Method for manufacturing powder and granular molded products

By employing aluminum nitrate nonahydrate and fumed silica in a specific mixing process, the method addresses the decrease in charge capacity per unit volume in secondary batteries, ensuring stable redox reaction performance.

JP7955012B1Active Publication Date: 2026-11-24CONNEXX SYST
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2026093401
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-06-06
Filing Date
2026-06-03
Publication Date
2026-11-24
Estimated Expiration
2046-06-03

AI Technical Summary

Technical Problem

Existing methods for producing secondary batteries using iron oxide result in a decrease in charge capacity per unit volume due to repeated redox reactions.

Method used

A manufacturing process involving the use of aluminum nitrate nonahydrate as a coating material and fumed silica as a binder, mixed in specific proportions, to produce granular molded products that reduce the decrease in charge capacity per unit volume.

Benefits of technology

The method effectively minimizes the decrease in charge capacity per unit volume associated with repeated oxidation-reduction reactions, maintaining optimal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955012000001_ABST
    Figure 0007955012000001_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing granular molded products that minimizes the decrease in charge capacity per unit volume associated with repeated oxidation-reduction reactions. [Solution] The method for producing a granular molded product involves mixing granular or sol iron raw material and granular or sol coating material raw material, firing and pulverizing them to produce a powdered pulverized product, mixing binder raw material with the pulverized product to produce a binder mixture, and molding the binder mixture to produce a granular molded product. The iron raw material is granular or sol iron oxide, and its materials include triiron tetroxide, diiron trioxide, etc. The coating material raw material is aluminum nitrate nonahydrate, granular or sol fumed alumina. The binder raw material is granular or sol binder, and its materials are a mixture of one or more of fumed alumina and fumed silica. The amount of binder contained in the binder raw material is 4 to 20% by weight relative to the amount of pulverized product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a granular molded product from a mixture containing a metal oxide, and particularly to a method for producing a granular molded product from a mixture of iron oxide and one or both of a coating material and a binder, the granular molded product having a small decrease in charge capacity per unit volume due to repeated redox reactions.

Background Art

[0002] As a next-generation secondary battery, one utilizing the redox reaction of iron has been disclosed. For example, Patent Document 1 discloses a secondary battery in which when charging power is supplied from the outside, a reduction reaction of iron occurs to discharge oxygen to the outside, and when the charging power is stopped and oxygen is supplied from the outside, an oxidation reaction of iron occurs to supply power to the outside. Since the iron for the secondary battery needs to prevent sintering caused by the redox reaction, it was produced by adding aluminum nitrate and iron oxide to ethanol as a solvent, heating and evaporating the solvent while stirring, and then firing at 400 to 800°C for about 2 hours.

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0004] However, the production method of Patent Document 1 has a problem that when the redox reaction is repeated, the iron for the secondary battery expands, so that the charge capacity per unit volume decreases.

[0005] The present invention has been made in view of such conventional problems, and an object of the present invention is to provide a method for producing a granular molded product capable of reducing a decrease in charge capacity per unit volume due to repeated redox reactions.

Means for Solving the Problems

[0006] To achieve the above objective, the inventors conducted extensive research and, as a result, discovered that by developing a new manufacturing process using aluminum nitrate nonahydrate as the coating material raw material and fumed silica as the binder raw material, it is possible to reduce the decrease in charging capacity per unit volume associated with repeated oxidation-reduction reactions.

[0007] Furthermore, the inventors have discovered that by mixing an additive containing one or more substances only once, instead of mixing the two substances, the coating material raw material and the binder raw material, in two separate steps, they can obtain almost the same effect, leading to the present invention.

[0008] That is, the first embodiment of the present invention The first teeth, A method for producing granular molded products for secondary batteries using the oxidation-reduction reaction of iron, Mix the iron raw material and the coating material raw material. A coating material mixing process for manufacturing a coating material mixture , The coating mixture is fired at a temperature of 300-500°C for 100-140 minutes. Firing The firing process for manufacturing fired products , fired products Crushed, containing iron and coating material powder Powder used to manufacture crushed products Crushing The process involves mixing binder raw materials with the crushed material to produce a binder mixture, and the process involves mixing the binder mixture Pressed into pellets The process includes a molding step to produce a granular molded product, wherein the iron raw material is granular or sol of iron oxide, and the coating material raw material is aluminum nitrate (nohydrate). things The binder material is a sol of alumina, and the binder material is a powder or sol of one or more mixtures selected from the group consisting of fumed alumina and fumed silica. The amount of coating material mixed in the pulverized material is equal to the amount of iron Fe contained in the pulverized material. 2 O 3 This is 4-6% by weight relative to the converted amount. This invention provides a method for producing granular molded products in which the amount of binder mixed into the binder raw material is 4 to 20% by weight relative to the amount of pulverized material in the binder mixing process.

[0009] Furthermore, the present invention 1st form The second teeth, A method for producing granular molded products for secondary batteries using the oxidation-reduction reaction of iron,a coating material mixing step of mixing an iron raw material and a coating material raw material to produce a coating material mixture, a firing step of firing the coating material mixture at a firing temperature of 300 to 500°C for 100 to 140 minutes to produce a fired product, and pulverizing the fired product , a powder containing iron and coating material a pulverization step of producing a pulverized product, The process includes a binder mixing step of mixing a binder raw material with pulverized material to produce a binder mixture, and a molding step of pressing the binder mixture into pellets to produce a granular molded product, wherein the iron raw material is iron oxide powder or sol, the coating material raw material is fumed alumina powder or sol, the binder raw material is fumed silica powder or sol, and the amount of coating material mixed in the pulverized material is equal to the amount of iron in the pulverized material. 2 O 3 This invention provides a method for producing granular molded products in which the binder content is 4-6% by weight relative to the converted amount, and the amount of binder mixed in the binder raw material is 4-20% by weight relative to the amount of pulverized material in the binder mixing process. .

[0010] In addition, a second embodiment of the present invention A method for producing granular molded products for secondary batteries using the oxidation-reduction reaction of iron, an additive material mixing step of mixing an additive material raw material with an iron raw material to produce an additive material mixture; and Pressed into pellets a molding step of molding the additive material mixture to produce a granular molded product, wherein the iron raw material is a granular iron oxide, the additive material raw material is a granular material of one or a mixture of two or more selected from the group consisting of fumed alumina and fumed silica, and the mixing amount of the additive material contained in the additive material raw material is 4 to 20% by weight based on the Fe2O3-equivalent amount of iron contained in the iron raw material in the additive material mixing step. The present invention provides a method for producing a granular molded product. [[Effects of the Invention]]

[0012] According to the present invention, a decrease in charge capacity per unit volume due to repetition of oxidation-reduction reactions can be reduced. [[Brief Description of Drawings]]

[0013] [Figure 1] It is a flowchart showing the method for producing a granular molded product according to the first embodiment of the present invention. [[Modes for Carrying Out the Invention]]

[0014] Hereinafter, the present invention will be described in detail based on preferred embodiments shown in the accompanying drawings. First, a method for producing a granular molded product according to a first embodiment of the present invention will be described in detail. FIG. 1 is a flowchart showing a method for producing a granular molded product according to a first embodiment of the present invention.

[0015] The method for producing a granular molded product according to the first embodiment of the present invention is a method in which an iron raw material in the form of powder / granules or sol is mixed with a coating material raw material, the mixture is fired and pulverized to produce a powdery pulverized product, a binder raw material is mixed with the pulverized product to produce a binder mixture, and the binder mixture is molded to produce a granular molded product. The iron raw material is iron oxide in the form of powder / granules or sol, and examples of the material include triiron tetroxide (molecular formula: Fe3O4, molecular weight: 231.53, so-called black rust) and diiron trioxide (molecular formula: Fe2O3, molecular weight: 159.69, so-called red rust). The coating material raw material is aluminum nitrate nonahydrate, fumed alumina in the form of powder / granules, or an alumina sol. The binder raw material is a binder in the form of powder / granules or sol, and the material is one or a mixture of two or more selected from fumed alumina and fumed silica.

[0016] The mixing amount of the binder contained in the binder raw material is 4 to 20% by weight based on the amount of the pulverized product. When the mixing amount of the binder is less than 4% by weight based on the amount of the pulverized product, the density decrease accompanying the repetition of the oxidation-reduction reaction becomes excessive, and when it exceeds 20% by weight, the charge capacity decrease accompanying the decrease in the mixing ratio of iron becomes excessive. The lower limit of the mixing amount of the binder is preferably 4% by weight or more, more preferably 5% by weight or more. The upper limit of the mixing amount of the binder is preferably 20% by weight or less, more preferably 15% by weight or less, 13% by weight or less, or 10% by weight or less.

[0017] Specifically, the method for producing a granular molded product according to the first embodiment of the present invention may include: a pulverized product production step including a coating material raw material mixing step, a firing step, and a pulverization step; a binder raw material mixing step; and a molding step. In this case, in the coating material raw material mixing step, the iron raw material and the coating material raw material are mixed to produce a coating material mixture. In the firing step, after heating the coating material mixture to a firing temperature of 300 to 500°C (preferably 350 to 450°C), the coating material mixture is fired at the firing temperature for 100 to 140 minutes (preferably 110 to 130 minutes) to produce a fired product, and the fired product is cooled. In the pulverization step, the cooled fired product is pulverized to produce a powdery pulverized product. In the binder raw material mixing step, the binder raw material is mixed with the pulverized product to produce a binder mixture. In the molding step, the binder mixture is molded to produce a granular molded product.

[0018] Alumina obtained by dissolving aluminum nitrate nonahydrate in ethanol and then evaporating the ethanol, commercially available fumed alumina powder and granules, and commercially available alumina sol exhibit very similar behavior when each mixture is subjected to oxidation-reduction, although there are slight differences in numerical values ​​such as reaction rate and charge capacity. Therefore, the data obtained from experimental evaluation of one of these, for example, a mixture with aluminum nitrate-derived alumina, is approximately the same as the data for the other mixtures, namely the mixture with commercially available fumed alumina powder and granules, and the mixture with commercially available alumina sol.

[0019] Furthermore, when fumed alumina and fumed silica are subjected to oxidation-reduction reactions with pulverized materials containing iron raw materials, they exhibit extremely similar behavior, although there are slight differences in numerical values ​​such as reaction rate and charge capacity. Therefore, data obtained from experimental evaluation of one of these mixtures, for example, a mixture with fumed silica, is roughly equivalent to the data obtained from the other mixtures, namely the mixture with fumed alumina.

[0020] Next, we will explain in detail the mixing process for the coating material raw materials. The mixing process for the coating material raw materials differs depending on whether aluminum nitrate notahydrate is used or alumina powder or sol is used. In the former case, aluminum nitrate notahydrate and ethanol are placed in a beaker, stirred with a hot stirrer to dissolve the aluminum nitrate notahydrate, then iron powder, which has been ground in a mortar and pestle, is added to the beaker, the beaker is stirred with a hot stirrer, and the ethanol is evaporated to produce the coating material mixture.

[0021] In the latter case, as shown in step S10, the iron raw material and the alumina powder or sol are placed in a mortar and mixed with a pestle at room temperature for 1 to 10 minutes to produce the coating mixture. If the mixing time is less than 1 minute, there is a risk of uneven mixing, and if it is more than 10 minutes, the production lead time will be unnecessarily long. Note that a container and mixing device may be used instead of a mortar and pestle. Here, room temperature means 20 to 30°C, with 25°C being a typical value.

[0022] Next, we will explain in detail the heating process during the firing stage. The heating process involves placing the coating mixture in an electric furnace and heating it from room temperature to a firing temperature of 300-500°C at a rate of 4.0-6.0°C / min, as shown in step S12. If the temperature rise rate is less than 4.0°C / min, the manufacturing lead time will be unnecessarily long. If it exceeds 6.0°C / min, there is a risk of cracks or breaks occurring in the alumina boats, crucibles, etc., used as containers due to the rapid temperature change, and there is a risk of the water, which is the dispersion medium for the sol, boiling over and scattering the mixture. Furthermore, if the firing temperature is less than 300°C, there are concerns about quality, and if it exceeds 500°C, the heating and cooling times will be extended, resulting in an unnecessarily long manufacturing lead time. Note that the heating process does not necessarily have to be part of the firing process. That is, it may be incorporated into the mixing process of the coating material raw materials and mixed while heating.

[0023] Next, we will explain the firing process in detail. As shown in step S14, the firing process involves firing the heated coating mixture at the firing temperature for 100 to 140 minutes to produce the fired product. If the firing time is less than 100 minutes, there is a risk of insufficient drying, which could negatively affect subsequent processes, and if it exceeds 140 minutes, the manufacturing lead time will be unnecessarily long.

[0024] Next, we will explain in detail the cooling process during the firing stage. The cooling process involves cooling the fired material from the firing temperature to room temperature at a rate of 4.0 to 6.0°C / min while it remains in the electric furnace, as shown in step S16. If the temperature decrease rate is less than 4.0°C / min, the manufacturing lead time will be unnecessarily long, and if it exceeds 6.0°C / min, there is a risk of cracks or breaks occurring in the alumina boats, crucibles, etc., used as containers due to the rapid temperature change. Note that the cooling process does not necessarily have to be part of the firing process. In other words, it may be incorporated into the grinding process, and the grinding may be performed while cooling.

[0025] Next, we will explain the grinding process in detail. The grinding process, as shown in step S18, involves placing the cooled calcined material into a mortar and grinding it with a pestle at room temperature for 2 to 20 minutes to produce a powder. If the grinding time is less than 2 minutes, there is a risk that it will not become a powder, and if it exceeds 20 minutes, the manufacturing lead time will be unnecessarily long. Alternatively, a container and grinding device may be used for grinding instead of a mortar and pestle.

[0026] Next, we will explain in detail the mixing process of the binder raw materials. The binder raw material mixing process, as shown in step S20, involves placing the ground material and binder raw materials in a mortar and mixing them with a pestle at room temperature for 1 to 10 minutes to produce the binder mixture. If the mixing time is less than 1 minute, there is a risk of uneven mixing, and if it exceeds 10 minutes, the manufacturing lead time will be unnecessarily long. Alternatively, a container and mixing device may be used for mixing instead of a mortar and pestle.

[0027] Next, we will explain the molding process in detail. The molding process, as shown in step S22, involves using a press to press a predetermined amount of binder mixture and form it into pellets to produce a granular material. The shape of the pellets is not particularly limited and may be polyhedron, prism, cylinder, or sphere, but cylindrical is preferred due to the press's design. The dimensions of the pellets are not particularly limited and can be arbitrarily set according to the press's specifications.

[0028] With this configuration, the method for producing a powder or granular molded product according to the first embodiment of the present invention can reduce the decrease in charge capacity per unit volume that occurs with repeated oxidation-reduction reactions.

[0029] Next, we will explain the numerical range for the amount of coating material mixed in the crushed material. The amount of coating material mixed in the pulverized material is preferably 4 to 6% by weight (more preferably 4.5 to 5.5% by weight) relative to the Fe2O3 equivalent amount of iron contained in the pulverized material. If the amount of coating material mixed in is less than 4% by weight, the amount and rate of the oxidation-reduction reaction will decrease significantly, and if it exceeds 6% by weight, the charge capacity will decrease significantly.

[0030] With this configuration, the method for producing a powder or granular molded product according to the first embodiment of the present invention can reduce the decrease in charge capacity per unit volume that occurs with repeated oxidation-reduction reactions. The method for producing a granular molded product according to the first embodiment of the present invention is basically configured as described above.

[0031] Next, a method for producing a powder or granular molded product according to the second embodiment of the present invention will be described in detail. The second embodiment of the present invention is a method for manufacturing a powder or granular molded product that omits the pulverization process (steps S10-S18) of the first embodiment of the present invention, and is a manufacturing method in which the additive material is mixed with the iron raw material without mixing the iron raw material and the coating material material. Accordingly, in the binder material mixing process (step S20), "pulverized material" is replaced with "iron raw material", "binder raw material" with "additive material", and "binder mixture" with "additive mixture", and in the molding process (step S22), "binder mixture" is replaced with "additive mixture".

[0032] The additive raw material is a powder or granular form of the additive, and its material is a mixture of one or more fumed alumina and fumed silica. The lower limit of the amount of additive mixed is preferably 4% by weight or more, and more preferably 5% by weight or more. The upper limit of the amount of additive mixed is preferably 20% by weight or less, and more preferably 15% by weight or less, 13% by weight or less, and 10% by weight or less.

[0033] With this configuration, the method for producing a powder or granular molded product according to the second embodiment of the present invention can reduce the decrease in charge capacity per unit volume that occurs with repeated oxidation-reduction reactions. The method for producing a powder or granular molded product according to the second embodiment of the present invention is basically configured as described above.

[0034] Next, a third embodiment of the present invention, a granular material molded product, will be described in detail. The third embodiment of the present invention is a granular molded product obtained by the method for manufacturing a granular molded product of the first embodiment or the method for manufacturing a granular molded product of the second embodiment. With this configuration, the powder and granular molded product of the third embodiment of the present invention can reduce the decrease in charge capacity per unit volume due to repeated oxidation-reduction reactions. The powder and granular molded product of the third embodiment of the present invention is basically configured as described above. [Examples]

[0035] Next, we will give specific examples of the present invention and explain it in more detail. First, we will describe the manufacturing procedure of the powder and granular molded product of Example 1.

[0036] (Step 1) First, aluminum nitrate notahydrate (Fujifilm Wako Pure Chemical Industries, Ltd.; Reagent Grade 018-01945) and ethanol were placed in a beaker and stirred at 200 RPM and 70°C using a hot stirrer (AS ONE Corporation; RSH-1DN) to dissolve the aluminum nitrate notahydrate. Meanwhile, iron powder (Ishihara Sangyo Co., Ltd.: MT iron oxide) was placed in a mortar and ground using a pestle. Next, the ground iron powder was added to the beaker and stirred at 200 RPM and 70°C for about 3 hours using a hot stirrer to evaporate the ethanol. Next, the dried mixture was transferred to an alumina boat (Tokyo Glass Instruments Co., Ltd.; CB-4), calcined in an electric furnace, and then pulverized. The amount of aluminum nitrate notahydrate was adjusted so that the alumina accounted for 5% of the Fe2O3 equivalent amount of iron contained in the pulverized material after calcination.

[0037] (Step 2) The pulverized material and fumed silica (Aerosil200, Nippon Aerosil Co., Ltd.) were placed in a mortar and mixed using a pestle. The amount of fumed silica was adjusted to 5% of the amount of pulverized material. (Step 3) Approximately 1 g of the mixture was weighed out, placed in a mold, and molded into disc-shaped pellets (diameter: approximately 13 mm, thickness: approximately 2.5 mm) using a press machine (Riken Seiki Co., Ltd.; P-1B) to produce the powder granular molded product of Example 1.

[0038] (Step 4) Next, the manufacturing procedure for the powder and granular molded product of Example 2 will be described. In Example 2, the same iron raw material as in Example 1 and fumed alumina (AEROXIDE Alu 130, Nippon Aerosil Co., Ltd.) were placed in a mortar and mixed using a pestle to produce an additive mixture. The additive mixture was then pressed using a press to form pellets, thereby producing the powder and granular material of Example 2. The amount of fumed alumina was adjusted to 10% by weight relative to the Fe2O3 equivalent amount of iron contained in the iron raw material.

[0039] (Step 5) Next, the manufacturing procedure for the powder and granular molded product of Example 3 will be described. In Example 2, fumed silica was mixed in place of fumed alumina. The amount of fumed silica was adjusted to 10% by weight relative to the Fe2O3 equivalent amount of iron contained in the iron raw material.

[0040] (Step 6) Next, the manufacturing procedure for the powder and granular molded product of Example 4 will be described. Fumed alumina was mixed in the same manner as in Example 2. The amount of fumed alumina was adjusted to 15% by weight relative to the Fe2O3 equivalent amount of iron contained in the iron raw material.

[0041] (Step 7) Next, the manufacturing procedure for the powder and granular molded product of Comparative Example 1 will be described. Step 2 of Example 1 was omitted, and the pulverized material from Step 1 was molded in Step 3 to produce the granular molded product of Comparative Example 1. The amount of aluminum nitrate nonahydrate was adjusted so that the alumina amount was 10% of the amount of iron in Fe2O3 equivalent contained in the pulverized material after calcination.

[0042] (Step 8) Next, the manufacturing procedure for the powder and granular molded product of Comparative Example 2 will be described. In Comparative Example 2, alumina sol (Nissan Chemical Corporation; AS-200) was mixed in place of aluminum nitrate xahydrate in step 1 of Example 1, step 2 was omitted, and the pulverized material from step 1 was molded in step 3 to produce the granular molded product of Comparative Example 2. The amount of alumina sol was adjusted so that the alumina amount was 10% of the Fe2O3 equivalent amount of iron contained in the pulverized material after calcination.

[0043] <Evaluation of charging capacity per unit volume> Next, the procedure for evaluating the charge capacity per unit volume of the powder and granular molded products of Examples 1-4 and Comparative Examples 1 and 2 will be explained. Table 1 shows the charge capacity per unit volume after 40 oxidation-reduction cycles. The target range for the charge capacity per unit volume is 1,000 mAh / mm² after 40 oxidation-reduction cycles. 3 That's all.

[0044] 1. Measurement of volume v and weight m after 40 oxidation-reduction cycles. (Procedure a) Next, each pellet from Examples 1-4 and Comparative Examples 1 and 2 was placed in a tubular furnace, and when the temperature of each pellet reached 730°C, it was maintained for 5 minutes while flowing dry argon gas at a flow rate of 280 ml / min. Then, the following procedures b-e were repeated 40 times. (Procedure b) To reduce each pellet, the pellets were kept at 730°C for 60 minutes while a hydrogen gas flow rate of 70 ml / min was passed through them. (Procedure c) The system was maintained at 730°C for 5 minutes while flowing dry argon gas at a flow rate of 280 ml / min.

[0045] (Procedure d) Each pellet was held at 730°C for 60 minutes while a flow rate of 70 ml / min of wet argon gas was passed through it to oxidize it. (Procedure e) The system was maintained at 730°C for 5 minutes while flowing dry argon gas at a flow rate of 280 ml / min. (Procedure f) Next, the volume v and weight m of each pellet were measured.

[0046] 2. Measurement of the weight ratio a after 360 minutes relative to the start of reduction. (Procedure g) First, each pellet from Examples 1-4 and Comparative Examples 1 and 2 was crushed with a hammer, and pellet fragments of about 70-100 mg were selected. These fragments were placed in a differential thermobalance (NETZSCH STA 2500 Regulus) and heated at a rate of 10°C / min while compressed air was flowed at a flow rate of 100 ml / min. The fragments were then held at a temperature of 730°C for 30 minutes.

[0047] (Procedure h) Next, the pellets were held at 730°C for 5 minutes while flowing argon gas at a flow rate of 100 ml / min, and the weight Ws of the pellet fragments was measured. Then, to reduce each pellet fragment, the pellets were held at 730°C for 360 minutes while flowing a mixed gas of hydrogen gas (7 vol%) and argon gas (93 vol%) at a flow rate of 100 ml / min. (Procedure i) Next, the weight of each pellet fragment was measured, and the weight ratio a was calculated by dividing that weight by the total weight Ws.

[0048] 3. Calculation of the charge capacity e per unit volume after 40 oxidation-reduction cycles. Next, the charge capacity e per unit volume after 40 oxidation-reduction cycles was calculated by substituting the weight ratio a after 360 minutes relative to the start of reduction, the conversion coefficient b, the volume v after 40 oxidation-reduction cycles, and the weight m into the following equations 1 to 3. Each measured value and each calculated value are shown in Tables 1(a) and 1(b).

[0049] [Math 1] c=(1-a)×b [Number 2] d=m / v [Math 3] e = c × d Here, the conversion coefficient b is a coefficient used to convert the weight ratio to the charging capacity per unit weight, and is specifically calculated using the procedure shown in Table 2.

[0050] [Table 1(a)] [Table 1(b)] [Table 2]

[0051] As a result, the mixed powders of Examples 1-4 had a charge capacity e per unit volume of 1.660 mAh / mm³ after 40 oxidation-reduction cycles. 3 , 1.925mAh / mm 3 , 1.416mAh / mm 3 , 1.716mAh / mm 3 As a result, everything fell within the target range. Furthermore, the mixed powders of Comparative Examples 1 and 2 had a charge capacity e per unit volume of 0.885 mAh / mm³ after 40 oxidation-reduction cycles. 3 , 0.991mAh / mm 3 As a result, it fell outside the target range.

[0052] These results clearly demonstrate that the methods for producing the mixed granular material in Examples 1 to 4 can minimize the decrease in charge capacity per unit volume associated with repeated oxidation-reduction reactions. Furthermore, it is clear that aluminum nitrate nonahydrate and alumina sols exhibit extremely similar behavior as coating material raw materials, and that fumed alumina powder and fumed silica powder and granular materials exhibit extremely similar behavior as additive raw materials.

[0053] The method for producing the powder and granular molded product of the present invention has been described in detail with reference to examples above. However, the present invention is not limited to the above description, and various improvements and modifications may be made without departing from the spirit of the present invention. 。 [Industrial applicability]

[0054] The method for producing granular molded products of the present invention has the effect of reducing the decrease in charge capacity per unit volume that occurs with repeated oxidation-reduction reactions, and is therefore industrially useful.

Claims

1. A method for producing a powder or granular molded product for a secondary battery utilizing the oxidation-reduction reaction of iron, A coating material mixing process involves mixing iron raw materials and coating material raw materials to produce a coating material mixture, A firing process to produce a fired product by firing the coating material mixture at a firing temperature of 300 to 500°C for 100 to 140 minutes, A grinding step of grinding the aforementioned calcined material to produce a powdered pulverized material containing iron and a coating material, A binder mixing step is performed to produce a binder mixture by mixing the aforementioned pulverized material with binder raw materials, The process includes a molding step of pressing the binder mixture to form pellets and producing a powder or granular molded product, The aforementioned iron raw material is a powder or sol of iron oxide. The coating material raw material is aluminum nitrate nonahydrate or alumina sol. The binder raw material is a powder or sol of one or more mixtures selected from the group consisting of fumed alumina and fumed silica. The amount of coating material mixed in the pulverized material is 4 to 6% by weight relative to the amount of iron in Fe₂O₃ equivalent contained in the pulverized material. A method for producing a granular molded product, wherein the amount of binder mixed in the binder raw material is 4 to 20% by weight relative to the amount of pulverized material in the binder mixing step.

2. A method for producing a powder or granular molded product for a secondary battery utilizing the oxidation-reduction reaction of iron, A coating material mixing process involves mixing iron raw materials and coating material raw materials to produce a coating material mixture, A firing process to produce a fired product by firing the coating material mixture at a firing temperature of 300 to 500°C for 100 to 140 minutes, A grinding step of grinding the aforementioned calcined material to produce a powdered pulverized material containing iron and a coating material, A binder mixing step is performed to produce a binder mixture by mixing the aforementioned pulverized material with binder raw materials, The process includes a molding step of pressing the binder mixture to form pellets and produce a powder or granular molded product, The aforementioned iron raw material is a powder or sol of iron oxide. The coating material raw material is fumed alumina powder, The binder raw material is fumed silica in powder or sol form. The amount of coating material mixed in the pulverized material is 4 to 6% by weight relative to the amount of iron in Fe₂O₃ equivalent contained in the pulverized material. A method for producing a granular molded product, wherein the amount of binder mixed in the binder raw material is 4 to 20% by weight relative to the amount of pulverized material in the binder mixing step.

3. A method for producing a powder or granular molded product for a secondary battery utilizing the oxidation-reduction reaction of iron, An additive mixing process involves mixing additive raw materials with iron raw materials to produce an additive mixture, The process includes a molding step of pressing the additive mixture to form pellets in order to produce a powder or granular molded product, The aforementioned iron raw material is a powder or granular form of iron oxide. The additive raw material is a powder or granular material of one or more mixtures selected from the group consisting of fumed alumina and fumed silica. The amount of additives mixed in the additive raw material is the amount of iron (Fe) contained in the iron raw material in the additive mixing step. 2 O 3 A method for producing a powder or granular molded product in a quantity of 4 to 20% by weight relative to the converted amount.

Citation Information

Patent Citations

  • Preparation method of silicon dioxide magnetic beads with high functional group loading capacity

    CN116947053A

  • Method of producing foamy egg white

    JP1977010450A

  • Spraying liquid car cover film composition, spraying car cover film and preparation method for spraying car cover film

    US12291645B1

  • Composite and method for preparing same

    US20230095866A1