Photosensitive resin composition and cured product of said composition
The photosensitive resin composition addresses issues of uneven alkali dissolution and insufficient crosslinking by using a specific alkali-soluble resin structure, ensuring precise pattern formation and thermal stability for applications such as color filters and circuit board fabrication.
Patent Information
- Application Number
- JP2021053443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Conventional photosensitive resin compositions face challenges in forming fine patterns with sharp angles and maintaining pattern dimensions due to uneven alkali dissolution rates, reduced exposure sensitivity with high pigment concentrations, and insufficient crosslinking density, leading to difficulties in creating rectangular cross-sectional shapes and pattern deformation during thermal curing.
A photosensitive resin composition using an alkali-soluble resin derived from reacting a carboxyl group-containing (meth)acrylate compound with an epoxy compound having multiple glycidyl ether groups, followed by reaction with a polyhydric alcohol compound and dicarboxylic acid or acid monoanhydride, incorporating both polymerizable unsaturated groups and carboxyl groups in one molecule.
The composition achieves improved photocurability, developability, and pattern accuracy, maintaining rectangular cross-sectional shapes and reducing thermal sagging, suitable for applications like solder resists, plating resists, and color filters with enhanced dimensional stability.
Smart Images

Figure 0007955050000001 
Figure 0007955050000002 
Figure 0007955050000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a photosensitive resin composition containing an alkali-soluble resin having a specific polymerizable unsaturated group structure as an essential component, and a cured product obtained by curing the same. [Background technology]
[0002] In recent years, with the increasing performance and resolution of electronic devices and display components, there has been a demand for miniaturization and higher density in the electronic components used therein. Furthermore, the processability of the insulating materials used in these devices is also being challenged, with demands for miniaturization and optimization of the cross-sectional shape of the processed patterns. Patterning by exposure and development is a known effective method for microfabrication of insulating materials, and photosensitive resin compositions have been used in this process. However, there is a growing demand for many other properties, such as high sensitivity, adhesion to the substrate, reliability, heat resistance, and chemical resistance. In addition, various studies have been conducted on using organic insulating materials in gate insulating films for organic TFTs, but there is a need to reduce the operating voltage of the organic TFT by thinning the gate insulating film. Here, in the case of organic insulating materials with a dielectric breakdown voltage of approximately 1 MV / cm, the application of a thin film thickness of approximately 0.2 μm for the insulating film is being considered.
[0003] Conventional insulating materials made from photosensitive resin compositions utilize a photocuring reaction between a photoreactive alkali-soluble resin and a photopolymerization initiator. The i-line (365 nm), one of the line spectra of mercury lamps, is mainly used as the exposure wavelength for photocuring. However, this i-line is absorbed by the photosensitive resin itself and the colorant, resulting in a decrease in the degree of photocuring. Moreover, this absorption increases with thicker films. As a result, a difference in crosslinking density occurs in the film thickness direction in the exposed areas. Consequently, even if the surface of the coating is sufficiently photocured, photocuring is difficult at the bottom surface of the coating, making it extremely difficult to create a difference in crosslinking density between the exposed and unexposed areas. Consequently, it is difficult to obtain a photosensitive insulating material that can be developed at high resolution with the desired pattern dimensional stability, development margin, pattern adhesion, pattern edge shape, and cross-sectional shape.
[0004] Generally, photosensitive resin compositions used in such applications contain polyfunctional photocurable monomers having polymerizable unsaturated bonds, alkali-soluble binder resins, photopolymerization initiators, etc., and photosensitive resin compositions disclosed in technical disclosures for use as color filter materials can be applied. For example, Patent Documents 1 and 2 disclose copolymers of (meth)acrylic acid or (meth)acrylic acid ester having carboxyl groups, maleic anhydride, and other polymerizable monomers as binder resins.
[0005] Furthermore, Patent Document 3 discloses that an alkali-soluble unsaturated compound having both a polymerizable unsaturated group and a carboxyl group in one molecule is effective for forming negative patterns in color filters and the like.
[0006] On the other hand, Patent Documents 4, 5, 6, and 7 disclose liquid resin compositions using reaction products of epoxy (meth)acrylate having a bisphenol fluorene structure and acid anhydride.
[0007] Furthermore, Patent Documents 8, 9, and 10 disclose alkali-developable unsaturated resin compositions obtained by copolymerization of a dihydroxypropyl acrylate compound and an acidic dianhydride, or alkali-developable unsaturated resin compositions obtained by copolymerization of an acidic monoanhydride and an acidic dianhydride with a dihydroxypropyl acrylate compound. In this case, copolymerization of the acidic dianhydride and the dihydroxypropyl acrylate compound proceeds to obtain an oligomer.
[0008] Furthermore, Patent Document 11 discloses the polyfunctionalization of an alkali-soluble resin composition that increases the molecular weight of a carboxyl group-containing copolymer. [Prior art documents] [Patent Documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 61-213213 [Patent Document 2] Japanese Patent Application Publication No. 1-152449 [Patent Document 3] Japanese Patent Application Publication No. 4-340965 [Patent Document 4] Japanese Patent Application Publication No. 4-345673 [Patent Document 5] Japanese Patent Application Publication No. 4-345608 [Patent Document 6] Japanese Patent Application Publication No. 4-355450 [Patent Document 7] Japanese Patent Application Publication No. 4-363311 [Patent Document 8] Japanese Patent Application Publication No. 5-339356 [Patent Document 9] Japanese Patent Application Publication No. 7-3122 [Patent Document 10] International Publication No. 94 / 00801 [Patent Document 11] Japanese Patent Application Publication No. 9-325494 [Overview of the Initiative] [Problems that the invention aims to solve]
[0010] However, the copolymers disclosed in Patent Documents 1 and 2 are random copolymers, which results in a distribution of alkali dissolution rates within the light-irradiated and un-irradiated areas, narrowing the margin during development and making it difficult to obtain sharp-angled pattern shapes or fine patterns. In particular, when high concentrations of pigment are included, the exposure sensitivity decreases significantly, making it impossible to obtain fine negative-type patterns.
[0011] In addition, since the alkali-soluble unsaturated compound described in Patent Document 3 is insolubilized by light irradiation, it is expected to have higher sensitivity than the combination of the aforementioned binder resin and polyfunctional polymerizable monomer. Here, examples of the compounds described in Patent Document 3 include compounds in which acrylic acid, which is a polymerizable unsaturated group, and an acid anhydride are arbitrarily added to the hydroxyl groups of phenol oligomers. Even in the compounds of Patent Document 3, since a wide distribution occurs in the molecular weight of each molecule and the amount of carboxyl groups, the distribution of the alkali dissolution rate of the alkali-soluble resin becomes wide, making it difficult to form fine negative patterns.
[0012] Furthermore, examples of the resin compositions described in Patent Document 4, Patent Document 5, Patent Document 6, and Patent Document 7 include reaction products of epoxy (meth)acrylate and acid monoanhydrides. Since this reaction product has a small molecular weight, it is difficult to increase the difference in alkali solubility between exposed and unexposed areas, making it impossible to form fine patterns.
[0013] In addition, the copolymers described in Patent Document 8, Patent Document 9, Patent Document 10, and Patent Document 11 have a small number of polymerizable unsaturated bonds, resulting in insufficient crosslinking density. Therefore, for example, it may be difficult to form fine line patterns under high-concentration pigment conditions. Therefore, there is room for improvement in the copolymer structure, such as increasing the proportion of polymerizable unsaturated bonds in one molecule.
[0014] An object of the present invention is to provide a photosensitive resin composition and a cured product thereof that can be applied even when it is necessary to maintain a rectangular cross-sectional shape of a pattern without causing significant deformation even after a thermal curing step after exposure and development, such as in resists for various color filters or resists for insulating films of semiconductor devices. In particular, when forming fine line patterns of 10 μm or less or via patterns with a diameter of 50 μm or less, it is necessary to minimize changes in pattern dimensions due to thermal sagging and maintain the pattern shape as a rectangle. Furthermore, due to the narrow spacing between fine line patterns or small via pattern dimensions, removal with a developer is difficult. While extending the development time or increasing the pH of the developer facilitates removal, this can lead to erosion of the coating film bottom surface by the developer or peeling of the pattern. That is, an object of the present invention is to provide a photosensitive resin composition and a cured product thereof that can increase the difference in solubility between exposed and unexposed areas in an alkaline developer. [Means for Solving the Problems]
[0015] As a result of intensive studies to solve the above problems, the present inventors have found that a photosensitive resin composition using an alkali-soluble resin obtained by reacting a carboxyl group-containing (meth)acrylate compound with an epoxy compound having two or more glycidyl ether groups derived from a naphthol polymer, and then reacting the resulting polyhydric alcohol compound having a polymerizable unsaturated group with a dicarboxylic acid, tricarboxylic acid, or acid monoanhydride thereof, is suitable for forming cured films requiring photopatterning.
[0016] That is, an embodiment of the present invention relates to an alkali-soluble resin represented by the following general formula (1) and having a carboxyl group and a polymerizable unsaturated group in one molecule.
[0017] [Chemical formula] (However, X represents a divalent hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group which may be substituted with a hydrocarbon group having 1 to 20 carbon atoms. Y is a hydrogen atom, a hydrocarbon group R having 1 to 5 carbon atoms, or a substituent Z, where substituent Z is a substituent represented by general formula (2) or general formula (3). However, at least two of Y are substituent Z. The average value of n is 1 to 20. Furthermore, some of the hydrogen atoms of the naphthalene ring may be substituted with R1, where R1 represents a hydrocarbon group having 1 to 5 carbon atoms, a halogen atom, or a phenyl group.)
[0018] [ka] (However, R3 represents a hydrogen atom or a methyl group. R4 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond. M1 represents a divalent residue derived from a dicarboxylic acid or its acid monoanhydride, and L represents a substituent represented by general formula (4).)
[0019] [ka] (However, R3 represents a hydrogen atom or a methyl group. R5 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond. L represents a substituent represented by general formula (4).)
[0020] [ka] (However, M2 represents a divalent or trivalent residue derived from a dicarboxylic acid, tricarboxylic acid, or their acid monoanhydride, and p is 1 or 2.)
[0021] Furthermore, another embodiment of the present invention involves the above-mentioned alkali-soluble resin and (ii) A photopolymerizable monomer having at least one polymerizable unsaturated group, (iii) Photopolymerization initiator, The present invention relates to a photosensitive resin composition characterized by containing as an essential component.
[0022] Another embodiment of the present invention relates to a cured product obtained by curing the above-mentioned photosensitive resin composition. [Effects of the Invention]
[0023] According to the present invention, by including an alkali-soluble resin represented by general formula (1), the cured film pattern, after exposure and development, exhibits less change in cross-sectional shape due to thermal sagging compared to conventional bisphenol A type epoxy acrylate anhydride adducts, and can maintain a cross-sectional shape close to rectangular. Furthermore, according to the present invention, it is possible to provide cured films with excellent dimensional accuracy and pattern cross-sectional shape formed by photolithography, including solder resists, plating resists, and etching resists for circuit board fabrication, as well as color filters and light-shielding films for liquid crystal displays, organic EL displays, μLED displays, image sensors, etc. [Modes for carrying out the invention]
[0024] The photosensitive resin composition of the present invention will be described in detail below. (i) Alkali-soluble resin represented by general formula (1) (ii) A photopolymerizable monomer having at least one polymerizable unsaturated group, (iii) Photopolymerization initiator, This invention relates to a photosensitive resin composition containing as an essential component, and a cured product obtained by curing the photosensitive resin composition.
[0025] The alkali-soluble resin represented by general formula (1) is obtained by reacting an epoxy compound having two or more glycidyl ether groups derived from a polymer of naphthols with (meth)acrylic acid, and then reacting the resulting polyhydric alcohol compound having polymerizable unsaturated groups with dicarboxylic acids, tricarboxylic acids, or their acid monoanhydrides.
[0026] The alkali-soluble resin represented by general formula (1) possesses both polymerizable unsaturated groups and carboxyl groups, resulting in alkali-developable photosensitive resin compositions with excellent photocurability, good developability, and patterning properties. Furthermore, when the photosensitive resin composition is cured, it can contribute to low thermal expansion and alkali resistance.
[0027] A method for producing an alkali-soluble resin represented by general formula (1) will be described in detail. As a preferred embodiment, an alkali-soluble resin is shown as an example in which, in general formula (1), Y is a hydrogen atom, a hydrocarbon group R having 1 to 5 carbon atoms, or a substituent Z, and the substituent Z is a substituent having a polymerizable double bond and a carboxyl group in the molecule represented by general formula (2) or general formula (3). In the above alkali-soluble resin, the number of moles of the hydrocarbon group R is C R , the number of moles of Z is C Z When C R / C Z The value of is preferably 0.05 to 2.0, and more preferably 0.1 to 1.5.
[0028] First, the alkali-soluble resin of general formula (1) is derived from a polyhydric alcohol compound containing polymerizable unsaturated groups obtained by reacting an epoxy compound having a naphthalene skeleton represented by general formula (5), which has two or more glycidyl ether groups obtained by converting the phenolic hydroxyl groups of naphthol polymers to glycidyl ethers, with (meth)acrylic acid. For example, the method for producing this epoxy compound having a naphthol skeleton can be based on the method described in Japanese Patent Application Publication No. 2006-160868.
[0029] [ka]
[0030] In general formula (5), X represents a divalent hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group which may be substituted with a hydrocarbon group having 1 to 20 carbon atoms. Specifically, X is preferably a divalent bonding group represented by -CH2-, -CH(CH3)-, -CH(C2H5)-, -CH(C6H5)-, general formula (6), general formula (7), and general formula (8). Here, X is preferably general formula (6), general formula (7), or general formula (8).
[0031] W represents a hydrocarbon group R having 1 to 5 carbon atoms, or a glycidyl group G, where at least two of W are glycidyl groups G. The number of moles of R is C. R , the number of moles of G C G When C R / C G The value of is preferably 0.05 to 2.0, and more preferably 0.1 to 1.5. R is preferably a methyl group or an ethyl group.
[0032] When producing a resin of general formula (5), it is usually obtained as a mixture of molecules with different numerical values of n, but the average value of n is preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6.
[0033] Furthermore, some of the hydrogen atoms in the naphthalene ring of general formula (5) may be substituted with substituent R1, and some of the hydrogen atoms in the benzene ring of general formulas (6) to (8) may be substituted with substituent R2. R1 and R2 independently represent a hydrocarbon group having 1 to 5 carbon atoms, a halogen atom, or a phenyl group.
[0034] [ka]
[0035] [ka]
[0036] [ka]
[0037] The polymerization method for naphthols can be based on general methods for producing phenolic resins and phenolic aralkyl resins. However, for a method of producing a compound of general formula (5) characterized by having a hydrocarbon group R as W, the method described in Japanese Patent Application Publication No. 2006-160868 can be used as a reference.
[0038] As the first step, naphthols and a crosslinking agent are condensed in the presence of an acidic catalyst. In this invention, 1-naphthol and / or 2-naphthol are used as naphthols, and examples of crosslinking agents include aldehyde compounds such as formaldehyde, acetaldehyde, and benzaldehyde; alkyl halogenated compounds such as 1,4-bis(chloromethyl)benzene, 1,4-bis(chloroethyl)benzene, 4,4'-bis(chloromethyl)biphenyl, and 4,4'-bis(chloromethylbiphenyl) ether; alcohols such as p-xylylene glycol, p-di(hydroxyethyl)benzene, 4,4'-bis(hydroxymethyl)biphenyl, 2,6-bis(hydroxymethyl)naphthalene, and 2,2'-bis(hydroxymethyl)diphenyl ether; dialkyl ethers of the above alcohols such as p-xylylene glycol dimethyl ether; and divinyl compounds such as divinylbenzene and divinylbiphenyl. The crosslinking agents used here are preferably 1,4-bis(chloromethyl)benzene, 1,4-bis(chloroethyl)benzene, 4,4'-bis(chloromethyl)biphenyl, p-xylylene glycol, p-di(hydroxyethyl)benzene, p-xylylene glycol dimethyl ether, and 4,4'-bis(hydroxymethyl)biphenyl. As the acidic catalyst, it can be appropriately selected from well-known inorganic acids and organic acids, for example, inorganic acids such as hydrochloric acid and sulfuric acid, organic acids such as formic acid, oxalic acid and p-toluenesulfonic acid, Lewis acids such as aluminum chloride, and solid acids such as activated clay and zeolite.
[0039] In the second step, the hydroxyl groups of the resin obtained by reacting the naphthols with a crosslinking agent are alkoxylated. For example, the resin obtained in the first step is reacted with alcohols under an acidic catalyst. Examples of alcohols that can be used include methanol, ethanol, propanol, butanol, and pentanol, and the acidic catalyst can be the catalyst exemplified in the first step.
[0040] Alternatively, a production method may be used in which, when condensing naphthols and crosslinking agents in the presence of an acidic catalyst, alkoxynaphthalenes may be used in combination with 1-naphthol and / or 2-naphthols as naphthols. Examples of alkoxynaphthalenes include 1-methoxynaphthalene, 2-methoxynaphthalene, 1-ethoxynaphthalene, 2-ethoxynaphthalene, 1-propoxynaphthalene, and 2-propoxynaphthalene.
[0041] Subsequently, the phenolic hydroxyl groups of the naphthol polymer are converted to glycidyl ethers to obtain an epoxy compound having a naphthalene skeleton represented by general formula (5) with two or more glycidyl ether groups. The manufacturing method can be carried out in the same manner as the usual epoxidation reaction of hydroxyl groups. For example, one method involves dissolving the naphthol polymer in excess epichlorohydrin and then reacting it in the presence of an alkali metal hydroxide such as sodium hydroxide at 20 to 150°C for 1 to 10 hours.
[0042] Next, the reaction between such epoxy compounds and carboxyl group-containing (meth)acrylate compounds can be carried out using known methods. For example, the reaction can be carried out using 1 mole of carboxyl group-containing (meth)acrylate compound for every 1 mole of epoxy group. To ensure that all epoxy groups react with the carboxyl group-containing (meth)acrylate compound, a slightly excess amount of the carboxyl group-containing (meth)acrylate compound may be used compared to equimolar amounts of epoxy groups and carboxyl groups. Carboxyl group-containing (meth)acrylate compounds are compounds having one carboxyl group and one or more (meth)acrylate groups in their molecule, and examples include 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl hexahydrophthalic acid, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyhexanoic acid, and 2-methacryloyloxyhexanoic acid.
[0043] The reactants obtained in this reaction are epoxy (meth)acrylate compounds represented by general formula (9).
[0044] [ka] (However, the definitions of X and n are the same as for the compound of general formula (5), and Q represents a hydrogen atom, a hydrocarbon group having 1 to 5 carbon atoms, or a substituent having a polymerizable unsaturated group in the molecule represented by general formula (10) or general formula (11). However, at least two of Q are substituents represented by general formula (10) or general formula (11).)
[0045] [ka] (However, R3 represents a hydrogen atom or a methyl group. R4 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond. M1 represents a divalent residue derived from a dicarboxylic acid or its acid monoanhydride.)
[0046] [ka] (However, R3 represents a hydrogen atom or a methyl group. R5 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond.)
[0047] The solvent, catalyst, and other reaction conditions used in this process are not particularly limited. For example, the solvent is preferably free of hydroxyl groups and has a boiling point higher than the reaction temperature. Examples of such solvents include cellosolve solvents, such as ethyl cellosolve acetate and butyl cellosolve acetate; high-boiling-point ether or ester solvents, such as diglyme, ethyl carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate; and ketone solvents, such as cyclohexanone and diisobutyl ketone. Examples of catalysts include ammonium salts, such as tetraethylammonium bromide and triethylbenzylammonium chloride; and known catalysts such as phosphines, such as triphenylphosphine and tris(2,6-dimethoxyphenyl)phosphine.
[0048] By reacting the hydroxyl group of a compound represented by general formula (9) with a dicarboxylic acid, tricarboxylic acid, or their acid monoanhydride, an alkali-soluble resin represented by general formula (1) can be obtained. Typically, the reaction is carried out using acid monoanhydrides, and therefore, examples of acid monoanhydrides are provided. Each hydrocarbon residue (the structure excluding the carboxyl group) of these acid monoanhydrides may be further substituted with substituents such as alkyl groups, cycloalkyl groups, or aromatic groups. Examples of acid monoanhydrides of saturated chain hydrocarbon dicarboxylic acids or tricarboxylic acids include succinic acid, acetylsuccinic acid, adipic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, and diglycolic acid. Examples of acid monoanhydrides of saturated cyclic hydrocarbon dicarboxylic acids or tricarboxylic acids include hexahydrophthalic acid, cyclobutanedicarboxylic acid, cyclopentanedicarboxylic acid, norbornanedicarboxylic acid, and hexahydrotrimellitic acid. Furthermore, examples of acid monoanhydrides of unsaturated dicarboxylic acids or tricarboxylic acids include acid monoanhydrides such as maleic acid, itaconic acid, tetrahydrophthalic acid, methyl-3,6-endomethylenetetrahydrophthalic acid, and chlorendic acid. In addition, examples of acid monoanhydrides of aromatic hydrocarbon dicarboxylic acids or tricarboxylic acids include acid monoanhydrides such as phthalic acid and trimellitic acid. Among these, the acid monoanhydride is preferably succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrophthalic acid, hexahydrotrimellitic acid, phthalic acid, or trimellitic acid, and more preferably succinic acid, maleic acid, itaconic acid, tetrahydrophthalic acid, phthalic acid, hexahydrotrimellitic acid, or trimellitic acid. Note that these acid monoanhydrides can be used individually or in combination of two or more types.
[0049] The hydroxyl group of the compound represented by general formula (9) is reacted with a dicarboxylic acid or tricarboxylic acid or their acid monoanhydride. The reaction temperature when synthesizing the compound represented by general formula (1) is preferably 20 to 120°C, and more preferably 40 to 90°C. The molar ratio of the acid monoanhydride when synthesizing the compound represented by general formula (1) can be arbitrarily changed to adjust the acid value of the alkali-soluble resin represented by general formula (1).
[0050] The preferred range for the acid value of the alkali-soluble resin represented by general formula (1) is preferably 20 mg KOH / g or more and 180 mg KOH / g or less, more preferably 40 mg KOH / g or more and 140 mg KOH / g or less, and even more preferably 50 mg KOH / g or more and 120 mg KOH / g or less. When the acid value is 20 mg KOH / g or more, residue is less likely to remain during alkaline development, and when it is 180 mg KOH / g or less, the penetration of the alkaline developer does not become too fast, so peeling development can be suppressed. The acid value can be determined, for example, by titration with a 1 / 10 N-KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).
[0051] Furthermore, the weight-average molecular weight (Mw) of the alkali-soluble resin represented by general formula (1) is preferably 1,000 to 100,000, more preferably 1,000 to 20,000, and even more preferably 1,000 to 6,000. When the weight-average molecular weight is 1,000 or more, the decrease in pattern adhesion during alkaline development can be suppressed. Also, when the weight-average molecular weight is 100,000 or less, it is easy to adjust the solution viscosity of the photosensitive resin composition to a level suitable for coating, and alkaline development does not take too long. The weight-average molecular weight (Mw) can be determined, for example, by gel permeation chromatography (GPC) measurement (HLC-8220GPC, manufactured by Tosoh Corporation) in terms of polystyrene equivalent.
[0052] The photosensitive resin composition of the present invention preferably contains 30 wt% or more, and more preferably 50 wt% or more, of the alkali-soluble resin represented by general formula (1) of (i) in the solid content excluding the solvent (the solid content includes monomers that become solid after curing).
[0053] In order to take advantage of the characteristics of the photosensitive resin composition, it is preferable to include the following components (i) to (iii) as essential components, and it is even more preferable to include the optionally added component (iv) as an essential component. (i) An alkali-soluble resin having a carboxyl group and a polymerizable unsaturated group in one molecule represented by general formula (1), (ii) A photopolymerizable monomer having at least one polymerizable unsaturated group, (iii) Photopolymerization initiator, (iv) Epoxy compounds
[0054] Among these, examples of photopolymerizable monomers having at least one polymerizable unsaturated group as component (ii) include monomers having hydroxyl groups such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and (meth)acrylic acid esters such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and glycerol (meth)acrylate. When it is necessary to form crosslinked structures between molecules of alkali-soluble resins, it is preferable to use a photopolymerizable monomer having two or more polymerizable unsaturated groups, and more preferable to use a photopolymerizable monomer having three or more polymerizable unsaturated groups. These compounds can be used individually or in combination of two or more.
[0055] The mixing ratio [(i) / (ii)] of these components (ii) and the alkali-soluble resin represented by general formula (1) [component (i)] is preferably 20 / 80 to 90 / 10, and more preferably 40 / 60 to 80 / 20. Here, if the mixing ratio of alkali-soluble resin is sufficiently high, the cured product after the photocuring reaction becomes sufficiently hard. Also, because the acid value of the coating film becomes sufficiently high, it dissolves well in the alkaline developer, and in the unexposed areas, the pattern edges become less jagged and tend to be sharper. Conversely, by not mixing in too much alkali-soluble resin, the proportion of photoreactive functional groups in the resin can be sufficiently high, allowing for sufficient formation of a cross-linked structure by the photocuring reaction. Also, because the acid value of the resin component is not too high, it is easier to suppress the solubility in the alkaline developer to a predetermined range, and it is easier to form a pattern with the desired line width in the exposed areas, making it less likely for the pattern to be missing.
[0056] Furthermore, examples of photopolymerization initiators in (iii) include acetophenones such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, and p-tert-butylacetophenone; benzophenones such as benzophenone, 2-chlorobenzophenone, and p,p'-bisdimethylaminobenzophenone; and benzyl, benzoin, benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Benzoin ethers such as tel; biimidazole compounds such as 2-(O-chlorophenyl)-4,5-phenylbiimidazole, 2-(O-chlorophenyl)-4,5-di(m-methoxyphenyl))biimidazole, 2-(O-fluorophenyl)-4,5-diphenylbiimidazole, 2-(O-methoxyphenyl)-4,5-diphenylbiimidazole, 2,4,5-triarylbiimidazole; 2-trichloromethyl-5-styryl-1,3,4-oxadiazole, 2-trichloromethyl-5-(p-cyano Halomethylthiazole compounds such as styryl)-1,3,4-oxadiazole and 2-trichloromethyl-5-(p-methoxystyryl)-1,3,4-oxadiazole; 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl Halomethyl-s-triazine compounds such as nyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,5-trimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, and 2-(4-methylthiostyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine;O-acyloxime compounds such as 1,2-octanedione, 1-[4-(phenylthio)phenyl]-,2-(O-benzoyloxime), 1-(4-phenylsulfanylphenyl)butane-1,2-dione-2-oxime-O-benzoate, 1-(4-methylsulfanylphenyl)butane-1,2-dione-2-oxime-O-acetate, and 1-(4-methylsulfanylphenyl)butane-1-one oxime-O-acetate; benzyldimethylketal, thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxane These include sulfur compounds such as thon, 2-methylthioxanthone, and 2-isopropylthioxanthone; anthraquinones such as 2-ethylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, and 2,3-diphenylanthraquinone; organic peroxides such as azobisisobutylnitrile, benzoyl peroxide, and cumene peroxide; thiol compounds such as 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, and 2-mercaptobenzothiazole; and tertiary amines such as triethanolamine and triethylamine. These photopolymerization initiators can be used individually or in combination of two or more.
[0057] The amount of photopolymerization initiator added is preferably 0.1 to 10 parts by mass, and more preferably 2 to 5 parts by mass, per 100 parts by mass of the total amount of (i) alkali-soluble resin and (ii) photopolymerizable monomer. Here, if the amount of photopolymerization initiator added is 0.1 parts by mass or more, the sensitivity becomes sufficiently high, and if the amount of photopolymerization initiator added is 10 parts by mass or less, halation, which causes the tapered shape (the shape of the film thickness in the cross-section of the developed pattern) to not be sharp and to have a trailing edge, becomes less likely. Furthermore, the possibility of decomposition gas generation when exposed to high temperatures in subsequent processes is also reduced.
[0058] Furthermore, the epoxy compound in (iv) can be any known compound that is commercially available as an epoxy resin, etc., without any particular restrictions. Examples of epoxy resins include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy resins, biphenyl type epoxy resins, bisphenol fluorene type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, glycidyl ethers of polyhydric alcohols, glycidyl esters of polyhydric carboxylic acids, polymers containing (meth)acrylate glycidyl as a unit, alicyclic epoxy compounds represented by 3,4-epoxycyclohexanecarboxylic acid [(3,4-epoxycyclohexyl)methyl], 1,2-epoxy-4-(2-oxyranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (e.g., "EHPE3150", manufactured by Daicel Corporation), phenyl glycidyl ethers, p-butylphenol glycidyl ethers, triglycidyl isocyanurates, diglycidyl isocyanurates, epoxidized polybutadiene (e.g., "NISSO-PB·JP-100", manufactured by Nippon Soda Co., Ltd.), and epoxy compounds having a silicone backbone. These components are preferably compounds with an epoxy equivalent of 100 to 300 g / eq and a number-average molecular weight of 100 to 5000. (iv) Component may be a single compound or two or more compounds may be used in combination. If it is necessary to increase the crosslinking density of the alkali-soluble resin, a compound having at least two epoxy groups is preferred.
[0059] When using the epoxy compound of (iv), the amount added is preferably 10 to 40 parts by mass per 100 parts by mass of the total of components (i) and (ii). One purpose of adding the epoxy compound is to reduce the amount of carboxyl groups remaining after the cured film is formed following patterning, in order to improve the reliability of the cured film. By adding 10 parts by mass or more of the epoxy compound, the moisture resistance reliability when used as an insulating film can be further improved. In addition, by adding 40 parts by mass or less of the epoxy compound, the amount of photosensitive groups in the resin component of the photosensitive resin composition can be sufficiently increased to provide sufficient sensitivity for patterning.
[0060] A photosensitive resin composition comprising (i) an alkali-soluble resin represented by general formula (1), (ii) a photopolymerizable monomer, and (iii) a photopolymerization initiator as essential components, and (iv) an epoxy compound as an optional component, can be used by dissolving it in a solvent or by adding various additives as needed. That is, when using the photosensitive resin composition of the present invention for insulating material applications, etc., it is preferable to use a solvent in addition to (i) to (iv). Examples of solvents include alcohols such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, and propylene glycol; terpenes such as α- or β-terpineol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; cellosolve, methyl cellosolve, ethyl cellosolve, carbitol, methyl carbitol, ethyl carbitol, butyl carbitol, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. This includes glycol ethers such as dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, and triethylene glycol monoethyl ether; and acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. By dissolving and mixing these individually or in combination of two or more, a homogeneous solution-like composition can be obtained.
[0061] The photosensitive resin composition of the present invention may further contain (v) a dispersed phase. As the dispersed phase, any known dispersed phase used in photosensitive resin compositions can be used without particular limitation, as long as it is dispersed with an average particle size of 1 to 1000 nm (average particle size measured by a laser diffraction-scattering particle size distribution analyzer or a dynamic light scattering particle size distribution analyzer). Examples of dispersed phases include organic pigments such as azo pigments, condensed azo pigments, azomethine pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, isoindoline pigments, dioxazine pigments, surene pigments, perylene pigments, perinone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, and thioindigo pigments; inorganic pigments such as titanium dioxide pigments and composite oxide pigments; pigments such as carbon black pigments (colorants that are substantially insoluble in the medium); organic fillers such as acrylic polymer particles and urethane polymer particles; inorganic fillers such as silica, talc, mica, glass fibers, carbon fibers, calcium silicate, magnesium carbonate, calcium carbonate, calcium sulfate, and barium sulfate; and nanoparticles of metals or metal oxides.
[0062] These (v) dispersed phases can be used individually or in combination depending on the desired function of the photosensitive resin composition. Examples of light-shielding resists used in the manufacture of the black matrix of a color filter include carbon black, titanium black, and black organic pigments. Examples of colored resists used in the manufacture of pixels of a color filter include red, orange, yellow, green, blue, and purple organic pigments. Examples of solder resists used in the manufacture of insulating films of printed circuit boards include organic pigments, inorganic pigments, and inorganic fillers. Examples of decorative resists used in the design of the front glass of a touch panel include carbon black, titanium black, black organic pigments, and white pigments. Examples of transparent resists with high hardness, high refractive index, and high durability include transparent fillers such as silica and titania. Each of these (v) dispersed phases can be selected and used as appropriate.
[0063] Furthermore, examples of cases where (v) the dispersed phase is a light-shielding material include black organic pigments, mixed organic pigments, and black inorganic pigments. In this case, the (v) dispersed phase (light-shielding material) is preferably excellent in insulating properties, heat resistance, light resistance, and solvent resistance, depending on the application. Here, examples of black organic pigments that are light-shielding materials include perylene black, aniline black, cyanine black, and lactam black. Examples of mixed organic pigments that are light-shielding materials include those made by mixing two or more pigments selected from red, blue, green, purple, yellow, cyanine, magenta, etc., to create a pseudo-black color. Examples of black inorganic pigments that are light-shielding materials include carbon black, chromium oxide, iron oxide, and titanium black. These (v) dispersed phases can be used individually or in combination of two or more types.
[0064] Examples of organic pigments that can be used as component (v) include, but are not limited to, those with the following color index numbers. Pigment Red 2, 3, 4, 5, 9, 12, 14, 22, 23, 31, 38, 112, 122, 144, 146, 147, 149, 166, 168, 170, 175, 176, 177, 178, 179, 184, 185, 187, 188, 202, 207, 208, 209, 210, 213, 214, 220, 221, 242, 247, 253, 254, 255, 256, 257, 262, 264, 266, 272, 279, etc. Pigment Orange 5, 13, 16, 34, 36, 38, 43, 61, 62, 64, 67, 68, 71, 72, 73, 74, 81, etc. Pigment Yellow 1, 3, 12, 13, 14, 16, 17, 55, 73, 74, 81, 83, 93, 95, 97, 109, 110, 111, 117, 120, 126, 127, 128, 129, 130, 136, 138, 139, 150, 151, 153, 154, 155, 173, 174, 175, 176, 180, 181, 183, 185, 191, 194, 199, 213, 214, etc. Pigment Green 7, 36, 58, etc. Pigment Blue in 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 60, 80, etc. Pigment Violet 19, 23, 37, etc.
[0065] Furthermore, known rubber components may be added as other dispersed phases to improve impact resistance, adhesion to plated metals during processing, etc. The rubber component is preferably a crosslinked elastic polymer having carboxyl groups to ensure developability. Examples of rubber components include crosslinked acrylic rubber having carboxyl groups, crosslinked NBR having carboxyl groups, and crosslinked MBS having carboxyl groups. When using a rubber component, it is preferable to add 3 to 10 parts by mass of a rubber component having an average particle size of 0.1 μm or less per 100 parts by mass of the resin component.
[0066] (v) It is preferable that the dispersed phase be dispersed in a solvent together with a dispersant beforehand to form a dispersion, and then incorporated as part of the photosensitive resin composition. In this case, one type of solvent may be used, or two or more types may be used in combination, as exemplified by the solvents used to dissolve the photosensitive resin composition of the present invention.
[0067] The proportion of the dispersed phase that forms the dispersed phase dispersion can be added to the photosensitive resin composition of the present invention in an amount of 1 to 95% by mass relative to the total solid content. The solid content refers to the components of the composition excluding the solvent. The solid content also includes component (ii) which becomes solid after photocuring. The wide range of 1 to 95% by mass for the amount of dispersed phase is because it is possible to use dispersed phases with low specific gravity, such as organic particles such as acrylic resin particles and rubber particles, as well as dispersed phases with high specific gravity, such as metal particles and metal oxide particles. For example, when adding dispersed phase for purposes such as coloring, it is preferable to use an amount of 5 to 80% by mass. By using an amount greater than 5% by mass of the solid content, it becomes easier to impart the desired function of the dispersed phase, such as achieving the desired coloring or providing the desired light-shielding properties. By using an amount of 80% by mass or less of the solid content, the content of the photosensitive resin, which is originally the binder, can be sufficiently high to ensure developing characteristics and film-forming ability. Therefore, the amount of component (v) in the solid content is more preferably 10 to 70% by mass, and even more preferably 20 to 60% by mass, in the case of a coloring agent (including a light-shielding agent).
[0068] Furthermore, to ensure stable dispersion of the dispersed phase, known dispersants such as polymeric dispersants may be used in the dispersed phase dispersion. The dispersant can be any known compound used in pigment dispersion (compounds commercially available under names such as dispersants, dispersion wetting agents, dispersion accelerators, etc.) without particular limitations. Examples of dispersants include cationic polymeric dispersants, anionic polymeric dispersants, nonionic polymeric dispersants, and pigment derivative-type dispersants (dispersion aids). In particular, the dispersant is preferably a cationic polymeric dispersant having cationic functional groups such as imidazolyl groups, pyrrolyl groups, pyridyl groups, or primary, secondary, or tertiary amino groups as adsorption sites on the dispersed phase, and having an amine value of 1 to 100 mgKOH / g and a number-average molecular weight in the range of 1,000 to 100,000. The amount of this dispersant is preferably 1 to 35% by mass, and more preferably 2 to 25% by mass, relative to the dispersed phase. Note that while high-viscosity substances such as resins generally have a dispersion-stabilizing effect, those that do not have dispersion-promoting ability are not treated as dispersants. However, this does not restrict its use for the purpose of stabilizing dispersion.
[0069] The dispersed phase dispersion obtained in this manner can be mixed with component (i) (or the remaining component (i) if component (i) was codispersed when preparing the dispersed phase dispersion), component (ii), component (iii), and optionally added component (iv), and by adding a solvent as needed to achieve an appropriate solution viscosity, a photosensitive resin composition containing the dispersed phase can be obtained.
[0070] Furthermore, the photosensitive resin composition of the present invention may contain additives such as curing accelerators, thermal polymerization inhibitors, antioxidants, plasticizers, leveling agents, defoamers, coupling agents, and surfactants as needed. Among these, known compounds such as curing accelerators, curing catalysts, and latent curing agents commonly applied to epoxy compounds can be used as curing accelerators, and include tertiary amines, quaternary ammonium salts, tertiary phosphines, quaternary phosphonium salts, borate esters, Lewis acids, organometallic compounds, imidazoles, and diazabicyclo compounds. Examples of thermal polymerization inhibitors and antioxidants include hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, hindered phenol antioxidants, and phosphorus-based heat stabilizers. Examples of plasticizers include dibutyl phthalate, dioctyl phthalate, and tricresyl phosphate. Examples of defoamers and leveling agents include silicone-based, fluorine-based, and acrylic compounds. Examples of coupling agents include vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-(glycidyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-aminopropyltriethoxysilane, 3-(phenylamino)propyltrimethoxysilane, and 3-ureidopropyltriethoxysilane. Examples of surfactants include fluorine-based surfactants and silicone-based surfactants.
[0071] The photosensitive resin composition of the present invention preferably contains, in its solid content (excluding solvent, including monomers that become solid after curing), a total of 70 wt% or more of (i) an alkali-soluble resin represented by general formula (1), (ii) a photopolymerizable monomer, (iii) a photopolymerization initiator, and an optional component (iv) an epoxy compound and / or (v) a dispersed phase, more preferably 80 wt% or more, and even more preferably 90 wt% or more. The amount of solvent varies depending on the target viscosity, but is preferably 10 to 80 wt% of the total amount.
[0072] Furthermore, the coating film (cured product) of the present invention can be obtained, for example, by applying a solution of a photosensitive resin composition to a substrate or the like, drying it, and curing it by irradiating it with light (including ultraviolet light, radiation, etc.). By using a photomask or the like to create areas that are exposed to light and areas that are not, only the areas exposed to light are cured, and the other areas are dissolved with an alkaline solution to obtain a coating film with a desired pattern.
[0073] Each step in the film formation method by coating and drying a photosensitive resin composition can be exemplified by using any known method when coating the substrate with the photosensitive resin composition, such as the solution immersion method, spray method, roller coater, land coater, slit coater, or spinner machine. After coating to the desired thickness using these methods, the film is formed by removing the solvent (pre-baking). Pre-baking is performed by heating in an oven, hot plate, vacuum drying, or a combination thereof. The heating temperature and time in pre-baking are appropriately selected depending on the solvent used, for example, 80 to 120°C for 1 to 10 minutes.
[0074] The radiation used for exposure can include, for example, visible light, ultraviolet light, far ultraviolet light, electron beams, and X-rays, but the wavelength range of the radiation is preferably 250 to 450 nm. Examples of developers suitable for this alkaline development include aqueous solutions of sodium carbonate, potassium carbonate, potassium hydroxide, diethanolamine, and tetramethylammonium hydroxide. These developers can be appropriately selected according to the characteristics of the resin layer, and it is also effective to add surfactants as needed. The development temperature is preferably 20 to 35°C, and fine images can be precisely formed using commercially available developers or ultrasonic cleaners. After alkaline development, the image is usually washed with water. As for development methods, shower development, spray development, dip development, and paddle development can be applied.
[0075] After development in this manner, heat treatment (post-bake) is performed at 180-250°C for 20-100 minutes. This post-bake is performed to improve the adhesion between the patterned coating and the substrate, among other purposes. Similar to pre-bake, this is done by heating using an oven, hot plate, etc. The patterned coating of the present invention is formed through the above steps of the photolithography method. Then, polymerization or curing (sometimes referred to as curing collectively) is completed by heat to form a cured film pattern. The curing temperature at this time is preferably 160-250°C.
[0076] The photosensitive resin composition of the present invention has a higher number of polymerizable unsaturated groups compared to conventional compositions, resulting in improved photocurability and increased crosslinking density after curing without increasing the amount of photopolymerization initiator. Specifically, when a thick film is irradiated with ultraviolet light or electron beam, the cured portion hardens to the bottom, eliminating the difference in solubility in alkaline developer between the exposed and unexposed portions. This improves pattern dimensional stability, development margin, and pattern adhesion, enabling high-resolution pattern formation. Furthermore, even in the case of thin films, the increased sensitivity allows for a significant improvement in the amount of residual film in the exposed area and suppression of peeling during development.
[0077] The photosensitive composition of the present invention is extremely useful for solder resists, plating resists, and etching resists for circuit board fabrication, as well as insulating films for multilayer wiring boards on which semiconductor elements are mounted, various insulating films for semiconductor devices, gate insulating films for semiconductors, and photosensitive adhesives (especially adhesives that require heat bonding performance even after pattern formation by photolithography). [Examples]
[0078] The present invention will be described in more detail below based on examples of alkali-soluble resins represented by general formula (1). However, the scope of the present invention is not limited by these examples. Furthermore, unless otherwise specified, the evaluation of the resins in these examples was carried out as follows.
[0079] [Solid content concentration] The resin solution, photosensitive resin composition, etc. (1g) obtained in Example 1 (and Comparative Example 1) was impregnated into a glass filter [mass: W0(g)] and weighed [W1(g)]. The mass [W2(g)] obtained after heating at 160°C for 2 hours was used to calculate the following formula. Solid content concentration (mass%) = 100 × (W2-W0) / (W1-W0)
[0080] [Acid value] The acid value was determined by dissolving the resin solution in tetrahydrofuran and titrating it with a 1 / 10N-KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.), and the amount of KOH required per gram of solid content was defined as the acid value.
[0081] [Molecular weight] The molecular weight was measured by gel permeation chromatography (GPC) ("HLC-8320GPC" manufactured by Tosoh Corporation, column: TSKgelSuperH2000 (2 columns) + TSKgelSuperH3000 (1 column) + TSKgelSuperH4000 (1 column) + TSKgelSuperH5000 (1 column) (all manufactured by Tosoh Corporation), solvent: tetrahydrofuran, temperature: 40°C, flow rate: 0.6 ml / min), and the value obtained as a converted value of standard polystyrene ("PS-oligomer kit" manufactured by Tosoh Corporation) was taken as the weight average molecular weight (Mw).
[0082] The abbreviations used in this example are as follows. NAMMEA-1: A compound obtained by reacting a reactant of 1-naphthol and p-xylylene glycol dimethyl ether (naphthol aralkyl resin) with methanol to methoxylate a portion of the hydroxyl groups (the proportion of methoxy groups relative to the total amount of hydroxyl groups and methoxy groups is 2%) with epichlorohydrin to obtain an epoxy compound (epoxy equivalent: 320; in general formula (5), X is general formula (6), W is a methyl group (R) and a glycidyl group (G), and C R / C G value is 0.39), and further reacting with 2-acryloyloxyethyl hexahydrophthalic acid (an equivalent reaction product of epoxy groups and carboxyl groups) NAMMEA-2: A compound obtained by reacting a reactant of 1-naphthol and p-xylylene glycol dimethyl ether (naphthol aralkyl resin) with methanol to methoxylate a portion of the hydroxyl groups (the proportion of methoxy groups relative to the total amount of hydroxyl groups and methoxy groups is 2%) with epichlorohydrin to obtain an epoxy compound (epoxy equivalent: 320; in general formula (5), X is general formula (6), W is a methyl group (R) and a glycidyl group (G), and C R / C G value is 0.39), and further reacting with 2-acryloyloxyethyl phthalic acid (an equivalent reaction product of epoxy groups and carboxyl groups) NAMMEA-3: An epoxy compound obtained by reacting a reaction product of 1-naphthol and p-xylylene glycol dimethyl ether (naphthol aralkyl resin) with methanol to methoxylate some of the hydroxyl groups (the ratio of methoxy groups to the total amount of hydroxyl and methoxy groups is 28%) with chloromethyloxirane (epoxy equivalent 320, in general formula (5), X is general formula (6), W is a methyl group (R) and a glycidyl group (G), and C R / C G The compound obtained by further reacting 2-acryloyloxyethyl succinic acid with a compound whose value is 0.39 (an isostoichiometric reaction product of epoxy groups and carboxyl groups) BPDA: 3,3',4,4'-biphenyltetracarboxylic acid dianhydride THPA:1,2,3,6-tetrahydrophthalic anhydride SA: Succinic anhydride TEAB: Tetraethylammonium bromide PGMEA: Propylene glycol monomethyl ether acetate
[0083] The following synthesis examples 1 to 4 are examples of the synthesis of alkali-soluble resins represented by general formula (1) and having a carboxyl group and a polymerizable unsaturated group in one molecule. Comparative synthesis example 1 is an alkali-soluble resin containing a polymerizable unsaturated group with a different skeleton from general formula (1), and is an epoxy acrylate adduct of a bisphenol A type epoxy compound.
[0084] [Synthesis Example 1] (Synthesis of alkali-soluble resins) 55% of NAMMEA-1 in a 1000 ml four-necked flask with a reflux condenser PG MEA solution (461.5g), THPA (49.1g), TEAB (0.90g), PG MEA (32.3g) was added and stirred at 120-125°C for 6 hours to obtain alkali-soluble resin (i)-1. The solid content concentration of the obtained resin was 56.4 wt%, the acid value (based on solid content) was 65 mg KOH / g, and the molecular weight (Mw) was 1250.
[0085] [Synthesis Example 2] (Synthesis of alkali-soluble resins) 55% of NAMMEA-2 in a 1000 ml four-necked flask with a reflux condenser PG MEA solution (456.8g), THPA (49.1g), TEAB (0.90g), PG MEA (34.5g) was added and stirred at 120-125°C for 6 hours to obtain alkali-soluble resin (i)-2. The solid content concentration of the obtained resin was 56.2 wt%, the acid value (based on solid content) was 65 mg KOH / g, and the molecular weight (Mw) was 1250.
[0086] [Synthesis Example 3] (Synthesis of alkali-soluble resins) 55% of NAMMEA-1 in a 1000 ml four-necked flask with a reflux condenser PG MEA solution (483.0g), SA (33.8g), TEAB (0.95g), PG MEA (21.7g) was added and stirred at 120-125°C for 6 hours to obtain alkali-soluble resin (i)-3. The solid content concentration of the obtained resin was 67.9 wt%, the acid value (based on solid content) was 69 mg KOH / g, and the molecular weight (Mw) was 2800.
[0087] [Synthesis Example 4] (Synthesis of alkali-soluble resins) 55% of NAMMEA-3 in a 1000 ml four-necked flask with a reflux condenser PG MEA solution (467.9g), SA (36.1g), TEAB (1.01g), PG MEA (24.4g) was added and stirred at 120-125°C for 6 hours to obtain alkali-soluble resin (i)-4. The solid content concentration of the obtained resin was 54.4 wt%, the acid value (based on solid content) was 73 mg KOH / g, and the molecular weight (Mw) was 2150.
[0088] [Comparative Synthesis Example 1] (Synthesis of alkali-soluble resins) In a 1000 ml four-necked flask equipped with a reflux condenser, charge a 50% PGMEA solution (442.0 g) of the reaction product of bisphenol A type epoxy compound (epoxy equivalent = 480) and acrylic acid, along with BPDA (20.6 g), THPA (24.3 g), and TEAB (0.84 g), and incubate at 120-125°C for 6 hours. Stirring Alkali-soluble resin solution (i)-5 was obtained. The solid content concentration of the obtained resin was 56.1 wt%, the acid value (based on solid content) was 63 mg KOH / g, and the molecular weight (Mw) was 9000.
[0089] Next, the present invention will be specifically described based on Examples 1 to 4 and Comparative Example 1 regarding the production and evaluation of photosensitive resin compositions and their cured products, but the present invention is not limited to these. Hereinafter, the raw materials and abbreviations used in the production of the photosensitive resin compositions of Examples 1 to 4 and Comparative Example 1 are as follows.
[0090] (i)-1: Alkali-soluble resin obtained in Synthesis Example 1 (i)-2: Alkali-soluble resin obtained in Synthesis Example 2 (i)-3: Alkali-soluble resin obtained in Synthesis Example 3 (i)-4: Alkali-soluble resin obtained in Synthesis Example 4 (i)-5: Alkali-soluble resin obtained in comparative synthesis example 1 (ii) Dipentaerythritol hexaacrylate (iii)-1:1-Hydroxycyclohexylphenyl ketone (Omnirad 184, manufactured by IGM RESINS BV) (iii)-2: p,p'-bis(dimethylamino)benzophenone (Michler ketone) (iv): Cresol novolac type epoxy resin (YDCN-700-7, epoxy equivalent 200 g / e q (Softening point 70°C, manufactured by Nippon Steel Chemical & Material Co., Ltd.) Solvent: Propylene glycol monomethyl ether acetate
[0091] The above-mentioned components were blended in the proportions shown in Table 1 to prepare the photosensitive resin compositions of Examples 1-4 and Comparative Example 1. All values in Table 1 represent parts by mass.
[0092] [Table 1]
[0093] [Evaluation of the photosensitive resin compositions of Examples 1-4 and Comparative Example 1] The photosensitive resin compositions shown in Table 1 were coated onto a 125 mm x 125 mm glass substrate "#1737" (Corning) using a spin coater to achieve a post-baking film thickness of 30 μm. The coated substrate was then pre-baked at 110°C for 5 minutes to produce a coated plate. Subsequently, a photomask for pattern formation was used to heat the substrate at 500 W / cm². 2 The exposed areas were irradiated with ultraviolet light at a wavelength of 365 nm using a high-pressure mercury lamp to perform a photocuring reaction. Next, the exposed coated plate was developed using a 0.8 wt% tetramethylammonium hydroxide (TMAH) aqueous solution in a shower development at 23°C for an additional 30 seconds from the time when the pattern began to appear, and then sprayed with water to remove the unexposed areas of the coating. After that, the plate was heat-cured using a hot air dryer at 230°C for 30 minutes to obtain the cured films according to Examples 1 to 4 and Comparative Example 1.
[0094] The following evaluations were performed on the above-mentioned cured film. The results are shown in Table 2.
[0095] (Adhesion and residue) The adhesion of the hardened film to the fine line pattern was confirmed using an optical microscope, "ECLIPSE LV100" (manufactured by Nikon Corporation).
[0096] (Criteria for evaluating adhesion) ○: Patterns with an L / S (line width / space width) of 30 μm / 30 μm or larger are formed. ×: Patterns where L / S (line width / space width) is less than 30 μm / 30 μm are not formed.
[0097] (Residue Evaluation Criteria) ○: Patterns with L / S (line width / space width) of 30 μm / 30 μm or more that have no residue between patterns. ×: Patterns where L / S (line width / space width) is 30 μm / 30 μm or larger show noticeable residue between patterns.
[0098] (linearity) The linearity of the fine line pattern of the cured film was confirmed using an optical microscope, "ECLIPSE LV100" (manufactured by Nikon Corporation).
[0099] (Linearity evaluation criteria) ○: No peeling or chipping of the fine line pattern on the glass substrate, and no jagged edges on the pattern ends are observed. ×: Peeling or chipping of the fine line pattern on the glass substrate, and jagged edges on the pattern are observed.
[0100] (Tapered shape) The tapered shape was determined by using a negative-type photomask with a line and space pattern of 1 to 100 μm. The exposed and developed pattern was observed using a scanning electron microscope "VE-7800" (manufactured by KEYENCE Corporation).
[0101] (Taper shape evaluation criteria) ◎: Cross-sectional shape is nearly vertical ○: The cross-sectional shape is trapezoidal, and the interior angle of the pattern end formed by the pattern side and the glass substrate is 60° to 90°. △: The cross-sectional shape is smooth and rounded. ×: The cross-sectional shape is trapezoidal, and the interior angle of the pattern edge formed by the pattern side and the glass substrate is greater than 90°.
[0102] [Table 2]
[0103] As shown in Table 2, the photosensitive resin compositions containing alkali-soluble resins prepared in Examples 1 to 4 demonstrate that they achieve both high adhesion and residue suppression, enabling the formation of cured film patterns with excellent tapered shapes.
[0104] Based on the above, the photosensitive resin composition containing the alkali-soluble resin of the present invention can be applied to applications where it is necessary to form a cured film with excellent dimensional accuracy and pattern cross-sectional shape, such as solder resists, plating resists, and etching resists for circuit board fabrication, as well as color filters and light-shielding films for liquid crystal displays, organic EL displays, μLED displays, image sensors, etc., which are formed by photolithography. [Industrial applicability]
[0105] The photosensitive resin composition of the present invention can be applied as a solder resist, plating resist, etching resist for circuit board fabrication, and insulating film resist for semiconductor devices, etc. The cured product can be applied as various cured films formed by photolithography, such as protective films, color filters, and light-shielding films, which are components of liquid crystal displays, organic EL displays, μLED displays, image sensors, etc.
Claims
1. (i) An alkali-soluble resin represented by the following general formula (1), having a carboxyl group and a polymerizable unsaturated group in one molecule, (ii) A photopolymerizable monomer having at least one polymerizable unsaturated group, which is different from the monomer in (i), (iii) Photopolymerization initiator and Includes, The total of 100 parts by mass of component (i) and component (ii) contains 2 to 5 parts by mass of component (iii), Photosensitive resin composition. 【Chemistry 1】 (However, X represents a substituent represented by general formula (6), general formula (7), or general formula (8). Y is a hydrogen atom, a hydrocarbon group R having 1 to 5 carbon atoms, or a substituent Z, and substituent Z is a substituent represented by general formula (2) or general formula (3). However, at least two of Y are substituent Z. The average value of n is 1 to 20. Furthermore, some of the hydrogen atoms of the naphthalene ring are R 1 It may also be replaced with R 1 (This represents a hydrocarbon group having 1 to 5 carbon atoms, a halogen atom, or a phenyl group.) 【Chemistry 2】 (However, R 3 R represents a hydrogen atom or a methyl group. 4 This represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond. 1 represents a divalent residue derived from a dicarboxylic acid or its acid monoanhydride, and L represents a substituent represented by general formula (4). In general formula (2), * represents a binding site to the structure represented by general formula (1). 【Transformation 3】 (However, R 3 R represents a hydrogen atom or a methyl group. 5 represents a divalent hydrocarbon group having 2 to 6 carbon atoms, which may contain an ether bond. L represents a substituent represented by general formula (4). * in general formula (3) indicates a bonding site to the structure represented by general formula (1). 【Chemistry 4】 (However, M 2 represents a divalent or trivalent residue derived from a dicarboxylic acid, tricarboxylic acid, or their acid monoanhydride, where p is 1 or 2. In general formula (4), * indicates a binding site to the structure represented by general formula (2) or general formula (3). 【Transformation 5】 【Transformation 6】 【Transformation 7】 (However, some of the hydrogen atoms on the benzene rings in general formulas (6) to (8) may be substituted by substituent R 2 which independently represents a hydrocarbon group having 1 to 5 carbon atoms, a halogen atom, or a phenyl group. In general formulas (6) to (8), * denotes the bonding site to the structure represented by general formula (1).) 2
2. The Y is a hydrocarbon group R having 1 to 5 carbon atoms or a substituent Z, and the number of moles of R is C R , the number of moles of Z C Z In that case, C R / C Z The photosensitive resin composition according to claim 1, characterized in that the value of is 0.05 to 2.
0.
3. The photosensitive resin composition according to claim 1 or claim 2, further characterized by containing (iv) an epoxy compound as an essential component.
4. The photosensitive resin composition according to claim 3, characterized in that it contains 10 to 40 parts by mass of component (iv) with respect to a total of 100 parts by mass of component (i) and component (ii).
5. Furthermore, (v) containing dispersed particles, The (v) dispersed phase is obtained by dispersing organic pigments, inorganic pigments, organic fillers, inorganic fillers, or nanoparticles of metals or metal oxides in the photosensitive resin composition with an average particle size of 1 to 1000 nm. A photosensitive resin composition according to any one of claims 1 to 4.
6. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Photo-polymerizable composition
JP1986213213A
Color filter
JP1989152449A
Photopolymerizable composition for color filter
JP1992340965A
Material for color filter and its cured product
JP1992345608A
Solder resist ink composition and cured item thereof
JP1992345673A