.SOLUTION: The present invention provides a coating liquid that comprises a solvent containing a cyclic ether-based solvent by 1 to 100 wt.% and an ester-based solvent by 0 to 99 wt.%, and an N-alkylmaleimide-based polymer. The present invention also provides a film-forming method of coating the coating liquid on a substrate and drying the coating liquid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a coating solution and a film-forming method, and more particularly to a coating solution comprising an N-alkylmaleimide polymer and a film-forming method using the same. [Background technology]

[0002] Homopolymers or copolymers obtained from N-alkylmaleimide (N-alkylmaleimide polymers) are known to exhibit higher heat resistance and superior transparency compared to general thermoplastic vinyl polymers. N-alkylmaleimide polymers are promising materials as transparent resins that can be used in a variety of applications in the field of optics (see, for example, Non-Patent Document 1).

[0003] On the other hand, N-alkylmaleimide polymers, including alternating copolymers of N-alkylmaleimide and vinyl aromatic hydrocarbons such as styrene, have been reported to enable the creation of polymer materials with simple compositions that exhibit low birefringence and can maintain that low birefringence over a wide range of ambient temperatures (see, for example, Patent Document 1).

[0004] As a method for producing films of these N-alkylmaleimide polymers, an efficient manufacturing method has been proposed in which a coating solution containing the N-alkylmaleimide polymer and a solvent is applied to a substrate, and the coating is dried by blowing drying air onto the coated surface while gradually increasing the temperature of the drying air (see, for example, Patent Document 2). However, coating solutions containing high molecular weight N-alkylmaleimide polymers may gel when stored at or near room temperature.

[0005] Furthermore, a method using chlorine-based solvents has been proposed (see, for example, Patent Document 1). However, chlorine-based solvents raise concerns about their harmful effects on health and the environment, and high-temperature drying is required during film formation in order to efficiently produce films with low residual solvent content. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 2020-126229 [Patent Document 2] Japanese Patent Publication No. 2010-96905 [Non-patent literature]

[0007] [Non-Patent Document 1] Takayuki Otsu, "Future Materials," Vol. 3, No. 1, pp. 74-79. [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] The present invention has been made in view of the above problems, and aims to provide a coating liquid that can suppress gelation without using chlorine-based solvents and that, when a film is formed, can be obtained with a small amount of residual solvent by low-temperature drying. [Means for solving the problem]

[0009] In order to solve the above problems, the inventors of the present invention conducted diligent research and, as a result, discovered a coating solution consisting of a specific solvent and an N-alkylmaleimide polymer, thereby completing the present invention.

[0010] In other words, one aspect [1] of the present invention relates to a coating solution comprising a solvent consisting of 1 to 100% by weight of a cyclic ether solvent and 0 to 99% by weight of an ester solvent, and an N-alkylmaleimide polymer.

[0011] In one embodiment of the coating liquid according to the present invention [2], in [1], the content of the cyclic ether solvent in the solvent is 1 to 50% by weight, and the content of the ester solvent in the solvent is 50 to 99% by weight.

[0012] In one embodiment of the coating solution according to the present invention [3], in [1] or [2], the cyclic ether solvent is 1,3-dioxolane.

[0013] In one aspect [4] of the coating liquid according to the present invention, in any one of [1] to [3], the ester solvent is methyl acetate.

[0014] In one aspect [5] of the coating liquid according to the present invention, in any one of [1] to [4], the structural unit of the N-alkylmaleimide polymer is represented by the following general formula (1): Contains N-alkylmaleimide residue units.

[0015] [Chemical formula]

[0016] In general formula (1), R represents a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms.

[0017] In one aspect [6] of the coating liquid according to the present invention, in any one of [1] to [5], the N-alkylmaleimide polymer has a weight average molecular weight of 800,000 to 1,500,000.

[0018] One aspect [7] of the present invention is a coating liquid comprising a solvent consisting of 1 to 100% by weight of a cyclic ether solvent and 0 to 99% by weight of an ester solvent, and an N-alkylmaleimide polymer. The present invention relates to a film forming method in which a liquid is coated on a substrate and dried.

[0019] In one aspect [8] of the film forming method according to the present invention, in [7], drying is performed at a temperature from room temperature to 160°C. [Effects of the Invention]

[0020] According to the present invention, it is possible to suppress gelation without using a chlorinated solvent, and it is possible to provide a coating liquid that can produce a film with a small amount of residual solvent by low-temperature drying when forming a film. [Mode for Carrying Out the Invention]

[0021] The various aspects of the present invention will be described in detail below. In this specification, numerical ranges indicated using "~" represent a range that includes the numbers before and after "~" as the minimum and maximum values, respectively.

[0022] <Coating liquid> A coating solution according to one aspect of the present invention comprises a solvent consisting of a cyclic ether solvent and an ester solvent, and an N-alkylmaleimide polymer. Examples of the cyclic ether solvent include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 1,4-dioxane. Among these, tetrahydrofuran or 1,3-dioxolane are preferred, and 1,3-dioxolane is particularly preferred, due to their excellent solubility of the N-alkylmaleimide polymer, the solution stability of the coating solution, and the effect of reducing the amount of residual solvent in the film after film formation.

[0023] The content of cyclic ether solvent in the solvent is 1 to 100% by weight. Since a film with a small amount of residual solvent can be obtained by low-temperature drying after film formation, the content of cyclic ether solvent in the solvent is preferably 1 to 50% by weight, and particularly preferably 1 to 30% by weight.

[0024] Examples of the ester-based solvents mentioned above include methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, and n-propyl acetate. Among these, methyl acetate or ethyl acetate are preferred, and methyl acetate is particularly preferred, due to their excellent solubility of N-alkylmaleimide polymers and their effect in reducing residual solvent volume.

[0025] The content of ester-based solvents in the solvent is 0 to 99% by weight. Since a film with a small amount of residual solvent can be obtained by low-temperature drying during film formation, the content of ester-based solvents in the solvent is preferably 50 to 99% by weight, and particularly preferably 70 to 99% by weight.

[0026] In the above-mentioned solvents, a preferred combination of a cyclic ether solvent and an ester solvent is the combination of 3-dioxolane and methyl acetate. In this combination, from the viewpoint of improving solution stability and reducing the amount of residual solvent in the optical film by low-temperature drying, the preferred content of 3-dioxolane in the solvent is 10 to 50% by weight, and the preferred content of methyl acetate in the solvent is 50 to 90% by weight.

[0027] In a coating liquid according to one aspect of the present invention, the solvent is substantially composed of only the aforementioned cyclic ether solvent and ester solvent. Here, "substantially composed of" means that the solvent may contain other solvents other than the cyclic ether solvent and ester solvent, as added later, to the extent that the effects of this embodiment can be obtained.

[0028] In one aspect of the present invention, the N-alkylmaleimide polymer is an N-alkylmaleimide homopolymer or a copolymer of N-alkylmaleimide and other copolymerizable monomers. The N-alkylmaleimide residue unit that constitutes the N-alkylmaleimide polymer is preferably an N-alkylmaleimide residue unit represented by the following general formula (1).

[0029] [ka]

[0030] In the N-alkylmaleimide residue unit represented by general formula (1), R represents a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms. In N-alkylmaleimide polymers, R may be the same or different.

[0031] Examples of linear alkyl groups having 1 to 12 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl groups. Examples of branched alkyl groups having 3 to 12 carbon atoms include isopropyl, isobutyl, sec-butyl, and tert-butyl groups. Examples of cyclic alkyl groups having 3 to 6 carbon atoms include cyclopropyl, cyclobutyl, and cyclohexyl groups. Among these, methyl, ethyl, isopropyl, tert-butyl, and cyclohexyl groups are preferred from the viewpoint of further improving the heat resistance of the resulting N-alkylmaleimide polymer film, and the ethyl group is even more preferred because it allows for the acquisition of an N-alkylmaleimide polymer film with low birefringence that can maintain its low birefringence over a wide range of ambient temperatures.

[0032] Examples of specific N-alkylmaleimide residue units represented by general formula (1) include one or more types such as N-methylmaleimide residue units, N-ethylmaleimide residue units, N-propylmaleimide residue units, N-isopropylmaleimide residue units, N-butylmaleimide residue units, N-isobutylmaleimide residue units, N-sec-butylmaleimide residue units, N-tert-butylmaleimide residue units, N-pentylmaleimide residue units, N-hexylmaleimide residue units, N-octylmaleimide residue units, N-decylmaleimide residue units, N-dodecylmaleimide residue units, N-cyclopropylmaleimide residue units, N-cyclobutylmaleimide residue units, and N-cyclohexylmaleimide residue units. Among these, N-methylmaleimide residue units, N-ethylmaleimide residue units, N-isopropylmaleimide residue units, N-tert-butylmaleimide residue units, or N-cyclohexylmaleimide residue units are preferred from the viewpoint of further improving the heat resistance of the resulting N-alkylmaleimide polymer film. N-ethylmaleimide residue units are even more preferred because they yield an N-alkylmaleimide polymer film that exhibits low birefringence and can maintain that low birefringence over a wide range of ambient temperatures.

[0033] Examples of other copolymerizable monomer residue units in one aspect of the present invention include one or more of the following: vinyl aromatic hydrocarbon residue units such as styrene residue units and α-methylstyrene residue units; olefin residue units such as ethylene residue units, propylene residue units, 1-butene residue units and isobutene residue units; alkyl acrylate residue units such as methyl acrylate residue units, ethyl acrylate residue units and butyl acrylate residue units; alkyl methacrylate residue units such as methyl methacrylate residue units, ethyl methacrylate residue units and butyl methacrylate residue units; and vinyl carboxylate residue units such as vinyl acetate residue units, vinyl propionate residue units and vinyl pivalate residue units. Among these, vinyl aromatic hydrocarbon residue units such as styrene residue units and α-methylstyrene residue units are preferred, and styrene residue units are particularly preferred, because they enable the realization of an N-alkylmaleimide polymer film with a simple composition, low birefringence, and the ability to maintain that low birefringence over a wide range of ambient temperatures.

[0034] In one embodiment of the present invention, the proportion of N-alkylmaleimide residue units in the total residue units of the N-alkylmaleimide polymer is preferably 20 to 100% by weight. Among these, the proportion is more preferably 35 to 100% by weight, particularly preferably 50 to 100% by weight, and even more preferably 55 to 80% by weight, as this yields an N-alkylmaleimide polymer with particularly excellent heat resistance and optical properties.

[0035] Furthermore, in one embodiment of the present invention, the proportion of other copolymerizable monomer residue units in the total residue units of the N-alkylmaleimide polymer is preferably 0 to 80% by weight. Among these, the proportion is more preferably 0 to 65% by weight, particularly preferably 0 to 50% by weight, and even more preferably 20 to 45% by weight, as this yields an N-alkylmaleimide polymer with particularly excellent heat resistance and optical properties.

[0036] In one aspect of the present invention, the weight-average molecular weight (Mw) of the N-alkylmaleimide polymer is preferably 200,000 to 2,000,000, more preferably 500,000 to 1,800,000, and particularly preferably 800,000 to 1,500,000, in order to produce an N-alkylmaleimide polymer film having excellent optical properties and mechanical strength.

[0037] In one embodiment of the present invention, an N-alkylmaleimide polymer may be produced by any method as long as the N-alkylmaleimide polymer is obtained. The N-alkylmaleimide polymer can be produced, for example, by radical copolymerization of N-alkylmaleimide with other copolymerizable monomers. Examples of N-alkylmaleimide in this case include one or more types such as N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-isobutylmaleimide, N-sec-butylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-octylmaleimide, N-decylmaleimide, N-dodecylmaleimide, N-cyclopropylmaleimide, N-cyclobutylmaleimide, and N-cyclohexylmaleimide. Other copolymerizable monomers include one or more of the following: vinyl aromatic hydrocarbons such as styrene and α-methylstyrene; olefins such as ethylene, propylene, 1-butene and isobutene; alkyl acrylates such as methyl acrylate, ethyl acrylate and butyl acrylate; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate and butyl methacrylate; and vinyl carboxylates such as vinyl acetate, vinyl propionate and vinyl pivalate.

[0038] Furthermore, the radical polymerization method can be carried out using known polymerization methods, such as bulk polymerization, solution polymerization, suspension polymerization, precipitation polymerization, and emulsion polymerization. Among these, bulk polymerization or suspension polymerization is preferred because it yields a high molecular weight N-alkylmaleimide polymer, and by using this to prepare a coating solution according to one aspect of the present invention and coating it onto a substrate, an N-alkylmaleimide polymer film with excellent mechanical strength can be obtained.

[0039] Examples of radical polymerization initiators used in radical polymerization include benzoyl peroxide, lauryl peroxide, octanoyl peroxide, acetyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3 Examples include organic peroxides such as 3-tetramethylbutylperoxy-2-ethylhexanoate, tert-butylperoxypivalate, tert-hexylperoxypivalate, tert-butylperoxyneodecanoate, and tert-hexylperoxyneodecanoate, as well as azo initiators such as 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-butyronitrile), 2,2'-azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, and 1,1'-azobis(cyclohexane-1-carbonitride).

[0040] The concentration of the N-alkylmaleimide polymer in the coating solution according to one embodiment of the present invention is not particularly limited as long as it dissolves in the coating solution and a film can be formed by coating, and is preferably 5 to 30% by weight, and particularly preferably 10 to 20% by weight.

[0041] By using a coating solution according to one embodiment of the present invention, gelation can be suppressed during storage of the coating solution. There are no particular restrictions on the storage temperature, for example, 0 to 50°C. There are no particular restrictions on the storage conditions, for example, standing or stirring. There are also no particular restrictions on the storage time, for example, 1 day to 6 months. There are no particular restrictions on the state of gelation, but for example, it ranges from the formation of microgels that can be observed visually to an increase in the overall viscosity of the coating solution that can be observed visually. The state of gelation can be evaluated by visual observation, for example, by comparing it with a standard sample that has not gelled.

[0042] A coating solution according to one embodiment of the present invention may further contain other components besides the aforementioned solvent and N-alkylmaleimide polymer, to the extent that the effects of the embodiments of the present invention are obtained. These other components may be one or more, and examples include various additives. The additives can be appropriately determined depending on the application of the coating solution and the film produced using it. The type and amount of additives used may be appropriately determined within a range that allows for both the effects of the embodiments of the present invention and the effects of the additives to be obtained.

[0043] <Film forming method> A film can be obtained by coating a coating solution according to one aspect of the present invention onto a substrate and drying it. Specifically, the film can be produced by coating a substrate with a coating solution consisting of a solvent comprising 1 to 100% by weight of a cyclic ether solvent and 0 to 99% by weight of an ester solvent, and an N-alkylmaleimide polymer, and drying it.

[0044] There are no particular limitations on the substrate, and examples include polymer substrates, glass substrates, metal substrates, and inorganic substrates. Examples of polymer substrates include polyesters such as polyethylene terephthalate and polyethylene naphthalate, halogen-containing polymers such as polycarbonate, polystyrene, polyethylene, polypropylene, polyacrylic, polyvinyl chloride, and polyvinylidene chloride, cellulose such as cellulose acetate and cellulose ether, sulfur-containing polymers such as polyvinyl alcohol, polyamide, polyimide, polyarylate, polysulfone, and polyethersulfone, polyether ketone, phenolic resin, epoxy resin, aliphatic cyclic polyolefin, and norbornene-based thermoplastic transparent resins. Examples of glass substrates include glass plates and quartz substrates. Examples of metal substrates include aluminum, stainless steel, and ferrotype. Examples of inorganic substrates include ceramic substrates.

[0045] Preferably, the above-mentioned base material is a polymer base material such as polyester (e.g., polyethylene terephthalate and polyethylene naphthalate), polypropylene, polyacrylic, cellulose (e.g., cellulose acetate and cellulose ether), polyimide, aliphatic cyclic polyolefin, and norbornene-based thermoplastic transparent resin. Particularly preferred are polymer base materials such as polyester (e.g., polyethylene terephthalate and polyethylene naphthalate), polypropylene, polyimide, aliphatic cyclic polyolefin, and norbornene-based thermoplastic transparent resin.

[0046] Coating methods include, for example, the T-die method, doctor blade method, bar coater method, slot die method, lip coater method, reverse gravure coating method, microgravure method, spin coating method, brush coating method, roll coating method, and flexographic printing method.

[0047] In a film-forming method according to one aspect of the present invention, it is preferable to dry the coated surface while blowing dry air onto it in order to suppress deterioration of appearance due to the generation of air bubbles.

[0048] In the film-forming method according to one embodiment of the present invention, the drying temperature is preferably room temperature to 200°C, more preferably room temperature to 180°C, and particularly preferably room temperature to 160°C, since drying is performed at a low temperature. In this embodiment of the present invention, room temperature refers to the temperature when there is no external heating or cooling, and is, for example, 10 to 30°C, or may be defined as 20°C.

[0049] In the film-forming method of the present invention, the drying temperature is preferably increased in stages to suppress deterioration of appearance due to bubble formation. For example, the first drying stage can be performed at room temperature to 80°C, the second drying stage at 70 to 155°C, and the third and subsequent drying stages at 130 to 200°C. The drying temperature at each stage is set to a temperature high enough to prevent deterioration of appearance due to bubble formation in order to perform efficient drying.

[0050] Furthermore, the number of heating stages is set to a small number that does not cause deterioration of the appearance due to bubble formation, in order to ensure efficient drying. For example, for the reasons mentioned above, the number of heating stages is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.

[0051] Furthermore, when drying is carried out in multiple stages, in order to ensure efficient drying, the film may be peeled off from the substrate at an intermediate stage, the edges of the film may be fixed, and the drying may be carried out at a drying temperature that does not cause deterioration of appearance due to bubble formation. When drying is carried out in multiple stages, the more stages there are, the more gradual the temperature rise becomes, which is advantageous from the viewpoint of suppressing deterioration of appearance due to bubble formation. The number of heating stages and the drying temperature at each stage can be appropriately determined from viewpoints such as appearance and the amount of residual solvent.

[0052] The drying time is not particularly limited as long as a film with a good appearance is obtained, but it is preferable to have a short drying time as productivity improves. Specifically, it is preferable that the total drying time other than drying at room temperature under a nitrogen atmosphere be 20 minutes or less.

[0053] <Optical film> The optical film obtained by the aforementioned film-forming method is obtained by a film-forming method in which a coating solution consisting of a solvent comprising 1 to 100% by weight of a cyclic ether solvent and 0 to 99% by weight of an ester solvent, and an N-alkylmaleimide polymer is applied to a substrate and dried. The optical film (also simply called "film") is a film with a small amount of residual solvent. In order to prevent deformation of the film such as curling caused by shrinkage stress due to the volatilization of residual solvent after film formation, the amount of residual solvent in the film is preferably less than 3% by weight, more preferably less than 2% by weight, and particularly preferably less than 1% by weight.

[0054] The glass transition temperature (Tg), which is an indicator of the heat resistance of an optical film, is not particularly limited, but is preferably 120°C or higher, more preferably 135°C or higher, and especially preferably 150°C or higher, as this yields a film with excellent heat resistance. This Tg can be adjusted, for example, by selecting N-alkylmaleimide residue units, their proportion in the N-alkylmaleimide polymer, selecting residue units of other copolymerizable monomers, and their proportion in the N-alkylmaleimide polymer.

[0055] The tensile stress, which is an indicator of the mechanical strength of an optical film, is a value that can be controlled by Mw. There are no particular restrictions on the tensile stress of an optical film, but it is preferably 30 MPa or higher, more preferably 35 MPa or higher, and particularly preferably 40 MPa or higher, as this yields a film with excellent mechanical strength.

[0056] The tensile elongation, which is an indicator of the mechanical strength of an optical film, is not particularly limited, but is preferably 2% or more, more preferably 2.5% or more, and especially preferably 3% or more, as this yields a film with excellent mechanical strength.

[0057] Haze, which is one index of the optical properties of an optical film, is a value that can be controlled by, for example, the type of dispersant as an additive, the amount of additive in the N-alkylmaleimide polymer, and the amount of residual monomer. The haze of the optical film is not particularly limited, but is preferably less than 3%, more preferably less than 2.5%, and particularly preferably less than 2%, since a film with excellent transparency can be obtained.

[0058] The photoelastic constant (C) and intrinsic birefringence (Δn 0 ), which are indices of the optical properties of the optical film, are constants that can be controlled by the type of monomer and the ratio of monomer units in the N-alkylmaleimide polymer. The C and Δn 0 of the optical film are not particularly limited in their absolute values, but since a film with low birefringence can be obtained, the absolute value of C is preferably 50×10 -12 Pa -1 or less, and the absolute value of Δn 0 is 20×10 -3 or less, more preferably the absolute value of C is 10×10 -12 Pa -1 or less, and the absolute value of Δn 0 is 5×10 -3 or less, particularly preferably the absolute value of C is 2×10 -12 Pa -1 or less, and the absolute value of Δn 0 is 1×10 -3 or less.

[0059] The temperature coefficient of intrinsic birefringence (dΔn 0 / dT), which is one index of the optical properties of the optical film, is a constant that can be controlled by the type of monomer and the ratio of monomer units in the N-alkylmaleimide polymer. Its absolute value is not particularly limited, but is preferably 2×10 -5 ℃ -1 or less, more preferably 1×10 -5 ℃ -1 or less, since a film that can maintain low birefringence under a wide range of environmental temperatures can be obtained.

[0060] Because optical films possess excellent optical properties, mechanical strength, and heat resistance, they can be used in various optical components, optical lenses, optical sheets, and optical films.

[0061] The coating solution according to one aspect of the present invention is a coating solution with good storage properties, and the optical film obtained by the film-forming method according to one aspect of the present invention is an optical film with a low amount of residual solvent. Therefore, according to one aspect of the present invention, it is expected to contribute to achieving the Sustainable Development Goals (SDGs) by ensuring sustainable consumption and production patterns.

[0062] The present invention is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. [Examples]

[0063] The present invention will be described below based on examples, but the present invention is not limited in any way by these examples. Unless otherwise specified, commercially available reagents were used. Polyvinylpyrrolidone (PVP) K30 was special grade from Fujifilm Wako Pure Chemical Corporation. Polyethylene glycol (PEG) was first grade from Fujifilm Wako Pure Chemical Corporation. Tert-butyl peroxy-2-ethylhexanoate was Perbutyl® O from NOF Corporation.

[0064] The following describes the evaluation and measurement methods for N-alkylmaleimide polymers obtained in the examples.

[0065] <N-alkylmaleimide content in the polymer> A predetermined amount of N-alkylmaleimide polymer was dissolved in deuterated chloroform (approximately 5% by weight), and the resulting solution was analyzed using a 400 MHz NMR spectrometer (JNM-ECZ400S / L1) from JEOL Ltd. 11H-NMR measurements were performed. For copolymers of N-ethylmaleimide and styrene, the content of N-alkylmaleimide residue units in the N-alkylmaleimide polymer was calculated from the integral ratio of the peak between 5.0 and 0.3 ppm to the peak between 8.0 and 5.5 ppm.

[0066] <Molecular weight of polymer> Molecular weight distribution was measured using a Tosoh GPC (HLC-8320GPC). Two Tosoh TSKgel Super HM-H columns were used, the column temperature was set to 40°C, and tetrahydrofuran was used as the eluent. A calibration curve for molecular weight was created using Tosoh standard polystyrene with known molecular weight.

[0067] Synthesis Example 1 In a 500 mL four-necked flask equipped with a stirrer, nitrogen inlet tube, and thermometer, 0.852 g of PVP K30, 346.4 g of distilled water, 103.9 g of N-ethylmaleimide, 25.8 g of styrene, 18.4 g of toluene, and 0.100 g of tert-butylperoxy-2-ethylhexanoate were added. After 1 hour of nitrogen bubbling, suspension polymerization was carried out by holding the mixture at 70°C for 3 hours while stirring at 600 rpm. After the suspension polymerization was complete, the contents were introduced into 2,500 g of distilled water stirred with a magnetic stirrer, and the resulting N-alkylmaleimide polymer particles were recovered by filtration. The recovered polymer particles were washed six times with 2,000 g of distilled water, and then five times with 1,582 g of methanol. Subsequently, the polymer particles were washed once with a mixed solvent of 487 g of toluene and 1,137 g of methanol, followed by five washes with 1,582 g of methanol. Furthermore, they were washed once with a mixed solvent of 827 g of toluene and 827 g of methanol, followed by five washes with 1,582 g of methanol. The washed polymer particles were placed in a dryer set to 95°C and dried under vacuum. Drying was stopped when there was no further weight loss due to drying, yielding 80.0 g of N-ethylmaleimide / styrene copolymer (N-ethylmaleimide polymer). The content of N-ethylmaleimide residue units in the copolymer was 65.4 mol% (69.5 wt%), the weight-average molecular weight Mw was 883,000, and the dispersion degree Mw / Mn was 3.0.

[0068] Example 1 (Preparation of coating solution) The N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in 1,3-dioxolane (DOL) to prepare a coating solution containing 15% by weight of the N-ethylmaleimide polymer component. The resulting coating solution was then left to stand at room temperature for one month, and the presence or absence of gel formation in the coating solution was checked to assess its solution stability. The composition and solution stability of the obtained coating solutions are shown in Table 1.

[0069] (Film formation evaluation) A polyethylene terephthalate film was used as the substrate, and the above coating solution was applied to the substrate using a coater. The resulting coating film was dried by first drying, second drying, and third drying in that order under the drying conditions shown in Table 2. The dried coating film was peeled off the substrate to obtain an optical film. The thickness of the obtained optical film was measured using a film thickness gauge (Ono Sokki, linear gauge sensor). The obtained optical film was dissolved in tetrahydrofuran (however, 1,1,2-trichloroethane when determining the chloroform content), and the gas chromatography (GC) (Shimadzu, capillary gas chromatograph, GC-2025) of the dissolved film solution was measured. The content of each solvent was determined from a calibration curve prepared in advance, and the amount of residual solvent in the optical film was determined by summing them up. The drying conditions, film thickness, and amount of residual solvent of the obtained optical film are shown in Table 2.

[0070] Example 2 (Film formation evaluation) An optical film was obtained in the same manner as in Example 1 (film formation evaluation), except that the edges of the film peeled from the substrate were secured with clips or the like to prevent movement in the dryer, and a fourth drying stage was performed at 155°C for 10 minutes, as shown in Table 2. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. The amount of residual solvent decreased due to the addition of the fourth drying stage after substrate peeling.

[0071] Example 3 (Film formation evaluation) An optical film was obtained using the same method as in Example 2 (film formation evaluation), except that the drying temperature in the fourth stage was set to 200°C. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. By increasing the drying temperature in the fourth stage compared to Example 2, an optical film with a lower residual solvent amount was obtained.

[0072] Example 4 (Preparation of coating solution) A coating solution was prepared in the same manner as in Example 1 (preparation of coating solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in a solvent consisting of 50% by weight of 1,3-dioxolane and 50% by weight of methyl acetate. The composition and solution stability of the obtained coating solution are shown in Table 1.

[0073] (Film formation evaluation) An optical film was obtained using the same method as in Example 2 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. Compared to Example 2, the amount of residual solvent decreased when methyl acetate was added to 1,3-dioxolane.

[0074] Example 5 (Preparation of coating solution) A coating solution was prepared in the same manner as in Example 1 (preparation of coating solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in a solvent consisting of 10% by weight of 1,3-dioxolane and 90% by weight of methyl acetate. The composition and solution stability of the obtained coating solution are shown in Table 1.

[0075] (Film formation evaluation) An optical film was obtained using the same method as in Example 4 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. Compared to Example 4, a film with less residual solvent was obtained by increasing the proportion of methyl acetate added.

[0076] Synthesis Example 2 The N-ethylmaleimide / styrene copolymer was prepared using the same method as in Synthesis Example 1, except that the amount of N-ethylmaleimide added was changed to 103.3 g, the amount of styrene added to 30.2 g, and 0.852 g of PVP K30 was replaced with 0.075 g of polyethylene glycol. As a result, 87.5 g of N-alkylmaleimide polymer (N-ethylmaleimide polymer) was obtained. The content of N-ethylmaleimide residue units in the copolymer was 63.9 mol% (68.0 wt%), the weight-average molecular weight Mw was 1,090,000, and the dispersion degree Mw / Mn was 3.0.

[0077] Example 6 (Preparation of coating solution) The coating solution was prepared in the same manner as in Example 5 (Preparation of Coating Solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was replaced with the N-ethylmaleimide polymer obtained in Synthesis Example 2. The composition and solution stability of the obtained coating solution are shown in Table 1.

[0078] (Film formation evaluation) An optical film was obtained using the same method as in Example 4 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and amount of residual solvent of the obtained optical film are shown in Table 2. Similar to Example 5, a film with less residual solvent was obtained by increasing the proportion of methyl acetate added.

[0079] Comparative Example 1 (Preparation of coating solution) A coating solution was prepared in the same manner as in Example 1 (preparation of coating solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in methyl acetate. The composition and solution stability of the obtained coating solution are shown in Table 1. It was confirmed that gelation occurred and solution stability was low when only an ester-based solvent was used.

[0080] (Film formation evaluation) An optical film was obtained using the same method as in Example 1 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2.

[0081] Comparative Example 2 (Preparation of coating solution) A coating solution was prepared in the same manner as in Example 1 (preparation of coating solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in cyclopentanone to a polymer concentration of 17% by weight. The composition and solution stability of the obtained coating solution are shown in Table 1.

[0082] (Film formation evaluation) An optical film was obtained using the same method as in Example 1 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. Compared to Example 1, the residual solvent amount was higher, causing the optical film to curl and lose its smoothness due to shrinkage stress caused by solvent evaporation during film storage.

[0083] Comparative Example 3 (Preparation of coating solution) The N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in chloroform, which is of concern to health and the environment, to prepare a coating solution in the same manner as in Example 1 (preparation of coating solution), except that the polymer concentration was 18% by weight. The composition and solution stability of the obtained coating solution are shown in Table 1.

[0084] (Film formation evaluation) An optical film was obtained using the same method as in Example 1 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. Compared to Example 1, the residual solvent amount was higher.

[0085] Comparative Example 4 (Preparation of coating solution) A coating solution was prepared in the same manner as in Example 1 (preparation of coating solution), except that the N-ethylmaleimide polymer obtained in Synthesis Example 1 was dissolved in a solvent consisting of 50% by weight of toluene and 50% by weight of methyl ethyl ketone (MEK). The composition and solution stability of the obtained coating solution are shown in Table 1. It was confirmed that gelation occurred and solution stability was low when a solvent consisting of toluene and ethyl methyl ketone was used.

[0086] (Film formation evaluation) An optical film was obtained using the same method as in Example 1 (film formation evaluation), except that the above-mentioned coating solution was used. The drying conditions, film thickness, and residual solvent amount of the obtained optical film are shown in Table 2. Compared to Example 1, the residual solvent amount was higher.

[0087] In Table 1 below, "DOL" represents 1,3-dioxolane and "MEK" represents methyl ethyl ketone. In addition, in the solution stability section of Table 1, "○" indicates that no gelation was observed, and "×" indicates that gelation was observed.

[0088] [Table 1]

[0089] [Table 2]

[0090] As is clear from Table 1, the coating solutions of Examples 1 to 6 all exhibit excellent solution stability, while the coating solutions of Comparative Examples 1 and 4 have lower solution stability compared to the coating solutions of Examples 1 to 6. Therefore, it can be seen that by configuring the solvent of the coating solution with 1,3-dioxolane alone or in combination with methyl acetate, the solution stability can be improved compared to using methyl acetate alone or a mixed solvent of toluene and methyl ethyl ketone.

[0091] Furthermore, as is clear from Table 2, the optical films obtained from the coating solutions of Comparative Examples 2 and 3, which also have high solution stability, have a larger amount of residual solvent compared to the optical film of Example 1, which was dried under similar conditions. Therefore, it can be seen that by using 1,3-dioxolane alone as the solvent in the above coating solution to manufacture an optical film, the amount of residual solvent in the optical film can be reduced compared to when using a coating solution containing cyclopentanone or chloroform.

[0092] Furthermore, as is clear from Table 2, the amount of residual solvent in the optical film of Example 2 is greater than that of the optical films of Examples 4, 5, and 6, which were dried under similar conditions. Therefore, it can be seen that by configuring the solvent of the above coating solution with a specific amount of 1,3-dioxolane and a specific amount of methyl acetate in combination, and manufacturing an optical film using this coating solution, the amount of residual solvent in the optical film can be reduced compared to using an optical film with a coating solution containing 1,3-dioxolane alone. [Industrial applicability]

[0093] This invention can be used to manufacture films suitable for optical components.

Claims

1. A coating solution comprising: a solvent comprising 1 to 50% by weight of one or more cyclic ether solvents selected from the group consisting of tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane and 1,4-dioxane; and 50 to 99% by weight of one or more ester solvents selected from the group consisting of methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate and n-propyl acetate; and an N-alkylmaleimide polymer having a weight-average molecular weight of 883,000 to 1,500,000.

2. The coating solution according to claim 1, characterized in that the cyclic ether solvent is 1,3-dioxolane.

3. The coating solution according to claim 1, characterized in that the ester solvent is methyl acetate.

4. The coating solution according to claim 1, characterized in that the constituent units of the N-alkylmaleimide polymer include N-alkylmaleimide residue units represented by the following general formula (1). 【Chemistry 1】 (In formula (1), R represents a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms.)

5. A method for forming a film, characterized by coating a substrate with a coating solution comprising 1 to 50% by weight of one or more cyclic ether solvents selected from the group consisting of tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 1,4-dioxane, and 50 to 99% by weight of one or more ester solvents selected from the group consisting of methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, and n-propyl acetate, and an N-alkylmaleimide polymer having a weight-average molecular weight of 883,000 to 1,500,000, and then drying it.

6. The film-forming method according to claim 5, characterized in that the drying is performed at a temperature from room temperature to 160°C.

Citation Information

Patent Citations

  • Optical film and its manufacturing method

    JP2001194532A

  • Maleimide copolymer and method for producing the same

    JP2002030119A

  • Transparent film

    JP2005239758A

  • Method for manufacturing optical compensation film

    JP2010096905A

  • Optical compensation film and method for manufacturing the same

    JP2010097115A