Spunbond nonwoven fabric and method for producing spunbond nonwoven fabric

The production of spunbond nonwoven fabrics using a copolymer of 4-methyl-1-pentene and α-olefins with specific structural units and a core-sheath structure addresses the spinning challenges, resulting in fabrics with enhanced properties.

JP7955052B2Active Publication Date: 2026-11-24エムエーライフマテリアルズ株式会社
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021060515
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2026-11-24
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing methods face difficulties in producing spunbond nonwoven fabrics using a copolymer of 4-methyl-1-pentene and propylene due to challenges in melt spinning under conventional conditions.

Method used

A spunbond nonwoven fabric containing fibers composed of a copolymer with 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins with 2 to 4 carbon atoms, with a core-sheath type composite fiber structure, and a draft ratio less than 2000 during melt spinning.

Benefits of technology

Enables the successful production of spunbond nonwoven fabrics with improved properties, such as stress relaxation and blocking resistance, using the specified copolymer composition and spinning conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955052000003
    Figure 0007955052000003
  • Figure 0007955052000004
    Figure 0007955052000004
  • Figure 0007955052000001
    Figure 0007955052000001
Patent Text Reader

Abstract

To provide a novel spun-bonded nonwoven fabric comprising a fiber having a constituent of copolymer mainly composed of a constitutional unit derived from 4-methyl-1-pentene.SOLUTION: A spun-bonded nonwoven fabric comprises a fiber having a constituent of copolymer A containing 50 mol% or more of a constitutional unit derived from 4-methyl-1-pentene and 1 mol% or more of a constitutional unit derived from α-olefin having 2 to 4 carbon atoms.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to spunbond nonwoven fabrics and methods for producing spunbond nonwoven fabrics. [Background technology]

[0002] In recent years, nonwoven fabrics made from fibers containing thermoplastic resins such as polypropylene and polyamide have been widely used in various applications due to their excellent breathability, flexibility, and lightweight properties. As for manufacturing methods for nonwoven fabrics, the melt-blown method and the spunbond method, which are suitable for mass production, are widely used.

[0003] Polypropylene and polyamide are the main thermoplastic resins used in the manufacture of nonwoven fabrics, but other polyolefins are sometimes used as well.

[0004] For example, Patent Document 1 describes a meltblown nonwoven fabric in which a copolymer of 4-methyl-1-pentene and propylene is used as the polyolefin, and this copolymer is considered preferable in terms of heat resistance and light weight. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2013-147771 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] The present inventors attempted to produce a spunbond nonwoven fabric using a copolymer of 4-methyl-1-pentene and propylene, as described in Patent Document 1, but found it difficult to produce the spunbond nonwoven fabric under the general conditions for producing spunbond nonwoven fabrics.

[0007] This disclosure has been made in view of the above, and aims to provide a novel spunbond nonwoven fabric containing fibers comprising a copolymer mainly composed of structural units derived from 4-methyl-1-pentene, and a method for producing the same. [Means for solving the problem]

[0008] The following embodiments are included as means to solve the above problems. <1> A spunbond nonwoven fabric containing fibers comprising copolymer A, which is composed of 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins having 2 to 4 carbon atoms. <2> The aforementioned fiber is a core-sheath type composite fiber comprising a core portion and a sheath portion. <1> The spunbond nonwoven fabric described above. <3> The core portion includes the copolymer A. <2> The spunbond nonwoven fabric described above. <4> The sheath portion comprises an α-olefin polymer (excluding copolymer A). <2> or <3> The spunbond nonwoven fabric described above. <5> The α-olefin polymer (excluding copolymer A) is at least one selected from the group consisting of polymer B, which contains 50 mol% or more of structural units derived from 4-methyl-1-pentene, has a content of 10 mol% or less of structural units derived from α-olefins having 8 or more carbon atoms relative to the total structural units, and has a content of less than 1 mol% of structural units derived from α-olefins having 2 to 4 carbon atoms relative to the total structural units, and a propylene polymer. <4> The spunbond nonwoven fabric described above. <6> The volume ratio of the sheath to the core, or core:sheath, is typically between 30:70 and 90:10. <2> ~ <5> Spunbond nonwoven fabric as described in any one of the following. <7> The aforementioned fiber is a monocomponent fiber. <1> The spunbond nonwoven fabric described above. <8> The average fiber diameter of the aforementioned fibers is 10 μm to 50 μm. <1> ~ <7> Spunbond nonwoven fabric as described in any one of the following. <9> A method for producing a spunbond nonwoven fabric, comprising discharging a thermoplastic resin or a thermoplastic resin composition containing the thermoplastic resin from a spinning nozzle and performing melt spinning, wherein the thermoplastic resin comprises a copolymer A containing 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from an α-olefin having 2 to 4 carbon atoms, wherein a draft ratio, which is a ratio of the fastest yarn speed to the yarn speed during discharging, is less than 2000. [Advantageous Effects of Invention]

[0009] According to the present disclosure, it is possible to provide a novel spunbond nonwoven fabric comprising fibers containing, as a component, a copolymer mainly containing structural units derived from 4-methyl-1-pentene, and a method for producing the same. [Brief Description of Drawings]

[0010] [Figure 1] Fig. 1 is a schematic view of a nonwoven fabric production apparatus used in a method 1 for producing a spunbond nonwoven fabric. [Figure 2] Fig. 2 is a schematic view of a nonwoven fabric production apparatus used in a method 2 for producing a spunbond nonwoven fabric. [Description of Embodiments]

[0011] In the present disclosure, a numerical range indicated using "to" refers to a range including the numerical values described before and after "to" as the minimum value and the maximum value, respectively. In the numerical ranges described stepwise in the present specification, the upper limit value or lower limit value described in a certain numerical range may be replaced with the upper limit value or lower limit value of another stepwise numerical range. Further, in the numerical ranges described in the present specification, the upper limit value or lower limit value described in a certain numerical range may be replaced with the values shown in Examples. In the present disclosure, the amount of each component in the composition means the total amount of the plurality of substances corresponding to the component present in the composition, unless otherwise specified, when a plurality of substances corresponding to each component are present in the composition. In this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.

[0012] <Spunbond nonwoven fabric> The spunbond nonwoven fabric of this disclosure contains fibers comprising a copolymer A as a component, which includes 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins having 2 to 4 carbon atoms.

[0013] When attempting to produce spunbond nonwoven fabric using a copolymer mainly containing structural units derived from 4-methyl-1-pentene, it is difficult to produce spunbond nonwoven fabric under general conditions for spunbond nonwoven fabric production. For example, when the aforementioned copolymer or resin composition containing the copolymer is extruded from a spinning nozzle, melt spinning may not be successful, making it difficult to obtain spunbond nonwoven fabric.

[0014] On the other hand, in this disclosure, a novel spunbond nonwoven fabric containing fibers made of the aforementioned copolymer can be obtained by adjusting the conditions for melt spinning the aforementioned copolymer or resin composition containing the copolymer that is extruded from a spinning nozzle.

[0015] The applications to which the spunbond nonwoven fabrics of this disclosure are applied are not particularly limited, and include, for example, absorbent articles (disposable diapers, disposable pants, sanitary napkins, incontinence pads, pet sheets, etc.), cosmetic materials (face masks, etc.); sanitary materials (poultices, sheets, towels, industrial masks, sanitary masks, hair caps, gauze, disposable underwear, supporters, poultices, adhesive patches, etc.); and packaging materials (oxygen absorbers, hand warmers, warming patches, food packaging materials, etc.).

[0016] The fibers contained in the spunbond nonwoven fabric of this disclosure are not particularly limited as long as they are composed of copolymer A, which comprises 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins having 2 to 4 carbon atoms.

[0017] The form of the fibers contained in the spunbond nonwoven fabric of this disclosure is not particularly limited and may be composite fibers or monocomponent fibers.

[0018] The composite fiber preferably comprises two or more thermoplastic resins, for example, two or more copolymers A as constituent components, or one or more copolymers A and one or more thermoplastic resins other than copolymer A as constituent components.

[0019] Examples of composite fibers include core-sheath type, side-by-side type, and sea-island type composite fibers, with core-sheath type composite fibers being preferred. Core-sheath type composite fibers only need to have a core and a sheath, and may be either homocore-core-sheath type or eccentric-core-sheath type. In eccentric-core-sheath type composite fibers, the core may or may not be exposed on the surface.

[0020] If the fibers contained in the spunbond nonwoven fabric of this disclosure are core-sheath type composite fibers, it is sufficient that copolymer A is contained in at least one of the core and sheath portions. Furthermore, it is preferable that copolymer A is contained in one of the core and sheath portions, and a thermoplastic resin other than copolymer A is contained in the other of the core and sheath portions. Examples of thermoplastic resins other than copolymer A include α-olefin polymers (excluding copolymer A) described later, and other thermoplastic resins.

[0021] When the fibers contained in the spunbond nonwoven fabric of this disclosure are core-sheath type composite fibers, the core portion may contain copolymer A, and the sheath portion may contain a thermoplastic resin other than copolymer A, preferably an α-olefin polymer (excluding copolymer A). From the viewpoint of suppressing blocking of the spunbond nonwoven fabric, it is preferable that the core portion contains copolymer A and the sheath portion contains a thermoplastic resin other than copolymer A, and it is preferable that the core portion contains copolymer A and the sheath portion contains an α-olefin polymer (excluding copolymer A). Furthermore, from the viewpoint of more effectively suppressing blocking of the spunbond nonwoven fabric by preventing the core portion containing copolymer A from being exposed from the surface, it is more preferable that the core-sheath type composite fiber is a homocore-core-sheath type, or an eccentric core-sheath type in which the core portion is not exposed from the surface.

[0022] If copolymer A is contained in the core, the content of copolymer A may be 80% to 100% by mass or 90% to 100% by mass relative to the total amount of the core. If a thermoplastic resin other than copolymer A or an α-olefin polymer (excluding copolymer A) is contained in the sheath, the content of the thermoplastic resin other than copolymer A or the content of the α-olefin polymer (excluding copolymer A) may be independently 80% to 100% by mass or 90% to 100% by mass relative to the total amount of the sheath.

[0023] In core-sheath composite fibers, the volume ratio of the core to the sheath, or core:sheath, is preferably 30:70 to 90:10, and more preferably 60:40 to 85:15 from the viewpoint of further improving stress relaxation. When the core contains copolymer A, a core volume of 30 or more (core:sheath ratio of 30:70 or more) tends to result in spunbond nonwoven fabrics exhibiting superior stress relaxation, while a core volume of 90 or less (core:sheath ratio of 90:10 or less) tends to allow for a reduction in the average fiber diameter of the core-sheath composite fiber and further improves blocking resistance. When the core contains copolymer A, a core:sheath ratio of 30:70 to 65:35 is preferred from the viewpoint of further improving blocking resistance.

[0024] A monocomponent fiber is a fiber whose constituent component is a single type of thermoplastic resin. When the fibers contained in the spunbond nonwoven fabric of this disclosure are monocomponent fibers, it is preferable that the monocomponent fiber is a fiber whose resin component is composed solely of copolymer A, and that the monocomponent fiber is a fiber whose resin component is composed solely of one type of copolymer A. In this disclosure, fibers other than composite fibers such as core-sheath type, side-by-side type, and sea-island type may be used as monocomponent fibers.

[0025] (Copolymer A) Copolymer A is a component of the fibers contained in spunbond nonwoven fabric, and contains 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins having 2 to 4 carbon atoms.

[0026] Examples of α-olefins having 2 to 4 carbon atoms include ethylene, propylene, and 1-butene, with propylene being preferred. Copolymer A may contain one structural unit derived from an α-olefin having 2 to 4 carbon atoms, or it may contain two or more structural units derived from α-olefins having 2 to 4 carbon atoms.

[0027] The content of structural units derived from 4-methyl-1-pentene in copolymer A is 50 mol% or more of the total structural units, preferably 60 mol% or more, and more preferably 70 mol% or more, from the viewpoint of dimensional stability. The content of structural units derived from 4-methyl-1-pentene is 99 mol% or less of the total structural units, preferably 90 mol% or less, and more preferably 80 mol% or less, from the viewpoint of further improving stress relaxation properties.

[0028] The content of constituent units derived from α-olefins with 2 to 4 carbon atoms in copolymer A is 1 mol% or more of the total constituent units, preferably 10 mol% or more, and more preferably 20 mol% or more, from the viewpoint of further improving stress relaxation properties. The content of constituent units derived from α-olefins with 2 to 4 carbon atoms is 50 mol% or less of the total constituent units, preferably 40 mol% or less, and more preferably 30 mol% or less, from the viewpoint of dimensional stability.

[0029] Copolymer A may contain constituent units derived from 4-methyl-1-pentene and polymerizable compounds other than α-olefins having 2 to 4 carbon atoms (hereinafter referred to as "other constituent units A"). From the viewpoint of shape stability and stress relaxation, the content of other constituent units A that may be contained in copolymer A is preferably 10 mol% or less, and more preferably 5 mol% or less, relative to the total constituent units.

[0030] The melt flow rate (MFR) of copolymer A is not particularly limited as long as it can be melt-spun, and may be 5 g / 10 min to 30 g / 10 min, or 7 g / 10 min to 20 g / 10 min. In this disclosure, the MFR is a value measured in accordance with ASTM D1238 at a temperature of 230°C and a load of 2.16 kg.

[0031] The density of copolymer A is not particularly limited as long as it can be melt-spun, and is approximately 0.820 g / cm³. 3 It may be ~0.870 g / cm³, or 0.830 g / cm³. 3 ~0.860g / cm 3 That's fine. The density of copolymer A can be measured by the method described in the examples below.

[0032] The melting point of copolymer A is not particularly limited as long as it can be melt-spun, and may be less than 200°C, and copolymer A does not need to exhibit a melting point. The melting point of copolymer A can be measured by the method described in the examples below.

[0033] Copolymer A can be obtained by polymerizing 4-methyl-1-pentene, an α-olefin having 2 to 4 carbon atoms, and, if necessary, other polymerizable compounds, using conventionally known catalysts, such as vanadium-based catalysts, titanium-based catalysts, magnesium-supported titanium catalysts, metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, Japanese Patent Publication No. 3-193796, or Japanese Patent Publication No. 02-41303.

[0034] (Thermoplastic resins other than copolymer A) Examples of thermoplastic resins other than copolymer A include α-olefin polymers (excluding copolymer A), other thermoplastic resins, and so on.

[0035] 《α-olefin polymers (excluding copolymer A)》 Examples of α-olefin polymers (excluding copolymer A) include α-olefin polymers containing 50 mol% or more of structural units derived from 4-methyl-1-pentene and not satisfying the conditions for copolymer A, and α-olefin polymers in which the content of structural units derived from 4-methyl-1-pentene is less than 50 mol%.

[0036] Examples of α-olefin polymers that contain 50 mol% or more of structural units derived from 4-methyl-1-pentene and do not satisfy the conditions for copolymer A include the polymers described in (1) and (2) below. (1) 4-methyl-1-pentene homopolymer (2) Copolymer having a content of 50 mol% or more of structural units derived from 4-methyl-1-pentene, and a content of less than 1 mol% of structural units derived from α-olefins having 2 to 4 carbon atoms.

[0037] As a polymer that satisfies either (1) or (2) above, polymer B is preferred, which contains 50 mol% or more of structural units derived from 4-methyl-1-pentene, has a content of 10 mol% or less of structural units derived from α-olefins having 8 or more carbon atoms relative to the total structural units, and has a content of less than 1 mol% of structural units derived from α-olefins having 2 to 4 carbon atoms relative to the total structural units.

[0038] Examples of α-olefins having 8 or more carbon atoms include 1-octene, 1-decene, 1-hexadecene, 1-heptadecene, and 1-octadecene. Polymer B may contain a constituent unit derived from one type of α-olefin having 8 or more carbon atoms, or it may contain a constituent unit derived from two or more types of α-olefins having 8 or more carbon atoms.

[0039] The content of 4-methyl-1-pentene-derived structural units in polymer B is 50 mol% to 100 mol% of the total structural units. If polymer B is a copolymer, the content of 4-methyl-1-pentene-derived structural units in polymer B may be 50 mol% to 99 mol%, or 60 mol% to 98 mol%, of the total structural units.

[0040] The content of constituent units derived from α-olefins with 8 or more carbon atoms that may be contained in polymer B is 10 mol% or less of the total constituent units, and may be 0.1 mol% to 5 mol%, or 0.5 mol% to 3 mol%.

[0041] The content of constituent units derived from α-olefins having 2 to 4 carbon atoms that may be contained in polymer B is less than 1 mol% of the total constituent units, and may be 0 mol% to 0.5 mol%, or 0 mol% to 0.3 mol%.

[0042] Polymer B may contain constituent units derived from 4-methyl-1-pentene, α-olefins having 8 or more carbon atoms, and polymerizable compounds other than α-olefins having 2 to 4 carbon atoms (hereinafter referred to as "other constituent units B"). The content of other constituent units B that may be contained in Polymer B may be 10 mol% or less, or 5 mol% or less, relative to the total constituent units.

[0043] The melt-spinning rate (MFR) of polymer B (measured in accordance with ASTM D1238 at a temperature of 260°C and a load of 5.0 kg) is not particularly limited as long as melt spinning is possible, and may be 5 g / 10 min to 600 g / 10 min, 70 g / 10 min to 500 g / 10 min, or 70 g / 10 min to 400 g / 10 min.

[0044] The density of polymer B is not particularly limited as long as it can be melt-spun, and is 0.820 g / cm³. 3 It may be ~0.870 g / cm³, or 0.825 g / cm³. 3 ~0.850g / cm 3 That's fine. The density of polymer B can be measured by the method described in the examples below.

[0045] The melting point of polymer B is not particularly limited as long as it can be melt-spun, and may be 200°C or higher, or 200°C to 250°C. The melting point of polymer B can be measured by the method described in the examples below.

[0046] Polymer B can be obtained by the same method as copolymer A described above.

[0047] Examples of α-olefin polymers having a content of less than 50 mol% of constituent units derived from 4-methyl-1-pentene include α-olefin polymers having a content of 50 mol% or more of constituent units derived from α-olefins other than 4-methyl-1-pentene (hereinafter also referred to as "specific α-olefin polymers").

[0048] Examples of specific α-olefin polymers include ethylene-based polymers and propylene-based polymers, with propylene-based polymers being preferred from the viewpoint of excellent spinnability and drawability.

[0049] Examples of ethylene-based polymers include ethylene-propylene random copolymers, high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), high-density polyethylene, and ethylene-1-butene random copolymers.

[0050] Examples of propylene polymers include propylene homopolymers and propylene random copolymers, which are copolymers of propylene as the main component and one or more α-olefins as minor components. Among these, propylene homopolymers are preferred. In propylene random copolymers, the content of constituent units derived from α-olefins is preferably 1 mol% to 10 mol%, and more preferably 1 mol% to 6 mol%, relative to the total number of constituent units.

[0051] For copolymerization of propylene random copolymers, α-olefins having 2 or more carbon atoms (excluding propylene) are preferred, and α-olefins having 2 or 4 to 8 carbon atoms are more preferred. Specific examples of α-olefins include ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene.

[0052] The melt-spinning rate (MFR) of the propylene polymer (measured in accordance with ASTM D1238 at a temperature of 230°C and a load of 2.16 kg) is not particularly limited as long as melt spinning is possible, and may be between 10 g / 10 min and 800 g / 10 min, or between 20 g / 10 min and 100 g / 10 min.

[0053] The density of the propylene polymer is not particularly limited as long as it can be melt-spun, and is 0.900 g / cm³. 3 ~0.945g / cm 3and may be 0.910 g / cm 3 to 0.940 g / cm 3 . The density of the propylene-based polymer can be measured by the method described in Examples below.

[0054] The melting point of the propylene-based polymer is not particularly limited as long as it can be melt-spun, and may be 125°C or higher, or 125°C to 165°C. The melting point of the propylene-based polymer can be measured by the method described in Examples below.

[0055] When a propylene / α-olefin random copolymer is used as the propylene-based polymer, its melting point (Tm) is preferably 153°C or lower, more preferably 125°C to 150°C. When a propylene homopolymer is used as the propylene-based polymer, its melting point (Tm) is preferably 155°C or higher, more preferably 157°C to 165°C.

[0056] The propylene-based polymer is usually produced by using a Ziegler-Natta catalyst, which is a combination of a so-called titanium-containing solid transition metal component and an organic metal component, or a metallocene catalyst comprising a transition metal compound of Groups 4 to 6 of the periodic table having at least one cyclopentadienyl skeleton and a promoter component, and homopolymerizing propylene or copolymerizing propylene with a small amount of α-olefin by slurry polymerization, gas phase polymerization, or bulk polymerization.

[0057] The α-olefin polymer (excluding copolymer A) is preferably at least one selected from the group consisting of the aforementioned polymer B and propylene-based polymers.

[0058] Other Thermoplastic Resins Other thermoplastic resins are not particularly limited and include polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon-6, nylon-66, and polymetaxylene adipamide; polyvinyl chloride; polyimide; ethylene-vinyl acetate copolymer; polyacrylonitrile; polycarbonate; polystyrene; and ionomers. The other thermoplastic resin may consist of one type or a mixture of two or more types.

[0059] (Additives) The fibers contained in the spunbond nonwoven fabric of this disclosure may optionally include various known additives such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, and waxes. The nonwoven fabrics disclosed herein may contain other components as needed. Examples of other components include various known additives such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antifogging agents, lubricants, dyes, pigments, light stabilizers, antiblocking agents, dispersants, nucleating agents, softeners, water repellents, fillers, natural oils, synthetic oils, waxes, antimicrobial agents, preservatives, matting agents, rust inhibitors, fragrances, defoamers, antifungal agents, and insect repellents. These other components may be contained within the fibers of the spunbond nonwoven fabric or may be attached to the surface of the fibers.

[0060] The average fiber diameter of the fibers contained in the spunbond nonwoven fabric of this disclosure is not particularly limited, but is preferably 10 μm to 50 μm, and more preferably 12 μm to 30 μm. The average fiber diameter of the fibers can be measured by the method described in the examples below.

[0061] The basis weight of the spunbond nonwoven fabrics of this disclosure is not particularly limited, but is 5 g / m². 2 ~100g / m 2 Preferably, it is 10 g / m 2 ~50g / m 2 It is preferable that it be so. The basis weight of the spunbond nonwoven fabric can be measured by the method described in the examples below.

[0062] The thickness of the spunbond nonwoven fabric of this disclosure is not particularly limited, but is preferably 0.05 mm to 10.0 mm, more preferably 0.07 mm to 5.0 mm, and even more preferably 0.10 mm to 1.0 mm. The thickness of the spunbond nonwoven fabric can be measured by the method described in the examples below.

[0063] The spunbond nonwoven fabric may have both a crimped portion and an uncrimped portion. The area ratio of the crimped portion is preferably 5% to 20%, and more preferably 6% to 19%. The area ratio of the crimped portion is determined by taking a 10 mm x 10 mm test piece from the spunbond nonwoven fabric, observing the contact surface of the test piece with the embossing roll using an electron microscope (magnification: 100x), and defining it as the ratio of the area of ​​the heat-crimped portion to the observed area of ​​the spunbond nonwoven fabric. The area ratio of the protrusions formed on the embossing roll that can form the crimped portion is also called the "embossed area ratio."

[0064] The spunbond nonwoven fabric of the present disclosure may have a structure in which two or more layers of the spunbond nonwoven fabric of the present disclosure are laminated, or it may have a structure in which at least one layer of the spunbond nonwoven fabric of the present disclosure is laminated with a nonwoven fabric other than the spunbond nonwoven fabric of the present disclosure, a knitted fabric, a woven fabric, paper, a film (including a sheet), etc., in any order. Examples of nonwoven fabrics other than the spunbond nonwoven fabric of this disclosure include, for example, spunbond nonwoven fabrics (excluding the spunbond nonwoven fabric of this disclosure), meltblown nonwoven fabrics, wet-laid nonwoven fabrics, spunlace nonwoven fabrics, dry-laid nonwoven fabrics, dry-pulp nonwoven fabrics, airlaid nonwoven fabrics, waterjet nonwoven fabrics, flash-spun nonwoven fabrics, open-fiber nonwoven fabrics, needle-punched nonwoven fabrics, and various other known short-fiber and long-fiber nonwoven fabrics (e.g., long-fiber cellulose nonwoven fabrics).

[0065] When laminating two or more layers of the spunbond nonwoven fabric of this disclosure, or when laminating at least one layer of the spunbond nonwoven fabric of this disclosure with a material other than the spunbond nonwoven fabric in any order, the method of laminating (e.g., bonding) each layer is not particularly limited. For example, various known methods can be used, including thermal embossing, thermal fusion methods such as ultrasonic bonding, mechanical entanglement methods such as needle punching and water jetting, adhesive methods such as hot melt adhesives and urethane adhesives, and extrusion lamination.

[0066] <Method for manufacturing spunbond nonwoven fabric> The method for manufacturing the spunbond nonwoven fabric of this disclosure will be described below. The spunbond nonwoven fabric of this disclosure may be manufactured by the method for manufacturing the spunbond nonwoven fabric of this disclosure described below, or by other manufacturing methods.

[0067] The present disclosure is a method for producing a spunbond nonwoven fabric, comprising extruding a thermoplastic resin or a thermoplastic resin composition containing the thermoplastic resin from a spinning nozzle and melt spinning it, wherein the thermoplastic resin contains copolymer A comprising 50 mol% or more of structural units derived from 4-methyl-1-pentene and 1 mol% or more of structural units derived from α-olefins having 2 to 4 carbon atoms, and the draft ratio, which is the ratio of the fastest yarn speed to the yarn speed at the time of extrusion, is less than 2000.

[0068] When attempting to use copolymer A, such as a copolymer of 4-methyl-1-pentene and propylene containing 50 mol% or more of structural units derived from 4-methyl-1-pentene (an example of copolymer A), in the production of spunbond nonwoven fabric, it is difficult to produce spunbond nonwoven fabric under the general conditions for spunbond nonwoven fabric production.

[0069] On the other hand, in the method for producing spunbond nonwoven fabric according to the present disclosure, when melt spinning a thermoplastic resin containing copolymer A, the draft ratio, which is the ratio of the fastest yarn speed to the yarn speed at the time of extrusion, is less than 2000. As a result, even when copolymer A is used in the production of spunbond nonwoven fabric, the spunbond nonwoven fabric can be suitably produced.

[0070] The configuration of the manufacturing method for the spunbond nonwoven fabric of this disclosure will be described below with reference to Figures 1 and 2. The configuration common to the spunbond nonwoven fabric of this disclosure described above will not be explained.

[0071] (Method for manufacturing spunbond nonwoven fabric 1) First, a method for manufacturing spunbond nonwoven fabric 1 will be described with reference to Figure 1. In the method for manufacturing spunbond nonwoven fabric 1 of this disclosure, as an example, a manufacturing apparatus equipped with a spinning section 11 having a closed cooling chamber structure as shown in Figure 1 can be used. In one embodiment, the cooling chamber may be open. The nonwoven fabric manufacturing apparatus shown in Figure 1 is an apparatus for manufacturing spunbond nonwoven fabric containing monocomponent fibers using a thermoplastic resin made of copolymer A, or a thermoplastic resin composition containing said thermoplastic resin.

[0072] The nonwoven fabric manufacturing apparatus comprises a spinning unit 11 for melt-spinning molten thermoplastic resin or thermoplastic resin composition, and for cooling and stretching the melt-spun continuous fiber group 22; a movable collection member 51 for collecting the stretched continuous fiber group 22; and a suction unit 39 for efficiently collecting the continuous fiber group 22 on the movable collection member 51.

[0073] The nonwoven fabric manufacturing apparatus may include an embossing roll and a flat roll for entanglement treatment of the nonwoven web 43 consisting of the collected continuous fiber group 22 by heat compression, and a winder for winding up the spunbond nonwoven fabric after heat compression.

[0074] Methods for entanglement of nonwoven webs are not limited to the aforementioned method of heat embossing using an embossing roll, but include various other methods such as ultrasonic fusion, water jet entanglement, hot air-through fusion, and needle punching.

[0075] The spinning unit 11 includes an extruder 32 for extruding a first thermoplastic polymer, a spinneret 34 for discharging molten thermoplastic resin or thermoplastic resin composition from a spinning nozzle, a cooling chamber 38C for cooling the continuous fiber group 22 discharged from the spinning nozzle of the spinneret 34, cooling air supply units 38A and 38B for supplying cooling air 36, and a stretching unit 38D for stretching the continuous fiber group 22.

[0076] In the spinning section 11, a thermoplastic resin or thermoplastic resin composition is extruded and introduced into the spinneret 34. Next, the molten thermoplastic resin or thermoplastic resin composition is discharged from the spinning nozzle of the spinneret 34 and melt-spun. The melting temperature of the thermoplastic resin is not particularly limited as long as it is capable of melting the thermoplastic resin.

[0077] The melt-spun continuous fiber group 22 is introduced into the cooling chamber 38C. The continuous fiber group 22 is cooled by cooling air 36 supplied from either or both of the cooling air supply unit 38A and the cooling air supply unit 38B. The cooled continuous fiber group 22 is introduced into the stretching unit 38D located downstream of the cooling chamber 38C. The stretching unit 38D is provided in a narrow passage shape. As the velocity of the cooling air increases in the narrow passage, the continuous fiber group 22 introduced into the stretching unit 38D is stretched.

[0078] When melt spinning thermoplastic resins, the draft ratio, which is the ratio of the fastest yarn speed to the yarn speed at extrusion, is less than 2000. The draft ratio can be adjusted to 2000 or more by adjusting the flow rate of the cooling air, the flow velocity of the cooling air, the pore size of the spinning nozzle, the single-hole extrusion rate, etc. For example, reducing the flow rate of the cooling air, the flow velocity of the cooling air, etc., tends to reduce the draft ratio.

[0079] The draft ratio is the ratio of the fastest yarn speed to the yarn speed during extrusion. The yarn speed during extrusion can be calculated from the nozzle pore diameter, the amount of thermoplastic resin extruded from the spinning nozzle, and the density of the thermoplastic resin. The yarn speed is maximum in the stretching section 38D. Therefore, the fastest yarn speed can be measured in the stretching section 38D, for example, by the laser Doppler method as described in the examples below.

[0080] The draft ratio may be, for example, 400 to 1500 or 500 to 1300. From the viewpoint of suitably producing spunbond nonwoven fabric containing monocomponent fibers, the draft ratio may be 400 to 1000 or 500 to 800.

[0081] The stretched continuous fiber group 22 is dispersed and collected on the mobile collection member 51. The dispersed continuous fiber group 22 is then efficiently collected on the mobile collection member 51 by a suction unit 39 located at the bottom of the collection surface of the mobile collection member 51, forming a nonwoven web 43 containing monocomponent fibers.

[0082] (Method for manufacturing spunbond nonwoven fabric 2) Next, with reference to Figure 2, Method 2 for Manufacturing Spunbond Nonwoven Fabric will be described. Method 2 for manufacturing spunbond nonwoven fabric differs from Method 1 for manufacturing spunbond nonwoven fabric described above in that it is a method for manufacturing spunbond nonwoven fabric containing composite fibers. Note that explanations of matters common to Method 1 for manufacturing spunbond nonwoven fabric described above will be omitted.

[0083] In the method for producing spunbond nonwoven fabric 2, a first thermoplastic resin consisting of copolymer A, or a first thermoplastic resin composition containing the first thermoplastic resin, and a second thermoplastic resin other than copolymer A (preferably an α-olefin polymer (excluding copolymer A)), or a second thermoplastic resin composition containing the second thermoplastic resin are used.

[0084] The spinning unit 12 includes a first extruder 32A for extruding a first thermoplastic resin, a second extruder 32B for extruding a second thermoplastic resin, a spinneret 34 for melt-spinning the molten first thermoplastic polymer and the second thermoplastic polymer, a cooling chamber 38C for cooling the continuous fiber group 23 melt-spun from the spinneret 34, cooling air supply units 38A and 38B for supplying cooling air 36, and a stretching unit 38D for stretching the continuous fiber group 23.

[0085] A continuous fiber group 23, which is a composite fiber, is obtained by extruding a first thermoplastic resin from a first extruder 32A and a second thermoplastic resin from a second extruder 32B, and then performing composite spinning. By appropriately changing the cross-sectional shape of the spinning nozzle that discharges the first thermoplastic resin and the second thermoplastic resin, composite fibers of the side-by-side type, concentric core-sheath type, or eccentric core-sheath type can be manufactured. Furthermore, by appropriately changing the cross-sectional shape of the spinning nozzle, the volume ratio of the core and sheath in the concentric core-sheath type or eccentric core-sheath type core-sheath composite fiber can be adjusted.

[0086] The draft ratio may be, for example, 400 to 1500 or 500 to 1300. From the viewpoint of suitably producing spunbond nonwoven fabrics containing composite fibers, preferably core-sheath type or eccentric core-sheath type composite fibers, the draft ratio may be 600 to 1500 or 700 to 1300. Furthermore, from the viewpoint of reducing the average fiber diameter of the composite fibers, the draft ratio may be 400 or more but less than 2000, or it may be 700 to 1900.

[0087] The stretched continuous fiber group 23 is dispersed and collected on the mobile collection member 51. The dispersed continuous fiber group 23 is then efficiently collected on the mobile collection member 51 by a suction unit 39 located at the bottom of the collection surface of the mobile collection member 51, forming a nonwoven web 44 containing composite fibers. [Examples]

[0088] The embodiments of the present invention will be described in more detail below based on the examples, but the present invention is not limited to these embodiments, which are one embodiment of the present invention. The physical properties and other values ​​in the examples and comparative examples were measured by the following method.

[0089] (1) Weight [g / m 2 ] Ten test specimens measuring 100 mm (flow direction: MD) × 100 mm (direction perpendicular to the flow direction: CD) were taken from the obtained nonwoven fabric. The test specimens were taken at 10 locations along the CD direction. Next, under conditions of 23°C and 50% RH relative humidity, the mass [g] of each test specimen was measured using a top-loading electronic balance (manufactured by Kensei Kogyo Co., Ltd.). The average mass of each test specimen was calculated. From the calculated average value, 1 m 2 Convert to mass per unit [g], round to two decimal places, and obtain the basis weight [g / m²] of each nonwoven fabric sample. 2 ]

[0090] (2) Thickness [mm] Ten test specimens measuring 100 mm (MD) x 100 mm (CD) were taken from the obtained nonwoven fabric. The test specimens were taken from the same location as the specimens used for basis weight measurement. Next, a load-type thickness gauge (manufactured by Ozaki Seisakusho Co., Ltd.) was used on each of the sampled test specimens to determine the thickness at 7 g / cm³ in accordance with the method described in JIS L 1096:2010. 2 The thickness [mm] was measured under a load. The average thickness of each test specimen was calculated. The average value was rounded to the third decimal place to obtain the thickness [mm] of each nonwoven fabric sample.

[0091] (3) Average fiber diameter (μm) The obtained nonwoven fabric was photographed at 200x magnification using an electron microscope (Hitachi S-3500N). The diameter (width) of the fibers was measured from the captured images, and the imaging and diameter measurement were repeated until the total number of fibers exceeded 100 (n=100). The arithmetic mean of the obtained fiber diameters was defined as the average fiber diameter (μm).

[0092] (4) Stress relaxation rate (%) A test specimen measuring 50 mm wide (CD) x 200 mm long (MD) was taken from the obtained nonwoven fabric. Using a tensile testing machine (Shimadzu Autograph AGS-J), the stress (initial stress) was measured when the test specimen was stretched by 10% under the conditions of a chuck distance of 100 mm and a head speed of 300 mm / min. The stretched test specimen was then held for 120 seconds, and the change in stress during that time was also measured. The stress relaxation rate (%) was then calculated from the difference between the initial stress and the stress 60 seconds after stretching.

[0093] (5) Evaluation of peel strength Two test specimens measuring 50 mm (CD) x 100 mm (MD) were taken from the obtained nonwoven fabric. These two specimens were stacked to form a two-layer test specimen measuring 50 mm (CD) x 100 mm (MD). Next, a 5 kg weight measuring 50 mm x 50 mm was placed on one side of the two-layer test specimen. With the weight still on the two-layer test specimen, it was left to stand in a 50°C air-drying oven for 20 minutes. After that, the two-layer test specimen was removed from the oven and left to stand at 25°C for 5 minutes. Next, the weight was moved from the two-layer test specimen, and the test specimen on the side without the weight was peeled off and gripped by the upper and lower chucks of a tensile testing machine. The maximum load (N) was measured under conditions of a tensile speed of 300 mm / min and 23°C. This was repeated three times, and the average value of the maximum load was calculated. The average of the obtained maximum loads (N) was used to evaluate the peel strength according to the evaluation criteria below. An evaluation of A or B indicates low peel strength and excellent blocking resistance. -Evaluation Criteria- A: The part where the weight is attached peels off naturally, making it impossible to measure the peel strength. B: The average peel strength is less than 1.0 N. C: The average peel strength is 1.0 N or greater, or the test specimen breaks without peeling.

[0094] [Synthesis of copolymer A] A 1.5-liter stainless steel autoclave with stirring blades, thoroughly purged with nitrogen, was charged with 300 mL of n-hexane (dried on activated alumina under a dry nitrogen atmosphere) and 450 mL of 4-methyl-1-pentene at 23°C. 0.75 mL of a 1.0 mmol / mL toluene solution of triisobutylaluminum (TIBAL) was then added to the autoclave and the mixture was stirred. Next, the autoclave was heated to an internal temperature of 60°C and pressurized with propylene to a total pressure of 0.40 MPa (gauge pressure). Subsequently, 0.34 mL of a toluene solution containing 1 mmol of methyl aluminoxane (in terms of Al) and 0.01 mmol of diphenylmethylene (1-ethyl-3-t-butyl-cyclopentadienyl)(2,7-di-t-butyl-fluorenyl) zirconium dichloride, which had been prepared in advance, was injected into the autoclave under nitrogen pressure to start polymerization. During the polymerization reaction, the temperature inside the autoclave was adjusted to 60°C. 60 minutes after the start of polymerization, 5 mL of methanol was injected into the autoclave under nitrogen pressure to stop the polymerization, and the autoclave was depressurized to atmospheric pressure. Acetone was poured into the reaction solution while stirring. The resulting powdered polymer containing the solvent was dried at 100°C under reduced pressure for 12 hours. The yield of copolymer A was 36.9 g, with 72 mol% of the constituent units derived from 4-methyl-1-pentene and 28 mol% derived from propylene. The obtained copolymer A had a MFR (measured according to ASTM D1238 at a temperature of 230°C and a load of 2.16 kg) of 11 g / 10 min, and its density, measured as follows, was 0.840 g / cm³. 3 Therefore, when we attempted to measure the melting point as follows, it did not show a melting point.

[0095] [Synthesis of Polymer B] Polymer B was obtained by synthesizing polymer A-1 of Japanese Patent Publication No. 2017-074775 according to the method described in the examples of Japanese Patent Publication No. 2017-074775. The constituent units derived from 4-methyl-1-pentene in polymer B amounted to 97.8 mol%, and the constituent units derived from 1-decene amounted to 2.2 mol%. The obtained polymer B was subjected to the MFR measurement according to the method described in the examples of Japanese Patent Publication No. 2017-074775, and its density and melting point were measured according to the following method. The MFR of polymer B (measured in accordance with ASTM D1238 at a temperature of 260°C and a load of 5.0 kg) was 100 g / 10 min, and its density was 0.833 g / cm³. 3 Its melting point was 232°C.

[0096] [Preparation of propylene homopolymer] In addition to copolymer A and polymer B mentioned above, propylene homopolymer (PP in the table) was prepared as a thermoplastic resin. For the propylene homopolymer, the MFR (measured according to ASTM D1238 at a temperature of 230°C and a load of 2.16 kg) was 60 g / 10 min, and the density measured as follows was 0.910 g / cm³. 3 The melting point, as measured as follows, was 160°C.

[0097] (density) The densities of copolymer A, polymer B, and propylene homopolymer were measured in accordance with JIS K7112 (density gradient tube method). 3 ) was used as an indicator of lightness. The melt density will be calculated from the PVT measurement.

[0098] (Melting point of copolymer A and melting point of propylene homopolymer) The melting points (Tm) of copolymer A and propylene homopolymer were measured using a differential scanning calorimeter (DSC220C model, Seiko Instruments). Approximately 5 mg of copolymer A was sealed in an aluminum pan for measurement and heated from room temperature to 200°C at a rate of 10°C / min. It was held at 200°C for 5 minutes, and then cooled to -50°C at a rate of 10°C / min. After holding at -50°C for 5 minutes, it was heated a second time to 200°C at a rate of 10°C / min, and the melting point (Tm) was calculated from the peak of the crystal melting peak in the calorimetry curve during this second heating.

[0099] (Melting point of polymer B) The melting point (Tm) of polymer B was measured using a differential scanning calorimeter (DSC220C model, Seiko Instruments Corporation). Approximately 5 mg of polymer B was sealed in an aluminum pan for measurement and heated from room temperature to 290°C at a rate of 100°C / min. It was held at 290°C for 5 minutes, and then cooled to -100°C at a rate of 10°C / min. The melting point (Tm) was calculated from the peak of the crystal melting peak in the calorific value curve when heating from -100°C to 290°C at a rate of 10°C / min.

[0100] [Example 1] A spunbond nonwoven fabric was manufactured using the spunbond method with a spunbond nonwoven fabric manufacturing apparatus equipped with a single extruder. A nozzle for monocomponent fibers was used as the nozzle. Copolymer A was melted in the extruder at a molding temperature of 250°C. 1 cm 2 Molten copolymer A was extruded at a rate of 0.6 g / min per nozzle from a spinneret having four 0.6 mmφ nozzles per nozzle. Cooling air was then supplied to the cooling chamber and the fibers were stretched in the stretching section, and melt spinning was performed using the spunbond method. After the stretched fibers were deposited on the collection surface, a basis weight of 20 g / m was achieved by thermal embossing. 2 We manufactured spunbond nonwoven fabric.

[0101] In the stretched section, the yarn velocity was measured using the laser Doppler method. A PIN-30N laser oscillator manufactured by Onizuka Glass Co., Ltd. was used. The laser wavelength was 10.6 μm, the nominal power rating was 30 W, the beam divergence angle was 1.0 mrad, and the polarization state was random. An Ophir AN / 2 laser power meter was used as the receiver. The draft ratio was calculated using the following formula from the fastest yarn velocity obtained and the yarn velocity at ejection, which was determined from the following formula. Discharge rate = Single-hole discharge volume / [(Nozzle diameter / 2)] 2 [xπ × resin density] Draft ratio = Fastest thread velocity / Thread velocity during discharge

[0102] [Examples 2, 3 and Comparative Examples 1-4] In Example 1, the nozzle diameter and single-hole discharge volume were changed as shown in Table 1, and the fastest yarn speed was adjusted by adjusting the amount and speed of the cooling air. Except for these changes, the spunbond nonwoven fabric was manufactured in the same manner as in Example 1.

[0103] [Example 4] Spunbond nonwoven fabric was manufactured using the spunbond method with a spunbond nonwoven fabric manufacturing apparatus equipped with two extruders. A concentric core-sheath type nozzle was used as the nozzle. Copolymer A and propylene homopolymer were melted at a molding temperature of 250°C by the two extruders. The ratio of core to sheath (core:sheath) was adjusted by controlling the discharge rate of the propylene homopolymer (core) and copolymer A (sheath) by controlling the rotation speed of two gear pumps. 1 cm 2 Molten copolymer A and propylene homopolymer were extruded at a rate of 0.6 g / min per nozzle from a spinneret having four 0.6 mmφ nozzles. Cooling air was then supplied to the cooling chamber and the fibers were stretched in the stretching section to perform composite melt spinning by the spunbond method. After the stretched fibers were deposited on the collection surface, a basis weight of 20 g / m was achieved by thermal embossing. 2 A spunbond nonwoven fabric was manufactured. The fibers contained in the spunbond nonwoven fabric obtained in Example 4 were concentric core-sheath composite fibers in which the core was a propylene homopolymer and the sheath was copolymer A, with a core-to-sheath ratio of 50:50.

[0104] [Examples 5-8] In Example 4, a spunbond nonwoven fabric containing core-sheath composite fibers was manufactured in the same manner as in Example 4, except that the types of resins constituting the core and sheath, the ratio of the core to the sheath (core:sheath), and the melting temperature were changed as shown in Table 1.

[0105] [Comparative Example 5] In Example 1, a spunbond nonwoven fabric was manufactured in the same manner as in Example 1, except that the type of resin, single-hole discharge volume, and melting temperature were changed as shown in Table 1.

[0106] [Comparative Example 6] Meltblown nonwoven fabric was manufactured by the meltblown method using a meltblown nonwoven fabric manufacturing apparatus equipped with a single extruder. A nozzle for monocomponent fibers was used as the nozzle. Copolymer A was melted by the extruder at a molding temperature of 250°C. Molten copolymer A was introduced from a spinning die with a 0.38 mmφ nozzle and a pore spacing of 1.0 mm, at a rate of 0.2 g / min per pore, using heated air (temperature: 250°C, flow rate: 240 Nm³) blown from both sides of the spinning nozzle. 3 The fibers were extruded at a rate of ( / hour / m) and melt-spinned using the melt-blown method. The fibers were deposited on the collection surface, with a basis weight of 20 g / m². 2 We manufactured meltblown nonwoven fabric.

[0107] For the obtained spunbond nonwovens and meltblown nonwovens, the draft ratio, basis weight, thickness, average fiber diameter, and stress relaxation rate were determined using the method described above, and the peel strength was evaluated using the method described above. The results are shown in Tables 1 and 2.

[0108] [Table 1]

[0109] [Table 2]

[0110] As shown in Comparative Examples 1-4 of Table 2, when the draft ratio during the production of spunbond nonwoven fabric was 2000 or higher, spinning was not possible, and therefore spunbond nonwoven fabric could not be produced. On the other hand, as shown in Examples 1 to 8 of Table 1, it was possible to manufacture spunbond nonwoven fabric when the draft ratio during the manufacturing process was less than 2000. Furthermore, as shown in Table 1, spunbond nonwoven fabrics containing concentric core-sheath composite fibers, in which the core is composed of copolymer A, were found to have good peel strength and excellent blocking resistance.

Claims

1. The fiber comprises a copolymer A containing 60 mol% to 99 mol% of structural units derived from 4-methyl-1-pentene and 1 mol% to 40 mol% of structural units derived from α-olefins having 2 to 4 carbon atoms. The aforementioned fiber is a core-sheath type composite fiber comprising a core portion and a sheath portion. The core portion is a spunbond nonwoven fabric containing the copolymer A.

2. The spunbond nonwoven fabric according to claim 1, wherein the sheath portion comprises an α-olefin polymer (excluding copolymer A).

3. The spunbond nonwoven fabric according to claim 2, wherein the α-olefin polymer (excluding copolymer A) is at least one selected from the group consisting of polymer B, which contains 50 mol% or more of structural units derived from 4-methyl-1-pentene, in which the content of structural units derived from α-olefins having 8 or more carbon atoms is 10 mol% or less of the total structural units, and the content of structural units derived from α-olefins having 2 to 4 carbon atoms is less than 1 mol% of the total structural units, and a propylene polymer.

4. The spunbond nonwoven fabric according to any one of claims 1 to 3, wherein the volume ratio of the sheath portion to the core portion, i.e., core portion:sheath portion, is 30:70 to 90:

10.

5. The spunbond nonwoven fabric according to any one of claims 1 to 4, wherein the average fiber diameter of the aforementioned fibers is 10 μm to 50 μm.

6. A method for producing a spunbond nonwoven fabric, comprising extruding a thermoplastic resin or a thermoplastic resin composition containing the thermoplastic resin from a spinning nozzle and melt spinning it, The thermoplastic resin comprises copolymer A, which contains 60 mol% to 99 mol% of structural units derived from 4-methyl-1-pentene and 1 mol% to 40 mol% of structural units derived from α-olefins having 2 to 4 carbon atoms. A method for producing a spunbond nonwoven fabric according to any one of claims 1 to 5, wherein the draft ratio, which is the ratio of the fastest yarn speed to the yarn speed at the time of discharge, is less than 2000.

Citation Information

Patent Citations

  • Production of composite fiber

    JP1981015417A

  • Production of porous hollow poly-4-methyl-pentene-1 fiber

    JP1988256712A

  • Special filament non-woven fabric and production thereof

    JP1991167361A

  • Melt-blown nonwoven fabric, application thereof and production method thereof

    JP2013147771A

  • Polyolefin multilayer filament

    JP2017197856A