Inkjet pretreatment solution, ink set, and method for manufacturing printed materials using the ink set

The use of DCDA/DETA sulfate and polyalkyleneimine in an inkjet pretreatment solution maintains neutral pH and high concentration, addressing corrosion issues and improving image fixation in inkjet printing on non-absorbent substrates.

JP7954940B2Active Publication Date: 2026-11-24GENERAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022207821
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2026-11-24
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Inkjet pretreatment solutions containing flocculants with halogens or cationic polymers with allylamine structural units can corrode metal components in inkjet printer ejection heads and degrade resin parts, reducing ejection stability and image fixation effectiveness, while neutralizing these solutions requires large amounts of neutralizing agents, diluting the coagulant concentration.

Method used

An inkjet pretreatment solution using a sulfate of a copolymer of dicyandiamide and diethylenetriamine (DCDA/DETA sulfate) as a flocculant, combined with a basic neutralizing agent like polyalkyleneimine, maintains a neutral pH and high concentration, preventing corrosion and ensuring stable ejection and improved image fixation.

Benefits of technology

The solution provides stable ejection over time without affecting printer components, enhances image fixation, and avoids environmental hazards by being halogen-free, with improved image quality and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954940000001
    Figure 0007954940000001
  • Figure 0007954940000002
    Figure 0007954940000002
  • Figure 0007954940000003
    Figure 0007954940000003
Patent Text Reader

Abstract

To provide an inkjet pretreatment liquid which can be stably discharged over a long period of time because it does not affect a metal component and a resin component constituting a discharge head of an inkjet printer, has an excellent effect for improving fixability of an image, and does not contain halogen and an ink set including the same, and a method for manufacturing a printed matter using the ink set.SOLUTION: An inkjet pretreatment liquid contains a sulfate of a copolymer of dicyandiamide and diethylene triamine, and water. An ink set contains an inkjet pretreatment liquid, and at least one kind of aqueous inkjet ink. A method for manufacturing a printed matter includes the steps of: printing an inkjet pretreatment liquid onto the surface of a non-absorptive base material by an inkjet printing method; and printing an image on a region printed with the inkjet pretreatment liquid of the surface of the base material using inkjet ink by an inkjet printing method.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an inkjet pretreatment liquid for pretreating the surface of a non-absorbent substrate when printing an image on the surface of the substrate by an inkjet printing method, an ink set including the same, and a method for producing a printed material using the ink set. [Background Art]

[0002] Techniques for printing images such as characters and patterns by inkjet printing on the surface of substrates that have no or low absorbency for water-based inkjet inks, such as calendar films (hereinafter sometimes collectively referred to as "non-absorbent substrates"), are becoming widespread. [Prior Art Documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Unexamined Patent Application Publication No. 2015-134493 [Patent Document 2] Japanese Unexamined Patent Application Publication No. 2019-111770 [Summary of Invention] [Problem to be Solved by the Invention]

[0004] When printing an image on the surface of a non-absorbent substrate, in order to improve the fixability of the printed image, it has been common to use, as the inkjet ink, not a normal water-based ink, but a non-water-based ink using an organic solvent, or a photocurable ink.

[0005] However, in recent years, in consideration of reducing the environmental burden caused by using organic solvents and simplifying the apparatus by omitting UV light sources and the like, there has been a growing demand for the use of water-based inkjet inks even for printing on such non-absorbent substrates.

[0006] Furthermore, as a water-based inkjet ink, pigment-dispersed types are becoming increasingly popular, which use pigments as colorants to improve the weather resistance of images, for example, by dispersing these pigments in the ink through their own self-dispersing properties (self-dispersing pigments) or by the function of an anionic dispersant.

[0007] Furthermore, in order to improve the image fixation on non-absorbent substrates using pigment-dispersed, water-based inkjet inks, it is being considered to pre-treat the surface of the substrate with an inkjet pre-treatment solution prior to printing.

[0008] Considering the ease of printing and other factors, the inkjet pretreatment solution can be dispensed from a dedicated ejection head on the inkjet printer, similar to inkjet ink, and printed on a predetermined area of ​​the substrate surface.

[0009] Examples of inkjet pretreatment solutions to be used with pigment-dispersed inkjet inks include aqueous solutions containing a water-soluble compound that is reactive with self-dispersing pigments or anionic dispersants as a flocculant. Examples of such flocculants include halogen salts of cationic polymers or cationic polymers containing allylamine structural units in their molecules (see Patent Documents 1 and 2, etc.).

[0010] When printing is performed on the surface of a substrate pretreated with an inkjet pretreatment solution containing these flocculants using a pigment-dispersed inkjet ink containing self-dispersing pigments, the pigments in the inkjet ink react with the flocculants on the substrate surface, promoting aggregation, which improves the fixation of the image composed of those pigments. Furthermore, when printing is performed on the surface of the above substrate using a pigment-dispersed inkjet ink containing a dispersant, the dispersant in the inkjet ink reacts with the flocculants on the substrate surface, separating from the pigments. This reduces the dispersibility of the pigments and promotes aggregation, resulting in improved fixation of the image composed of those pigments.

[0011] However, inkjet pretreatment solutions containing flocculants with halogens in their molecules, such as halogenated salts of cationic polymers, exhibit strong acidity. Therefore, prolonged use can corrode metal components, such as those in the ejection head of an inkjet printer, reducing the ejection stability of the inkjet pretreatment solution. Furthermore, the halogen-containing components in such inkjet pretreatment solutions contribute to the generation of environmentally harmful substances, leading to restrictions on their use.

[0012] On the other hand, inkjet pretreatment solutions containing cationic polymers with allylamine structural units in their molecules as flocculants tend to exhibit strong acidity or strong alkalinity depending on the type of cationic polymer. Of these, strongly acidic inkjet pretreatment solutions, like the halogen salts mentioned above, may corrode metal components and other parts that make up the ejection head of an inkjet printer. Furthermore, strongly alkaline inkjet pretreatment solutions may degrade resin components and other parts that make up the ejection head, for example.

[0013] Therefore, in either case, prolonged use may reduce the ejection stability of the inkjet pretreatment solution. Furthermore, with highly basic inkjet pretreatment solutions, the reaction between the coagulant and self-dispersing pigments or dispersants may be inhibited, resulting in insufficient improvement in image fixation. Considering these points, inkjet pretreatment solutions should ideally be close to neutral.

[0014] Therefore, it is conceivable to add a neutralizing agent to the inkjet pretreatment solution. However, as mentioned above, neutralizing a highly acidic or basic inkjet pretreatment solution requires the addition of a large amount of neutralizing agent. As a result, the concentration of the coagulant contained in the inkjet pretreatment solution decreases, and the effect of the coagulant in improving image fixation may not be sufficiently obtained.

[0015] The object of the present invention is to provide an inkjet pretreatment solution that does not affect metal or resin parts that constitute the ejection head of an inkjet printer, thus enabling stable ejection over a long period of time, and that is excellent in improving image fixation, and is halogen-free. Another object of the present invention is to provide an ink set containing such an inkjet pretreatment solution and a method for manufacturing printed materials using the ink set. [Means for solving the problem]

[0016] The present invention relates to an inkjet pretreatment solution containing a sulfate of a copolymer of dicyandiamide and diethylenetriamine as a flocculant, and water.

[0017] Furthermore, the present invention relates to an ink set comprising the inkjet pretreatment solution of the present invention and at least one aqueous inkjet ink.

[0018] Furthermore, the present invention is a method for manufacturing a printed material, comprising a pretreatment step of printing an inkjet pretreatment liquid from such an ink set onto the surface of a non-absorbent substrate by an inkjet printing method, and a printing step of printing an image onto the area on the surface of the substrate where the inkjet pretreatment liquid has been printed, using an inkjet ink by an inkjet printing method. [Effects of the Invention]

[0019] According to the present invention, it is possible to provide an inkjet pretreatment solution that does not affect metal or resin parts that constitute the ejection head of an inkjet printer, thus enabling stable ejection over a long period of time, and that has an excellent effect in improving image fixation, while also being halogen-free. Furthermore, according to the present invention, it is possible to provide an ink set containing such an inkjet pretreatment solution and a method for manufacturing printed materials using the ink set. [Modes for carrying out the invention]

[0020] Inkjet pretreatment liquid As described above, the inkjet pretreatment liquid of the present invention contains a sulfate of a copolymer of dicyandiamide and diethylenetriamine as an aggregating agent (hereinafter may be abbreviated as "DCDA / DETA sulfate"), and water. The inkjet pretreatment liquid is characterized in that it contains water.

[0021] According to the present invention, since the hydrogen ion exponent (pH) of the aqueous solution of DCDA / DETA sulfate is close to neutral, by selecting and using the DCDA / DETA sulfate as the aggregating agent, the pH of the inkjet pretreatment liquid can also be maintained near neutral. Therefore, the inkjet pretreatment liquid can be stably discharged from the discharge head over a long period of time without affecting metal parts, resin parts, etc. constituting the discharge head of the inkjet printer.

[0022] Further, since it is not necessary to blend a large amount of neutralizing agent, the concentration of DCDA / DETA sulfate as an aggregating agent contained in the inkjet pretreatment liquid is maintained at a high concentration, and the effect of improving image fixability by the DCDA / DETA sulfate can be further enhanced. In addition, since the DCDA / DETA sulfate does not contain halogen in the molecule and does not cause generation of environmentally hazardous substances, there is also an advantage that its use is not likely to be restricted in the future.

[0023] <Aggregating agent> As the aggregating agent, DCDA / DETA sulfate is selectively used as described above. Specific examples of the DCDA / DETA sulfate include, but are not limited to, the following products among the water-soluble cationic polymers of the Unisense series manufactured by Senka Co., Ltd., all of which are supplied as aqueous solutions of DCDA / DETA sulfate.

[0024] Unisense KHP 10LU (yellowish brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 150 mPa·s), 11LU (yellowish brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 100 mPa·s), 12LU (yellowish brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 150 mPa·s), etc.

[0025] These products not only have the above-mentioned excellent effects, but also have a high solid content concentration as described above and low viscosity, thereby suppressing an increase in the viscosity of the inkjet pretreatment liquid, maintaining good dischargeability from the nozzle of the discharge head, and also improving the fixability of an image. One or more of these DCDA / DETA sulfates can be used.

[0026] (Amount of DCDA / DETA sulfate) The amount of the DCDA / DETA sulfate is preferably 0.2% by mass or more, particularly 0.4% by mass or more, and preferably 6% by mass or less, particularly 5% by mass or less, based on the total amount of the inkjet pretreatment liquid in terms of solid content.

[0027] If the amount of the DCDA / DETA sulfate is less than this range, the effect of improving image fixability by the DCDA / DETA sulfate may not be sufficiently obtained. On the other hand, when the amount of the DCDA / DETA sulfate exceeds the above range, the acidity of the inkjet pretreatment liquid becomes strong, which corrodes metal parts and the like constituting the discharge head of the inkjet printer, and may reduce the discharge stability of the inkjet pretreatment liquid. In addition, the solid content concentration may increase, the viscosity of the inkjet pretreatment liquid may increase, and good discharge may not be achieved.

[0028] On the other hand, by setting the amount of the DCDA / DETA sulfate within the above range, it is possible to suppress an increase in the viscosity of the inkjet pretreatment liquid and corrosion of metal parts and the like constituting the discharge head, and further improve image fixability while stably maintaining good discharge for a long period of time.

[0029] <Neutralizing Agent> Although the DCDA / DETA sulfate has a pH of an aqueous solution close to neutral as described above, since it is a cationic polymer, the pH of the inkjet pretreatment liquid may shift to acidity, and therefore, a basic neutralizing agent may be added to the inkjet pretreatment liquid. By blending a basic neutralizing agent, the pH of the inkjet pretreatment liquid can be adjusted to around neutral (weakly acidic to weakly basic).

[0030] Various basic compounds, such as diethanolamine, can be used as basic neutralizing agents, but polyalkyleneimines are particularly preferred. Examples of polyalkyleneimines include polymers of at least one alkyleneimine having 2 to 4 carbon atoms, or modified products thereof.

[0031] Among these, alkylene imines having 2 to 4 carbon atoms can be one or more of the following: ethyleneimine, propyleneimine, methylethyleneimine, butyleneimine, ethylethyleneimine, dimethylethyleneimine, etc. Examples of modification include modification with alkylene oxide, alkyl glycidyl ether, glycidylamine, epoxide (epihalohydrin, etc.), (meth)acrylate ((meth)acrylic acid, (meth)acrylate, etc.), and acid anhydride (succinic anhydride, phthalic anhydride, maleic anhydride, etc.).

[0032] Polyethyleneimine is particularly preferred as a neutralizing agent for basics. Polyethyleneimine not only functions as a neutralizing agent for basics but also reacts with self-dispersing pigments and dispersants, and functions as a pigment flocculant. Therefore, when used in combination with DCDA / DETA sulfate, the image fixation can be further improved. Specific examples of polyethyleneimine, though not limited to these, include the following products from the Epomin® series manufactured by Nippon Shokubai Co., Ltd. One or more of these polyethyleneimines can be used.

[0033] SP-003 [Pale yellow transparent liquid, molecular weight: 300, resin content: 98% or more, viscosity: 200~500mPa s 25℃, pH (5% aqueous solution): 10~12], SP-00 6 [Pale yellow transparent liquid, molecular weight: 600, resin content: 98% or more, viscosity: 500~2500mPa s 25℃, pH (5% aqueous solution): 10~12], SP-012 [Pale yellow Color transparent liquid, molecular weight: 1200, resin content: 98% or more, viscosity: 3500~7500mPa s · 25℃, pH (5% aqueous solution): 10~12], SP-018 [light yellow transparent] Bright liquid, molecular weight: 1800, resin content: 98% or more, viscosity: 8500~15000mPa s · 25℃, pH (5% aqueous solution): 10~12], SP-200 [light yellow transparent liquid] body, molecular weight: 10,000, resin content: 98% or more, viscosity: 40,000~150,000mPa s · 25℃, pH (5% aqueous solution): 10~12], P-1000 [water dilution, Transparent viscous liquid, molecular weight: 70000, resin content: 30±1%, viscosity: 400~900mPa s 25℃, pH (5% aqueous solution): 10~12], P-3000 [water dilution, Transparent viscous liquid, molecular weight: 100000, resin content: 35±1%, viscosity: approx. 1300mPa s 25℃, pH (5% aqueous solution): 10~12], HM-2000 [water dilution, Pale yellow transparent liquid, molecular weight: 30,000, resin content: 93~95%, 50% water dilution viscosity: 5,000~15,000 mPa·s · 25℃, pH (5% aqueous solution): 10~12], etc.

[0034] (pH range of inkjet pretreatment solution and amount of neutralizing agent) As mentioned above, the inkjet pretreatment solution is preferably weakly acidic or weakly basic. More specifically, the pH of the inkjet pretreatment solution is preferably 5 or higher, particularly 7 or higher, and preferably 10 or lower, particularly 9 or lower.

[0035] If the pH of the inkjet pretreatment solution is below this range, the solution is too acidic, which can corrode metal components and other parts of the inkjet printer's ejection head, reducing the stability of the inkjet pretreatment solution ejection. On the other hand, if the pH of the inkjet pretreatment solution exceeds the above range, the solution is too basic, which can degrade resin components and other parts of the ejection head, reducing the stability of the inkjet pretreatment solution ejection.

[0036] Furthermore, the reaction between DCDA / DETA sulfate, used as a flocculant, and self-dispersing pigments or dispersants may be inhibited, resulting in insufficient improvement in image fixation. In contrast, by setting the pH of the inkjet pretreatment solution within the above range, the impact on metal and resin components constituting the inkjet printer's ejection head can be suppressed, allowing for stable and good ejection over a long period while further improving image fixation.

[0037] The amount of basic neutralizing agent, such as polyethyleneimine, used to adjust the pH of the inkjet pretreatment solution to the above range can be arbitrarily set depending on the type and amount of DCDA / DETA sulfate and other components. For example, the amount of basic neutralizing agent to be added to an inkjet pretreatment solution containing DCDA / DETA sulfate with a pH of approximately 7 in the aforementioned amount is preferably 1.6% by mass or less, and particularly 1.4% by mass or less, of the total amount of the inkjet pretreatment solution.

[0038] Furthermore, there is no particular lower limit to the amount of basic neutralizing agent. That is, the pH of an inkjet pretreatment solution containing DCDA / DETA sulfate with a pH of approximately 7 in the aforementioned amount is generally within the preferred range described above, and in such cases, it is not necessary to add a basic neutralizing agent. In other words, the lower limit of the amount of basic neutralizing agent may be 0% by mass of the total amount of the inkjet pretreatment solution.

[0039] However, in order to bring the pH of the inkjet pretreatment solution closer to neutral, it is preferable to add a basic neutralizing agent, and the amount thereof is preferably 0.6% by mass or more, and particularly preferably 0.8% by mass or more, of the total amount of the inkjet pretreatment solution.

[0040] <Humidifier> A water-soluble organic solvent with a boiling point higher than water may be added to the inkjet pretreatment solution as a humectant. In a method for manufacturing printed materials using an ink set containing an inkjet pretreatment solution, the inkjet pretreatment solution is printed onto the surface of the substrate for pretreatment, then the image is printed using inkjet ink, and then, if necessary, the substrate is heated and dried.

[0041] Even if inkjet ink is printed on top of a previously printed inkjet pretreatment solution that has completely dried, the reaction between the DCDA / DETA sulfate and the self-dispersing pigment or dispersant will proceed to some extent due to the moisture in the inkjet ink. However, the entire surface may dry out due to heat drying before the pigment has sufficiently aggregated, resulting in insufficient image fixation.

[0042] In contrast, by incorporating a water-soluble organic solvent with a higher boiling point than water, the organic solvent acts as a humectant, allowing the inkjet pretreatment solution to dry as slowly as possible. This enables the inkjet ink to be printed before the inkjet pretreatment solution dries, and the pigments in the inkjet ink are sufficiently aggregated by the DCDA / DETA sulfate before heat drying, thereby improving image fixation.

[0043] Furthermore, by incorporating organic solvents, the wettability of the inkjet pretreatment solution on the surface of non-absorbent substrates can be improved, reducing the repulsion of the inkjet pretreatment solution. As a result, unevenness in the inkjet pretreatment solution caused by repulsion can be suppressed, allowing DCDA / DETA sulfate to be distributed as uniformly as possible over a predetermined area of ​​the surface of the non-absorbent substrate, thereby improving the fixation of the image formed thereon with nearly uniformity across the entire surface.

[0044] Examples of humectants include glycerol and various glycols, with glycols being particularly preferred. Preferably, the glycol has a boiling point at 1 atm that is above 100°C and below 250°C. However, if the drying rate of the inkjet pretreatment solution is too low, the inkjet ink printed on it may bleed, resulting in an unclear image. Therefore, it is preferable to use a combination of glycols: one that spreads relatively easily (hereinafter referred to as "humectant A") and one that has a relatively high moisturizing effect (hereinafter referred to as "humectant B").

[0045] As described above, humectant B excels at slowing down the drying of the inkjet pretreatment solution. Humidifier A, on the other hand, has higher wettability on the surface of non-absorbent substrates compared to humectant B, thus making it easier for the inkjet pretreatment solution to spread on the substrate surface and promoting its drying. Therefore, by using humectants A and B together, the drying speed of the inkjet pretreatment solution can be appropriately adjusted, improving both image fixation and sharpness.

[0046] As humectant A, one or more of the following can be used, for example: 1,2-hexanediol (boiling point at 223°C, 1 atm, the same applies below), 1,2-pentanediol (120°C), 1,2-butanediol (190.5°C), diethylene glycol monobutyl ether (231°C), propylene glycol monopropyl ether (149°C), etc.

[0047] Furthermore, as humectant B, one or more of the following can be used: 1,2-propanediol (propylene glycol, 187.4°C), 1,3-propanediol (213°C), 1,3-butanediol (207.5°C), 1,4-butanediol (235°C), 1,5-pentanediol (238°C), 1,6-hexanediol (249°C), etc.

[0048] When using humectant A and humectant B in combination, the ratio of the two, expressed as a mass ratio (humectant A) / (humectant B), is preferably 1 / 4 or more, particularly 1 / 3 or more, and preferably 1 / 3 or less, particularly 1 / 1 or less.

[0049] If the proportion of humectant A is higher than this range, the drying speed of the inkjet pretreatment solution may become too high, potentially reducing image fixation. On the other hand, if the proportion of humectant A is lower than the above range, the drying speed of the inkjet pretreatment solution may become too low, potentially reducing image clarity. In contrast, by setting the mass ratio of humectant A to humectant B (humectant A) / (humectant B) within the above range, the drying speed of the inkjet pretreatment solution can be appropriately adjusted as described above, further improving both image fixation and clarity.

[0050] Furthermore, the amount of the humectant is preferably 15% by mass or more, particularly 18% by mass or more, of the total amount of the inkjet pretreatment solution, and preferably 25% by mass or less, particularly 22% by mass or less.

[0051] If the amount of humectant is below this range, the aforementioned effect of slowing the drying of the inkjet pretreatment solution and improving image fixation, achieved by incorporating the humectant, may not be fully obtained. Furthermore, the effect of improving the wettability of the inkjet pretreatment solution on the surface of non-absorbent substrates and reducing their repulsion may not be fully obtained, resulting in uneven distribution of DCDA / DETA sulfate and uneven image fixation formed on the substrate.

[0052] On the other hand, if the amount of humectant exceeds the above range, the amount of DCDA / DETA sulfate may be relatively insufficient, and the effect of DCDA / DETA sulfate in improving image fixation may not be fully obtained. In addition, excessive humectants may cause environmental burden.

[0053] In contrast, by setting the amount of humectant within the above range, it is possible to improve the wettability of the inkjet pretreatment solution on the surface of a non-absorbent substrate while reducing the environmental burden, and to adjust its drying speed. As a result, the image fixation can be improved as uniformly as possible on the surface of a non-absorbent substrate.

[0054] As mentioned above, when using two types of moisturizers, moisturizer A and moisturizer B, the total amount should be within the range specified above.

[0055] <Other Components> The inkjet pretreatment solution may contain various conventionally known additives used for inkjet inks. Examples of such additives include leveling agents, antifungal agents, preservatives, and antibacterial agents. The amounts of each of these additives can be set arbitrarily. By adding water to each of the above components to make a total volume of 100% by mass, an aqueous inkjet pretreatment solution is prepared.

[0056] Ink Set The ink set of the present invention is characterized by comprising the inkjet pretreatment liquid of the present invention described above and at least one aqueous inkjet ink. As the aqueous inkjet ink, as described above, a pigment dispersion type is preferably used, in which a pigment is used as a coloring agent and such pigment is dispersed in the ink by its own self-dispersing properties or by an anionic dispersant.

[0057] <Pigments> Any inorganic pigment and / or organic pigment can be used as pigments. Examples of inorganic pigments include metal compounds such as titanium dioxide and iron oxide, or various types of carbon black, such as neutral, acidic, and basic, produced by known methods such as the contact method, furnace method, and thermal method.

[0058] Examples of organic pigments include azo pigments (including azo lakes, insoluble azo pigments, condensed azo pigments, or chelated azo pigments), polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, or quinophthalone pigments), dye chelates (e.g., basic dye chelates, acid dye chelates), nitro pigments, nitroso pigments, and aniline black. One or more types of pigments can be used depending on the color of the inkjet ink. Specific examples of pigments are listed below.

[0059] (Yellow Pigment) CI Pigment Yellow 1, 2, 3, 12, 13, 14, 14C, 16, 17, 20, 24, 73, 74, 75, 83, 86, 93, 94, 95, 97, 98, 109, 110, 114, 117, 120, 125, 128, 129, 130, 137, 138, 139, 147, 148, 150, 151, 154, 155, 166, 168, 180, 185, 213, 214 (Magenta Pigment) CI Pigment Red 5, 7, 9, 12, 48(Ca), 48(Mn), 49, 52, 53, 57(Ca), 57:1, 97, 112, 122, 123, 149, 168, 177, 178, 179, 184, 202, 206, 207, 209, 242, 254, 255 (Cyan Pigment) CI Pigment Blue 1, 2, 3, 15, 15:1, 15:3, 15:4, 15:6, 15:34, 16, 22, 60 (Black Pigment) CI Pigment Black 7 (Orange Pigment) CI Pigment Orange 36, 43, 51, 55, 59, 61, 71, 74 (Green Pigment) CI Pigment Green 7, 36 (Violet Pigment) CI Pigment Violet 19, 23, 29, 30, 37, 40, 50 (Pigment Dispersion) As mentioned above, it is preferable to incorporate pigments into inkjet inks as pigment dispersions, which are dispersed in an aqueous dispersion medium such as water, either by their own self-dispersing properties or by the function of an anionic dispersant, in order to improve the dispersibility of the pigments.

[0060] Examples of anionic dispersants used to form such pigment dispersions and disperse pigments include DISPERBYK® 180, 190, 191, and 2010 from Bic Chemie, and Solspers® J400, W100, 40000, and 45000 from Lubrizol.

[0061] Specific examples of pigment dispersions, though not limited to these, include, for example, the CAB-O-JET® series products manufactured by CABOT, which are carbon black pigment dispersions, in the case of black. The CAB-O-JET series pigment dispersions are made by dispersing carbon black in an aqueous dispersion medium using its own self-dispersing properties. One or more of these pigment dispersions can be used.

[0062] (Amount of pigment and dispersant) The amount of pigment to be incorporated into the inkjet ink can be arbitrarily set according to the color and color density of the inkjet ink. The amount of dispersant can also be set to any amount that can properly disperse the pigment in the water-based inkjet ink, depending on the amount of pigment, but it is particularly preferable that it be 2% by mass or more, and 60% by mass or less, relative to the total amount of pigment.

[0063] <Binder Resin> Binder resin may be added to inkjet ink. When binder resin is added, it functions as a binder between the surface of the substrate treated with the inkjet pretreatment solution and the pigment, thereby improving the water resistance, scratch resistance, and sharpness of the image.

[0064] In particular, it is preferable to use an aqueous emulsion or aqueous dispersion of a water-insoluble resin as the binder resin. Since aqueous emulsions and dispersions dissolve well in water, the inkjet ink is liquid, but the binder resin that is dried after printing and deposited on the surface of the substrate is insoluble in water, thus improving the water resistance of the printed image. As the water-insoluble binder resin that constitutes the aqueous emulsion or dispersion, for example, one or more of the following types of binder resins can be used.

[0065] Acrylic resins such as polyacrylic acid, acrylic acid-acrylonitrile copolymer, potassium acrylate-acrylonitrile copolymer, vinyl acetate-acrylic acid ester copolymer, and acrylic acid-alkyl acrylate copolymer; styrene-acrylic acid resins such as styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, styrene-methacrylic acid-alkyl acrylate copolymer, styrene-α-methylstyrene-acrylic acid copolymer, and styrene-α-methylstyrene-acrylic acid-alkyl acrylate copolymer; maleic acid resin, fumaric acid resin, styrene-maleic acid copolymer, and styrene-maleic anhydride copolymer.

[0066] Specific examples of binder resins, though not limited to these, include various products in the JONCRYL (registered trademark) series manufactured by BASF, which are aqueous emulsions of styrene-acrylic acid copolymer. One or more of these aqueous emulsions can be used.

[0067] (Amount of Binder Resin) The amount of binder resin is preferably 1% by mass or more, and preferably 20% by mass or less, of the total amount of inkjet ink in terms of solid content. If the amount of binder resin is less than this range, the effect of improving the water resistance, scratch resistance, and clarity of the image by incorporating the binder resin may not be sufficiently obtained. On the other hand, if the amount of binder resin exceeds the above range, the viscosity of the inkjet ink may increase, and it may not be able to be ejected properly from the nozzle of the ejection head of the inkjet printer. In addition, when used in a thermal ejection head in particular, it may be more prone to causing so-called coagulation.

[0068] In contrast, by setting the amount of binder resin within the above range, it is possible to suppress the increase in viscosity of the inkjet pretreatment solution, maintain good ejection performance, and reduce the likelihood of coagulation, while also improving the water resistance, scratch resistance, and clarity of the image.

[0069] <Other Components> Various conventionally known additives may be added to the inkjet ink. Examples of such additives include surfactants for adjusting the wettability of the inkjet ink, or humectants, leveling agents, fungicides, preservatives, and antibacterial agents similar to those used in inkjet pretreatment solutions. The amounts of each of these additives can be set arbitrarily. Water-based inkjet ink is prepared by adding water to each of the above components to make a total volume of 100% by mass.

[0070] <Ink Set> The inkjet inks constituting the ink set of the present invention may be single-color, or they may be multi-color inkjet inks of, for example, three colors such as cyan (C), magenta (M), and yellow (Y), four colors such as the above three colors plus black (B), or more.

[0071] 《Method for Manufacturing Printed Materials》 The method for manufacturing printed materials of the present invention is characterized by comprising a pretreatment step of printing an inkjet pretreatment liquid from the ink set of the present invention onto the surface of a non-absorbent substrate by an inkjet printing method, and a printing step of printing an image on the area of ​​the substrate surface on which the inkjet pretreatment liquid has been printed using an inkjet ink by an inkjet printing method. Furthermore, as described above, the method for manufacturing printed materials of the present invention may also include a heat drying step of heating and drying the substrate after the image has been printed.

[0072] In this case, considering the need to improve image fixation, it is preferable to perform the printing process after the pretreatment process and before the inkjet pretreatment solution printed on the surface of the substrate dries, as explained earlier. To achieve this, for example, a humectant can be added to the inkjet pretreatment solution as described above, or the distance between the inkjet pretreatment solution ejection head and the inkjet ink ejection head of the inkjet printer, as well as the substrate transport speed, can be adjusted.

[0073] The configuration of an inkjet printer for carrying out the printing method of the present invention can be arbitrarily set. Specifically, for example, an inkjet printer can be configured by arranging an inkjet pretreatment liquid, an inkjet ink ejection head, and a heating and drying mechanism in order along a transport path that transports a long substrate wound in a roll shape at a constant speed while unwinding it.

[0074] For the inkjet pretreatment solution and inkjet ink ejection heads, either on-demand or continuous type ejection heads, and either thermal or piezo-type ejection heads can be used. However, since both the inkjet pretreatment solution and inkjet ink contain polymers and binder resins that are prone to coagulation, it is preferable to use a piezo-type ejection head to improve ejection stability.

[0075] As the non-absorbent substrate used in the method for manufacturing printed materials of the present invention described above, various conventionally known substrates that do not absorb or have low absorbency to water-based inkjet inks can be used. Examples of such non-absorbent substrates include thermoplastic resin substrates such as polyvinyl chloride sheets, polyethylene terephthalate (PET) film, polypropylene film, polyethylene film, nylon film, polystyrene film, and polyvinyl alcohol film; metal substrates such as aluminum foil; and coated papers for printing such as glossy paper, specialty paper, cloth, film, OHP sheets, and general-purpose printing paper. Specific examples of coated papers for printing include various coated papers used in commercial and publishing printing, such as cast-coated paper, art paper, coated paper, lightweight coated paper, and lightly coated paper.

[0076] The substrate may have a smooth or textured surface for printing, and may be transparent, translucent, or opaque. Furthermore, two or more of these substrates may be laminated together. A release adhesive layer may be provided on the opposite side of the printing surface, or an adhesive layer may be provided on the printing surface after printing. The substrate may be in the form of a roll or a sheet. Polyvinyl chloride film and coated paper are particularly preferred as substrates. [Examples]

[0077] The present invention will be further described below based on examples and comparative examples, but the configuration of the present invention is not limited to these examples.

[0078] <Example 1> An aqueous solution of DCDA / DETA sulfate as a flocculant [Unisense KHP 11LU manufactured by Senka Co., Ltd., yellowish-brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 100 mPa·s], polyethyleneimine as a neutralizing agent [Epomin P-1000 manufactured by Nippon Shokubai Co., Ltd.], 1,2-hexanediol as humectant A, 1,3-propanediol as humectant B, leveling agent [Tego® Wet 280 manufactured by Evonik], preservative [Proxel® GXL manufactured by SC Johnson], and ion-exchanged water were each mixed in the proportions shown in Table 1, and after mixing, the mixture was filtered using a 5 μm membrane filter to prepare an inkjet pretreatment solution.

[0079] [Table 1] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0080] <Example 2> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of an aqueous solution of DCDA / DETA sulfate [Unisense KHP 12LU manufactured by Senka Co., Ltd., yellowish-brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 150 mPa·s] was added as a flocculant.

[0081] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0082] <Example 3> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of diethanolamine was added as a neutralizing agent.

[0083] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of diethanolamine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to humectants B was (humectant A) / (humectant B) = 1 / 1.9.

[0084] <Example 4> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that no neutralizing agent was added and the amount of ion-exchanged water was 75.9% by mass.

[0085] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 0% by mass of a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0086] <Comparative Example 1> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that 4.9% by mass of an aqueous solution of a phosphate of a copolymer of diallylamine and acrylamide (hereinafter sometimes abbreviated as "DAA / AAm phosphate") [Unisense KCA 100LU manufactured by Senka Co., Ltd., yellow-reddish-brown liquid, solid content concentration: 41%, molecular weight: 20,000 to 100,000, pH: 3, viscosity: 150 mPa·s] was added as a flocculant, and the amount of ion-exchanged water was 72.9% by mass.

[0087] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DAA / AAm phosphate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the sum of humectants A and B. The mass ratio of humectants A to humectants B was (humectant A) / (humectant B) = 1 / 1.9.

[0088] <Comparative Example 2> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that 10.1% by mass of an aqueous solution of methyl sulfate of a polymer of dimethylaminoethyl methacrylate (hereinafter sometimes abbreviated as "DMAEM methyl sulfate") [Unisense FPV 1000LU manufactured by Senka Co., Ltd., pale yellow liquid, solid content concentration: 20%, molecular weight: 100,000 to 500,000, pH: 5, viscosity 120 mPa·s] was added as a flocculant, and the amount of polyethyleneimine was 2.0% by mass and the amount of ion-exchanged water was 66.7% by mass.

[0089] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DMAEM methyl sulfate (solids) as a flocculant, 2.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0090] <Comparative Example 3> An inkjet pretreatment solution was prepared in the same manner as in Comparative Example 2, except that the amount of polyethyleneimine was 1.0% by mass and the amount of deionized water was 67.7% by mass.

[0091] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DMAEM methyl sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0092] <Comparative Example 4> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that 10.1% by mass of an aqueous solution of dimethylaminoethyl methacrylate polymer sulfate (hereinafter sometimes abbreviated as "DMAEM sulfate") [Unisense KPV 1000LU manufactured by Senka Co., Ltd., light brown liquid, solid content concentration: 20%, molecular weight: 100,000 to 500,000, pH: 4, viscosity 2700 mPa·s] was added as a flocculant, and the amount of ion-exchanged water was 67.7% by mass.

[0093] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DMAEM sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0094] <Example 5> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of aqueous solution of DCDA / DETA sulfate as a coagulant was 0.4% by mass, and the amount of ion-exchanged water was 77.4% by mass.

[0095] The total amount of the inkjet pretreatment solution consisted of 0.3% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0096] <Example 6> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of aqueous solution of DCDA / DETA sulfate as a coagulant was 0.7% by mass, and the amount of ion-exchanged water was 77.1% by mass.

[0097] The total amount of the inkjet pretreatment solution consisted of 0.5% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0098] <Example 7> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of aqueous solution of DCDA / DETA sulfate as a coagulant was 7.1% by mass, and the amount of ion-exchanged water was 70.7% by mass.

[0099] The total amount of the inkjet pretreatment solution consisted of 5.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0100] <Example 8> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of aqueous solution of DCDA / DETA sulfate as a coagulant was 8.5% by mass, and the amount of ion-exchanged water was 69.3% by mass.

[0101] The total amount of the inkjet pretreatment solution consisted of 6.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0102] <Example 9> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of polyethyleneimine as a neutralizing agent was 1.3% by mass and the amount of deionized water was 74.6% by mass.

[0103] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.3% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0104] <Example 10> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of polyethyleneimine as a neutralizing agent was 1.5% by mass and the amount of deionized water was 74.4% by mass.

[0105] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.5% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0106] <Example 11> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of glycerol was added instead of humectant A.

[0107] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of glycerol and humectant B combined.

[0108] <Example 12> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of 1,4-butanediol was added as humectant B.

[0109] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0110] <Example 13> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of 1,2-propanediol was added as humectant B.

[0111] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0112] <Example 14> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of 1,2-butanediol was added as humectant A.

[0113] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0114] <Example 15> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of diethylene glycol monobutyl ether was added as humectant A.

[0115] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0116] <Example 16> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the same amount of 1,2-butanediol was added as humectant A, and the same amount of 1,4-butanediol was added as humectant B.

[0117] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 1.9.

[0118] <Example 17> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of 1,2-hexanediol as humectant A was 15.0% by mass and the amount of 1,3-propanediol as humectant B was 5.0% by mass.

[0119] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 3 / 1.

[0120] <Example 18> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of 1,2-hexanediol as humectant A was 10.0% by mass and the amount of 1,3-propanediol as humectant B was 10.0% by mass.

[0121] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the sum of humectants A and B. The mass ratio of humectants A to humectants B was (humectant A) / (humectant B) = 1 / 1.

[0122] <Example 19> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of 1,2-hexanediol as humectant A was 5.0% by mass and the amount of 1,3-propanediol as humectant B was 15.0% by mass.

[0123] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 3. <Example 20> An inkjet pretreatment solution was prepared in the same manner as in Example 1, except that the amount of 1,2-hexanediol as humectant A was 4.0% by mass and the amount of 1,3-propanediol as humectant B was 16.0% by mass.

[0124] The total amount of the inkjet pretreatment solution consisted of 2.0% by mass of DCDA / DETA sulfate (solids) as a flocculant, 1.0% by mass of polyethyleneimine as a neutralizing agent, and 20.0% by mass of the combined amount of humectants A and B. The mass ratio of humectants A to B was (humectant A) / (humectant B) = 1 / 4.

[0125] <Inkjet Ink> A black inkjet ink was prepared by mixing a carbon black pigment dispersion [CAB-O-JET200 manufactured by Cabot Corporation, carbon black concentration: 20%], an aqueous emulsion of styrene-acrylic acid copolymer [Joncryl 8211 manufactured by BASF Corporation, solids content concentration: 44%], 1,2-butanediol as a humectant, a leveling agent [Tego Wet 280 manufactured by Evonik], a preservative [Proxel GXL manufactured by SC Johnson], and deionized water in the proportions shown in Table 2, and then filtering the mixture through a 5 μm membrane filter.

[0126] [Table 2] 《Actual Testing》 As described earlier, the inkjet printer was prepared with an inkjet pretreatment solution, an inkjet ink ejection head, and a heating and drying mechanism arranged in sequence along a transport path that transported a long roll of substrate at a constant speed while unwinding it. The substrate transport speed was set to 0.5 m / second, the distance between the inkjet pretreatment solution ejection head and the inkjet ink ejection head was set to 1.5 m, and the inkjet ink was printed 3 seconds after the inkjet pretreatment solution was printed. As the substrate, white PVC media 5829R manufactured by MacTac was used. When the state of the inkjet pretreatment solution in the examples and comparative examples was observed immediately before printing the inkjet ink, it was confirmed that in all cases, although the progress of drying differed, the material was not completely dry.

[0127] <Evaluation of Image Fixability> Using the inkjet pretreatment solution and inkjet ink prepared in each example and comparative example, a rectangular image with a length of 5 cm and a width of 5 mm in the substrate transport direction was printed on a substrate pretreated with the inkjet pretreatment solution at a resolution of 600 dpi. Next, the image after heat drying was scratched with a fingernail and its condition was observed to evaluate the image fixability according to the following criteria.

[0128] (Evaluation) ○: No scratch marks remained, and no changes were observed in the image. △: Faint scratch marks remained in the image, but the image did not peel off. ×: The image peeled off.

[0129] <Evaluation of Corrosion and Deterioration of the Discharge Head> The pH of the inkjet pretreatment solution prepared in each example and comparative example was measured, and the following criteria were used to evaluate whether there was a risk of corrosion or deterioration of the discharge head.

[0130] (Evaluation) ○: pH was between 7.0 and 9.0. △: pH was between 5.0 and 7.0, or above 9.0 and 10.0. ×: pH was below 5.0 or above 10.0.

[0131] <Evaluation of Discharge Stability> The inkjet pretreatment solutions prepared in each example and comparative example were used in the aforementioned inkjet printer, and when ejected 10,000 times continuously from the ejection head, the nozzle clogging was observed to evaluate the discharge stability according to the following criteria.

[0132] (Evaluation) ○: No nozzle clogging occurred up to 10,000 discharges. △: Nozzle clogging occurred between 100 and 1,000 discharges. ×: Nozzle clogging occurred in less than 100 discharges.

[0133] <Image Clarity Evaluation> The inkjet pretreatment solution and inkjet ink prepared in each example and comparative example were used with the above-mentioned inkjet printer to print MS Mincho font character images, a mixture of hiragana and kanji, in 4-point and 6-point font sizes at a resolution of 600 dpi onto substrates pretreated with the inkjet pretreatment solution. The printed character images were then observed and their clarity was evaluated according to the following criteria.

[0134] (Evaluation) ○: Both the 4-point and 6-point text images were clear and easily legible. △: The 4-point text image was not clear enough to be legible, but the 6-point text image, while slightly less clear, was still legible. ×: Both the 4-point and 6-point text images were unclear and illegible.

[0135] The results are shown in Tables 3 to 8. In the tables, "DCDA / DETA sulfate (I) aqueous solution" in the coagulant column refers to Unisense KHP 11LU [yellowish-brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 100 mPa·s], and "DCDA / DETA sulfate (II) aqueous solution" refers to Unisense KHP 12LU [yellowish-brown liquid, solid content concentration: 70%, molecular weight: less than 20,000, pH: 7, viscosity: 150 mPa·s].

[0136] [Table 3]

[0137] [Table 4]

[0138] [Table 5]

[0139] [Table 6]

[0140] [Table 7]

[0141] [Table 8] From the results of Examples 1-20 and Comparative Examples 1-4 in Tables 3-8, it was found that by selecting and using DCDA / DETA sulfate as a flocculant, it is possible to obtain an inkjet pretreatment solution that does not affect the metal and resin parts that make up the ejection head of an inkjet printer, allowing for stable ejection over a long period of time, and that also has an excellent effect in improving image fixation, while also being halogen-free.

[0142] From the results of Examples 1 to 10, it was found that, in order to further improve the above effects, it is preferable to include a neutralizing agent in the inkjet pretreatment solution, and that polyethyleneimine, which can also function as a flocculant, is preferred as the neutralizing agent. Furthermore, it was found that by adjusting the amounts of DCDA / DETA sulfate and the neutralizing agent, the pH of the inkjet pretreatment solution should be 5 or higher, particularly 7 or higher, and 10 or lower, particularly 9 or lower.

[0143] From the results of Examples 1, 11-16, it was found that, considering the need to appropriately adjust the drying speed of the inkjet pretreatment solution to improve both image fixation and sharpness, it is preferable to include a humectant in the inkjet pretreatment solution, and that it is preferable to use humectant A and humectant B in combination as described above.

[0144] Furthermore, from the results of Examples 1, 17-20, it was found that, in order to further improve the above effects, it is preferable to use humectant A and humectant B in a mass ratio of 1 / 4 or more, particularly 1 / 3 or more, expressed as (humectant A) / (humectant B), and it is preferable to use them in a ratio of 1 / 3 or less, particularly 1 / 1 or less.

Claims

1. The flocculant comprises a sulfate of a copolymer of dicyandiamide and diethylenetriamine, and water. Furthermore, the inkjet pretreatment solution contains polyethyleneimine as a neutralizing agent.

2. The inkjet pretreatment solution according to claim 1, further comprising: humectant A selected from the group consisting of 1,2-hexanediol, 1,2-pentanediol, 1,2-butanediol, diethylene glycol monobutyl ether, and propylene glycol monopropyl ether; and humectant B selected from the group consisting of 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.

3. The inkjet pretreatment solution according to claim 2, comprising the humectant A and the humectant B in a mass ratio of 1 / 4 or more and 1 / 3 or less, expressed as (humectant A) / (humectant B).

4. An inkjet pretreatment solution according to any one of claims 1 to 3, wherein the hydrogen ion concentration (pH) is 5 or higher and 10 or lower.

5. An ink set comprising the inkjet pretreatment solution described in claim 1 and at least one aqueous inkjet ink.

6. The ink set according to claim 5, wherein the inkjet ink comprises a pigment as a coloring agent.

7. A method for manufacturing a printed material, comprising a pretreatment step of printing the inkjet pretreatment liquid from the ink set described in claim 5 onto the surface of a non-absorbent substrate by an inkjet printing method, and a printing step of printing an image on the area of ​​the substrate surface on which the inkjet pretreatment liquid has been printed by an inkjet printing method using the inkjet ink.

8. The method for manufacturing a printed article according to claim 7, wherein the printing step is performed after the pretreatment step and before the inkjet pretreatment liquid printed on the surface of the substrate dries.

Citation Information

Patent Citations

  • Pre-processing liquid for recording material and image recording method

    JP2002079739A

  • Inkjet recording method and inkjet recording device

    JP2015134493A

  • Toner for positive charging, liquid developer, developer, developer cartridge, process cartridge, and image forming apparatus

    JP2016126088A

  • Inkjet recording method and inkjet recording apparatus

    JP2018192787A

  • Aqueous pretreatment liquid, aqueous recording liquid set, and method for producing printed matter

    JP2019111770A