Cathode material for lithium-sulfur secondary batteries, cathode for lithium-sulfur secondary batteries, and lithium-sulfur secondary batteries

By forming secondary particles from granulated primary particles of sulfur-supported carbonaceous material in lithium-sulfur batteries, the issues of electrolyte depletion and cycle stopping are mitigated, ensuring high discharge capacity and stability.

JP7954936B2Active Publication Date: 2026-11-24KANSAI UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022175077
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2026-11-24
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

Lithium-sulfur secondary batteries face issues with electrolyte depletion during early charge-discharge cycles, leading to decreased discharge capacity and potential cycle stopping due to the large specific surface area of primary particles of sulfur-supported activated carbon, which causes aggregation, electrolyte decomposition, and reduced reaction interfaces.

Method used

The use of secondary particles formed by granulating primary particles of a sulfur-supported carbonaceous material, with a controlled median diameter range, to maintain a suitable reaction interface and prevent electrolyte depletion, thereby enhancing discharge capacity and cycle stability.

Benefits of technology

The secondary particles with a moderate particle size ensure high discharge capacity and reduced cycle stalling, even with a small amount of electrolyte, by minimizing aggregation and electrolyte decomposition, thus improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954936000002
    Figure 0007954936000002
  • Figure 0007954936000003
    Figure 0007954936000003
  • Figure 0007954936000004
    Figure 0007954936000004
Patent Text Reader

Abstract

To provide a positive electrode material for a lithium sulphur secondary battery that can be used to manufacture a lithium sulphur secondary battery with a high discharge capacity even after the initial (e.g. first) cycle of a charge-discharge cycle and that is difficult to stop the charge-discharge cycle.SOLUTION: The positive electrode material for a lithium sulphur secondary battery has secondary particles, which are granulates formed from primary particles of positive electrode active material in which sulphur and carbonaceous material are composited.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a positive electrode material for lithium-sulfur secondary batteries, a positive electrode for lithium-sulfur secondary batteries, and a lithium-sulfur secondary battery. [Background technology]

[0002] Lithium-ion batteries are currently widely used as rechargeable batteries in mobile phones, personal computers, digital cameras, etc., but there is a need for further improvements in energy density and cost reduction.

[0003] This is where lithium-sulfur secondary batteries are attracting attention. Lithium-sulfur secondary batteries use sulfur as the positive electrode active material and lithium metal as the negative electrode active material, and lithium ions (Li + A lithium-sulfur secondary battery is a rechargeable battery that charges and discharges by the movement of lithium between the positive and negative electrodes. In a lithium-sulfur secondary battery, during discharge, lithium moves from the negative electrode to the negative electrode. + Ions dissolve and react with sulfur at the positive electrode to produce Li2S, while an electric current flows to the external circuit.

[0004] Sulfur atoms have a large number of electrons per unit weight involved in oxidation-reduction reactions, and theoretically, they are expected to have an energy density more than five times higher than conventional lithium-ion batteries. Furthermore, since sulfur is inexpensive and easily available, it is possible to reduce material costs. For these reasons, lithium-sulfur secondary batteries are being actively researched as a next-generation type of secondary battery.

[0005] For example, Non-Patent Document 1 discloses a positive electrode active material for a lithium-sulfur secondary battery consisting of primary particles of activated carbon supported with sulfur. It is also known that when the positive electrode active material for a lithium-sulfur secondary battery is made of fine particles with a particle size of 1 μm, the discharge capacity of the lithium-sulfur secondary battery using it can be increased by increasing its specific surface area. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] Abstracts of the 86th Annual Meeting of the Electrochemical Society of Japan, 2019; Presentation Number 1031 (2019) [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] In lithium-sulfur secondary batteries, it is necessary to reduce the amount of electrolyte in order to increase the energy density. Here, we consider the case where a positive electrode material for lithium-sulfur secondary batteries, which contains a positive electrode active material consisting of primary particles of activated carbon supported with sulfur, having a particle size of 1 μm, is used in a lithium-sulfur secondary battery with a small amount of electrolyte. In this case, because the specific surface area of ​​the positive electrode active material is too large, electrolyte depletion occurs in the early stages of the charge-discharge cycle (for example, the first cycle), and problems occur such as a decrease in discharge capacity in subsequent cycles and / or the charge-discharge cycle stopping.

[0008] One aspect of the present invention aims to provide a positive electrode material for lithium-sulfur secondary batteries that can be used in the manufacture of lithium-sulfur secondary batteries that have high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and that are less likely to stop during the charge-discharge cycle. [Means for solving the problem]

[0009] To solve the aforementioned problems, the inventors investigated the use of secondary particles obtained by granulating primary particles of a sulfur-supported carbonaceous material as a constituent material for a lithium-sulfur secondary battery cathode. They found that by using a lithium-sulfur secondary battery cathode material containing these secondary particles, it is possible to obtain a lithium-sulfur secondary battery that maintains high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and that is less prone to stalling during the charge-discharge cycle.

[0010] In other words, the present invention includes the configurations shown in (A) and (B) below. (A) A positive electrode material for a lithium-sulfur secondary battery, comprising secondary particles that are granules formed from primary particles of a positive electrode active material in which sulfur and a carbonaceous material are composited. (B) A method for producing a positive electrode material for a lithium-sulfur secondary battery, comprising a step of granulating primary particles of a positive electrode active material in which sulfur is composited with a carbonaceous material to produce secondary particles. [Effects of the Invention]

[0011] According to one aspect of the present invention, it is possible to provide a positive electrode material for a lithium-sulfur secondary battery that can be used to produce a lithium-sulfur secondary battery that maintains a high discharge capacity even after the initial charge / discharge cycles (for example, the first cycle) and that is less likely to have charge / discharge cycles interrupted. [Brief Description of Drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a method for producing a positive electrode material for a lithium-sulfur secondary battery according to an embodiment of the present invention, and an embodiment of the positive electrode material for a lithium-sulfur secondary battery according to an embodiment of the present invention produced by the production method. In FIG. 1, portions supporting sulfur are indicated by diagonal lines. [Figure 2] FIG. 2 is a graph showing measurement results of discharge capacity when charge / discharge cycles of lithium-sulfur secondary batteries including the positive electrode materials for lithium-sulfur secondary batteries produced in Examples 1 to 3 and Comparative Example 1 of the present application and having an E / S ratio of approximately 8 were repeated. [Figure 3] FIG. 3 is a graph showing measurement results of discharge capacity when charge / discharge cycles of lithium-sulfur secondary batteries including the positive electrode materials for lithium-sulfur secondary batteries produced in Examples 1 to 3 and Comparative Example 1 of the present application and having an E / S ratio of 3 were repeated. [Figure 4] FIG. 4 is a graph showing measurement results of discharge capacity when charge / discharge cycles of lithium-sulfur secondary batteries including the positive electrode materials for lithium-sulfur secondary batteries produced in Example 4 and Comparative Example 2 of the present application and having an E / S ratio of approximately 8 were repeated. [Figure 5]FIG. 6 is a graph showing discharge capacity measurement results when charge-discharge cycles of a lithium-sulfur secondary battery including the positive electrode material for a lithium-sulfur secondary battery produced in Example 4 and Comparative Example 2 of the present application and having an E / S ratio of 3 are repeated. [Description of Embodiments]

[0013] Hereinafter, an embodiment of the present invention will be described in detail. However, the present invention is not limited thereto, and various modifications can be made within the scope of the description. For example, an embodiment obtained by appropriately combining technical means disclosed in different embodiments is also included in the technical scope of the present invention. Unless otherwise specified in this specification, the numerical range "A to B" means "A or more and B or less".

[0014] [1. Positive Electrode Material for Lithium-Sulfur Secondary Battery] A positive electrode material for a lithium-sulfur secondary battery according to an embodiment of the present invention includes secondary particles, which are granules formed from primary particles of a positive electrode active material in which sulfur and a carbonaceous material are composited.

[0015] In an embodiment of the present invention, the "positive electrode active material in which sulfur and a carbonaceous material are composited" is particulate, and is a carbonaceous material supporting sulfur. The positive electrode material for a lithium-sulfur secondary battery includes secondary particles, which are granules formed from the primary particles of the positive electrode active material.

[0016] Here, the "primary particles" mean a state of one particle (single particle). In this specification, the "secondary particles" mean granules of a plurality of single particles (primary particles). Examples of the granules include a state in which a plurality of single particles (primary particles) are aggregated. As will be described later, the granules can be prepared, for example, by applying vibration to the plurality of single particles (primary particles).

[0017] The primary particles constituting the granules are primary particles made of a carbonaceous material supporting sulfur.

[0018] Figure 1 is a schematic diagram showing an example of a method for manufacturing a lithium-sulfur secondary battery cathode material (described later) according to one embodiment of the present invention, and the form of the lithium-sulfur secondary battery cathode material manufactured by the manufacturing method. The primary particles constituting the secondary particles are primary particles made of carbonaceous material particles supporting sulfur, as shown in the lower left of Figure 1. The lithium-sulfur secondary battery cathode material has secondary particles which are granules of the primary particles, as shown in the lower right of Figure 1.

[0019] In conventional secondary batteries such as lithium-ion batteries, electrode active materials have primarily been used in the form of secondary particles, mainly due to the ease of preparing the coating solution (slurry) for electrode fabrication. On the other hand, in lithium-sulfur secondary batteries, there have been no previous examples of using electrode active materials in the form of granulated secondary particles. Therefore, it was not known that using these secondary particles would facilitate the preparation of the coating solution for electrode fabrication and improve battery performance such as discharge capacity and cycle characteristics in lithium-sulfur secondary batteries. Furthermore, the relationship between using electrode active materials in the form of granulated secondary particles and preventing the deterioration of lithium-sulfur secondary battery performance caused by the aforementioned liquid depletion was also completely unknown.

[0020] However, surprisingly, the positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention can prevent a decrease in battery performance by having the secondary particles. The reason why the positive electrode material for a lithium-sulfur secondary battery exhibits such an effect is presumed to be as follows. When using a positive electrode active material in the form of a powder with extremely small particle size (e.g., 100 nm or less), i.e., primary particles, as a constituent material for the positive electrode material of a lithium-sulfur secondary battery, the positive electrode active material may aggregate during the preparation process of the coating solution (slurry) for manufacturing the positive electrode. Furthermore, during the drying process after coating the coating solution containing the primary particles of the positive electrode active material onto a current collector, heating can cause convection in the coating solution (slurry), which can lead to the aggregation of the positive electrode active material. As a result, regions where the positive electrode active material has aggregated, so-called "clumps," are formed in the coating solution (coating layer) applied to the substrate. In this case, the structure of the manufactured electrode differs between the portion generated from the aggregated region of the positive electrode active material and the portion generated from other regions. Consequently, electrode cracking is more likely to occur at the boundary between the two. In addition, current concentration may occur in the portion of the electrode generated from the aggregated region of the positive electrode active material, leading to electrolyte decomposition and the generation of dead lithium, which can significantly reduce battery performance. Furthermore, even if clumps do not form in the coating layer, the positive electrode active material, which is the primary particle, has a large specific surface area, making it prone to side reactions between the positive electrode active material and the electrolyte, and thus prone to electrolyte decomposition. The occurrence of the aforementioned side reactions and electrolyte decomposition can easily lead to a decrease in battery performance. On the other hand, if the particle size of the positive electrode active material is excessively large, the specific surface area of ​​the positive electrode active material becomes too small, resulting in an excessive reduction of the reaction interface between lithium ions and the electrolyte. As a result, battery performance may decrease. The positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention has secondary particles which are granules formed from primary particles of a positive electrode active material in which sulfur and a carbonaceous material are composited. The particle size of the secondary particles is a moderate particle size (e.g., several hundred nm) which is larger than the particle size of the primary particles. As a result, aggregation of the positive electrode active material is less likely to occur, and the coating liquid prepared using the positive electrode active material becomes smoother. Therefore, the performance of a lithium-sulfur secondary battery equipped with a positive electrode made using the coating liquid is improved, and it is possible to provide a lithium-sulfur secondary battery that has a high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and is less likely to stall during the charge-discharge cycle. The positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention has secondary particles, and therefore its surface morphology is uneven. Thus, the positive electrode material for a lithium-sulfur secondary battery has a larger particle size and a reduced specific surface area than primary particles, while still having a specific surface area of ​​a predetermined size. As a result, the area of ​​the reaction interface where lithium ions and electrolyte react is ensured. Consequently, it is possible to prevent a decrease in battery performance, such as discharge capacity, caused by a reduction in the reaction interface. In addition, the positive electrode material for lithium-sulfur secondary batteries according to one embodiment of the present invention has secondary particles, which suppresses the decomposition of the electrolyte and reduces the volume of voids within the electrode. Furthermore, the positive electrode material for lithium-sulfur secondary batteries has reduced inter-particle contact resistance compared to particles in the primary particle state. Therefore, a lithium-sulfur secondary battery equipped with a positive electrode containing the positive electrode material for lithium-sulfur secondary batteries has improved discharge capacity and can perform charge-discharge cycles with a smaller amount of electrolyte. Consequently, even in lithium-sulfur secondary batteries that use a small amount of electrolyte, it is possible to prevent the occurrence of electrolyte depletion, maintain high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle), and provide a lithium-sulfur secondary battery that is less likely to stop during the charge-discharge cycle.

[0021] From the viewpoint of preventing the aggregation of the positive electrode active material as described above, as well as the deterioration of battery performance caused by the occurrence of the aforementioned side reactions and electrolyte decomposition, the median diameter of the secondary particles is preferably 4 μm or more, and more preferably 9.7 μm or more.

[0022] On the other hand, if the median diameter of the secondary particles is excessively large, even if their surface morphology is uneven, their specific surface area may become too small, potentially leading to an excessive reduction in the reaction interface. In this case, the sulfur in the primary particles may also be incorporated into the secondary particles, preventing contact with the electrolyte, which could also lead to an excessive reduction in the reaction interface. Therefore, the upper limit of the median diameter of the secondary particles is preferably 20 μm or less, and more preferably 12.9 μm or less.

[0023] By having the median diameter of the secondary particles within the aforementioned preferred range, it becomes easier to provide a lithium-sulfur secondary battery that maintains high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and is less prone to stalling during the charge-discharge cycle.

[0024] In addition, from the viewpoint of more easily preventing the occurrence of liquid depletion, the median diameter of the secondary particles is more preferably 9.7 μm or more at the lower limit, and particularly preferably 12.9 μm or more. On the other hand, from the same viewpoint, the median diameter of the secondary particles is more preferably 20 μm or less at the upper limit, and particularly preferably 17 μm or less.

[0025] By having the median diameter within the aforementioned preferred range, it becomes easier to provide a lithium-sulfur secondary battery that maintains high discharge capacity even when using a small amount of electrolyte, and that is less prone to stalling during the initial stages of the charge-discharge cycle (e.g., the first cycle).

[0026] The median diameter of the primary particle is preferably 2.8 μm or more at the lower limit, more preferably 1.5 μm or more, even more preferably 1.0 μm or more, and particularly preferably 0.8 μm or more. The median diameter of the primary particle is preferably 13.0 μm or less at the upper limit, more preferably 12.0 μm or less, even more preferably 10.3 μm or less, and particularly preferably 7.1 μm or less.

[0027] By having the median diameter of the primary particles within the aforementioned range, the median diameter of the secondary particles, which are granules containing the primary particles, can be easily controlled to within the aforementioned preferred range.

[0028] In this specification, "median diameter" refers to the 50% diameter (D50) in the cumulative frequency % diameter (particle size distribution) calculated by the method shown below.

[0029] The cumulative frequency % diameter can be measured, for example, by a wet batch measurement method using a scattering particle size distribution analyzer (RASER SCATTERING PARTICLE SIZE DISTRIBUTION ANALYZER LA-950 (manufactured by HORIBA)).

[0030] The wet batch measurement method can be performed using the following method.

[0031] (i) Mix the primary particles or secondary particles with a dispersion medium (carboxymethylcellulose, surfactant, etc.) to prepare a dispersion in which the primary particles or secondary particles are dispersed.

[0032] (ii) Next, a glass cell that has been treated with a special coating is filled with pure water, and a few drops of the dispersion are added to it to prepare a sample. Furthermore, the sample is stirred using a stirrer to disperse the dispersion within the cell.

[0033] (iii) After the dispersion is dispersed, the sample is irradiated with semiconductor laser light to measure the transmittance of the sample, and the particle size of the primary particles or the secondary particles is calculated from the transmittance.

[0034] While there are other methods for measuring cumulative frequency % diameter, such as the flow method and the dry method, the wet batch method is convenient because it requires only a small amount of primary or secondary particles for measurement, and generates only a small amount of wastewater after measurement.

[0035] In one embodiment of the present invention, the positive electrode active material is a composite of sulfur and a carbonaceous material. As mentioned above, "a composite of sulfur and a carbonaceous material" means that the sulfur is supported on the carbonaceous material.

[0036] Examples of the carbonaceous material include activated carbon, carbon nanotubes, and graphene. The carbonaceous material may be a single substance or a mixture of two or more substances.

[0037] The loading of sulfur onto the carbonaceous material may be by physical adsorption or by chemical adsorption. For example, the loading of sulfur onto the carbonaceous material can be carried out by mixing the carbonaceous material and sulfur using a mortar and pestle, and then heating the resulting mixture in a muffle furnace. Commercially available sulfurous powder can be used as the sulfur.

[0038] The carbonaceous material preferably has pores. In this case, the sulfur diffuses and is adsorbed within the pores. Therefore, the carbonaceous material having pores can support the sulfur more strongly.

[0039] As described later, the "positive electrode active material in which sulfur and carbonaceous material are compounded" preferably has 60% by weight or more of sulfur supported relative to the weight of the positive electrode active material. As a method for making the weight percentage (by weight) of sulfur in the positive electrode active material a desired value, for example, in the method of supporting sulfur on the carbonaceous material described above, the conditions can be adjusted as shown in (A) and (B) below. (A) The amount of sulfur used is adjusted to be 1 to 4% by weight more than the desired value of the weight percentage of sulfur in the positive electrode active material. (B) The heat treatment conditions shall be those shown in Manufacturing Examples 1 and 2 described later.

[0040] In this specification, the form of sulfur is not particularly limited. For example, one or more sulfurs selected from the group consisting of α-sulfur (orthorhombic sulfur), β-sulfur (monoclinic sulfur), γ-sulfur (monoclinic sulfur), rubbery sulfur, and plastic sulfur can be used.

[0041] When the carbonaceous material has pores, the larger the specific surface area and the volume of the pores, the more suitable the structure of the carbonaceous material is for supporting a large amount of sulfur. Therefore, from the viewpoint of providing a suitable structure for supporting a large amount of sulfur, examples of the carbonaceous material preferably include activated carbon obtained by carbonizing a resin, a fossil resource material, or the like, and then activating the carbonized material with an alkali such as potassium hydroxide, and template-molded porous carbon. Examples of the template-molded porous carbon include template-molded porous carbon obtained using magnesium oxide as a template. Specific examples of the template-molded porous carbon include Knobel (registered trademark).

[0042] The specific surface area of the carbonaceous material is preferably 150 0m 2 m -1 / g to 290 0m 2 m -1 / g, and more preferably 220 0m 2 m -1 / g to 290 0m 2 m -1 / g, from the viewpoint of supporting a large amount of sulfur.

[0043] The specific surface area is a value measured by the BET method. The specific surface area can be measured using, for example, AUTOSORB iQ manufactured by Quantachrome.

[0044] When the carbonaceous material has pores, the volume of the pores is preferably 0.6 cc·g -1 to 1.2 cc·g -1 , and more preferably 0.9 cc·g -1 to 2.0 cc·g -1 , from the viewpoint of supporting a large amount of sulfur.

[0045] The pore volume can be measured using, for example, AUTOSORB iQ manufactured by Quantachrome.

[0046] The aforementioned "positive electrode active material, which is a composite of sulfur and a carbonaceous material," preferably carries 60% by weight or more of sulfur relative to the total weight of the positive electrode active material. In other words, it is preferable that the ratio of the weight of sulfur to the sum of the weight of sulfur and carbonaceous material constituting the positive electrode active material is 60% by weight or more.

[0047] When the weight percentage of sulfur is 60% by weight or more, the amount of sulfur supported is high, making it possible to provide a lithium-sulfur battery that meets the recent demand for increased sulfur content in the positive electrode material.

[0048] The weight percentage of sulfur is more preferably 70% by weight or more, and a higher percentage is preferable, but the upper limit can be determined by the loading capacity of the carbonaceous material, etc. For example, if the carbonaceous material is activated carbon, the upper limit is about 60-66% by weight. The amount of sulfur loaded can be confirmed by the method described later in the examples.

[0049] [2. Positive electrode for lithium-sulfur secondary batteries] A positive electrode for a lithium-sulfur secondary battery according to one embodiment of the present invention includes a positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention. More specifically, the positive electrode for a lithium-sulfur secondary battery has a configuration in which a positive electrode mixture for a lithium-sulfur secondary battery (hereinafter simply referred to as "positive electrode mixture") containing the positive electrode material is supported on a current collector. By having the above configuration, the positive electrode for a lithium-sulfur secondary battery has the effect of being usable in the manufacture of a lithium-sulfur secondary battery that has a high discharge capacity even after the initial stages of the charge-discharge cycle (for example, the first cycle) and is less likely to stop during the charge-discharge cycle.

[0050] The positive electrode mixture may contain other components in addition to the positive electrode material for lithium-sulfur secondary batteries. Examples of these other components include conductive additives and aqueous binders.

[0051] Any electrically conductive material that does not adversely affect battery performance can be used as a conductive additive. Typically, carbon black such as acetylene black or Ketjenblack is used, but conductive materials such as natural graphite (scaly graphite, flake graphite, earthy graphite, etc.), carbon nanotubes, artificial graphite, carbon whiskers, carbon fiber powder, metal (copper, nickel, aluminum, silver, gold, etc.) powder, metal fibers, and conductive ceramic materials may also be used. These may be used individually or as a mixture of two or more types.

[0052] The aqueous binder is not particularly limited as long as it can bind the positive electrode active material particles and the conductive additive, etc. As the aqueous binder, one or more types of styrene-butadiene rubber (SBR) aqueous dispersion, carboxymethylcellulose (CMC), alginate, polyglutamate, etc. can be used.

[0053] Preferably, the positive electrode mixture contains 90% to 95% by weight of the positive electrode material and 5% to 10% by weight of the other components, based on the total weight of the positive electrode mixture.

[0054] The positive electrode mixture can be prepared by conventionally known methods. For example, a method for preparing the positive electrode mixture is to homogeneously mix the positive electrode material and the other components.

[0055] The positive electrode for the lithium-sulfur secondary battery can be manufactured by conventionally known methods. For example, it can be manufactured by preparing a coating liquid (slurry) for manufacturing a positive electrode containing the positive electrode mixture and solvent, applying or filling (coating) the coating liquid to a current collector, drying it, then press-molding it, and further drying it by air drying and / or vacuum drying.

[0056] As the current collector, an electron conductor that does not adversely affect the constructed battery can be used. Examples include aluminum, titanium, stainless steel, nickel, calcined carbon, conductive polymer, and conductive glass. For the purpose of improving adhesion, conductivity, oxidation resistance, etc., a current collector with a surface treated with carbon, nickel, titanium, or silver may also be used.

[0057] The shape of the current collector can be foil-like, film-like, sheet-like, net-like, or any other shape. Among these, a current collector having a three-dimensional structure, such as a honeycomb shape, is preferred because it can be filled with a larger amount of the coating liquid and thus enable a larger capacity.

[0058] [3. Lithium-sulfur secondary battery] A lithium-sulfur secondary battery according to one embodiment of the present invention comprises a positive electrode for a lithium-sulfur secondary battery according to one embodiment of the present invention. More specifically, the lithium-sulfur secondary battery comprises a structure in which a battery element impregnated with an electrolyte is contained within a casing material, the positive electrode and negative electrode for the lithium-sulfur secondary battery facing each other via a separator. Because the lithium-sulfur secondary battery comprises a positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention, it exhibits the effect of high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and makes it difficult for the charge-discharge cycle to stop.

[0059] The negative electrode can be manufactured by attaching metallic lithium as the active material to a current collector. Alternatively, a negative electrode mixture for lithium-sulfur secondary batteries containing silicon powder, the aforementioned conductive additive, and a water-based binder can be manufactured by coating or supporting it on a current collector, for example, in the same manner as the method for manufacturing the positive electrode for lithium-sulfur secondary batteries described above. As the current collector, for example, metal foil can be used. Specific examples of the metal foil include copper foil and stainless steel foil.

[0060] The electrolyte is preferably an electrolyte containing lithium and one or more solvents selected from the group consisting of carbonates, ethers, sulfur compounds, halogenated hydrocarbons, phosphate ester compounds, sulfolane hydrocarbons, and ionic liquids.

[0061] Examples of lithium-containing electrolytes include LiPF6, LiBF4, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI). Among these, LiPF6, LiFSI, and LiTFSI are preferred, and LiTFSI is even more preferred. The lithium-containing electrolyte may be used alone or in combination of two or more types.

[0062] The solvent more preferably includes one or more solvents selected from the group consisting of carbonates and ethers.

[0063] The carbonates mentioned above are preferably cyclic carbonates such as chloroethylene carbonate (CLEC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), and vinylene carbonate (VC); or linear carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).

[0064] The ethers are preferably cyclic ethers such as dioxolane (DOL) and tetrahydrofuran; or linear ethers such as dimethoxyethane (DME), triglyme (G3), tetraglyme (G4), and 1,1,2,2-tetrafluoro-3-(1,1,2,2-tetrafluoroethoxy)-propane (HFE).

[0065] In particular, the solvent is more preferably a solvent containing the carbonates. From the viewpoint that an SEI film can be formed on a carbonaceous material whose pores are micropores and mesopores during the first discharge of a lithium-sulfur secondary battery, the solvent containing the carbonates is particularly preferably a mixture of CLEC or FEC and HFE.

[0066] A lithium-sulfur secondary battery according to one embodiment of the present invention preferably further comprises an electrolyte adjusted so that the volume of the electrolyte / the weight of sulfur in the positive electrode for the lithium-sulfur secondary battery (E / S) ≈ 8, or an electrolyte adjusted so that E / S = 3. In the above E / S, the unit of the volume of the electrolyte is "mL", and the unit of the weight of sulfur is "g".

[0067] The electrolyte is as described above. "Weight of sulfur in the positive electrode for lithium-sulfur secondary batteries" refers to the weight of sulfur contained in the positive electrode material for lithium-sulfur secondary batteries according to one embodiment of the present invention. Furthermore, "Volume of electrolyte / Weight of sulfur in the positive electrode for lithium-sulfur secondary batteries (E / S) ≈ 8" means that E / S is 7.95 or more and less than 8.05.

[0068] A lithium-sulfur secondary battery according to one embodiment of the present invention can be manufactured by assembling a positive electrode, negative electrode, electrolyte, separator, housing, etc., using a conventionally known method.

[0069] [4. Method for manufacturing positive electrode material for lithium-sulfur secondary batteries] A method for producing a positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention includes a step of producing secondary particles by granulating primary particles of a positive electrode active material in which sulfur is compounded with a carbonaceous material.

[0070] The above manufacturing method can be used to produce a positive electrode material for a lithium-sulfur secondary battery according to one embodiment of the present invention. Therefore, the above manufacturing method has the effect of producing a positive electrode material for a lithium-sulfur secondary battery that can be used in the manufacture of a lithium-sulfur secondary battery that has a high discharge capacity even after the initial stages of the charge-discharge cycle (for example, the first cycle) and is less likely to stop during the charge-discharge cycle.

[0071] Details already described in other embodiments will be omitted below.

[0072] The method for preparing the primary particles used in the above process is not limited. For example, as shown in Figure 1, one method is to compound sulfur with the carbonaceous material, and then pulverize the positive electrode active material, which is a compound of sulfur and the carbonaceous material, to prepare the primary particles. Another method is to pulverize the carbonaceous material to obtain fine particles of the carbonaceous material, and then compound sulfur with the fine particles to prepare the primary particles. Alternatively, for example, one can prepare the primary particles by compounding sulfur with a carbonaceous material having a particle size suitable for primary particles, without pulverizing the carbonaceous material.

[0073] The method for carrying out the aforementioned grinding is not particularly limited and may include, for example, a method using a vibrating type or planetary type ball mill.

[0074] Conventional known methods can be used to composite sulfur with carbonaceous materials. Examples of such methods include the following methods (i) and (ii). (i) Mix the positive electrode active material and sulfur using a mortar and pestle or the like, such that the ratio of the weight of sulfur to the weight of the positive electrode active material in which sulfur is compounded with a carbonaceous material is 1 to 4% by weight more than the desired value. (ii) The obtained mixture is placed into a heating device such as a muffle furnace and subjected to heat treatment.

[0075] The heat treatment can be carried out, for example, as follows: First, the temperature inside the heating device is raised to preferably 145°C to 155°C, more preferably 150°C to 155°C, and then held for a predetermined time to melt the sulfur and support it in the pores of the carbonaceous material. The predetermined time is preferably 3 hours to 10 hours, more preferably 5 hours to 10 hours.

[0076] Next, the temperature inside the heating device is further increased, preferably to 280°C or higher and 320°C or lower, more preferably to 300°C or higher and 320°C or lower, and then held for a predetermined time to sublimate any excess sulfur adhering to the surface of the carbonaceous material. The predetermined time is preferably 1.0 hour or higher and 5.0 hours or lower, more preferably 1.0 hour or higher and 2.0 hours or lower, and even more preferably 1.5 hours or higher and 2.0 hours or lower. Examples of the conditions in the heat treatment can be found in the conditions shown in Manufacturing Examples 1 and 2 described later.

[0077] In the process of producing secondary particles by granulating primary particles of a positive electrode active material in which sulfur is compounded with a carbonaceous material, the following methods can be used as granulation methods: • A method of continuing to apply vibration to primary particles within the ball mill even after preparing primary particles using the ball mill as described above. For example, known granulation methods such as chemical substitution and sintering.

[0078] When using a vibrating ball mill, preferred operating conditions include, for example, a vibration frequency of 10 to 35 Hz for 0.5 to 5.0 hours to apply vibration to the primary particles. When using a planetary ball mill, preferred operating conditions include, for example, a rotational speed of 100 to 400 rpm for 0.5 to 5.0 hours to apply vibration to the primary particles.

[0079] During the granulation process, the sulfur in the primary particles of the positive electrode active material, which is a composite of sulfur and carbonaceous material, functions as an adhesive that holds multiple primary particles together. As a result, secondary particles are produced, which are granules containing primary particles of the positive electrode active material, which is a composite of sulfur and carbonaceous material.

[0080] The manufacturing method may include, in addition to the above steps, a step of mixing the obtained secondary particles with other components of the lithium-ion secondary battery cathode material. Known mixing methods can be used for the mixing.

[0081] 〔summary〕 The present invention includes the following embodiments. (1) A positive electrode material for lithium-sulfur secondary batteries having secondary particles which are granules formed from primary particles of a positive electrode active material which is a composite of sulfur and a carbonaceous material. (2) The secondary particles are the positive electrode material for lithium sulfur secondary batteries described in (1), wherein the median diameter is 4 μm or more and 20 μm or less. (3) The secondary particles are positive electrode materials for lithium sulfur secondary batteries as described in (1) or (2), wherein the median diameter is 9.7 μm or more and 12.9 μm or less. A positive electrode for a lithium-sulfur secondary battery, comprising the positive electrode material for lithium-sulfur secondary batteries described in any one of (4) (1) to (3). A lithium-sulfur secondary battery equipped with the positive electrode for lithium-sulfur secondary batteries described in <5> and <4>. <6> The lithium sulfur secondary battery according to <5>, further comprising an electrolyte adjusted so that the volume of the electrolyte / the weight of sulfur in the positive electrode for the lithium sulfur secondary battery (E / S) is approximately 8, or an electrolyte adjusted so that E / S = 3. (7) A method for producing a positive electrode material for a lithium-sulfur secondary battery, comprising the step of granulating primary particles of a positive electrode active material in which sulfur is compounded with a carbonaceous material to produce secondary particles. [Examples]

[0082] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0083] [Measurement method] The physical properties of the lithium-sulfur secondary battery cathode materials manufactured in Examples 1-4 and Comparative Examples 1 and 2, and the performance of lithium-sulfur secondary batteries manufactured using these lithium-sulfur secondary battery cathode materials were measured and calculated using the methods described below.

[0084] <Median diameter> The cumulative frequency % diameter (particle size distribution) of the lithium-sulfur secondary battery cathode material was measured by the methods shown in (a) to (c) below. The 50th percentile diameter (D50) of the measured cumulative frequency % diameter was defined as the median diameter of the lithium-sulfur secondary battery cathode material. (a) The positive electrode material for lithium-sulfur secondary batteries was mixed with a dispersion medium (carboxymethylcellulose, surfactant, etc.) to prepare a dispersion in which the positive electrode material for lithium-sulfur secondary batteries was dispersed. (b) Next, a glass cell with a special coating was filled with pure water, and a few drops of the dispersion were added to it to prepare a sample. Furthermore, the sample was stirred using a stirrer to disperse the dispersion within the cell. (c) After dispersing the dispersion, the sample was irradiated with semiconductor laser light to measure the transmittance of the sample, and the particle size of the cathode material was calculated from the transmittance. A scattering particle size distribution analyzer (RASER SCATTERING PARTICLE SIZE DISTRIBUTION ANALYZER LA-950 (manufactured by HORIBA)) was used as the measuring device.

[0085] <Specific surface area> The specific surface area of ​​the lithium-sulfur secondary battery cathode material was measured using the BET method with Quantachrome's AUTOSORB iQ.

[0086] <Sulfur content per hour> The lithium-sulfur secondary battery cathode material was placed in an alumina cell, and thermogravimetric analysis (TGA) was performed using a Shimadzu DTG-60AH. The measurement was performed under the following conditions: measurement gas Ar, gas flow rate 50 ml / min, heating rate 5°C / min, and upper temperature limit 600°C. From the obtained TGA results, the ratio of the weight of sulfur supported by the lithium-sulfur secondary battery cathode material to the total weight of the lithium-sulfur secondary battery cathode material (sulfur load, unit: weight %) was calculated.

[0087] <Charge / Discharge Test (Cycle Characteristics Test)> Using the lithium-sulfur secondary battery cathode material described above and manufactured by the method described below, the cathode of the lithium-sulfur secondary battery was used as the working electrode, and a constant current charge-discharge test was performed using an AUTO BATTERY EVALUATION (manufactured by Electrofield). The charging mode was the CC method ("CC" is an abbreviation for constant current), and the discharging mode was the CC mode. The set current density was 167.2 mA / g (a current density of 1672 mA / g is defined as 1C; hereinafter, 167.2 mA / g will be referred to as 0.1C). The cutoff voltage was set to a lower limit of 1.0V and an upper limit of 3.0V. The test was conducted in an environment of 25°C. That is, the charge-discharge rate was set to 0.1 / 0.1C, and a charge-discharge cycle was performed.

[0088] Note that the charging and discharging capacities are based on the weight of sulfur, and the unit is mA·h (g sulfur). -1 This was defined as follows.

[0089] [Manufacturing Example 1: Preparation of a positive electrode active material composed of sulfur and carbonaceous material] 0.34 g of activated carbon with a particle size of approximately 1.7 μm or 2.8 μm and 0.66 g of sulfurous powder (manufactured by Wako Pure Chemical, purity exceeding 99%) were mixed using an agate mortar to obtain a mixture. The mixture was transferred to a heat-resistant metal container and placed in a muffle furnace for heat treatment in the atmosphere.

[0090] Specifically, the heat-resistant metal container containing the mixture was placed inside the muffle furnace, the internal temperature was raised to 155°C, and this temperature was maintained for 5 hours to melt the sulfur. Next, the internal temperature was raised at a rate of 5°C / min to 300°C, and this temperature was maintained for 2 hours. After that, the inside was thoroughly air-cooled, and the heat-resistant metal container was removed from it. From the heat-resistant metal container, activated carbon on which sulfur was supported, i.e., a positive electrode active material composed of sulfur and a carbonaceous material, was obtained.

[0091] Hereinafter, a positive electrode active material in which sulfur and carbonaceous material are composited, with a particle size (median diameter) of approximately 1.7 μm, will be referred to as sulfur-supported positive electrode active material (1). Sulfur-supported positive electrode active material (1) consists of primary particles.

[0092] Furthermore, a positive electrode active material that is a composite of sulfur and carbonaceous material, with a particle size (median diameter) of approximately 2.8 μm, is defined as sulfur-supported positive electrode active material (2). Sulfur-supported positive electrode active material (2) is also a primary particle.

[0093] [Example 1] (Preparation of secondary particles, which are granules containing primary particles of a positive electrode active material that is a composite of sulfur and carbonaceous material) 2.5 g of sulfur-supported cathode active material (1) and 20 ml of 1 mm zirconia bead mill were placed in a container. Subsequently, the sulfur-supported cathode active material (1) and the 1 mm zirconia bead mill were vibrated for 3 hours at a vibration frequency of 35 Hz using the vibrating ball mill machine (Retsch, product name: MM500nano) in the container. As a result, the sulfur-supported cathode active material (1) was pulverized, and primary particles were generated. These primary particles were then granulated to produce secondary particles. The produced secondary particles were used as the cathode material (1).

[0094] Using a portion of the obtained positive electrode material (1), the median diameter, specific surface area, and sulfur load of the positive electrode material (1) were measured using the method described above. The physical properties of the positive electrode material (1) were: median diameter: 4.2646 μm, specific surface area: 15875 cm²2 / cm 3 The sulfur content was 60% by weight. The measurement results are shown in Table 1 below.

[0095] (Pressure electrode mixture and cathode preparation for lithium-sulfur secondary batteries) The positive electrode material (1), activated carbon without sulfur support, carbon nanotubes as a conductive additive, and a water-based binder (polyglutamate) as a binder were measured out in a weight ratio of 75:19:1:5 to form the materials for the positive electrode mixture for lithium-sulfur secondary batteries. The activated carbon without sulfur support was the same activated carbon with a particle size of approximately 1.7 μm used in Production Example 1.

[0096] The measured materials were mixed using an agate mortar, and the resulting mixture was transferred to an ointment case. Next, the mixture was stirred using a rotating / revolving mixer at a rotation speed of 2000 rpm for a total of 25 minutes to obtain a positive electrode mixture for lithium sulfur secondary batteries.

[0097] Next, the lithium-sulfur secondary battery positive electrode mixture was filled into a 3D aluminum current collector (Cellmet®, manufactured by Sumitomo Electric Industries, Ltd.) and dried at 40°C for 1 hour using a hot plate. The dried current collector was rolled using a roll press, then cut into 2.4cm x 2.4cm pieces using scissors to obtain molded bodies, which were then dried for a further 12 hours in a bell jar at 50°C to produce a lithium-sulfur secondary battery positive electrode.

[0098] (Preparation of electrolyte for lithium-sulfur secondary batteries) Lithium bis(trifluoromethanesulfonyl)imide (hereinafter referred to as LiTFSI) was used as the lithium-containing electrolyte. In addition, a mixed solvent of chloroethylene carbonate (hereinafter referred to as CLEC) and 1,1,2,2-tetrafluoro-3-(1,1,2,2-tetrafluoroethoxy)-propane (hereinafter referred to as HFE) was used as the non-aqueous solvent.

[0099] The method for preparing the electrolyte is described in more detail below. CLEC and HFE were mixed in a volume ratio of 7:3 to form a mixed solvent. Next, LiTFSI was dissolved in the mixed solvent to a concentration of 1.0 mol / L LiTFSI / CLEC:HFE, and vinylene carbonate (VC) was added at a concentration of 10 volume% relative to 90 volume% LiTFSI / CLEC:HFE to form the electrolyte for the lithium-sulfur secondary battery.

[0100] (Manufacturing of lithium-sulfur secondary batteries) Cell shapes include cylindrical metal can type, coin type, and laminate type, but a laminate type cell was used in this test. Using the lithium sulfur secondary battery positive electrode and electrolyte prepared as described above, and lithium foil as the negative electrode, separator and electrolyte, a lithium sulfur battery was fabricated in an atmospheric environment with a dew point of -40°C or lower using the following procedure.

[0101] First, a laminate, consisting of a positive electrode, a separator, and a negative electrode stacked in that order, was placed inside an aluminum laminate film that had been formed into a bag shape by thermocompression bonding. Furthermore, after injecting an electrolyte into the laminate film, thermocompression bonding was performed while vacuuming the inside of the laminate film to produce a lithium-sulfur secondary battery.

[0102] In detail, a lithium-sulfur secondary battery was fabricated by adjusting the amount of electrolyte used so that the ratio of the volume of electrolyte to the weight of sulfur in the positive electrode of the lithium-sulfur secondary battery (E / S) was approximately 8. Another lithium-sulfur secondary battery was fabricated by adjusting the amount of electrolyte used so that E / S = 3.

[0103] Charge-discharge tests (cycle characteristic tests) were performed on each of the two lithium-sulfur secondary batteries fabricated using the method described above. The results are shown in Table 1 and Figures 2 and 3.

[0104] [Example 2] (Preparation of secondary particles, which are granules containing primary particles of a positive electrode active material that is a composite of sulfur and carbonaceous material) Secondary particles were prepared in the same manner as in Example 1, except that the amount of sulfur-supported cathode active material (1) used was changed to 1 g and the vibration time was changed to 45 minutes. The prepared secondary particles were designated as cathode material (2). Furthermore, using a portion of the obtained cathode material (2), the median diameter, specific surface area, and sulfur-supported amount of cathode material (2) were measured in the same manner as in Example 1. The physical properties of cathode material (2) were median diameter: 9.7457 μm, specific surface area: 6664 cm². 2 / cm 3 The sulfur content was 61% by weight. The measurement results are shown in Table 1 below.

[0105] (Manufacturing of lithium-sulfur secondary batteries) Two lithium-sulfur secondary batteries were fabricated using the same method as in Example 1, except that cathode material (2) was used instead of cathode material (1). Charge-discharge tests (cycle characteristic tests) were performed on each of the two fabricated lithium-sulfur secondary batteries. The results are shown in Table 1 and Figures 2 and 3.

[0106] [Example 3] (Preparation of secondary particles, which are granules containing primary particles of a positive electrode active material that is a composite of sulfur and carbonaceous material) Secondary particles were prepared in the same manner as in Example 1, except that 2 g of sulfur-supported cathode active material (2) was used instead of sulfur-supported cathode active material (1). The prepared secondary particles were designated as cathode material (3). Furthermore, using a portion of the obtained cathode material (3), the median diameter, specific surface area, and sulfur-supported amount of cathode material (3) were measured in the same manner as in Example 1. The physical properties of cathode material (3) were: median diameter: 12.8749 μm, specific surface area: 5668 cm² 2 / cm 3 The sulfur content was 66% by weight. The measurement results are shown in Table 1 below.

[0107] (Manufacturing of lithium-sulfur secondary batteries) Two lithium-sulfur secondary batteries were fabricated using the same method as in Example 1, except for the following points. • The use of positive electrode material (3) instead of positive electrode material (1). - Instead of using activated carbon with a particle size of approximately 1.7 μm as the activated carbon that does not support sulfur, activated carbon with a particle size of approximately 2.8 μm, as used in Production Example 1, was used.

[0108] Charge-discharge tests (cycle characteristic tests) were conducted on each of the two lithium-sulfur secondary batteries that were fabricated. The results are shown in Table 1 and Figures 2 and 3.

[0109] [Comparative Example 1] (Preparation of primary particles of a positive electrode active material composed of sulfur and carbonaceous material) 1.5 g of sulfur-supported cathode active material (2) and 100 g of 5 mm SUS balls were placed in a SUS container. Subsequently, using a planetary ball mill (Philitsch, product name: P5), the sulfur-supported cathode active material (2) was pulverized in the SUS container at 200 rpm for 2 hours. As a result, the sulfur-supported cathode active material (2) was pulverized, and primary particles were generated. The generated primary particles were designated as the comparative cathode material (1).

[0110] Using a portion of the obtained comparative cathode material (1), the median diameter, specific surface area, and sulfur load of comparative cathode material (1) were measured using the method described above. The physical properties of comparative cathode material (1) were: median diameter: 1.9973 μm, specific surface area: 37884 cm². 2 / cm 3 The sulfur content was 64% by weight. The measurement results are shown in Table 1 below.

[0111] (Manufacturing of lithium-sulfur secondary batteries) Two lithium-sulfur secondary batteries were fabricated using the same method as in Example 1, except that a comparative positive electrode material (1) was used instead of positive electrode material (1). Charge-discharge tests (cycle characteristic tests) were performed on each of the two fabricated lithium-sulfur secondary batteries. The results are shown in Table 1 and Figures 2 and 3.

[0112] [Manufacturing Example 2: Preparation of a positive electrode active material with supported sulfur] 0.35 g of Knobel® (particle size: 3.8 μm, manufactured by Toyo Tanso Co., Ltd.) and 0.65 g of sulfurous powder (manufactured by Wako Pure Chemical Co., Ltd., purity over 99%) were mixed using an agate mortar to obtain a mixture. The mixture was transferred to a heat-resistant metal container and placed in a muffle furnace for heat treatment in the atmosphere. Specifically, after placing the heat-resistant metal container containing the mixture into the muffle furnace, the temperature inside was raised to 155°C and maintained at this temperature for 5 hours to melt the sulfurous powder, which was then supported within the pores of the Knobel. After that, the inside was thoroughly air-cooled and the heat-resistant metal container was removed from the inside. From the heat-resistant metal container, the Knobel with sulfur supported, i.e., a positive electrode active material composed of sulfur and carbonaceous material, was obtained. The obtained positive electrode active material is referred to as sulfur-supported positive electrode active material (3).

[0113] [Example 4] (Preparation of secondary particles of a positive electrode active material composed of sulfur and carbonaceous material) Secondary particles were prepared in the same manner as in Example 1, except that sulfur-supported cathode active material (3) was used instead of sulfur-supported cathode active material (1). The prepared secondary particles were used as cathode material (4). Furthermore, using a portion of the obtained cathode material (4), the median diameter, specific surface area, and sulfur-supported amount of cathode material (4) were measured in the same manner as in Example 1. The physical properties of cathode material (4) were median diameter: 5.9030 μm, specific surface area: 12162 cm². 2 / cm 3 The sulfur content was 64% by weight. The measurement results are shown in Table 1 below.

[0114] (Manufacturing of lithium-sulfur secondary batteries) Except for the following points, two lithium-sulfur secondary batteries were fabricated using the same method as in Example 1. • The use of positive electrode material (4) instead of positive electrode material (1). • The materials for the positive electrode mixture for lithium-sulfur secondary batteries were measured out in a weight ratio of 94:1:5, consisting of the positive electrode material (4), a conductive additive (carbon nanotube), and a binder (water-based binder (polyglutamate)).

[0115] Charge-discharge tests (cycle characteristic tests) were conducted on each of the two lithium-sulfur secondary batteries that were fabricated. The results are shown in Table 1 and Figures 4 and 5.

[0116] [Comparative Example 2] (Preparation of primary particles of a positive electrode active material composed of sulfur and carbonaceous material) Primary particles were produced in the same manner as in Comparative Example 1, except that sulfur-supported cathode active material (3) was used instead of sulfur-supported cathode active material (2). The produced primary particles were used as comparative cathode material (2).

[0117] Using a portion of the obtained comparative cathode material (2), the median diameter, specific surface area, and sulfur load of comparative cathode material (2) were measured using the method described above. The physical properties of comparative cathode material (2) were: median diameter: 3.7591 μm, specific surface area: 23311 cm² 2 / cm 3 The sulfur content was 65% by weight. The measurement results are shown in Table 1 below.

[0118] (Manufacturing of lithium-sulfur secondary batteries) Two lithium-sulfur secondary batteries were fabricated using the same method as in Example 4, except that a comparative positive electrode material (2) was used instead of positive electrode material (4). Charge-discharge tests (cycle characteristic tests) were performed on each of the two fabricated lithium-sulfur secondary batteries. The results are shown in Table 1 and Figures 4 and 5.

[0119] [Conclusion]

[0120] [Table 1] As shown in Table 1 and Figures 2 and 3, the lithium-sulfur secondary batteries described in Examples 1 to 3 have a higher discharge capacity than the lithium-sulfur secondary battery described in Comparative Example 1. As shown in Figures 2 and 3, these lithium-sulfur secondary batteries exhibit excellent discharge capacity regardless of the amount of electrolyte used. Therefore, these lithium-sulfur secondary batteries are capable of solving the problems of the present invention.

[0121] As shown in Table 1 and Figures 4 and 5, the lithium-sulfur secondary battery described in Example 4 has a higher discharge capacity than the lithium-sulfur secondary battery described in Comparative Example 2. Furthermore, as shown in Figures 2 and 3, the lithium-sulfur secondary batteries described in Examples 1 to 3 have a higher number of charge-discharge cycles before stopping than the lithium-sulfur secondary battery described in Comparative Example 1. In addition, as shown in Table 1 and Figure 3, the discharge capacity of lithium-sulfur secondary batteries with a small amount of electrolyte (E / S=3) is higher in Examples 2 and 3 than in Example 1.

[0122] In other words, from the viewpoint of achieving a high discharge capacity when the amount of electrolyte used is small (E / S=3), it is most preferable that the median diameter of the secondary particles constituting the positive electrode active material be around 12.8 μm, and more preferably around 9.7 μm. That is, in this case, it is preferable that the median diameter of the secondary particles be within the range of 9.7 to 12.9 μm.

[0123] On the other hand, from the viewpoint of achieving a higher discharge capacity when a larger amount of electrolyte is used (E / S=8), it is found that the median diameter of the secondary particles constituting the positive electrode active material is most preferably around 4.2 μm, and more preferably around 9.7 μm. In other words, in this case, it is found that the median diameter of the secondary particles is preferably within the range of 4.2 to 9.7 μm.

[0124] From the above, it was found that a lithium-sulfur secondary battery made using the cathode material according to one embodiment of the present invention can achieve a high discharge capacity even after the initial stages of the charge-discharge cycle. Furthermore, it was found that a lithium-sulfur secondary battery made using the cathode material according to one embodiment of the present invention is less likely to stop during the charge-discharge cycle, even when the amount of electrolyte used is small.

[0125] Furthermore, the results from Examples 2 and 3 showed that cathode materials with a median diameter of secondary particles between 9.7 μm and 12.9 μm exhibit superior discharge capacity from the initial stages of the charge-discharge cycle in lithium-sulfur secondary batteries that use less electrolyte. [Industrial applicability]

[0126] The positive electrode material for lithium-sulfur secondary batteries according to one embodiment of the present invention can be used to manufacture lithium-sulfur secondary batteries that have a high discharge capacity even after the initial stages of the charge-discharge cycle (e.g., the first cycle) and that are less likely to stop during the charge-discharge cycle.

Claims

1. A positive electrode material for a lithium-sulfur secondary battery, having secondary particles which are granules formed from primary particles of a positive electrode active material in which sulfur and carbonaceous material are composites, The amount of sulfur supported in the positive electrode material for the lithium-sulfur secondary battery is 60% by weight or more and 66% by weight or less. A lithium-sulfur secondary battery positive electrode material having a specific surface area of ​​5668 cm² / cm³ or more and 15875 cm² / cm³ or less.

2. The positive electrode material for a lithium sulfur secondary battery according to claim 1, wherein the carbonaceous material is activated carbon.

3. A positive electrode for a lithium-sulfur secondary battery, comprising the positive electrode material for a lithium-sulfur secondary battery described in claim 1 or 2.

4. A lithium-sulfur secondary battery comprising the positive electrode for a lithium-sulfur secondary battery described in claim 3.

5. The lithium sulfur secondary battery according to claim 4, further comprising an electrolyte adjusted so that the volume of the electrolyte / the weight of sulfur in the positive electrode for the lithium sulfur secondary battery (E / S) is approximately 8, or an electrolyte adjusted so that E / S = 3.

6. A method for producing a positive electrode material for a lithium-sulfur secondary battery, comprising the step of granulating primary particles of a positive electrode active material in which sulfur is compounded with a carbonaceous material to produce secondary particles, The amount of sulfur supported in the positive electrode material for the lithium-sulfur secondary battery is 60% by weight or more and 66% by weight or less. A method for manufacturing a lithium-sulfur secondary battery positive electrode material, wherein the specific surface area of ​​the positive electrode material for a lithium-sulfur secondary battery is 5668 cm² / cm³ or more and 15875 cm² / cm³ or less.

7. The method for producing a positive electrode material for a lithium sulfur secondary battery according to claim 6, wherein the carbonaceous material is activated carbon.

Citation Information

Patent Citations

  • Lithium-sulphur battery with high specific energy

    JP2014067717A

  • Carbon nanotube-sulfur composite containing carbon nanotube aggregates and method for producing the same

    JP2016535716A

  • Carbon-sulfur composite, method for producing the same, cathode and lithium-sulfur battery including the same

    JP2019513673A

  • Alkali metal-sulfur secondary battery including a protected sulfur cathode and method of manufacture

    JP2020509540A

  • Method for producing cathode material for lithium-sulfur battery, cathode material for lithium-sulfur battery, and lithium-sulfur battery

    WO2016068043A1