Method for producing sulfur-containing compositions
By monitoring and adjusting SO2 emissions during the heating of sulfur and carbon sources in a rotary kiln, the method simplifies and enhances the control over the composition of sulfur-containing products, addressing the inefficiencies of previous methods.
Patent Information
- Application Number
- JP2022031987
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-03-02
AI Technical Summary
Existing methods for producing sulfur-containing compositions require multiple iterations to adjust component ratios, making the process cumbersome and inefficient.
A method involving heating a sulfur source and carbon source in a rotary kiln while monitoring SO2 emissions from the exhaust gas to adjust preparation and operating conditions, allowing for precise control over the composition of the sulfur-containing product.
Enables a simpler and more efficient method to change the ratios of components in sulfur-containing compositions by monitoring and adjusting SO2 emissions during the heating process.
Smart Images

Figure 0007955061000007 
Figure 0007955061000008 
Figure 0007955061000009
Abstract
Description
[Technical Field]
[0001] This invention relates to a method for producing a sulfur-containing composition. [Background technology]
[0002] A method for producing a sulfur-containing composition is known, which involves heating a sulfur source containing sulfur and a carbon source containing carbon. For example, Patent Document 1 discloses a method for obtaining calcium sulfide by mixing gypsum and a pulverized carbon source and heating them under a reducing atmosphere. Patent Document 2 discloses a method for producing a heavy metal elution inhibitor containing sulfides by adding an oxide to a raw material containing a reducing agent and a metal sulfate, granulating it, and then heating and melting it. Patent Document 2 also describes a method for producing a heavy metal elution inhibitor containing metal sulfides, which involves melting a raw material containing a reducing agent such as carbon and a metal sulfate at 1200 to 1600°C under an oxidizing atmosphere. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2005-306911 [Patent Document 2] Japanese Patent Publication No. 2004-337677 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Conventionally, the ratios of various components in the sulfur-containing composition, which is the product, were determined by analyzing the sulfur-containing composition after its manufacture. Therefore, if it was necessary to change the ratios of the various components, it was necessary to perform the manufacture several times with different conditions and analyze each product, which was cumbersome. Consequently, a simpler method for changing the ratios of various components in a sulfur-containing composition is desired.
[0005] This invention has been made in view of the above circumstances, and aims to provide a manufacturing method that allows for a simpler change in the ratio of various components contained in a sulfur-containing composition. [Means for solving the problem]
[0006] The present invention provides a method for producing a sulfur-containing composition, comprising a heating step of heating raw materials containing a sulfur source and a carbon source in a rotary kiln, and checking the amount of SO2 discharged from the kiln exhaust gas during the heating step, and adjusting the preparation conditions of the raw materials or the operating conditions of the heating step.
[0007] The operating conditions adjusted in the above heating process may be at least one of the heating temperature in the rotary kiln, the oxygen concentration in the rotary kiln, and the residence time of the raw material.
[0008] The residence time of the raw material in the above heating process may be adjusted by changing at least one of the following: the kiln rotation speed, the kiln tilt angle, the amount of raw material input, the shape of the raw material, and the size of the raw material.
[0009] The process may further include a step of contacting the kiln exhaust gas described above with a slurry containing a calcium compound to obtain sulfites. [Effects of the Invention]
[0010] According to the present invention, a manufacturing method is provided that allows for a simpler change in the ratio of various components contained in a sulfur-containing composition. [Brief explanation of the drawing]
[0011] [Figure 1] Figure 1 shows the relationship between the product of the SO2 concentration and airflow rate of the kiln exhaust gas, and calcium oxide in the sulfur-containing composition. [Figure 2] Figure 2 is a plot of Example 1, showing the values obtained by multiplying the kiln exhaust gas flow rate by the SO2 concentration, and the CaS and CaO content in the obtained sulfur-containing composition. [Figure 3]FIG. 3 is a graph plotting, for Example 2, the value obtained by multiplying the air volume of kiln exhaust gas by the SO2 concentration, against the CaS and CaO contents in the obtained sulfur-containing composition. [Figure 4] FIG. 4 is a graph plotting, for Example 3, the value obtained by multiplying the air volume of kiln exhaust gas by the SO2 concentration, against the CaS and CaO contents in the obtained sulfur-containing composition. [Figure 5] FIG. 5 is a graph plotting, for Example 4, the value obtained by multiplying the air volume of kiln exhaust gas by the SO2 concentration, against the CaS and CaO contents in the obtained sulfur-containing composition. [Figure 6] FIG. 6 is a schematic diagram showing an example of a calcination apparatus for carrying out the production method of the present embodiment. [Description of Embodiments]
[0012] A method for producing a sulfur-containing composition according to an embodiment of the present invention includes a heating step of heating a raw material containing a sulfur source and a carbon source in a rotary kiln, and during the heating step, the amount of SO2 emissions from kiln exhaust gas is checked to adjust the preparation conditions of the raw material or the operating conditions of the rotary kiln. In this specification, the SO2 emission amount is the product of the SO2 concentration in the kiln exhaust gas and the air volume flowing through the exhaust duct (unit: volume ppm·Nm 3 / min).
[0013] (Mixing Step) The production method of the present embodiment may first include a mixing step of mixing a sulfur source and a carbon source, which are raw materials. The mixing method is not particularly limited, and mixing may be performed using a mixer or the like. Mixing may be performed either wet or dry.
[0014] As the sulfur source, any raw material containing sulfur can be used without particular limitation. The sulfur source may contain a compound containing sulfur having a positive oxidation number, and may be a compound containing an oxoacid of sulfur (such as an oxoacid salt of sulfur). Examples of such compounds include sulfates, sulfites, bisulfates (hydrogen sulfates), and the like. These salts may be hydrates. The sulfur source may include one or more types of sulfur-containing compounds.
[0015] Furthermore, the sulfur source may contain a metal element. The metal element is not particularly limited, and may be an alkali metal, an alkaline earth metal, or the like. Examples of the alkali metal include lithium, sodium, potassium, rubidium, cesium, and the like. Examples of the alkaline earth metal include magnesium, calcium, barium, strontium, and the like, and may be magnesium or calcium. The metal element contained in the sulfur source may be one type or two or more types.
[0016] Specifically, the sulfur source may include gypsum. The sulfur source containing gypsum is not particularly limited, and examples thereof include anhydrous gypsum, hemihydrate gypsum, dihydrate gypsum, waste gypsum board, gypsum waste materials such as gypsum molds for casting molding and industrial model gypsum molds. The waste gypsum board may contain paper. When waste gypsum board is used as the sulfur source, a pulverization step of pulverizing the waste gypsum board may be provided before the mixing step. The pulverization step can be performed using a conventional pulverizer.
[0017] Examples of the carbon source include, in addition to carbon, coal, coke, charcoal, and wood, coal ash containing unburned carbon discharged from coal-fired power plants, gasification slag discharged from coal gasification furnaces, pulp sludge discharged from paper mills, waste plastics, waste wood, and biomass waste such as felled trees. When the sulfur source contains a compound containing sulfur having a positive oxidation number, the carbon contained in the carbon source can reduce the sulfur during heating.
[0018] The molar ratio of carbon in the carbon source to sulfur in the sulfur source in the mixed raw materials may be 1.0 or higher, 1.5 or higher, 2.0 or higher, or 2.2 or higher, from the viewpoint of increasing the content of sulfur-containing compounds in the resulting sulfur-containing composition. Furthermore, the molar ratio of carbon in the carbon source to sulfur in the sulfur source in the mixed raw materials may be 10 or lower, 5 or lower, 3 or lower, or 2.5 or lower, from the viewpoint of reducing unreacted carbon and suppressing the generation of oxides due to excessive reaction.
[0019] For example, if the sulfur source contains gypsum (CaSO4), the ratio of the carbon source to the sulfur source can be expressed as [C] / [CaSO4], which is the molar ratio of carbon (C) to CaSO4 contained in the carbon source.
[0020] The mixed raw materials may contain a granulation accelerator (binder) in addition to a sulfur source and a carbon source. The granulation accelerator may be either inorganic or organic. Examples of inorganic granulation accelerators include bentonite. Examples of organic granulation accelerators include molasses, starch, alginic acid, polyvinyl alcohol, carboxymethylcellulose, etc.
[0021] The mixed raw materials may contain ash derived from a carbon source (e.g., SiO2, Al2O3).
[0022] (granulation process) The manufacturing method of this embodiment may include a granulation step for granulating the mixed raw materials obtained in the mixing step. In the granulation step, the mixed raw materials obtained in the mixing step are granulated. The granulation step may be carried out by rolling granulation. The rolling granulation method is not particularly limited, but may be carried out using a pan-type granulator, a drum-type granulator, a vibrating granulator, a high-speed mixer, etc. The size and particle size distribution of the granulated raw materials can be changed and adjusted by appropriately adjusting the granulation conditions according to the granulation method. For example, with a pan-type granulator, water may be sprayed in a mist onto the powdered raw materials placed in the pan, causing the particles to roll along the rotation direction of the granulation container and collide and bond with each other, thereby granulating particles of the required size. For other granulation methods, the granulation size and particle size distribution can be adjusted by appropriately adjusting the amount of water and binder added, the rotation speed of the drum and stirring screw, the motor vibration frequency, etc.
[0023] (Heating process) The heating method is not particularly limited, but may be carried out in a heating furnace. The heating furnace is not particularly limited as long as it can heat to a predetermined temperature, such as an internal combustion burner rotary kiln, an external heating rotary kiln, a double-cylinder rotary kiln type carbonization furnace, a batch type carbonization furnace, etc.
[0024] The heating temperature may be 1200°C or lower, or 1100°C or lower. The oxygen concentration inside the heating furnace may be 20% or lower, 3-20%, or 5-15%. If the raw material is briquette-granulated, the heating temperature may be 1080-1150°C.
[0025] The resulting sulfur-containing composition may be subjected to classification. Classification can be carried out, for example, using a sieve in accordance with JIS Z 8801-1:2019.
[0026] Examples of sulfur-containing compounds included in the sulfur-containing composition obtained by the heating process include compounds containing sulfur with a lower oxidation state than the sulfur contained in the sulfur source of the raw material, such as metal sulfides and metal sulfites (i.e., compounds in which the sulfur has been reduced). Such sulfur-containing compounds containing sulfur with a lower oxidation state can be used as a reducing agent for hexavalent chromium. Examples of metal sulfides include calcium sulfide, calcium polysulfide, and magnesium sulfide. The metal sulfide may be calcium sulfide. Examples of metal sulfites include calcium sulfite and magnesium sulfite.
[0027] In the heating process, for example, if gypsum (CaSO4) is used as the sulfur source, the reaction represented by the following reaction equation (1) proceeds. Simultaneously, the reaction represented by the following reaction equation (2) may also proceed, and SO2 may be generated. CaSO4 + 2C → CaS + 2CO2 (1) CaSO4 + CaS → 2CaO + 2SO2(2)
[0028] In the method of this embodiment, when the sulfur-containing composition contains metal sulfides, the metal sulfides are reduced and produced by reaction with a carbon source, as shown in equation (1) above. The generated metal sulfides then undergo further reactions, as shown in equation (2), producing metal oxides and SO2. Therefore, the SO2 concentration in the kiln exhaust gas serves as an indicator of the degree of metal oxide formation, and the ratio of metal sulfides to metal oxides in the sulfur-containing composition can be adjusted in a timely manner by adjusting the SO2 concentration in the kiln exhaust gas.
[0029] The SO2 concentration in the kiln exhaust gas can be changed by adjusting at least one of the operating conditions: the heating temperature inside the rotary kiln, the oxygen concentration inside the rotary kiln, and the residence time of the raw materials. Generally, the higher any of the reaction temperature, oxygen concentration, or residence time inside the rotary kiln, the greater the amount of metal oxide produced. The SO2 concentration in the kiln exhaust gas can be adjusted by changing one or more of these operating conditions. For example, if the SO2 concentration in the kiln exhaust gas is high, the SO2 concentration can be adjusted by lowering the oxygen concentration inside the rotary kiln.
[0030] The residence time of the raw material in the rotary kiln can be controlled by changing at least one of the following: the kiln rotation speed, the kiln inclination angle, the amount of raw material input, the shape of the raw material, and the size of the raw material. The kiln rotation speed can range from 0.1 to 3 minutes. -1 It is fine to do so within 0.2 to 2.5 minutes. -1 It is fine to have a duration of 0.5 to 2.2 minutes. -1 That's fine.
[0031] Furthermore, the SO2 concentration in the kiln exhaust gas can be changed by adjusting the blending conditions of the raw materials, which include a sulfur source and a carbon source. If the SO2 concentration in the kiln exhaust gas is high, it can be adjusted by reducing the amount of carbon source. Other conditions for preparing the raw materials include the particle size of the carbon source and sulfur source, and whether or not the mixed raw materials are granulated.
[0032] The SO2 concentration in the kiln exhaust gas can be easily determined by conducting trial runs with a predetermined raw material to find appropriate operating conditions.
[0033] Figure 1 plots the product of the SO2 concentration in the kiln exhaust gas (unit: ppm by volume) and the airflow rate through the exhaust duct (i.e., the amount of SO2 emitted per unit time by the kiln exhaust gas) on the horizontal axis, and the percentage of calcium oxide in the sulfur-containing composition (also called the product) on the vertical axis. Note that the airflow rate is the flow rate converted to standard conditions (unit: Nm³). 3 / min, where min is minutes.) Standard conditions can be, for example, 0°C and 1 atmosphere (101325 Pa). The experimental conditions for each point in Figure 1 are shown in Table 1. As raw materials, crushed waste gypsum board (94% dihydrate gypsum content, including paper) was used as the sulfur source and coal gasification coarse slag was used as the carbon source. In Table 1, "5mm rolling granulation" indicates that a roughly spherical granulated raw material with a particle size of 5 mm, obtained by rolling granulation using a high-speed mixer (FS100, manufactured by Earth Technica Co., Ltd.), was used as the raw material. Also, in Table 1, "24mm briquette" and "15mm briquette" refer to flat, almond-shaped raw materials obtained by granulation using a briquette machine (KP-102H, manufactured by Furukawa Sangyo Co., Ltd.), where "24mm" means 10mm × 24mm × 16mm and "15mm" means 7mm × 10mm × 15mm, respectively, as measured with calipers.
[0034] [Table 1]
[0035] Prior to use, at least one of the raw material preparation conditions and operating conditions may be changed for the rotary kiln to be used, as shown in Table 1, to explore preferred conditions. Once preliminary measurements have been taken, the operating conditions can be adjusted while checking the product of the SO2 concentration in the kiln exhaust gas and the airflow rate through the exhaust duct under the predetermined material preparation conditions, thereby adjusting the composition of the sulfur-containing composition to the desired level. For example, if there is a large amount of unreacted sulfur source, the reaction efficiency of the sulfur source can be increased by raising the temperature (heating temperature) inside the kiln or increasing the rotation speed of the kiln, thereby increasing the amount of SO2 emitted from the kiln exhaust gas. When reducing the proportion of oxides to sulfur-containing compounds in the sulfur-containing composition, uneven burning may occur on the workpiece inside the kiln. If the amount of SO2 emitted from the kiln exhaust gas decreases by increasing the rotation speed of the kiln, the proportion of oxides can be reduced. Also, if the reaction amount of the sulfur source is large, it may be considered to increase the tilt angle of the kiln to speed up emission or to lower the reaction temperature inside the kiln in order to reduce the proportion of oxides.
[0036] The content of metal oxides in the sulfur-containing composition may be 0.1 to 30% by mass, or 1 to 15% by mass. Including metal oxides in the sulfur-containing composition within the above range can suppress the generation of H2S derived from metal sulfides during storage. The content of metal sulfides in the sulfur-containing composition may be 10 to 99.9% by mass, or 20 to 99.9% by mass. Since metal sulfides function as reducing agents, having a metal sulfide content within the above range can increase the efficiency of reducing agent production. The molar ratio of metal sulfides to metal oxides in the sulfur-containing composition may be [metal oxide] / [metal sulfide] = 0.01 to 1, or 0.1 to 0.25.
[0037] The total amount of metal sulfides and metal oxides in a sulfur-containing composition converted to the amount (e.g., by mass) of the raw material sulfur source (sulfur source equivalent amount) and the amount of unreacted sulfur source may be 20% or more, 30% or more, 50% or more, or 60% or more. The content of unreacted sulfur source and / or metal oxides in the sulfur-containing composition may be substantially 0%.
[0038] If it is desired to increase the content of metal sulfides, for example, in a sulfur-containing composition, the ratio of metal sulfides to the total amount of unreacted sulfur source metal sulfides and metal oxides (hereinafter also referred to as sulfur source equivalent %) may be 40-95%, 50-92%, or 60-90%. In this case, in a sulfur-containing composition, the sulfur source equivalent % of metal oxides may be 1-30%, 3-25%, or 5-20%. If it is desired to increase the content of metal oxides, for example, in a sulfur-containing composition, the proportion of metal oxides (hereinafter also referred to as sulfur source equivalent %) may be 30-90%, 40-85%, or 50-80%. In this case, in a sulfur-containing composition, the sulfur source equivalent % of metal oxides may be 5-40%, 8-30%, 10-25%, or 10-20%.
[0039] In the heating process, it is preferable that the number of moles of gypsum (CaSO4) supplied to the heating section and the number of moles of the carbon source (C) satisfy the following formula (3), more preferably the following formula (4), and even more preferably the following formula (5). This makes the reaction between gypsum and the carbon source proceed more easily. C / CaSO4≧3 (3) C / CaSO4>4 (4) C / CaSO4>5 (5)
[0040] The sulfur-containing composition may contain components other than sulfur-containing compounds. Such components include calcium oxide, unreacted gypsum, and impurities derived from raw materials such as gypsum. By adding a sulfur-containing composition containing sulfides to the grinding process, which is one of the cement manufacturing processes for producing cement compositions, and grinding it together with cement clinker and gypsum, a cement composition capable of reducing hexavalent chromium leaching can be produced. The sulfur-containing composition may also be added in the grinding process as a dry powder or alkaline slurry.
[0041] The calcium sulfide content of a sulfur-containing composition can be determined by analyzing the diffraction pattern obtained by powder X-ray diffraction measurement using the Rietveld method. The calcium sulfide content of the sulfur-containing composition is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 70% by mass or more. From the viewpoint of ease of manufacture, the calcium sulfide content of the sulfur-containing composition may be 95% by mass or less.
[0042] The manufacturing method of this embodiment may further include a step of contacting kiln exhaust gas with a slurry containing a calcium compound to obtain sulfites. This allows for the capture and effective utilization of SO2 contained in the kiln exhaust gas. When using kiln exhaust gas in this way, a higher SO2 concentration is preferable. The SO2 concentration in the kiln exhaust gas can be adjusted by changing, for example, the temperature inside the kiln (which can be adjusted by the burner opening, the amount of leaked air entering the kiln, etc. The higher the temperature, the more the reaction proceeds and the higher the SO2 concentration), the reactivity of the raw materials (the finer the carbon source, the higher the reactivity and the easier it is for the SO2 concentration to rise; the more carbon in the raw materials, the easier it is for decomposition to proceed and the easier it is for the SO2 concentration to rise), and the residence time of the raw materials inside the kiln (the longer the total length of the kiln, the easier it is for decomposition to proceed and the easier it is for the SO2 concentration to rise. The residence time can also be adjusted by changing the rotation speed, tilt, etc. of the kiln).
[0043] Figure 6 is a schematic diagram showing an example of a firing apparatus for carrying out the manufacturing method of this embodiment. In Figure 6, the firing apparatus 200 has a rotary kiln 20 and a rising duct 14 connected to the kiln end 22 of the rotary kiln 20, and a raw material introduction passage 18 is further connected to the kiln end 22 of the rotary kiln 20. The sulfur source and carbon source may be pre-mixed and supplied to the rotary kiln 20 from the raw material introduction passage 18 as mixed raw materials. The mixed raw materials, as the material to be processed 58, are heated by a burner 24 as they move within the main body 26 of the rotary kiln 20 from the kiln end 22 to the kiln front 28.
[0044] An analytical gas sampling tube 52 is connected to the rising duct 14. During the heating process, the kiln exhaust gas generated can be extracted through the analytical gas sampling tube 52, and the oxygen concentration and SO2 concentration can be analyzed. By extracting the kiln exhaust gas through the analytical gas sampling tube 52, the kiln exhaust gas can be analyzed without being affected by the outside air. The kiln exhaust gas may also be drawn out by a pump or the like, which is separately connected to the analytical gas sampling tube 52.
[0045] From the viewpoint of reducing the unreacted sulfur source, the product of the flow rate of kiln exhaust gas and the concentration of SO₂ in the kiln exhaust gas is 10000 Nm 3 ·min -1 ·ppm or more, and may be 12000 to 60000 Nm 3 ·min -1 ·ppm, and may be 15000 to 50000 Nm 3 ·min -1 ·ppm. The operating conditions of the kiln and the preparation conditions of the raw material such as the composition and particle size of the raw material may be adjusted so that the product of the flow rate of the kiln exhaust gas and the concentration of SO₂ in the kiln exhaust gas falls within the above range. The flow rate of the kiln exhaust gas and the concentration of SO₂ in the kiln exhaust gas may be measured continuously or intermittently. [Examples]
[0046] (Example 1) A raw material obtained by mixing crushed waste gypsum board (dihydrate gypsum content 94%, containing paper) as gypsum and a carbon source (coal gasification coarse slag, manufactured by Ube Industries, Ltd.) at a ratio of [C] / [CaSO₄]=2.4 (molar ratio) was put into a rotary kiln (total length: about 3 m, rotation speed: 0.5 min) at a feeding rate of 50 kg / h -1 ) while changing the temperature inside the kiln, to obtain a sulfur-containing composition (also referred to as a product herein). The mixed raw material was not granulated before firing. The temperature inside the kiln was measured by an infrared radiation thermometer (model number: AD-5616, manufactured by A&D Company, Limited) through a viewing window provided in the rotary kiln to measure the temperature of the raw material and product retained in the kiln. In addition, a part of the exhaust gas immediately after exiting the kiln was collected from the exhaust duct directly above the kiln outlet, and the O₂ concentration and SO₂ concentration (both in volume ppm; the same applies herein unless otherwise specified) were measured using a combustion exhaust gas analyzer (testo 350, manufactured by Testo Co., Ltd.). The flow rate of the kiln exhaust gas was obtained by converting the value measured by a flow meter installed in the exhaust duct to a standard state using the following formula.
[0047] [Formula] In the formula, V and K are the measured values of the flow rate and temperature of the kiln exhaust gas in the exhaust duct, respectively. N The temperature is 0°C (273K). Table 2 summarizes the kiln operating conditions and the airflow rate, O2 concentration, and SO2 concentration of the kiln exhaust gas. Furthermore, chemical composition analysis of the obtained sulfur-containing composition by powder X-ray diffraction revealed that the composition contained unreacted gypsum (CaSO4) and the products calcium sulfide (CaS) and calcium oxide (CaO). The amounts of CaS and CaO produced were converted to the amount of the raw material CaSO4, and the content of these (gypsum equivalent %) relative to the total amount of unreacted CaSO4 and the converted CaS and CaO is shown in Table 2. Figure 2 plots the values obtained by multiplying the airflow rate of the kiln exhaust gas by the SO2 concentration against the CaS and CaO content in the obtained sulfur-containing composition for Example 1. In Figure 2, the kiln temperature is plotted on the horizontal axis, the SO2 concentration in the kiln exhaust gas multiplied by the airflow rate (× in Figure 2), and the CaO (▲ in Figure 2) and CaS (〇 in Figure 2) content (gypsum equivalent %) in the produced product are plotted on the vertical axis.
[0048] [Table 2]
[0049] (Example 2) As gypsum, crushed waste gypsum board (containing 94% dihydrate gypsum, including paper) and a carbon source (coal gasification coarse slag, manufactured by Ube Industries, Ltd.) were mixed in a ratio of [C] / [CaSO4] = 2.4 (molar ratio) to obtain a granulated raw material with a particle size of approximately 5 mm, which was then tumbling-granulated using a high-speed mixer (FS100, manufactured by Earth Technica Co., Ltd.). The obtained granulated raw material was fed into a rotary kiln (total length approximately 3 m, rotation speed 0.5 min) at an input speed of 100 kg / h. -1The kiln temperature was changed during firing. Various measurements were performed in the same manner as in Example 1. Table 3 shows the kiln operating conditions, the composition of the kiln exhaust gas, and the results of the analysis of the chemical composition of the obtained sulfur-containing composition. Figure 3 is a plot of Example 2 showing the value obtained by multiplying the airflow rate of the kiln exhaust gas by the SO2 concentration and the CaS and CaO content in the obtained sulfur-containing composition. In Figure 3, the kiln temperature is plotted on the horizontal axis, the value obtained by multiplying the SO2 concentration in the kiln exhaust gas by the airflow rate (× in Figure 3), and the CaO (▲ in Figure 3) and CaS (〇 in Figure 3) content (gypsum equivalent %) in the produced product are plotted on the vertical axis.
[0050] [Table 3]
[0051] (Example 3) As gypsum, crushed waste gypsum board (containing 94% dihydrate gypsum, including paper) and a carbon source (coal gasification coarse slag, manufactured by Ube Industries, Ltd.) were mixed in a ratio of [C] / [CaSO4] = 2.4 (molar ratio) to obtain a raw material. This mixture was then granulated using a briquette machine (Furukawa Sangyo Co., Ltd. KP-102H) to obtain flat, almond-shaped granulated raw material (measured with calipers: 10mm x 24mm x 16mm). The obtained granulated raw material was fed into a rotary kiln (total length approximately 3m, rotation speeds 0.5, 1, 2 min) at an input speed of 50 kg / h. -1 The mixture was fired at 1090-1100°C. Various measurements were performed in the same manner as in Example 1. Table 4 shows the operating conditions of the kiln, the composition of the kiln exhaust gas, and the results of the analysis of the chemical composition of the obtained sulfur-containing composition. Figure 4 is a plot of Example 3 showing the value obtained by multiplying the airflow rate of the kiln exhaust gas by the SO2 concentration and the CaS and CaO content in the obtained sulfur-containing composition. In Figure 4, the horizontal axis represents the rotation speed of the kiln, and the vertical axis represents the value obtained by multiplying the SO2 concentration in the kiln exhaust gas by the airflow rate (× in Figure 4) and the CaO (▲ in Figure 4) and CaS (〇 in Figure 4) content (gypsum equivalent %) in the produced product.
[0052] [Table 4]
[0053] (Example 4) As gypsum, crushed waste gypsum board (containing 94% dihydrate gypsum, including paper) and a carbon source (coal gasification coarse slag, manufactured by Ube Industries, Ltd.) were mixed in a ratio of [C] / [CaSO4] = 1.5, 2.4, or 4 (molar ratio). This raw material was granulated using a briquette machine (KP-102H, manufactured by Furukawa Sangyo Co., Ltd.) to obtain flat, almond-shaped granulated raw material (measured with calipers: 10mm x 24mm x 16mm). The obtained granulated raw material was fed into a rotary kiln (total length approximately 3m, rotation speed 0.5min) at an input speed of 50kg / h. -1 The mixture was fired at 1070°C. Various measurements were performed in the same manner as in Example 1. Table 5 shows the operating conditions of the kiln, the composition of the kiln exhaust gas, and the results of the analysis of the chemical composition of the obtained sulfur-containing composition. Figure 5 is a plot of Example 4 showing the value obtained by multiplying the airflow rate of the kiln exhaust gas by the SO2 concentration and the CaS and CaO content in the obtained sulfur-containing composition. In Figure 5, [C] / [CaSO4] is plotted on the horizontal axis, and the value obtained by multiplying the SO2 concentration in the kiln exhaust gas by the airflow rate (× in Figure 5) and the CaO (▲ in Figure 5) and CaS (〇 in Figure 5) content (gypsum equivalent %) in the produced product are plotted on the vertical axis.
[0054] [Table 5] [Explanation of Symbols]
[0055] 14...Rising duct (exhaust duct), 18...Raw material introduction path, 20...Rotary kiln, 22...Kiln end, 24...Burner, 26...Main body, 28...Kiln front, 58...Workpiece to be processed, 200...Firing equipment.
Claims
1. The process includes a heating step in which raw materials containing a sulfur source and a carbon source are heated in a rotary kiln. The aforementioned heating step involves the use of SO4 by kiln exhaust gas during the process. 2 Check the emissions of the SO 2 This includes adjusting the preparation conditions of the raw materials or the operating conditions of the rotary kiln in order to control the ratio of metal sulfides to metal oxides in the sulfur-containing composition produced from the raw materials based on the amount of emissions, The aforementioned SO 2 The amount of emissions is SO2 in the kiln exhaust gas. 2 It is the product of the concentration and the airflow rate through the exhaust duct. The adjustment of the aforementioned preparation conditions or operating conditions is performed by confirming the SO 2 It is based on emissions, To reduce the proportion of the metal oxide, at least one of the following adjustments may be made: shortening the residence time of the raw material in the rotary kiln by changing at least one of the kiln rotation speed, kiln tilt angle, raw material input amount, raw material shape, and raw material size; lowering the reaction temperature in the rotary kiln; and lowering the oxygen concentration in the rotary kiln. A method for producing a sulfur-containing composition, comprising adjusting at least one of the following in order to increase the proportion of the metal oxide: changing the kiln rotation speed, kiln inclination angle, amount of raw material input, shape of raw material, and size of raw material to lengthen the residence time of the raw material in the rotary kiln, increasing the reaction temperature in the rotary kiln, and increasing the oxygen concentration in the rotary kiln.
2. A method for producing a sulfur-containing composition according to claim 1, further comprising the step of contacting the kiln exhaust gas with a slurry containing a calcium compound to obtain sulfites.
Citation Information
Patent Citations
Controlling Cement Clinker Production by Analysis of End Product Sulfur Content
JP2001524449A
Process for preparing calcium sulfide-based heavy metal fixing agent
JP2004269822A
Method of producing heavy metal elution suppression material
JP2004337677A
Heavy metal fixation material, manufacturing method for heavy metal fixation material, manufacturing method for ground improving material, and treatment method for soil to be treated
JP2005306911A
Operation managing method and operation managing system for cement manufacturing apparatus
JP2008024559A