Polyester containers and polyester preforms
A polyester container with a virgin polyester mouth and multilayer recycled polyester structure addresses thermal deformation issues, ensuring airtightness and ease of opening, while preventing antimony leaching and maintaining hygiene.
Patent Information
- Application Number
- JP2019137975
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-07-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2039-07-26
AI Technical Summary
Polyester containers contaminated with antimony catalysts from recycling processes face issues with airtightness and ease of opening when heated, due to thermal deformation of recycled polyester layers, leading to potential leaching of contaminants into contents.
A polyester container design with a mouth portion made of virgin polyester and other layers made of recycled polyester, ensuring airtightness and ease of opening by reducing thermal deformation, while preventing antimony leaching.
The design maintains high hygiene and environmental impact reduction by preventing antimony leaching and ensuring cap sealing performance even when heated, with improved thermal stability and ease of opening.
Smart Images

Figure 0007955038000003 
Figure 0007955038000004 
Figure 0007955038000005
Abstract
Description
Technical Field
[0001] The present invention relates to a polyester container and a polyester preform for use in producing the polyester container. Background Art
[0002] Polyesters such as polyethylene terephthalate are excellent in mechanical properties, chemical stability, heat resistance, gas barrier properties, transparency and the like, and are inexpensive. Thus, such polyesters are widely used for producing containers for filling beverages and the like.
[0003] Polyesters used for producing containers include those using an antimony catalyst as a polymerization catalyst (hereinafter referred to as antimony catalyst polyester) and those using a germanium catalyst (hereinafter referred to as germanium catalyst polyester). Among these polymerization catalysts, the antimony catalyst polyester is particularly frequently used in terms of cost.
[0004] In recent years, for the purpose of reducing environmental load, used polyester containers have been recycled by various methods, and containers have been produced using the obtained polyester (hereinafter referred to as recycled polyester).
[0005] However, polyester containers are not recycled for each polymerization catalyst used in polyester synthesis. Therefore, recycled polyester is very likely to contain an antimony catalyst. Polyester containers may also be contaminated during the collection process or depending on the intended use such as storage of non-food items (e.g., agricultural chemicals or machine oils). It is difficult to completely remove contaminants from recycled polyester.
[0006] Therefore, when polyester containers are repeatedly recycled, contaminants and antimony catalysts that could not be removed accumulate in the recycled polyester, raising concerns about their leaching into the contents filled in the recycled polyester containers. Furthermore, in convenience stores and other establishments, containers filled with contents are often sold upright in a hot warmer, and the aforementioned antimony leaching becomes a particular problem under such heated conditions.
[0007] Incidentally, polyester containers have a cap screwed onto the opening to seal the contents at the time of sale. At the opening of such polyester containers, a male threaded portion for screwing on the cap is formed to protrude from the outer wall, and a flange-shaped support ring is formed to protrude below this male threaded portion (Patent Document 1). Furthermore, as described in Patent Document 2, there are also bottles equipped with an anti-tampering function (tamper-evident), and at the opening of such bottles, a lid is formed between the male threaded portion and the support ring. In addition, there are bottles with a press-fit cap, as described in Patent Document 3. [Prior art documents] [Patent Documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 2001-113589 [Patent Document 2] Japanese Patent Publication No. 2004-26201 [Patent Document 3] Japanese Patent Publication No. 2012-206486 [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] The inventors hypothesized that a polyester container having an inner layer made of virgin polyester without antimony catalyst polyester and an outer layer made of recycled polyester could suppress the leaching of contaminants and antimony into the contents. However, when such a polyester container was filled with contents, sealed with a cap, and then heated in a hot warmer, a problem arose in which the airtightness and ease of opening of the cap were impaired. After diligent investigation, the inventors found that even with a multilayer polyester container having a virgin polyester layer and a recycled polyester layer, the airtightness and ease of opening of the cap can be ensured even when the container is heated by making the mouth portion a single layer of virgin polyester.
[0010] This invention has been made in view of the above findings, and its purpose is to provide a polyester container that has high hygiene and high environmental impact reduction, while also ensuring the airtightness and ease of opening of the cap even when the container is heated. Furthermore, the invention provides a polyester preform used in the manufacture of this polyester container. [Means for solving the problem]
[0011] The present invention relates to a polyester container comprising a mouth portion, a neck portion, shoulder portions, a body portion, and a bottom portion, The opening is a single layer made of virgin polyester. Except for the opening, the structure is multilayered, having at least one layer made of virgin polyester located on the innermost surface and one layer made of recycled polyester. The virgin polyester is characterized by being one or more polyesters selected from manganese-catalyzed polyester, titanium-catalyzed polyester, aluminum-catalyzed polyester, lithium-catalyzed polyester, and germanium-catalyzed polyester.
[0012] In one embodiment, the mouth portion is provided with a support ring at the lower end of the mouth portion.
[0013] In one embodiment, the mouth portion includes an outer fitting portion between an upper end of the mouth portion and the support ring.
[0014] In one embodiment, the mouth portion includes a flange between the outer fitting portion and the support ring.
[0015] In one embodiment, a distance from an upper end to a lower end of the mouth portion is 5 mm or more and 30 mm or less.
[0016] In one embodiment, the polyester container of the present invention has an eluted antimony concentration of less than 6 ppb.
[0017] In one embodiment, a content of the recycled polyester is 40 parts by mass or more and 90 parts by mass or less based on 100 parts by mass of a total amount of the resin material contained in the polyester container.
[0018] In one embodiment, a thickness of the virgin polyester layer is 0.01 mm or more and 0.21 mm or less.
[0019] In one embodiment, the polyester container of the present invention is a container for heating.
[0020] A polyester preform of the present invention is a polyester preform for producing the polyester container described above, the polyester preform includes a mouth portion, a body portion, and a bottom portion, the mouth portion is a single layer made of virgin polyester, a portion other than the mouth portion is a multilayer including a layer made of virgin polyester positioned on an innermost surface and a layer made of recycled polyester, the virgin polyester is one or more polyesters selected from a manganese-catalyzed polyester, a titanium-catalyzed polyester, an aluminum-catalyzed polyester, a lithium-catalyzed polyester, and a germanium-catalyzed polyester.
Effect of the Invention
[0021] According to the present invention, it is possible to provide a polyester container that has high hygiene properties and high environmental load reduction properties, and can ensure cap sealing performance and opening performance even when the container is heated. It is also possible to provide a polyester preform used for manufacturing this polyester container. [Brief Description of the Drawings]
[0022] [Figure 1] Fig. 1 is a schematic half cross-sectional view showing an embodiment of the polyester container of the present invention. [Figure 2] Fig. 2 is a schematic half cross-sectional view showing an embodiment of the polyester container of the present invention. [Figure 3] Fig. 3 is a half cross-sectional view showing a state in which a cap is screwed onto the mouth portion of Fig. 2. [Figure 4] Fig. 4 is a schematic half cross-sectional view showing an embodiment of the polyester preform of the present invention. [Figure 5] Fig. 5 is a schematic half cross-sectional view showing an embodiment of the polyester preform of the present invention. [Detailed Description of the Preferred Embodiments]
[0023] (Polyester Container) As shown in Fig. 1 and Fig. 2, the polyester container 10 of the present invention includes a mouth portion 13, a neck portion 14, a shoulder portion 15, a body portion 16, and a bottom portion 17. In one embodiment, the polyester container 10 has a cylindrical shape whose diameter gradually increases from the neck portion 14 side toward the body portion 16 side. Furthermore, in each of the above-described parts constituting the polyester container 10 of the present invention, all parts except the mouth portion 13 have a multilayer cross-section having a layer made of virgin polyester (hereinafter also referred to as the virgin polyester layer) 11 located on the innermost surface and a layer made of recycled polyester (hereinafter also referred to as the recycled polyester layer) 12, while only the mouth portion 13 has a single-layer cross-section. In one embodiment of the present invention, the polyester container 10 may have a vapor-deposited film over the entire inner surface (not shown). In the polyester container of the present invention, "all parts except the mouth portion" means at least any part of the polyester container excluding the mouth portion, and does not mean all parts excluding the mouth portion. In one embodiment, "all parts except the mouth portion" may be the neck portion, the shoulder portion, the body portion, and the bottom portion.
[0024] In one embodiment, the opening 13, as shown in Figure 1, includes an outer fitting portion 18 into which the cap is fitted (sealed) and a support ring 19. The outer fitting portion is not particularly limited in shape as long as it can accommodate the cap, and may, for example, have a circumferential convex shape or a male screw shape. The opening 13 may be provided with a support ring 19 at its lower end. Alternatively, the opening 13 may be provided with an outer fitting portion 18 between its upper end and the support ring 19. This allows the polyester container to be sealed by fitting a cap onto the opening after it has been filled with contents.
[0025] In one embodiment, the mouth portion 13, as shown in Figure 2, includes an outer fitting portion 18 to which a cap is screwed, a hub 20, and a support ring 19. The opening 13 may be provided with a support ring 19 at its lower end. Alternatively, the opening 13 may be provided with an outer fitting portion 18 between its upper end and the support ring 19. This allows the polyester container to be sealed by screwing a cap onto the opening after it has been filled with contents. Furthermore, the opening portion 13 may include a caliper 20 between the outer fitting portion 18 and the support ring 19. This allows the release ring, which has been separated from the cap body after the cap has been opened, to be held in the opening portion. The following describes one embodiment of a cap used in combination with a polyester container.
[0026] Figure 3 is a semi-cross-sectional view showing the polyester container 10 in Figure 2 with a screw-on cap 30 attached to the opening 13. The polyester container 10 is sealed when the cap 30 is screwed onto the opening 13. Here, the cap 30 has a tamper-evident function (tamper-proof feature).
[0027] The cap 30 comprises a cap body 31 and a release ring 32. The cap body 31 has a disc-shaped lid portion 33 that covers the upper part of the opening 13 and a cylindrical portion 34 that covers the sides of the opening 13. The cylindrical portion 34 is a part that hangs down from the periphery of the lid portion 33. An inner fitting portion 35 is formed on the inner circumferential surface of the cylindrical portion 34, which screws into the outer fitting portion 18 of the opening 13. The release ring 32 is connected to the lower end of the cylindrical portion 34 via a detachable break portion 36. A projection 37 (locking portion) is formed on the lower inner surface of the release ring 32, facing upward and inward, and the projection 37 engages with the stepped portion of the cap 20. The outer ring 38 is in close contact with the outer circumferential surface of the mouth portion 13, and the inner ring 39 is in close contact with the inner circumferential surface of the mouth portion 13. This ensures the airtightness and ease of opening of the cap 30.
[0028] When the cap 30 is rotated in the opening direction from the state shown in Figure 3, with the opening 13 sealed by the cap 30, the break portion 36 breaks. The release ring 32 is then separated from the cap body 31 and falls onto the upper surface of the support ring 19.
[0029] After falling, the release ring 32 has its upper end facing the cab 20 and is held in place by the support ring 19 and the cab 20 so that it cannot easily come off in the vertical direction. More specifically, the release ring 32 that remains in the opening 13 after opening is restricted from moving downward by the support ring 19, and its upward movement is restricted by the projection 37 abutting against the cab 20.
[0030] The polyester container of the present invention is characterized by having a single layer of virgin polyester at the opening. This ensures both airtightness and ease of opening. The reason for this is not entirely clear, but it is presumed to be as follows. Recycled polyester tends to have a lower number-average molecular weight after undergoing the recycling process. That is, the number of polymers with shorter molecular chains increases in the polyester resin, and the number of molecular chain ends increases. When the number of molecular chain ends in the polyester resin increases, it is thought that the thermal deformation rate increases when heated. In contrast, virgin polyester has not undergone such a recycling process and its number-average molecular weight does not change, so it is thought that the thermal deformation rate can be maintained. As explained with reference to Figure 3, in the unopened state of the cap 30, the outer ring 38 that is in close contact with the outer surface of the mouth 13 and the inner ring 39 that is in close contact with the inner surface of the mouth 13 ensure airtightness and ease of opening. When the polyester container 10 is heated, if the mouth 13 is made of recycled polyester, it is prone to deformation, and the upper part of the mouth 13 deforms inward. As a result, the airtightness and ease of opening of the cap 30 are impaired. According to the present invention, by making the mouth portion 13 of the polyester container 10 a single layer made of virgin polyester, thermal deformation of the mouth portion 13 can be reduced, and the airtightness and ease of opening of the cap 30 can be ensured. Furthermore, antimony-catalyzed polyester is known to have higher thermal deformation properties than polyester using other catalysts. Therefore, in a polyester container where the mouth portion 13 is a single layer made of virgin polyester, thermal deformation of the mouth portion 13 is reduced, ensuring the airtightness and ease of opening of the cap 30. Furthermore, in the unopened state, the cap 30, as shown in Figure 3, has tamper-evident properties, with the cap body 31 and the release ring 32 being integrated. When the polyester container 10 is heated, if the mouth portion 13 is made of recycled polyester, the mouth portion 13 undergoes a large degree of thermal expansion in the vertical direction. As a result, the projection 37 of the cap 30 strikes the cap 20, causing the break portion 36 to break before opening, separating the cap body 31 and the release ring 32. Therefore, by making the mouth portion 13 of the polyester container 10 a single layer made of virgin polyester, the thermal expansion in the vertical direction of the mouth portion 13 can be reduced, and the tamper-evident properties of the cap 30 can be ensured.
[0031] In the polyester container of the present invention, by making the mouth portion a single layer made of virgin polyester, the contents can be drunk without the recycled polyester layer coming into contact with the mouth. Therefore, the polyester container of the present invention can be made highly hygienic. The hygiene of the mouth area can be evaluated by measuring the elution concentrations of contaminants such as diethyl ketone, benzophenone, toluene, and phenylcyclohexane contained in pesticides and machine oils. The elution concentration of each contaminant is preferably less than 2 ppb. In this invention, the "elution concentration of contaminants in the polyester container" is determined by sealing the mouth of the polyester container of the present invention, placing the polyester container upside down inside a metal container, immersing only the mouth of the container in 300 mL of ultrapure water, and then leaving the sealed metal container undisturbed at 60°C for one month before measuring the ultrapure water.
[0032] The polyester container of the present invention can prevent antimony and other substances from leaching into the contents, even when filled with high-temperature contents or when heated after filling, and has high hygiene properties, making it suitable for use as a heating container.
[0033] In one embodiment, the bottom portion 17, as shown in Figures 1 and 2, includes a recessed portion 21 located in the center and a contact portion 22 provided around the recessed portion 21. This configuration makes it possible to suppress deformation of the container due to increases or decreases in internal pressure when heated contents are filled into the polyester container or when the contents are heated after filling.
[0034] In one embodiment, as shown in Figures 1 and 2, the body 16 of the polyester container 10 is provided with a panel portion 23. This configuration makes it possible to suppress deformation of the container due to increases or decreases in internal pressure when heated contents are filled into the polyester container or during heating and cooling after filling.
[0035] In the polyester container of the present invention, the distance from the upper end to the lower end of the opening is preferably 5 mm or more, more preferably 15 mm or more, and even more preferably 20 mm or more. Furthermore, the distance from the upper end to the lower end of the opening is preferably 30 mm or less, more preferably 26 mm or less, and even more preferably 22 mm or less.
[0036] The polyester container of the present invention preferably has a capacity / weight of 5 mL / g or more and 50 mL / g or less, and more preferably 8 mL / g or more and 45 mL / g or less. By setting the capacity / weight of the polyester container to 5 mL / g or more, the blow-molding properties of the polyester container can be improved. Furthermore, by limiting the capacity / weight of the polyester container to 50 mL / g or less, the heat resistance and strength of the polyester container can be improved.
[0037] The polyester container of the present invention may have a vapor-deposited film covering the entire inner surface. This can improve the gas barrier properties of the polyester container.
[0038] Examples of vapor-deposited films include those composed of metals such as aluminum, inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and barium oxide, organosilicon compounds such as hexamethyldisiloxane, and hard carbon films such as DLC (Diamond-Like Carbon) films. Furthermore, a hard carbon film made of DLC film is also called i-carbon film or hydrogenated amorphous carbon film (aC:H), and is an amorphous carbon film mainly composed of SP3 bonds.
[0039] Furthermore, the thickness of the deposited film is not particularly limited and can be, for example, between 1 nm and 150 nm.
[0040] The deposition film can be formed using conventionally known methods, such as physical vapor deposition (PVD) methods including vacuum deposition, sputtering, and ion plating, and chemical vapor deposition (CVD) methods including plasma chemical vapor deposition, thermochemical vapor deposition, and photochemical vapor deposition.
[0041] The following provides a more detailed explanation of the single layer at the mouth and the multi-layer structure outside the mouth.
[0042] (Single layer) In the polyester container of the present invention, the single layer of the mouth portion is characterized by being made of a virgin polyester selected from manganese-catalyzed polyester, titanium-catalyzed polyester, aluminum-catalyzed polyester, lithium-catalyzed polyester, and germanium-catalyzed polyester. This reduces thermal deformation of the mouth portion and ensures the airtightness and ease of opening of the cap. Furthermore, in the case of a cap as shown in Figure 3, the tamper-proof properties of the cap can be ensured. In this invention, "virgin polyester" refers to polyester that has not undergone the recycling process described below, i.e., unused polyester.
[0043] Examples of manganese catalysts include manganese fatty acid salts such as manganese acetate, manganese carbonate, manganese chloride, manganese acetylacetonate salts, and manganese hydroxide. Examples of titanium catalysts include titanium alkoxides such as tetra-n-propyl titanate, tetra-i-propyl titanate, tetra-n-butyl titanate, tetra-n-butyl titanate tetramer, tetra-t-butyl titanate, tetracyclohexyl titanate, tetraphenyl titanate, and tetrabenzyl titanate; titanium oxides obtained by hydrolysis of titanium alkoxides; titanium acetate; titanium oxalate; titanium oxalate; potassium titanium oxalate; sodium titanium oxalate; potassium titanate; sodium titanate; titanium titanate-aluminum hydroxide mixtures; titanium chloride; titanium chloride-aluminum chloride mixtures; titanium bromide; titanium fluoride; potassium hexafluoritate; cobalt hexafluoritate; manganese hexafluoritate; ammonium hexafluoritate; and titanium acetylacetonate. Examples of aluminum catalysts include aluminum trisacetylacetate, aluminum monoacetylacetonate bis(ethylacetoacetate), and ethylacetoacetate aluminum diisopropylate. Examples of lithium catalysts include ethyllithium, propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, and phenyllithium. Examples of germanium catalysts include germanium dioxide, germanium tetroxide, germanium tetramethoxide, germanium tetraethoxide, germanium tetrapropoxide, germanium tetrabutoxide, germanium tetrapentoxide, and germanium tetrahexoxide.
[0044] In the present invention, "polyester" means a copolymer of a dicarboxylic acid compound and a diol compound. Examples of dicarboxylic acid compounds include malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedionic acid, eicosanedionic acid, pimelic acid, azelaic acid, methylmalonic acid and ethylmalonic acid, adamantanedicarboxylic acid, norbornenedicarboxylic acid, cyclohexanedicarboxylic acid, decalindicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodium sulfisoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenantradiocarboxylic acid, 9,9'-bis(4-carboxyphenyl)fluorenic acid and their ester derivatives. Examples of diol compounds include ethylene glycol, 1,2-propanediol, 1,3-propanediol, butanediol, 2-methyl-1,3-propanediol, hexanediol, neopentyl glycol, cyclohexanedimethanol, cyclohexanediethanol, decahydronaphthalenedimethanol, decahydronaphthalenediethanol, norbornanediethanol, norbornanediethanol, tricyclodecanedimethanol, tricyclodecaneethanol, tetracyclododecanedimethanol, tetracyclododecaneethanol, decalindiethanol, decalindiethanol, 5 Examples include methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane, cyclohexanediol, bicyclohexyl-4,4'-diol, 2,2-bis(4-hydroxycyclohexylpropane), 2,2-bis(4-(2-hydroxyethoxy)cyclohexyl)propane, cyclopentanediol, 3-methyl-1,2-cyclopentadiol, 4-cyclopentene-1,3-diol, adamandiol, paraxylene glycol, bisphenol A, bisphenol S, styrene glycol, trimethylolpropane, and pentaerythritol. Among polyesters, polyethylene terephthalate, which is a copolymer of terephthalic acid and ethylene glycol, or modified polyethylene terephthalate, to which copolymer monomers have been added, is preferred.
[0045] Within the limits that do not impair the properties of the present invention, the polyester may contain monomers other than dicarboxylic acid compounds and diol compounds, but the content thereof is preferably 10 mol% or less, more preferably 5 mol% or less, and even more preferably 3 mol% or less, relative to the total constituent units.
[0046] Within the limits that do not impair the properties of the present invention, the single layer may contain additives, such as oxygen absorbers, gas barrier resins (polyamides such as nylon 6, nylon 6,6 and polymetaxylylene adipamide (MXD6)), plasticizers, UV stabilizers, antioxidants, color inhibitors, matting agents, deodorants, flame retardants, weather-resistant agents, antistatic agents, thread friction reducers, slip agents, mold release agents, antioxidants, ion exchangers, acetaldehyde absorbers (e.g., AA Scavengers from Color Matrix), and colorants.
[0047] (multilayer) In the polyester container of the present invention, the multilayer structure other than the mouth portion comprises at least a virgin polyester layer located on the innermost surface and a recycled polyester layer. The multilayer structure other than the mouth portion may consist of three or more layers, for example, a virgin polyester layer, a recycled polyester layer, and a virgin polyester layer in that order from the inside. From the viewpoint of being able to easily adjust the thickness of each layer and easily increase the amount of recycled polyester used, the multilayer structure other than the mouth portion preferably consists of two layers: an inner layer made of virgin polyester and an outer layer made of recycled polyester.
[0048] In the polyester container of the present invention, the virgin polyester constituting the multilayer virgin polyester can be the same as that used for the single layer virgin polyester. With this configuration, even when recycled polyester is used in the polyester container, the leaching of antimony into the contents can be prevented.
[0049] Within the limits that do not impair the properties of the present invention, the virgin polyester layer may contain the above-mentioned additives, such as oxygen absorbers, gas barrier resins (polyamides such as nylon 6, nylon 6,6 and polymetaxylylene adipamide (MXD6)), plasticizers, UV stabilizers, antioxidants, color inhibitors, matting agents, deodorants, flame retardants, weather-resistant agents, antistatic agents, yarn friction reducers, slip agents, mold release agents, antioxidants, ion exchangers, acetaldehyde absorbers (e.g., AA Scavengers from Color Matrix), and colorants.
[0050] The thickness of the virgin polyester layer in a polyester container is preferably 0.01 mm or more and 0.21 mm or less, and preferably 0.025 mm or more and 0.1 mm or less. By making the thickness of the virgin polyester layer in a polyester container 0.01 mm or more, antimony leaching into the contents can be effectively prevented, even when recycled polyester is used in the polyester container. Furthermore, by making the thickness of the virgin polyester layer in polyester containers 0.21 mm or less, the proportion of recycled polyester in polyester containers can be increased, further improving the environmental impact reduction of polyester containers. The thickness of the virgin polyester layer refers to, for example, the point in the body of a polyester container where the virgin polyester layer is thinnest.
[0051] In the present invention, "recycled polyester" constituting the multilayer recycled polyester layer refers to chemically recycled polyester or mechanically recycled polyester. Chemically recycled polyester refers to polyester obtained by decomposing polyester containers down to the monomer level and then repolymerizing them. Mechanically recycled polyester refers to polyester obtained by sorting, crushing, and washing polyester containers to remove contaminants and foreign matter, obtaining flakes, and then further treating the flakes at high temperature and reduced pressure for a certain period of time to remove contaminants from inside the resin.
[0052] Within the limits that do not impair the properties of the present invention, the recycled polyester layer may contain additives, such as oxygen absorbers, gas barrier resins (polyamides such as nylon 6, nylon 6,6, and polymetaxylylene adipamide (MXD6)), plasticizers, UV stabilizers, antioxidants, color inhibitors, matting agents, deodorants, flame retardants, weather-resistant agents, antistatic agents, yarn friction reducers, slip agents, mold release agents, antioxidants, ion exchangers, acetaldehyde absorbers (e.g., AA Scavengers from Color Matrix), and colorants.
[0053] The thickness of the recycled polyester layer in the polyester container is preferably 0.04 mm or more and 0.33 mm or less, and preferably 0.1 mm or more and 0.2 mm or less. By making the thickness of the recycled polyester layer in polyester containers 0.04 mm or more, the environmental impact reduction of polyester containers can be further improved. Furthermore, by making the thickness of the recycled polyester layer in the polyester container 0.33 mm or less, it is possible to prevent the recycled polyester from being exposed to the contents during the manufacturing of the polyester container. The thickness of the recycled polyester layer refers, for example, to the point in the body of the polyester container where the recycled polyester layer is thinnest.
[0054] The eluted antimony concentration of the polyester container of the present invention is preferably less than 6 ppb, and more preferably less than 3 ppb. It is preferable to keep the eluted antimony concentration below 6 ppb, as this will meet the value recommended by the U.S. Food and Drug Administration (FDA) under Chapter 21 of the Common Facts (CFR). Furthermore, depending on the type of contents filled into the polyester container of the present invention, it may already contain trace amounts of antimony. By keeping the eluted antimony concentration of the polyester container below 3 ppb, the amount of antimony ultimately dissolved in the contents can be reduced. In this invention, the "antimony elution concentration of the polyester container" is measured by filling the polyester container of the present invention with ultrapure water at 23°C, leaving it upright in a 70°C environment for 14 days, and then removing the water from the polyester container.
[0055] In the polyester container of the present invention, the recycled polyester content is preferably 40 parts by mass or more and 90 parts by mass or less, and more preferably 60 parts by mass or more and 80 parts by mass or less, based on 100 parts by mass of the total amount of resin material contained in the polyester container. By setting the recycled polyester content to 40 parts by mass or more per 100 parts by mass of the total amount of resin material contained in the polyester container, the environmental impact reduction of the polyester container can be further improved. By limiting the recycled polyester content to 90 parts by mass or less per 100 parts by mass of the total amount of resin material contained in the polyester container, it is possible to prevent the recycled polyester from being exposed to the contents during the manufacturing of the polyester container.
[0056] (Polyester preform) As shown in Figures 4 and 5, the polyester preform 40 of the present invention comprises a mouth portion 43, a body portion 44, and a bottom portion 45. Furthermore, in each part of the polyester preform 40 of the present invention, all parts except the opening 43 have a multilayer cross-section consisting of a virgin polyester layer 41 located on the innermost surface and a recycled polyester layer 42, while only the opening 43 has a single-layer cross-section. In the polyester preform of the present invention, "all parts except the opening" means at least any part of the polyester preform excluding the opening, and does not mean all parts excluding the opening. In one embodiment, "all parts except the opening" may be the body and the bottom.
[0057] In one embodiment, the opening 43, as shown in Figure 4, includes an outer fitting portion 46 into which the cap is fitted (sealed) and a support ring 47. The outer fitting portion is not particularly limited in shape as long as it can accommodate the cap, and may, for example, be circumferentially convex or have a male screw shape. The opening 43 may be provided with a support ring 47 at its lower end. Alternatively, the opening 43 may be provided with an outer fitting portion 46 between its upper end and the support ring 47. This allows the polyester container made from polyester preform to be sealed by fitting a cap onto the opening after the contents have been filled.
[0058] In one embodiment, the mouth portion 13, as shown in Figure 5, includes an outer fitting portion 46 to which a cap is screwed, a hub 48, and a support ring 47. The opening 43 may be provided with a support ring 47 at its lower end. Alternatively, the opening 43 may be provided with an outer fitting portion 46 between its upper end and the support ring 47. This allows the polyester container made from polyester preform to be sealed by screwing a cap onto the opening after it has been filled with contents. Furthermore, the mouth portion 43 may be provided with a caliper 48 between the outer fitting portion 46 and the support ring 47. This allows the release ring, which has been separated from the cap body, to be held in the mouth portion of a polyester container made from polyester preform after the cap has been opened.
[0059] In the polyester preform of the present invention, the distance from the upper end to the lower end of the opening is preferably 5 mm or more, more preferably 15 mm or more, and even more preferably 20 mm or more. Furthermore, the distance from the upper end to the lower end of the opening is preferably 30 mm or less, more preferably 26 mm or less, and even more preferably 22 mm or less.
[0060] (Single layer) The materials that make up the single layer have been described above, so they will not be described here.
[0061] (multilayer) In the polyester preform of the present invention, the multilayer layers other than the opening have at least a virgin polyester layer located on the innermost surface and a recycled polyester layer. The multilayer layers other than the opening may consist of three or more layers, for example, a virgin polyester layer, a recycled polyester layer, and a virgin polyester layer in that order from the inside. From the viewpoint of being able to easily adjust the thickness of each layer and easily increase the amount of recycled polyester used, the multilayer layers other than the opening are preferably two layers having an inner layer made of virgin polyester and an outer layer made of recycled polyester.
[0062] The materials constituting the virgin polyester layer have been described above, so they will not be described here.
[0063] The thickness of the virgin polyester layer in the polyester preform is preferably 0.1 mm to 1.2 mm, and more preferably 0.2 mm to 0.5 mm. By setting the thickness of the virgin polyester layer in the polyester preform within the above range, the polyester container described above can be obtained. Note that the thickness of the virgin polyester layer refers to, for example, the point in the body of the polyester preform where the virgin polyester layer is thinnest.
[0064] The materials that make up the recycled polyester layer have been described above, so they will not be described here.
[0065] The thickness of the recycled polyester layer in the polyester preform is preferably 1.2 mm to 3.5 mm, and more preferably 1.9 mm to 2.2 mm. By setting the thickness of the recycled polyester layer in the polyester preform within the above range, the polyester container described above can be obtained. The thickness of the recycled polyester layer refers, for example, to the point in the torso of the polyester preform where the recycled polyester layer is thinnest.
[0066] (Method of manufacturing polyester containers) The polyester container of the present invention can be manufactured by co-injecting materials that constitute the single layer and the multilayer having a virgin polyester layer and a recycled polyester layer to produce a polyester preform, and then blow molding the preform. The formation position of each layer can be adjusted by injection molding conditions such as resin temperature.
[0067] Furthermore, the polyester container of the present invention can also be manufactured by utilizing two-color molding or insert molding. Furthermore, the polyester container of the present invention can be manufactured by injection molding virgin polyester in an internal mold to form a single layer at the mouth and a virgin polyester layer located on the innermost surface of the parts other than the mouth, then retracting the internal mold to create a gap between the internal mold and the virgin polyester layer, and injecting recycled polyester into this gap to form the recycled polyester layer of the parts other than the mouth. [Examples]
[0068] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0069] Example 1 We prepared virgin polyester (germanium catalyst PET, manufactured by Mitsui Chemicals, Inc., J-125S) and mechanically recycled polyester (manufactured by Kyoei Sangyo Co., Ltd., NA-BT7906). These were used to create a polyester preform comprising a mouth section, a body section, and a bottom section using an injection molding machine. In the production of the polyester preform, first, only virgin polyester was injected to form the mouth section, which is a single layer made of virgin polyester. Subsequently, virgin polyester and mechanically recycled polyester were continuously injected together to form the body section and bottom section, which are multilayer structures having a layer made of virgin polyester on the innermost surface and a layer made of mechanically recycled polyester. The mouth section of the polyester preform is provided with a male screw section, a cap, and a support ring in that order from the top end of the mouth section. The amount of mechanically recycled polyester used was adjusted to 80 parts by mass per 100 parts by mass of the resin material constituting the polyester preform. The distance from the top edge to the bottom edge of the opening of the polyester preform was 21 mm. The polyester preform had a thickness of 2.8 mm in the body and bottom sections, and a basis weight of 22 g.
[0070] Next, the polyester preform was heated to 110°C and biaxial stretch blow molding was performed in a blow molding die to obtain a polyester container with a capacity of 500 mL and the shape shown in Figure 2. In this polyester container, the mouth portion is a single layer made of virgin polyester, while the neck portion, shoulder portion, body portion, and bottom portion are multilayered, having a layer made of virgin polyester located on the innermost surface and a layer made of recycled polyester. The distance from the top to the bottom of the opening of the polyester container was 21 mm.
[0071] Comparative Example 1 A polyester preform was prepared in the same manner as in Example 1, except that the mouth, body, and bottom of the polyester preform were all multilayered, each consisting of a layer made of virgin polyester and a layer made of mechanically recycled polyester. A polyester container was also prepared using the polyester preform of this comparative example in the same manner as in Example 1.
[0072] Comparative Example 2 A polyester preform was prepared in the same manner as in Example 1, except that the mouth, body, and bottom of the polyester preform were all made of a single layer of virgin polyester as described above. A polyester container was also prepared using the polyester preform of this comparative example in the same manner as in Example 1.
[0073] Comparative Example 3 A polyester preform was prepared in the same manner as in Example 1, except that the mouth, body, and bottom of the polyester preform were all made of a single layer of the mechanically recycled polyester described above. A polyester container was also prepared using the polyester preform of this comparative example in the same manner as in Example 1.
[0074] <<Evaluation of Eluted Antimony Concentration>> In the above examples and comparative examples, 480 mL of ultrapure water was filled into the polyester containers obtained. In each container, the ultrapure water was filled from a position 28.7 mm from the top of the opening to the bottom. Next, the product was left undisturbed for 14 days in a hot warmer set to 70°C, with the container lying on its side. After standing, water was removed from the polyester container, and its antimony concentration was measured by inductively coupled plasma mass spectrometry (ICP-MS). The measurement results are summarized in Table 1.
[0075] <<Sealability Test>> In the above examples and comparative examples, 480 mL of water was filled into the polyester containers obtained, and caps (MA caps manufactured by Nippon Closure) were sealed using an automated machine. The containers were then left upright in a hot warmer set to 70°C for one week. The crimping angle of the caps was 150 degrees. After standing, the pressure was increased to 0.30 MPa and held for 1 minute. Leakage was then checked, and the system was evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) OK: No leaks occurred in any of the 100 polyester containers. NG: Leakage occurred in one or more polyester containers out of 100.
[0076] <<Opening Test>> In the above examples and comparative examples, 480 mL of water was filled into the polyester containers obtained, and caps (MA caps manufactured by Nippon Closure) were sealed using an automated machine. The containers were then left upright in a hot warmer set to 70°C for one week. The crimping angle of the caps was 150 degrees. After standing, the initial opening torque value (the torque value when the cap starts to move after being rotated in the opening direction) was measured and evaluated based on the evaluation criteria below. The evaluation results are summarized in Table 1. (Evaluation Criteria) OK: In all 100 polyester containers tested, the initial opening torque was between 50 and 140 N·cm. NG: In one or more polyester containers out of 100, the initial opening torque value was less than 50 N·cm or greater than 140 N·cm.
[0077] <<Tamper Evidence Test>> In the above examples and comparative examples, 480 mL of water was filled into the polyester containers obtained, and caps (MA caps manufactured by Nippon Closure) were sealed using an automated machine. The containers were then left upright in a hot warmer set to 70°C for one week. The crimping angle of the caps was 150 degrees. After standing, the tamper-evident properties were evaluated based on the following criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) OK: In all 100 samples, the cap body and release ring did not break in any of the polyester containers. NG: In one or more out of 100 polyester containers, the cap body and release ring broke.
[0078] <<Evaluation of eluted toluene concentration>> In the above examples and comparative examples, 480 mL of water was filled into the polyester containers obtained and sealed with aluminum seals. Next, with the polyester container inverted inside the metal container, only the opening was immersed in 300 mL of ultrapure water, and the metal container was sealed and left undisturbed at 60°C for one month. After standing, the ultrapure water at 60°C was slowly cooled to 23°C, and its toluene concentration was measured using a gas chromatograph-mass spectrometer (GC-MS). The measurement results are summarized in Table 2.
[0079] <<Energy load reduction>> Based on the content of recycled polyester relative to 100 parts by mass of the total amount of resin material contained in the polyester containers obtained in the above examples and comparative examples, the level of environmental impact reduction was defined as follows. OK: Contains 30 parts by mass or more of recycled polyester. NG: Recycled polyester content is less than 30 parts by mass.
[0080] [Table 1]
[0081] [Table 2]
[0082] As is clear from the table above, the polyester container of the present invention has excellent environmental impact reduction properties. Furthermore, the polyester container of the present invention effectively reduces the concentration of eluted antimony after heating, and can be suitably used as a heating container. Furthermore, the polyester container of the present invention has a reduced concentration of toluene eluted at the opening, indicating that it is a highly hygienic polyester container. Furthermore, it can be seen that the polyester container of the present invention maintains airtightness, ease of opening, and tamper-proof properties. [Explanation of Symbols]
[0083] 10: Polyester container 11: Virgin polyester layer 12: Recycled polyester layer 13: Mouth 14: Neck 15:Shoulder 16: Torso 17: Bottom 18:Outer fitting part 19: Support Ring 20: Kabura 21: Sinkhole 22: Grounding part 23: Panel section 30: Cap 31: Cap body 32: Detachment ring 33: Lid part 34: Cylindrical section 35: Inner mating part 36: Fracture 37:Protrusion 38: Outer ring 39: Inner Ring 40: Polyester preform 41: Virgin polyester layer 42: Recycled polyester layer 43: Mouth 44: Torso 45: Bottom 46:Outer fitting part 47: Support Ring 48: Kabura
Claims
1. A process for producing a polyester preform by co-injection molding a multilayer material having a layer made of virgin polyester and a layer made of recycled polyester, A process for manufacturing a polyester container for a heating container by blow molding the aforementioned polyester preform, A method for manufacturing a polyester container for a heating container, comprising: The aforementioned polyester container for heating comprises a mouth, a neck, shoulders, body, and bottom. The mouth portion is a single layer made of virgin polyester, Apart from the aforementioned opening, the structure consists of two layers: a layer made of virgin polyester located on the innermost surface, and a layer made of recycled polyester. The virgin polyester is one or more polyesters selected from manganese-catalyzed polyester, titanium-catalyzed polyester, aluminum-catalyzed polyester, lithium-catalyzed polyester, and germanium-catalyzed polyester. The recycled polyester contains an antimony catalyst, A method for manufacturing a polyester container for a heating container, characterized in that the amount of recycled polyester is 60 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total amount of resin material contained in the polyester container for a heating container.
2. The method for manufacturing a polyester container for a heating container according to claim 1, wherein the opening portion is provided with a support ring at the lower end of the opening portion.
3. The method for manufacturing a polyester container for a heating container according to claim 2, wherein the opening portion has an outer fitting portion between the upper end of the opening portion and the support ring.
4. The method for manufacturing a polyester container for a heating container according to claim 3, wherein the opening portion is provided with a lid between the outer fitting portion and the support ring.
5. A method for manufacturing a polyester container for a heating container according to any one of claims 1 to 4, wherein the distance from the upper end to the lower end of the opening is 5 mm or more and 30 mm or less.
6. A method for manufacturing a polyester container for a heating container according to any one of claims 1 to 5, wherein the eluted antimony concentration of the polyester container for the heating container is less than 6 ppb.
7. A method for manufacturing a polyester container for a heating container according to any one of claims 1 to 6, wherein the thickness of the virgin polyester layer constituting the multilayer is 0.01 mm or more and 0.21 mm or less.
8. A method for manufacturing a polyester preform, comprising the step of producing a polyester preform by co-injection molding a multilayer material having a layer made of virgin polyester and a layer made of recycled polyester, The polyester preform is a polyester preform used in the method for manufacturing a polyester container for a heating container according to any one of claims 1 to 7. The polyester preform comprises a mouth, a body, and a bottom. The mouth portion is a single layer made of virgin polyester, Apart from the aforementioned opening, the structure consists of two layers: a layer made of virgin polyester located on the innermost surface, and a layer made of recycled polyester. The virgin polyester is one or more polyesters selected from manganese-catalyzed polyester, titanium-catalyzed polyester, aluminum-catalyzed polyester, lithium-catalyzed polyester, and germanium-catalyzed polyester. The recycled polyester contains an antimony catalyst, A method for producing a polyester preform, characterized in that the content of the recycled polyester is 60 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total amount of resin material contained in the polyester preform.
Citation Information
Patent Citations
Distance relay
JP1982020123A
forced burner
JP1994006911U
Multilayer food container
JP1996253222A
Preparation of multilayer preform having recovered polyester resin layer and multilayer preform
JP1999077744A
Thin-wall bottle and method of manufacturing the same
JP2001113589A