Alloys, aggregates of alloy nanoparticles, and catalysts

Alloys with high uniformity of solid solution, composed of elements that do not form solid solutions, address the issue of phase separation and performance degradation under high temperatures, ensuring stable catalyst performance.

JP7954943B2Active Publication Date: 2026-11-24THE JAPAN SCI & TECH AGENCY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022535337
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-06
Filing Date
2021-07-06
Publication Date
2026-11-24
Estimated Expiration
2041-07-06

AI Technical Summary

Technical Problem

Existing alloys and high-entropy alloy nanoparticles suffer from non-uniform solid solution uniformity, leading to phase separation and reduced catalyst performance when exposed to high temperatures.

Method used

Development of alloys composed of three or more elements with a standard deviation of elemental distribution within 15 atomic% or less, ensuring high uniformity and stability, particularly suitable for high-entropy alloys with elements that do not form solid solutions in phase equilibrium diagrams.

Benefits of technology

The novel alloys exhibit enhanced compositional stability and durability, maintaining catalyst performance under high temperatures, suitable for long-lasting chemical reaction catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954943000026
    Figure 0007954943000026
  • Figure 0007954943000027
    Figure 0007954943000027
  • Figure 0007954943000028
    Figure 0007954943000028
Patent Text Reader

Abstract

Provided is a novel alloy configured from three or more elements, wherein: the standard deviation of the distributions, within the alloy, of the elements constituting the alloy is equal to or less than 15 at%; and the alloy has high solid-solution uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to alloys, aggregates of alloy nanoparticles, and catalysts. In particular, it relates to novel alloys or aggregates of alloy nanoparticles composed of three or more elements and exhibiting high solid solution uniformity, and catalysts containing such alloys or aggregates of alloy nanoparticles. [Background technology]

[0002] Alloys in which metal elements in combinations that cannot be mixed at the atomic level are dissolved in solid solution, as well as high-entropy alloy nanoparticles, are known (see Patent Document 1 and Non-Patent Documents 1-4).

[0003] Patent Document 1 describes that by adding a third element M (M = at least one of Rh, Ir, Au, Ag, and Pt) to PdRu, catalytic performance can be maintained even when used at high temperatures for a long time. Patent Document 1 did not specify the uniformity of the solid solution (or mixture) of the alloy.

[0004] Non-Patent Document 1 describes a method for producing high-entropy alloy nanoparticles, in which five or more types of metal salts are supported on a carbon material (carbon nanofiber), a large current is applied, the material is rapidly heated to a high temperature of 2000K or higher, and then rapidly cooled. On page 3 of Non-Patent Document 1, in the right column, it is stated that the elemental composition variation of a five-type mixture of PtPdCoNiFe is about 10%, which is small compared to lithography methods where the variation exceeds 50%.

[0005] Non-patent document 2 describes a manufacturing method for forming high-entropy alloy nanoparticles on a graphene support by mechanically pulverizing a graphene support and a metal. The elemental composition of the FeCrCoCuNi nanoparticles shown in Fig. 9 did not show a uniform mixture.

[0006] Non-patent document 3 describes a manufacturing method for obtaining nanoparticles by irradiating a target of bulk high-entropy alloys of 3d transition metals (period 4) with a laser. Table 2 lists the composition of CoCrFeMnNi nanoparticles, but the uniformity of the mixture was not shown.

[0007] Non-patent document 4 describes a manufacturing method for obtaining nanoparticles by solvent thermal synthesis at approximately 200°C using organometallic salts of platinum group elements. Fig. 5 shows scanning transmission electron microscope (STEM)-energy dispersive X-ray analysis (EDS, also known as EDX) images of PtRhRu and PtPdIrRhRu particles, but the homogeneity of the mixture at the atomic level could not be determined from the images. [Prior art documents] [Patent Documents]

[0008] [Patent Document 1] WO2017 / 150596 [Non-patent literature]

[0009] [Non-Patent Document 1] Science (2018) 359, 1489-1494 [Non-Patent Document 2] SCIENTIFIC REPORTS (2018) 8:8737 [Non-Patent Document 3] RSC Adv. (2019) 9, 18547-18558 [Non-Patent Document 4] Adv.Funct.Mater. (2019) 1905933 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] Non-Patent Document 4 states in the lower-left section on page 6 that the obtained nanoparticles are stable up to 700 K (427°C). In particular, an XRD pattern corresponding to hcp appears at 800 K, suggesting the emergence of an hcp Ru-rich phase. On the other hand, it is stated that the peak positions of fcc remain almost unchanged. If a homogeneous alloy is initially formed and Ru primarily precipitates, as shown in Table S1, since Ru has a smaller atomic radius compared to others, its lattice constant expands according to Vegard's law. Furthermore, Fig. S16 shows the relationship between melting point and crystallite size, and it is noted that Ru as a single metal has a size of 2 nm or less. Based on these, although an fcc alloy with large crystallites and small Ru-rich particles are initially precipitated non-uniformly, Non-Patent Document 4 treats it as a homogeneous fcc alloy being formed in XRD due to the small size of the crystals. When the nanoparticles are heated, the small hcp particles coarsen and prominent peaks appear in XRD, while the peak positions of fcc do not change, so it is considered that there is almost no change in the metal composition ratio (Ru does not precipitate from the alloy and exists as separate particles). That is, it is considered that the nanoparticles obtained in Non-Patent Document 4 are not uniformly mixed. In the case of solvothermal synthesis, since the sealed vial is gradually heated, metals that are easily decomposed and reduced react gradually, and since the reduction rate differs for each metal, it is considered that it is difficult to form a homogeneous alloy.

[0011] As described above, in alloys in which metal elements of combinations that cannot be mixed at the atomic level are solid-solubilized, and in high-entropy alloy nanoparticles, there is room for improvement in the uniformity of solid solution. The problem to be solved by the present invention is to provide a novel alloy that is composed of three or more elements and has high uniformity of solid solution. [Means for Solving the Problems]

[0012] In the present invention, a novel alloy having remarkably high uniformity of solid solution, which has not been known in the past, has been found to solve the above-mentioned problems. Such an alloy, when viewed macroscopically as a bulk or an aggregate of particles (powder), is a novel alloy with completely different physical properties in that it has high uniformity of solid solution even if the average composition is comparable to that of conventional alloys. The configuration of the present invention, which is a specific means for solving the above-mentioned problems, and a preferred configuration of the present invention will be described below.

[0013] [1] An alloy composed of three or more elements, An alloy, wherein the standard deviation of the distribution of each element constituting the alloy in the alloy is all 15 atomic% or less. [2] The alloy according to [1], wherein the correlation coefficient of the distribution of two elements constituting the alloy is all within ±0.50. [3] The alloy according to [1] or [2], wherein the elements constituting the alloy include a combination of elements that do not form a solid solution in a phase equilibrium diagram. [4] The alloy according to any one of [1] to [3], wherein the elements constituting the alloy include at least three types selected from the group consisting of platinum group (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, Cd, Hg, In, Tl, Sn, Pb, Sb, Bi, Mo, W, Tc, Re, 3d metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), Ga, Ge, As, H, B, Al, C, Si, N, P, Y, Zr, Nb, lanthanoids, Hf, and Ta. [5] The alloy according to any one of [1] to [4], wherein the elements constituting the alloy include at least one type selected from the group consisting of Ru, Rh, Pd, Os, Ir, Pt, Ag, Au, and Ni. [6] The number of elements constituting the alloy is m, where m is an integer of 3 or more, For each i element constituting the alloy, where i is an integer of 1 or more and m or less, the average composition in the alloy is C i When expressed in atomic%, The standard deviation of the distribution of each element in the alloy is all represented by the following formula 1, s i Using 2.5×s i The alloy according to any one of [1] to [5], which is atomic% or less.

number

[10] The alloy according to [8], wherein nanoparticles are supported on a carrier.

[11] The alloy according to

[10] , wherein the carrier is a non-carbon material carrier or a particulate carbon carrier.

[12] [8] An aggregate of alloy nanoparticles containing 98% or more of the alloy described above.

[13] A catalyst comprising an alloy as described in any one of items [1] to

[11] , or an aggregate of alloy nanoparticles as described in

[12] . [Effects of the Invention]

[0014] According to the present invention, it is possible to provide a novel alloy composed of three or more elements and exhibiting high uniformity of solid solution. [Brief explanation of the drawing]

[0015] [Figure 1] Figure 1 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 1 using STEM-EDS. [Figure 2] Figure 2(A) is a graph showing the characteristic X-ray counts for each position (distance from the 0.00 nm position; the same applies to subsequent graphs) in the area indicated by the arrow in Figure 1. Figure 2(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 1. [Figure 3]Figure 3 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 1 using STEM-EDS. [Figure 4] Figure 4(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 3. Figure 4(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 3. [Figure 5] Figure 5 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 1 using STEM-EDS. [Figure 6] Figure 6(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 5. Figure 6(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 5. [Figure 7] Figure 7 shows the high-angle annular dark field (HAADF) STEM image and energy-dispersive X-ray analysis (EDS) map of the alloy obtained in Example 1. [Figure 8] Figure 8 shows the energy powder X-ray diffraction (XRD or PXRD) pattern of the alloy obtained in Example 1. [Figure 9] Figure 9 is a transmission electron microscope (TEM) image of the alloy obtained in Example 1. [Figure 10] Figure 10(A) is a graph showing the hydrogen evolution reaction (HER) catalytic activity of the alloy obtained in Example 1. Figure 10(B) is a graph comparing the HER catalytic activity of the alloy obtained in Example 1 when measured three times. [Figure 11] Figure 11 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 11 using STEM-EDS. [Figure 12] Figure 12(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 11. Figure 12(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 11. [Figure 13]Figure 13 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 11 using STEM-EDS. [Figure 14] Figure 14(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 13. Figure 14(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 13. [Figure 15] Figure 15 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 11 using STEM-EDS. [Figure 16] Figure 16(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 15. Figure 16(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 15. [Figure 17] Figure 17 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 11 using STEM-EDS. [Figure 18] Figure 18(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 17. Figure 18(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 17. [Figure 19] Figure 19 shows the HAADF-STEM image and energy-dispersive X-ray analysis (EDS) map of the alloy obtained in Example 11. [Figure 20] Figure 20 shows the energy powder X-ray diffraction (XRD or PXRD) pattern of the alloy obtained in Example 11. [Figure 21] Figure 21 is a transmission electron microscope (TEM) image of the alloy obtained in Example 11. [Figure 22] Figure 22(A) is a graph showing the HER catalytic activity of the alloy obtained in Example 11. Figure 22(B) is a graph comparing the HER catalytic activity of the alloy obtained in Example 11 when measured three times. [Figure 23] Figure 23 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 21 using STEM-EDS. [Figure 24]Figure 24(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 23. Figure 24(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 23. [Figure 25] Figure 25 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 21 using STEM-EDS. [Figure 26] Figure 26(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 25. Figure 26(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 25. [Figure 27] Figure 27 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 21 using STEM-EDS. [Figure 28] Figure 28(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 27. Figure 28(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 27. [Figure 29] Figure 29 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 22 using STEM-EDS. [Figure 30] Figure 30(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 29. Figure 30(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 29. [Figure 31] Figure 31 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Example 22 using STEM-EDS. [Figure 32] Figure 32(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 31. Figure 32(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 31. [Figure 33] Figure 33 shows the HAADF-STEM image and energy-dispersive X-ray analysis (EDS) map of the alloy obtained in Example 21. [Figure 34]Figure 34 shows the HAADF-STEM image and energy-dispersive X-ray analysis (EDS) map of the alloy obtained in Example 22. [Figure 35] Figure 35 shows the energy powder X-ray diffraction (XRD or PXRD) patterns of the alloys obtained in Examples 21 and 22. [Figure 36] Figure 36(A) is a transmission electron microscope (TEM) image of the alloy obtained in Example 21. Figure 36(B) is a transmission electron microscope (TEM) image of the alloy obtained in Example 22. [Figure 37] Figure 37 is a graph showing the HER catalytic activity of the alloys obtained in Examples 21 and 22. [Figure 38] Figure 38 shows the HAADF-STEM image and energy-dispersive X-ray analysis (EDS) map of the alloy obtained in Example 31. [Figure 39] Figure 39 shows the HAADF-STEM image and electron energy loss spectroscopy (EELS) map of the alloy obtained in Example 31. [Figure 40] Figure 40 shows the energy powder X-ray diffraction (XRD or PXRD) pattern of the alloy obtained in Example 31. [Figure 41] Figure 41(A) is a transmission electron microscope (TEM) image of the alloy obtained in Example 31. Figure 41(B) is a transmission electron microscope (TEM) image of PdRu used as a raw material in Example 31. [Figure 42] Figure 42 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 41 using STEM-EDS. [Figure 43] Figure 43(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 42. Figure 43(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 42. [Figure 44] Figure 44 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Comparative Example 42 using STEM-EDS. [Figure 45]Figure 45(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 44. Figure 45(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 44. [Figure 46] Figure 46 is a scanning transmission electron microscope image used in another EDS line analysis of the alloy obtained in Comparative Example 42 using STEM-EDS. [Figure 47] Figure 47(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 46. Figure 47(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 46. [Figure 48] Figure 48 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 51 using STEM-EDS. [Figure 49] Figure 49(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 48. Figure 49(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 48. [Figure 50] Figure 50 is a scanning transmission electron microscope image used in the EDS line analysis of the alloy obtained in Example 61 using STEM-EDS. [Figure 51] Figure 51(A) is a graph showing the characteristic X-ray counts for each position in the area indicated by the arrow in Figure 50. Figure 51(B) is a graph showing the composition of each position in the area indicated by the arrow in Figure 50. [Modes for carrying out the invention]

[0016] The present invention will be described in detail below. The following descriptions of constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, numerical ranges represented by "~" mean a range that includes the numbers written before and after "~" as the lower and upper limits.

[0017] [alloy] The alloy of the present invention is an alloy composed of three or more elements, wherein the standard deviation of the distribution of each element constituting the alloy within the alloy is 15 atomic percent or less. This configuration makes it possible to provide a novel alloy composed of three or more elements with high solid solution uniformity. Solid solution uniformity of an alloy refers to a measure of the solid solution state, specifically how uniform the compositional distribution of the solid solution is. Conventionally, alloys composed of multiple non-solid-solution elements have sometimes experienced a gradual uneven distribution of metals over time, ultimately leading to phase separation. Alloys with low solid-solution uniformity and standard deviations exceeding the upper limit of the range specified herein may also experience a gradual uneven distribution of metals over time, ultimately leading to phase separation. Compared to the alloys of the present invention, such alloys may exhibit inferior catalyst performance and may have a short lifespan or become unstable when used in environments exposed to high temperatures for extended periods. In contrast, the alloy of the present invention is highly homogenized, resulting in excellent compositional stability and less susceptibility to phase separation. Therefore, the alloy of the present invention is suitable for applications requiring high durability, such as chemical reaction catalysts, which are exposed to high temperatures for extended periods. In other words, long-lasting catalysts can be produced using the alloy of the present invention. It is more preferable that the alloy exhibits a stable structure when heated and has high material uniformity. In particular, in high-entropy alloys with five or more elements, the large configuration entropy S leads to a stable, uniform solid solution phase at high temperatures, exceeding the Gibbs free energy G = H - TS (where H is enthalpy, T is absolute temperature, and S is entropy). It is especially preferable that the alloy exhibits a stable structure and high material uniformity when heated to, for example, 500K or higher (preferably 700K or higher, more preferably 900K or higher). Material uniformity can be confirmed by in situ XRD or STEM-EDS. Furthermore, it is preferable that the alloy is composed of elements mixed at the atomic level. Specifically, when the alloy is used as an aggregate of alloy nanoparticles, it is preferable that the aggregate of alloy nanoparticles contains 98% or more of the alloy of the present invention. Alternatively, it is preferable that any alloy nanoparticles constituting the aggregate of alloy nanoparticles contain all of three or more elements as constituent elements. Also, when used as a catalyst containing a large number of alloy nanoparticles, it is preferable that the alloy nanoparticles contained in the catalyst contain 98% or more of the alloy nanoparticles of the present invention. Alternatively, it is preferable that any alloy nanoparticles contained in the catalyst contain all of three or more elements as constituent elements. Preferred embodiments of the present invention will be described below.

[0018] <Element> The alloy of the present invention is composed of three or more elements, preferably composed of 3 to 50 elements, more preferably composed of 3 to 25 elements, particularly preferably composed of 3 to 10 elements, even more preferably composed of 3 to 5 elements, and even more preferably composed of 3 or 4 elements.

[0019] There are no particular restrictions on the types of elements that make up the alloy of the present invention. The elements constituting the alloy may include combinations of elements that do not form solid solutions in the phase equilibrium phase diagram, or they may not include combinations of elements that do not form solid solutions in the phase equilibrium phase diagram. In other words, the alloy may be a combination of elements that cannot easily form solid solutions, or a combination of elements that can easily form solid solutions. The phase equilibrium phase diagram is also called a phase diagram, phase diagram, alloy phase diagram, etc., and all diagrams similar to these may be used as phase equilibrium phase diagrams in this specification. The phase equilibrium phase diagram may be a phase equilibrium phase diagram of two elements, or a phase equilibrium phase diagram of three or more elements.

[0020] According to the present invention, a novel alloy with high solid solution uniformity can be provided using a wide variety of elements. Therefore, it is preferable that the elements constituting the alloy include combinations of elements that do not form a solid solution in the phase equilibrium phase diagram. In a phase equilibrium diagram, a combination of elements that does not form a solid solution is one in which there is an immiscible region of 30 atomic percent or more at 1000°C and a pressure of 1 atm (normal pressure). It is more preferable that the elements constituting the alloy include a combination of elements that do not form a solid solution in a two-phase equilibrium phase diagram or a three-phase equilibrium phase diagram, and it is particularly preferable that the combination of elements does not form a solid solution in both a two-phase equilibrium phase diagram and a three-phase equilibrium phase diagram. It is preferable that the two combinations of elements constituting the alloy include at least one combination of elements that do not form a solid solution in a binary phase equilibrium phase diagram, and it is more preferable that the combination includes two or more combinations of elements that do not form a solid solution in a binary phase equilibrium phase diagram.

[0021] Combinations of elements that do not form a solid solution in at least one pair of binary phase equilibrium phase diagrams among the two elements constituting the alloy include PdRu, AuIr, AgRh, AuRh, AuRu, CuRu, CuIr, AgCu, FeCu, AgIr, AgRu, MoRu, RhC, RuN, RuSn, PdOs, CuOs, AgOs, AuOs, CuRh, IrRh, IrPd, AgPt, AuPt, and combinations of other precious metals with most non-precious metals. Alloy nanoparticles containing combinations of two elements that do not form a solid solution in a binary phase equilibrium phase diagram among three or more elements constituting the alloy include PdRuB, AuRuIr, RuRhAu, PtIrRu, FeRuRh, AuIrRh, AgIrRh, and AuPdRu. Examples of alloy nanoparticles containing combinations of two elements that do not form a solid solution in a two-phase equilibrium phase diagram among the five or more elements that make up the alloy include combinations of PdRuRhOsIr and Pt, combinations of RuRhPdIr and Pt, and AuRuRhIrPt. Among the three combinations of elements that make up an alloy, combinations of elements that do not form a solid solution in at least one set of ternary phase equilibrium phase diagrams include PdRuB, AuRuIr, RuRhAu, PtIrRu, FeRuRh, AuIrRh, AgIrRh, and AuPdRu. Even for combinations of elements for which a two-phase equilibrium phase diagram is not known, if there is an immiscible region of 30 atomic percent or more at 1000°C and a pressure of 1 atm, the combination is included in the list of elements that do not form solid solutions in the phase equilibrium phase diagram.

[0022] It is preferable that the alloy contains an oxidation-resistant metal as a constituent element. An oxidation-resistant metal refers to a metal that maintains its metallic state (where the metallic structure can be confirmed, such as fcc, bcc, hcp, etc.) with a particle size of 50 nm or less, such as noble metals or Ni.

[0023] The alloy of the present invention preferably contains at least three types from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, Cd, Hg, In, Tl, Sn, Pb, Sb, Bi, Mo, W, Tc, Re, 3d metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), Ga, Ge, As, H, B, Al, C, Si, N, P, Y, Zr, Nb, lanthanides, Hf, and Ta. It is more preferable that the elements constituting the alloy include at least three from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, Cd, Hg, In, Tl, Sn, Pb, Sb, Bi, Mo, W, Tc, Re, 3d metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), Ga, Ge, As, B, Al, C, Si, N, P, and lanthanides. Among these, it is particularly preferable that the elements constituting the alloy include three types from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, In, Tl, Sn, Mo, W, Re, 3d metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), B, C, N, and lanthanides. It is more preferable that the elements constituting the alloy include at least three from the group consisting of Ru, Rh, Ir, Pt, Au, Ag, Sn, Cu, Mo, W, Re, Fe, Co, Ni, B, and N.

[0024] On the other hand, it is preferable that the elements constituting the alloy include at least one from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, and Ni, and more preferably two. It is particularly preferable that it includes at least one from the group consisting of Ru, Rh, Ir, Pt, Ag, Au, and Ni, and more particularly preferable that it includes two.

[0025] There are no particular restrictions on the crystal structure of the alloy. Depending on the composition of the alloy and the overall average number of valence electrons, the alloy may have crystal structures such as fcc (face-centered cubic), hcp (close-packed hexagonal), or bcc (body-centered cubic). One preferred embodiment of the present invention is an alloy (particle) with an fcc or hcp solid solution. However, if the alloy is an ordered alloy (i.e., has an ordered phase), forms an amorphous structure, or forms an intermetallic compound, it can maintain a structure other than those described above. Note that when elements with significantly different atomic radii or electronegativity are mixed, intermetallic compounds may be formed. In the case of intermetallic compounds, the atomic arrangement is not random, but rather an ordered alloy. Examples include cases where at least one of the two combinations of elements constituting the alloy is RhC, PdB, a combination of a noble metal and a transition metal, or a combination of a noble metal such as RuSn and a typical metal. However, in the case of an ordered alloy with many constituent elements, the atomic sites within the ordered alloy may be randomly composed of specific elements. For example, at the atomic sites of elements with large atomic radii, elements with large atomic radii may be randomly arranged, and at the atomic sites of elements with small atomic radii, elements with small atomic radii may be randomly arranged. Of the six elements of the platinum group, four are fcc (face-centered cubic) (Rh, Pd, Ir, and Pt), and two are hcp (closest-packed hexagonal) (Os and Ru). One preferred embodiment of the present invention is an alloy (particle) with an fcc structure containing platinum group elements. Another preferred embodiment of the present invention is an alloy with an hcp structure containing platinum group elements. Even when using the six elements of the platinum group, the proportion of the fcc structure may be higher, as in the original proportions, or the proportion of the hcp structure may be higher.

[0026] Because the alloy of the present invention exhibits high solid solution uniformity, it is preferable that three or more elements are uniformly distributed and dissolved in the solid solution. Here, "uniformly distributed" means that there is no bias in the distribution of the three or more elements, and that the standard deviation of the distribution of each element constituting the alloy within the alloy is all below a certain value (for example, 15 atomic percent or less). Furthermore, it is preferable to confirm that there is no bias in the distribution of each element (atom) using energy-dispersive X-ray analysis (EDS) maps. It is also preferable to confirm a single fcc, bcc, or hcp pattern from powder X-ray diffraction (XRD). For example, even if fcc and hcp coexist, if the interatomic distances of both structures are equal, the constituent elements are considered to be uniformly distributed in each structure. In that case, the metallic composition of both the fcc and hcp structures will be equivalent, and therefore the interatomic distances will be equal to each other.

[0027] (Percentage of elements) In the present invention, there are no particular restrictions on the proportion (also called the composition ratio) of each element constituting the alloy. In other words, there are no particular restrictions on the average composition of the alloy of the present invention. In one preferred embodiment of the present invention, the upper limit of the proportion of the most abundant element when the entire alloy is considered as 100 atomic%, is 99.9 atomic% or less, 80 atomic% or less, 70 atomic% or less, 60 atomic% or less, 50 atomic% or less, 45 atomic% or less, 40 atomic% or less, or 35 atomic% or less. The lower limit for the proportion of the smallest element when the entire alloy is considered as 100 atomic percent is 0.1 atomic percent or more, 1 atomic percent or more, 5 atomic percent or more, 9 atomic percent or more, 10 atomic percent or more, or 15 atomic percent or more. Furthermore, the element with the highest atomic ratio is preferably 1 to 500 times, more preferably 1 to 5 times, even more preferably 1 to 3 times, particularly preferably 1 to 2 times, and most preferably 1 to 1.5 times, that of the element with the lowest atomic ratio. When the alloy of the present invention is a high-entropy solid solution alloy, it is preferable that the atomic ratios of the three or more elements be as close as possible.

[0028] <Standard deviation of the distribution> The alloy of the present invention has a standard deviation of the distribution of each element constituting the alloy within the alloy of 15 atomic percent or less, more preferably 14 atomic percent or less, particularly preferably 13 atomic percent or less, more preferably 12 atomic percent or less, even more preferably 11 atomic percent or less, even more preferably 10 atomic percent or less, and even more preferably 8.7 atomic percent or less. Furthermore, the standard deviation of the distribution of at least two elements constituting the alloy within the alloy is 15 atomic percent or less, more preferably 14 atomic percent or less, particularly preferably 13 atomic percent or less, even more preferably 12 atomic percent or less, even more preferably 11 atomic percent or less, even more preferably 10 atomic percent or less, and even more preferably 8.7 atomic percent or less. The standard deviation of the distribution of each element constituting the alloy within the alloy is preferably 50% or less of the composition ratio of that element within the alloy, more preferably 40% or less, particularly preferably 30% or less, and most preferably 20% or less.

[0029] It is preferable that the standard deviation of the distribution of each element within the alloy falls within a low range, as the number of elements constituting the alloy increases. When there are three elements constituting the alloy, it is preferable that the distribution falls within the above range. Consider a random alloy of m elements, where the elements constituting the alloy are uniform, and divide it into a small volume to perform a statistical analysis of the spatial distribution. The average composition of the alloy is (C1, C2, ..., C m If we assume that ) atoms are %, and N is the total number of atoms contained in a minute space (number of atoms per minute volume measured), then the statistical distribution of the number of atoms of each element contained in each minute volume can be approximated by a multinomial distribution in the case of a random alloy. In this case, the fluctuation in composition can be evaluated by the standard deviation, which is the spread of the distribution. The standard deviation s for each element i of the compositional distribution of a minute volume is... i The standard deviation of the compositional distribution for each element i in the minute volume to be measured can be expressed by the following equation 1.

number

[0030] The standard deviation of the distribution of each element constituting the alloy within the alloy can be determined by the following method using STEM-EDS analysis. Elemental analysis is performed using line scan with multiple fields of view of a scanning transmission electron microscope. From the multiple fields, it is preferable to select a field containing a large number of particles, where the particles are appropriately distanced from surrounding particles, do not overlap, and have an average particle size. Dispersion and other parameters may be calculated as the average of data from multiple measurement points. Size dependence may also be investigated and used as an average value, but a particle of average size can be used as a representative point. The particle used as the representative point can be selected after determining the average composition at each measurement point from multiple measurement points, and then selecting the particle that most closely matches the composition obtained by elemental analysis using XRF, or the particle that most closely matches the initial composition of each element in the mixed solution obtained by mixing the raw material solutions. The line scan method involves selecting one or more particles in the field of view of a specific measurement point and analyzing them in the direction of the arrow. However, similar results can be obtained by arbitrarily selecting and analyzing one or more other particles, and the same quality results can be obtained even if the direction of the arrow, particle shape, and particle size differ. Therefore, it is considered that similar results can be obtained for any alloy nanoparticle constituting an aggregate. Within a given field of view, the range (position range) for line analysis is adjusted to cover a range longer than the particle size of the alloy (e.g., the shape of nanoparticles). From the viewpoint of confirming uniformity across the entirety of the selected one or more particles, it is preferable that the range for line analysis traverses the entirety of the particles. That is, it is preferable that the two end points of the range for line analysis are not inside the particles, but on the outer circumference of the particles or in locations where no particles exist. It is more preferable that the range for line analysis traverses the longest possible portion of the particles; for example, if traversing the entirety of a single particle, it is more preferable to traverse the long axis of that particle (the line segment containing the two points that represent the longest distance on the outer circumference of the particle). The count is measured for each position with a length approximately equal to the interplanar spacing of atoms or the lattice constant. For example, the measurement point spacing (position spacing) is preferably 0.5 nm or less, more preferably 0.30 nm or less, and particularly preferably 0.25 nm or less. From the perspective of improving accuracy, it is preferable that the integral count of the characteristic X-ray peak be 400 counts or higher. If the count is low, the standard deviation will be overestimated. The count can be increased by increasing the number of measurements or the measurement time when repeatedly scanning a specific area. Background counts vary depending on the measurement. The background count is calculated from the integrated count of the portion of the sample where the element is clearly absent, and the background threshold is determined. Assuming that each element is present in the position portion where the count exceeds the background threshold, the proportion (composition) of each element at each position is determined based on the count. For the composition of the position portion of counts exceeding the background threshold, the mean composition and standard deviation are calculated using the usual arithmetic mean. When determining the standard deviation of the distribution of each element constituting an alloy within the alloy using an elemental map, 2D analysis may be performed. Pixels can be assigned to the STEM data. It is preferable to adjust the measurement point interval in 1D analysis (line analysis) and the pixel size in 2D analysis according to the grain size of the alloy.

[0031] <Correlation coefficient of the distribution> In the present invention, the correlation coefficients of the distributions of the two elements constituting the alloy are preferably less than ±0.50, more preferably within ±0.45, and particularly preferably within ±0.40, from the viewpoint of preventing segregation. The alloy of the present invention preferably has a correlation coefficient of less than ±0.50 for the distribution of at least two elements constituting the alloy, more preferably within ±0.45, and particularly preferably within ±0.40. As the segregation of elemental distribution within an alloy decreases, the correlation coefficients of the distributions of each element change from a state where the elements are close together (positive value close to 1) or mutually exclusive (negative value close to 1) to a state where there is almost no correlation (absolute value close to 0).

[0032] The calculation of the correlation coefficient for composition can be adapted to the analysis of alloys using methods previously employed in geology to evaluate the compositional distribution of minerals (rocks). The correlation coefficient between the distributions of two elements constituting an alloy can be determined by the following method. For details, please refer to Jour. Geol. Soc. Japan (2006) Vol. 112, No.3, pp.173-187, which is incorporated herein by reference. First, a centered log ratio transformation (CLR) is performed on the sample composition vectors at each measurement point, creating a one-to-one coordinate transformation from a composition space restricted to values ​​between 0 and 1 to the real space (this coordinate transformation allows for the application of standard multivariate analysis to the sample data of composition vectors). The variance and covariance are then calculated from the following formulas for the sample vectors of composition after the coordinate transformation, and the correlation coefficient is calculated. Centered logarithmic ratio transformation: clr(vec_x)=(ln x_A / g(x), ln x_B / g(x), ln x_C / g(x)) = (z_A, z_B, z_C) Here, g(x) = (Πx_i) (1 / 3) (i=A,B,C) Multivariate analysis using the transformed vectors is the same as that performed in ordinary real space and can be carried out using known methods. Note that while an inverse transform is not necessary for the correlation coefficient, the statistical value obtained by performing an inverse CLR transform afterward is inversely mapped to the composition space to obtain the calculated value.

[0033] <Shape of alloy> The shape of the alloy of the present invention may be in the form of a bulk, particulate, or aggregate of particles (powder), and is not particularly limited, but is preferably particulate (fine particles), and more preferably alloy nanoparticles. When the alloy of the present invention is in particulate form or aggregate form (powder), each particle is in contact with an interface. Alloy nanoparticles are particles with an average particle size of less than 1000 nm. The alloy nanoparticles can take on various shapes, including spherical, ellipsoidal, tubular, cylindrical, cuboidal, rectangular, and flaky, with spherical or ellipsoidal shapes being preferred. The average particle size of the alloy nanoparticles is preferably 0.5 to 50 nm, more preferably 0.5 to 30 nm, and even more preferably 0.5 to 20 nm. The average particle size of the alloy nanoparticles can be calculated as an arithmetic mean by direct observation, for example, using a transmission electron microscope (TEM). The above average particle size of the alloy nanoparticles is the average particle size of the alloy, and if supported on a carrier, it is the average particle size of the alloy portion other than the carrier. The particle size distribution of the alloy nanoparticles is preferably an average particle size of ±0.1 to 15 nm, more preferably ±0.3 to 15 nm, and particularly preferably ±1.0 to 10 nm.

[0034] The alloy of the present invention may be in the form of an aggregate of alloy nanoparticles, or it may be in the form of being supported on a carrier.

[0035] (An aggregate of alloy nanoparticles) An aggregate of alloy nanoparticles refers to a powder composed of a large number of alloy nanoparticles. For example, it is preferable that the aggregate of alloy nanoparticles substantially does not contain a carrier or the like, or is not supported on a carrier. The aggregate of alloy nanoparticles may contain protective agents such as polymers. Furthermore, the aggregate of alloy nanoparticles may have an oxide coating or the like on the surface of each alloy nanoparticle. The aggregate of alloy nanoparticles may contain impurity particles in addition to the alloy (alloy nanoparticles) of the present invention. However, the aggregate of alloy nanoparticles preferably contains 90% or more of the alloy of the present invention, more preferably 98% or more, particularly preferably 99% or more, and most particularly preferably 100%. The aggregate of alloy nanoparticles may contain alloy nanoparticles in which all three or more elements contained in the compound used in its manufacture are dissolved, as well as alloy nanoparticles in which only some of the three or more elements contained in the compound used in its manufacture are dissolved. However, it is preferable that the proportion of alloy nanoparticles in which the same type of element is dissolved is high. It is preferable that the aggregate of alloy nanoparticles contains 90% or more alloy nanoparticles that contain all three or more elements as constituent elements, more preferably 98% or more, particularly preferably 99% or more, and most preferably 100%. The proportion of each particle in an aggregate of alloy nanoparticles can be determined within the field of view obtained by observing a portion of the aggregate. For example, it is preferable that within a certain field of view obtained by observing a portion of the aggregate of alloy nanoparticles, alloy nanoparticles constituting the aggregate include all five or more constituent elements within that range. However, it is more preferable to determine the proportion of each particle in the aggregate of alloy nanoparticles by averaging across multiple fields of view obtained by observing a portion of the aggregate.

[0036] (carrier) There are no particular restrictions on the carrier. There are no particular restrictions on the type of support material used, but specific examples include oxides, nitrides, carbides, elemental carbon, and elemental metals. Examples of oxides used as carriers include silica, alumina, ceria, titania, zirconia, and niobia oxides, as well as composite oxides such as silica-alumina, titania-zirconia, ceria-zirconia, and strontium titanate. Examples of elemental carbon include activated carbon, carbon black, graphite, carbon nanotubes, and activated carbon fibers. Examples of nitrides include boron nitride, silicon nitride, gallium nitride, indium nitride, aluminum nitride, zirconium nitride, vanadium nitride, tungsten nitride, molybdenum nitride, titanium nitride, and niobium nitride. Carbides include silicon carbide, gallium carbide, indium carbide, aluminum carbide, zirconium carbide, vanadium carbide, tungsten carbide, molybdenum carbide, titanium carbide, niobium carbide, and boron carbide. Examples of elemental metals include pure metals such as iron, copper, and aluminum, as well as alloys such as stainless steel. In the present invention, the carrier is preferably a non-carbon fiber carrier or a non-graphene carrier, more preferably a non-carbon material carrier (a material that is not made of elemental carbon) or a particulate carbon carrier, particularly preferably a non-carbon material carrier from the viewpoint that the carrier does not burn in a high-temperature oxidizing atmosphere, and more particularly preferably an oxide carrier. As a particulate carbon carrier, activated carbon and the like can be used.

[0037] <Protective agent> The solid solution of the present invention may be coated with a protective agent (preferably a surface protective agent). Examples of protective agents include polymers such as polyvinylpyrrolidone (PVP) and polyethylene glycol (PEG), amines such as oleylamine, and carboxylic acids such as oleic acid.

[0038] <Method for manufacturing alloys> In the method for producing the alloy of the present invention, it is preferable to simultaneously reduce the metal ions contained in the mixed solution. There are no particular limitations on the method for simultaneously reducing the metal ions contained in the mixed solution, but the following methods can be given as examples. (1) A method of mixing solutions (raw material solutions) of compounds containing each element that constitutes the alloy after treating them individually with ultrasound. (2) In rapid reactions in a flow reactor, a method for strictly maintaining constant temperature, flow rate, and pressure from the start to the completion of the introduction of the chemical solution (reducing agent solution, raw material solution, or a mixture thereof) into the reaction system. (3) In a spray system, a method for controlling the spray state to be constant. In the alloy manufacturing method of the present invention, solutions of compounds containing each element constituting the alloy (raw material solutions) are individually ultrasonically treated before being mixed. It is preferable to mix the mixed solution with a reducing agent. It is even more preferable to mix the mixed solution with a heated reducing agent that has sufficient reducing power. The following describes preferred embodiments of the alloy manufacturing method.

[0039] (Preparation of raw material solution) The method for manufacturing the alloy preferably includes a step of individually preparing solutions (raw material solutions) of compounds containing each element that constitutes the alloy. Each element that makes up the alloy is dissolved in the solvent. Suitable polar solvents include water, alcohols (methanol, ethanol, isopropanol, etc.), polyols (ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, glycerin, etc.), polyethers (polyethylene glycol, etc.), acetonitrile, acetone, dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone. Among these, water and alcohols are preferred. Nonpolar solvents that can be used include hexane, benzene, toluene, diethyl ether, chloroform, ethyl acetate, and THF. As the raw material solution, it is preferable to use an aqueous solution containing a water-soluble salt of a metal element or a water-soluble salt of a non-metal element. However, in the case of a combination of nonpolar metal salts, a nonpolar solvent containing the nonpolar metal salt may be used. By adjusting the molar ratio of compounds containing each element, the molar ratio of each element in the resulting alloy can be adjusted.

[0040] Examples of water-soluble elemental salts include the following: Known water-soluble salts of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, Cd, Hg, In, Tl, Sn, Pb, Sb, Bi, Mo, W, Tc, Re, 3d metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), Ga, Ge, As, B, Al, C, Si, N, P, Y, Zr, Nb, lanthanides, Hf, and Ta (e.g., sulfates, nitrates, acetates, chlorides, bromides, iodides, potassium cyanate salts, sodium cyanate salts, hydroxides, carbonates, etc.). The following are particularly preferred. Ru: Ruthenium halides such as RuCl3, RuCl3·nH2O, RuBr3, K2RuCl5(NO), ruthenium nitrate, Ru3(CO) 12 , Ru(NO)(NO3) a (OH) b , Ru(acac)3, etc. Rh: Rhodium acetate, rhodium nitrate, rhodium chloride (RhCl3), RhCl3·3H2O, etc. Pd: K2PdCl4, Na2PdCl4, K2PdBr4, Na2PdBr4, palladium nitrate, etc. Os: Osmium halides such as OsCl3 and OsBr3. Ir: Iridium chloride, iridium acetylacetonate (acac; acac systems are preferably dissolved in a nonpolar solvent), potassium iridium cyanate, potassium iridate, H2IrCl6, etc. Pt: K2PtCl4, (NH4)2K2PtCl4, (NH4)2PtCl6, Na2PtCl6, H2PtCl6, Pt(acac)2, etc. Au: AuCl3, HAuCl4, K[AuCl4], Na[AuCl4], K[Au(CN)2], K[Au(CN)4], AuBr3, HAuBr4, etc. Ag: AgNO3, Ag(CH3COO), etc. In: InCl3·4H2O, etc. Sn: Examples include SnCl3·2H2O and Sn(ethyhex)2. Mo: Mo(CO)6, etc. Cu: Cu(NO3)2, CuSO4, Cu(CH3COO)2, CuCO3, CuCl, CuCl2, etc. Fe: FeCl3·6H2O, Fe(NO3)3, etc. B: BH3, etc. N: Ru(NO)(NO3) a (OH) b ammonia, nitrate, hydrazine, etc.

[0041] (Individual ultrasonic treatment) The method for manufacturing the alloy preferably includes a step of ultrasonically treating each solution of the compound containing each element that constitutes the alloy (raw material solution) individually. By ultrasonically treating the raw material solutions individually, an alloy with significantly higher solid solution uniformity can be obtained compared to when a solution containing all the elements that constitute the alloy is ultrasonically treated together. Ultrasonic treatment is preferably performed while shielding from light, from the viewpoint of suppressing the photo-induced reduction of compounds containing each element. Furthermore, ultrasonic treatment is preferably performed at low temperatures, such as in an ice bath, from the viewpoint of suppressing the thermal reduction of metal salts. The effects of individual ultrasonic treatment, as well as the effects of light shielding and temperature during ultrasonic treatment, may vary depending on the types of elements constituting the alloy and the types of raw material solutions. Therefore, the degree to which the uniformity of solid solution is improved by these processes may differ depending on the types of elements constituting the alloy and the types of raw material solutions. However, if there is a method that can uniformly prepare individual raw material solutions at a speed equivalent to that of individual ultrasonic treatment, as an alternative to the process of individually ultrasonically treating the raw material solutions, that method may be used.

[0042] (Preparation of reducing agent) In the method for manufacturing the alloy, it is preferable to include a step of preparing a reducing agent. The reducing agent is preferably a liquid reducing agent. Examples of liquid reducing agents include polyhydric alcohols such as ethylene glycol, glycerin, diethylene glycol, and triethylene glycol; lower alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol under high pressure; aqueous alcohols such as aqueous ethanol under high pressure; THF solution of BH3 (THF complex); or hydrazine, NaBH4 solution, or sodium naphthalenide solution. In addition, each element constituting the alloy may be used as a reducing agent. For example, an alloy containing element B may be formed using a THF solution of BH3 (THF complex) as a reducing agent. When mixing and heating under pressure using the flow apparatus described later, a low-boiling-point reducing agent can be preferably used. The boiling point of a preferred reducing agent, a lower alcohol, is approximately 130°C from room temperature, more preferably 40-120°C, and even more preferably 60-100°C. Because these reducing agents have low boiling points under normal pressure, they are less likely to reduce compounds containing each element constituting the alloy (such as metal compounds) and form alloys composed of metals that do not form solid solutions in the phase equilibrium phase diagram. By reacting them at high temperatures under pressure, they can acquire reducing properties and function as reducing agents for obtaining alloys composed of metals that do not form solid solutions in the phase equilibrium phase diagram. The reducing agent is used in an amount of 1 equivalent or more, preferably in excess, for the reduction of compounds (preferably water-soluble salts) containing each element that constitutes the alloy.

[0043] (mixture) In the method for manufacturing the alloy, it is preferable to include a step of mixing individually ultrasonically treated raw material solutions to form a mixed solution. It is preferable to mix the reducing agent into the raw material solution before or during heating of the mixed solution. In the method for producing the alloy, it is preferable to include a step of heating the mixed solution to trigger a reaction. The reaction time during heating can range from approximately 1 minute to 12 hours. Heating is preferably carried out under stirring. The reaction temperature during heating is preferably around 170 to 300°C, more preferably around 180 to 250°C. Furthermore, when using a reducing agent such as NaBH4, it may be used at room temperature or after cooling.

[0044] There are no particular restrictions on the method of mixing or heating; for example, the reducing agent and one or both of the mixed solutions may be heated before mixing. Furthermore, the method for manufacturing the alloy preferably includes a step of heating the reducing agent, and it is preferable to mix the raw material solution with the reduced agent heated in this step and allow the heating reaction to occur. For example, the reducing agent may be heated and then the mixed solution may be added dropwise using a pump (syringe pump) or sprayed using a spray device. Alternatively, a flow reactor may be used to mix and heat the raw material solutions and reducing agent solutions, which have been subjected to three or more separate ultrasonic treatments, into a reaction vessel and then heat them under pressure. When pressurized using a flow apparatus, the pressures of the raw material solution and the reducing agent solution are approximately 0.1 to 10 MPa, preferably 0.2 to 9 MPa. The pressure inside the reaction vessel is also approximately 0.1 to 10 MPa, preferably 0.2 to 9 MPa. The temperature of the reaction vessel (reaction temperature) when pressurized is approximately 100 to 500°C, preferably 150 to 400°C, more preferably 180 to 300°C.

[0045] (Alloy separation) In the method for producing the alloy, it is preferable to include a step of separating the precipitate from the solution after the heating reaction. This process makes it possible to obtain an alloy containing three or more metals in a solid solution state. Methods for separating the precipitate include vacuum drying, centrifugation, filtration, sedimentation, reprecipitation, and separation using a powder separator (cyclone). Before separating the precipitate, it is preferable to allow the reaction solution to cool or rapidly cool.

[0046] By adding a protective agent to a mixed solution, a reducing agent, or a reaction solution containing these, particles (preferably alloy nanoparticles) with suppressed aggregation can be obtained. When a protective agent is used, it is included in the reaction solution, which is obtained by mixing the mixed raw material solution and the reducing agent, at a concentration preferably 0.01 to 100 times, more preferably 0.5 to 50 times, and even more preferably 1 to 10 times the total amount of the metal compound by mass ratio. The protective agent may be included in the raw material solution, in the reducing agent, or in both the raw material solution and the reducing agent.

[0047] Furthermore, by coexisting a support in a mixed solution, a reducing agent, or a reaction solution containing a mixture thereof, a supported catalyst in which an alloy is supported on the support can be obtained. By coexisting a support in the reaction solution, a supported catalyst can be obtained in which a multi-component solid solution is supported on the support. When the multi-component solid solution is in the form of fine particles, a supported catalyst can be obtained in which aggregation of the fine particles is suppressed by adding a protective agent simultaneously with the support in the reaction solution for producing the multi-component solid solution fine particles.

[0048] On the other hand, neither a protective agent nor a support is added to the mixed solution, reducing agent, or reaction solution containing a mixture thereof. This makes it possible to obtain an alloy, which is an aggregate of alloy nanoparticles. In this case, a supported catalyst can be obtained by mixing the alloy, which is an aggregate of alloy nanoparticles, and the support in a solution or as powders in a non-solvent or solvent system, and then molding the mixture. If a solvent is used, it may be filtered and dried as needed.

[0049] [catalyst] The alloy of the present invention can be used as a catalyst exhibiting excellent performance. There are no particular restrictions on the form of the alloy when used as a catalyst. It can also be used as a supported catalyst mounted on a carrier.

[0050] There are no particular limitations on the catalytic reactions in which the alloy of the present invention exhibits excellent catalytic performance, but examples include reactions generally known to use catalysts containing platinum group elements. Specifically, these include chemical reactions such as reduction reactions including hydrogenation, dehydrogenation reactions, oxidation reactions including combustion, and coupling reactions. Furthermore, by utilizing these catalytic properties, it can be suitably used in various processes and equipment. There are no particular limitations on the applications in which it can be suitably used, but examples include catalysts for hydrogen evolution reactions (HER), hydrogenation reactions, hydrogen oxidation reactions, oxygen reduction reactions (ORR), oxygen evolution reactions (OER), nitrogen oxide (NOx) reduction reactions, carbon monoxide (CO) oxidation reactions, dehydrogenation reactions, VVOC or VOC oxidation reactions, exhaust gas purification catalysts, water electrolysis reactions, and hydrogen fuel cells. [Examples]

[0051] The present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, proportions, processing content, and processing procedures shown in the following examples can be modified as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following specific examples.

[0052] [Device] In the examples, the following apparatus was used. Unless otherwise specified, the PXRD used was the Rigaku Miniflex600 (Cu Kα). (i-1)Powder X-ray Diffraction (PXRD) Rigaku Miniflex600 (Cu Kα) (i-2)PXRD SPring-8 BL02B2(λ=0.63Å, 0.58Å) (i-3)PXRD SPring-8 BL04B2 (ii) Energy-dispersive X-ray spectroscopy in scanning transmission electron microscopy (STEM-EDS) and EELS JEOL JEM-ARM200CF (accelerating voltage: 120 kV) (iii) X-ray fluorescence analysis (XRF) X-ray fluorescence spectrometer ZSX Primus IV

[0053] [Example 1]: AuRuIr <Individual ultrasonication of metal ion solutions> A metal ion solution was prepared by dissolving HAuBr₄ in diethylene glycol (DEG), and ultrasonicated for 5 minutes in a light-shielded state. Unless otherwise specified, ultrasonication was performed at low temperature with ice cooling. A metal ion solution was prepared by dissolving K₂RuCl₅(NO) in diethylene glycol (DEG), and ultrasonicated for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving H₂IrCl₆ in diethylene glycol (DEG), and ultrasonicated for 5 minutes. The three types of metal ion solutions individually ultrasonicated were mixed at a ratio of 1:1:1, and each mixed solution containing 0.15 mmol of metal ions in DEG was dissolved and combined to a total volume of approximately 3 ml, then adjusted to 10 ml.

[0054] <Preparation of alloy> 100 ml of ethylene glycol (EG) containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Corporation) was heated and stirred at 195 °C. To this solution, the mixed metal ion solution was added dropwise at a rate of 1.5 ml / min using a syringe pump, and the mixture was maintained at 195 °C for 10 minutes. Thereafter, it was allowed to cool to room temperature. The resulting precipitate, i.e., nanoparticles, was separated by centrifugation.

[0055] <Elemental analysis by STEM-EDS> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was conducted using line scans with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of three elements was calculated. The line analysis methods in each of the following examples and comparative examples are based on actual data obtained by selecting one or more particles in the field of view of a specific measurement point and analyzing them in the direction of the arrow. However, almost the same results were obtained even when one or more other particles were arbitrarily selected and analyzed, and the same quality was obtained even when the direction of the arrow, particle shape, and particle size differed. Therefore, it is considered that almost the same results can be obtained for any alloy nanoparticle constituting the aggregate. At the measurement points in Figure 1, elemental analysis was performed at 100 points from the 0.00 nm position to the 25.90 nm position, with intervals of 0.15 to 0.30 nm, for the area indicated by the arrow. The background threshold was set to 30 counts. Nanoparticles were counted from the 4.67 nm position to the 17.70 nm position, and the length of the nanoparticles in this area indicated by the arrow was approximately 13.03 nm. Graphs of the characteristic X-ray counts and composition for each position in the area indicated by the arrow in Figure 1 are shown in Figures 2(A) and 2(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated at the measurement points shown in Figure 1 and are listed in Table 2 below. The average composition was calculated using the usual arithmetic mean. The standard deviation was calculated using the usual arithmetic mean. The correlation coefficient was obtained using a centered log ratio transformation (CLR). The CLR transformation was based on Jour. Geol. Soc. Japan (2006) Vol. 112, No.3, pp. 173-187. Specifically, the EDX line analysis data was converted to compositional data using the EDX measurement software Noran system 7 (Thermo Fisher Scientific), and the correlation coefficient was calculated using the statistical calculation software R and the R library package Compositions. Compositions is a library for the statistical analysis of compositional data (see “Analyzing Compositional Data with R”, van den Boogaart, K. Gerald, Tolosana-Delgado, Raimon, Softcover ISBN:978-3-642-36808-0, published by Springer).

[0056] [Table 2]

[0057] At the measurement points in Figure 3, elemental analysis of the nanoparticles obtained in Example 1 was performed at intervals of 0.15 to 0.30 nm in the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition at each position in the areas indicated by the arrows in Figure 2 are shown in Figures 3(A) and 3(B), respectively. The average composition and the standard deviation of the distribution of each element constituting the alloy within the alloy were calculated and are shown in Table 3 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0058] [Table 3]

[0059] At the measurement points in FIG. 5, elemental analysis of the nanoparticles obtained in Example 1 was performed at intervals of 0.15 to 0.30 nm along the arrowed portion. The background threshold was set to 30 counts. Graphs of the characteristic X-ray count numbers and compositions at each position in the arrowed portion of FIG. 5 are shown in FIG. 6(A) and FIG. 6(B), respectively. The average composition and the standard deviation of the distribution of each element constituting the alloy within the alloy were determined and listed in Table 4 below. The average composition, standard deviation, and correlation coefficient were determined in the same manner as in Example 1.

[0060] [Table 4]

[0061] From Tables 2 to 4, it was found that the alloy of the present invention has high uniformity of solid solution in the shape of the nanoparticles.

[0062] In addition, HAADF-STEM images and EDS maps of a part of all the obtained alloys are shown in FIG. 7. As shown in FIG. 7, as far as observed in the STEM image, it was confirmed that all elements were dissolved in each nanoparticle. That is, within the range of the field of view confirmed in this example, the aggregate of alloy nanoparticles contained 100% by number of alloy nanoparticles in which all of the three types of elements contained in the compounds used for production as constituent elements were in solid solution. Further, it can be seen that in the alloy of the present invention, any alloy nanoparticles constituting the aggregate contain all of the three types of elements contained in the compounds used for production as constituent elements.

[0063] <XRD analysis> The obtained AuRuIr nanoparticles were subjected to XRD analysis using SPring-8 BL02B2. The obtained results are shown in FIG. 8.

[0064] <Analysis by TEM> A TEM photograph of the obtained AuRuIr nanoparticles is shown in FIG. 9. From FIG. 9, the average particle size of the obtained nanoparticles was 8.9±1.7 nm.

[0065] <Production of electrode> An electrode catalyst (alloy / C: 20 wt% metal content) was fabricated by supporting the obtained AuRuIr nanoparticles on carbon particles. The nanoparticles were 0.05 mg in size. Synthesized alloy nanoparticles were mixed in water at a ratio of 20 wt% to carbon particles (Vulcan-XC-72R), supported on the carbon by ultrasonic dispersion, recovered by centrifugation, and dried to produce a catalyst powder. 2.5 mg of this catalyst powder was dispersed in a mixed solution of 6.55 ml of isopropanol and 3.44 ml of water, and 0.01 ml of 5 wt% Nafion® solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and thoroughly mixed to prepare a catalyst ink. A catalyst electrode was fabricated by applying an appropriate amount of this ink to a working electrode such as a rotating ring disk electrode or a glassy carbon electrode.

[0066] <Catalytic activity> Current measuring device: Potentiostat (BAS ALS760E) Measurement method: Using a rotating ring disk electrode on which the obtained AuRuIr nanoparticles were supported on carbon particles as the cathode, the current I was measured when the potential E was swept from 0.1V to -0.4V (vs. RHE) at 5mV / s in a three-electrode cell (counter electrode: platinum wire, reference electrode: silver-silver chloride electrode (Ag / AgCl), electrolyte: 0.1M HClO4 aqueous solution, 25℃, oxygen saturated) to evaluate the HER catalytic activity three times. The results are shown in Figures 10(A) and 10(B).

number

[0067] [Example 11]: RuRhAu <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving HAuBr4 in diethylene glycol DEG, and the solution was sonicated for 5 minutes while protected from light. A metal ion solution was prepared by dissolving K2RuCl5(NO) in diethylene glycol DEG, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving RhCl3 in diethylene glycol DEG, and the solution was sonicated for 5 minutes. Three different metal ion solutions, each individually ultrasonically treated, were mixed in a 1:1:1 ratio. Approximately 3 ml of each metal ion mixture in 0.15 mmol DEG solution was then dissolved in the mixture to prepare a total volume of 10 ml.

[0068] <Preparation of alloys> 100 ml of ethylene glycol (EG) containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was heated and stirred at 195°C. To this solution, a mixed metal ion solution was added dropwise using a syringe pump at a rate of 1.5 ml / min, and the mixture was maintained at 195°C for 10 minutes. Afterward, it was allowed to cool to room temperature. The resulting precipitate, consisting of nanoparticles, was separated by centrifugation.

[0069] <Elemental analysis> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was conducted using line scans with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of three elements was calculated. At the measurement points in Figure 11, elemental analysis was performed at 120 points from the 0.00 nm position to the 19.20 nm position, with intervals of 0.10 to 0.20 nm, for the area indicated by the arrow. The background threshold was set to 35 counts. Nanoparticles were counted from the 3.86 nm position to the 13.40 nm position, and the length of the nanoparticles in this area indicated by the arrow was approximately 9.54 nm. Graphs of the count and composition at each position in the area indicated by the arrow in Figure 11 are shown in Figures 12(A) and 12(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were determined at the measurement points shown in Figure 11, in the same manner as in Example 1, and are listed in Table 5 below.

[0070] [Table 5]

[0071] At the measurement points in Figure 13, elemental analysis of the nanoparticles obtained in Example 11 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 13 are shown in Figures 14(A) and 14(B), respectively. The average composition and the standard deviation of the distribution of each element constituting the alloy within the alloy were calculated and are shown in Table 6 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0072] [Table 6]

[0073] At the measurement points in Figure 15, elemental analysis of the nanoparticles obtained in Example 11 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 15 are shown in Figures 16(A) and 16(B), respectively. The average composition and the standard deviation of the distribution of each element constituting the alloy within the alloy were calculated and are shown in Table 7 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0074] [Table 7]

[0075] At the measurement points in Figure 17, elemental analysis of the nanoparticles obtained in Example 11 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 17 are shown in Figures 18(A) and 18(B), respectively. The average composition and the standard deviation of the distribution of each element constituting the alloy within the alloy were calculated and are shown in Table 8 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0076] [Table 8]

[0077] From Tables 5 to 8, it was found that the alloy of the present invention has high uniformity of solid solution in the shape of nanoparticles.

[0078] In addition, HAADF-STEM images and EDS maps of a part of all the obtained alloys are shown in FIG. 19. From FIG. 19, it was confirmed that all elements were dissolved in each nanoparticle as far as observed in the STEM image. That is, within the range of the field of view confirmed in this example, it can be seen that the aggregate of alloy nanoparticles contains 100 number% of alloy nanoparticles in which all three types of elements contained in the compound used for production as constituent elements are solid-dissolved. In addition, it can be seen that in the alloy of the present invention, any alloy nanoparticles constituting the aggregate contain all three types of elements contained in the compound used for production as constituent elements.

[0079] <XRD analysis> The obtained RuRhAu nanoparticles were subjected to XRD analysis using SPring-8 BL02B2. The obtained results are shown in FIG. 20.

[0080] <Elemental analysis by TEM and XRF> A TEM photograph of the obtained RuRhAu nanoparticles is shown in FIG. 21. From FIG. 21, the average particle size of the obtained nanoparticles was 11.1±2.5 nm. Elemental analysis was performed by XRF. As a result, Ru:Rh:Au=35.1 atomic%:34.3 atomic%:30.6 atomic%.

[0081] <Catalytic activity> An electrode catalyst (alloy / C: metal content 20 wt%) in which the obtained RuRhAu nanoparticles were supported on carbon particles was produced. The amount of nanoparticles was 0.05 mg. An electrode was manufactured in the same manner as in Example 1. Current measuring device: Potentiostat (ALS760E manufactured by BAS) Measurement method: The obtained RuRhAu nanoparticles were supported on carbon particles to form a rotating ring disk electrode, which was used as the cathode. Using a three-electrode cell (counter electrode: platinum wire, reference electrode: silver-silver chloride electrode (Ag / AgCl), electrolyte: 0.1 M HClO4 aqueous solution, 25°C, oxygen saturated), the current I was measured when the potential E was swept from 0.1 V to -0.4 V (vs. RHE) at 5 mV / s, and the HER catalytic activity was evaluated. The results are shown in Figures 22(A) and 22(B).

[0082] [Example 21]: fcc-PtIrRu <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving K2RuCl5(NO) in deionized water, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving H2PtCl6 in deionized water and subjected to sonication for 5 minutes. A metal ion solution was prepared by dissolving H2IrCl6 in deionized water and subjected to sonication for 5 minutes. Three different metal ion solutions, each individually ultrasonically treated, were mixed in a ratio of H2PtCl6:K2RuCl5(NO):H2IrCl6 = 1.5:7:1.5. Each of these metal ion mixtures was then dissolved in a 0.2 mmol aqueous solution to prepare a total volume of 20 ml.

[0083] <Preparation of alloys> 100 ml of ethylene glycol (EG) containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was heated and stirred at 190°C. A mixed metal ion solution was added to this solution by spraying, and the mixture was maintained at 190°C for 10 minutes. It was then allowed to cool to room temperature. The resulting precipitate, consisting of nanoparticles, was separated by centrifugation to prepare the alloy of Example 21, which consisted of nanoparticles.

[0084] [Example 22]: hcp-PtIrRu <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving K2RuCl5(NO) in diethylene glycol (DEG), and was ultrasonicated for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving Pt(acac)2 in diethylene glycol (DEG), and was ultrasonicated for 5 minutes. A metal ion solution was prepared by dissolving H2IrCl6 in diethylene glycol (DEG), and was ultrasonicated for 5 minutes. The three types of metal ion solutions individually ultrasonicated were mixed at a ratio of Pt(acac)2:K2RuCl5(NO):H2IrCl6=1.5:7:1.5 to prepare a metal ion mixed solution of 0.2 mmol diethylene glycol (DEG) solution (10 ml).

[0085] <Preparation of alloy> 100 ml of ethylene glycol (EG) containing polyvinylpyrrolidone (PVP) K30 (0.6 mmol; manufactured by Fujifilm Wako Pure Chemical Corporation) was heated and stirred at 180°C. To this solution, the metal ion mixed solution was fed (dropped) at a rate of 3.0 ml / min using a syringe pump, and then rapidly cooled to room temperature. The resulting nanoparticles, which are precipitates, were separated by centrifugation to prepare the alloy of Example 22 as nanoparticles.

[0086] <Elemental analysis by STEM-EDS> STEM-EDS analysis of the separated alloys of Example 21 and Example 22 is performed in the same manner as in Example 1. First, the alloy (fcc-PtIrRu) nanoparticles obtained in Example 21 were subjected to elemental analysis by line scan using multiple fields of view of a scanning transmission electron microscope, and the metal compositions of the three elements were calculated. At the measurement points in Figure 23, elemental analysis of the nanoparticles obtained in Example 21 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 23 are shown in Figures 24(A) and 24(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 9 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0087] [Table 9]

[0088] At the measurement points in Figure 25, elemental analysis of the nanoparticles obtained in Example 21 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 25 are shown in Figures 26(A) and 26(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 10 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0089] [Table 10]

[0090] At the measurement points in Figure 27, elemental analysis of the nanoparticles obtained in Example 21 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 27 are shown in Figures 28(A) and 28(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 11 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0091] [Table 11]

[0092] Tables 9-11 show that the alloy of the present invention, which is the alloy (fcc-PtIrRu) nanoparticle obtained in Example 21, exhibits high uniformity of solid solution in the shape of the nanoparticles.

[0093] Next, elemental analysis of the alloy (hcp-PtIrRu) nanoparticles obtained in Example 22 was performed using line scan with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of three elements was calculated. At the measurement points in Figure 29, elemental analysis of the nanoparticles obtained in Example 22 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 29 are shown in Figures 30(A) and 30(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 12 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0094] [Table 12]

[0095] At the measurement points in Figure 31, elemental analysis of the nanoparticles obtained in Example 22 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 31 are shown in Figures 32(A) and 32(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 13 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0096] [Table 13]

[0097] From Tables 12 and 13, it can be seen that the alloy of the present invention, which is the (Hcp-PtIrRu) alloy nanoparticles obtained in Example 22, has high uniformity of solid solution in the shape of the nanoparticles.

[0098] In addition, HAADF-STEM images and EDS maps of some of all the alloys (fcc-PtIrRu) obtained in Example 21 are shown in FIG. 33. HAADF-STEM images and EDS maps of some of all the alloys (hcp-PtIrRu) obtained in Example 22 are shown in FIG. 34. From FIGS. 33 and 34, as far as observed in the STEM image, it was confirmed that all elements were dissolved in each nanoparticle. That is, within the range of the field of view confirmed in this example, the aggregate of alloy nanoparticles contains 100% by number of alloy nanoparticles in which all three types of elements contained in the compound used for production as constituent elements are in solid solution. In addition, in the alloy of the present invention, it can be seen that any alloy nanoparticles constituting the aggregate contain all three types of elements contained in the compound used for production as constituent elements.

[0099] <XRD analysis> XRD analysis was performed on the obtained alloy of Example 21 and alloy of Example 22. The obtained results are shown in FIG. 35.

[0100] <Elemental analysis by TEM and XRF> A TEM photograph of the obtained nanoparticles of the alloy (fcc-PtIrRu) of Example 21 is shown in FIG. 36(A). From FIG. 36(A), the average particle size of the obtained nanoparticles was 3.5±0.56 nm. A TEM photograph of the nanoparticles of the alloy (hcp-PtIrRu) of Example 22 is shown in FIG. 36(B). From FIG. 36(B), the average particle size of the obtained nanoparticles was 3.0±0.34 nm. Elemental analysis was performed using XRF. As a result, the alloy of Example 21 (fcc-PtIrRu) had Pt:Ru:Ir = 14.3 atoms:71.4 atoms:14.35 atoms. The alloy of Example 22 (fcc-PtIrRu) had Pt:Ru:Ir = 14.7 atoms:70.1 atoms:15.2 atoms.

[0101] <Catalytic activity> An electrode catalyst (alloy / C: 20 wt% metal content) was prepared by supporting nanoparticles of the alloy (fcc-PtIrRu) obtained in Example 21 or the alloy (hcp-PtIrRu) obtained in Example 22 onto carbon particles. The amount of nanoparticles used was 10 μg. Current measuring device: Potentiostat (BAS ALS760E) Measurement method: The obtained AuRuIr nanoparticles were supported on carbon particles to form a rotating ring disk electrode, which was used as the cathode. Using a three-electrode cell (counter electrode: platinum wire, reference electrode: silver-silver chloride electrode (Ag / AgCl), electrolyte: 1M KOH aqueous solution, 25°C, oxygen saturated), the current value I was measured when the potential E was swept from 0.00V to -0.15V (vs. RHE) at an LSV of 5mV / s, and the HER catalytic activity was evaluated. The results are shown in Figure 37.

number

[0102] As shown in Figure 37, the alloy from Example 22 (hcp-PtIrRu) showed better catalytic activity than the alloy from Example 22 (fcc-PtIrRu) and the commercially available Pt / C catalyst (Alpha Acer).

[0103] [Example 31]: PdRuB (1) Preparation of PdRu nanoparticles <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving K2PdCl4 in deionized water, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving K2RuCl5(NO) in deionized water, and then subjected to sonication for 5 minutes while shielded from light. Two types of metal ion solutions that had been individually subjected to ultrasonic treatment were mixed at a K2PdCl4:K2RuCl5(NO) ratio of 1:1 to prepare a metal ion mixed solution consisting of an aqueous solution (35 ml) containing 0.7 mmol of Pd and 0.85 mmol of Ru.

[0104] <Preparation of Alloy> A triethylene glycol solution (150 ml) containing polyvinylpyrrolidone (PVP) K30 (0.6 mmol; manufactured by Fujifilm Wako Pure Chemical Corporation) was heated and stirred at 200°C. The metal ion mixed solution was added to this solution by spraying, and then the mixture was rapidly cooled to room temperature. The resulting precipitate, which consisted of nanoparticles, was separated by centrifugation to prepare PdRu nanoparticles.

[0105] (2) Preparation of PdRuB Nanoparticles Using the obtained PdRu nanoparticles as a raw material, degassing was performed using a vacuum pump at 80°C overnight. Thereafter, the inside of the system was purged with nitrogen gas. A 1M solution of BH3 in THF (manufactured by Sigma-Aldrich) was added and mixed in an excess amount relative to the PdRu nanoparticles, and the mixture was heated and stirred at 80°C for 2 days under a nitrogen atmosphere. The resulting precipitate, which consisted of nanoparticles, was separated by centrifugation to prepare PdRuB nanoparticles.

[0106] <Elemental Analysis by STEM-EDS> STEM-EDS analysis of the separated PdRuB nanoparticles is performed in the same manner as in Example 1. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of the two elements constituting the alloy are determined. It can be seen that the alloy of the present invention has high uniformity of solid solution in the shape of the nanoparticles.

[0107] In addition, a portion of the HAADF-STEM images and EDS maps of all the obtained PdRuB nanoparticles are shown in Figure 38, and the HAADF-STEM images and EELS maps are shown in Figure 39, respectively. From Figures 38 and 39, as far as observed in the STEM images, it was confirmed that all elements were solid-dissolved in each nanoparticle. That is, within the range of the field of view confirmed in this example, it can be seen that the aggregate of alloy nanoparticles contains 100% by number of alloy nanoparticles in which all three types of elements contained in the compounds used for production as constituent elements are solid-dissolved. Furthermore, it can be seen that in the alloy of the present invention, any alloy nanoparticles constituting the aggregate contain all three types of elements contained in the compounds used for production as constituent elements.

[0108] <XRD analysis> The obtained PdRuB nanoparticle alloy was subjected to XRD analysis using SPring-8 BL04B2. The obtained results are shown in Figure 40.

[0109] <Elemental analysis by TEM and XRF> A TEM image of the obtained PdRuB nanoparticles is shown in Figure 41(A). From Figure 41(A), the average particle size of the obtained nanoparticles was 12.9±1.9 nm. A TEM image of the intermediate product PdRu nanoparticles is shown in Figure 41(B). From Figure 41(B), the average particle size of the obtained nanoparticles was 12.9±1.8 nm. Elemental analysis was performed by XRF. As a result, the composition of the intermediate product PdRu nanoparticles was Pd:Ru=48 atomic%:52 atomic%.

[0110] [Example 41]: AuPdRu <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving HAuCl4·3H2O in ion-exchanged water, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving K2PdCl4 in ion-exchanged water, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving RuCl3·nH2O in deionized water, and then subjected to sonication for 5 minutes while shielded from light. Three different metal ion solutions, each individually ultrasonically treated, were mixed in a 1:1:1 ratio. Each of these metal ion mixtures was then dissolved in approximately 13.3 ml of 0.35 mmol aqueous solution to prepare a total volume of 40 ml.

[0111] <Preparation of alloys> 300 ml of triethylene glycol (TEG) containing polyvinylpyrrolidone (PVP) K30 (10 mmol; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was heated and stirred at 225°C. To this solution, a mixed metal ion solution was added by spray at a rate that did not cause the TEG solution temperature to drop below 220°C, and the mixture was maintained at 225°C for 10 minutes. Afterward, it was allowed to cool to room temperature. The resulting precipitate, consisting of nanoparticles, was separated by centrifugation.

[0112] <Elemental analysis> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was performed using line scan with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of three elements was calculated. The uniformity of the solid solution is improved… At the measurement points in Figure 42, elemental analysis of the nanoparticles obtained in Example 41 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 42 are shown in Figures 43(A) and 43(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient of the distribution of two elements constituting the alloy were calculated and are listed in Table 14 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0113] [Table 14]

[0114] Table 14 shows that the alloy of the present invention exhibits high uniformity of solid solution in the shape of nanoparticles.

[0115] [Comparative example 42]:AuPdRu <Preparation of alloys> A metal ion solution was prepared by dissolving HAuCl4·3H2O in deionized water. A metal ion solution was prepared by dissolving K2PdCl4 in deionized water. A metal ion solution was prepared by dissolving RuCl3·nH2O in deionized water. Three metal ion solutions that have not undergone individual ultrasonic treatment are mixed in a 1:1:1 ratio. A 0.35 mmol aqueous solution of each metal ion mixture was dissolved in approximately 13.3 ml of each solution to prepare a total volume of 40 ml.

[0116] 300 ml of triethylene glycol (TEG) containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was heated and stirred at 225°C. To this solution, a mixed metal ion solution was added by spray at a rate that did not cause the TEG solution temperature to drop below 220°C, and the mixture was maintained at 225°C for 10 minutes. Afterward, it was allowed to cool to room temperature. The resulting precipitate, consisting of nanoparticles, was separated by centrifugation.

[0117] <Elemental analysis> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was conducted using line scans with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of three elements was calculated. At the measurement points in Figure 44, elemental analysis of the nanoparticles obtained in Comparative Example 42 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 44 are shown in Figures 45(A) and 45(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 15 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0118] [Table 15]

[0119] At the measurement points in Figure 46, elemental analysis of the nanoparticles obtained in Comparative Example 42 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position in the areas indicated by the arrows in Figure 46 are shown in Figures 47(A) and 47(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are listed in Table 16 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0120] [Table 16]

[0121] Tables 15 and 16 show that in Comparative Example 42, the standard deviation of the distribution of each element (Ru) constituting the alloy within the alloy was 19% to 23%, exceeding 15%, indicating low uniformity of solid solution in the nanoparticle shape.

[0122] [Example 51]:RuRhPdOsIrPt <Individual ultrasonic treatment of metal ion solutions> A metal ion solution was prepared by dissolving K2PdCl4 in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving RuCl3·nH2O in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving RhCl3·3H2O in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving OsCl3·3H2O in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving IrCl4·xH2O in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. A metal ion solution was prepared by dissolving K2[PtCl4] in an ion-exchange aqueous solution, and then subjected to sonication for 5 minutes while shielded from light. Six different metal ion solutions, each individually ultrasonically treated, were mixed in a 1:1:1:1:1:1 ratio. Each of these metal ion mixtures was then dissolved in approximately 1.5 ml of 0.167 mmol TEG solution to prepare a total volume of 10 ml.

[0123] <Preparation of alloys> 100 ml of triethylene glycol TEG containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was heated and stirred at 230°C. To this solution, a metal ion mixture was added dropwise using a syringe pump at a rate of 1.5 ml / min, and the mixture was maintained at 230°C for 10 minutes. Afterward, it was allowed to cool to room temperature. The resulting precipitate, consisting of nanoparticles, was separated by centrifugation.

[0124] <Elemental analysis> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was conducted using line scans with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of six elements was calculated. At the measurement points in Figure 48, elemental analysis of the nanoparticles obtained in Example 51 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position at the areas indicated by the arrows in Figure 48 are shown in Figures 49(A) and 49(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are shown in Tables 17 and 18 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0125] [Table 17]

[0126] [Table 18]

[0127] From Tables 17 and 18, it was found that the alloy of the present invention has high uniformity of solid solution in the form of nanoparticles.

[0128] [Example 61]: PdRuIrPtRh <Individual Ultrasonic Treatment of Metal Ion Solutions> A metal ion solution was prepared by dissolving K2PdCl4 in an ion-exchanged aqueous solution, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving RuCl3·nH2O in an ion-exchanged aqueous solution, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving RhCl3·3H2O in an ion-exchanged aqueous solution, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving IrCl4·xH2O in an ion-exchanged aqueous solution, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. A metal ion solution was prepared by dissolving K2[PtCl4] in an ion-exchanged aqueous solution, and subjected to ultrasonic treatment for 5 minutes in a light-shielded state. Five types of metal ion solutions individually subjected to ultrasonic treatment were mixed at a ratio of 1:1:1:1:1, and 0.200 mmol of each metal ion mixed solution was dissolved in approximately 2.0 ml of TEG solution, and adjusted to a total volume of 10 ml.

[0129] <Preparation of Alloy> 100 ml of triethylene glycol (TEG) containing polyvinylpyrrolidone (PVP) K30 (4 mmol; manufactured by Fujifilm Wako Pure Chemical Corporation) was heated and stirred at 230°C. To this solution, the metal ion mixed solution was added dropwise at a rate of 1.5 ml / min using a syringe pump, and the mixture was maintained at 230°C for 10 minutes. Thereafter, the mixture was allowed to cool to room temperature. The resulting precipitate, which was nanoparticles, was separated by centrifugation.

[0130] <Elemental Analysis> STEM-EDS analysis was performed on the separated nanoparticles. Elemental analysis was conducted using line scans with multiple fields of view of a scanning transmission electron microscope, and the metallic composition of five elements was calculated. At the measurement points in Figure 50, elemental analysis of the nanoparticles obtained in Example 61 was performed at intervals of 0.15 to 0.30 nm for the areas indicated by the arrows. The background threshold was set to 30 counts. Graphs of the characteristic X-ray counts and composition for each position at the areas indicated by the arrows in Figure 50 are shown in Figures 51(A) and 51(B), respectively. The average composition, the standard deviation of the distribution of each element constituting the alloy within the alloy, and the correlation coefficient between the distributions of two elements constituting the alloy were calculated and are shown in Tables 19 and 20 below. The average composition, standard deviation, and correlation coefficient were calculated in the same manner as in Example 1.

[0131] [Table 19]

[0132] [Table 20]

[0133] Tables 19 and 20 show that the alloy of the present invention exhibits high uniformity of solid solution in the shape of nanoparticles.

Claims

1. Alloy nanoparticles composed of three or more elements, In elemental analysis by line analysis using Energy-dispersive x-ray spectrum analysis in scanning transmission electron microscopy (STEM-EDS), the standard deviation of the distribution of each element constituting the alloy nanoparticle within the alloy nanoparticle, determined from elemental analysis by line analysis where the line analysis range is defined as being on a line crossing the alloy nanoparticle and the outer circumference of the particle or a location where no particle exists, is 15 atomic percent or less for all of them. The elements constituting the alloy nanoparticles include at least three from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt), Ag, Au, Cd, Hg, In, Tl, Sn, Pb, Sb, Bi, Mo, W, Tc, Re, 3d metals (Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn), Ga, Ge, As, Zr, Nb, and Ta. The elements constituting the alloy nanoparticles include at least one from the group consisting of platinum group metals (Ru, Rh, Pd, Os, Ir, Pt) and Au. The particle size is 0.5 to 50 nm. Alloy nanoparticles.

2. The alloy nanoparticle according to claim 1, wherein the lower limit of the proportion of the smallest element when the total alloy nanoparticles are considered to be 100 atomic percent is 1 atomic percent or more.

3. The alloy nanoparticle according to claim 1, wherein the lower limit of the proportion of the least abundant element when the total alloy nanoparticles are considered to be 100 atomic percent is 5 atomic percent or more.

4. The alloy nanoparticle according to claim 1, wherein the element with the highest atomic ratio is 1 to 500 times greater than the element with the lowest atomic ratio.

5. The alloy nanoparticle according to any one of claims 1 to 4, wherein the correlation coefficients of the distributions of the two elements constituting the alloy nanoparticle are both within ±0.

50.

6. The alloy nanoparticle according to any one of claims 1 to 5, wherein the elements constituting the alloy nanoparticle include a combination of elements that do not form a solid solution in the phase equilibrium phase diagram.

7. When m is an integer of 3 or more, the elements constituting the alloy nanoparticles are of type m. With i being an integer between 1 and m, the average composition within the alloy nanoparticles of each i element constituting the alloy nanoparticles is C i If it is an atomic percentage, The standard deviation of the distribution of each element within the alloy nanoparticles is given by the following equation 1: i Using 2.5 × s i The alloy nanoparticles according to any one of claims 1 to 6, wherein the amount is 100 atomic percent or less. [Math 1] (In formula 1, s i The minute volume to be measured is 1 nm 3 This represents the standard deviation of the compositional distribution for each element i, where N is the minute volume measured (1 nm). 3 (Represents the number of atoms per unit.)

8. The alloy nanoparticle according to any one of claims 1 to 7, wherein the standard deviation of the distribution of each element constituting the alloy nanoparticle within the alloy nanoparticle is 40% or less of the composition ratio of that element within the alloy nanoparticle.

9. The alloy nanoparticles according to any one of claims 1 to 8, wherein the nanoparticles have a particle size of 0.5 to 30 nm.

10. The alloy nanoparticles according to claim 9, wherein the nanoparticles are supported on a carrier.

11. The alloy nanoparticle according to claim 10, wherein the carrier is a non-carbon material carrier or a particulate carbon carrier.

12. An aggregate of alloy nanoparticles, comprising the alloy nanoparticles described in any one of claims 1 to 11.

13. An aggregate of alloy nanoparticles containing 98% or more of the alloy nanoparticles described in any one of claims 1 to 11.

14. A catalyst comprising alloy nanoparticles according to any one of claims 1 to 11, or an aggregate of alloy nanoparticles according to claim 12 or 13.

Citation Information

Patent Citations

  • Manufacturing method of electrode catalyst powder for polymer electrolyte fuel cell, electrode catalyst powder for polymer electrolyte fuel cell, and polymer electrolyte fuel cell

    JP2006202698A

  • Manufacturing method of metal supported catalyst

    JP2008049336A

  • Alloy nanoparticle and method for producing the same

    JP2016138324A

  • Solid dissolution nanoparticle and method for producing the same, and catalyst

    JP2018141232A

  • Multicomponent solid solution microparticles and method for producing same, and catalyst

    WO2017150596A1