Silane-based coating liquid composition
The silane-based coating liquid composition addresses the limitations of conventional coatings by providing adjustable properties, enhancing substrates with flexibility, water repellency, and durability, suitable for various industrial uses.
Patent Information
- Application Number
- JP2025024295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-18
- Filing Date
- 2025-02-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2040-01-17
AI Technical Summary
Conventional coating liquids do not provide sufficient functionality to substrates, such as water repellency, flexibility, and durability, limiting their industrial applications.
A silane-based coating liquid composition comprising specific chemical compounds, catalysts, and solvents, allowing for adjustable properties like flexibility, water repellency, and durability by controlling the hydrolyzable and non-hydrolyzable substituents on silicon atoms, and incorporating acrylic resin for enhanced properties.
The composition imparts adjustable strength, light transmittance, water repellency, flexibility, and abrasion resistance to substrates like paper and cloth, enabling versatile industrial applications.
Smart Images

Figure 0007954971000012 
Figure 0007954971000013 
Figure 0007954971000014
Abstract
Description
[Technical Field]
[0001] The present invention relates to a silane-based coating liquid composition, and more particularly to a silane-based coating liquid composition that can be used as a coating agent. [Background technology]
[0002] Conventionally, various coating liquids have been developed to impart various functionalities. For example, coating liquids have been developed to improve the properties of paper materials and coating liquids for radiation shielding. Paper materials, with the exception of paraffin paper and cellophane paper, are inherently weak against water. In other words, known papers generally have poor water repellency. If not limited to paper, there are materials that possess light transmittance and water repellency, but these are made, for example, by stretching plastic or vinyl materials into sheets. Paper materials are also widely used in residential buildings. For example, shoji screens used as partitions for opening and closing doors in Japanese-style rooms use shoji paper, rayon shoji paper made by blending rayon or polypropylene with pulp in a predetermined ratio, shoji paper made by laminating this rayon shoji paper with a plastic film, or shoji paper made by laminating acrylic or polyvinyl chloride material onto the surface of washi paper.
[0003] As an attempt to further improve these materials while making the most of their inherent characteristics, for example, an impregnated paper is known in which a silane coupling agent or a composition containing a silane coupling agent and one or more paper-modifying agents are dispersed in the paper, and the paper does not lose its water resistance even when boiled in hot water (Patent Document 1). [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-315494 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] However, while conventional technologies, including the aforementioned patent documents, impart properties such as liquid stability and water resistance to the substrate, there is a need for the development of liquid formulations with even greater functionality. A stable liquid formulation can be cured and solidified at the desired time of use to impart the desired properties to the substrate. Furthermore, if various functions can be imparted to the substrate depending on the application, such as rigidity or flexibility, it would be possible to provide materials with high industrial value. However, such coating liquid compositions have not been known until now.
[0006] Therefore, the object of the present invention is to provide a silane-based coating liquid composition that can impart various functionalities. [Means for solving the problem]
[0007] In order to achieve the above objectives, the inventors diligently studied modifiers for silane-based coating liquid compositions, and as a result, discovered the present invention.
[0008] In other words, the silane-based coating liquid composition of the present invention has the following chemical formula [Chemical Formula 1] as its main component: [ka] The present invention is characterized by comprising a compound represented by (however, in [Chemical Formula 1], R1, R2, R3, and R4 may each be the same or different, and are hydrogen or alkyl groups having 1 to 4 carbon atoms. Also, n is 2 to 10.), a catalyst, a solvent, and a modifier.
[0009] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, the adjusting agent is characterized by being at least one of hydrogen peroxide, acetic acid, and ammonia.
[0010] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, the catalyst is characterized in that it is an organometallic compound.
[0011] In a preferred embodiment of the silane-based coating liquid composition of the present invention, in addition to the main component, the composition contains a compound represented by the following chemical formula [Chemical Formula 2] which has three hydrolyzable substituents and one non-hydrolyzable substituent: [Chemical Formula] (In [Chemical Formula 2], R5, R6 and R7 may be the same or different and each is a monomer composed of hydrogen, an alkyl group or an alkenyl group; the bond between R5O, R6O or R7O and Si is an oligomer composed of a siloxane bond; R8 is an alkenyl group or a phenyl group which may contain an epoxy group or a glycidyl group in its molecule.)
[0012] In a preferred embodiment of the silane-based coating liquid composition of the present invention, in addition to the main component, the composition contains a compound represented by the following chemical formula [Chemical Formula 3] which has two hydrolyzable substituents and two non-hydrolyzable substituents: [Chemical Formula] (In [Chemical Formula 3], R9 and R 11 may be the same or different and each is a monomer composed of hydrogen, an alkyl group or an alkenyl group; the bond between R9O or R 11 O and Si is an oligomer composed of a siloxane bond; R 10 and R 12 are each an alkyl group, an alkenyl group or a phenyl group which may contain an epoxy group or a glycidyl group in its molecule.)
[0013] In a preferred embodiment of the silane-based coating liquid composition of the present invention, the composition further contains an acrylic resin.
[0014] In a preferred embodiment of the silane-based coating liquid composition of the present invention, the composition has a decomposition function, an antibacterial function or an adsorption function.
[0015] Furthermore, the method for producing a functional material of the present invention comprises the steps of: applying the silane-based coating liquid composition of the present invention to a substrate; and drying the substrate coated with said coating composition.
[0016] Furthermore, the coated material of the present invention is characterized in that it is obtained by applying the silane-based coating liquid composition of the present invention to a substrate.
[0017] Furthermore, the solidified body of the present invention is characterized in that it is obtained by solidifying the silane-based coating liquid composition of the present invention. [[Effects of the Invention]]
[0018] In the present invention, among the four substituents of the silicon atom, when a condensate of a compound substituted with a substituent R4 that cannot be hydrolyzed and does not participate in polycondensation between compounds is used, according to the aspect, it is possible to impart appropriate strength, good light transmittance, good water repellency and flexibility, as well as abrasion resistance and flame retardancy (heat resistance) to the fiber material by coating. This provides the advantageous effect of being achievable.
[0019] Furthermore, according to the present invention, as is clear from the description of the examples described later, the flexibility of fiber materials such as Japanese paper, Western paper, and cloth that are commonly available is utilized, and the advantageous effect of being able to provide a coated material imparted with various characteristics as described above is achieved. Moreover, the various characteristics imparted to these coated materials can be adjusted relatively freely by the practitioner, for example, by arbitrarily selecting and adjusting the type and amount of the organometallic catalyst used as the catalyst, the type and amount of the compounds of [Chemical Formula 2] and / or [Chemical Formula 3], and the application amount of the coating liquid composition. This also provides the advantageous effect of being adjustable.
[0020] Furthermore, unlike materials that could only be manufactured through factory production, the present invention offers the advantageous effect of imparting strength, light transmittance, water repellency, flame retardancy, and abrasion resistance to readily available and easily obtainable base materials such as ordinary paper, while maintaining their flexibility. In addition, the present invention offers the advantageous effect of optimizing the performance of the desired function by adjusting the ratio of the main agent, catalyst, and modifier.
[0021] Furthermore, the method for manufacturing functional materials according to the present invention allows for arbitrary adjustment of not only the degree of various properties provided by the coating film, but also the thickness of the coating film. This offers the advantage of being able to adjust the type and amount of each compound as needed, for example, when used in products exposed to wind and rain outdoors, or for interior decoration such as wallpaper, thereby manufacturing and providing the optimal coating material. Moreover, according to the present invention, it is possible to manufacture a coating liquid with UV resistance, which can be used on benches, stakes, and other outdoor applications to maintain durability. [Brief explanation of the drawing]
[0022] [Figure 1] Figure 1 shows SEM images of Nos. 2, 3, 5, and 7. [Figure 2] Figure 2 shows the functionality of the solidified body in one embodiment of the present invention. [Figure 3] Figure 3 shows an example of the present invention in one embodiment, applied to a resin used for tents in buildings. [Figure 4] Figure 4 shows the functionality of the solidified body in one embodiment of the present invention. A decrease in methylene blue concentration is observed even under dark conditions, but a difference from light conditions can be confirmed. [Figure 5] Figure 5 shows the functionality of the solidified body in one embodiment of the present invention. The effect can also be confirmed by JIS testing. [Figure 6] Figure 6 shows the functionality of the solidified body in one embodiment of the present invention. [Figure 7]Figure 7 shows a micrograph of a solidified body (No. 7) in one embodiment of the present invention. K represents 1,000x magnification, and for example, 300K represents 300,000x magnification. [Figure 8] Figure 8 shows the results of an adsorption performance test of a solidified body (No. 7) in one embodiment of the present invention. [Modes for carrying out the invention]
[0023] The silane-based coating liquid composition of the present invention has the following chemical formula [Chemical Formula 1] as its main component: [ka] The present invention is characterized by comprising a compound represented by [Chemical Formula 1] (wherein R1, R2, R3, and R4 may be the same or different, and each is hydrogen or an alkyl group having 1 to 4 carbon atoms. Also, n is 2 to 10.), a catalyst, a solvent, and a modifier. In the present invention, as shown in [Chemical Formula 1], a compound can be formed in which one of the four substituents of the silicon atom is replaced with a substituent that cannot be hydrolyzed, as a repeating unit. By coating a substrate such as a fiber material with this compound, flexibility can be imparted to the substrate. That is, although there is one less strong siloxane bond between adjacent silicon atoms, the unreacted bond remains in a kind of "suspended" state, thus maintaining the flexibility of the coating film, and consequently maintaining the flexibility of the coated material.
[0024] For example, taking alkoxysilane as the main component of [Chemical Formula 1], the following applies: Examples of trifunctional silanes include methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, butyltriethoxysilane, methyltripropoxysilane, ethyltripropoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-glycidoxypropyltrimethoxysilane, amino Examples include propyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, γ-(methacryloxypropyl)triethoxysilane, γ-glycidoxypropyltriethoxysilane, aminopropyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, and polymers of these polymers of about 2 to 10 molecules. These polymers may be obtained by polymerizing only one type of monomer, or by polymerizing two or more types of monomers.
[0025] Examples of tetrafunctional silanes include polymers of tetramethoxysilane, tetraethoxysilane, tetraporoboxysilane, and tetrabutoxysilane. These polymers may be formed by polymerizing only one monomer or by polymerizing two or more monomers. Tetrafunctional silanes may be used individually or as a mixture of two or more monomers.
[0026] Furthermore, in [Chemical Formula 1], R1, R2, R3, and R4 are hydrogen atoms or alkyl groups having 1 to 4 carbon atoms, and may be the same or different, from the viewpoint that a trifunctional silane reacts with a hydrolyzable organometallic compound under an organic solvent. Also, n is 2 to 10. In [Chemical Formula 1], the reason why the repeating of the main chain is n=2 to 10 is that if n=1, i.e., a monomer is used, polymerization takes a long time, making it difficult to produce a coating film with sufficient strength in a short time. However, if n is 11 or more, conversely, when applied to a fiber material, there will be insufficient alkoxy groups, etc., for polymerization on the fiber material, making it difficult to produce a coating film with sufficient strength. Therefore, in the present invention, condensates with n=2 to 10, and especially n=2 to 8, are preferred.
[0027] Generally speaking, when synthesizing condensates like [Chemical Formula 1] from monomers, it is practically impossible to precisely control the degree of polymerization. Therefore, the use of n=2 to 10, preferably n=2 to 8, in this invention means using a coating solution that, in terms of the distribution of degrees of polymerization, mainly contains n=2 to 10, preferably mainly 2 to 8, and it is acceptable even if a compound with n=11 or higher is included. Such compounds can be obtained by condensing monomers (e.g., methyltrimethoxysilane).
[0028] As described above, the raw materials (monomers) for obtaining the compound in Chemical Formula 1 can be purchased at a similarly low cost compared to tetraalkoxysilanes, which are inexpensive but have strong inorganic properties. Therefore, by using the compound in Chemical Formula 1, it is possible to manufacture a coating material with sufficient organic properties and sufficient strength without having to use expensive so-called silane coupling.
[0029] Examples of compounds represented by Formula 1 include condensates of methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, butyltriethoxysilane, methyltripropoxysilane, and ethyltripropoxysilane. The compound in Formula 1 may be formed by condensing only one of these monomers, or by condensing two or more of the monomers exemplified above.
[0030] The primary role of the non-hydrolyzable substituent (R4) in the compound of Formula 1 is to provide flexibility to the coating film. However, if the coating film is also to be given water repellency, then R4 should be an alkyl group. Generally, the more carbon atoms an organic substituent has, the more organic it is, i.e., the more water-repellent it becomes. However, if the number of carbon atoms becomes too large, steric hindrance can cause strain within the coating film, leading to a decrease in film strength. Therefore, it is preferable to determine the number of carbon atoms of the alkyl group and the types and amounts of each monomer constituting the compound of Formula 1 (condensate) by conducting preliminary manufacturing tests, referring to the examples in this specification. However, since the imparting of water repellency to the coating film can also be achieved by adding the compounds of Formula 2 or Formula 3 described later, it is not essential that R4 in the compound of Formula 1 be an alkyl group.
[0031] Furthermore, in the present invention, the content of the compound shown in Chemical Formula 1 is not particularly limited, but the content of the compound shown in Chemical Formula 1 can be preferably 20 to 70% by weight, more preferably 30 to 50% by weight, in terms of organoalkoxysilane. If it is 10% by weight or less, the binder effect may be reduced. If no other additives are considered, it may be 50% by weight or more.
[0032] Furthermore, the catalyst in this invention is not particularly limited. In order for the main component element and the catalyst element to undergo a sol-gel reaction together, thereby enabling the main component element (Si (silicon)) to effectively support the catalyst element, and for the catalyst to exert its function without the catalyst element directly affecting the coated substrate, organometallic compounds can be cited as examples of catalysts.
[0033] When an organometallic compound is mixed with the compound in Formula 1 to form a coating liquid composition, and this is applied to a fibrous material such as paper, the organometallic compound absorbs moisture from the paper or from the air (humidity), and hydrolyzes itself. At this time, it forms a network with the compound in Formula 1, and the compound in Formula 1 can be hardened and solidified. Examples of organometallic compounds preferably used in the present invention include those containing titanium, zircon, aluminum, or tin. More specifically, examples include tetrapropoxytitanate, tetrabutoxytitanate, tetrapropoxydylconate, tetrabutoxydylconate, tripropoxyaluminate, aluminum acetylacetonate, dibutyltin diacetate, or dibutyltin dilaurate.
[0034] Furthermore, while the catalyst content is not particularly limited in this invention, from the viewpoint of enabling hydrolysis and polycondensation reactions to cure and solidify the silane-based coating liquid, which is the main component, the catalyst content can preferably be 1 to 10% by weight, and more preferably 3 to 7% by weight.
[0035] In addition, any commonly used catalyst can be used without special restrictions as a catalyst for curing and solidifying the compound shown in Formula 1. For example, examples of acid catalysts include hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, formic acid, or acetic acid. Examples of base catalysts include ammonia, tetramethylammonium hydroxide, 2-hydroxyethyltrimethylammonium hydroxide, ethanolamine, diethanolamine, or triethanolamine. When using these ordinary catalysts, reaction water is added in the presence of the reaction water to cure and solidify the compound in Formula 1.
[0036] The coating solution composition provided by the present invention can contain the compound of Chemical Formula 1, a catalyst, and reaction water, as described above. While there are no particular problems during normal use, a challenge arises during long-term storage: the coating solution tends to gel due to the reaction water. To solve this, it is preferable to use a hydrolyzable organometallic compound as a catalyst instead of the conventional catalyst described above. Using a hydrolyzable organometallic compound eliminates the need for reaction water, resulting in improved long-term storage stability, which is desirable.
[0037] Furthermore, a solvent may be added to the coating liquid composition of the present invention to uniformly mix the compound of Chemical Formula 1, the catalyst, and, if necessary, the reaction water. Examples of solvents used for this purpose include alcohols. More specifically, methanol, ethanol, propanol, isopropanol, butanol, pentanol, or hexanol can be given as examples. In addition, the viscosity and drying speed of the coating liquid can be adjusted by controlling the amount of solvent added.
[0038] For the purpose of such adjustments, it is particularly preferable to use one or more organic solvents with high viscosity and boiling point, such as glycols including ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, dipropylene glycol, and polypropylene glycol, or cellosolves such as methoxyethanol, propoxyethanol, butoxyethanol, methoxypropanol, ethoxypropanol, propoxypropanol, or butoxypropanol, either individually or in combination of two or more. Of course, the alcohols may also be added simultaneously with one or more of the above-mentioned organic solvents with high viscosity and boiling point. Furthermore, if the purpose is to adjust the viscosity or drying speed of the coating solution, the same effect can be achieved not only with the above-mentioned organic solvents but also with surfactants.
[0039] In particular, the glycols and cellosolves mentioned above have hydroxyl groups in their molecules, and therefore can be introduced into the siloxane bond network formed by the condensation reaction of the compounds in Formula 1. Since glycols and cellosolves are organic, their introduction increases the organic properties of the resulting coating film, that is, increases the organic properties of the coating material.
[0040] Furthermore, while the solvent content is not particularly limited in the present invention, from the viewpoint of base material, function, and appropriate concentration, the solvent content can preferably be 2 to 95% by weight, and more preferably 25 to 50% by weight.
[0041] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, the adjusting agent is characterized by being hydrogen peroxide and / or acetic acid, from the viewpoint of effectively imparting the functions inherent to the compounds constituting the main component and catalyst. The adjusting agent can be a weakly acidic or basic catalyst, and can be at least one of acetic acid, hydrogen peroxide, or ammonia. This adjusting agent can also be called a second catalyst, and the inventors have found that by adding it, new functions can be created, such as the formation of a new elemental arrangement. This adjusting agent is completely different in action and function from those of strong acids and large amounts of water (H2O) used in conventional sol-gel methods.
[0042] In other words, although most issues remain unresolved, the inventors have surprisingly discovered that by adding these modifiers such as acid groups, it is possible to efficiently express the functions inherent in the compounds constituting the added metal catalyst. Specifically, as will be clear from the examples described later, for example, using an organometallic compound, such as tetrabutoxytitanium, as a catalyst, the inventors succeeded in synthesizing titanium dioxide with adsorption and decomposition functions, which are present in the compounds constituting the catalyst, through the action of the modifiers, and were able to find a composition that can contain this functional component in a liquid state.
[0043] In the present invention, there are no particular limitations on the content of the modifier, but from the viewpoint of secondary function expression, the content of the modifier can preferably be 0.5 to 5% by weight, and more preferably 1 to 2% by weight.
[0044] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, in addition to the main component, a compound represented by the following chemical formula [Chemical Formula 2], having three hydrolyzable substituents and one non-hydrolyzable substituent: [ka] (However, in [Chemical Formula 2], R5, R6, and R7 may be the same or different, and are monomers consisting of hydrogen, an alkyl group, or an alkenyl group; the bond between R5O, R6O, and R7O and Si is an oligomer consisting of a siloxane bond; and R8 is an alkenyl group or a phenyl group, which may contain an epoxy group or a glycidyl group within its molecule.)
[0045] In this invention, by using a coating solution containing the compound in Chemical Formula 2 in addition to the compound in Chemical Formula 1, it is possible to newly impart or increase the organic properties and other characteristics of the compound in Chemical Formula 2 compared to a coating material produced without using this solution. The compound in Chemical Formula 2 added for this purpose is a compound in which three of the four substituents are hydrolyzable substituents and the remaining one substituent is not hydrolyzable.
[0046] In chemical formula 2, R5, R6, and R7 may be the same or different, and are monomers consisting of hydrogen or an alkyl group or alkenyl group having 1 to 10 carbon atoms. The bonds between R5O, R6O, and R7O and Si are oligomers consisting of siloxane bonds. R8 is an alkyl group, alkenyl group, or phenyl group having 1 to 10 carbon atoms, and may contain an epoxy group or a glycidyl group within its molecule.
[0047] In the present invention, examples of compounds represented by Formula 2 include vinyltrimethoxysilane, phenyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-glycidoxypropyltrimethoxysilane, aminopropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, -(methacryloxypropyl)triethoxysilane, γ-glycidoxypropyltriethoxysilane, aminopropyltriethoxysilane, vinyltris(βmethoxyethoxy)silane, and condensates of these compounds of about 2 to 10 molecules.
[0048] Furthermore, the compound in formula 2 may be two or more of the aforementioned monomers. When using a condensate of two or more molecules as the compound in formula 2, it may be a compound formed by the condensation of two or more of the aforementioned monomers.
[0049] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, in addition to the main component, a compound represented by the following chemical formula [Chemical Formula 3] having two hydrolyzable substituents and two non-hydrolyzable substituents: [ka] (However, in [Chemical Formula 3], R9 and R 11 These may be the same or different monomers consisting of hydrogen, an alkyl group, or an alkenyl group, and R9O and R 11 The bond between O and Si is an oligomer consisting of a siloxane bond, R 10 and R 12 This is characterized by containing an alkyl group, alkenyl group, or phenyl group, which may contain an epoxy group or a glycidyl group within its molecule.
[0050] In the present invention, by using a coating liquid composition obtained by adding the compound of Chemical Formula 3 to a coating liquid composition containing the compound of Chemical Formula 1, or to a coating liquid composition containing both the compound of Chemical Formula 1 and the compound of Chemical Formula 2, it is possible to newly impart properties such as organic properties possessed by the compound of Chemical Formula 3 to the coating material, or to increase properties such as organic properties, as compared with a coating material produced without using the compound of Chemical Formula 3.
[0051] The compound of Chemical Formula 3 is a compound in which two of the four substituents are hydrolyzable substituents and the other two are non-hydrolyzable substituents. In Chemical Formula 3, R9 and R 11 may be the same or different from each other, and are monomers consisting of hydrogen, an alkyl group having 1 to 10 carbon atoms, or an alkenyl group, and R9 and R 11 and Si is an oligomer composed of a siloxane bond, and R 10 and R 12 is an alkyl group having 1 to 10 carbon atoms, an alkenyl group, or a phenyl group, which may contain an epoxy group or a glycidyl group in its molecule.
[0052] Specific examples of the compound represented by Chemical Formula 3 include dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, and condensates of about 2 to 10 molecules thereof. The compound of Chemical Formula 3 may be two or more of such monomers, and when using a condensate of two or more molecules, it may be a condensate of two or more of such monomers.
[0053] By adding either the compound of Chemical Formula 2 or the compound of Chemical Formula 3 as described above to the coating liquid composition, the organic properties of the coating film can be increased. However, if both the compounds of Chemical Formula 2 and Chemical Formula 3 are added to the coating liquid composition, the organic properties of the coating film can be further improved, and as a result, the water repellency and the like of the coating material can be further improved.
[0054] It is preferable to add the compound of Chemical Formula 2 and / or the compound of Chemical Formula 3 to the coating liquid composition in a total amount not exceeding 50% of the compound represented by Chemical Formula 1, which is the main component of the coating liquid composition. If the total amount of both added exceeds this range, when the coating liquid composition is applied to the fiber material, it may not bond well with the main component, the compound of Chemical Formula 1, and the strength of the coating film may become insufficient. Therefore, when actually adding the compound of Chemical Formula 2 and / or the compound of Chemical Formula 3, it is preferable to assume that the strength of the coating film will decrease depending on the amount added, and to conduct preliminary manufacturing tests while referring to the examples in this specification, etc., to clarify the range of amounts that can achieve the objective, and then minimize the amount added.
[0055] Furthermore, the non-hydrolyzable substituents (R8, R) in the compound of Chemical Formula 2 and the compound of Chemical Formula 3 10 , R 12 The primary role of these substituents is to provide flexibility to the coating film, but since they are organic substitutions such as alkyl groups, they also play a role in imparting water repellency to the coating film. Generally, the more carbon atoms an organic substituent has, the more organic it is, i.e., the more water-repellent it becomes. However, if the number of carbon atoms becomes too large, steric hindrance can cause strain within the coating film, leading to a decrease in film strength. Therefore, it is preferable to determine the number of carbon atoms of the organic substituent and the types and amounts of each monomer constituting the compounds (condensates) of Formula 2 and / or Formula 3 by conducting preliminary manufacturing tests, referring to the examples in this specification.
[0056] Siloxane bonds, while possessing strong heat and abrasion resistance, are also what is known as "hard" bonds. Because of this "hardness," applying them to fibrous materials such as paper can impart abrasion resistance to those materials. However, fibrous materials like paper are characterized by their flexibility, and sometimes the coating material needs to possess a similar flexibility to the paper or other fibrous material itself.
[0057] Conventional sol-gel coat solutions commonly used utilize tetraalkoxysilane (Si(OR)4) or its oligomers as starting materials. When these are completely hydrolyzed (as described later in reaction equation 1 (1) to (3)) to form a coating film, all four bonds of the silicon atoms form a hard siloxane bond network. This results in a film that is hard like ceramic, but brittle and lacks flexibility, making it virtually impossible to manufacture coating materials that utilize the flexibility of paper or similar materials.
[0058] However, the present invention solves this problem by using the compound shown in Formula 1, in which one of the four substituents on the silicon atom is not hydrolyzable, as the main component of the coating solution composition. Furthermore, in the present invention, flexibility and other properties can be further increased by adding the compounds shown in Formula 2 and Formula 3, each having one or two substituents that are not hydrolyzable, to the coating solution composition.
[0059] Furthermore, a preferred embodiment of the silane-based coating liquid composition of the present invention is characterized by further comprising an acrylic resin.
[0060] In the present invention, the acrylic resin is not particularly limited, but for example, an acrylic monomer and one obtained by radical copolymerization of an acrylic monomer and another monomer copolymerizable with the acrylic monomer can be used.
[0061] Among these, the acrylic monomers are not particularly limited, but examples include alkyl group-containing (meth)acrylic monomers such as methyl (meth)acrylate (indicating either methyl acrylate or methyl methacrylate; the same applies hereinafter), ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate; hydroxyl group-containing (meth)acrylic monomers such as 2-hydroxyethyl (meth)acrylate; ethylenically unsaturated carboxylic acids such as (meth)acrylic acid; amino group-containing (meth)acrylic monomers such as dimethylaminoethyl (meth)acrylate and dimethylaminopropyl (meth)acrylate; amide-containing (meth)acrylic monomers such as (meth)acrylamide and ethyl (meth)acrylamide; nitrile group-containing (meth)acrylic monomers such as acrylonitrile; and epoxy group-containing (meth)acrylic monomers such as glycidyl (meth)acrylate.
[0062] Other monomers copolymerizable with acrylic monomers include aromatic hydrocarbon vinyl monomers such as styrene, methylstyrene, chlorostyrene, and vinyltoluene; ethylenically unsaturated carboxylic acids such as maleic acid, itaconic acid, crotonic acid, fumaric acid, and citraconic acid; sulfonic acid-containing vinyl monomers such as styrenesulfonic acid and vinylsulfonic acid; acid anhydrides such as maleic anhydride and itaconic anhydride; chlorine-containing monomers such as vinyl chloride, vinylidene chloride, and chloroprene; hydroxyl group-containing alkyl vinyl ethers such as hydroxyethyl vinyl ether and hydroxypropyl vinyl ether; alkylene glycol monoallyl ethers such as ethylene glycol monoallyl ether and propylene glycol monoallyl ether and diethylene glycol monoallyl ether; α-olefins such as ethylene, propylene, and isobutylene; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl pivalate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, and cyclohexyl vinyl ether; and allyl ethers such as ethyl allyl ether and butyl allyl ether.
[0063] The above-mentioned acrylic resin can be obtained, for example, by emulsion polymerization. There are no particular restrictions on the emulsion polymerization method; an acrylic resin emulsion can be produced by polymerizing monomers in a dispersion system in an aqueous medium, where the monomers, chain transfer agent, surfactant, radical polymerization initiator, and other additive components used as optional components are the basic components, using conventionally known methods.
[0064] In the present invention, the acrylic resin is present in an amount of 10 to 30% by weight, preferably 25 to 30% by weight, on a solid content basis, relative to the total amount of the composition of the present invention. If the amount is less than 10% by weight, the resulting coating film tends to become hard and brittle, while if it exceeds 30% by weight, the coating film is soft, but if functional components are added, the amount of such components added will decrease, which may reduce the functionality of those components.
[0065] Furthermore, in a preferred embodiment of the silane-based coating liquid composition of the present invention, the composition is characterized by having a decomposition function, an antibacterial function, or an adsorption function.
[0066] Furthermore, the silane-based coating liquid composition of the present invention can be safely stored in a sealed state by low-temperature storage, etc. That is, even when containing the compound of Chemical Formula 1, a catalyst, and adjusting agents, a stable liquid composition can be obtained. Reactions and polycondensation reactions can be carried out by OH groups (moisture / water) in the air, or by OH groups (intrinsic moisture) in the substrate when coating. Being a stable coating liquid composition is one of the features of the present invention.
[0067] A major difference from conventional sol-gel glass production methods is that it does not require, or even requires, large amounts of water or acid catalysts such as sulfuric acid, nitric acid, phosphoric acid, or hydrochloric acid. While sol-gel glass is strongly alkaline, the glass produced by coating agents No. 1 to 17 in the examples described later is weakly acidic to neutral, making it possible to produce safe glass that does not harm the human body or the environment.
[0068] Thus, one of the important features of the coating liquid composition of the present invention is that, even with a catalyst added, it does not harden or solidify unless it comes into contact with moisture in the air or reacts with moisture in the substrate. If kept sealed, it can be easily applied at any time, and is also inexpensive. In other words, because the present invention is a liquid with good wettability, it is possible to coat even complex shapes down to the smallest details to form a protective film and achieve the desired function.
[0069] The coating liquid composition of the present invention may be used after solidifying as is, or it may be used after being applied to a substrate, as described later.
[0070] Furthermore, the method for producing the functional material of the present invention is characterized by comprising the steps of applying the silane-based coating liquid composition of the present invention to a substrate and drying the substrate to which the coating composition has been applied. With regard to the silane-based coating liquid composition, the above-described description of the silane-based coating liquid composition of the present invention can be directly applied to the method for producing the functional material.
[0071] In the present invention, the substrate to be coated is not particularly limited. Examples include fabrics such as knitted fabrics, woven fabrics, nonwoven fabrics, and paper, as well as films and sheets. Specifically, examples include fabrics and films made of polyamide fibers, polyester fibers, rayon fibers, cotton, pulp, etc., as well as Japanese paper, copy paper, Tyvek (a polyethylene nonwoven fabric manufactured by DuPont), wallpaper, fusuma paper, shoji paper, ceiling paper, tablecloths, curtains, mats, and rubber sheets. In addition to the above-mentioned paper, etc., trees, wood products, and buildings can also be used as substrates. Furthermore, since siloxane bonding is possible even in inorganic materials, metals, concrete, carbon compounds, glass, and products thereof can also be given as examples of substrates.
[0072] Coating a substrate with the composition of the present invention can be performed using methods such as brush application, spraying, dipping, roll coating, and printing. A single coat can form a coating with the desired dry thickness, and it can also be applied in 2 to 5 additional coats. In the case of multiple coats, heating and drying treatment may be performed after each coat.
[0073] When the composition of the present invention is coated onto a substrate, at a temperature of room temperature to 60°C, (a) the organoalkoxysilane undergoes hydrolysis and polycondensation simultaneously to produce a sol, and the reaction can further proceed to form a gel, i.e., an organopolysiloxane. By leaving this at room temperature for 1 to 6 days or heating it at 80 to 150°C for 10 to 60 minutes, the solvent volatilizes and the organopolysiloxane, and optionally an acrylic resin, co-condenses, and if functional components are included, a cured coating film composite of those components can be formed. However, the reaction temperature and the standing or heating time are not limited to those stated above, as they vary depending on the type and proportion of each component used.
[0074] In the method for producing a functional material according to the present invention, first, any fiber material can be cut and processed to any size and shape, and then the coating liquid composition of the present invention described above can be applied thereto. The specific application method is not particularly limited, but for example, it can be done by immersing the fiber material in the coating liquid, applying the coating liquid to the fiber material, or spraying the coating liquid onto the fiber material. In addition, as a coating method, for example, cloth rubbing, brush application, roller method, spray method, immersion method, gravure printing machine coating method, and oven drying method can be used.
[0075] Furthermore, the drying process is not particularly limited. For example, the liquids in Examples No. 1 to 17 described later can basically be cured and solidified by natural drying (at ambient temperature and humidity). Heating is effective when the reaction is accelerated and the curing and solidification film formation is promoted more quickly.
[0076] In this invention, functional materials such as coating materials can be manufactured using fiber materials such as dried bark fibers, high-grade handmade Japanese paper, ordinary machine-made Japanese paper, Western paper or Japanese paper, fibers made from non-woven fabric, and ordinary cloth. Furthermore, by applying a predetermined pretreatment to the fiber material prior to applying the coating liquid composition, the bond between the fiber material surface and the coating film can be strengthened compared to materials that have not undergone such pretreatment.
[0077] As an example of this pretreatment, for instance, a substrate such as a fiber material is immersed in high-purity isopropyl alcohol of about 98% for about 30 minutes, then left at a high temperature of about 100°C to dry completely, and then irradiated with ultraviolet light for about 30 minutes. When the coating liquid composition is applied to a substrate such as a fiber material that has undergone or has not undergone the above-described pretreatment, the compound in Chemical Formula 1 undergoes hydrolysis, and a siloxane bond (Si-O-Si) is formed through the reactions shown in (1) to (3) of Reaction Formula 1 below.
[0078] Reaction equation 1: (1)Si-OR+H2O → Si-OH+ROH (2)Si-OH+HO-Si → Si-O-Si+H2O (3)Si-OH+RO-Si → Si-O-Si+ROH
[0079] The bond energy of the Si-O bond within the siloxane bond (Si-O-Si) formed in this manner is 106 kcal / mol. On the other hand, the bond energy of the CC bond, a typical bond in organic compounds, is 82.6 kcal / mol. Therefore, it can be seen that the glassy coating film containing siloxane bonds, produced by the hydrolysis of the compound in Chemical Formula 1, has a much more thermally stable bond than that of the organic compound. Due to this thermally stable bond, the coating film formed by the present invention has excellent heat resistance and abrasion resistance, and as a result, it becomes possible to manufacture a coating material with excellent heat resistance and abrasion resistance.
[0080] Furthermore, if the coating liquid composition of the present invention contains the aforementioned organometallic compound (e.g., tetrabutoxytitanium) as a catalyst, the reactions (1) to (3) in reaction formula 1 above will proceed even if the coating liquid does not contain reaction water. In this case, the reaction will proceed in detail as shown in (4) and (5) in reaction formula 2 below.
[0081] Reaction equation 2: (4)Ti-OR+H2O → Ti-OH+ROH (5)Ti-OH+RO-Si → Ti-O-Si
[0082] As described above, the introduction of Ti-O bonds into the coating film further improves heat resistance and wear resistance compared to coating films with only siloxane bonds. Thus, using organometallic compounds as catalysts not only eliminates the need for reaction water, but also further improves the heat resistance and wear resistance of the coating film, and ultimately makes the coating material even more heat-resistant and wear-resistant.
[0083] In the present invention, the modifier is further included. As mentioned above, the present invention does not use the common sol-gel method which involves adding large amounts of water, acid, and base, but rather allows for the use of sol-gel reactions of both the main component and the catalyst by adding a modifier as needed. The inventors have found that this makes it possible to provide a novel functional material that can stably exhibit the original functions of the elements of the main component and catalyst, contrary to conventional technical knowledge.
[0084] Furthermore, the coating material of the present invention is characterized by being obtained by applying the silane-based coating liquid composition of the present invention to a substrate. Furthermore, the solidified body of the present invention is characterized by being obtained by solidifying the silane-based coating liquid composition of the present invention. For the silane-based coating liquid composition, substrate, application and solidification methods of the present invention, etc., refer directly to the above-described explanation of the silane-based coating liquid composition or the method for producing the functional material of the present invention. [Examples]
[0085] The present invention will be described in more detail below based on examples, but these examples are merely illustrative, and the present invention is not to be interpreted as being limited to these examples. Furthermore, it goes without saying that the present invention can be modified as appropriate without departing from its essence.
[0086] Examples 1-16 Preparation of alkoxysilane condensates: Methyltrimethoxysilane condensates were synthesized as follows.
[0087] In a 500 ml three-necked flask, 181 g of methyltrimethoxysilane, 50 g of methanol, and 18 g of pure water were added and thoroughly stirred. Then, 2 g of 61% nitric acid was added and the mixture was heated and refluxed for 3 hours while stirring. After the reaction was complete, the reaction vessel was reduced in pressure while heating to remove the methanol. Gas chromatography analysis of the resulting methyltrimethoxysilane revealed that it was mainly composed of 3-4 mers.
[0088] Next, the coating liquid composition was prepared and the functional materials (coating materials) were manufactured. Using the alkoxysilane condensates synthesized as described above, 16 types of functional materials of the present invention, as shown in Table 1, were prepared, containing these as the main components (the unit of mixed weight is g). In Table 1, specifically for main compound A, Nos. 1-7 and 11-14 are methyltrimethoxysilane (trifunctional), and Nos. 8-10 are tetraethoxysilane oligomers (tetrafunctional). Specifically for compound B and C, Nos. 5-7 are tetraethoxysilane oligomers (tetrafunctional), and Nos. 12, 15, and 16 are polyalkylalkoxysilanes (trifunctional) (in No. 15, Ti powder is used as a modifier to improve adhesion). Specifically for the organic solvent, Nos. 1-11 and 14-16 are isopropyl alcohol, and Nos. 12 and 13 are ethyl acetate. Furthermore, regarding the reaction accelerator (catalyst), specifically, Nos. 1 to 16 are tetrabutoxytitanium. Function 1 indicates water repellency, Function 2 indicates flame retardancy, Function 3 indicates light transmittance, Function 4 indicates decomposition, antibacterial, antifouling, and adsorption, and Function 5 indicates adhesion. The sources of the components used are as follows. • Acrylic acid ester polymer (Toagosei Co., Ltd.) • Tetraethoxysilane oligomer (Tama Chemical Industry Co., Ltd.) • Polymethylphenylsiloxane (Shin-Etsu Chemical Co., Ltd.) • Tetramethoxysilane oligomer (Mitsubishi Chemical Corporation) • Acrylic acid ester copolymer (Toagosei Co., Ltd.) • Polyalkylalkoxysilane (Shin-Etsu Chemical Co., Ltd.) • Polymethylhydrogen siloxane (Merck) Isopropyl alcohol (Sankyo Chemical Industry Co., Ltd.) • Ethyl acetate (Showa Denko Corporation) • Tetrabutoxytitanium (Nippon Soda Co., Ltd.)
[0089] [Table 1]
[0090] Manufacturing of functional materials (coating materials) Functional materials were manufactured in the applicant's laboratory (room temperature 25°C, humidity 70%) by applying coating liquid compositions No. 1 to 16 to a cellulose fiber material. First, several sheets of washi paper were prepared as the fiber material, and these sheets were immersed in each coating liquid composition for 30 seconds. Then, to prevent the washi paper from being thermally deformed, drying was started at 60°C, and the temperature was gradually increased until it reached 100°C, completely drying the washi paper and producing the functional material (washi paper) of the present invention.
[0091] For example, in the examples, liquid agent No. 1 can be dried at room temperature (5°C to 40°C) after coating the substrate (wood). Once the surface is dry, it can be placed in a drying oven at 80°C to 140°C for 1 hour. Liquid agent No. 2 can be dried at 120°C for 60 minutes after immersion in the substrate (glass fiber) and drying for 10 minutes. Liquid agents No. 3 to No. 10 are applied to the substrate using the same process as No. 1, but the temperature may be raised to 80°C to 400°C depending on the type of substrate. Liquid agents No. 11, No. 15, and No. 16 are multi-purpose substrate coating agents using acrylic ester polymers, so 5°C to 140°C for about 1 hour is appropriate. The appropriate temperature can be determined by the substrate. Furthermore, liquids No. 12 to 14 are designed to create a glassy film and impart water repellency (without using fluorine) without impairing the properties of the flexible substrate, and drying is suitable at room temperature to around 120 degrees Celsius.
[0092] Next, evaluation experiments were conducted on the manufactured functional materials regarding water repellency, flame retardancy, light transmittance, antibacterial / antifouling properties, air purification, and adhesion. Table 1 shows the results of each evaluation, taking into account an overall assessment, using double circles, circles, and triangles. Double circles indicate excellent performance, circles indicate good performance, and triangles indicate slightly inferior performance.
[0093] (1) Evaluation of light transmittance: In evaluating light transmittance, in addition to washi paper, crumpled washi paper, water-dropped washi paper with patterns, wood chip paper made from collected wood chips, and cardboard were used to manufacture coating materials (functional materials) and subject to evaluation.
[0094] The evaluation involved illuminating each manufactured coated material from below with a lightbox and observing it with the naked eye to assess gloss, color development, transparency, etc. As a result, the coated material manufactured from washi paper using this coating liquid composition had a glossy, semi-transparent surface because the coating liquid itself was colorless and transparent. The color of the washi paper became more intense, and the white parts of the washi paper remained white, exhibiting a glossy, semi-transparent appearance. On the other hand, with the comparative coating liquid, the coating liquid itself was yellowish, so the white parts of the washi paper were slightly yellowish, glossy, and semi-transparent.
[0095] (2) Mechanical strength and light transmittance were evaluated for the coated material made from crumpled paper. When the material was folded by hand, the hardness (mechanical strength) of each coated film was evaluated by visual observation to see if the coating film peeled off. In the case of the coated material made using this coating liquid composition, the surface did not peel off even when the paper was folded. Furthermore, it was found that all washi paper airplanes coated with the coating liquid could withstand a wind speed of Mach 7 in the 200-degree high-temperature wind tunnel experimental facility at JAXA on the Kashiwa Campus of the University of Tokyo.
[0096] The above results indicate that the coated film formed by this coating liquid composition exhibits greater flexibility and overall increased mechanical strength. This is presumed to be because, during the process of hydrolysis and polycondensation on the crumpled paper, the main component (compound in Chemical Formula 1), the added silane compounds (compounds in Chemical Formulas 2 and / or 3), and the catalyst contained in the coating liquid penetrate into the fine parts of the crumpled paper, physically bonding with the paper fibers and mechanically intertwining, or hydrophobic bonding between organic parts, and also due to chemical bonding between the hydroxyl groups of cellulose, the main component of paper, and the silane compounds, resulting in increased mechanical strength.
[0097] Furthermore, the liquid tensile hardness and tear strength of handmade Japanese paper were measured at the Tokyo Metropolitan Industrial Technology Research Center. For the tensile strength test, a constant-speed elongation tensile test (RTF-1250, manufactured by A.END.D. Co., Ltd.) was used (test specimen width: 25 mm, tensile speed: 50 mm / min, gripping distance: 100 mm, number of measurements: 3). For the tear strength test, an Elmendorf type tear tester (No. 445, manufactured by Yasuda Seiki Seisakusho Co., Ltd.) was used (number of measurements: 5).
[0098] As a result, the tensile strength of the base paper was improved as follows: Liquid No. 2 for glass coating of base paper sheets increased 2.24 times, Liquid No. 3 for semiconductors increased 2.25 times, Liquid No. 5 increased 2.18 times, and Liquid No. 7 for titanium dioxide function increased 2.4 times. The sheet with Liquid No. 7 showed the best values in both the length and width. It was clearly demonstrated that the photo-functional liquid did not destroy the organic matter, the paper did not crumble, and each individual fiber was firmly protected by the siloxane bonding film. However, the tear strength decreased inversely to the tensile strength because the flexibility of the uncoated paper was lost due to the hardening and solidification of the liquid.
[0099] Figure 1 shows SEM images of samples No. 2, 3, 5, and 7. Figure 1(a) shows the original paper, (b) shows No. 2, (c) shows No. 3, (d) shows No. 5, and (e) shows No. 7. The white areas between the fibers are the glassy spaces that create the adhesive function.
[0100] (3) Evaluation of water repellency The water repellency was evaluated based on the "Test method for water repellency of paper and cardboard (JIS-P8137)". First, in accordance with JIS P8110 (Test paper sampling method), test pieces of 300 mm or longer and 200 mm in width, free from folds, wrinkles, gaps, etc., were taken from the coated material manufactured from Japanese paper, and these were pretreated according to the conditions shown in JIS P8111 (Pretreatment of test paper).
[0101] (4) Regarding the evaluation of flame retardancy, the coating material manufactured by the present invention has applications as a building material, such as stained glass, covers and shades for lamps, exterior wall protection materials, interior decorative wallpaper, shoji paper, etc. Therefore, an evaluation was conducted to determine whether or not it possesses the flame retardancy required for building materials. In this flame retardancy evaluation, horizontal and vertical combustion tests were conducted in accordance with the UL standard (a standard set by the Underwriter's Laboratories operated by the United States Fire Insurance Commission, concerning fire prevention, electrical safety, theft prevention, etc., and products that conform to this UL standard are given the UL approval label), using the following method.
[0102] In conducting this combustion test, the method described in the above example was used for 1 m of washi paper. 2 Each coating solution was immersed in 7.5g of each coating solution, resulting in "7.5g / m 2 " and 1 meter of washi paper 2 Each coating solution was immersed in 15g of the "15g / m²" coating solution. 2 These materials were manufactured and cut to a length of 125±5mm, a width of 13.0±0.3mm, and a thickness of approximately 0.18mm to create test specimens. In addition, washi paper that had not been immersed in any of the coating solutions was cut to the same dimensions and used as a "blank" test specimen. Each test specimen was then left for 48 hours at a temperature of 23±2℃ and a humidity of 50±5% or less as a pretreatment.
[0103] A chamber, enclosure, or laboratory hood without ventilation was prepared, along with a burner measuring 100±10mm in length and 9.5±0.3mm in inner diameter, supplied with industrial-grade methanol gas (minimum purity 98%), equipped with a regulator and flow meter. A clock (accuracy 1 second), a manometer with accuracy to 0.01mm, and a ring stand with clamps to support the test specimens were also prepared. For the horizontal combustion test (compliant with UL standard 94HB), lines were first drawn at 25mm and 100mm from the ignition end of each prepared test specimen.
[0104] Next, a 125mm x 125mm 20-mesh wire mesh was placed horizontally at a predetermined height on the ring stand. The other end of the ignition end in the long direction of the test specimen was supported with a clamp at a predetermined distance above the wire mesh. The burner was ignited at a distance from the test specimen, and the gas flow rate and other settings were adjusted so that there was no yellow flame and the flame height was 20±1mm. The burner flame was then positioned so that it reached 6±1mm from one end of the test specimen, and the flame was applied for 30 seconds. If the burning of the test specimen reached the line at the 25mm position within 30 seconds, the burner was moved away. If it continued to burn, the horizontal burning time from the line at the 25mm position to the line at the 100mm position was measured three times.
[0105] As described above, when the flame retardancy was evaluated, the coated material produced using this coating liquid composition showed good results in the horizontal combustion test.
[0106] Furthermore, the vertical combustion test (compliant with UL standard 94V-0) used the same test specimens as in the horizontal combustion test. First, the specimens coated with non-combustible material were tested at 7.5 g / m². 2 "Test specimen and "15g / m² coated with non-combustible material" 2 A test specimen was prepared, its length perpendicular to the surface, and its upper end supported by the clamp of the ring stand. After adjusting the burner so that the flame height was 20 ± 1 mm, the tip of the flame was placed 10 mm below the center of the lower edge of the test specimen, and the flame was applied for 10 seconds. Then, the burner was moved at least 150 mm away from the test specimen, and the first afterflame time measurement was performed. After the afterflame subsided, the burner was placed again 10 mm below the center of the lower edge, and the flame was applied for 10 seconds. The burner was then moved at least 150 mm away from the test specimen, and the second afterflame time measurement was performed, along with the residual smoke time at this time.
[0107] To summarize the above, the following can be said: No. 1 can be used mainly as a penetrating liquid agent for wood. It is a trifunctional, highly water-repellent, and creates a fine surface bonding film for wood. When applied to paper, the fine reaction improves the tensile and tear strength of the paper. No. 2 can be used mainly as a liquid agent for glass fibers. It is a trifunctional, water-repellent, and elongated modified reaction liquid agent that can create porous films. No. 3 can be used for semiconductors, metal surface coatings, non-porous films, wood finishing agents, water- and oil-resistant paper, etc. It is water-repellent, oil-repellent, and has high film strength, creating a flat glass-hardened and solidified film on the substrate. Transparency is increased depending on the substrate. No. 4 can be used as an antibacterial liquid agent. It is a modified version of liquid agent No. 2 with a base modifier added for modification. It is a trifunctional function generating liquid agent, and by increasing the amount of polyorganosiloxane composition, new antibacterial functions are generated in the glass coating film. It has very high transparency. No. 5 is a tetrafunctional + trifunctional additive type liquid agent. It provides flexibility to the cured film while maintaining the robust vitrification reaction of the tetrafunctional components. It has high water repellency and good abrasion resistance. It also has good adhesion to films. The glass-cured and solidified film is rigid. It reacts well with nylon, polyester, and urethane, resulting in good adhesion. It can also prevent the migration of dyes from polyester fibers, etc. No. 6 is a tetrafunctional + trifunctional + acid group modifier additive type liquid agent. It is a liquid agent that exhibits a strong and flat reaction film layer in the glass-cured film. The film is rigid and has very high light transmittance. No. 7 is a liquid agent with adsorption and decomposition functions. It is a tetrafunctional + trifunctional + additive + trace amount of acetic acid. The glass-cured film is strong, but the reaction film has low light transmittance.
[0108] No. 8 is a tetrafunctional liquid agent, and the porous reaction film is a firm, hard glass film. It can be applied to PVC without a primer to form the reaction film. Furthermore, adding a small amount of acetic acid to liquid No. 8 makes the reaction bonds even denser, resulting in improved surface strength. Therefore, improved strength of synthetic fibers can also be expected. Although not shown in the diagram, similar strength improvements were observed in Nos. 1, 2, 5, and 11-14 in Table 1 above, when modifiers such as acetic acid were added compared to those without. No. 9 is a tetrafunctional liquid agent. Adding H2O2 to liquid No. 8 results in a hard film layer, but the surface film layer forms a smooth crystalline structure. No. 10 is a tetrafunctional liquid agent. Adding 0.5-2.0% CH3COOH per total weight to liquid No. 8 preserves the function of titanium dioxide synthesized by reaction with the organometallic titanium catalyst within the solidified coating film. This effect is also observed in bulk flakes. (Photocatalytic titanium dioxide function exhibited) The hardness of the coated and solidified film is maximized. No. 11 is a trifunctional applied liquid agent. By adding an acrylic acid ester copolymer to the side chain, the surface coating of the liquid agent becomes smooth and provides waterproofing and barrier properties. It is also effective as an anchoring agent, and because the reaction film layer is flexible, it can be applied to paper to create paper that can be sewn with a sewing machine. It is also effective as a paper dust inhibitor. A liquid agent mixed with an ultraviolet inhibitor is expected to be an anti-deterioration agent for wood outdoors. No. 12 is a trifunctional + bifunctional additive type liquid agent. By changing the solvent and adding functional agents to the side chain functional groups, the glass solidified product has a moderate hardness and softness and exhibits water repellency, slipperiness, and oil repellency. In addition to the organometallic titanium catalyst, a platinum compound catalyst is also used in this liquid agent. It is expected to be used in woodworking products, paper products, etc. No. 13 is a trifunctional + bifunctional liquid agent. No. 12 has been modified in terms of its formulation ratio to achieve oil resistance, peelability, and superhydrophobicity. It is fluorine-free and environmentally friendly. No. 14 is a trifunctional, solvent-modified liquid agent. The film layer is flexible and has strong water repellency. It is fluorine-free and an environmentally friendly water-repellent agent. No. 15 is a liquid agent consisting of a trifunctional additive + acrylic ester polymer + titanium powder. No. 16 is a liquid agent consisting of a trifunctional additive + acrylic ester polymer + benzenepropanoic acid + titanium powder. It is a liquid agent that can be used to create radiation shielding sheets.This liquid agent reacts with the OH groups on the surface of metal powders to form a porous, soft coating film. It is thought that achieving an effect equivalent to that of liquid agent No. 7 could be possible by doubling the amount of organometallic catalyst and adding acetic acid; therefore, two possible liquid agents are expected to be No. 2 and No. 10.
[0109] Example 17 Next, for No. 7, the coating liquid composition of the present invention was cured and solidified to obtain a solidified body. The effect of the functional material was investigated on this solidified body. Specifically, the data shows the process when the solidified body was placed in a methylene blue solution. Data is also shown for when the liquid agent was applied to paper with a brush, and the cut paper pieces were placed in a methylene blue solution. As a result, the decomposition of the methylene blue pigment was confirmed in both the glass flakes and the coated sheets.
[0110] Figure 2 shows the functionality of the solidified material in one embodiment of the present invention. Figure 2(a) shows a photograph of the solidified material (glass flakes) of the present invention. Figure 2(b) shows the state after immersing 3g of the solidified material of the present invention in 0.00375g of methylene blue / 100g of water (September 27). Figure 2(c) shows the subsequent progress of Figure 2(b) (October 3). The one on the left (with a white lid) was placed by a window, and the one on the right (with a yellow lid) was stored in a locker. Figure 2(d) shows the subsequent progress of Figure 2(b) (October 9). It can be seen that the one on the left has become transparent due to the discoloration of the solution and the solidified material at the bottom due to the effect of sunlight. Figure 2(f) shows the sample from the second test irradiated with sunlight. Figure 2(g) shows that the one on the left has become transparent, while the one on the right has not changed. These results show that the reaction can be further advanced by irradiation with visible light, etc., to exhibit functionality. The sample on the left has become transparent, and decomposition has occurred after adsorption (exhibition of titanium dioxide), while the sample on the right is adsorbed onto the solidified body but exhibits a blue color, so it is judged to be adsorption. It is expected that the sample on the right will also exhibit decomposition function with further light irradiation (exhibition of titanium dioxide). In the retest, glass solidified body No. 7 was used, and in the second retest, paper coated with liquid No. 7 and dried was cut into 5 x 20 cm pieces and placed in a methylene blue solution, and it was found that the decomposition of titanium dioxide functionality had occurred.
[0111] In one embodiment of the present invention, example liquid agent No. 7 has the structure of [Chemical Formula 1], [Chemical Formula 2], etc., and uses trifunctional and tetrafunctional silanes of oreganoalkoxysilanes. When the mixed liquid agent is applied as a coating, the reaction of [Chemical Formula 1] first occurs, forming a glassy thin film on the substrate. Subsequently, it is presumed that the polycondensation reaction of [Chemical Formula 2] occurs. At this time, the adjusting agent CH3COOH etc. added after mixing the liquid agents acts to generate TiO2 in the liquid agent, but the liquid agent maintains transparency, has low viscosity (2cP to 500cP, liquid agent No. 7 is 2cP to 30cP), and possesses new photocatalytic titanium dioxide functions such as decomposability, adsorption, and antibacterial properties. It is stable, easy to use, does not require high-temperature calcination like conventional photocatalytic titanium dioxide powder, contributes to CO2 reduction, and makes it possible to provide a coating agent that is stable, safe, inexpensive, and greatly contributes to the environment. Note that 1) Methylene blue experimental diagram (decomposition function). 2) Diagram of coating experiment on deteriorated tent film (decomposition function) (Figure 3) 3) Adsorption data of KSP, 4) Antibacterial test data on No. 7 liquid coated paper (Kanagawa Prefectural Industrial Technology Research Institute, Tonomachi Branch, Research and Development Department, Practical Application Demonstration Project, Photocatalyst Group, Antibacterial / Antiviral Research Group, Antibacterial Test Laboratory. The test result report of the [Antibacterial Performance Evaluation Test using Bacteria] evaluated it as having "antibacterial effect"). The effects were confirmed, and it was found that all of them exhibited good functions, namely decomposition function, adsorption function, and antibacterial function.
[0112] Figure 3 shows an example of the present invention in one embodiment, applied to a resin used for tents in buildings. Specifically, it shows the effect of sunlight when the coating liquid composition of the present invention is applied. Figure 3(a), labeled "light," is a photograph showing that the brown coating film turns white under visible light after one week. Figure 3(b), labeled "dark," is a photograph showing that the brown film remains brown even after one week of being shielded from light in a dark room. In other words, it turns white after one week of sunlight, but remains unchanged when shielded from light. Although not shown, when applied to a resin film of a tent, it was confirmed by high-magnification electron microscope images that it seals defects in the resin and forms a complete coating. Therefore, it can be seen that pollutants remain on the surface and are removed by the photocatalytic reaction. Conventional photocatalysts coat the resin by supporting titanium dioxide particles so that they do not directly touch the resin, resulting in defects in the titanium layer. The pollutants in the defective areas accumulate without being removed, causing the contamination to spread and the photocatalytic function itself to be lost. However, the present invention can solve these problems.
[0113] Furthermore, a restorative function was observed, which also restored contaminated materials. Specifically, when the composition of the present invention was applied to a tent piece that had deteriorated and turned brown due to prolonged use, and exposed to sunlight for one week, it restored its original white color, sealed minute cracks in the test piece, and completely covered the surface, demonstrating a complete catalytic effect across the entire surface.
[0114] Example 18 Next, a solution was prepared by adding 0.0013% Pt catalyst to the aforementioned (coating solution No. 7) (coating solution No. 17 (=coating solution No. 7 + Pt catalyst)). Except for the use of the Pt catalyst, the weights of each component in coating solution No. 17 were the same as those in coating solution No. 7. The effects of functional materials were investigated on the solidified body obtained by curing and solidifying using the composition of coating solution No. 17 (Figures 4-6).
[0115] <Specimen Preparation> A frosted glass (50-100 mm) was coated with liquid agent No. 17 and dried at 120°C for 1 hour. The coating method involved immersing the frosted glass in a petri dish containing liquid agent No. 17, immediately removing it, and drying it.
[0116] Next, the decomposition performance of the solidified material produced using No. 17 was investigated. The test method used was the JIS R1703-2 wet decomposition performance measurement. Measurements were taken after 3 hours of light irradiation according to the standard, followed by measurements after 24 hours to observe changes over longer periods. Further measurements were taken as needed depending on the results. Photocatalysts have the property of generating strong oxidizing power when exposed to ultraviolet light, decomposing organic matter into carbon dioxide and water. In the JIS photocatalyst test using methylene blue, water containing an organic dye (methylene blue) is brought into contact with a test piece coated with the photocatalyst, and the initial absorbance (degree of light absorption) is measured using a spectrophotometer. The change in absorbance indicates the performance of the photocatalyst. In this case, "bright" refers to the condition under which ultraviolet light from an ultraviolet irradiation reaction system is irradiated. The ultraviolet irradiance on the catalyst surface at this time was 10 W / m². 2 The test specimen is exposed to both ultraviolet light and visible light, so the decomposition of methylene blue occurs due to both types of light, and the amount of decomposition is denoted as A. Since it is necessary to observe the effect of ultraviolet light alone, a dark condition is also required. Darkness is the situation where ultraviolet light is not irradiated, and the photocatalytic action is performed by visible light, causing the methylene blue to decompose. The amount of decomposition is denoted as B. Then, by taking the difference between the two (AB), the amount of decomposition due to the photocatalytic action of ultraviolet light can be measured. The blank (bright) condition is the situation where ultraviolet light is irradiated onto a sample that has not been coated with the photocatalytic agent. This measures the amount of methylene blue decomposition due to ultraviolet light itself, and the amount of decomposition is denoted as C. In the end, the net amount of decomposition by the photocatalytic agent under ultraviolet irradiation is AB minus C, but in reality, the amount of C is small, so it can be evaluated using AB.
[0117] The following samples were used: (1) Ground glass coated with liquid agent No. 17 under light conditions 1 and 2 (light conditions 1 and 2 represent test specimens 1 and 2 under light conditions, respectively), (2) Ground glass coated with liquid agent No. 17 under dark conditions 1 and 2 (dark conditions 1 and 2 represent test specimens 1 and 2 under dark conditions, respectively), and (3) Ground glass under light conditions (blanks 1 and 2 in Figure 4 (test specimens 1 and 2 in the blank)).
[0118] If there is a difference between (1) and (2) above, the effect of light irradiation can be confirmed. In addition, (3) we also checked whether there was any change in methylene blue after prolonged UV irradiation.
[0119] As a result, although a slight decrease in methylene blue concentration was observed even under dark conditions, a significant decrease in methylene blue concentration was found in the solidified material using No. 17 under all light conditions, confirming its decomposition. Thus, it was found that the solidified material using liquid No. 17, which has 0.0013% by weight of Pt catalyst added to liquid No. 7, also exhibits the effects of an excellent functional material.
[0120] Example 19 Furthermore, an adsorption performance test was conducted on the glass flakes obtained using No. 7 as described above. Since methylene blue can be decomposed by photocatalysis, the photocatalytic performance can be evaluated by measuring the decomposition rate under ultraviolet irradiation. This performance is expressed by the decomposition activity index R. If the index is 5 or higher, it is determined to have photocatalytic properties.
[0121] In this experiment, conducted at Kanagawa Science Park (KSP), the sample and methylene blue concentration test conditions were made equivalent to those of a normal photocatalytic decomposition test, but the concentration change of methylene blue was measured in the dark instead of under light irradiation. Specifically, glass flakes made from solution No. 7 were placed in a methylene blue solution of a fixed concentration, and the concentration change of methylene blue was measured in the dark. In this experiment, the methylene blue in the solution is adsorbed onto the glass flakes, and the concentration of methylene blue in the solution decreases. The concentration change is shown in Figure 8. Evaluating the decomposition activity index from this concentration change, a high decomposition activity index of 15.3 nmol / L / min was obtained. This high decomposition index demonstrates the adsorption performance of the glass flakes. In this experiment, the solution becomes clear and the glass flakes turn blue.
[0122] Furthermore, following the manufacturing method described above, the solidified body obtained using liquid agent No. 7 was observed using a transmission electron microscope at the Institute for Solid State Physics, Kashiwa Campus, University of Tokyo, to determine what substance caused the aforementioned photocatalytic properties. Figure 7 shows a micrograph of the solidified body (No. 7) in one embodiment of the present invention. K indicates a magnification of 1,000 times, for example, 300K indicates a magnification of 300,000 times. As a result, nanoparticle dispersion was observed in the micrograph of the solidified body obtained using liquid agent No. 7 according to the present invention, which exhibited photocatalytic function. Crystals of anatase-type titanium dioxide were identified, and although it cannot be confirmed with 100% certainty, it is highly likely that these are titanium dioxide, and it can be inferred that this is what caused the photocatalytic effect.
[0123] The following are the drawbacks of conventional titanium dioxide (photocatalyst) alone (it is a powder): 1) It is ineffective without sunlight (natural) light (ultraviolet light). 2) When applied directly to organic matter, it decomposes the substrate (base), requiring a primer, and repeated application (such as two coats) is time-consuming and costly. 3) When mixed with organic matter, it decomposes the organic matter, so direct mixing of the powder is not possible. 4) Decomposition is not possible unless the powder surface is in contact with the material for a certain period of time, resulting in only a partial effect on the surface.
[0124] Regarding 1) above, it has been found that the functional material (No. 7) of the present invention has the characteristic that adsorption and decomposition by liquid coating are effective even in visible light and that it has adsorption function even in the dark. Regarding 2) above, it has been found that the functional material (No. 7) of the present invention protects against organic decomposition by a siloxane bonding film on the substrate, and the photocatalytic function is sufficiently expressed with a single surface coating, so the cost is low. Regarding 3) above, it has been found that the liquid of the functional material (No. 7) of the present invention is composed of 3 and 4 side-chain functional groups, and even if a functional agent is incorporated into the open part of one of the 3 functional groups, it is not decomposed by the 4-functional bonding film, so it does not affect organic functional products and can be blended. Regarding 4) above, it has been found that the functional material (No. 7) of the present invention is transparent, has low viscosity and good permeability and good drying properties. It has been found that it is highly effective because it forms a penetrating coating film not only on the surface but also in the Z direction. Furthermore, it is possible to create bulk glass from very thin films with this liquid. It is a transparent, glass-solidified material.
[0125] Although the discovery of the liquid titanium dioxide of the present invention is not yet fully understood, it is clear that, unlike conventional photocatalytic titanium dioxide, it is not a "particulate body," can be coated anywhere, possesses similar decomposition performance to titanium dioxide, and can be synthesized as a three-dimensional structure like plastic, making it extremely useful.
[0126] In other words, the functional material of the present invention, taking titanium as an example, differs from conventional powdered photocatalytic titanium dioxide in that it does not require the powder to be attached to the surface with an adhesive, nor does it require the use of an adsorbent underneath. It is a transparent liquid coating agent with photocatalytic titanium dioxide functionality that exhibits both "decomposition performance" and "adsorption performance." Titanium dioxide powder is usually a "white powder" and is a photocatalytic titanium dioxide that cannot exhibit its function unless it is scattered on a surface. On the other hand, the functional material of the present invention is a liquid agent that can be coated and exhibit its function anywhere using siloxane bonding reactive groups, which is significant because it can greatly expand the range of applications for titanium dioxide. [Industrial applicability]
[0127] The silane-based coating liquid composition of the present invention can provide materials with various functionalities at a low cost, and is therefore expected to make a significant contribution to industrial development in a wide range of fields.
Claims
1. The main component is the following chemical formula (1): 【Chemistry 1】 (However, R 1 , R 2 , R 3 and R 4 A silane-based coating liquid composition comprising a compound represented by (where each is the same or different, hydrogen or an alkyl group having 1 to 4 carbon atoms, and n is 2 to 10), a catalyst consisting of a hydrolyzable organometallic compound, a adjusting agent consisting of a weakly acidic catalyst or a basic catalyst, and an organic solvent, The compound is a monomer polycondensate in the case where n is 1 in the chemical formula (1), and is a polycondensate in which the solvent used during the polycondensation of the monomer has been removed. It does not contain reaction water to polycondense the aforementioned compound, The silane-based coating solution composition is characterized in that the hydrolyzable organometallic compound is tetrabutoxytitanium.
2. The silane-based coating liquid composition according to claim 1, characterized in that the adjusting agent is at least one of acetic acid, hydrogen peroxide, and ammonia.
3. The silane-based coating liquid composition according to claim 1 or 2, characterized in that the content of the adjusting agent is 0.5 to 5% by weight.
4. The silane-based coating liquid composition according to any one of claims 1 to 3, characterized in that, during use, the compound undergoes polycondensation via the catalyst made of tetrabutoxytitanium due to moisture in the air and / or hydroxyl groups or moisture contained in the substrate to which the coating liquid composition has been applied.
5. The silane-based coating liquid composition according to claim 4, characterized in that the catalyst comprising tetrabutoxytitanium causes polycondensation of the compound and generates titanium dioxide dispersed in the polycondensate of the compound by hydrolysis of the tetrabutoxytitanium, thereby also exhibiting the function of the titanium dioxide.
6. The silane-based coating liquid composition according to claim 5, characterized in that the catalyst comprising tetrabutoxytitanium exhibits at least one of the functions of titanium oxide: antibacterial function, decomposition function, and adsorption function.
7. The silane-based coating liquid composition according to claim 5 or 6, characterized in that the reaction in which titanium oxide is produced from tetrabutoxytitanium is influenced by the action of the adjusting agent.
8. In addition to the aforementioned main component, the compound represented by the following chemical formula (2) has three hydrolyzable substituents and one non-hydrolyzable substituent: 【Chemistry 2】 (wherein R 5 , R 6 and R 7 may each be the same or different and are each a monomer consisting of hydrogen, an alkyl group or an alkenyl group, and R 5 O, R 6 O and R 7 O and Si form an oligomer composed of siloxane bonds, and R 8 is an alkenyl group or a phenyl group, which may contain an epoxy group or a glycidyl group in its molecule) The silane-based coating liquid composition according to any one of claims 1 to 7, comprising:
9. In addition to the main component mentioned above, the compound represented by the following chemical formula (3) has two hydrolyzable substituents and two non-hydrolyzable substituents: 【Transformation 3】 (However, R 9 and R 11 Each of these may be the same or different, and is a monomer consisting of hydrogen, an alkyl group, or an alkenyl group, R 9 O and R 11 The bond between O and Si is an oligomer consisting of a siloxane bond, R 10 and R 12 The silane-based coating liquid composition according to any one of claims 1 to 8, characterized in that it contains an alkyl group, alkenyl group, or phenyl group, which may contain an epoxy group or a glycidyl group in its molecule.
10. Furthermore, the silane-based coating liquid composition according to any one of claims 1 to 9, characterized in that it further contains an acrylic resin.
11. The main component is the following chemical formula (1): 【Chemistry 4】 (However, R 1 , R 2 , R 3 and R 4 A method for producing a silane-based coating liquid composition comprising a compound represented by (where each is the same or different hydrogen or an alkyl group having 1 to 4 carbon atoms, and n is 2 to 10), a catalyst consisting of a hydrolyzable organometallic compound, a adjusting agent consisting of a weakly acidic catalyst or a basic catalyst, and an organic solvent, A method for producing a silane-based coating liquid composition, comprising the steps of: polycondensing the monomer in the case where n is 1 in the chemical formula (1) in the presence of a solvent; removing the solvent used during the polycondensation of the monomer from the obtained polycondensate by heating and reducing pressure; and mixing the obtained compound with a catalyst consisting of the hydrolyzable organometallic compound, the adjusting agent, and the organic solvent, wherein the hydrolyzable organometallic compound is tetrabutoxytitanium, and no reaction water for hydrolyzing the compound is present.
12. The method for producing a silane-based coating solution composition according to claim 11, characterized in that the adjusting agent is at least one of acetic acid, hydrogen peroxide, and ammonia.
13. A functional material characterized by being obtained by applying a silane-based coating liquid composition according to any one of claims 1 to 10 to a substrate and allowing it to solidify.
14. The functional material according to claim 13, comprising titanium dioxide dispersed in a polycondensate of the compound, which is produced by hydrolysis of a catalyst consisting of tetrabutoxytitanium, and having a function due to the titanium dioxide.
15. The functional material according to claim 14, characterized in that the titanium oxide has at least one of the following functions: antibacterial function, decomposition function, and adsorption function.
16. A method for producing a functional material, comprising the steps of: applying a silane-based coating liquid composition according to any one of claims 1 to 10 to a substrate; polycondensing the compound via a catalyst made of tetrabutoxytitanium using moisture in the air and / or hydroxyl groups or moisture contained in the substrate; and drying the substrate to which the coating liquid composition has been applied.
17. A method for producing a functional material according to claim 16, characterized in that the compound is polycondensed using a catalyst consisting of tetrabutoxytitanium, and titanium dioxide dispersed in the polycondensate of the compound is generated by hydrolysis of the tetrabutoxytitanium, thereby also exhibiting the function of the titanium dioxide.
18. The method for producing a functional material according to claim 17, characterized in that the titanium oxide exhibits at least one of the following functions: antibacterial function, decomposition function, and adsorption function.
19. A coated material obtained by applying a silane-based coating liquid composition according to any one of claims 1 to 10 to a substrate.
20. A solidified body obtained by solidifying the silane-based coating liquid composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Hard coating agent and article formed with hard coating film
JP1996238683A
Film forming composition and preparation thereof
JP1997279096A
Impregnated paper
JP1999315494A
Film-forming composition, manufacture thereof and material for layer insulating film
JP2000256621A
Film-forming composition and insulating film-forming material
JP2001187866A