Method for manufacturing polarizing film
The manufacturing method for polarizing films using a curable aqueous dispersion composition addresses issues of polarization degradation and interference in automotive applications by reducing refractive index differences and enhancing humidification reliability.
Patent Information
- Application Number
- JP2022022822
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-02-17
AI Technical Summary
Conventional polarizing films used in automotive applications face issues with decreased polarization degree under humidified conditions and interference unevenness due to reflected light, particularly in thinner films.
A method for manufacturing polarizing films involving a coating step with a curable aqueous dispersion composition containing water and a polymerizable compound, followed by a drying step to form a resin layer, which includes a surfactant and is cured with active energy rays, reducing refractive index differences and enhancing humidification reliability.
The method produces polarizing films with improved appearance by suppressing interference unevenness and maintaining high polarization under harsh conditions of high temperature and humidity.
Smart Images

Figure 0007955022000008 
Figure 0007955022000009 
Figure 0007955022000010
Abstract
Description
[Technical Field]
[0001] This invention relates to a method for manufacturing a polarizing film. The polarizing film can be used alone or laminated to form an optical film that can be used to form image display devices such as mobile phones, car navigation systems, personal computer monitors, and televisions. [Background technology]
[0002] Liquid crystal display (LCD) displays are rapidly expanding into the market for mobile phones, car navigation systems, PC monitors, and televisions. LCDs visualize the polarization state created by switching liquid crystals, and due to their display principle, polarizers are used. In particular, applications such as TVs require increasingly high brightness, high contrast, and wide viewing angles, and polarizing films are increasingly required to have high transmittance, high polarization degree, and high color reproduction.
[0003] As polarizers, iodine-based polarizers, which have high transmittance and high polarization degree, are most commonly and widely used. For example, iodine-based polarizers have a structure in which iodine is adsorbed onto polyvinyl alcohol (hereinafter also simply referred to as "PVA") and then stretched. Generally, polarizing films are made by laminating a transparent protective film to both sides of the polarizer using a so-called water-based adhesive, which is a polyvinyl alcohol-based material dissolved in water (see Patent Document 1 below). As the transparent protective film, triacetylcellulose with high moisture permeability is used. When the aforementioned water-based adhesive is used (so-called wet lamination), a drying process is required after laminating the polarizer and the transparent protective film.
[0004] On the other hand, instead of the aforementioned water-based adhesives, active energy ray-curable adhesives have been proposed. When polarizing films are manufactured using active energy ray-curable adhesives, a drying process is not required, thus improving the productivity of polarizing films. For example, a radical polymerization type active energy ray-curable adhesive using an N-substituted amide monomer as the curing component has been proposed (see Patent Document 2 below). An adhesive layer formed using the active energy ray-curable adhesive described in Patent Document 2 can adequately pass a water resistance test to evaluate the presence or absence of discoloration and peeling after immersion in 60°C hot water for 6 hours, for example. However, in recent years, polarizing films are often used not only in mobile applications such as mobile phones, but also in image display devices for automotive applications. Automotive applications require durability testing under higher temperature and humidity conditions compared to mobile applications. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2001-296427 [Patent Document 2] Japanese Patent Publication No. 2012-052000 [Overview of the project] [Problems that the invention aims to solve]
[0006] For polarizing films used in automotive applications, a durability test is required, such as a humidified durability test in which the film is exposed to an environment of 85°C and 85% humidity for a predetermined time. However, with conventional polarizing films, there is a possibility of a decrease in the degree of polarization, indicating that there is room for further improvement in terms of humidified reliability.
[0007] Incidentally, in recent years there has been a demand for thinner polarizing films regardless of the application, and as a result thin polarizers are frequently used. However, with thin polarizers, interference unevenness due to reflected light can sometimes become a problem. Therefore, there has been a demand to improve the appearance by suppressing interference unevenness in polarizing films.
[0008] This invention was developed in view of the above circumstances, and aims to provide a method for manufacturing a polarizing film that has excellent appearance by having superior humidification reliability and suppressing interference unevenness. [Means for solving the problem]
[0009] The above problems can be solved by the following configuration. That is, the present invention relates to a method for manufacturing a polarizing film comprising at least a polarizer, comprising a coating step of coating a curable aqueous dispersion composition on at least one surface of the polarizer, and a drying step of forming a resin layer by drying the curable aqueous dispersion composition, wherein the curable aqueous dispersion composition contains water as a solvent and polymerizable compound A.
[0010] In the above method for producing a polarizing film, it is preferable that the curable aqueous dispersion composition contains a polymerizable compound A that has a viscosity of 100 mPa·s or more or is solid at 25°C.
[0011] In the above method for producing a polarizing film, it is preferable that the curable aqueous dispersion composition contains, as the polymerizable compound A, a hydrophobic polymerizable compound with a LogPow of 1.0 or higher.
[0012] In the above method for producing a polarizing film, it is preferable that the curable aqueous dispersion composition contains at least a trifunctional or polyfunctional polymerizable compound as the polymerizable compound A.
[0013] In the above method for producing a polarizing film, it is preferable that the curable aqueous dispersion composition further contains a surfactant.
[0014] In the above method for producing a polarizing film, it is preferable that the curable aqueous dispersion composition is a forced emulsion using the surfactant as an emulsifier.
[0015] In the method for producing a polarizing film described above, the surfactant is preferably composed of two or more types of surfactants.
[0016] In the method for producing a polarizing film described above, the surfactant is preferably composed of at least two selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
[0017] In the method for producing a polarizing film described above, it is preferable to include a curing step of forming a cured product layer formed by irradiating active energy rays after the drying step to cure the resin layer.
[0018] In the method for producing a polarizing film described above, the polarizing film is a polarizing film in which the polarizer and a transparent protective film are laminated via an adhesive layer, and after the drying step, active energy rays are irradiated to cure the resin layer. It is preferable to include a curing step of forming the adhesive layer including at least the cured product layer formed by curing.
Effects of the Invention
[0019] Generally, a polarizer included in a polarizing film has a higher refractive index in the absorption axis direction on the long wavelength side. On the other hand, for example, when an adhesive layer (cured product layer of a resin layer) is formed on a polarizer to adhere the polarizer to another substrate, the adhesive layer tends to gradually decrease in refractive index as the wavelength shifts from the short wavelength side to the long wavelength side. Therefore, especially on the long wavelength side, the difference in refractive index between the polarizer and the adhesive layer becomes large, which easily causes interference unevenness, and as a result, the appearance of the polarizing film tends to be impaired.
[0020] The method for manufacturing a polarizing film according to the present invention comprises a coating step of coating a curable aqueous dispersion composition onto at least one surface of a polarizer, and a drying step of forming a resin layer by drying the curable aqueous dispersion composition. In this coating step, when coating at least one surface of the polarizer with a curable aqueous dispersion composition containing water as a solvent and polymerizable compound A, the coated water dissolves the iodine complex present on the polarizer surface. This makes it possible to lower the refractive index of the polarizer on the long-wavelength side, and when an adhesive layer is finally formed on the polarizer, it is possible to reduce the refractive index difference between the polarizer and the adhesive layer, especially on the long-wavelength side. As a result, it is possible to manufacture a polarizing film that is less prone to interference unevenness and has excellent appearance.
[0021] Furthermore, in the drying process following the coating process, even though water evaporates, the iodine complex dissolved in water remains within the resin layer when the polymerizable compound A is formed. As a result, even when a polarizing film having a cured layer (adhesive layer) formed by irradiating the resin layer formed after the drying process with active energy rays is placed under harsh conditions of high temperature and high humidity, the elution of iodine within the polarizer is suppressed. Therefore, the method for manufacturing a polarizing film according to the present invention makes it possible to produce a polarizing film with excellent humidification reliability.
[0022] Furthermore, in the method for producing a polarizing film according to the present invention, if the polymerizable compound A contained in the curable aqueous dispersion composition has a viscosity of 100 mPa·s or more or is solid at 25°C, and if the curable aqueous dispersion composition contains a surfactant, the cured layer formed by irradiating the resin layer formed after the drying process with active energy rays is formed with a rigid skeleton and exhibits hydrophobicity. As a result, even when the polarizing film is placed in a harsh environment of high temperature and high humidity, the elution of iodine from the polarizer is suppressed to a higher level. As a result, a polarizing film with particularly excellent humidification reliability can be produced. [Brief explanation of the drawing]
[0023] [Figure 1]This is an example of a schematic cross-sectional view of a polarizing film manufactured by the manufacturing method of the present invention. [Figure 2] This is another example of a schematic cross-sectional view of a polarizing film manufactured by the manufacturing method of the present invention. [Figure 3] This is another example of a schematic cross-sectional view of a polarizing film manufactured by the manufacturing method of the present invention. [Modes for carrying out the invention]
[0024] The method for manufacturing a polarizing film according to the present invention comprises a coating step of coating at least one surface of a polarizer with a curable aqueous dispersion composition, and a drying step of drying the curable aqueous dispersion composition to form a resin layer.
[0025] The curable aqueous dispersion composition used in the present invention contains water as a solvent and polymerizable compound A. The components are described below.
[0026] The water used as a solvent preferably does not contain organic solvents such as alcohol. If it does contain organic solvents, the content of organic solvents such as alcohol is preferably 10% by weight or less, more preferably 5% by weight or less, preferably 1% by weight or less, and particularly preferably 0.1% by weight or less, when the total solvent is considered to be 100% by weight or less.
[0027] Polymerizable compound A is preferably a polymerizable compound that has a viscosity of 100 mPa·s or more or is solid at 25°C. In the present invention, polymerizable compounds having such properties can be broadly classified into "polyfunctional polymerizable compounds with at least three functions," "hydrophobic polymerizable compounds with a LogPow of 1.0 or more," or "polymerizable compounds having a ring structure."
[0028] Examples of polyfunctional polymerizable compounds with at least three functions include pentaerythritol triacrylate (trifunctional, 600-1000 mPa·s / 25℃), pentaerythritol tetraacrylate (tetrafunctional, solid at 25℃), dipentaerythritol hexaacrylate (trifunctional, 600-1000 mPa·s / 25℃), polypentaerythritol acrylate (trifunctional or more, 9000-15000 mPa·s / 25℃), tris(2-acryloyloxyethyl) isocyanurate (trifunctional, solid at 25℃), and ditrimethylolpropanetetraacrylate (tetrafunctional, 1000 mPa·s / 25℃).
[0029] Examples of hydrophobic polymerizable compounds with a LogPow of 1.0 or higher include macromonomers containing polymethyl methacrylate groups (Mn≒6000) (solid at 25°C), macromonomers containing polybutyl acrylate groups (Mn≒6000) (10000 (mPa·s / 25°C) or higher), and macromonomers having both a hydrophobic segment and a polymerizable functional group.
[0030] The octanol / water partition coefficient (logPow) is an indicator of a substance's lipophilicity and represents the logarithm of the octanol / water partition coefficient. A high logPow indicates lipophilicity, which in turn means low water absorption. While logPow values can be measured (using the flask immersion method described in JIS-Z-7260), they can also be calculated. In this specification, logPow values calculated using CambridgeSoft's ChemDraw Ultra are used.
[0031] Polymerizable compounds having a ring structure include dimethylol-tricyclodecanediaacrylate (bifunctional, 130-170 (mPa·s / 25℃)), ethoxylated bisphenol A dimethacrylate (bifunctional, 2.3 ethylene oxide repeating units (1220 (mPa·s / 25℃), 2.6 ethylene oxide repeating units (1000 (mPa·s / 25℃), 4 ethylene oxide repeating units (640 (mPa·s / 25℃), 10 ethylene oxide repeating units (450 (mPa·s / 25℃)), 17 ethylene oxide repeating units (500 (mPa·s / 25℃), 30 ethylene oxide repeating units (660 (mPa·s / 25℃))), and ethoxylated-o-phenylphenol acrylate (monofunctional, 130 Examples include (mPa·s / 25℃), 9,9-bis[4-(2-hydroxyethoxy)phenyl]ful orange acrylate (difunctional, 91000 (mPa·s / 60℃)), 1-pyrenylmethyl methacrylate (monofunctional, solid at 25℃), 2-naphthyl methacrylate (monofunctional, solid at 25℃), 9-anthrylmethyl methacrylate (monofunctional, solid at 25℃), 1,3-adamantanediol diacrylate (monofunctional, solid at 25℃), and rosin acrylate (monofunctional, 10000 (mPa·s / 40℃)).
[0032] Other polymerizable compounds A include polybutadiene-terminated diacrylates (bifunctional, 4000-8000 (mPa·s / 25℃)).
[0033] In the curable aqueous dispersion composition used in the present invention, the content of polymerizable compound A is preferably 10 to 95% by weight, more preferably 20 to 93% by weight, and even more preferably 30 to 90% by weight, when the total amount excluding water as a solvent is considered to be 100% by weight.
[0034] The curable aqueous dispersion composition used in the present invention preferably contains a surfactant in addition to water as a solvent and polymerizable compound A. Examples of surfactants include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
[0035] Anionic surfactants include carboxylates such as sodium stearate, sodium N-lauroyl sarcosinate, sodium palmitate, sodium laurate, N-lauroyl sarcosine, sodium N-decanoyl sarcosinate, N-oleoyl sarcosine, sodium myristate, sodium cholate, and sodium oleate; phosphate esters such as sodium monododecyl phosphate; sodium dimethyl sodium 5-sulfoisophthalate, sodium 1-undecanesulfonate, sodium 1-pentadecanesulfonate, sodium bis(2-ethylhexyl) sulfosuccinate, and sodium 1-octadecanesulfonate. Examples include sulfonates such as sodium dodecylbenzenesulfonate, sodium alkylnaphthalenesulfonate, sodium 1-decanesulfonate, and sodium 1-dodecanesulfonate; sulfate esters such as sodium decyl sulfate, sodium dodecyl sulfate, sodium hexadecyl sulfate, and sodium dodecyl sulfate; polyoxyethylene styrene-methylphenyl ether sulfate, polyoxyethylene alkyl ether sulfate, polyoxyethylene cumylphenyl ether sulfate, and polycyclic phenyl ether methacrylate sulfate.
[0036] Cationic surfactants include n-octyltrimethylammonium bromide, trimethylstearylammonium bromide, hexadecyltrimethylammonium chloride, trimethylstearylammonium chloride, hexadecyltrimethylammonium chloride, trimethylstearylammonium chloride, n-octylamine hydrochloride, octadecylamine hydrochloride, n-octylamine hydrobromide, n-octyltrimethylammonium chloride, trimethyltetradecylammonium chloride, heptadecyltrimethylammonium bromide, butyltrimethylammonium bromide, hexadecyltrimethylammonium hexafluorophosphate, hexadecyltrimethylammonium perchlorate, decyltrimethylammonium chloride, dodecyltrimethylammonium chloride, decyltrimethylammonium bromide, di-n-alkyldimethylammonium chloride, hexadecyltrimethylammonium hydroxide, and hexadecyltrimethylammonium Examples include aliphatic amine salts or aliphatic quaternary ammonium salts such as bromide, trimethylnonylammonium bromide, dodecylamine hydrochloride, hexadecyltrimethylammonium tetrafluoroborate, hexyltrimethylammonium bromide, hexadecyltrimethylammonium bisulfate, dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, and dodecylamine hydrobromide; heterocyclic quaternary ammonium salts such as 1-hexadecyl-4-methylpyridinium chloride hydrate, hexadecylpyridinium chloride monohydrate, hexadecylpyridinium bromide hydrate, and 1-dodecylpyridinium chloride; and aromatic quaternary ammonium salts such as benzyldodecyldimethylammonium bromide, benzethonium chloride, benzyldimethylstearylammonium chloride, benzylcetyldimethylammonium chloride, benzyldodecyldimethylammonium chloride dihydrate, and benzyldimethyltetradecylammonium chloride.
[0037] Examples of amphoteric surfactants include octadecyldimethyl(3-sulfopropyl)ammonium hydroxide intramolecular salt, 3-[(3-collamidopropyl)dimethylammonio]-1-propanesulfonate, and dodecyldimethyl(3-sulfopropyl)ammonium hydroxide intramolecular salt.
[0038] Nonionic surfactants include ester ether types such as polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan monolaurate; polyethylene glycol monomethyl ether 1000, octaethylene glycol monododecyl ether, hexaethylene glycol monododecyl ether, polyethylene glycol monooleyl ether (n ≈ approx. 10), polyethylene glycol monooleyl ether (n ≈ approx. 2), pentaethylene glycol monododecyl ether, polyethylene glycol monododecyl ether (n ≈ approx. 25), polyethylene glycol 1000, polyethylene glycol monooleyl ether (n ≈ approx. 7), and polyethylene glycol Ether forms such as polyethylene glycol mono-4-nonylphenyl ether (n ≈ approx. 15), polyethylene glycol monooleyl ether (n ≈ approx. 50), polyethylene glycol monocetyl ether (n ≈ approx. 23), triethylene glycol monododecyl ether, polyethylene glycol mono-4-nonylphenyl ether (n ≈ approx. 2), polyethylene glycol mono-4-octylphenyl ether (n ≈ approx. 10), polyethylene glycol monooleyl ether (n ≈ approx. 20), polyethylene glycol monomethyl ether 400, polyethylene glycol monomethyl ether 4000, polyethylene glycol mono-4-nonylphenyl ether (n ≈ approx. 20), diethylene glycol monododecyl ether, polyethylene glycol monomethyl ether 550, polyethylene glycol monomethyl ether 2000, polyethylene glycol mono-4-nonylphenyl ether (n ≈ approx. 18), polyethylene glycol 20000, etc.Examples include ester-type surfactants such as sorbitan monooleate, sorbitan trioleate, sorbitan monopalmitate, monostearin, monopalmitin, polyethylene glycol monolaurate (n ≈ 10), sorbitan monostearate, sorbitan monolaurate, polyethylene glycol monostearate (n ≈ 45), polyethylene glycol monostearate (n ≈ 55), sorbitan sesquioleate, polyethylene glycol monostearate (n ≈ 2), monomyristate, polyethylene glycol monostearate (n ≈ 25), polyethylene glycol monostearate (n ≈ 4), polyethylene glycol monostearate (n ≈ 40), polyethylene glycol monostearate (n ≈ 10), acetylene alcohol-based surfactants, acetylene glycol-based surfactants, and other acetylene-based surfactants containing acetylene bonds, as well as fluorine-based surfactants.
[0039] The curable aqueous dispersion composition used in the present invention preferably contains two or more surfactants as surfactants in order to achieve both the dispersibility of polymerizable compound A and the appearance of the coating film, and more preferably contains at least two surfactants selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants and nonionic surfactants.
[0040] In order to achieve both the dispersibility of polymerizable compound A and the appearance of the coating film, the surfactant content in the curable aqueous dispersion composition used in the present invention is preferably 0.1 to 20% by weight, and more preferably 1 to 15% by weight, when the total amount excluding water as a solvent is considered to be 100% by weight.
[0041] The curable aqueous dispersion composition used in the present invention preferably contains a photopolymerization initiator. The photopolymerization initiator is appropriately selected based on the active energy ray. When curing is performed by ultraviolet light or visible light, a photopolymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of the photopolymerization initiators include benzophenone compounds such as benzyl, benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and α-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzioin methyl ether, benzioin ethyl ether, benzoin isopropyl ether, and Examples include benzoin ether compounds such as benzoin butyl ether and anisoin methyl ether; aromatic ketal compounds such as benzyldimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.
[0042] The amount of the photopolymerization initiator is 20 parts by weight or less per 100 parts by weight of the total amount of polymerizable compound A. Preferably, the amount of the photopolymerization initiator is 0.01 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight.
[0043] Furthermore, when the curable aqueous dispersion composition used in the present invention is curable with visible light, it is particularly preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or higher. Photopolymerization initiators highly sensitive to light of 380 nm or higher will be described later.
[0044] The aforementioned photopolymerization initiator is a compound represented by the following general formula (1); [ka] (In the formula, R 1 and R 2 R represents -H, -CH2CH3, -iPr, or Cl. 1 and R 2 It is preferable to use the compound represented by general formula (1) alone (which may be the same or different) or to use it in combination with a photopolymerization initiator that is highly sensitive to light of 380 nm or higher, as described later. When the compound represented by general formula (1) is used, the adhesion is superior to when the photopolymerization initiator that is highly sensitive to light of 380 nm or higher is used alone. Among the compounds represented by general formula (1), R 1 and R 2 Diethylthioxanthones, where -CH2CH3, are particularly preferred. The composition ratio of the compound represented by general formula (1) in the curable aqueous dispersion composition is preferably 0.1 to 5% by weight, more preferably 0.5 to 4% by weight, and even more preferably 0.9 to 3% by weight, based on the total amount of the curable aqueous dispersion composition.
[0045] Furthermore, it is preferable to add polymerization initiators as needed. Examples of polymerization initiators include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate, with ethyl 4-dimethylaminobenzoate being particularly preferred. When using polymerization initiators, the amount added is usually 0 to 5% by weight, preferably 0 to 4% by weight, and most preferably 0 to 3% by weight, relative to the total amount of the curable resin composition.
[0046] Furthermore, known photopolymerization initiators can be used in combination as needed. Since transparent protective films with UV absorption ability do not transmit light below 380 nm, it is preferable to use a photopolymerization initiator that is highly sensitive to light above 380 nm. Specifically, examples include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrole-1-yl)-phenyl)titanium.
[0047] The curable aqueous dispersion composition used in the present invention preferably contains a silane coupling agent. Specific examples of silane coupling agents include active energy ray curable compounds such as vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.
[0048] Preferably, these are 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0049] The amount of silane coupling agent added is preferably in the range of 0.01 to 20% by mass, more preferably 0.05 to 15% by mass, and more preferably 0.1 to 10% by mass, relative to the total amount of the curable aqueous dispersion composition. This is because if the amount exceeds 20% by mass, the storage stability of the curable aqueous dispersion composition deteriorates, and if it is less than 0.1% by mass, the adhesive water resistance effect is not sufficiently exhibited.
[0050] Specific examples of silane coupling agents that are not curable by active energy rays other than those mentioned above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatetopropyltriethoxysilane, and imidazolesilane.
[0051] The curable aqueous dispersion composition used in the present invention may contain polymerizable compounds other than polymerizable compound A, which has a viscosity of 100 mPa·s or more or is solid at 25°C. An example of a polymerizable compound that can be contained is polymerizable compound B, which is a raw material for the curable resin composition described later. Polymerizable compound B will be described later.
[0052] The curable aqueous dispersion composition used in the present invention may further include, if necessary, the compound described in the following general formula (3);
[0053] [ka] (However, X is a functional group containing a reactive group, and R 6 and R 7 Each of these independently represents a hydrogen atom, an aliphatic hydrocarbon group which may have substituents, an aryl group, or a heterocyclic group), preferably the compound described in the general formula (3');
[0054] [ka] (wherein Y is an organic group, X' is a reactive group contained in X, R 6 and R 7 are the same as defined above), more preferably compounds represented by general formulas (3a) to (3d) described below;
[0055] [Chemical formula] can be incorporated. When these compounds are incorporated into the curable water-dispersible composition, adhesion to a polarizer or a transparent protective film may be improved, which is preferable. From the viewpoint of improving the adhesion and water resistance of the polarizer to the transparent protective film, the content of the compound represented by general formula (3) in the curable water-dispersible composition is 100% by weight based on the total amount excluding water as a solvent. When expressed in terms of %, it is preferably 0.001 to 50% by mass, more preferably 0.1 to 30% by mass, and most preferably 1 to 10% by mass.
[0056] In the general formula (3), the aliphatic hydrocarbon group includes a linear or branched alkyl group which may have a substituent having 1 to 20 carbon atoms, and a cyclic alkyl group which may have a substituent having 3 to 20 carbon atoms. Examples of the aryl group include a phenyl group which may have a substituent having 6 to 20 carbon atoms, and a naphthyl group which may have a substituent having 10 to 20 carbon atoms. Examples of the heterocyclic group include a 5-membered or 6-membered ring group containing at least one hetero atom and optionally having a substituent. These may be linked to each other to form a ring. In general formula (3), R 6 and R 7 is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and most preferably a hydrogen atom.
[0057] The compound represented by general formula (3) has a functional group X which contains a reactive group and is a functional group that can react with the curable component constituting the adhesive layer. Examples of reactive groups that X contains include hydroxyl groups, amino groups, aldehyde groups, carboxyl groups, vinyl groups, (meth)acrylic groups, styryl groups, (meth)acrylamide groups, vinyl ether groups, epoxy groups, oxetane groups, α,β-unsaturated carbonyl groups, mercapto groups, halogen groups, and the like. When the curable resin composition constituting the adhesive layer is curable by active energy rays, the reactive group contained in X is preferably at least one reactive group selected from the group consisting of vinyl group, (meth)acrylic group, styryl group, (meth)acrylamide group, vinyl ether group, epoxy group, oxetane group, and mercapto group. In particular, when the adhesive composition constituting the adhesive layer is radical polymerizable, the reactive group contained in X is preferably at least one reactive group selected from the group consisting of (meth)acrylic group, styryl group, and (meth)acrylamide group. When the compound represented by general formula (1) has a (meth)acrylamide group, it is more preferable because it is highly reactive and increases the copolymerization rate with the active energy ray curable resin composition. Furthermore, it is also preferable because the (meth)acrylamide group has high polarity and excellent adhesiveness, which allows the effects of the present invention to be obtained efficiently. When the curable resin composition constituting the adhesive layer is cationic polymerizable, the reactive group contained in X preferably has at least one functional group selected from hydroxyl group, amino group, aldehyde, carboxyl group, vinyl ether group, epoxy group, oxetane group, and mercapto group. In particular, the presence of an epoxy group is preferred because it provides excellent adhesion between the resulting curable resin layer and the adherend, and the presence of a vinyl ether group is preferred because it provides excellent curability of the curable resin composition.
[0058] In the present invention, the compound represented by general formula (3) may be one in which the reactive group and the boron atom are directly bonded. However, as shown in the specific examples above, it is preferable that the compound represented by general formula (3) is one in which the reactive group and the boron atom are bonded via an organic group, that is, a compound represented by general formula (3'). When the compound represented by general formula (3) is bonded to the reactive group via, for example, an oxygen atom bonded to the boron atom, the adhesive water resistance of the polarizing film tends to deteriorate. On the other hand, when the compound represented by general formula (3) does not have a boron-oxygen bond, but rather has a boron-carbon bond formed by the bonding of the boron atom to an organic group, while also containing a reactive group (in the case of general formula (3')), it is preferable because the adhesive water resistance of the polarizing film improves. Specifically, the aforementioned organic group refers to an organic group having 1 to 20 carbon atoms that may have substituents. More specifically, examples include a linear or branched alkylene group that may have substituents with 1 to 20 carbon atoms, a cyclic alkylene group that may have substituents with 3 to 20 carbon atoms, a phenylene group that may have substituents with 6 to 20 carbon atoms, and a naphthylene group that may have substituents with 10 to 20 carbon atoms.
[0059] In addition to the compounds exemplified above, examples of compounds represented by general formula (3) include esters of (meth)acrylates and boric acid, such as esters of hydroxyethyl acrylamide and boric acid, esters of methylol acrylamide and boric acid, esters of hydroxyethyl acrylate and boric acid, and esters of hydroxybutyl acrylate and boric acid.
[0060] In the present invention, the curable aqueous dispersion composition is preferably a forced-emulsification emulsion using a surfactant as an emulsifier in order to achieve both the dispersibility of polymerizable compound A, which has a viscosity of 100 mPa·s or more or is solid at 25°C, and the appearance of the coating film, and furthermore, to improve the humidification reliability of the polarizing film. In the case of a self-emulsifying type in which hydrophilic groups are introduced into the polymerizable compound or polymer compound contained in the curable aqueous dispersion composition, it may not be possible to improve the appearance of the coating film and the humidification reliability of the polarizing film. Methods for forcibly emulsifying the curable aqueous dispersion composition can be, for example, by an ultrasonic homogenizer, a high-speed rotary homogenizer, other pulverizing devices that use cavitation phenomena, or a wet atomizing device that causes liquids to collide obliquely with each other under high pressure, or by a media pulverizing device such as a ball mill, or a stirrer using stirring blades. In the present invention, methods known to those skilled in the art are not limited to these and can be used.
[0061] A polarizing film produced by the manufacturing method according to the present invention is a polarizing film having a cured layer on at least one surface, characterized in that the cured layer is a cured layer of the curable aqueous dispersion composition described above. In the present invention, it is preferable that the polarizing film is a polarizing film in which a polarizer and a transparent protective film are laminated with an adhesive layer in between, and that the adhesive layer comprises a cured layer of a resin layer formed by coating and drying the curable aqueous dispersion composition.
[0062] In the present invention, the polarizer is not particularly limited and various types can be used. Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol-based films, partially formalized polyvinyl alcohol-based films, and partially saponified ethylene-vinyl acetate copolymer films, to which iodine is adsorbed and then uniaxially stretched. Examples of polarizer thickness include 3 to 20 μm.
[0063] However, in this invention, from the viewpoint of improving humidification reliability in harsh environments with high temperature and high humidity, it is preferable to use a thin polarizer with a thickness of 3 μm or more and 15 μm or less as the polarizer. It is particularly preferable that it be 12 μm or less, even more preferably 10 μm or less, and especially preferably 8 μm or less. Such thin polarizers have little thickness variation, excellent visibility, and excellent durability against thermal shock due to little dimensional change.
[0064] A polarizer made by dyeing a polyvinyl alcohol-based film with iodine and then uniaxially stretching it can be produced, for example, by dyeing the polyvinyl alcohol by immersing it in an aqueous solution of iodine and then stretching it to 3 to 7 times its original length. Boric acid, zinc sulfate, zinc chloride, etc., may be included as needed, or the film may be immersed in an aqueous solution of potassium iodide, etc. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water removes dirt and anti-blocking agents from the film surface, and also prevents uneven dyeing by swelling the film. Stretching may be performed after dyeing with iodine, while dyeing, or after stretching. Stretching can also be performed in aqueous solutions of boric acid or potassium iodide, or even in a water bath.
[0065] It is preferable for the polarizer to contain boric acid from the viewpoint of stretch stability and humidification reliability. Furthermore, from the viewpoint of suppressing the occurrence of through cracks, the boric acid content in the polarizer is preferably 22% by mass or less, and more preferably 20% by mass or less, relative to the total amount of the polarizer. From the viewpoint of stretch stability and humidification reliability, the boric acid content relative to the total amount of the polarizer is preferably 10% by mass or more, and more preferably 12% by mass or more.
[0066] Typical examples of thin polarizers include, Patent No. 4751486 specification, Patent No. 4751481 specification, Patent No. 4815544 specification, Patent No. 5048120 specification, International Publication No. 2014 / 077599 pamphlet, International Publication No. 2014 / 077636 pamphlet, Examples include thin polarizers described in the text or thin polarizers obtained from the manufacturing methods described therein.
[0067] As for the thin polarizers, among manufacturing methods that include a step of stretching in a laminated state and a step of dyeing, those obtained by a manufacturing method that includes a step of stretching in a boric acid aqueous solution, as described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, and Japanese Patent No. 4815544, are preferred because they can be stretched to a high magnification and their polarization performance can be improved. In particular, those obtained by a manufacturing method that includes a step of auxiliary air stretching before stretching in a boric acid aqueous solution, as described in Japanese Patent No. 4751481 and Japanese Patent No. 4815544, are preferred. These thin polarizers can be obtained by a manufacturing method that includes a step of stretching a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a stretching resin substrate in a laminated state and a step of dyeing. With this manufacturing method, even if the PVA-based resin layer is thin, it is possible to stretch it without problems such as breakage due to stretching because it is supported by the stretching resin substrate.
[0068] In the method for manufacturing a polarizing film according to the present invention, it is preferable to include a treatment step in which an activation treatment is performed on the coated surface of the curable aqueous dispersion composition before the coating step in which the curable aqueous dispersion composition is coated on at least one surface of the polarizer. The activation treatment introduces hydrophilic functional groups (-COOH and -OH) and radical active species to the surface of the polarizer (polyvinyl alcohol-based polarizer). The introduced hydrophilic functional groups and radical active species improve the wettability of the curable aqueous dispersion composition, which is preferable because it improves the adhesion between the resin layer formed after the drying step and the polarizer. In addition, it is preferable because when the resin layer is cured and a cured product layer (adhesive layer) is formed, the polymerizable compound A constituting the resin layer reacts with the hydrophilic functional groups and radical active species on the polarizer surface, resulting in strong adhesion between the adhesive layer and the polarizer.
[0069] The activation treatment can be at least one of the following: corona treatment, plasma treatment, glow treatment, and ozone treatment. Corona treatment can be performed, for example, by discharging a discharge in atmospheric pressure air using a corona treatment machine. Plasma treatment can be performed, for example, by discharging a discharge in atmospheric pressure air or in an inert gas atmosphere such as nitrogen or argon using a plasma discharge machine. Glow treatment and ozone treatment can also be performed according to conventional methods. Among these, corona treatment is preferable in terms of equipment costs and processing costs.
[0070] The activation treatment can be performed by appropriately adjusting the treatment conditions so that hydrophilic functional groups or radical-active species can be introduced to the polarizer surface. For example, in corona treatment, the discharge rate can be 10 to 500 W / m 2 Approximately 20-300 W / m² / min 2 It is preferable to adjust it to / min.
[0071] As materials constituting the transparent protective film, for example, thermoplastic resins that are excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy are used. Specific examples of such thermoplastic resins include cellulose resins such as triacetylcellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The transparent protective film may contain one or more suitable additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, mold release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the above thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the above-mentioned thermoplastic resin in the transparent protective film is 50% by weight or less, the high transparency and other properties inherent to the thermoplastic resin may not be fully realized.
[0072] Furthermore, the material used to form the transparent protective film is preferably one that is excellent in terms of transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy, and is particularly good if it has a moisture permeability of 150 g / m². 2 It is more preferable that the amount is 24 hours or less, and 140 g / m² 2 Products with a shelf life of 24 hours or less are particularly preferred, and the density is 120 g / m². 2 Even better are those with a shelf life of 24 hours or less.
[0073] Functional layers such as a hard coat layer, anti-reflective layer, anti-sticking layer, diffusion layer, or anti-glare layer can be provided on the surface of the transparent protective film to which the polarizer is not attached. These functional layers can be provided on the transparent protective film itself, or they can be provided separately from the transparent protective film.
[0074] The thickness of the transparent protective film can be determined as appropriate, but generally it is about 1 to 500 μm, preferably 1 to 300 μm, and more preferably 5 to 200 μm, considering factors such as strength, workability, and thinness. Furthermore, 10 to 200 μm is preferred, and 20 to 80 μm is preferred.
[0075] As the transparent protective film, a phase difference film having a front phase difference of 40 nm or more and / or a thickness direction phase difference of 80 nm or more can be used. The front phase difference is usually controlled in the range of 40 to 200 nm, and the thickness direction phase difference is usually controlled in the range of 80 to 300 nm. When a phase difference film is used as the transparent protective film, the phase difference film also functions as a transparent protective film, thus enabling a thinner design.
[0076] To enhance adhesion to the polarizer, the transparent protective film may be subjected to a surface modification treatment on the bonding surface with the polarizer. Specific treatments include corona treatment, plasma treatment, flame treatment, ozone treatment, primer treatment, glow treatment, saponification treatment, and treatment with coupling agents. Among these, corona treatment is preferable in terms of equipment and processing costs. Treatment conditions, such as discharge amount, are the same as those used when treating the polarizer.
[0077] Examples of phase difference films include birefringent films made by uniaxial or biaxial stretching of polymer materials, liquid crystal polymer orientation films, and films in which a liquid crystal polymer orientation layer is supported by a film. There are no particular restrictions on the thickness of the phase difference film, but it is generally around 20 to 150 μm.
[0078] As for the phase difference film, the following formulas (1) to (3): 0.70 <Re
[0450] / Re
[0550] <0.97···(1) 1.5 × 10 -3 <Δn<6×10 -3 ...(2) 1.13 <NZ<1.50···(3) A reverse wavelength-dispersive phase difference film that satisfies the following equation may also be used: (In the formula, Re
[0450] and Re
[0550] are the in-plane phase difference values of the phase difference film measured with light of wavelengths 450 nm and 550 nm at 23°C, respectively; Δn is the in-plane birefringence nx-ny when the refractive indices in the slow axis direction and the fast axis direction of the phase difference film are nx and ny, respectively; and NZ is the ratio of the thickness-direction birefringence nx-nz to the in-plane birefringence nx-ny when nz is the refractive index in the thickness direction of the phase difference film).
[0079] A polarizing film manufactured by the manufacturing method according to the present invention may be provided with a phase difference layer. The phase difference layer may be a single layer or multiple layers, and the phase difference layer may also serve as a protective layer for the polarizer. In the polarizing film of the present invention, for example, a first phase difference layer and a second phase difference layer are bonded together via an adhesive layer. The type, number, combination, arrangement position, and characteristics of the phase difference layer can be appropriately set according to the purpose.
[0080] Liquid crystalline compounds are preferably used to form the phase difference layer. A solvent containing the liquid crystalline compound can be applied using, for example, a wire bar, gap coater, comma coater, gravure coater, or slot die. The applied liquid crystalline solution may be air-dried or heat-dried. It is preferable to apply the liquid crystalline solution at a concentration lower than the isotropic phase-liquid crystal phase transition concentration, i.e., in an isotropic phase state. In this case, the solution can be stably oriented by methods such as rubbing or photo-alignment.
[0081] In the polarizing film manufactured by the manufacturing method according to the present invention, it is preferable that a polarizer and a transparent protective film are laminated together via an adhesive layer. The adhesive layer may consist only of a cured product layer of a curable aqueous dispersion composition, or only of a cured product layer of a curable resin composition, or it may contain both a cured product layer of a curable aqueous dispersion composition and a cured product layer of a curable resin composition. In the polarizing film shown in Figure 1, the polarizer 1 and the transparent protective film 3 are laminated together via an adhesive layer 7 containing a cured product layer 2 of a curable aqueous dispersion composition and a cured product layer 4 of a curable resin composition, and furthermore, the side of the polarizer 1 opposite to the cured product layer 2 is bonded to a glass substrate 6 via an adhesive layer 5. The adhesive layer 7 may have a structure in which the cured product layer 2 and the cured product layer 4 are separated, or it may have a structure in which at least a part of the cured product layer 2 and the cured product layer 4 are compatible.
[0082] Furthermore, the polarizing film produced by the manufacturing method according to the present invention may include a laminate in which a transparent protective film, a phase difference film, or a phase difference layer is laminated via an adhesive layer. The adhesive layer may consist only of a cured product layer of a curable aqueous dispersion composition, or only of a cured product layer of a curable resin composition, or it may contain both a cured product layer of a curable aqueous dispersion composition and a cured product layer of a curable resin composition. A polarizing film in which the laminate is further laminated with a polarizer can also be preferably used in the present invention.
[0083] In the polarizing film shown in Figure 1, the film thickness of the cured product layer 2 of the curable water-dispersible composition is preferably 0.1 to 5.0 μm, and more preferably 0.3 to 3.0 μm, from the viewpoint of improving humidification reliability. Furthermore, the film thickness of the cured product layer 4 of the curable resin composition is preferably 0.1 to 3.0 μm, and more preferably 0.3 to 2.0 μm, from the viewpoint of improving humidification reliability and adhesion. In addition, the thickness of the adhesive layer 7 (the total film thickness of the cured product layer 2 of the curable water-dispersible composition and the cured product layer 4 of the curable resin composition) is preferably 0.2 to 5.1 μm, and more preferably 0.5 to 3.0 μm.
[0084] The polarizing film produced by the manufacturing method according to the present invention may have a configuration other than that shown in Figure 1. In the polarizing film shown in Figure 2, the polarizer 1 and the transparent protective film 3 are laminated via an adhesive layer 7 which comprises only a cured product layer 2 of a curable water-dispersible composition, and the side of the polarizer 1 opposite to the cured product layer 2 is further bonded to the glass substrate 6 via an adhesive layer 5. The thickness of the cured product layer 2 of the curable water-dispersible composition (= thickness of the adhesive layer 7) is preferably 0.1 to 5.0 μm, and more preferably 0.3 to 3.0 μm, from the viewpoint of improving humidification reliability.
[0085] The polarizing film shown in Figure 3 has a cured product layer 2 of a curable water-dispersible composition on one side of the polarizer 1, and the side of the polarizer 1 opposite to the cured product layer 2 is bonded to a transparent protective film 3 via a cured product layer 4 of a curable resin composition. The side of the transparent protective film 3 opposite to the cured product layer 4 is bonded to a glass substrate 6 via an adhesive layer 5. The polarizing film shown in Figure 3 does not contain a cured product layer 2 of a curable water-dispersible composition in the adhesive layer (cured product layer 4 of a curable resin composition) between the polarizer 1 and the transparent protective film 3, but because the polarizer 1 has a cured product layer 2 on the side opposite to the transparent protective film, the elution of iodine from the polarizer is suppressed, and the humidification reliability is significantly improved.
[0086] In the polarizing film shown in Figure 3, the film thickness of the cured product layer 2 of the curable water-dispersible composition is preferably 0.1 to 10 μm, and more preferably 0.3 to 5.0 μm, from the viewpoint of improving humidification reliability. Furthermore, the film thickness of the cured product layer (adhesive layer) 4 of the curable resin composition is preferably 0.1 to 3.0 μm, and more preferably 0.3 to 2.0 μm, from the viewpoint of improving humidification reliability and adhesion.
[0087] The following describes the curable resin composition that constitutes the adhesive layer (cured layer) of the polarizing film produced by the manufacturing method according to the present invention. In the present invention, the "curable water dispersion composition" contains water as a solvent and polymerizable compound A, and preferably polymerizable compound A contains polymerizable compound A having a viscosity of 100 mPa·s or more or being solid at 25°C, and a surfactant. On the other hand, the "curable resin composition" mainly contains polymerizable compound B other than polymerizable compound A and does not contain water as a solvent, and even if it does contain water, the water content is 5.0% by weight or less, particularly 2.0% by weight or less, and even more particularly 1.0% by weight or less, when the total amount in the curable resin composition is 100% by weight.
[0088] Curable resin compositions can be classified into radical polymerization curable resin compositions and cationic polymerization curable resin compositions. In this invention, active energy rays in the wavelength range of 10 nm to less than 380 nm are denoted as ultraviolet light, and active energy rays in the wavelength range of 380 nm to 800 nm are denoted as visible light.
[0089] Examples of monomer components constituting the radical polymerization-curable resin composition include polymerizable compound B other than polymerizable compound A, preferably polymerizable compound having a viscosity of less than 100 mPa·s at 25°C, and more preferably polymerizable compound having a viscosity of 50 mPa·s or less at 25°C.
[0090] Polymerizable compound B includes compounds having a radically polymerizable functional group of a carbon-carbon double bond, such as a (meth)acryloyl group or a vinyl group. These monomer components can be either monofunctional radical polymerizable compounds or polyfunctional radical polymerizable compounds having two or more polymerizable functional groups. Furthermore, these radical polymerizable compounds can be used individually or in combination of two or more. As these radical polymerizable compounds, for example, compounds having a (meth)acryloyl group are preferred. In this invention, (meth)acryloyl means an acryloyl group and / or a methacryloyl group, and "(meth)" has the same meaning hereafter.
[0091] Examples of monofunctional radical polymerizable compounds include (meth)acrylamide derivatives having a (meth)acrylamide group. (Meth)acrylamide derivatives are preferred for ensuring adhesion to polarizers and various transparent protective films, and for their fast polymerization rate and excellent productivity. Specific examples of (meth)acrylamide derivatives include, for example, N-alkyl group-containing (meth)acrylamide derivatives such as N-methyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and N-hexyl(meth)acrylamide; N-hydroxyalkyl group-containing (meth)acrylamide derivatives such as N-methylol(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N-methylol-N-propane(meth)acrylamide; N-aminoalkyl group-containing (meth)acrylamide derivatives such as aminomethyl(meth)acrylamide and aminoethyl(meth)acrylamide; N-alkoxy group-containing (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide; and N-mercaptoalkyl group-containing (meth)acrylamide derivatives such as mercaptomethyl(meth)acrylamide and mercaptoethyl(meth)acrylamide. Furthermore, examples of heterocyclic (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocycle include N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine.
[0092] Among the (meth)acrylamide derivatives mentioned above, N-hydroxyalkyl group-containing (meth)acrylamide derivatives are preferred from the viewpoint of adhesion to polarizers and various transparent protective films. Examples of monofunctional radical polymerizable compounds include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specifically, examples include alkyl esters of (meth)acrylic acid (with 1-20 carbon atoms), such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.
[0093] Furthermore, the (meth)acrylic acid derivatives include, for example, cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-ylmethyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyl acrylate. Examples include polycyclic (meth)acrylates such as methyl (meth)acrylate and dicyclopentanyl (meth)acrylate; and alkoxy group or phenoxy group-containing (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxy polyethylene glycol (meth)acrylate.
[0094] Furthermore, the (meth)acrylic acid derivatives include hydroxyalkyl compounds such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. (meth)acrylates, hydroxyl group-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl(meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl(meth)acrylate and 4-hydroxybutyl(meth)acrylate glycidyl ether; 2,2,2-trifluoroethyl(meth)acrylate and 2,2,2-trifluoroethylethyl(meth)acrylate Halogen-containing (meth)acrylates such as acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate Examples include oxetane group-containing (meth)acrylates such as rilate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, and 3-hexyl-oxetanylmethyl (meth)acrylate; heterocyclic (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate; and neopentyl glycol (meth)acrylic acid adduct of hydroxypivalate and p-phenylphenol (meth)acrylate.
[0095] Furthermore, examples of monofunctional radical polymerizable compounds include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0096] Examples of monofunctional radical polymerizable compounds include lactam-based vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; and nitrogen-containing heterocyclic vinyl monomers such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine.
[0097] Furthermore, as a monofunctional radical polymerizable compound, a radical polymerizable compound having an active methylene group can be used. A radical polymerizable compound having an active methylene group is a compound that has an active double bond group such as a (meth)acrylic group at its terminal or in the molecule, and also has an active methylene group. Examples of active methylene groups include an acetoacetyl group, an alkoxymalonyl group, or a cyanoacetyl group. It is preferable that the active methylene group is an acetoacetyl group. Specific examples of radical polymerizable compounds having an active methylene group include acetoacetoxyalkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and 2-acetoacetoxy-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxymethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radical polymerizable compound having an active methylene group is preferably an acetoacetoxyalkyl (meth)acrylate.
[0098] Furthermore, examples of polyfunctional radical polymerizable compounds having two or more polymerizable functional groups include tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol Examples include esters of (meth)acrylic acid with polyhydric alcohols such as di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dioxaneglycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerin tetra(meth)acrylate, as well as 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include Aronics M-220 (manufactured by Toagosei Co., Ltd.), Light Acrylate 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer), CD-536 (manufactured by Sartomer), etc. In addition, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, and various (meth)acrylate monomers may be used as needed.
[0099] In the present invention, the curable resin composition may contain, in addition to the radical polymerizable compound, an acrylic oligomer obtained by polymerizing (meth)acrylic monomer. By including an acrylic oligomer in the adhesive composition, curing shrinkage when the composition is irradiated and cured with active energy rays can be reduced, and interfacial stress between the adhesive layer and the adherend such as a polarizer and optical film can be reduced. As a result, a decrease in adhesion between the adhesive layer and the adherend can be suppressed.
[0100] When considering workability and uniformity during coating, it is preferable for the curable resin composition to have low viscosity; therefore, it is preferable for the acrylic oligomer obtained by polymerizing (meth)acrylic monomer to also have low viscosity. As an acrylic oligomer that has low viscosity and can prevent curing shrinkage of the adhesive layer, it is preferable that the weight-average molecular weight (Mw) of the acrylic oligomer is 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to sufficiently suppress curing shrinkage of the cured product layer (adhesive layer), it is preferable that the weight-average molecular weight (Mw) of the acrylic oligomer is 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more. Examples of (meth)acrylic monomers that constitute acrylic oligomers include, specifically, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, S-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,Alkyl esters of (meth)acrylic acid (C1-C20) such as 2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, N-octadecyl (meth)acrylate, and also, for example, cycloalkyl (meth)acrylates (e.g., cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, etc.), aralkyl (meth)acrylates (e.g., benzyl (meth)acrylate, etc.), polycyclic (meth)acrylates (e.g., 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl ( (meth)acrylates, etc.), hydroxyl group-containing (meth)acrylic acid esters (e.g., hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethyl-butyl (meth)methacrylate, etc.), alkoxy group- or phenoxy group-containing (meth)acrylic acid esters (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), epoxy group-containing (meth)acrylic acid esters (e.g., glycidyl (meth)acrylate, etc.), halogen-containing (meth)acrylic acid esters (e.g., 2,2,2-trifluoroethyl (meth)acrylate, 2,2Examples include 2-trifluoroethylethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, etc., and alkylaminoalkyl (meth)acrylates (e.g., dimethylaminoethyl (meth)acrylate). These (meth)acrylates can be used alone or in combination of two or more types. Specific examples of acrylic oligomers (E) include "ARUFON" from Toagosei Co., Ltd., "Actflow" from Soken Chemical Co., Ltd., and "JONCRYL" from BASF Japan.
[0101] The amount of acrylic oligomer blended is preferably 15 parts by weight or less per 100 parts by weight of the total monomer components in the curable resin composition. If the acrylic oligomer content in the composition is too high, the reaction rate when the composition is irradiated with active energy rays will decrease drastically, which may result in poor curing. On the other hand, in order to sufficiently suppress curing shrinkage of the adhesive layer, it is preferable to contain 3 parts by weight or more of acrylic oligomer in the composition.
[0102] It is preferable to incorporate a photopolymerization initiator into the curable resin composition, and the same photopolymerization initiators that can be incorporated into the curable aqueous dispersion composition can be used as such.
[0103] Cationic polymerizable compounds used in cationic polymerizable resin compositions are classified into monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule, and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule. Monofunctional cationic polymerizable compounds have relatively low liquid viscosity, and by including them in cationic polymerizable resin compositions, the liquid viscosity can be reduced. Furthermore, monofunctional cationic polymerizable compounds often have functional groups that exhibit various functions, and by including them in cationic polymerizable resin compositions, various functions can be exhibited in the cationic polymerizable resin composition and / or the cured product of the cationic polymerizable resin composition. Polyfunctional cationic polymerizable compounds can cause three-dimensional crosslinking of the cured product of the cationic polymerizable resin composition, and therefore, it is preferable to include them in cationic polymerizable resin compositions. The ratio of monofunctional cationic polymerizable compounds to polyfunctional cationic polymerizable compounds is preferably in the range of 10 to 1000 parts by weight of polyfunctional cationic polymerizable compounds per 100 parts by weight of monofunctional cationic polymerizable compounds. Examples of cationic polymerizable functional groups include epoxy groups, oxetanyl groups, and vinyl ether groups. Examples of compounds having epoxy groups include aliphatic epoxy compounds, alicyclic epoxy compounds, and aromatic epoxy compounds. The cationic polymerizable adhesive composition of the present invention is particularly preferably composed of an alicyclic epoxy compound because it exhibits excellent curability and adhesion. Examples of alicyclic epoxy compounds include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified, trimethylcaprolactone-modified, and valerolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and specifically, Celoxide 2021, Celoxide 2021A, Celoxide 2021P, Celoxide 2081, Celoxide 2083, Celoxide 2085 (all manufactured by Daicel Chemical Industries, Ltd.), and Cyracure UVR-6105, Cyracure UVR-6107, Cyracure 30, R-6110 (all manufactured by Dow Chemical Japan Ltd.).Compounds containing an oxetanyl group are preferable to include in cationic polymerizable adhesive compositions because they improve the curability of the composition and reduce its liquid viscosity. Examples of compounds containing an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and phenol novolac oxetane. Aronoxetane OXT-101, Aronoxetane OXT-121, Aronoxetane OXT-211, Aronoxetane OXT-221, and Aronoxetane OXT-212 (all manufactured by Toagosei Co., Ltd.) are commercially available. Compounds having vinyl ether groups are preferable to include because they have the effect of improving the curability of cationic polymerizable adhesive compositions and reducing the liquid viscosity of the compositions. Examples of compounds having vinyl ether groups include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, cyclohexanedimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol-type tetravinyl ether.
[0104] Cationic polymerization curable resin compositions contain at least one compound selected from the epoxy group-containing compounds, oxetanyl group-containing compounds, and vinyl ether group-containing compounds described above as curable components, all of which cure by cationic polymerization; therefore, a photocationic polymerization initiator is incorporated. This photocationic polymerization initiator generates cationic species or Lewis acids upon irradiation with active energy rays such as visible light, ultraviolet light, X-rays, and electron beams, and initiates the polymerization reaction of epoxy groups and oxetanyl groups. As the photocationic polymerization initiator, the photoacid generator described later is preferably used. Furthermore, when using a cationic polymerization adhesive composition that is curable with visible light, it is preferable to use a photocationic polymerization initiator that is particularly sensitive to light of 380 nm or higher. However, since photocationic polymerization initiators are generally compounds that show maximum absorption around 300 nm or shorter wavelengths, by incorporating a photosensitizer that shows maximum absorption in a longer wavelength range, specifically light with wavelengths longer than 380 nm, it is possible to stimulate light of this wavelength range and promote the generation of cationic species or acids from the photocationic polymerization initiator. Examples of photosensitizers include anthracene compounds, pyrene compounds, carbonyl compounds, organosulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, and photoreducible dyes. Two or more of these may be used in combination. Anthracene compounds are particularly preferred due to their excellent photosensitizing effect, and specific examples include Anthracure UVS-1331 and Anthracure UVS-1221 (manufactured by Kawasaki Chemical Co., Ltd.). The photosensitizer content is preferably 0.1% to 5% by weight, and more preferably 0.5% to 3% by weight.
[0105] The method for manufacturing a polarizing film according to the present invention comprises a coating step of coating a curable aqueous dispersion composition onto at least one surface of a polarizer, and a drying step of forming a resin layer by drying the curable aqueous dispersion composition. Preferably, after the drying step, the method further comprises a curing step of irradiating the resin layer with active energy rays to cure it, thereby forming a cured product layer, or an adhesive layer comprising at least the cured product layer. Preferably, the method also comprises a processing step of performing an activation treatment on the coated surface of the curable aqueous dispersion composition before the coating step of coating at least one surface of the polarizer. Each step will be described below.
[0106] (Coating process) In the coating process, a curable aqueous dispersion composition is applied to at least one surface of the polarizer. In this coating process, when a curable aqueous dispersion composition containing water as a solvent and polymerizable compound A is applied to at least one surface of the polarizer, the applied water dissolves the iodine complex present on the polarizer surface. This makes it possible to lower the refractive index of the polarizer on the long-wavelength side, and when an adhesive layer is finally formed on the polarizer, it is possible to reduce the refractive index difference between the polarizer and the adhesive layer, especially on the long-wavelength side. As a result, a polarizing film with excellent appearance and less interference unevenness can be manufactured. The method for applying the curable aqueous dispersion composition and / or curable resin composition is appropriately selected depending on the viscosity of the composition and the desired thickness, and examples include reverse coaters, gravure coaters (direct, reverse, and offset), bar reverse coaters, roll coaters, die coaters, bar coaters, and rod coaters. Lamination of substrates such as polarizers and optical films can be performed using a roll laminator or the like.
[0107] When manufacturing optical films, particularly polarizing films, according to the present invention in a continuous line, the line speed depends on the curing time of the curable aqueous dispersion composition and / or curable resin composition, but is preferably 5 to 100 m / min, more preferably 10 to 50 m / min, and even more preferably 20 to 30 m / min. If the line speed is too low, productivity will be poor, or the damage to the transparent protective film will be too great, making it impossible to produce a polarizing film that can withstand durability tests, etc. If the line speed is too high, the curing of the curable aqueous dispersion composition and / or curable resin composition will be insufficient, and the desired adhesion may not be obtained.
[0108] (drying process) In the drying process, a resin layer is formed by drying the curable aqueous dispersion composition. During the drying process, although water evaporates, the iodine complex dissolved in water remains in the resin layer when the resin layer containing polymerizable compound A is formed. As a result, even when a polarizing film having a cured layer (adhesive layer) formed by irradiating the resin layer formed after the drying process with active energy rays is placed under harsh environments of high temperature and high humidity, the elution of iodine in the polarizer is suppressed. Therefore, the method for manufacturing a polarizing film according to the present invention makes it possible to manufacture a polarizing film with excellent humidification reliability. As drying means used in the drying process, methods known to those skilled in the art (e.g., a blower (with temperature control as needed)) can be used.
[0109] (hardening process) In the curing process, after the drying process, the resin layer is irradiated with active energy rays to harden it, thereby forming a cured layer, or an adhesive layer comprising at least the cured layer. The irradiation direction of the active energy rays (electron beams, ultraviolet rays, visible light, etc.) can be any appropriate direction.
[0110] (Processing steps) In the processing step, before the coating step in which the curable aqueous dispersion composition is applied to at least one surface of the polarizer, an activation treatment is performed on the surface of the curable aqueous dispersion composition. As described above, hydrophilic functional groups and radical active species are introduced to the surface of the polarizer by an activation treatment such as corona treatment. If the polarizing film is a polarizing film in which a polarizer and a transparent protective film are laminated with an adhesive layer in between, the processing step may also be performed on the transparent protective film.
[0111] The polarizing film produced by the manufacturing method of the present invention can be used in practical applications as an optical film laminated with other optical layers. There are no particular limitations on the optical layers, but for example, one or more optical layers that are used in the formation of liquid crystal display devices such as reflectors, semitransparent plates, phase difference plates (including 1 / 2 and 1 / 4 wave plates), and viewing angle compensation films can be used. Particularly preferred are reflective polarizing films or semitransparent polarizing films in which a reflector or semitransparent reflector is further laminated on the polarizing film of the present invention, elliptic polarizing films or circular polarizing films in which a phase difference plate is further laminated on the polarizing film, wide-viewing-angle polarizing films in which a viewing angle compensation film is further laminated on the polarizing film, or polarizing films in which a brightness-enhancing film is further laminated on the polarizing film.
[0112] An optical film, formed by laminating the above-mentioned optical layer onto a polarizing film, can be formed by sequentially laminating the layers separately during the manufacturing process of liquid crystal display devices, etc. However, a pre-laminated optical film offers advantages such as superior quality stability and ease of assembly, which can improve the manufacturing process of liquid crystal display devices, etc. Appropriate adhesive means, such as an adhesive layer, can be used for lamination. When bonding the above-mentioned polarizing film and other optical films, their optical axes can be positioned at an appropriate angle depending on the desired phase difference characteristics.
[0113] The aforementioned polarizing film, or an optical film having at least one layer of polarizing film laminated on it, may also be provided with an adhesive layer for bonding to other components such as liquid crystal cells. The adhesive used to form the adhesive layer is not particularly limited, but for example, an adhesive based on polymers such as acrylic polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyethers, fluorine-based or rubber-based polymers can be appropriately selected and used. In particular, adhesives that have excellent optical transparency, exhibit appropriate wettability, cohesiveness and adhesive properties, and have excellent weather resistance and heat resistance, such as acrylic adhesives, are preferably used.
[0114] The adhesive layer can be provided on one or both sides of the polarizing film or optical film as a superimposed layer of different compositions or types. When provided on both sides, the adhesive layers on the front and back of the polarizing film or optical film can have different compositions, types, or thicknesses. The thickness of the adhesive layer can be appropriately determined according to the intended use and adhesive strength, and is generally 1 to 100 μm, preferably 5 to 30 μm, and particularly preferably 10 to 20 μm.
[0115] For the exposed surface of the adhesive layer, a separator is temporarily attached and covered to prevent contamination until it is put into practical use. This prevents contact with the adhesive layer under normal handling conditions. As for the separator, apart from the thickness conditions mentioned above, suitable thin materials such as plastic film, rubber sheet, paper, cloth, nonwoven fabric, net, foam sheet, metal foil, or laminates thereof can be used, and may be coated with a suitable release agent such as silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide as needed, in accordance with conventional methods.
[0116] The polarizing film produced by the manufacturing method of the present invention can be suitably used in the formation of various devices such as liquid crystal display devices. The formation of liquid crystal display devices can be carried out in accordance with conventional methods. That is, liquid crystal display devices are generally formed by appropriately assembling components such as liquid crystal cells, polarizing films or optical films, and, if necessary, lighting systems, and incorporating drive circuits. However, the present invention is not particularly limited except for the use of the polarizing film or optical film according to the present invention, and can be carried out in accordance with conventional methods. Any type of liquid crystal cell can be used, such as TN type, STN type, or π type.
[0117] Appropriate liquid crystal display devices can be formed, such as liquid crystal display devices in which a polarizing film or optical film is placed on one or both sides of a liquid crystal cell, or in which a backlight or reflector is used in the lighting system. In this case, the polarizing film or optical film according to the present invention can be installed on one or both sides of the liquid crystal cell. When polarizing films or optical films are provided on both sides, they may be the same or different. Furthermore, when forming a liquid crystal display device, appropriate components such as a diffuser plate, anti-glare layer, anti-reflective film, protective plate, prism array, lens array sheet, light diffuser plate, and backlight can be placed in appropriate positions in one or more layers. Furthermore, examples of image display devices of the present invention include organic EL (electroluminescent) display devices, PDP (plasma display panel), and electronic paper, and are particularly preferably used in organic EL, which uses a polarizer with high transmittance. In addition, as an application for the image display device, it can be preferably applied to applications that require components that have durability characteristics in high humidity and heat environments, such as foldable display devices and in-vehicle display devices. [Examples]
[0118] The following describes some embodiments of the present invention, but the embodiments of the present invention are not limited to these.
[0119] <Manufacturing of polarizers> A laminate was formed by air-assisted stretching at a stretching temperature of 130°C from an amorphous PET substrate with a 9 μm thick PVA layer. Next, a colored laminate was formed by dyeing the stretched laminate. Furthermore, an optical film laminate containing a 5 μm thick PVA layer was formed by stretching the colored laminate in boric acid water at a stretching temperature of 65°C, integrally with the amorphous PET substrate, to achieve a total stretching ratio of 5.94 times. This two-stage stretching process resulted in an optical film laminate containing a 5 μm thick PVA layer, in which the PVA molecules in the PVA layer formed on the amorphous PET substrate were highly oriented, and the iodine adsorbed by dyeing formed a polyiodide ion complex highly oriented in one direction, constituting a thin polarizer.
[0120] <Transparent protective film> The following film was used as a transparent protective film. "PET"; PET film (product name "Cosmoshine 4300", thickness 50μm, manufactured by Toyobo Co., Ltd.) "TAC"; Triacetylcellulose (TAC) film (product name "TG60UL", thickness 60 μm, manufactured by Fujifilm Corporation)
[0121] <Activated energy rays> The active energy source is visible light (gallium-filled metal halide lamp). Irradiation device: Light HAMMER10 manufactured by Fusion UV Systems, Inc. Bulb: V-bulb Peak illuminance: 1600 mW / cm 2 Total irradiation dose 1000 / mJ / cm 2 (Wavelengths of 380-440 nm were used.) Illuminance of visible light was measured using a Solatell Sola-Check system.
[0122] The curable aqueous dispersion compositions used in Examples 1 to 7 were prepared according to the formulations listed in Table 1 and the methods described below. Each of the materials listed in Table 1 will be described later.
[0123] According to the formulations listed in Table 1, the materials excluding water as the solvent were uniformly mixed. Then, water was added as the solvent, and the mixture was emulsified using a high-pressure homogenizer (device name "L-ES008", manufactured by Yoshida Machinery Industry Co., Ltd.) under conditions of a pressurized pressure of 200 MPa and a temperature of 25°C to prepare the curable aqueous dispersion compositions, which are forced-emulsification type emulsions used in Examples 1 to 8.
[0124] [Table 1]
[0125] The curable resin compositions, which do not contain water as a solvent, were prepared by mixing the compositions used in Comparative Examples 1 to 4, according to the formulations listed in Table 2.
[0126] [Table 2]
[0127] The materials listed in Tables 1 and 2 are as follows: <Polymerizable compound A> • Ethoxylated bisphenol A dimethacrylate [(liquid) / 1220 (mPa·s / 25℃)], product name "BPE-80N", manufactured by Shin Nakamura Chemical Industry Co., Ltd. Ethoxylated o-phenylphenol acrylate [(liquid) / 130 (mPa·s / 25℃)], product name "A-LEN-10", manufactured by Shin Nakamura Chemical Industry Co., Ltd. 9,9-Bis[4-(2-acryloyloxyethoxy)phenyl]fluorene[(liquid) / >100000(mPa·s / 25℃)], manufactured by Shin Nakamura Chemical Industry Co., Ltd. • Dimethylol-tricyclodecanediaacrylate [(liquid) / viscosity 150 (mPa·s / 25℃)], product name "Light Acrylate DCP-A", manufactured by Kyoeisha Chemical Co., Ltd. • Epoxy monomer 1 with a binaphthyl skeleton [(liquid) / >100,000 (mPa·s / 25℃)], trade name "TBIS-RXG", manufactured by Taoka Chemical Industries Co., Ltd. • Epoxy monomer 2[(solid) / -] with a binaphthyl skeleton, trade name "TBIS-GG", manufactured by Taoka Chemical Industries Co., Ltd. Naphthalene-type epoxy monomer [(liquid) / 23000 (mPa·s / 25℃)], product name "HP-4032D", manufactured by DIC Corporation. • Bisphenol-type epoxy monomer [(liquid) / 13000 (mPa·s / 25℃)], product name "jER828", manufactured by Mitsubishi Chemical Corporation. • Dicyclopentadiene type epoxy monomer [(liquid) / 230 (mPa·s / 25℃)], product name "EP-4088S", manufactured by ADEKA Corporation.
[0128] <Polymerizable compound B> • 3-Phenoxybenzyl acrylate [(liquid) / 18 (mPa·s / 25℃)], product name "Light Acrylate POB-A", manufactured by Kyoeisha Chemical Co., Ltd. • Benzyl acrylate [(liquid) / 3 (mPa·s / 25℃)], product name "Viscoat #160", manufactured by Osaka Organic Chemical Industry Co., Ltd. Phenoxyethyl acrylate [(liquid) / 9 (mPa·s / 25℃)], product name "Viscoat #192", manufactured by Osaka Organic Chemical Industry Co., Ltd. • p-tert-butylphenyl glycidyl ether [(liquid) / 20 (mPa·s / 25℃)], trade name "Denacol EX-146", manufactured by Nagase ChemteX Corporation. • Acryloylmorpholin [(liquid) / 12 (mPa·s / 25℃)], trade name "ACMO", manufactured by KJ Chemicals. • 1,4-Cyclohexanedimethanol monoacrylate [(liquid) / 88 (mPa·s / 25℃)], trade name "CHDMMA", manufactured by Mitsubishi Chemical Corporation. • Polypropylene glycol diacrylate [(liquid) / 14 (mPa·s / 25℃)], product name "Aronics M-220", manufactured by Toagosei Co., Ltd. • Alicyclic epoxy compound [(liquid) / 20 (mPa·s / 25℃)], product name "Epocalic THI-DE", manufactured by ENEOS Corporation. 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane [(liquid) / 12 (mPa·s / 25℃)], trade name "Aron Oxetane OXT-221", manufactured by Toagosei Co., Ltd.
[0129] <Silane coupling agent> • 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, trade name "KBM403", manufactured by Shin-Etsu Chemical Co., Ltd. • 3-Methacryloxypropyltrimethoxysilane, trade name "KBM503", manufactured by Shin-Etsu Chemical Co., Ltd. <Photoradical Generator> • Bis(2,4,6-trimethylbenzoyl)phenylphosphorine oxide, trade name "Omnirad 819", manufactured by IGMresins. • 1-Hydroxycyclohexyl-phenyl ketone, trade name "Omnirad 184", manufactured by IGMresins. <Photoacid Generator> • 4-methylphenyl)[4-(2-methylpropyl)phenyl]iodonium hexafluorophosphate (propylene carbonate solution, 75% solids), trade name "Omnicat 250D", manufactured by IGMresins. <Photosensitizer> • Diethylthioxanthone, trade name "KAYACURE DETX-S", manufactured by Nippon Kayaku Co., Ltd. <Surfactants> • Sodium polyoxyethylene styrene-methylphenyl ether sulfate (anionic surfactant, trade name "Newcol 707-SN", manufactured by Nippon Emulsifier Co., Ltd.) <Surface modifier> ·Product name: “EXP.4200”, manufactured by Nissin Chemical Industry Co., Ltd.
[0130] (Manufacturing of polarizing film (the polarizing film shown in Figure 2)) Using a corona irradiation machine (Kasuga Electric Co., Ltd., CT-0212), the thin polarizer side of the optical film laminate (the coated side of the curable aqueous dispersion composition) and the transparent protective film (the laminated side of "PET" and "TAC") were subjected to a discharge of 50 W / m². 2 Corona treatment was performed at / min (processing step).
[0131] Using an MCD coater (manufactured by Fuji Machinery Co., Ltd.) (cell shape: honeycomb, gravure roll line count: as shown in Table 1, rotation speed 140% / line speed), the curable aqueous dispersion composition used in Examples 1-7 or the curable resin composition used in Comparative Examples 1-4 was coated onto the thin polarizer side (processed side) of the optical film laminate (coating process), and then air-dried using a blower (drying process). The coated side of the thin polarizer with the curable aqueous dispersion composition (or curable resin composition) and the processed side of the transparent protective film 3 of the type shown in Table 3 were bonded together using a roll machine (bonding line speed 25 m / min). Subsequently, the curable aqueous dispersion composition and the curable resin composition were cured by irradiating them with a visible light irradiation device from the protective film 3 side (curing step). Then, the amorphous PET substrate of the optical film laminate was peeled off, thereby producing polarizing films in which the polarizer 1 and the transparent protective film 3 were laminated via the cured product layer (=adhesive layer) 2 of the curable aqueous dispersion composition in Examples 1 to 8, and via the cured product layer (=adhesive layer) 2 of the curable resin composition in Comparative Examples 1 to 4. The thickness of the adhesive layer of the obtained polarizing films is shown in Table 1.
[0132] <Humidification durability test> Polarizing films (samples for humidification durability testing) were prepared by laminating the polarizing films produced in Examples 1-8 or Comparative Examples 1-4 to one side of an alkali-free glass 6 with a thickness of 0.7 mm via an adhesive layer (thickness 20 μm) 5. After placing the samples in an environment of 85°C and 85% humidity, a humidification durability test was conducted. Details of the humidification durability test are shown below.
[0133] The obtained polarizing films were exposed to an environment of 85°C and 85% RH for 120 hours. The degree of polarization before and after exposure was measured using a spectrophotometer with an integrating sphere (V7100, manufactured by JASCO Corporation), and the change in degree of polarization ΔY (%) = |(degree of polarization before exposure (%)) - (degree of polarization after exposure (%))| was calculated. A smaller change in degree of polarization ΔY was judged to indicate superior optical durability under harsh humid environments.
[0134] <Appearance (Interference Unevenness) Evaluation Test> In the polarizing films manufactured in Examples 1-8 or Comparative Examples 1-4, the refractive index (along the absorption axis direction of the polarizer) of the polarizer, adhesive layer, and protective film was measured at both the long-wavelength side (782 nm) and the short-wavelength side (594 nm). Interference unevenness occurs when either the refractive index difference between the polarizer and the adhesive layer, or the refractive index difference between the transparent protective film and the adhesive layer, is large at both the long-wavelength side (782 nm) and the short-wavelength side (594 nm). The presence or absence of interference unevenness was evaluated visually, with ◎ indicating no interference unevenness, ○ indicating almost no interference unevenness, and × indicating interference unevenness. The results are shown in Table 3. The methods for measuring the refractive index along the absorption axis direction of the polarizer, and the methods for measuring the refractive index of the adhesive layer and transparent protective film, are described below.
[0135] (Method for measuring the refractive index of a polarizer in the absorption axis direction) The optical film laminates (laminated layers of stretched substrate and polarizing film) obtained during the manufacturing process of each of the above-described examples and comparative examples were uniformly roughened on the surface opposite to the polarizer surface (i.e., the PET surface) with sandpaper, and then colored by applying black paint so that the visible light transmittance was 5% or less. Then, using a spectrophotometer (Hitachi High-Tech Corporation, product name "U-4100"), polarized light was incident on the measurement surface, i.e., the polarizer, at an incident angle of 10 degrees, and the reflectance in the transmission axis direction and absorption axis direction of the polarizer was measured for wavelengths of 594 nm and 782 nm.
[0136] From the values of the reflectance Rt in the transmission axis direction and the reflectance Ra in the absorption axis direction measured above, and assuming the refractive index of air is 1, the refractive index of the polarizer in the transmission axis direction is nt, and the refractive index in the absorption axis direction is na, the relationship is: Rt = ((1-nt) / (1+nt)) 2 Ra = ((1-na) / (1+na)) 2 Using this method, the refractive index of the polarizer at the long wavelength side (782 nm) and the short wavelength side (594 nm) was derived (reduced refractive index).
[0137] (Manufacturing of adhesive layers for refractive index measurement) The adhesive layers formed by curing the curable aqueous dispersion compositions used in Examples 1 to 7 or the curable resin compositions used in Comparative Examples 1 to 4 were prepared for refractive index measurement by the following method.
[0138] Using a wire bar #10, each of the above-mentioned curable aqueous dispersion compositions was coated onto the surface of a COP film (ZF14, 23 μm, manufactured by Zeon Corporation). Another COP film was then bonded to the coated surface of the curable aqueous dispersion composition, and an adhesive layer was formed by irradiating it with active energy rays using a UV lamp (gallium lamp). Subsequently, the adhesive layer for refractive index measurement was prepared by peeling off both COP films.
[0139] (Method for measuring the refractive index of adhesive layers and transparent protective films) The refractive indices of the adhesive layer and transparent protective film obtained above were measured using a prism coupler device (2010 / M) manufactured by METRICON, based on the following measurement conditions. (Measurement conditions) Light source: 594nm or 782nm Mode: TE Scan: 300~-300 Measurement type:Bulk / Substrate The mode (called Knee) was detected by measurement. The refractive index obtained from the measurement of both the adhesive layer for refractive index measurement and the transparent protective film is shown in Table 3.
[0140] [Table 3] The results in Table 3 show that in the polarizing films produced in Examples 1 to 7, the refractive index difference between the polarizer and the adhesive layer is significantly reduced, especially on the long-wavelength side, compared to the polarizing films produced in Comparative Examples 1 to 4. Therefore, it can be seen that in Examples 1 to 8, interference unevenness is sufficiently suppressed, resulting in a polarizing film with excellent appearance and superior humidification reliability.
Claims
1. A method for manufacturing a polarizing film comprising at least a polarizer, The aforementioned polarizer is an iodine-based polarizer containing iodine, A coating step of coating at least one surface of the polarizer with a curable aqueous dispersion composition, A drying step in which a resin layer is formed by drying the curable aqueous dispersion composition, The process includes a curing step in which, after the drying step, an active energy ray is irradiated to harden the resin layer, thereby forming a cured material layer, or an adhesive layer comprising at least the cured material layer, A method for producing a polarizing film, characterized in that the curable aqueous dispersion composition contains water as a solvent and polymerizable compound A, which has a viscosity of 100 mPa·s or more or is solid at 25°C.
2. The method for producing a polarizing film according to claim 1, wherein the curable aqueous dispersion composition contains, as the polymerizable compound A, a hydrophobic polymerizable compound having at least a LogPow of 1.0 or higher.
3. The method for producing a polarizing film according to claim 1 or 2, wherein the curable aqueous dispersion composition contains, as the polymerizable compound A, a polyfunctional polymerizable compound with at least three or more functions.
4. A method for producing a polarizing film according to any one of claims 1 to 3, wherein the curable aqueous dispersion composition further contains a surfactant.
5. The method for producing a polarizing film according to claim 4, wherein the curable aqueous dispersion composition is a forced emulsion using the surfactant as an emulsifier.
6. The method for producing a polarizing film according to claim 4 or 5, wherein the surfactant comprises two or more types of surfactants.
7. A method for producing a polarizing film according to any one of claims 4 to 6, wherein the surfactant is at least two selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
8. The polarizing film is a polarizing film in which the polarizer and the transparent protective film are laminated with an adhesive layer in between. A method for manufacturing a polarizing film according to any one of claims 1 to 7, further comprising a curing step of forming the adhesive layer having at least a cured layer formed by irradiating it with active energy rays after the drying step to harden the resin layer.
Citation Information
Patent Citations
Water-based emulsion composition and adhesive composition
JP2001220474A
Method for manufacturing polarizing plate and liquid crystal display device
JP2001296427A
Aqueous resin emulsion composition for bonding cycloolefinic resin molded product, dry film, method for bonding and cycloolefinic resin laminate
JP2005344022A
Polarizing plate
JP2008261914A
Active energy ray-curable resin composition, adhesive layer, polarizing plate, optical film, and image display device
JP2012052000A