Ion exchange membrane, method for manufacturing an ion exchange membrane, and electrolytic cell
An ion exchange membrane with a specific coating layer composition addresses gas adhesion and impurity issues, reducing electrolysis voltage and ensuring stable performance in alkali chloride electrolysis.
Patent Information
- Application Number
- JP2020102542
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-17
- Filing Date
- 2020-06-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Existing ion exchange membranes used in alkali chloride electrolysis face issues with gas adhesion and impurity accumulation, leading to increased electrolysis voltage and reduced current efficiency, despite efforts to address these problems in prior art.
The development of an ion exchange membrane with a coating layer containing inorganic particles and a binder, where the binder-to-particle mass ratio is between 0.3 and 0.9, and the coating coverage is 50% or more, which reduces gas adhesion and minimizes the impact of impurities on electrolytic performance.
The membrane achieves lower electrolysis voltage and stable electrolytic performance by effectively preventing gas adhesion and suppressing the influence of impurities, enhancing energy efficiency in alkali chloride electrolysis.
Smart Images

Figure 0007955041000002 
Figure 0007955041000003 
Figure 0007955041000001
Abstract
Description
[Technical Field]
[0001] This invention relates to an ion exchange membrane, a method for producing an ion exchange membrane, and an electrolytic cell. [Background technology]
[0002] Fluorine-containing ion exchange membranes have excellent heat resistance and chemical resistance, and are widely used as electrolytic diaphragms in various applications such as alkali chloride electrolysis, ozone generation electrolysis, fuel cells, water electrolysis, and hydrochloric acid electrolysis, and are expanding into even newer applications.
[0003] Among these methods, the ion exchange membrane method has become the mainstream in recent years for the electrolysis of alkali chloride, which produces chlorine and alkali hydroxide. In addition, in order to reduce power consumption per unit, the ion exchange membrane method is increasingly being used for alkali chloride electrolysis, with the ion exchange membrane and the anode and cathode in close contact in a natural circulation type zero-gap electrolytic cell. Ion exchange membranes used in the electrolysis of alkali chloride require various performance characteristics. Among these, high production efficiency relative to the current applied is particularly desired from a productivity standpoint, and low electrolysis voltage is required from an economic standpoint. Furthermore, in alkali chloride electrolysis, when performing electrolysis at an industrial level, even a slight reduction in the electrolysis voltage and a slight increase in current efficiency can lead to significant energy savings. In alkali chloride electrolysis, it is generally known that the electrolysis voltage increases due to the adhesion of gases generated by the electrolysis reaction to the surface of the ion exchange membrane. As a countermeasure, for example, Patent Document 1 proposes reducing the electrolysis voltage by suppressing gas adhesion to the surface of the ion exchange membrane and reducing the electrolysis voltage by providing a layer (surface layer) containing a hydrophilic binder and inorganic particles on the surface of the membrane. Furthermore, alkaline chloride aqueous solutions contain impurities such as metals, and when these impurities accumulate inside the cation exchange membrane, they cause an increase in electrolysis voltage, a decrease in current efficiency, and an increase in the impurity concentration in the alkali. In particular, unlike cation impurities such as Ca and Mg, I is an impurity that is difficult to reduce even by pre-treating the electrolyte, so there is a need for a cation exchange membrane that is less affected by I. As a countermeasure, for example, Patent Document 2 proposes that by coating the ion exchange membrane with specific inorganic fine particles, the influence of impurities in the electrolyte on electrolysis performance is reduced, and stable electrolysis performance can be obtained. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] International Publication No. 2015 / 098769 [Patent Document 2] Japanese Patent Publication No. 2014-58707 [Overview of the project] [Problems that the invention aims to solve]
[0005] To make the film surface hydrophilic and obtain a sufficient gas adhesion prevention effect, it is necessary to increase the mass ratio of the binder to the total amount of inorganic particles and binder contained in the surface layer, while forming a uniform surface layer on the film surface. However, in the method described in Patent Document 1, when the mass ratio of the binder is increased, a uniform surface layer is not formed, and the effect of preventing gas adhesion is reduced. Furthermore, the ion exchange membranes described in Patent Documents 1 and 2 still lack sufficient resistance to impurities, and the stability of the electrolytic performance of the ion exchange membranes against impurities remains insufficient.
[0006] The present invention has been made in view of the above problems, and aims to provide an ion exchange membrane, a method for manufacturing an ion exchange membrane, and an electrolytic cell that can reduce the electrolytic voltage by preventing gas adhesion when subjected to electrolysis, and can also suppress the influence of impurities in the electrolyte on the electrolytic performance. [Means for solving the problem]
[0007] The inventors of the present invention conducted extensive research to solve the above problems and found that by ensuring that the coverage rate of the film body by the coating layer is above a certain level, a gas adhesion suppression effect is achieved, and furthermore, the influence of impurities in the electrolyte on the electrolytic performance can be suppressed. Based on this result, further intensive research was conducted and found that even when the binder ratio in the coating solution during coating layer formation is increased, the above-mentioned coverage rate can be obtained by lowering the viscosity of the coating solution, thus leading to the present invention.
[0008] In other words, the present invention encompasses the following embodiments. [1] A membrane body containing a fluorine-containing polymer having ion exchange groups, A coating layer disposed on at least one surface of the aforementioned film body, An ion exchange membrane having, The coating layer comprises inorganic particles and a binder. The mass ratio of the binder to the total mass of the inorganic particles and the binder in the coating layer is 0.3 or more and 0.9 or less. An ion exchange membrane in which the coating layer covers the membrane body at a rate of 50% or more. [2] The ion exchange membrane according to [1], wherein the inorganic particles include at least one inorganic substance selected from the group consisting of oxides of Group IV elements of the periodic table, nitrides of Group IV elements of the periodic table, and carbides of Group IV elements of the periodic table. [3] The ion exchange membrane according to [1] or [2], wherein the inorganic particles are zirconium oxide particles. [4] The ion-exchange membrane according to any one of [1] to [3], wherein the binder comprises a fluoropolymer. [5] The ion-exchange membrane according to any one of [1] to [4], wherein the binder comprises a fluoropolymer having ion-exchange groups derived from carboxyl groups or sulfo groups. [6] A method for producing an ion-exchange membrane according to any one of [1] to [5], comprising: forming a coating layer on the surface of the membrane main body by spraying a coating solution containing inorganic particles, a binder, and a solvent by a spray method and drying the sprayed coating solution, wherein the coating solution has a viscosity of 13 mPa·s or less. [7] An electrolytic cell comprising the ion-exchange membrane according to any one of [1] to [5].
Effects of the Invention
[0009] According to the present invention, it is possible to provide an ion-exchange membrane, a method for producing the ion-exchange membrane, and an electrolytic cell, which can reduce electrolysis voltage when subjected to electrolysis, are less affected by impurities in an electrolytic solution on electrolysis performance, and exhibit stable electrolysis performance.
Brief Description of Drawings
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of an ion-exchange membrane. [Figure 2] FIG. 2 is a schematic cross-sectional view illustrating one embodiment of an electrolytic cell.
Modes for Carrying Out the Invention
[0011] Hereinafter, modes for carrying out the present invention (hereinafter, simply referred to as "present embodiments") will be described in detail. The following present embodiments are examples for describing the present invention, and are not intended to limit the present invention to the following contents. The present invention can be appropriately modified and carried out within the scope of the gist thereof. In the description of the drawings, identical or equivalent elements are denoted by the same reference numeral, and redundant descriptions are omitted. Furthermore, unless otherwise specified, positional relationships such as top, bottom, left, and right in the drawings are based on the positional relationships shown in the drawings, and the dimensional ratios in the drawings are not limited to the ratios shown. However, these drawings are merely examples of this embodiment, and this embodiment should not be interpreted as being limited to these examples.
[0012] The ion exchange membrane of this embodiment comprises a membrane body containing a fluorine-containing polymer having ion exchange groups, and a coating layer disposed on at least one surface of the membrane body, wherein the coating layer contains inorganic particles and a binder, the mass ratio of the binder to the total mass of the inorganic particles and binder in the coating layer is 0.3 or more and 0.9 or less, and the coverage rate of the membrane body by the coating layer is 50% or more. Because of this configuration, the ion exchange membrane of this embodiment can reduce the electrolytic voltage when subjected to electrolysis, and the influence of impurities in the electrolyte on the electrolytic performance is small, allowing for stable electrolytic performance. Therefore, the ion exchange membrane of this embodiment and the electrolytic cell containing the same can be preferably used for alkali chloride electrolysis (particularly sodium chloride electrolysis).
[0013] Figure 1 is a schematic cross-sectional view showing one embodiment of an ion exchange membrane. The ion exchange membrane 1 of this embodiment has a membrane body 10 containing a fluorine-containing polymer having ion exchange groups, and coating layers 11a and 11b formed on both sides of the membrane body 10.
[0014] As illustrated in Figure 1, in the ion exchange membrane 1, the membrane body 10 has ion exchange groups (-SO3) derived from sulfo groups. - A sulfonic acid layer 3 having a group represented by (hereinafter also called a "sulfonic acid group") and an ion exchange group (-CO2) derived from a carboxyl group. -The ion exchange membrane 1 may comprise a carboxylic acid layer 2 having a group represented by (hereinafter also referred to as a "carboxylic acid group"), and further reinforcement material 4 may enhance its strength and dimensional stability. When the ion exchange membrane 1 comprises a sulfonic acid layer 3 and a carboxylic acid layer 2, it tends to exhibit superior performance as an ion exchange membrane.
[0015] The ion exchange membrane of this embodiment is not limited to the configuration illustrated in Figure 1, and may have only one of the sulfonic acid layer and the carboxylic acid layer. Furthermore, the ion exchange membrane of this embodiment does not necessarily need to be reinforced with reinforcing material, and the arrangement of the reinforcing material is not limited to the example in Figure 1. Moreover, the coating layer does not necessarily need to be arranged on both sides of the membrane body, and may be arranged on only one surface of the membrane body.
[0016] (Membrane body) First, the membrane body 10 that constitutes the ion exchange membrane 1 of this embodiment will be described. The membrane body 10 has the function of selectively permeating cations and may contain a fluorine-containing polymer having ion exchange groups. Its composition and materials are not particularly limited, and various known fluorine-containing polymers can be appropriately selected and used.
[0017] The fluorine-containing polymer having ion exchange groups in the membrane body 10 can be obtained, for example, from a fluorine-containing polymer having an ion exchange group precursor that can become an ion exchange group by hydrolysis or the like. Specifically, for example, a precursor for the membrane body 10 can be prepared using a polymer whose main chain consists of a fluorinated hydrocarbon, which has a group that can be converted into an ion exchange group by hydrolysis or the like (ion exchange group precursor) as a pendant side chain, and which is melt-processable (hereinafter, sometimes referred to as "fluorine-containing polymer (a)"). Then, the membrane body 10 can be obtained by converting the ion exchange group precursor into an ion exchange group.
[0018] Fluorine-containing polymers (a) can be produced, for example, by copolymerizing at least one monomer selected from the following Group 1 with at least one monomer selected from the following Group 2 and / or Group 3. Alternatively, they can be produced by homopolymerization of one monomer selected from any of the following Group 1, Group 2, and Group 3.
[0019] Examples of monomers in the first group include, but are not limited to, vinyl fluoride compounds. Examples of vinyl fluoride compounds include, but are not limited to, vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, and perfluoro(alkyl vinyl ether). In particular, when the ion exchange membrane of this embodiment is used for alkaline electrolysis, the vinyl fluoride compound is preferably a perfluoro monomer, and a perfluoro monomer selected from the group consisting of tetrafluoroethylene, hexafluoropropylene, and perfluoro(alkyl vinyl ether) is preferred.
[0020] Examples of monomers in the second group include, but are not limited to, vinyl compounds having a functional group that can be converted to a carboxylic acid-type ion exchange group (carboxylic acid group). Examples of vinyl compounds having a functional group that can be converted to a carboxylic acid group include, but are not limited to, CF2=CF(OCF2CYF) s -O(CZF) t Examples include monomers represented as -COOR (where s represents an integer from 0 to 2, t represents an integer from 1 to 12, Y and Z independently represent F or CF3, and R represents a lower alkyl group. Lower alkyl groups are, for example, alkyl groups having 1 to 3 carbon atoms).
[0021] Among these, CF2 = CF(OCF2CYF) n -O(CF2) m Compounds represented as -COOR are preferred. Here, n represents an integer from 0 to 2, m represents an integer from 1 to 4, Y represents F or CF3, and R represents CH3, C2H5, or C3H7.
[0022] When using the ion exchange membrane of this embodiment as an ion exchange membrane for alkaline electrolysis, it is preferable to use at least a perfluoro compound as the monomer. However, since the alkyl group of the ester group (see R above) is lost from the polymer when hydrolysis occurs, the alkyl group (R) does not have to be a perfluoroalkyl group in which all hydrogen atoms are replaced with fluorine atoms.
[0023] Among the monomers in the second group, the monomers shown below are more preferable. CF2=CFOCF2-CF(CF3)OCF2COOCH3, CF2=CFOCF2CF(CF3)O(CF2)2COOCH3, CF2=CF[OCF2-CF(CF3)]2O(CF2)2COOCH3, CF2=CFOCF2CF(CF3)O(CF2)3COOCH3, CF2 = CFO(CF2)2COOCH3, CF2 = CFO(CF2)3COOCH3.
[0024] Examples of monomers in the third group include vinyl compounds having a functional group that can be converted into a sulfone-type ion exchange group (sulfonic acid group). Preferred vinyl compounds having a functional group that can be converted into a sulfonic acid group include monomers represented as CF2=CFO-X-CF2-SO2F (where X represents a perfluoroalkylene group). Specific examples of these include the monomers shown below. CF2 = CFOCF2CF2SO2F, CF2=CFOCF2CF(CF3)OCF2CF2SO2F, CF2=CFOCF2CF(CF3)OCF2CF2CF2SO2F, CF2 = CF(CF2)2SO2F, CF2=CFO〔CF2CF(CF3)O〕2CF2CF2SO2F, CF2=CFOCF2CF(CF2OCF3)OCF2CF2SO2F.
[0025] Among these, CF2=CFOCF2CF(CF3)OCF2CF2CF2SO2F and CF2=CFOCF2CF(CF3)OCF2CF2SO2F are more preferred.
[0026] Copolymers obtained from these monomers can be produced by polymerization methods developed for the homopolymerization and copolymerization of fluoroethylene, particularly general polymerization methods used for tetrafluoroethylene. For example, in non-aqueous methods, polymerization reactions can be carried out using inert solvents such as perfluorohydrocarbons and chlorofluorocarbons, in the presence of radical polymerization initiators such as perfluorocarbon peroxides and azo compounds, under conditions of a temperature of 0 to 200°C and a pressure of 0.1 to 20 MPa.
[0027] In the copolymerization described above, the type and proportion of the monomer combinations are not particularly limited and can be selected and determined based on the type and amount of functional groups to be imparted to the resulting fluorine-containing polymer. For example, to obtain a fluorine-containing polymer containing only carboxylic acid groups, at least one monomer from each of the first and second groups can be selected and copolymerized. To obtain a fluorine-containing polymer containing only sulfonic acid groups, at least one monomer from each of the first and third groups can be selected and copolymerized. Furthermore, to obtain a fluorine-containing polymer having both carboxylic acid and sulfonic acid groups, at least one monomer from each of the first, second, and third groups can be selected and copolymerized. In this case, the desired fluorine-containing polymer can also be obtained by separately producing copolymers consisting of the first and second groups and copolymers consisting of the first and third groups, and then mixing them. Furthermore, while the mixing ratio of each monomer is not particularly limited, if the amount of functional groups per unit polymer is increased, the proportion of monomers selected from the second and third groups described above should be increased.
[0028] The total ion exchange capacity of the fluorine-containing polymer is not particularly limited, but is preferably 0.5 equivalents / g or more and 2.0 mg equivalents / g or less, and more preferably 0.6 equivalents / g or more and 1.5 mg equivalents / g or less. Here, total ion exchange capacity refers to the equivalent amount of exchange groups per unit weight of the dry resin, and can be measured by neutralization titration or the like.
[0029] In the ion exchange membrane 1 illustrated in Figure 1, the membrane body 10 consists of a sulfonic acid layer 3 containing a fluorine-containing polymer having sulfonic acid groups and a carboxylic acid layer 2 containing a fluorine-containing polymer having carboxylic acid groups, which are laminated together. When the membrane body 10 has such a layered structure, the selective permeability of cations such as sodium ions tends to be further improved.
[0030] When the ion exchange membrane 1 illustrated in Figure 1 is placed in an electrolytic cell, the sulfonic acid layer 3 is usually positioned on the anode side of the electrolytic cell, and the carboxylic acid layer 2 is positioned on the cathode side of the electrolytic cell.
[0031] The sulfonic acid layer 3 is preferably made of a material with low electrical resistance, and from the viewpoint of film strength, it is preferable that its film thickness is greater than that of the carboxylic acid layer 2. The film thickness of the sulfonic acid layer 3 is preferably 2 to 25 times that of the carboxylic acid layer 2, and more preferably 3 to 15 times.
[0032] The carboxylic acid layer 2 is preferably thin but has high anion exclusion properties. Here, anion exclusion properties refer to the property of preventing anions from entering or permeating into the ion exchange membrane 1. To increase anion exclusion properties, it is effective to arrange a carboxylic acid layer with a small ion exchange capacity in relation to the sulfonic acid layer.
[0033] As the fluorine-containing polymer used in the sulfonic acid layer 3, it is preferable to use, for example, a polymer obtained using CF2=CFOCF2CF(CF3)OCF2CF2SO2F as the monomer of the third group.
[0034] As the fluorine-containing polymer used in the carboxylic acid layer 2, it is preferable to use, for example, a polymer obtained using CF2=CFOCF2CF(CF2)O(CF2)2COOCH3 as the monomer of the second group.
[0035] (covering layer) The ion exchange membrane of this embodiment has a coating layer disposed on at least one surface of the membrane body. In the ion exchange membrane 1 illustrated in Figure 1, coating layers 11a and 11b are formed on both surfaces of the membrane body 10, respectively.
[0036] In this embodiment, the coating layer comprises inorganic particles and a binder, and the coverage rate of the film body by the coating layer is 50% or more. Here, the above coverage rate is a value calculated by the measurement method described in the examples later. In this embodiment, a sufficiently high coverage rate can suppress gas adhesion to the ion exchange membrane during electrolysis, and as a result, the electrolysis voltage can be sufficiently reduced. From a similar viewpoint, the above coverage rate is more preferably 60% or more, and even more preferably 65% or more. A higher coverage rate is preferable, and from this viewpoint, the coverage rate can also be set to 100%. The specific method for measuring the coverage rate is as follows: An ion exchange membrane with a coating layer is observed from the coating layer side using a microscope (Keyence Corporation, VHX-6000, 500x magnification). Because the coated area appears brighter due to light scattering by inorganic particles and the binder, the area with a brightness of 150 or more in the observed image is designated as the coated area, and the area with a brightness of less than 150 is designated as the uncoated area, and binarization is performed. The percentage of the coated area relative to the entire observed image is calculated as the coverage rate. The coverage rate is information about the coating layer obtained within the field of view of the microscope (0.7 × 0.5 mm) as described above. In contrast, the distribution density of the coating layer, which will be described later, is information about the coating layer obtained within the measurement range of the fluorescent X-ray (10 × 10 mm). Thus, the coverage rate provides information about a more microscopic area than the distribution density. The coverage rate of the coating layer in this embodiment is not limited to the following, but can be adjusted to the above range by, for example, sufficiently reducing the viscosity of the coating liquid when spraying the coating liquid by spray, as will be described later.
[0037] The average particle size of the inorganic particles in this embodiment is not particularly limited, but is preferably 0.90 μm or larger. When the average particle size of the inorganic particles is 0.90 μm or larger, the resistance to impurities tends to improve. In this embodiment, it is preferable to use irregularly shaped inorganic particles, and more preferably to use inorganic particles obtained by crushing raw materials.
[0038] Furthermore, the average particle size of the inorganic particles can be 2 μm or less. When the average particle size of the inorganic particles is 2 μm or less, there is a tendency to further prevent film damage caused by inorganic particles. The average particle size of the inorganic particles is more preferably 0.90 μm or more and 1.2 μm or less. Even more preferably 1 μm or more and 1.2 μm or less.
[0039] In this specification, the average particle size refers to the median diameter (D50), which can be measured by a particle size distribution analyzer ("SALD2200" Shimadzu Corporation).
[0040] In this embodiment, the inorganic particles are preferably hydrophilic. Hydrophilicity refers to the property of a solid surface being easily wetted by water. Generally, a small contact angle can be evaluated as hydrophilic. For example, inorganic particles with a contact angle of about 90° can be evaluated as hydrophilic, and a contact angle of 90° or less is preferable, and 40° or less is more preferable. Here, the contact angle refers to the angle between the tangent to the liquid surface and the solid surface at the point of contact between the solid and the liquid. It can be calculated by using a contact angle meter ("DMo-601", manufactured by Kyowa Interface Chemical) to bring a droplet into contact with the solid surface and analyzing the image at the time of droplet placement. When the inorganic particles are hydrophilic, they tend to be oriented on the surface of the coating layer, which further suppresses gas adhesion to the ion exchange film during electrolysis. It is more preferable to include at least one inorganic substance selected from the group consisting of oxides of Group IV elements of the periodic table, nitrides of Group IV elements of the periodic table, and carbides of Group IV elements of the periodic table. Specific examples of these materials include, but are not limited to, zirconium oxide, silica oxide, tin oxide, titanium oxide, nickel oxide, SiC, and ZrC. From the viewpoint of durability, zirconium oxide particles are even more preferred.
[0041] In this embodiment, the inorganic particles are preferably inorganic particles produced by crushing a raw inorganic particle material. Alternatively, inorganic particles can be produced by melting and refining a raw inorganic particle material, and spherical particles with uniform diameters can be used as inorganic particles in the coating layer.
[0042] While not particularly limited, grinding methods include ball mills, bead mills, colloid mills, conical mills, disc mills, edge mills, flour mills, hammer mills, pellet mills, VSI mills, Willie mills, roller mills, and jet mills. Furthermore, it is preferable to wash the material after grinding, and acid treatment is preferred as the washing method. This reduces impurities such as iron adhering to the surface of the inorganic particles.
[0043] In this embodiment, the coating layer includes a binder. The binder is a component that holds inorganic particles on the surface of the ion exchange membrane, forming the coating layer. From the viewpoint of resistance to electrolytes and electrolytic products, the binder preferably includes a fluorine-containing polymer. The fluorine-containing polymer included in the coating layer as a binder can be the same type as the fluorine-containing polymer that constitutes the membrane body, or a different type can be used. In addition to such fluorine-containing polymers, various known compounds can be used as binder components in the coating layer, but the content of fluorine-containing polymers in the binder is preferably 90% by mass or more.
[0044] In this embodiment, the binder is more preferably a fluorine-containing polymer having a carboxylic acid group or a sulfonic acid group, from the viewpoint of resistance to the electrolyte and electrolytic products, and adhesion to the surface of the ion exchange membrane. When a coating layer is provided on a layer containing a fluorine-containing polymer having a sulfonic acid group (sulfonic acid layer), it is even more preferable to use a fluorine-containing polymer having a sulfonic acid group as the binder for the coating layer. Furthermore, when a coating layer is provided on a layer containing a fluorine-containing polymer having a carboxylic acid group (carboxylic acid layer), it is even more preferable to use a fluorine-containing polymer having a carboxylic acid group as the binder for the coating layer.
[0045] In this embodiment, the mass ratio of the binder to the total mass of the inorganic particles and binder in the coating layer is 0.3 or more and 0.9 or less. The inventors have found that increasing the mass ratio of the binder in the coating layer reduces the ion permeation resistance of the ion exchange membrane itself. That is, by setting the binder mass ratio to 0.3 or more, the ion permeation resistance of the ion exchange membrane itself is further reduced, and, in combination with increasing the coverage of the coating layer as described above, the electrolytic voltage can be greatly reduced. Furthermore, by setting the binder mass ratio to 0.9 or less, an effect of preventing gas adhesion by inorganic particles can be obtained, thereby reducing the electrolytic voltage. From a similar viewpoint, the binder mass ratio is preferably 0.32 or more and 0.9 or less, more preferably 0.35 or more and 0.9 or less, and even more preferably 0.4 or more and 0.9 or less.
[0046] The distribution density of the coating layer in an ion exchange membrane is not particularly limited, but 1 cm 2 Preferably, the amount is 0.05 mg or more and 2 mg or less per 1 cm 2 It is more preferable that the amount is between 0.5 mg and 2 mg per unit. The above distribution density can be measured by the method described in the examples below. Furthermore, the above distribution density can be adjusted to the above range by, for example, changing the discharge amount during spraying or changing the number of coats applied.
[0047] (Reinforcement material) In this embodiment, it is preferable that the ion exchange membrane has a reinforcing material disposed inside the membrane body.
[0048] In this embodiment, the reinforcing material functions as at least one of the reinforcing yarn and the sacrificial yarn, and examples of such materials include, but are not limited to, woven fabrics made of reinforcing yarn and sacrificial yarn. By placing the reinforcing material inside the membrane body, the expansion and contraction of the ion exchange membrane can be controlled to a desired range. Such an ion exchange membrane does not expand or contract excessively during electrolysis, etc., and can maintain excellent dimensional stability over a long period of time.
[0049] The composition of the reinforcing material is not particularly limited; for example, it may be formed by spinning a yarn called a reinforcing yarn. The term "reinforcing yarn" here refers to a component of the reinforcing material that can impart desired dimensional stability and mechanical strength to the ion exchange membrane, and that can exist stably within the ion exchange membrane. By using a reinforcing material made by spinning such reinforcing yarn, even better dimensional stability and mechanical strength can be imparted to the ion exchange membrane.
[0050] The materials used for the reinforcing material and the reinforcing yarn are not particularly limited, but are preferably materials that are resistant to acids and alkalis, and from the viewpoint of providing long-term heat resistance and chemical resistance, fibers made of fluorine-containing polymers are preferred.
[0051] As for fluorine-containing polymers used as reinforcing materials, the same ones used for the main body of the film described above can be used, but examples include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-ethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer, trifluorochloroethylene-ethylene copolymer, and vinylidene fluoride polymer (PVDF). Of these, it is preferable to use fibers made of polytetrafluoroethylene, especially from the viewpoint of heat resistance and chemical resistance.
[0052] The diameter of the reinforcing yarn used in the reinforcing material is not particularly limited, but is preferably 20 to 300 denier, more preferably 50 to 250 denier. The weave density (number of threads per unit length) is preferably 5 to 50 threads / inch. The form of the reinforcing material is not particularly limited, and for example, woven fabric, nonwoven fabric, knitted fabric, etc. can be used, but woven fabric is preferred. Furthermore, the thickness of the woven fabric is preferably 30 to 250 μm, more preferably 30 to 150 μm.
[0053] Woven or knitted fabrics can be made from monofilament, multifilament, or yarns thereof, slit yarn, etc., and various weaving methods such as plain weave, leno weave, knit weave, cord weave, and shasakka can be used.
[0054] The weaving method and arrangement of the reinforcing material in the membrane body are not particularly limited, and can be appropriately arranged considering the size and shape of the ion exchange membrane, the desired physical properties of the ion exchange membrane, and the operating environment.
[0055] For example, reinforcing materials may be arranged along a predetermined one direction of the membrane body, but from the viewpoint of dimensional stability, it is preferable to arrange reinforcing materials along a predetermined first direction and another reinforcing material along a second direction that is substantially perpendicular to the first direction. By arranging multiple reinforcing materials substantially perpendicular within the interior of the membrane body in the longitudinal direction, even better dimensional stability and mechanical strength can be provided in multiple directions. For example, it is preferable to weave reinforcing materials (warp threads) arranged along the longitudinal direction and reinforcing materials (weft threads) arranged along the transverse direction on the surface of the membrane body. From the viewpoint of dimensional stability, mechanical strength and ease of manufacture, it is more preferable to use plain weave, in which warp and weft threads are alternately raised and lowered and beaten into the fabric; leno weave, in which two warp threads are twisted and woven with the weft threads; or diagonal weave, in which the same number of weft threads are beaten into warp threads arranged in pairs or severals.
[0056] In particular, it is preferable that the reinforcing material is arranged along both the MD direction (Machine Direction) and the TD direction (Transverse Direction) of the ion exchange membrane. That is, it is preferable that the material is plain woven in the MD and TD directions. Here, the MD direction refers to the direction (flow direction) in which the membrane body and reinforcing material are transported during the manufacturing process of the ion exchange membrane, which will be described later, and the TD direction refers to the direction approximately perpendicular to the MD direction. The yarn woven along the MD direction is called the MD yarn, and the yarn woven along the TD direction is called the TD yarn. Typically, ion exchange membranes used in electrolysis are rectangular in shape, with the longitudinal direction being the MD direction and the width direction being the TD direction. By weaving in reinforcing material that is both MD yarn and TD yarn, even greater dimensional stability and mechanical strength can be provided in multiple directions.
[0057] The spacing of the reinforcing materials is not particularly limited and can be appropriately arranged considering the desired physical properties of the ion exchange membrane and the operating environment.
[0058] Among the reinforcing materials, particularly preferred forms are tape yarns or highly oriented monofilaments containing PTFE, from the viewpoint of chemical resistance and heat resistance. Specifically, it is more preferable to use tape yarns obtained by slitting a high-strength porous sheet made of PTFE into a tape shape, or highly oriented monofilaments made of PTFE with a denier of 50 to 300, and to have a plain weave with a weave density of 10 to 50 threads / inch and a thickness in the range of 50 to 100 μm. It is even more preferable that the aperture ratio of the ion exchange membrane containing such a reinforcing material be 60% or more.
[0059] Examples of reinforcing thread shapes include round threads and tape-shaped threads. Round threads are preferred.
[0060] (Communication hole) In this embodiment, it is preferable that the ion exchange membrane has communication holes inside the membrane body.
[0061] Communication pores are holes that can serve as pathways for cations and electrolytes generated during electrolysis. Furthermore, communication pores are tubular holes formed within the membrane itself, created by the elution of reinforcing material (sacrificial threads), which will be described later. The shape and diameter of these communication pores can be controlled by selecting the shape and diameter of the reinforcing material (sacrificial threads).
[0062] By forming interconnected pores in the ion exchange membrane, the mobility of alkali ions and electrolyte generated during electrolysis can be ensured. The shape of the interconnected pores is not particularly limited, but according to the manufacturing method described later, they can be shaped like the reinforcing material (sacrificial thread) used to form the interconnected pores.
[0063] In this embodiment, it is preferable that the communication holes are formed so as to alternately pass through the anode side (sulfonic acid layer side) and cathode side (carboxylic acid layer side) of the reinforcing material. With this structure, in the portion of the reinforcing material where communication holes are formed on the cathode side, cations (e.g., sodium ions) transported through the electrolyte filling the communication holes can also flow to the cathode side of the reinforcing material. As a result, the flow of cations is not obstructed, and the electrical resistance of the ion exchange membrane can be further reduced.
[0064] The communication holes may be formed along only one predetermined direction of the membrane body constituting the ion exchange membrane of this embodiment, but from the viewpoint of exhibiting more stable electrolytic performance, it is preferable that they be formed in both the vertical and horizontal directions of the membrane body.
[0065] [Manufacturing method] The method for manufacturing the ion exchange membrane according to this embodiment is not particularly limited as long as an ion exchange membrane having the above-described configuration can be obtained, but it is preferable to manufacture it by a method having the following steps (1) to (6). (1) Step: A step to produce a fluorine-containing polymer having an ion exchange group or an ion exchange group precursor that can become an ion exchange group by hydrolysis. (2) Process: A process to obtain a reinforcing material in which sacrificial threads are placed between adjacent reinforcing threads by weaving together, if necessary, a plurality of reinforcing threads and sacrificial threads that have the property of dissolving in acid or alkali and form connecting holes. (3) Step: A step of forming a film of the fluorine-containing polymer having an ion exchange group or an ion exchange group precursor that can become an ion exchange group by hydrolysis. (4) Step: A step of embedding the reinforcing material into the film as necessary to obtain a membrane body in which the reinforcing material is arranged inside. (5) Step: A step in which the membrane body obtained in step (4) is hydrolyzed (hydrolysis step). (6) Step: A step of applying a coating layer to the film body obtained in step (5) (coating step).
[0066] The method for manufacturing an ion exchange membrane according to this embodiment is mainly characterized by adjusting the viscosity of the coating solution in the (6) coating step. Each step will be described in detail below.
[0067] (1) Process: Process for producing fluorine-containing polymers (1) In the first step, a fluorine-containing polymer is produced using the monomers of the raw materials described in Groups 1 to 3 above. To control the ion exchange capacity of the fluorine-containing polymer, the mixing ratio of the monomers of the raw materials can be adjusted in the production of the fluorine-containing polymer that forms each layer.
[0068] (2) Process: Manufacturing process for reinforcing materials Reinforcement materials are woven fabrics or other materials containing reinforcing threads. By embedding the reinforcement material within the membrane, a membrane body containing the reinforcement material can be obtained.
[0069] (3) Process: Film formation process (3) In step (1), the fluorine-containing polymer obtained in step (1) is made into a film using an extruder. The film may be a single layer, a two-layer structure of a sulfonic acid layer and a carboxylic acid layer as described above, or a multilayer structure of three or more layers.
[0070] (4) Step: Step to obtain the membrane body (4) In step (2), the reinforcing material obtained in step (2) is embedded inside the film obtained in step (3) to obtain a film body containing the reinforcing material.
[0071] A preferred method for forming the film body is to (i) co-extrude a fluorine-containing polymer having a carboxylic acid group precursor (e.g., a carboxylic acid ester functional group) located on the cathode side (hereinafter referred to as the first layer) and a fluorine-containing polymer having a sulfonic acid group precursor (e.g., a sulfonyl fluoride functional group) (hereinafter referred to as the second layer) to form a film, and, if necessary, use a heating source and a vacuum source to form a reinforcing material and a second / first layer composite film in the order of a flat plate or drum having numerous pores on its surface, via a permeable heat-resistant release paper. (ii) A method of laminating and integrating the polymers while removing the air between each layer by reducing the pressure at the temperature at which each polymer melts; (ii) Separately from the second / first layer composite film, a fluorine-containing polymer (third layer) having a sulfonic acid group precursor is first made into a film on its own, and if necessary, a heat source and a vacuum source are used to laminate the third layer film, reinforcing material, and the second / first layer composite film in that order on a flat plate or drum having many pores on its surface via a permeable heat-resistant release paper, while removing the air between each layer by reducing the pressure at the temperature at which each polymer melts.
[0072] In this case, co-extruding the first and second layers is preferable because it contributes to increasing the adhesive strength of the interface.
[0073] Furthermore, the method of integration under reduced pressure is preferable to the pressure pressing method because it tends to result in a larger thickness of the third layer on the reinforcing material, and because the reinforcing material is fixed to the inner surface of the membrane body, the mechanical strength of the ion exchange membrane tends to be sufficiently maintained.
[0074] The lamination variations described here are just examples. Considering the desired layer structure and physical properties of the film body, a suitable lamination pattern (for example, a combination of each layer) can be selected and co-extruded accordingly.
[0075] Furthermore, in order to further enhance the electrical performance of the ion exchange membrane, it is possible to interpose a fourth layer made of a fluorine-containing polymer having both a carboxylic acid group precursor and a sulfonic acid group precursor between the first and second layers, or to use a fourth layer made of a fluorine-containing polymer having both a carboxylic acid group precursor and a sulfonic acid group precursor instead of the second layer.
[0076] The method for forming the fourth layer may involve separately producing a fluorine-containing polymer having a carboxylic acid group precursor and a fluorine-containing polymer having a sulfonic acid group precursor, and then mixing them, or it may involve using a copolymer of a monomer having a carboxylic acid group precursor and a monomer having a sulfonic acid group precursor.
[0077] If the fourth layer is to be an ion exchange membrane, the first and fourth layers may be co-extruded to form a film, and the third and second layers may be separately made into films and laminated using the method described above, or the first, fourth, and second layers may be co-extruded into a film at the same time.
[0078] In this case, the direction in which the extruded film flows is the MD direction. In this way, a film body containing a fluorine-containing polymer having ion exchange groups can be formed on the reinforcing material.
[0079] Furthermore, the ion exchange membrane of this embodiment preferably has protruding portions, i.e., convex portions, made of a fluorine-containing polymer having sulfonic acid groups on the surface side, which is made of a sulfonic acid layer. The method for forming such convex portions is not particularly limited, and known methods for forming convex portions on a resin surface can be employed. Specifically, for example, one method is to emboss the surface of the membrane body. For example, when integrating the composite film with a reinforcing material, the above-mentioned convex portions can be formed by using a release paper that has been embossed in advance. When forming convex portions by embossing, the height and density of the convex portions can be controlled by controlling the embossed shape (shape of the release paper) to be transferred.
[0080] (5) Hydrolysis step In step (5), a step (hydrolysis step) is performed in which the membrane main body obtained in step (4) is hydrolyzed to convert the ion-exchange group precursor into an ion-exchange group.
[0081] Further, in step (5), elution pores can be formed in the membrane main body by dissolving and removing the sacrificial yarn contained in the membrane main body with acid or alkali. The sacrificial yarn may remain in the communicating pores without being completely dissolved and removed. Further, the sacrificial yarn remaining in the communicating pores may be dissolved and removed by the electrolytic solution when the ion-exchange membrane is subjected to electrolysis.
[0082] The sacrificial yarn is soluble in acid or alkali in the production process of the ion-exchange membrane or in an electrolytic environment, and when the sacrificial yarn is eluted, communicating pores are formed in that area.
[0083] (6) Coating step In step (6), a coating liquid containing inorganic particles, a binder, and a solvent is sprayed by a spray method, and dried to form a coating layer on the surface of the membrane main body. In the present embodiment, by sufficiently reducing the viscosity of the coating liquid, when the coating liquid is sprayed, the coating liquid easily wets and spreads on the surface of the membrane main body, and the formed coating layer is uniformly formed on the surface of the membrane main body. Thus, by sufficiently reducing the viscosity of the coating liquid, the coverage of the coating layer can be sufficiently increased despite the use of a coating liquid with a high binder ratio.
[0084] As the inorganic particles, those obtained by crushing raw ore can be preferably used. As the binder, a fluorine-containing polymer having an ion-exchange group precursor is hydrolyzed with an aqueous solution containing dimethyl sulfoxide (DMSO) and potassium hydroxide (KOH), and then immersed in hydrochloric acid to convert the counter ion of the ion-exchange group to H + A substituted binder (for example, a fluorine-containing polymer having a carboxyl group or a sulfo group) can be preferably used. Such a binder is preferable because it easily dissolves in water or ethanol, which will be described later.
[0085] It is preferable to dissolve this binder in a solution of water and ethanol, for example. The preferred volume ratio of water to ethanol is 10:1 to 1:10, more preferably 5:1 to 1:5, and even more preferably 2:1 to 1:2. In this manner, inorganic particles are dispersed in the resulting solution using a ball mill to obtain a coating solution. By adjusting the time and rotation speed during dispersion, the average particle size of the inorganic particles and the viscosity of the coating solution can be adjusted. From the viewpoint of further reducing the ion permeability resistance of the ion exchange membrane itself, the preferred ratio of inorganic particles to binder in the coating solution is 0.3 to 0.9 as the binder ratio to the total mass of inorganic particles and binder in the coating solution. Since the binder mass ratio in the coating solution as the initial charge ratio is the same as the binder ratio after the coating layer is formed, the binder ratio in the coating layer of the ion exchange membrane can be determined from the initial charge ratio.
[0086] Furthermore, a surfactant may be added to the dispersion when dispersing inorganic particles. Nonionic surfactants are preferred as the surfactant, and are not limited to the following, but examples include HS-210, NS-210, P-210, and E-212 manufactured by NOF Corporation. The coating solution obtained in this manner preferably has a viscosity of 13 mPa·s or less, and more preferably 11 mPa·s or less. A low viscosity allows for uniform wetting and spreading across the film surface, enabling the gas adhesion prevention effect to be fully realized. Viscosity can be controlled using known methods. For example, this can be achieved by changing the conditions during binder polymer dissolution, changing the conditions during inorganic particle dispersion, or by adding the aforementioned surfactants or viscosity modifiers. The viscosity of the above coating solution can be measured by the method described in the examples.
[0087] The obtained coating solution is applied to at least one surface of the film body by spray coating to form a coating layer, thereby obtaining the ion exchange film of this embodiment.
[0088] As described above, the method for manufacturing an ion exchange membrane according to this embodiment includes a step of forming a coating layer on the surface of the membrane body by spraying a coating solution containing inorganic particles, a binder, and a solvent using a spray method and drying it, and it is preferable that the viscosity of the coating solution is 13 mPa·s or less.
[0089] [Electrolytic cell] The ion exchange membrane of this embodiment can be used as a component of an electrolytic cell. That is, the electrolytic cell of this embodiment is equipped with the ion exchange membrane of this embodiment. Figure 2 is a schematic diagram of one embodiment of the electrolytic cell according to this embodiment.
[0090] The electrolytic cell 100 of this embodiment comprises at least an anode 200, a cathode 300, and an ion exchange membrane 1 of this embodiment disposed between the anode 200 and the cathode 300. Here, the electrolytic cell 100 equipped with the ion exchange membrane 1 described above is described as an example, but it is not limited to this, and various configurations can be modified and implemented within the scope of the effects of this embodiment.
[0091] Such an electrolytic cell 100 can be used for various electrolysis processes, but below, as a representative example, we will describe its use in the electrolysis of an alkaline chloride aqueous solution.
[0092] The electrolysis conditions are not particularly limited and can be carried out under known conditions. For example, an aqueous alkali chloride solution of 2.5 to 5.5 N is supplied to the anode chamber, and water or a diluted aqueous alkali hydroxide solution is supplied to the cathode chamber, and electrolysis is carried out with a direct current.
[0093] The configuration of the electrolytic cell according to this embodiment is not particularly limited, and may be, for example, a unipolar or bipolar type. The materials constituting the electrolytic cell 100 are not particularly limited, but for example, titanium, which is resistant to alkali chloride and chlorine, is preferred as the material for the anode chamber, and nickel, which is resistant to alkali hydroxide and hydrogen, is preferred as the material for the cathode chamber. The electrodes may be arranged with an appropriate gap between the ion exchange membrane 1 and the anode 200, but it can be used without any problems even if the anode 200 and the ion exchange membrane 1 are in contact. In addition, although the cathode is generally arranged with an appropriate gap between it and the ion exchange membrane, a contact-type electrolytic cell (zero-gap electrolytic cell) without this gap can also be used without any problems. [Examples]
[0094] The embodiments will be described in more detail below based on examples. These embodiments are not limited to these examples.
[0095] (viscosity measurement) The viscosity of the coating solution was measured using an E-type viscometer (TV-35L, manufactured by Toki Sangyo Co., Ltd., standard cone rotor) at a temperature of 25°C and a rotation speed of 10 rpm.
[0096] (Coverage) The ion exchange membrane was observed from the coating layer side using a microscope (Keyence VHX-6000, 500x magnification). Because the coated area appears brighter due to light scattering by inorganic particles and the binder, areas with a brightness of 150 or higher were designated as coated areas, and areas with a brightness below 150 were designated as uncoated areas. Binarization was then performed. The coverage rate was calculated as the percentage of the coated area relative to the entire observed image (which was set to 100).
[0097] (Distribution density of the coating layer) The amount of zirconium present in the dried coating layer was quantified using an X-ray fluorescence analyzer (X-MET8000, manufactured by Horiba, Ltd.). The distribution density was calculated by converting the zirconium content to the total weight of the coating layer including the binder using a pre-prepared calibration curve. For the preparation of the calibration curve, samples with known distribution densities obtained by gravimetric measurement were used, and a calibration curve was created for each coating solution with a different binder ratio.
[0098] [Electrolytic evaluation] The electrolytic cell used for electrolysis had a structure in which an ion exchange membrane was placed between the anode and cathode, and consisted of four natural-circulation type zero-gap electrolytic cells arranged in series. For the cathode, a woven mesh was used, consisting of 0.15 mm diameter nickel wires coated with cerium oxide and ruthenium oxide as catalysts, woven together with a 50-mesh opening. To ensure close contact between the cathode and the ion exchange membrane, a mat woven from nickel wires was placed between the current collector, made of nickel expanded metal, and the cathode. For the anode, a titanium expanded metal coated with ruthenium oxide, iridium oxide, and titanium oxide as catalysts was used. Using the electrolytic cell described above, brine was supplied to the anode side while adjusting the concentration to 205 g / L, and water was supplied to the cathode side while maintaining a caustic soda concentration of 32 mass%. The electrolytic cell temperature was set to 85°C, and the current flow rate was 6 kA / m². 2 Electrolysis was performed at the specified current density, with the electrolyte pressure on the cathode side of the electrolytic cell being 5.3 kPa higher than the electrolyte pressure on the anode side. The voltage between the anode and cathode of the electrolytic cell was measured daily using a KEYENCE TR-V1000 voltmeter, and the average value over 7 days was calculated as the electrolysis voltage.
[0099] [Impurity resistance test] Using the electrolytic cell described above, brine was supplied to the anode side while adjusting the concentration to 205 g / L, and water was supplied to the cathode side while maintaining a caustic soda concentration of 32 mass%. Then, using brine containing 10 ppm of I and 0.03 ppm of Ba as impurities, the electrolytic cell temperature was set to 85°C, and the current flow rate was 6 kA / m². 2Electrolysis was performed for 9 days at a current density where the liquid pressure on the cathode side of the electrolytic cell was 5.3 kPa higher than the liquid pressure on the anode side. Subsequently, the increase or decrease in the current efficiency value from the value on the first day of electrolysis to the value on the ninth day after electrolysis was measured and calculated as a daily rate of change. This test was an accelerated test in which impurities were added at a concentration significantly higher than that acceptable under normal electrolysis conditions. If the decrease in current efficiency in this test was 0.75% / day or less, it was evaluated that the decrease in current efficiency due to impurities would not occur under normal electrolysis conditions. In addition, if the decrease in current efficiency in this test was 0.55% / day or less, it was evaluated that the decrease in current efficiency due to the temporary increase in impurity concentration caused by problems in the brine purification system, etc., could be suppressed.
[0100] [Example 1] As the reinforcing yarn, a 100-denier tape yarn made of polytetrafluoroethylene (PTFE) was used, twisted 900 times / m to form a yarn (hereinafter referred to as PTFE yarn). As the warp sacrificial yarn, a 35-denier, 8-filament polyethylene terephthalate (PET) yarn twisted 200 times / m was used (hereinafter referred to as PET yarn). Similarly, as the weft sacrificial yarn, a 35-denier, 8-filament polyethylene terephthalate (PET) yarn twisted 200 times / m was used (hereinafter referred to as PET yarn). First, a plain weave was performed with 24 PTFE yarns per inch and 2 sacrificial yarns placed between adjacent PTFE yarns to obtain a woven fabric with a thickness of 100 μm.
[0101] Next, a dry resin polymer (A1) was prepared, which is a copolymer of CF2=CF2 and CF2=CFOCF2CF(CF3)OCF2CF2COOCH3 with an ion exchange capacity of 0.85 mg equivalent / g. A dry resin polymer (B1) was prepared, which is a copolymer of CF2=CF2 and CF2=CFOCF2CF(CF3)OCF2CF2SO2F with an ion exchange capacity of 1.03 mg equivalent / g. Using these polymers (A1) and (B1), a two-layer film X was obtained by co-extrusion T-die method, with a polymer (A1) layer thickness of 20 μm and a polymer (B1) layer thickness of 94 μm. The ion exchange capacity of each polymer represents the ion exchange capacity when the ion exchange group precursor of each polymer is hydrolyzed and converted into an ion exchange group.
[0102] A polymer with an ion exchange capacity of 1.05 mg equivalent / g was obtained by copolymerizing CF2=CF2 and CF2=CFO-CF2CF(CF3)O-(CF2)2-SO2F. This polymer was extruded using a single-layer T-die to obtain a single-layer film Y with a thickness of 20 μm.
[0103] Next, a drum having a heating source and a vacuum source inside and a surface with micropores was used to laminate pre-embossed release paper, film Y, reinforcing material (the woven fabric obtained above), and film X in that order. After heating and depressurizing the drum at a drum temperature of 240°C and a pressure of 0.067 MPa for 2 minutes, the release paper was removed to obtain a composite film with an uneven surface. The obtained composite film was saponified by immersing it in an aqueous solution containing 30% by mass of dimethyl sulfoxide (DMSO) and 15% by mass of potassium hydroxide (KOH) at 90°C for 1 hour, then immersed in 0.5N NaOH at 90°C for 1 hour to replace the ions attached to the ion exchange groups with Na, followed by washing with water. It was then dried at 60°C to obtain the film body.
[0104] Furthermore, polymer (B3), a dry resin copolymer of CF2=CF2 and CF2=CFOCF2CF(CF3)OCF2CF2SO2F with an ion exchange capacity of 1.05 mg equivalent / g, was hydrolyzed and then converted to an acidic form with hydrochloric acid. This acidic polymer (B3) was dissolved in a 50 / 50 (mass ratio) mixture of water and ethanol at a ratio of 5% by mass. Zirconium oxide particles with a primary particle size of 1.15 μm were added to this solution so that the mass ratio of polymer (B3) to the combined mass of polymer (B3) and zirconium oxide particles was 0.4. Subsequently, the zirconium oxide particles were dispersed in a ball mill until the average particle size in the suspension was 0.94 μm to obtain a coating solution. To the obtained coating solution, HS-210, manufactured by NOF Corporation, was added as a nonionic surfactant to adjust the viscosity of the coating solution to 9.3 mPa·s. The viscosity of the coating solution was measured by the method described above, and crushed raw zirconium oxide was used.
[0105] This suspension was applied to both surfaces of the membrane body by spraying and dried to obtain an ion exchange membrane having a coating layer containing polymer (B3) and zirconium oxide particles.
[0106] The distribution density measured by the method described above is 1 cm 2 The dose was 0.5 mg per unit. Furthermore, the coverage rate, as measured by the method described above, was 83.3%.
[0107] After wetting the ion exchange membrane to increase its mass by 2%, the electrolytic performance was evaluated using this membrane. The voltage was a low value of 3.07V, and impurity resistance tests showed that the decrease in current efficiency was small at 0.51% / day, indicating high impurity resistance.
[0108] [Example 2] In Example 1, an ion exchange membrane was prepared in the same manner as in Example 1, except that the amount of HS-210 used was reduced and the viscosity was changed to 12.0 mPa·s. In this ion exchange membrane, the content of fluorine-containing polymer in the binder was 100% by mass.
[0109] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1 and was found to be 56.5%.
[0110] [Electrolytic evaluation] Using this ion exchange membrane, electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was a low value of 3.08V, and impurity resistance measurements showed a small decrease in current efficiency of 0.74% / day, indicating high impurity resistance.
[0111] [Example 3] In Example 1, an ion exchange membrane was prepared in the same manner as in Example 1, except that the amount of HS-210 used was increased and the viscosity was changed to 8.5 mPa·s. In this ion exchange membrane, the content of fluorine-containing polymer in the binder was 100% by mass.
[0112] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1, and the result was 92.9%.
[0113] [Electrolytic evaluation] Using this ion exchange membrane, electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was a low value of 3.06V, and impurity resistance measurements showed a small decrease in current efficiency of 0.42% / day, indicating high impurity resistance.
[0114] [Example 4] An ion exchange membrane was prepared in the same manner as in Example 1, except that a suspension was used in which the mass ratio of polymer (B3) to the combined mass of polymer (B3) and zirconium oxide particles was 0.7. In this case, the amount of HS-210 used was the same as in Example 1, and the viscosity of the coating solution was 11.0 mPa·s. In this ion exchange membrane, the content of fluorine-containing polymer in the binder was 100% by mass.
[0115] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1 and was found to be 66.8%.
[0116] [Electrolytic evaluation] Using this ion exchange membrane, electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was a low value of 3.06V, and impurity resistance measurements showed a small decrease in current efficiency of 0.27% / day, indicating high impurity resistance.
[0117] [Example 5] An ion exchange membrane was prepared in the same manner as in Example 1, except that a suspension was used in which the mass ratio of polymer (B3) to the combined mass of polymer (B3) and zirconium oxide particles was 0.32. In this case, the amount of HS-210 used was the same as in Example 1, and the viscosity of the coating solution was 8.6 mPa·s. In this ion exchange membrane, the content of fluorine-containing polymer in the binder was 100% by mass.
[0118] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1 and was found to be 90.1%.
[0119] [Electrolytic evaluation] Using this ion exchange membrane, electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was a low value of 3.08V, and impurity resistance measurements showed a small decrease in current efficiency of 0.61% / day, indicating high impurity resistance.
[0120] [Comparative Example 1] An ion exchange membrane was prepared in the same manner as in Example 1, except that a suspension was used in which the mass ratio of polymer (B3) to the total mass of polymer (B3) and zirconium oxide particles was 0.2. In this case, the amount of HS-210 used was the same as in Example 1, and the viscosity of the coating solution was 8.6 mPa·s. In this ion exchange membrane, the content of fluorine-containing polymer in the binder was 100% by mass.
[0121] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1, and the result was 98.1%.
[0122] [Electrolytic evaluation] Using this ion exchange membrane, the electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was high at 3.13V, and impurity tolerance measurements showed a significant decrease in current efficiency of 1.01% / day, indicating a strong influence from impurities.
[0123] [Comparative Example 2] In Example 1, an ion exchange membrane was prepared in the same manner as in Example 1, except that a suspension was used in which the mass ratio of polymer (B3) to the combined mass of polymer (B3) and zirconium oxide particles was 0.2, and viscosity adjustment with HS-210 was not performed. At this time, the viscosity of the coating solution was 9.0 mPa·s, and the content of fluorine-containing polymer in the binder of this ion exchange membrane was 100% by mass.
[0124] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1, and the result was 97.7%.
[0125] [Electrolytic evaluation] Using this ion exchange membrane, the electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was high at 3.14V, and impurity tolerance measurements showed a significant decrease in current efficiency of 1.02% / day, indicating a strong influence from impurities.
[0126] [Comparative Example 3] In Example 1, an ion exchange membrane was prepared in the same manner as in Example 1, except that viscosity adjustment with HS-210 was not performed. At this time, the viscosity of the coating solution was 14.0 mPa·s, and the content of fluorine-containing polymer in the binder of this ion exchange membrane was 100% by mass.
[0127] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1 and was found to be 40.0%.
[0128] [Electrolytic evaluation] Using this ion exchange membrane, the electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was high at 3.12V, and impurity tolerance measurements showed a significant decrease in current efficiency of 0.91% / day, indicating a strong influence from impurities.
[0129] [Comparative Example 4] In Example 1, an ion exchange membrane was prepared in the same manner as in Example 1, except that a suspension was used in which the mass ratio of polymer (B3) to the combined mass of polymer (B3) and zirconium oxide particles was 0.6, and viscosity adjustment with HS-210 was not performed. At this time, the viscosity of the coating solution was 22.0 mPa·s, and the content of fluorine-containing polymer in the binder of this ion exchange membrane was 100% by mass.
[0130] The distribution density was measured in the same manner as in Example 1, and the result was 1 cm 2 The amount was 0.5 mg per unit. Furthermore, the coverage rate was measured in the same manner as in Example 1 and was found to be 30.0%.
[0131] [Electrolytic evaluation] Using this ion exchange membrane, the electrolytic performance was evaluated under the same conditions as in Example 1. The voltage was a high value of 3.11V, and the impurity tolerance measurement showed a significant decrease in current efficiency of 0.82% / day, indicating a strong influence from impurities.
[0132] The results above are summarized in Table 1 below.
[0133] [Table 1] [Explanation of Symbols]
[0134] 1...Ion exchange membrane, 2...Carboxylic acid layer, 3...Sulfonic acid layer, 4...Reinforcement material, 10...Membrane body, 11a,11b...Coating layer, 100...Electrolytic cell, 200...Anode, 300...Cathode
Claims
1. A membrane body containing a fluorine-containing polymer having ion exchange groups, A coating layer disposed on at least one surface of the aforementioned film body, An ion exchange membrane having, The coating layer comprises inorganic particles and a binder. The mass ratio of the binder to the total mass of the inorganic particles and the binder in the coating layer is 0.35 or more and 0.9 or less. The contact angle of the inorganic particles is 90° or less. The binder comprises a fluorine-containing polymer having ion exchange groups derived from carboxyl groups or sulfo groups. An ion exchange membrane in which the coating layer covers the membrane body at a rate of 60% or more.
2. The ion exchange membrane according to claim 1, wherein the inorganic particles are particles comprising at least one inorganic substance selected from the group consisting of oxides of Group IV elements of the periodic table, nitrides of Group IV elements of the periodic table, and carbides of Group IV elements of the periodic table.
3. The ion exchange membrane according to claim 1 or 2, wherein the inorganic particles are zirconium oxide particles.
4. A method for producing an ion exchange membrane according to any one of claims 1 to 3, The process includes a step of spraying a coating solution containing inorganic particles, a binder, and a solvent using a spray method and drying it to form a coating layer on the surface of the film body. A method for producing an ion exchange membrane, wherein the viscosity of the coating solution is 13 mPa·s or less.
5. The coating solution further contains a surfactant, The method for producing an ion exchange membrane according to claim 4, wherein the viscosity is 11 mPa·s or less.
6. An electrolytic cell comprising an ion exchange membrane according to any one of claims 1 to 3.
Citation Information
Patent Citations
Ion exchange membrane, method of producing ion exchange membrane and electrolytic cell
JP2014058707A
Cation exchange membrane and electrolytic tank
JP2018059163A
Production method for fluorinated cation exchange membrane
WO2015098769A1