Method for producing vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups.

The flow synthesis method addresses the inefficiencies in producing vinyl-based and allyl-based polymers with quaternary ammonium groups by enabling continuous production, achieving cost-effective and efficient polymer manufacturing.

JP7954982B1Active Publication Date: 2026-11-24SENKA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2025168615
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-10-06
Publication Date
2026-11-24
Estimated Expiration
2045-10-06

AI Technical Summary

Technical Problem

Existing methods for producing vinyl-based and/or allyl-based polymers and polymers containing quaternary ammonium groups are inefficient and lack a continuous production process.

Method used

A method for continuously producing these polymers using flow synthesis, involving steps such as preparing aqueous solutions of monomers and polymerization initiators, heating and cooling reactor portions, and recovering the polymer, with specific monomers and polymerization regulators used to achieve continuous production.

Benefits of technology

Enables the continuous production of vinyl-based and/or allyl-based polymers and polymers with quaternary ammonium groups in an industrially and economically advantageous manner, allowing for low molecular weight diallylamine-based polymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954982000001
    Figure 0007954982000001
  • Figure 0007954982000002
    Figure 0007954982000002
  • Figure 0007954982000003
    Figure 0007954982000003
Patent Text Reader

Abstract

The object of the present invention is to provide a method for producing new vinyl-based and / or allyl-based polymers, as well as polymers containing quaternary ammonium groups. [Solution] A method for producing vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group. [Background Art]

[0002] Patent Document 1 discloses a method for polymerizing diallylamine and a derivative thereof, in which hypophosphorous acid and / or a salt thereof is used as a polymerization regulator, and a monomer is polymerized to batch-produce a polymer. [Prior Art Document] [Patent Document]

[0003] [Patent Document 1] Japanese Unexamined Patent Publication (Kokai) No. Hei 03-109407 [Summary of the Invention] [Problem to be Solved by the Invention]

[0004] An object of the present invention is to newly provide a method for producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group. [Means for Solving the Problem]

[0005] The present inventors have found a method for continuously producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group by a flow synthesis method. The present invention includes the following method for producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group.

[0006] Item 1. A method for producing a polymer, (1A) including a step of producing a polymer by radical polymerization of a monomer having a vinyl group and / or an allyl group, The step of producing the polymer is (i) A step of preparing an aqueous solution containing the monomer and an aqueous solution containing a polymerization initiator as raw material solutions for polymer production. (ii) A step of supplying the aqueous solution to the polymerization reactor, (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) a step of recovering the manufactured polymer, A manufacturing method for continuously producing polymers by flow synthesis.

[0007] Section 2. The manufacturing method according to item 1, wherein step (i) comprises preparing an aqueous solution containing a polymerization regulator as a raw material solution for the polymer production.

[0008] Section 3. The monomer is at least one monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC), diallylamine salts, (meth)acrylamide, (meth)acrylic acid and / or salts thereof, and (meth)acrylate. The manufacturing method according to item 1, wherein a polymer is continuously produced by flow synthesis using at least one of the monomers or a combination of two or more of the monomers.

[0009] Section 4. A method for producing a polymer, (1B) The process includes a step of producing a polymer by addition polymerization using a secondary amine and an epihalohydrin as essential components. The process for manufacturing the polymer is: (i) A step of preparing a mixed aqueous solution of raw materials containing the essential components as a raw material solution for polymer production, (ii) A step of supplying the aqueous solution to the polymerization reactor, (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) a step of recovering the manufactured polymer, A production method for continuously producing a polymer by flow synthesis.

[0010] Item 5. The secondary amine is dimethylamine, The epihalohydrin is epichlorohydrin, The production method according to Item 4, wherein the polymer is continuously produced by flow synthesis.

[0011] Item 6. A method for producing a polymer, comprising: (2) A step of exchanging all or part of chloride ions of a polymer containing quaternary ammonium groups with hydroxide ions, A production method for producing a polymer containing quaternary ammonium hydroxide groups.

[0012] Item 7. The production method according to Item 6, wherein the polymer containing quaternary ammonium groups is a polymer produced by the production method according to Item 1 or 4.

[0013] Item 8. The production method according to Item 6, wherein the polymer containing quaternary ammonium groups is a polymer produced using a monomer containing DADMAC, and a polymer containing diallyldimethylammonium hydroxide groups is produced.

[0014] Item 9. The polymer containing quaternary ammonium groups is a polymer produced using a monomer containing dimethylamine and epichlorohydrin, The production method according to Item 6, wherein a polymer is produced in which the counter ion of the quaternary ammonium group of the dimethylamine / epichlorohydrin addition polymer is a hydroxide ion.

[0015] Item 10. The production method according to Item 6, wherein the step (2) of exchanging all or part of chloride ions of a polymer containing quaternary ammonium groups with hydroxide ions is an electrodialysis method using an ion exchange membrane or an ion exchange method using an ion exchange resin.

[0016] Claim 11. A method for producing a polymer, (3) comprising a step of neutralizing the polymer of claim 6 using at least one acid selected from the group consisting of inorganic acids (provided that the inorganic acid excludes hydrochloric acid) and organic acids, The production method for producing a diallyldimethylammonium salt polymer or a dimethylamine / epichlorohydrin addition polymer having a counterion other than chloride ion.

[0017] The method for producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group according to the present invention can continuously produce a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group by a flow synthesis method.

[0018] The present invention can produce a low molecular weight diallylamine-based polymer sufficiently advantageously from an industrial and economical perspective. [Effects of the Invention]

[0019] The present invention can newly provide a method for producing a vinyl-based and / or allyl-based polymer and a polymer containing a quaternary ammonium group. [Brief Description of the Drawings]

[0020] [Figure 1] Figure 1 is a diagram illustrating the flow device of the present invention. The heating bath A of the flow device is heated. An aqueous monomer solution, a polymerization regulator, a polymerization initiator, and the like are sequentially charged into the container A. The mixed aqueous solution of the monomer, polymerization regulator, polymerization initiator, and the like in the container A is flowed into the heating bath A. The reaction product that has passed through the cooling bath from the heating bath A is collected (collection container). [Figure 2]Figure 2 illustrates the flow apparatus of the present invention. The heating baths A and B of the flow apparatus are heated. A monomer aqueous solution is placed in container A. A polymerization initiator is placed in container B. The monomer aqueous solution in container A and the initiator aqueous solution in container B are flowed into heating bath A, and the reaction product that has passed through heating bath B and the cooling bath is collected (collection container). [Figure 3] Figure 3 illustrates the flow apparatus of the present invention. The heating baths A and B of the flow apparatus are heated. A polymerization initiator is placed in container A. A polymerization regulator is placed in container B. An aqueous monomer solution is placed in container C. The aqueous polymerization initiator solution in container A, the aqueous polymerization regulator solution in container B, and the aqueous monomer solution in container C are flowed into heating bath A, and the reaction products that have passed through heating bath B and the cooling bath are recovered (recovery container). The present invention is not limited to Figures 1-3 when producing polymers, and for example, it is also possible to add a container and a static mixer after heating bath A. [Figure 4] Figure 4 is a diagram illustrating an electrodialysis machine. A polymer aqueous solution is placed in tank A of the electrodialysis machine. A sodium sulfate aqueous solution is placed in tank B. A sodium hydroxide aqueous solution is placed in tank C. Pumps A, B, and C are operated at predetermined voltage and current settings, and dialysis is started in a dialysis machine equipped with an anion exchange membrane. The chloride ion concentration is measured using the mercury thiocyanate method. [Modes for carrying out the invention]

[0021] The present invention will be described in detail below. The embodiments illustrating the present invention are for the purpose of providing a better understanding of the spirit of the invention and do not limit the scope of the invention unless otherwise specified.

[0022] In this specification, "contains" and "include" are concepts that encompass all of "comprise," "consist essentially of," and "consist of."

[0023] In this specification, when a numerical range is indicated as "A to B", it means "greater than or equal to A and less than or equal to B".

[0024] In this specification, when expressions such as parts and percentages are used, they generally represent parts by mass, parts by weight, mass%, or weight.

[0025] [1] Methods for producing vinyl-based and / or allyl-based polymers and polymers containing quaternary ammonium groups The present invention includes methods for producing the following vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups.

[0026] Process (1A) (Radical polymerization) The present invention provides a method for producing a polymer, which includes the step of producing a polymer by radical polymerization of a monomer having a vinyl group and / or an allyl group (1A).

[0027] In the polymer manufacturing method of the present invention, the step of manufacturing the polymer is: (i) A step of preparing an aqueous solution containing a monomer and an aqueous solution containing a polymerization initiator as raw material solutions for polymer production. (ii) A step of supplying an aqueous solution to a radical polymerization reactor, (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) a step of recovering the manufactured polymer, Polymers are continuously produced by flow synthesis.

[0028] The present invention provides a method for producing vinyl-based and / or allyl-based polymers by flow synthesis, which allows for the continuous production of vinyl-based and / or allyl-based polymers, and enables the production of low molecular weight diallylamine-based polymers in an industrially and economically advantageous manner.

[0029] The polymer production method of the present invention includes the step of producing a polymer by radical polymerization of a monomer having a vinyl group and / or an allyl group. The monomer is preferably at least one monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC), diallylamine salts, (meth)acrylamide, (meth)acrylic acid and / or salts thereof, and (meth)acrylate.

[0030] The present invention provides a method for producing vinyl-based and / or allyl-based polymers, in which monomers may be used individually or mixed (blended) with two or more monomers, and the polymers are continuously produced by flow synthesis.

[0031] Radical polymerization is carried out using common production conditions for diallylamine-based polymers.

[0032] The concentration of the monomer depends on the cooling capacity of the polymer manufacturing apparatus. From an economic standpoint, the concentration of the monomer in the monomer aqueous solution is preferably adjusted to 10% by mass or more and about 55% by mass.

[0033] The polymerization initiator can be a radical polymerization initiator commonly used in the production of diallylamine-based polymers.

[0034] The polymerization initiator (radical polymerization initiator) is preferably a water-soluble organic or inorganic peroxide such as hydrogen peroxide, ammonium persulfate (APS, ammonium peroxodisulfate), potassium persulfate (potassium peroxodisulfate), t-butyl hydroperoxide, or cumene hydroperoxide. The polymerization initiator may be a water-soluble organic or inorganic peroxide used alone, or a mixture (blend) of two or more types.

[0035] Preferably, the polymerization initiator is a water-soluble azo compound (azo polymerization initiator) such as 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis(2-amidinobutane)dihydrochloride, 2,2'-azobis(N-phenylamidinopropane)dihydrochloride, 2,2'-azobis(N,N-dimethylamidinopropane)dihydrochloride, 2,2'-azobis(N-hydroxyethylamidinopropane)dihydrochloride, 2,2'-azobis(2-imidazolinylpropane)dihydrochloride, azobisvaleronitrile, or 2,2'-azobis(2-methylpropionamidine)dihydrochloride. The polymerization initiator may be a single water-soluble azo compound or a mixture (blend) of two or more.

[0036] (i) The step includes preparing an aqueous solution, preferably containing a polymerization regulator, as a raw material solution for polymer production.

[0037] Radical polymerization is preferably carried out in the presence of a polymerization regulator. The polymerization regulator is preferably a sulfur compound or a phosphoric acid compound. More preferably, the polymerization regulator is hypophosphorous acid (H3PO2) and / or its salt, methallyl sulfonic acid and / or its salt. As hypophosphorous acid and methallyl sulfonic acid, preferably free acids, salts of Na, Li, K, NH4, amines, etc., or hydrates of these salts are used. Radical polymerization may be carried out using one polymerization regulator alone or by mixing (blending) two or more types.

[0038] The polymerization regulator is used while adjusting the polymerization rate and polymerization state of the monomer, and the concentration used is generally adjusted considering economic efficiency and ease of control of the polymerization reaction. The amount of polymerization regulator used is adjusted arbitrarily depending on the desired degree of polymerization, and usually, an amount of 0.3% to 4% by mass relative to the total amount charged is sufficient to achieve the desired effect. In the monomer aqueous solution, water is used as the reaction solvent, the monomer concentration is 5% to 65% by mass, and the polymerization regulator is preferably used at an amount of 0.3% to 4% by mass relative to the total amount charged.

[0039] Radical polymerization is carried out by applying general production conditions for diallylamine polymers, adjusting the reaction temperature, reaction time, and pH during the reaction. The reaction temperature is preferably between 50°C and 80°C. The reaction time is preferably 30 minutes or more to complete the polymerization.

[0040] Process (1B) (Addition polymerization) The present invention provides a method for producing polymers, which includes a step of producing a polymer by addition polymerization using (1B) a secondary amine and an epihalohydrin as essential components.

[0041] In the polymer production method of the present invention, the step of producing the polymer is: (i) preparing a mixed aqueous solution of raw materials containing essential components (secondary amine and epihalohydrin) as a raw material solution for polymer production; (ii) A step of supplying an aqueous solution to the polymerization reactor, (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) a step of recovering the manufactured polymer, Polymers are continuously produced by flow synthesis.

[0042] The present invention provides a method for producing an addition polymerization polymer of a secondary amine and an epihalohydrin by flow synthesis, which allows for the continuous production of the addition polymerization polymer of a secondary amine and an epihalohydrin, and is industrially and economically advantageous.

[0043] The present invention provides a method for producing a polymer, which includes the step of producing a polymer by addition polymerization using (1B) a secondary amine and an epihalohydrin as essential components.

[0044] The polymer is produced by addition polymerization using (a) a secondary amine and (b) an epihalohydrin as essential components. The monomer (a) secondary amine is preferably a secondary amine such as dimethylamine, diethylamine, methylethylamine, methylpropylamine, methylbutylamine, piperidine, pyrrole, or carbazole. The monomer (b) epihalohydrin is preferably an epihalohydrin such as epichlorohydrin, epiiodohydrin, or epibromohydrin.

[0045] The monomer may be (a) a secondary amine, used alone or as a mixture (blend) of two or more. The monomer may be (b) an epihalohydrin, used alone or as a mixture (blend) of two or more. The monomer is preferably dimethylamine and epichlorohydrin, and the polymer is continuously produced by addition polymerization via flow synthesis.

[0046] Process (i) In the polymer production method of the present invention, the steps for producing the polymer (step (1A, radical polymerization) and step (1B, addition polymerization) include (i) preparing an aqueous solution containing a monomer and / or an aqueous solution containing a polymerization initiator as a raw material solution for polymer production, and additionally, an aqueous solution containing a polymerization modifier.

[0047] The aqueous solution may contain a polar organic solvent. Preferred polar organic solvents are methanol, ethanol, 1-propanol, 2-propanol, ethylene glycol, diethylene glycol, and butylene glycol. The aqueous solution may use one polar organic solvent alone, or two or more may be mixed (blended). The polar organic solvent may be contained in the aqueous solution in any proportion, for example, about 1% to 10% by volume.

[0048] (Radical polymerization) (i) The step preferably includes preparing an aqueous solution containing a polymerization regulator as a raw material solution for polymer production. The step preferably involves sequentially charging and mixing an aqueous monomer solution (such as DADMAC), water, a polymerization regulator (such as sodium hypophosphite), and a polymerization initiator (such as ammonium persulfate) into container A of a flow apparatus (Figure 1). The step preferably involves sequentially charging and mixing an aqueous monomer solution (such as DADMAC, acrylic acid, etc.), an aqueous sodium hydroxide solution, water, and a polymerization initiator (such as V-50) into container A of a flow apparatus (Figure 1).

[0049] Step (i) preferably involves neutralizing and mixing a monomer (such as diallylamine) and hydrochloric acid in container A of the flow apparatus (Figure 2) (maintaining the temperature below 30°C). Then, a monomer (such as acrylamide) is stirred and mixed into container A. In container B of the flow apparatus, water and a polymerization initiator (such as ammonium persulfate) are mixed and dissolved.

[0050] Step (i) preferably involves mixing and dissolving a polymerization initiator (such as ammonium persulfate) and water in container A of the flow apparatus (Figure 3). Mixing and dissolving a polymerization regulator (such as sodium hypophosphite) and water in container B of the flow apparatus. Charging an aqueous solution containing a monomer (such as DADMAC) into container C of the flow apparatus.

[0051] (Addition polymerization) In step (i), preferably, monomers (dimethylamine, epichlorohydrin, etc.), water, ammonia water, and a pH adjuster (hydrochloric acid, etc.) are sequentially added to container A of the flow apparatus (Figure 1) while controlling the temperature.

[0052] Process (ii) In the polymer production method of the present invention, the steps for producing the polymer (step (1A, radical polymerization) and step (1B, addition polymerization)) include (ii) the step of supplying an aqueous solution to the polymerization reactor.

[0053] (Radical polymerization) In step (ii), preferably, the monomer / polymerization regulator / polymerization initiator mixed aqueous solution (flow rate: about 5.0 ml / min) from container A of the flow apparatus (Figure 1) is flowed into the heating bath A (polymerization reactor, also simply referred to as the reactor). In step (ii), preferably, the monomer / polymerization initiator mixed aqueous solution (flow rate: about 10.0 ml / min) from container A of the flow apparatus (Figure 1) is flowed into the heating bath A (reactor).

[0054] In step (ii), preferably, the monomer aqueous solution in container A of the flow apparatus (Figure 2) (flow rate: approximately 180 ml / min) and the polymerization initiator aqueous solution in container B (flow rate: approximately 120 ml / min) are flowed into the heating bath A (reactor). Preferably, they are passed through a static mixer.

[0055] In step (ii), preferably, the polymerization initiator aqueous solution in container A of the flow apparatus (Figure 3) (flow rate: approximately 80 ml / min), the polymerization regulator aqueous solution in container B (flow rate: approximately 60 ml / min), and the monomer aqueous solution in container C (flow rate: approximately 260 ml / min) are flowed into the heating bath A (reactor). Preferably, they are passed through a static mixer.

[0056] (Addition polymerization) In step (ii), preferably, the monomer / ammonia water / pH adjusting agent mixed aqueous solution (flow rate: approximately 5.0 ml / min) from container A of the flow apparatus (Figure 1) is flowed into the heating bath A (reactor).

[0057] Process (iii) In the polymer production method of the present invention, the steps for producing the polymer (step (1A, radical polymerization) and step (1B, addition polymerization)) include (iii) a step of heating the reaction vessel portion of the reactor.

[0058] Step (iii) preferably involves raising the temperature of the heating bath A (reactor) of the flow apparatus (Figure 1) to 70°C or higher.

[0059] Step (iii) preferably involves raising the temperature of heating bath A (reactor, approximately 55°C) and heating bath B (reactor, approximately 70°C) of the flow apparatus (Figure 2).

[0060] Step (iii) preferably involves raising the temperature of heating bath A (reactor, approximately 70°C) and heating bath B (reactor, approximately 87°C) of the flow apparatus (Figure 3).

[0061] The process is (iv) In the polymer production method of the present invention, the steps for producing the polymer (step (1A, radical polymerization) and step (1B, addition polymerization)) include (iv) a step of cooling the cooling bath portion of the reactor.

[0062] Process (v) In the polymer production method of the present invention, the steps for producing the polymer (step (1A, radical polymerization) and step (1B, addition polymerization)) include (v) a step of recovering the produced polymer.

[0063] After the flow synthesis has started (preferably 60 to 150 minutes after the start of flow), the reaction products discharged from the cooling bath (polymers, DADMAC polymers, DADMAC / sodium acrylate copolymers, diallylamine hydrochloride / acrylamide copolymers, dimethylamine / epichlorohydrin, etc.) are continuously collected (in a collection container) for at least 30 minutes.

[0064] The obtained polymers (DADMAC polymers, DADMAC / sodium acrylate copolymers, diallylamine hydrochloride / acrylamide copolymers, dimethylamine / epichlorohydrin, etc.) are subjected to GPC (gel permeation chromatography) to determine their weight-average molecular weight (Mw) in PEG terms.

[0065] In the polymer production method of the present invention, the polymer production steps (steps (1A) and (1B)) include steps (i), (ii), (iii), (iv), and (v), and the polymer is continuously produced by flow synthesis. The method for producing vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups, of the present invention allows for the continuous production of vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups, by flow synthesis, in an industrially and economically advantageous manner.

[0066] [2] Ion exchange method for vinyl-based and / or allyl-based polymers and polymers containing quaternary ammonium groups The present invention encompasses methods for ion exchange of the following vinyl-based and / or allyl-based polymers, and polymers containing quaternary ammonium groups.

[0067] Process (2) The present invention provides a method for producing a polymer, comprising (2) a step of replacing all or part of the chloride ions of a polymer containing a quaternary ammonium group with hydroxide ions, thereby producing a polymer containing a quaternary ammonium hydroxide group. The monomer preferably contains DADMAC.

[0068] (2) The step of exchanging all or part of the chloride ions of the polymer containing quaternary ammonium groups for hydroxide ions (ion exchange method) is preferably an electrodialysis method using an ion exchange membrane or an ion exchange method using an ion exchange resin.

[0069] The polymers containing quaternary ammonium groups are preferably (1A) polymers produced by a process of radical polymerization of monomers having vinyl groups and / or allyl groups, or (1B) polymers produced by an addition polymerization process using a secondary amine and an epihalohydrin as essential components.

[0070] The polymer production method of the present invention produces a polymer containing a diallyldimethylammonium hydroxide group, preferably a polymer produced using a monomer containing DADMAC.

[0071] The present invention provides a polymer production method in which a polymer containing a quaternary ammonium group is produced using a monomer containing dimethylamine and epichlorohydrin, and the counterion of the quaternary ammonium group of the dimethylamine / epichlorohydrin addition polymer is a hydroxide ion.

[0072] Electrodialysis of polymers (such as DADMAC polymers) is performed using an electrodialysis apparatus (Figure 4). The prepared aqueous solution of polymers (such as DADMAC polymers) is placed in tank A, preferably an aqueous sodium sulfate solution in tank B, and preferably an aqueous sodium hydroxide solution in tank C. Using the electrodialysis apparatus, the voltage and current are set to the predetermined values, and pumps A, B, and C (Figure 4) are operated to start dialysis.

[0073] After dialysis is complete, the chloride ion concentration of the polymer (DADMAC polymer, etc.) is measured using the mercury thiocyanate method, and the ion exchange rate is calculated.

[0074] [3] Method for producing diallyldimethylammonium salt polymers in which the counterion is not a chloride ion The present invention includes a method for producing diallyldimethylammonium salt polymers in which the following counterions are other than chloride ions.

[0075] Process (3) The present invention provides a method for producing a polymer, comprising the step of neutralizing the polymer (diallyldimethylammonium hydroxide polymer) prepared in the step of (3)(2) exchanging chloride ions for hydroxide ions using at least one acid selected from the group consisting of inorganic acids (except hydrochloric acid) and organic acids (preferably acetic acid), thereby producing a diallyldimethylammonium salt polymer whose counterion is not a chloride ion.

[0076] An aqueous solution of a polymer (diallyldimethylammonium hydroxide polymer) prepared in a process of exchanging chloride ions for hydroxide ions is placed in a container (such as a 500 ml container) equipped with a thermometer and a stirring device, and an organic acid such as acetic acid is added while stirring. [Examples]

[0077] The present invention will be specifically described below with reference to examples and reference examples.

[0078] The present invention is not limited to the following specific embodiments. The present invention is not limited to Figures 1-3 when producing polymers, and for example, it is also possible to add a container and a static mixer after the heating bath A.

[0079] <Polymer manufacturing> (Example 1) Flow synthesis of low molecular weight (11-12-mer) DADMAC polymers

[0080] (DADMAC: Diallyldimethylammonium chloride) The heating bath A of the flow apparatus (Figure 1) is heated to 85°C.

[0081] In container A, sequentially add 1.00 kg of 65% DADMAC (monomer) aqueous solution, 1.60 kg of water, 0.30 kg of sodium hypophosphite (polymerization regulator), and 0.10 kg of ammonium persulfate (polymerization initiator).

[0082] The monomer / polymerization regulator / polymerization initiator aqueous solution from container A is flowed into heating bath A at a flow rate of 5.0 ml / min, and then into a cooling bath.

[0083] 90 minutes after the start of the flow, the discharged reaction products were continuously collected over a period of 7 hours (collection container).

[0084] The obtained DADMAC polymer was subjected to GPC (gel permeation chromatography), and its weight-average molecular weight (Mw) in PEG terms was determined to be 1,900.

[0085] (Comparative Example 1) Batch manufacturing of Example 1 In a 1000 ml container equipped with a thermometer and a stirring device, add 0.33 kg of 65% DADMAC (monomer) aqueous solution, 0.10 kg of sodium hypophosphite (polymerization regulator), and 0.42 kg of water, and heat to 85°C while stirring.

[0086] After raising the temperature, 0.15 kg of a 20% ammonium persulfate (polymerization initiator) aqueous solution was added and the reaction was carried out.

[0087] Ten seconds after addition, the internal liquid temperature reached 95°C, and cooling was insufficient. Therefore, ice water was added to the container to lower the internal liquid temperature to below 40°C and stop the reaction.

[0088] (Example 2) Flow synthesis of DADMAC / sodium acrylate copolymer The heating bath A of the flow apparatus (Figure 1) is heated to 65°C.

[0089] In container A, sequentially add and mix 0.27 kg of 65% DADMAC (monomer) aqueous solution, 0.50 kg of 80% acrylic acid (monomer) aqueous solution, 0.05 kg of 48% sodium hydroxide aqueous solution, 0.01 kg of V-50 (polymerization initiator), and 0.12 kg of water.

[0090] The monomer / polymerization initiator aqueous solution from container A is flowed into heating bath A at a flow rate of 10.0 ml / min, and then into a cooling bath.

[0091] 100 minutes after the start of the flow, the discharged reaction products were continuously collected over the course of one hour (collection container).

[0092] The obtained DADMAC / sodium acrylate copolymer was subjected to GPC to determine its weight-average molecular weight in PEG terms, which was found to be Mw: 218,300.

[0093] (Example 3) Flow synthesis of diallylamine hydrochloride / acrylamide copolymer The heating bath A of the flow apparatus (Figure 2) is heated to 55°C, and the heating bath B is heated to 70°C.

[0094] In container A, neutralize and mix 10.00 kg of diallylamine (monomer) with 11.00 kg of 35% hydrochloric acid while maintaining the temperature below 30°C. Then, stir and mix in 1.00 kg of 50% acrylamide (monomer). In container B, mix 20.00 kg of water with 1.00 kg of ammonium persulfate (polymerization initiator) and dissolve.

[0095] The monomer aqueous solution in container A and the polymerization initiator aqueous solution in container B are passed through a static mixer to heating bath A at a flow rate of 180 ml / min and 120 ml / min, respectively. Then they are passed to heating bath B, and then to a cooling bath.

[0096] 100 minutes after the start of the flow, the discharged reaction products were continuously collected over a period of 2 hours (collection container).

[0097] The weight-average molecular weight (Mw) of the obtained diallylamine hydrochloride / acrylamide copolymer was determined by GPC (Gross Propagation) to be 20,300.

[0098] (Example 4) Flow synthesis of DADMAC polymer The heating bath A of the flow apparatus (Figure 3) is heated to 70°C, and the heating bath B is heated to 87°C.

[0099] Mix 2.00 kg of ammonium persulfate (polymerization initiator) and 30.00 kg of water in container A and dissolve. Mix 1.00 kg of sodium hypophosphite (polymerization regulator) and 30.00 kg of water in container B and dissolve. Add 150.00 kg of 65% DADMAC (monomer) aqueous solution to container C.

[0100] The polymerization initiator aqueous solution in container A is flowed at a flow rate of 80 ml / min, the polymerization regulator aqueous solution in container B at a flow rate of 60 ml / min, and the monomer aqueous solution in container C at a flow rate of 260 ml / min. These solutions are then passed through a static mixer to heating bath A. Next, they are passed to heating bath B, and then to a cooling bath.

[0101] 100 minutes after the start of the flow, the discharged reaction products were continuously collected over an 8-hour period (collection container).

[0102] The weight-average molecular weight of the obtained DADMAC polymer, calculated in PEG terms using GPC, was found to be Mw: 23,500.

[0103] (Example 5) Dimethylamine / epichlorohydrin addition polymer The heating bath A of the flow apparatus (Figure 1) is heated to 70°C.

[0104] In container A, add 0.36 kg of 50% dimethylamine aqueous solution, 0.01 kg of 25% ammonia water, 0.22 kg of water, 0.38 kg of epichlorohydrin, and 0.03 kg of 35% hydrochloric acid, adjusting the temperature to below 25°C.

[0105] The monomer aqueous solution from container A was flowed into heating bath A at a flow rate of 5.0 ml / min, and then into a cooling bath. After 120 minutes from the start of flow, the discharged reaction product was continuously collected over 1 hour (collection container).

[0106] The weight-average molecular weight (Mw) of the obtained dimethylamine / epichlorohydrin addition polymer was determined by GPC (Gross Propagation) and was found to be 5,200.

[0107] <Polymer electrodialysis> (Example 6) Electrodialysis of low molecular weight (11-12-mer) DADMAC polymers In tank A of the electrodialysis machine (Figure 4), 1.50 kg of a 15% aqueous solution of DADMAC polymer prepared in Example 1 (chloride ion concentration: 6.00 g / L) is placed. In tank B, 1.50 kg of a 2% aqueous solution of sodium sulfate is placed. In tank C, 20.00 kg of a 24% aqueous solution of sodium hydroxide is placed.

[0108] Pumps A, B, and C were set to the predetermined voltage and current, and dialysis was started in a dialysis cell equipped with an anion exchange membrane.

[0109] After 30 minutes, the chloride ion concentration was measured using the mercury thiocyanate method and found to be 0.12 g / L, yielding 2.21 kg of a 10% aqueous solution of the polymer with an ion exchange rate of 97.0%.

[0110] (Example 7) Electrodialysis of addition polymerization polymer In tank A of the electrodialysis machine (Figure 4), 1.50 kg of a 30% aqueous solution of dimethylamine / epichlorohydrin addition polymer prepared in Example 5 (chloride ion concentration: 15.00 g / L) is charged. In tank B, 1.50 kg of a 2% aqueous solution of sodium sulfate is charged. In tank C, 20.00 kg of a 24% aqueous solution of sodium hydroxide is charged.

[0111] Pumps A, B, and C were set to the predetermined voltage and current, and dialysis was started in a dialysis cell equipped with an anion exchange membrane.

[0112] After 30 minutes, the chloride ion concentration was measured by the mercury thiocyanate method and found to be 0.30 g / L, yielding 2.19 kg of a 20% aqueous solution of the addition polymer with an ion exchange rate of 97.0%.

[0113] (Example 8) Ion exchange using DADMAC polymer anion exchange resin A glass column (30 mm inner diameter) is packed in the following order: cotton wool, and 20 g of anion exchange resin whose counterion is hydroxide ions.

[0114] Next, 100 g of a 15% aqueous solution of DADMAC polymer prepared in Example 1 (chloride ion concentration: 6.00 g / L) was added, and the aqueous solution that passed through the resin was collected. The collected aqueous solution was passed through the column again, and the aqueous solution that passed through the resin was collected again.

[0115] The chloride ion concentration of the recovered aqueous solution was measured using the mercury thiocyanate method and found to be 0.13 g / L, yielding 147 g of a 10% aqueous solution of the polymer with an ion exchange rate of 96.8%.

[0116] (Example 9) Ion exchange using anion exchange resin of addition polymerization polymer A glass column (30 mm inner diameter) is packed in the following order: cotton wool, followed by 20 g of anion exchange resin whose counterion is hydroxide ions.

[0117] To this, 100 g of a 30% aqueous solution of the dimethylamine / epichlorohydrin addition polymer prepared in Example 5 (chloride ion concentration: 15.00 g / L) was added, and the aqueous solution that passed through the resin was collected. The collected aqueous solution was passed through the column again, and the aqueous solution that passed through the resin was collected again.

[0118] The chloride ion concentration of the recovered aqueous solution was measured using the mercury thiocyanate method and found to be 0.24 g / L, yielding 146 g of a 20% aqueous solution of the addition polymer with an ion exchange rate of 97.8%.

[0119] (Example 10) Production of diallyldimethylammonium salt polymers in which the counterion is not a chloride ion. 0.20 kg of the diallyldimethylammonium hydroxide polymer aqueous solution prepared in Example 6 was charged into a 500 ml coruben equipped with a thermometer and a stirring device, and 0.30 kg of 90% acetic acid was gradually added while stirring.

[0120] The weight-average molecular weight of the obtained neutralized product, calculated using GPC (Gross Propagation), was found to be 1,900.

[0121] (Example 11) Production of an addition polymerization polymer in which the counterion is not a chloride ion. In a 500 ml container equipped with a thermometer and a stirring device, 0.20 kg of an aqueous solution of the polymer prepared in Example 7, in which the counterion of the quaternary ammonium group of the dimethylamine / epichlorohydrin addition polymer is a hydroxide ion, was charged, and 0.30 kg of 90% acetic acid was gradually added while stirring.

[0122] The weight-average molecular weight of the obtained neutralized product, calculated using GPC (Gross Propagation), was found to be 5,100. [Industrial applicability]

[0123] The present invention provides a method for producing vinyl-based and / or allyl-based polymers, as well as polymers containing quaternary ammonium groups, by flow synthesis. This method allows for the continuous production of vinyl-based and / or allyl-based polymers, as well as polymers containing quaternary ammonium groups, and enables the production of low molecular weight diallylamine-based polymers in an industrially and economically advantageous manner.

Claims

1. A method for producing a polymer, (1) A process comprising the step of radical polymerization of a monomer having a vinyl group and / or an allyl group to produce a polymer containing a quaternary ammonium group, The process for manufacturing the polymer is: (i) A step of preparing an aqueous solution containing the monomer and an aqueous solution containing a polymerization initiator as raw material solutions for polymer production. (ii) A step of supplying the aqueous solution to a polymerization reactor having a structure in which the liquid flows in one direction from upstream to downstream of the flow, (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) The process includes a step of recovering the manufactured polymer, wherein the radical polymerization is carried out at a reaction temperature of 50°C or higher and 87°C or lower for 30 minutes or more. Polymers are continuously produced by flow synthesis. After step (1) above, (2) A step of replacing all or part of the chloride ions of the polymer containing the quaternary ammonium group with hydroxide ions, To produce a polymer containing a quaternary ammonium hydroxide group, Manufacturing method.

2. The manufacturing method according to claim 1, wherein step (i) comprises preparing an aqueous solution containing a polymerization regulator as a raw material solution for the polymer production.

3. The manufacturing method according to claim 2, wherein the amount of polymerization regulator used is 0.3% by mass or more and 4% by mass or less of the total amount of ingredients.

4. The monomer is at least one monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC), diallylamine salts, (meth)acrylamide, (meth)acrylic acid and / or salts thereof, and (meth)acrylate. The manufacturing method according to claim 1, wherein a polymer is continuously produced by flow synthesis using at least one of the monomers or a combination of two or more of the monomers.

5. The polymer containing the quaternary ammonium group is a polymer produced using a monomer containing DADMAC, and the method for producing a polymer containing a diallyldimethylammonium hydroxide group is as described in claim 1.

6. The manufacturing method according to claim 1, wherein the step of replacing all or part of the chloride ions of the polymer containing the quaternary ammonium group with hydroxide ions is an electrodialysis method using an ion exchange membrane or an ion exchange method using an ion exchange resin.

7. A method for producing a polymer, After step (2) described in claim 1, (3) The process includes a step of neutralizing the polymer with at least one acid selected from the group consisting of inorganic acids (except hydrochloric acid) and organic acids, A method for producing diallyldimethylammonium salt polymers in which the counterion is not a chloride ion.

8. A method for producing a polymer, (1) A process comprising the step of producing a polymer by radical polymerization of a monomer having a vinyl group and / or an allyl group, wherein the monomer includes at least one monomer having an allyl group, The process for manufacturing the polymer is: (i) A step of preparing an aqueous solution containing the monomer and an aqueous solution containing a polymerization initiator as raw material solutions for polymer production. (ii) A step of supplying the aqueous solution to a polymerization reactor having a structure in which the liquid flows in one direction from upstream to downstream at a flow rate of 5.0 ml / min, 10.0 ml / min, 60 ml / min, 80 ml / min, 120 ml / min, 180 ml / min, or 260 ml / min. (iii) A step of heating the reaction vessel portion of the reactor, (iv) A step of cooling the cooling tank portion of the reactor, (v) The process includes a step of recovering the manufactured polymer at a flow rate of 5.0 ml / min, 10.0 ml / min, 300 ml / min, or 400 ml / min, and carrying out the radical polymerization at a reaction temperature of 50°C or higher and 87°C or lower for 30 minutes or more. A manufacturing method for continuously producing polymers by flow synthesis.

9. The manufacturing method according to claim 8, wherein step (i) comprises preparing an aqueous solution containing a polymerization regulator as a raw material solution for the polymer production.

10. The manufacturing method according to claim 9, wherein the amount of polymerization regulator used is 0.3% by mass or more and 4% by mass or less of the total amount of ingredients.

11. The monomer is at least one monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC), diallylamine salts, (meth)acrylamide, (meth)acrylic acid and / or salts thereof, and (meth)acrylate. When two or more monomers are combined, the combination includes at least one monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC) and diallylamine salts, and further includes a monomer selected from the group consisting of diallyldimethylammonium chloride (DADMAC), diallylamine salts, (meth)acrylamide, (meth)acrylic acid and / or salts thereof, and (meth)acrylate. The manufacturing method according to claim 8, wherein a polymer is continuously produced by flow synthesis using at least one of the monomers or a combination of two or more of the monomers.

Citation Information

Patent Citations

  • Method for polymerizing diallylamine and derivative thereof

    JP1991109407A

  • Preparation of block copolymer

    JP2010180353A

  • Method of producing emulsion dispersion

    JP2015071772A

  • Continuous process for the production of hyperbranched polymers based on c3-c8 monoethylenically unsaturated mono- or dicarboxylic acids or their anhydrides and salts

    JP2016515657A

  • Synthesis of acrylic polymers in a flow reactor

    JP2017524797A