Heat storage material composition and method for manufacturing the same
A heat storage material composition with tetradecane and a higher alcohol stabilizes temperature between 2°C and 8°C, prevents supercooling, and avoids hazardous classification, addressing safety and efficiency issues in conventional materials.
Patent Information
- Application Number
- JP2022111980
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-07-12
AI Technical Summary
Conventional heat storage materials using higher hydrocarbons as a main component face issues with safety, temperature retention, and supercooling, making them hazardous and difficult to stabilize at 2°C to 8°C or freeze at 4°C, necessitating costly and time-consuming cooling to -20°C.
A heat storage material composition comprising tetradecane and a higher alcohol with 14 carbon atoms, along with a gelling agent, where the higher alcohol content is 1.0 to 5.0 mol% and the gelling agent is 3.0 to 10.0% by weight, ensuring stable temperature maintenance between 2°C and 8°C and freezing at 4°C without being classified as hazardous.
The composition maintains stable temperature control between 2°C and 8°C, prevents supercooling, and avoids hazardous material classification, reducing storage and transportation restrictions, while allowing for efficient thermal energy absorption and release during phase transitions.
Smart Images

Figure 0007955085000005 
Figure 0007955085000006 
Figure 0007955085000001
Abstract
Description
Technical Field
[0001] The present invention relates to a heat storage material composition and a method for producing the same.
Background Art
[0002] Some items such as pharmaceuticals and foods need to be kept cool or warm within a predetermined temperature range in order to maintain their quality. When transporting such items, a method of keeping the items cool or warm within a predetermined temperature range may become a problem.
[0003] Conventionally, as a method for keeping such items cool or warm, a heat storage material that has been melted or solidified in advance is placed in a heat-insulating transport container, and the latent heat of the heat storage material is used to keep the items stored in the transport container cool or warm. A method is known.
[0004] As such a heat storage material, a heat storage material composition using a higher hydrocarbon as a main component (phase change agent) is known (Patent Documents 1 and 2).
Prior Art Documents
Patent Documents
[0005]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0006] The conventional heat storage material composition containing a higher hydrocarbon as a main component as described above has room for improvement from the viewpoints of safety, temperature retention, and freezable temperature of the heat storage material composition.
[0007] Therefore, one aspect of the present invention aims to provide a heat storage material composition that does not fall under the category of Class 4 hazardous materials under the Fire Service Act of Japan, can stably maintain the temperature of temperature-controlled articles between 2°C and 8°C, and can stably freeze when the temperature is controlled to 4°C. [Means for solving the problem]
[0008] To solve the above problems, one embodiment of the present invention includes the following configuration: [1] A heat storage material composition comprising a main component comprising tetradecane (A) and a higher alcohol having 14 carbon atoms (B1), and a gelling agent (C), wherein the main component contains more than 1.0 mol% of the higher alcohol (B1) in a total amount of 100.0 mol% of the tetradecane (A) and the higher alcohol (B1), and more than 3% by weight of the gelling agent (C) in a total amount of 100% by weight of the heat storage material composition. [2] The heat storage material composition according to [1], wherein the main component contains more than 1.0 mol% and 5.0 mol% or less of the higher alcohol (B) in 100 mol% of the main component. [3] The heat storage material composition according to [1] or [2], wherein the heat storage material composition contains more than 3.0% by weight and 10.0% by weight or less of the gelling agent (C) in 100% by weight of the heat storage material composition. [4] The heat storage material composition according to any one of [1] to [3], wherein the difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is 1.0°C or less, and the crystal nucleation temperature derived from the higher alcohol (B1) is greater than or equal to the supercooling temperature of tetradecane (A) and 8.0°C or less. [5] A heat storage material composition according to any one of [1] to [4], wherein the difference (ΔT) between the melting temperature and the solidification temperature is 1.0℃ or less. [6] The heat storage material composition according to any one of [1] to [5], wherein the higher alcohol (B1) is myristyl alcohol. [7] The heat storage material composition according to any one of [1] to [6], wherein the gelling agent (C) is aluminum 2-ethylhexanoate. [8] A heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B2) having 15 to 18 carbon atoms, and a gelling agent (C), wherein the main component contains 1.0 mol% or more of the higher alcohol (B2) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B2), and the gelling agent (C) in a total amount of 100% by weight of the heat storage material composition. [9] The heat storage material composition according to [8], wherein the main component is present in an amount of 1.0 mol% to 5.0 mol% of the higher alcohol (B2).
[10] The heat storage material composition according to [8] or
[10] , wherein the heat storage material composition contains more than 3.0% by weight and 10.0% by weight or less of the gelling agent (C) in 100% by weight of the heat storage material composition.
[11] The heat storage material composition according to any one of [8] to
[10] , wherein the difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is 1.0°C or less, and the crystal nucleation temperature derived from the higher alcohol (B2) is greater than or equal to the supercooling temperature of tetradecane (A) and 8.0°C or less.
[12] A heat storage material composition according to any one of [8] to
[11] , wherein the difference (ΔT) between the melting temperature and the solidification temperature is 1.0℃ or less.
[13] The higher alcohol (B2) is cetyl alcohol or Octadecanol The heat storage material composition described in any one of [8] to
[12] .
[14] The heat storage material composition according to any one of [8] to
[13] , wherein the gelling agent (C) is aluminum 2-ethylhexanoate. A heat storage material comprising the heat storage material composition described in any one of
[15] [1] to
[14] .
[16] A method for producing a heat storage material composition, comprising: a preparation step of preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B1), and a gelling agent (C); and a filling step of filling a container with the heat storage material composition obtained in the preparation step, wherein the main component contains more than 1.0 mol% of the higher alcohol (B1) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B1), and more than 3.0% by weight of the gelling agent (C) in a total amount of 100% by weight of the heat storage material composition, and the heat storage material composition is maintained at a temperature of 20.0°C or lower in the preparation step and the filling step.
[17] A method for producing a heat storage material composition, comprising: a preparation step of preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B2), and a gelling agent (C); and a filling step of filling a container with the heat storage material composition obtained in the preparation step, wherein the main component contains 1.0 mol% or more of the higher alcohol (B2) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B2), and contains more than 3.0% by weight of the gelling agent (C) in a total amount of 100% by weight of the heat storage material composition, and the heat storage material composition is maintained at a temperature of 20.0°C or lower in the preparation step and the filling step. [Effects of the Invention]
[0009] According to one embodiment of the present invention, it is possible to provide a heat storage material composition that does not fall under the category of Class 4 hazardous materials under the Fire Service Act of Japan, can stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and can stably freeze when the temperature is controlled to 4°C. [Brief explanation of the drawing]
[0010] [Figure 1] The upper figure is a schematic graph showing the temperature change of the heat storage material composition during the phase transition from the molten state to the solidified state (solidification process), and the lower figure is a schematic graph showing the temperature change of the heat storage material composition during the phase transition from the solidified state to the molten state (melting process). [Figure 2] This is a schematic perspective view showing an example of a heat storage material according to one embodiment of the present invention. [Description of Embodiments]
[0011] While one embodiment of the present invention will be described below, the present invention is not limited to such embodiment. That is, the present invention is not limited to each configuration described below, and various modifications are possible within the scope shown in the claims, and embodiments and examples obtained by appropriately combining technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. In addition, all the academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range intends to be "A or more and B or less".
[0012] <1. Technical idea of the present invention> As a heat storage material (5°C type heat storage material) for the purpose of maintaining a temperature of 2 to 8°C, which is widely used for transporting articles requiring strict temperature control such as biopharmaceuticals (temperature-controlled articles), a heat storage material (latent heat storage material) that uses a higher alkane such as tetradecane as a main agent and maintains the temperature by utilizing latent heat accompanying the phase transition of the higher alkane is known.
[0013] Among higher alkanes, tetradecane having a melting temperature of about 5°C is particularly suitable as the main agent of the heat storage material composition used for the 5°C type heat storage material, but tetradecane corresponds to Category 4 hazardous materials under the Fire Service Act of Japan and is basically treated as a hazardous material.
[0014] Hazardous materials corresponding to Category 4 hazardous materials under the Fire Service Act of Japan may be subject to special restrictions in storage, such as requiring storage and management in a hazardous material warehouse, and limiting the storage amount, and may also be subject to special restrictions in transportation, such as requiring labeling and procedures for being a hazardous material when transported by transportation means such as vehicles, aircraft, and ships, and limiting the loading amount.
[0015] Conversely, heat storage material compositions treated as non-hazardous materials under the Fire Service Act have many advantages over those treated as hazardous materials, such as not requiring storage and management in hazardous materials warehouses, not requiring labeling and procedures as hazardous materials during transportation by means of transport such as vehicles, aircraft, and ships, and being subject to relaxed restrictions on the amount that can be carried. Therefore, it is desirable that heat storage material compositions do not fall under the category of hazardous materials of Class 4 under the Fire Service Act of Japan.
[0016] Furthermore, to prevent temperature deviations during the initial stages of temperature retention, the 5°C type heat storage material needs to be adjusted to a temperature range of 2-8°C before packing.
[0017] When using a 5°C type heat storage material in environments where the ambient temperature exceeds 8°C, such as during summer or in warm climates, it is necessary to pack the heat storage material in a frozen state. Conventional heat storage materials are cooled to a very low temperature (e.g., -20°C) to ensure that the heat storage material composition within the material freezes completely, and then the temperature is adjusted to approximately 2°C (2°C temperature control) before packing. The reason why it is necessary to cool the heat storage material to a very low temperature before the 2°C temperature control is that supercooling may occur in the heat storage material composition. If supercooling is present in the heat storage material composition, 2°C temperature control alone will result in unstable freezing of the heat storage material composition, leading to a mixture of frozen and unfrozen products, or even the inability to obtain frozen products at all, making it difficult to stably maintain the temperature of temperature-controlled items.
[0018] However, cooling to extremely low temperatures such as -20°C is time-consuming and costly, and can lead to operational errors. Furthermore, from the perspective of more easily freezing 5°C type heat storage materials, there is a demand for heat storage materials that can stably freeze in higher temperature environments, specifically at 4°C, which is the standard temperature setting for refrigerators used in ordinary households, and in which supercooling is suppressed.
[0019] One method for suppressing supercooling of a heat storage material composition is to add a suitable nucleating agent to the composition. For example, if the main component is a higher alkane, a higher alcohol can function as a nucleating agent. By adding a higher alcohol having a solidification temperature higher than that of the higher alkane as a nucleating agent, when the heat storage material composition solidifies, crystals derived from the nucleating agent that are formed prior to the solidification of the higher alkane act as nuclei, promoting the solidification of the higher alkane and thereby suppressing supercooling.
[0020] On the other hand, when using a 5°C type heat storage material in winter or in cold regions where the ambient temperature is below 2°C, the heat storage material is temperature-controlled to approximately 8°C (8°C temperature control) and packed in a molten state. If crystals of the nucleating agent are formed when the material is temperature-controlled to 8°C, there is a risk that the solidification of the higher alkanes will begin using these crystals as nuclei. In this way, if the solidification of the higher alkanes begins when the material is temperature-controlled to 8°C, it becomes impossible to determine whether the heat storage material composition is frozen or unfrozen at the time of packing, and the latent heat that should be consumed during solidification is consumed before the temperature control of the temperature-controlled item begins, making it difficult to stably maintain the temperature of the temperature-controlled item. In other words, from the viewpoint of stably maintaining the temperature of the temperature-controlled item in the temperature range of 2 to 8°C, it is desirable that the nucleating agent does not form nuclei when temperature-controlled to 8°C, for example, that the nucleating temperature is 8°C or lower.
[0021] In light of the above circumstances, the inventors diligently conducted research with the aim of providing a heat storage material composition that can solve all of the above-mentioned problems at once, that is, a heat storage material composition that does not fall under the category of hazardous materials of Class 4 under the Fire Service Act of Japan, can stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and can stably freeze when the temperature is controlled to 4°C. As a result, they found that a heat storage material composition having the following configuration (heat storage material composition (i) or heat storage material composition (ii)) can provide a heat storage material composition that can solve all of the above-mentioned problems, and thus completed the present invention: A heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol having 14 carbon atoms (B1), and a gelling agent (C), wherein the main component contains more than 1.0 mol% of the higher alcohol (B1) in a total amount of tetradecane (A) and the higher alcohol (B1) of 100 mol%, and more than 3.0 wt% of the gelling agent (C) in a total amount of 100 wt% of the heat storage material composition (heat storage material composition (i)); A heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B2) having 16 to 18 carbon atoms, and a gelling agent (C), wherein the main component contains 1.0 mol% or more of the higher alcohol (B2) in a total amount of tetradecane (A) and the higher alcohol (B2) of 100 mol%, and the gelling agent (C) in a total amount of 3.0% by weight of the heat storage material composition (heat storage material composition (ii)).
[0022] Furthermore, regarding the heat storage material compositions (i) and (ii) according to one embodiment of the present invention, the inventors speculate that the reason for the difference in the required content of higher alcohols in the main component is as follows: The crystal nucleation temperature in a heat storage material composition containing tetradecane and a higher alcohol as a crystal nucleating agent changes in proportion to the melting point and concentration of the higher alcohol used. Basically, the higher the melting point of the higher alcohol and the higher its concentration (amount), the higher the crystal nucleation temperature of the heat storage material composition. The melting point of the higher alcohol also tends to change in proportion to its number of carbon atoms. A higher alcohol with a relatively small number of carbon atoms, 14 carbon atoms (higher alcohol (B1)), has a relatively low melting point, so if its amount is small (1.0 mol% or less), the crystal nucleation temperature of the heat storage material composition drops too low (below the supercooling temperature of tetradecane). On the other hand, higher alcohols with a relatively large number of carbon atoms, such as 15-18 carbon atoms (higher alcohols (B2)), have relatively high melting points, so even a relatively small amount (1.0 mol%) does not cause the crystal nucleation temperature to drop too low (it can maintain a temperature above the supercooling temperature of tetradecane).
[0023] Furthermore, since higher alcohols with fewer than 14 carbon atoms have low melting points, even if their amount (mol%) is increased (for example, to about 5.0 mol%), a sufficient crystal nucleation temperature (above the supercooling temperature of tetradecane) cannot be achieved. Conversely, since higher alcohols with more than 18 carbon atoms have high melting points, even if their amount is considerably reduced (for example, to about 0.5 mol%), the crystal nucleation temperature becomes too high (above 8°C). In addition, higher alcohols with more than 18 carbon atoms may precipitate and settle when stored at room temperature, losing their function as crystal nuclei. For these reasons, higher alcohols with fewer than 14 carbon atoms and higher alcohols with more than 18 carbon atoms (sometimes referred to as other higher alcohols) are not preferable as crystal nucleating agents for the heat storage material composition according to one embodiment of the present invention.
[0024] [2. Heat storage material composition] <<Heat storage material composition (i)>> A heat storage material composition (i) according to one embodiment of the present invention (hereinafter sometimes referred to as "this heat storage material composition (i)") will be described. This heat storage material composition (i) is a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B1) having 14 carbon atoms, and a gelling agent (C), wherein the main component contains more than 1.0 mol% of the higher alcohol (B1) in the total amount of tetradecane (A) and the higher alcohol (B1) in 100 mol%, and more than 3.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition.
[0025] Having the above configuration, this heat storage material composition (i) does not fall under the category of hazardous materials of Class 4 under the Fire Service Act of Japan, and has the advantage of being able to stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and to provide a heat storage material composition that can be stably frozen at 4°C.
[0026] This heat storage material composition can be used as a latent heat storage material by absorbing thermal energy during the phase transition from a solidified state to a molten state (liquid) (in other words, during the melting process). Furthermore, this heat storage material composition can also be used as a latent heat storage material by releasing thermal energy during the phase transition from a molten state (liquid) to a solidified state (solid) (in other words, during the solidification process). Therefore, this heat storage material composition can also be called a "latent heat storage material composition."
[0027] <Main ingredient> This heat storage material composition (i) contains a main component comprising tetradecane (A) and a higher alcohol (B1) having 14 carbon atoms.
[0028] The content of the main component in this heat storage material composition (i) is 90.0% by weight or more and less than 97.0% by weight, preferably 92.0% to 96.5% by weight, and more preferably 94.0% to 96.0% by weight, based on 100% by weight of the heat storage material composition. By having the content of the main component in this heat storage material composition within the above range, this heat storage material composition can fully exhibit temperature retention based on the latent heat effect due to the phase transition of tetradecane contained in the main component.
[0029] (Tetradecan(A)) The main component of this heat storage material composition (i) contains tetradecane (A). Tetradecane (A) can also be called n-tetradecane.
[0030] The main component of this heat storage material composition (i) contains 95.0 mol% or more and less than 99.0 mol% of tetradecane (A) in the total amount of tetradecane (A) and higher alcohol (B1) of 100 mol%, preferably 95.5 mol% to 98.5 mol%, more preferably 96.0 mol% to 98.0 mol%, and even more preferably 96.5 mol% to 97.5 mol%. With the above configuration, it is possible to provide a heat storage material composition that can sufficiently exhibit temperature retention based on the latent heat effect due to the phase transition of tetradecane.
[0031] (Higher alcohol (B1)) The main component of this heat storage material composition (i) contains more than 1.0 mol% of higher alcohol (B1) in the total amount of tetradecane (A) and higher alcohol (B1) (100 mol%). Higher alcohol (B1) is a higher alcohol with 14 carbon atoms. Higher alcohol (B1) is a substance that functions as a crystal nucleating agent when this heat storage material composition is frozen. Therefore, it can also be said that higher alcohol (B1) is a crystal nucleating agent.
[0032] A specific example of a higher alcohol (B1) is myristyl alcohol.
[0033] The main component of the heat storage material composition (i) contains, in a total amount of 100 mol% of tetradecane (A) and higher alcohol (B1), higher alcohol (B1) in amounts of more than 1.0 mol% and 5.0 mol% or less, preferably 1.5 mol% to 4.5 mol%, more preferably 1.0 mol% to 4.0 mol%, and even more preferably 96.5 mol% to 97.5 mol%. With the above configuration, the higher alcohol (B) functions as a crystal nucleus, thereby suppressing supercooling of the heat storage material composition, enabling stable freezing at 4°C, and adjusting the crystal nucleation temperature to a range suitable for stably maintaining the temperature of temperature-controlled articles between 2°C and 8°C, which is above the supercooling temperature of tetradecane (A) and below 8°C.
[0034] <Gelling agent (C)> The heat storage material composition (i) contains more than 3.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition.
[0035] This heat storage material composition contains tetradecane as its main ingredient. Since tetradecane is treated as a hazardous material (Class 4 hazardous material) under the Fire Service Act, there is a risk that the heat storage material composition containing tetradecane may also be treated as a hazardous material.
[0036] On the other hand, this heat storage material composition (i), by containing more than 3.0% by weight of the gelling agent (C), maintains a gel-like state even in a molten state (under conditions above the melting temperature of the heat storage material composition). Therefore, in the 40°C liquidity confirmation test for hazardous materials determination under the Fire Service Act, it is determined to maintain its shape. A heat storage material composition determined to maintain its shape at 40°C by the above test is determined to be "not liquid at 40°C" by the test based on the Class 4 and designated combustible material determination flowchart prescribed by the Fire and Disaster Management Agency of the Ministry of Internal Affairs and Communications. Therefore, this heat storage material composition (i), determined to maintain its shape at 40°C by the above test, does not fall under the category of hazardous materials (Class 4 hazardous materials) under the Fire Service Act of Japan.
[0037] Substances treated as hazardous materials under the Fire Service Act are subject to special restrictions on storage, require labeling and procedures as hazardous materials, and may have restrictions on the amount that can be carried. However, this heat storage material composition is not treated as a hazardous material under the Fire Service Act. Therefore, it does not require storage and management in a hazardous materials warehouse, and offers many advantages such as not requiring labeling and procedures as a hazardous material during transportation by means of transport such as vehicles, aircraft, and ships, and allowing for relaxed restrictions on the amount that can be carried.
[0038] Examples of gelling agents (C) that may be included in this heat storage material composition (i) include aluminum 2-ethylhexanoate, fumed silica, precipitated silica, gel-like silica, higher fatty acids (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, behenic acid, undecylenic acid, oleic acid, linoleic acid, linolenic acid, etc.) or their esters, hydroxypropyl cellulose, hydroxyethyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, polyvinylpyrrolidone, and carboxyvinyl polymer. One of these gelling agents (C) may be used alone, or two or more may be used in combination.
[0039] Among the gelling agents (C) mentioned above, aluminum 2-ethylhexanoate is preferred because it has the advantage of providing a heat storage material composition that maintains its shape at 40°C with only a small amount added. In other words, the heat storage material composition (i) preferably contains aluminum 2-ethylhexanoate as the gelling agent (C), and more preferably contains only aluminum 2-ethylhexanoate as the gelling agent (C).
[0040] The content of the gelling agent (C) in this heat storage material composition (i) is more than 3.0% by weight and 10.0% by weight or less, preferably 3.5% to 8.0% by weight, and more preferably 4.0% to 6.0% by weight, based on 100% by weight of the heat storage material composition. By having a gelling agent (C) content of more than 3.0% by weight in this heat storage material composition (i), it is possible to provide a heat storage material composition that is judged to maintain its shape in the 40°C liquid confirmation test for hazardous materials determination under the Fire Service Act, that is, a heat storage material composition that does not fall under the category of hazardous materials under the Fire Service Act. Furthermore, by having a gelling agent (C) content of 10.0% by weight or less in this heat storage material composition (i), it is possible to increase the proportion of tetradecane in the heat storage material composition, which has the advantage of being able to fully exhibit temperature retention based on the latent heat effect due to the phase transition of tetradecane.
[0041] <Other ingredients> The heat storage material composition (i) may contain components other than the main component and gelling agent (C). Other components include higher alcohols with fewer than 14 carbon atoms, higher alcohols with 15 or more carbon atoms, crystal nucleating agents other than higher alcohols (e.g., sodium tetraborate decahydrate, silicates, or cryolite), phase separation inhibitors (e.g., oleic acid, sodium oleate, potassium oleate, potassium metaphosphate, sodium silicate, or potassium isostearate), fragrances, colorants, antibacterial agents, polymers, surfactants, thermally conductive substances, reaction accelerators, flame retardants, aggregates, buffers, dispersants, crosslinking agents, pH adjusters, preservatives, antifungal agents, antibacterial agents, antialgal agents, wetting agents, defoaming agents, ultraviolet absorbers, antioxidants, light stabilizers, other organic compounds, or other inorganic compounds.
[0042] The content of other components in this heat storage material composition (i) can be appropriately determined by those skilled in the art depending on the desired purpose.
[0043] ≪Heat storage material composition (ii)≫ A heat storage material composition (ii) according to one embodiment of the present invention (hereinafter sometimes referred to as "this heat storage material composition (ii)") will be described below. This heat storage material composition (ii) is a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B2) having 15 to 18 carbon atoms, and a gelling agent (C), wherein the main component contains more than 1.0 mol% of the higher alcohol (B2) in the total amount of tetradecane (A) and the higher alcohol (B2) in 100 mol%, and more than 3.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition.
[0044] Having the above configuration, this heat storage material composition (ii) does not fall under the category of hazardous materials of Class 4 under the Fire Service Act of Japan, and has the advantage of being able to provide a heat storage material composition that can stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and can be stably frozen at 4°C.
[0045] <Main ingredient> This heat storage material composition (ii) contains a main component comprising tetradecane (A) and a higher alcohol (B2) having 15 to 18 carbon atoms.
[0046] The content of the main component in this heat storage material composition (ii) is 90.0% by weight or more and less than 97.0% by weight, preferably 92.0% to 96.0% by weight, and more preferably 94.0% to 96.0% by weight, based on 100% by weight of the heat storage material composition. By having the content of the main component in this heat storage material composition within the above range, this heat storage material composition can fully exhibit temperature retention based on the latent heat effect due to the phase transition of tetradecane contained in the main component.
[0047] (Tetradecan(A)) The main component of this heat storage material composition (ii) contains tetradecane (A). Tetradecane (A) can also be called n-tetradecane.
[0048] The main component of the heat storage material composition (ii) contains 95.0 mol% to 99.0 mol% of tetradecane (A) out of a total amount of 100 mol% of tetradecane (A) and higher alcohol (B2), preferably 95.5 mol% to 98.5 mol%, more preferably 96.0 mol% to 98.0 mol%, and even more preferably 96.5 mol% to 97.5 mol%. With the above configuration, it is possible to provide a heat storage material composition that can sufficiently exhibit temperature retention based on the latent heat effect due to the phase transition of tetradecane.
[0049] (Higher alcohol (B2)) The main component of this heat storage material composition (ii) contains more than 1.0 mol% of higher alcohol (B2) in the total amount of tetradecane (A) and higher alcohol (B2) per 100 mol%. Higher alcohol (B2) is a higher alcohol having 15 to 18 carbon atoms. Higher alcohol (B2) is a substance that functions as a crystal nucleating agent when this heat storage material composition is frozen. Therefore, it can also be said that higher alcohol (B2) is a crystal nucleating agent.
[0050] Examples of higher alcohols (B2) include pentadecanol (15 carbon atoms), cetyl alcohol (16 carbon atoms), and heptadecanol (17 carbon atoms). Octadecanol Examples include (18 carbon atoms). These may be used individually or in combination of two or more. Among these, higher alcohols (B2) are suitable because they have a moderate melting point difference with tetradecane, making it easy to adjust the crystal nucleation temperature of the heat storage material composition to within 8°C, and suppressing crystal precipitation and sedimentation when the heat storage material composition is stored at room temperature. These include cetyl alcohol and / or Octadecanol Preferably contains cetyl alcohol and / or Octadecanol It is more preferable to include only that.
[0051] The main component of the heat storage material composition (ii) contains 1.0 mol% or more of higher alcohol (B2) in the total amount of tetradecane (A) and higher alcohol (B2) of 100 mol%, preferably 1.0 mol% to 5.0 mol%, more preferably 1.5 mol% to 4.5 mol%, even more preferably 1.0 mol% to 4.0 mol%, and even more preferably 96.5 mol% to 97.5 mol%. With the above configuration, the higher alcohol (B2) functions as a crystal nucleus, thereby suppressing supercooling of the heat storage material composition, enabling stable freezing at 4°C, and adjusting the crystal nucleation temperature to a range suitable for stably maintaining the temperature of temperature-controlled articles between 2°C and 8°C, which is above the supercooling temperature of tetradecane (A) and below 8°C.
[0052] <Gelling agent (C)> The heat storage material composition (ii) contains more than 3.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition. The description of the gelling agent (C) in the section on "Heat Storage Material Composition (i)" above shall be appropriately referenced. That is, the embodiment of the gelling agent (C) in the heat storage material composition (ii), including preferred embodiments and the reasons therefor, is the same as that of the gelling agent (C) in the heat storage material composition (i).
[0053] <Other ingredients> The heat storage material composition (ii) may contain components other than the main component and the gelling agent (C). Examples of other components include crystal nucleating agents other than higher alcohols (e.g., sodium tetraborate decahydrate, silicates, or cryolite), gelling aids, fragrances, colorants, antibacterial agents, polymers, surfactants, thermal conductive substances, reaction accelerators, flame retardants, aggregates, buffers, dispersants, crosslinking agents, pH adjusters, preservatives, antifungal agents, antibacterial agents, antialgal agents, wetting agents, defoaming agents, ultraviolet absorbers, antioxidants, light stabilizers, other organic compounds, or other inorganic compounds.
[0054] Examples of gelling aids include fatty acids, fatty acid metal salts, fatty acid esters and other fatty acid compounds; and higher alcohols. These gelling aids can also be called gelling support agents.
[0055] The above fatty acid compound is not particularly limited, and may, for example, be a fatty acid compound that is solid at room temperature (e.g., 25°C), but it is preferable that it be a fatty acid compound that is liquid at room temperature.
[0056] The fatty acids in the above fatty acid compounds may be saturated fatty acids or unsaturated fatty acids. The lower limit of the number of carbon atoms constituting the fatty acid compound is not limited and may be, for example, 4, 5, 6, 7, or 8. The upper limit of the number of carbon atoms constituting the fatty acid compound is not limited and may be, for example, 30, 28, 26, 24, or 22.
[0057] Specific examples of the above fatty acids include, for example, caprylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, and behenic acid, as well as mixtures of these fatty acids.
[0058] Specific examples of metal salts of the above fatty acids include, for example, sodium caprylate, sodium laurate, sodium myristate, sodium palmitate, sodium stearate, sodium oleate, and sodium behenate, as well as mixtures of these metal salts.
[0059] A specific example of the above-mentioned fatty acid esters is, for instance, sorbitan fatty acid esters.
[0060] Specific examples of the above sorbitan fatty acid esters include, for example, sorbitan monocaprylate, sorbitan monolaurate, sorbitan monomyristate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan monobehenate, sorbitan dicaprylate, sorbitan dilaurate, sorbitan dimyristate, sorbitan dipalmitate, sorbitan distearate, sorbitan dioleate, and sorbitan dioleate. Examples include rubitane dibehenate, sorbitan tricaprylate, sorbitan trilaurate, sorbitan trimyristate, sorbitan tripalmitate, sorbitan tristearate, sorbitan trioleate, sorbitan tribehenate, sorbitan sesquicaprylate, sorbitan sesquilaurate, sorbitan sesquimyristate, sorbitan sesquipalmitate, sorbitan sesquistearate, sorbitan sesquioleate, sorbitan sesquibehenate, etc.
[0061] Furthermore, as long as it has an ester bond consisting of sorbitan and a fatty acid, sorbitan fatty acid esters may also have other structures, such as the structure of polyoxyethylene (also called poly(oxyethylene, POE)) (structural formula: -[OCH2CH2]n- (where n is any natural number)). Sorbitan fatty acid esters having the structure of polyoxyethylene are sometimes called POE sorbitan fatty acid esters or POE(X) sorbitan fatty acid esters. The above X represents the number of repeating units of oxyethylene and represents the value of n in the above structural formula.
[0062] Specific examples of POE sorbitan fatty acid esters include, for example, POE(20) sorbitan monolaurate, POE(6) sorbitan monolaurate, POE(20) sorbitan monopalmitate, POE(20) sorbitan monostearate, POE(6) sorbitan monostearate, POE(20) sorbitan tristearate, POE(20) sorbitan monooleate, POE(6) sorbitan monooleate, POE(20) sorbitan trioleate, POE(160) sorbitan triisostearate, and POE(20) sorbitan monolaurate.
[0063] Among the exemplified compounds, the sorbitan fatty acid ester is preferably a sorbitan monofatty acid ester in which one fatty acid is ester-bonded to sorbitan, and / or a sorbitan sesquifatty acid ester in which three fatty acids are bonded to two molecules of sorbitan. It is more preferably at least one selected from the group consisting of sorbitan monooleate, sorbitan monolaurate, sorbitan sesquioleate, and sorbitan monostearate, and even more preferably at least one selected from the group consisting of sorbitan monooleate and sorbitan sesquioleate. This configuration makes it easy to control the solidification start temperature of the resulting heat storage material composition to 2°C to 8°C. As a result, it has the advantage of providing a heat storage material composition that can more stably and accurately maintain the temperature of a temperature-controlled article within the range of 2°C to 8°C and at a desired controlled temperature.
[0064] As mentioned above, higher alcohols can also be used as gelling aids. The higher alcohols (B1) or (B2) described above can be used as gelling aids. Specific examples of these higher alcohols (B1) or (B2) are shown in the section on higher alcohols (B1) or (B2) above.
[0065] Furthermore, the higher alcohol used as a gelling aid is intended to be a different component from the higher alcohol component in the main component. Specifically, in this heat storage material composition (i), for example, higher alcohol (B2) is used as a gelling aid, and higher alcohol (B1) is not used. Also, in this heat storage material composition (ii), for example, higher alcohol (B1) is used as a gelling aid, and higher alcohol (B2) is not used.
[0066] As a gelling aid, either the fatty acid compound or the higher alcohol described above may be used alone, or a combination of the fatty acid compound and the higher alcohol may be used. Furthermore, either one type of fatty acid compound or higher alcohol may be used alone, or two or more types may be used in combination.
[0067] In this heat storage material composition, the amount of gelling aid is preferably 1 / 2 to 1 / 3 the amount of gelling agent when the gelling aid is a fatty acid compound. When the gelling aid is a higher alcohol, the amount of gelling aid in this heat storage material composition is preferably 1 to 6 times the amount of gelling agent. With this configuration, not only can the gelation of the heat storage material composition be delayed for a long time, but the heat storage material composition can also be sufficiently gelled in the container.
[0068] As described above, the preferred content of the gelling aid in this heat storage material composition varies depending on the type of gelling aid used and the content of the gelling agent, but for example, 0.1% to 30.0% by weight is preferred in 100% by weight of the heat storage material composition. When the gelling aid is a fatty acid compound, the preferred content of the gelling aid in the heat storage material composition is 0.2% to 5.0% by weight, more preferably 0.3% to 4.0% by weight, and particularly preferably 0.4% to 3.0% by weight. Furthermore, when the gelling aid is a higher alcohol, the preferred content of the gelling aid in the heat storage material composition is 1.0% to 30.0% by weight, more preferably 3.0% to 30.0% by weight, and particularly preferably 5.0% to 25.0% by weight.
[0069] The content of components other than the gelling aid in the heat storage material compositions (i) and (ii) can be appropriately determined by those skilled in the art depending on the desired purpose.
[0070] ≪Physical Properties of Heat Storage Material Compositions≫ The physical properties of this heat storage material composition will be described below. In this specification, when the term "this heat storage material composition" is used without specifying whether it is this heat storage material composition (i) or this heat storage material composition (ii), both of these are intended.
[0071] (Melting temperature) The melting temperature of this heat storage material composition is preferably 2.0°C to 8.0°C, more preferably 3.0°C to 7.0°C, even more preferably 3.5°C to 6.5°C, even more preferably 4.0°C to 6.0°C, and particularly preferably 4.5°C to 5.5°C. The fact that the melting temperature of this heat storage material composition is within the above range means that the heat storage material composition undergoes a phase transition from a solidified state to a molten state within the above temperature range and exhibits a latent heat effect, that is, it can maintain the temperature of the temperature-controlled article within the above temperature range.
[0072] In this specification, the "melting temperature" of a heat storage material composition broadly refers to "the temperature exhibited by a solid heat storage material composition from the time it begins to melt until it liquefies," and is the value measured by the method described in the examples. The term "liquefaction" also includes the "gelation" described above.
[0073] (solidification temperature) The solidification temperature of this heat storage material composition is preferably 2.0°C to 8.0°C, more preferably 3.0°C to 7.0°C, even more preferably 3.5°C to 6.5°C, even more preferably 4.0°C to 6.0°C, and particularly preferably 4.5°C to 5.5°C. The fact that the solidification temperature of this heat storage material composition is within the above range means that the heat storage material composition undergoes a phase transition from a molten state to a solidified state within the above temperature range and exhibits a latent heat effect, that is, it can maintain the temperature of the temperature-controlled article within the above temperature range.
[0074] In this specification, the "solidification temperature" of a heat storage material composition broadly refers to "the temperature exhibited by the liquid heat storage material composition while it solidifies," and is a value measured by the method described in the examples.
[0075] (The difference between the supercooling temperature and the solidification initiation temperature) The difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is preferably 1.0°C or less, more preferably 0.8°C or less, even more preferably 0.6°C or less, and even more preferably 0.5°C or less. A difference between the supercooling temperature and the solidification start temperature of the heat storage material composition being within the above range means that the heat storage material composition is one in which supercooling is suppressed, resulting in small variations in the degree of freezing among individual heat storage material compositions when the temperature is controlled (e.g., 4°C controlled), and that the heat storage material composition can freeze stably. On the other hand, a difference between the supercooling temperature and the solidification start temperature of the heat storage material composition exceeding 1.0°C means that significant supercooling occurs in the heat storage material composition, resulting in large variations in the degree of freezing among individual heat storage material compositions when the temperature is controlled (e.g., 4°C controlled), and that the heat storage material composition cannot freeze stably. Furthermore, a difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is particularly preferably 0°C. A difference of 0°C between the supercooling temperature and the solidification start temperature of a heat storage material composition means that the heat storage material composition is one in which supercooling does not occur, and that there is no variation in the degree of freezing among individual heat storage material compositions when the temperature is controlled (for example, controlled to 4°C), and that the heat storage material composition can freeze stably below the solidification start temperature (for example, in an environment of 4°C).
[0076] In this specification, the difference between the supercooling temperature and the solidification onset temperature of the heat storage material composition is the value obtained by subtracting the supercooling temperature from the solidification onset temperature of the heat storage material composition. The supercooling temperature and the solidification onset temperature of the heat storage material composition are values measured by the method described in the examples.
[0077] (crystal nucleation temperature) The nucleation temperature of this heat storage material composition is preferably above the supercooling temperature of tetradecane (A) and below 8.0°C. The fact that the nucleation temperature of this heat storage material composition is within the above range means that (1) the nucleating agent generates nuclei before the solidification of tetradecane and promotes the solidification of tetradecane, thereby suppressing the supercooling of the heat storage material composition, and (2) when the temperature is controlled to 8°C, it does not generate nuclei and there is no risk of promoting unintended solidification of the heat storage material composition when the temperature is controlled to 8°C.
[0078] In this specification, the "crystal nucleation temperature" of the heat storage material composition refers to the temperature at which crystal nuclei derived from the crystal nucleating agent, which is a higher alcohol (higher alcohol (B1) or higher alcohol (B2)), are formed, and is a value measured by the method described in the examples.
[0079] From the viewpoint of providing a heat storage material composition that can stably maintain the temperature of temperature-controlled articles at 2°C to 8°C and stably freeze when the temperature is controlled at 4°C, it is preferable that the difference between the supercooling temperature and the solidification start temperature of this heat storage material composition is 1.0°C or less, and that the crystal nucleation temperature derived from the higher alcohol (higher alcohol (B1) or higher alcohol (B2)) is above the supercooling temperature of tetradecane (A) and 8°C or less.
[0080] (The difference between the melting temperature and the solidification temperature) The difference between the melting temperature and solidification temperature of the heat storage material composition is preferably greater than -1.0°C and 1.0°C or less, more preferably between -0.8°C and 0.8°C, and even more preferably between -0.6°C and 0.6°C. Since this simplifies the temperature setting for temperature control (melting and solidification) and storage of the heat storage material composition, and enables more precise temperature control of temperature-controlled articles, the smaller the absolute value of the difference between the melting temperature and solidification temperature of the heat storage material composition, the more preferable it is, and particularly preferably 0°C. In other words, it is preferable that the melting temperature and solidification temperature of the heat storage material composition are the same. In this specification, the difference between the melting temperature and solidification temperature of the heat storage material composition may be referred to as "ΔT".
[0081] In this specification, the difference between the melting temperature and the solidification temperature of the heat storage material composition is the value obtained by subtracting the solidification temperature from the melting temperature of the heat storage material composition. The melting temperature and solidification temperature of the heat storage material composition are the values measured by the method described in the examples above.
[0082] (Whether or not freezing occurred after 48 hours in a 4°C constant temperature bath) Preferably, this heat storage material composition is one in which the molten state of the heat storage material composition freezes after being left to stand in a 4°C constant temperature bath for 48 hours.
[0083] A heat storage material composition that can be stably frozen when kept at a temperature of 4°C can be frozen in a commercially available refrigerator, making it suitable for consumer use (patient carrying applications).
[0084] [3. Heat storage material] One embodiment of the present invention also provides a heat storage material comprising the heat storage material composition described above. The heat storage material according to one embodiment of the present invention only needs to be comprising the heat storage material composition described above, and is not limited to other components, materials, etc. The heat storage material according to one embodiment of the present invention can also be said to be a heat storage material that includes the heat storage material composition as a phase change agent.
[0085] A heat storage material according to one embodiment of the present invention can be used as a latent heat type heat storage material by absorbing thermal energy during the phase transition of the heat storage material composition forming the heat storage material from a solidified state to a molten state (liquid) (in other words, during melting). Therefore, a heat storage material according to one embodiment of the present invention can also be called a "molten latent heat storage material". Furthermore, a heat storage material according to one embodiment of the present invention can also be used as a latent heat type heat storage material by releasing thermal energy during the phase transition of the heat storage material composition forming the heat storage material from a molten state (liquid) to a solidified state (solid) (in other words, during solidification). Therefore, a heat storage material according to one embodiment of the present invention can also be called a "solidified latent heat storage material". A heat storage material according to one embodiment of the present invention can also be called a "latent heat storage material".
[0086] In this specification, the melting temperature of a heat storage material refers to the temperature exhibited by the heat storage material during the transition from a solidified state to a molten state (liquid) in its main phase state. In this specification, the "solidification temperature" of a heat storage material refers to the temperature exhibited by the heat storage material during the transition from a molten state to a solidified state (liquid) in its main phase state. Here, "phase state of the main part of the heat storage material" refers to the phase state of the main component of the heat storage material composition that forms the heat storage material. If 80% by weight of the heat storage material composition that forms the heat storage material is solid and 20% by weight is liquid, the phase state of this heat storage material is considered to be solid (solidified). Here, "phase state" refers to a general state of solid, liquid, gel, or gas. In this invention, mainly solid and liquid, or solid and gel phase states are utilized.
[0087] A heat storage material according to one embodiment of the present invention may be a heat storage material composition described above that is filled into a container or bag or the like.
[0088] The container or bag used in one embodiment of the present invention is not particularly limited in its other configuration, as long as it is capable of containing the heat storage material composition. The container or bag may be a flexible, soft container or a rigid, non-flexible container. Preferably, the container or bag is made of a material that is impermeable to the heat storage material composition and has a melting point higher than the melting point of the heat storage material composition. Furthermore, when the liquid (or gel-like) heat storage material composition solidifies into a solid, a force (internal pressure) may be applied inside the container or bag due to volume expansion caused by solidification. Also, when the heat storage material is applied to a living environment for the purpose of maintaining a comfortable temperature in the living space, the heat storage material may be used as a building material. In this case, the container or bag forming the heat storage material may be subjected to external impact. Therefore, it is preferable that the container or bag has excellent mechanical strength, such as tear strength and rupture strength.
[0089] Examples of materials that make up the above-mentioned container or bag include metal and resin (for example, synthetic resin).
[0090] Examples of metals include copper, aluminum, iron, brass, zinc, magnesium, and nickel.
[0091] Examples of resins include polypropylene resin, polyvinyl chloride resin, polycarbonate resin, nylon resin, polyethylene resin, and polyethylene terephthalate resin (PET resin), polystyrene resin, and polyester resin.
[0092] The above-mentioned container or bag may be made of a material consisting of one type of component, or it may be made of a material consisting of a combination of two or more components in order to enhance heat resistance, strength, and barrier properties.
[0093] Materials composed of two or more of the above-mentioned components include, for example, multilayer materials. Examples of multilayer structures include (a) a multilayer structure in which a layer of metal such as aluminum foil is laminated on a layer of thermoplastic resin, and (b) a structural layer sheet material formed by inserting a layer of metal such as aluminum foil between multiple layers of thermoplastic resin.
[0094] When using a multilayered material as the material for the above-mentioned container or bag, the innermost layer, i.e., the layer in contact with the heat storage material composition, is preferably a layer formed from resin because it has excellent corrosion resistance to the heat storage material composition.
[0095] The above-mentioned containers or bags are not particularly limited, but include olefin materials such as Midea from Tatsuno Chemical Co., Ltd. and Emmasoft from Okamoto Co., Ltd., PVC materials such as the Tarpaulin series from Kanbo Plus Co., Ltd., and aluminum laminate films from Keihan Cellophane Co., Ltd., MA Packaging Co., Ltd., and Showa Denko Packaging Co., Ltd., etc. Among these, multilayer laminate films with high barrier properties are particularly preferred because the contents are less likely to bleed (smear). Examples include aluminum laminate films from Keihan Cellophane Co., Ltd., MA Packaging Co., Ltd., and Showa Denko Packaging Co., Ltd.
[0096] The shape of the above-mentioned container or bag is not particularly limited, but from the viewpoint of efficiently exchanging heat between the heat storage material composition and the temperature-controlled article or the surrounding space via the container or bag, a shape that is thin and has a large surface area is preferred. A heat storage material can be formed by filling these containers or bags with the heat storage material composition.
[0097] An example of a heat storage material according to one embodiment of the present invention is shown in Figure 2. Figure 2 is a schematic perspective view showing a heat storage material 201 according to one embodiment of the present invention. As shown in Figure 2, the heat storage material 201 according to one embodiment of the present invention consists of a container 10 having an opening, a cap 11, and a heat storage material composition 20 that is filled inside the container 10 through the opening. In the heat storage material 201, the opening of the container 10 is completely sealed by the cap 11.
[0098] For more specific examples of the above-mentioned containers or bags, the containers or bags disclosed in Japanese Patent Publication No. 2015-78307 may be used. This document is incorporated herein by reference.
[0099] The melting temperature and solidification temperature of the heat storage material according to one embodiment of the present invention can be considered to be the same as the melting temperature and solidification temperature of the heat storage material composition contained in the heat storage material. The melting temperature and / or solidification temperature of the heat storage material according to one embodiment of the present invention is preferably around 2.0°C to 8.0°C.
[0100] The heat storage material according to one embodiment of the present invention does not fall under the category of hazardous materials (Class 4) under Japan's Fire Service Act, can stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and can stably freeze when the temperature is controlled to 4°C. Therefore, it can be suitably used for applications such as the transportation of items requiring strict temperature control (temperature-controlled items), such as biopharmaceuticals.
[0101] [4. Heat storage material composition and method for manufacturing the heat storage material] A method for manufacturing a heat storage material comprising a heat storage material composition according to one embodiment of the present invention (hereinafter sometimes referred to as the "method for manufacturing the heat storage material") is not particularly limited, but for example, a heat storage material comprising the heat storage material composition (i) can be manufactured by the following method: a preparation step of preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B1), and a gelling agent (C); and a filling step of filling a container with the heat storage material composition obtained in the preparation step, wherein the main component contains more than 1.0 mol% of the higher alcohol (B1) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B1), and more than 3.0 wt% of the gelling agent (C) in a total amount of 100 wt% of the heat storage material composition, and the heat storage material composition is maintained at a temperature of 20.0°C or lower in the preparation step and the filling step.
[0102] Furthermore, when manufacturing a heat storage material comprising the heat storage material composition (ii), the following method can be applied: a preparation step of preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol (B2), and a gelling agent (C); and a filling step of filling a container with the heat storage material composition obtained in the preparation step, wherein the main component contains 1.0 mol% or more of the higher alcohol (B2) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B2), and contains more than 3.0 wt% of the gelling agent (C) in a total amount of 100 wt% of the heat storage material composition, and the heat storage material composition is maintained at a temperature of 20.0°C or lower in the preparation step and the filling step.
[0103] Regarding the manufacturing method of this heat storage material, the descriptions in sections [2. Heat Storage Material Composition] and [3. Heat Storage Material] may be applied as appropriate, except for matters described in detail below.
[0104] This heat storage material composition contains a predetermined amount of gelling agent (C) and therefore has gel-like properties. However, immediately after manufacturing (immediately after adding the gelling agent (C) to the heat storage material composition in the adjustment process), gelation has not yet progressed, and it has liquid properties. In the subsequent filling process, when filling the heat storage material composition into a container, it is preferable that the heat storage material composition be in liquid form from the viewpoint of workability, filling efficiency, and preventing the gelled heat storage material composition from remaining in the filling equipment. In other words, it is preferable to perform the filling process before the gelation of the heat storage material composition progresses.
[0105] In particular, when manufacturing heat storage materials on a large scale industrially, it is necessary to prepare a large amount of heat storage material composition at once and then fill this large amount of heat storage material composition into multiple containers individually (in multiple steps) or into a large container all at once. In either case, the filling process takes a long time (for example, about 3 hours). Therefore, in order to prepare heat storage material compositions efficiently and on a large scale, it is necessary to maintain the properties of the heat storage material composition in a liquid state during such a long filling process, and to do so, it is necessary to suppress the progression of gelation of the heat storage material composition.
[0106] In this method for manufacturing the heat storage material, the time required for the heat storage material composition to gel can be extended by maintaining the heat storage material composition at a temperature of 20.0°C or lower during the preparation and filling processes. For example, in this manufacturing method, the heat storage material composition can remain liquid for 3.0 hours or more immediately after production. Therefore, in this manufacturing method, a sufficiently long working time can be secured between the preparation and filling of the prepared heat storage material composition into containers. Furthermore, in one embodiment, any additional process can be performed between the preparation and filling processes.
[0107] In the preparation step for the manufacturing method of this heat storage material, (1) a heat storage material composition may be prepared by stirring tetradecane (A), a higher alcohol (B1) or (B2), a gelling agent (C), and optionally other components (e.g., a gelling aid) during mixing; (2) the above components may be blended to prepare a heat storage material composition, and then the heat storage material composition may be stirred; or (3) both of the stirring methods described in (1) and (2) above may be performed. Alternatively, tetradecane (A), a higher alcohol (B1) or (B2), a gelling agent (C), and optionally other components may be mixed together, or a main component may be prepared by first mixing tetradecane (A) and a higher alcohol (B1) or (B2), and then the gelling agent (C) and optionally other components may be mixed separately into the obtained main component. The method of stirring the heat storage material composition is not limited, and for example, it may be stirred using a known stirrer such as a static mixer.
[0108] In each of the stirring processes described in (1) to (3) above, (i) stirring may be performed for a desired time by repeating a cycle consisting of stirring and non-stirring treatments a desired number of times, or (ii) stirring may be performed for a desired time by performing only the stirring treatment.
[0109] In the preparation and filling steps of the manufacturing method for this heat storage material, the heat storage material composition is maintained (controlled) at a temperature of 20.0°C or lower. The temperature at which the heat storage material composition is maintained in the preparation and filling steps is not particularly limited as long as it is 20.0°C or lower, and may be 19.0°C or lower, or 18.0°C or lower. Furthermore, the lower limit of this temperature is not particularly limited, but from the viewpoint of suppressing the crystallization of higher alcohols (B1) and (B2) during the manufacturing process, it is preferable that it be 15.0°C or higher. By maintaining the heat storage material composition at the above temperature, the time required for the gelation of the heat storage material composition can be extended for a longer period.
[0110] In this heat storage material manufacturing method, it is sufficient to maintain the "heat storage material composition" at 20.0°C or below during the preparation and filling processes; it is not necessary to maintain other substances at 20.0°C or below. For example, when preparing the main component by mixing tetradecane (A) and a higher alcohol (B1) or (B2) prior to adding the gelling agent (C), the temperature at which the main component is prepared, in other words, the temperature at which tetradecane (A) and the higher alcohol (B1) or (B2) are mixed, does not need to be controlled to 20.0°C or below; the mixing may be performed at a temperature above 20.0°C. In this manufacturing method, if tetradecane (A) and the higher alcohol (B1) or (B2) are mixed at a temperature above 20.0°C, it is sufficient to control the temperature to 20.0°C or below from the point at which the gelling agent (C) is added to the mixture to prepare the heat storage material composition. For example, after mixing tetradecane (A) with a higher alcohol (B1) or (B2) at a temperature above 20.0°C, the mixture can be adjusted to 20.0°C or below before adding a gelling agent (C) to the resulting mixture.
[0111] In the method for manufacturing this heat storage material, the method for maintaining the heat storage material composition at the above-mentioned temperature is not particularly limited. For example, the preparation process may be carried out in a tank set to the above-mentioned temperature range by a cooling device.
[0112] The method for manufacturing the heat storage material may include a gelling step in addition to the preparation step and the filling step. The gelling step is a step to complete the gelling of a heat storage material composition that is not gelled or has not yet completed gelling. The form of the gelling step is not particularly limited as long as it can complete the gelling of the heat storage material composition, but for example, a method of maintaining the heat storage material composition at a temperature above 20.0°C for a certain period of time may be used.
[0113] The temperature at which the heat storage material composition is maintained during the gelation process is not particularly limited as long as it is above 20.0°C, but from the viewpoint of ensuring stable and rapid gelation of the heat storage material composition, it is preferable that the temperature be 30.0°C or higher, and more preferably 40.0°C or higher.
[0114] Furthermore, while there is no particular limit to the time for maintaining the heat storage material composition at the above temperature during the gelation process, it is preferable to maintain it for 4 hours or more, and more preferably for 6 hours or more, from the viewpoint of ensuring that the gelation of the heat storage material composition is completed reliably.
[0115] In the gelation step of the manufacturing method for this heat storage material, the method for maintaining the heat storage material composition at the above-mentioned temperature is not particularly limited. For example, the gelation step may be carried out in a tank set to the above-mentioned temperature range by a heating device.
[0116] In another embodiment of the present invention, a method for producing the heat storage material can also be applied that has a two-liquid preparation step, in which agent A, which contains tetradecane (A), a higher alcohol (B2), and optionally other components (e.g., a gelling aid), and agent B, which contains tetradecane (A) and a gelling agent (C), are prepared separately. A method for producing a heat storage material that has a two-liquid preparation step, in which the heat storage material composition is prepared in two types, agent A and agent B, is sometimes referred to as a two-liquid filling method. A two-liquid filling method is preferred as a method for producing the heat storage material composition because it reduces the workload.
[0117] When applying a method having a two-liquid preparation step as a method for manufacturing this heat storage material, (I) in the subsequent filling step, the prepared A and B agents may be sequentially filled into a container, and then the A and B agents may be mixed in the container to prepare the heat storage material composition within the container; or (II) the prepared A and B agents may be mixed immediately before filling into the container in the subsequent filling step (after preparing the heat storage material composition) and then filled into the container. In (II) above, the method of mixing the heat storage material composition is not limited, and for example, it may be mixed using a static mixer or the like.
[0118] Accordingly, in another embodiment of the present invention, the following method may also be applied as a method for producing a heat storage material comprising the heat storage material composition (i): a two-liquid preparation step of preparing agent A comprising tetradecane (A), a higher alcohol (B1), and optionally other components (e.g., a gelling aid), and agent B comprising tetradecane (A) and a gelling agent (C); and a two-liquid filling step of filling a container with agent A and agent B obtained in the two-liquid preparation step, wherein in the two-liquid filling step, (I) agent A and agent B are sequentially filled into a container and then mixed in the container, or (II) agent A and agent B are mixed immediately before filling into the container and then filled into the container.
[0119] Furthermore, in another embodiment of the present invention, the following method may be applied as a method for producing a heat storage material comprising the heat storage material composition (ii): a two-liquid preparation step of preparing agent A comprising tetradecane (A), a higher alcohol (B2), and optionally other components (e.g., a gelling aid), and agent B comprising tetradecane (A) and a gelling agent (C); and a two-liquid filling step of filling a container with agent A and agent B obtained in the two-liquid preparation step, wherein in the two-liquid filling step, (I) agent A and agent B are sequentially filled into a container and then mixed in the container, or (II) agent A and agent B are mixed immediately before filling into the container and then filled into the container.
[0120] Even when applying a two-liquid filling method as the manufacturing method for this heat storage material, it is preferable to maintain (control) the heat storage material composition at a temperature of 20.0°C or lower during the two-liquid preparation step and the two-liquid filling step, for the same reasons as those for the preparation step and the filling step described above. Furthermore, even when applying a two-liquid filling method, the manufacturing method for this heat storage material may include a gelation step. The specific embodiments related to temperature maintenance and the gelation step are as described above.
[0121] The present invention is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. [Examples]
[0122] The raw materials used in the examples and comparative examples were as follows:
[0123] [Tetradecan (A)] Tetradecane (manufactured by ISU, product name: N-PAR14, C 14 (Molecular weight: 198.34, melting point: 5.1℃) [Higher alcohol (B)] (Higher alcohol (B1)) Myristyl alcohol (manufactured by Kao Corporation, product name: Calcol 4098, C 14 -OH (14 carbon atoms), molecular weight: 214.39, melting point: 37.2℃) (Higher alcohol (B2)) Cetyl alcohol (manufactured by Kao Corporation, product name: Calcol 6098, C) 16 -OH (16 carbon atoms), molecular weight: 242.44, melting point: 48.3°C) Octadecanol (Manufactured by Fujifilm Wako Co., Ltd., C 18 -OH (18 carbon atoms), molecular weight: 270.49, melting point: 57.3℃) [Gelling agent (C)] Aluminum 2-ethylhexanoate (manufactured by Hope Pharmaceutical Co., Ltd., product name: Octop Aluminum A) [Other higher alcohols] Lauryl alcohol (manufactured by Kao Corporation, product name: Calcol 2098, C 12 -OH (12 carbon atoms), molecular weight: 186.34, melting point: 23.4℃) Tridecyl alcohol (manufactured by Fujifilm Wako Co., Ltd., C 13 -OH (13 carbon atoms), molecular weight: 200.36, melting point: 31.1℃) Eicosyl alcohol (manufactured by Fujifilm Wako Co., Ltd., C 20 -OH (20 carbon atoms), molecular weight: 298.55, melting point: 63.7°C) Furthermore, lauryl alcohol, tridecyl alcohol, and eicosyl alcohol used as other higher alcohols have 12, 13, or 20 carbon atoms, respectively, and do not satisfy the requirements of either a higher alcohol (B1) with 14 carbon atoms or a higher alcohol (B2) with 15 to 18 carbon atoms. Therefore, they are not considered "higher alcohol (B)" according to one embodiment of the present invention.
[0124] The measurements and evaluations in the examples and comparative examples were performed under the following conditions and methods.
[0125] [Shape retention test at 40°C] For each heat storage material composition, the following tests were conducted to determine whether or not it maintained its shape at 40°C (in other words, whether or not it was fluid): (1) A flat-bottomed cylindrical transparent glass tube with an inner diameter of 30 mm and a height of 120 mm was filled with a heat storage material composition (sample) to a height of 55 mm from the bottom. A marking was made on the glass tube at 85 mm from the bottom. (2) The glass tube was left upright in a constant temperature water bath adjusted to 40°C for 10 minutes; (3) After standing for 10 minutes, the glass tube was removed from the constant temperature water bath and tilted horizontally; (4) The glass tube was tilted horizontally, and the time taken until the sample inside the glass tube exceeded the 85 mm mark was measured. (5) Based on the measurement results, the following criteria were used to determine whether the heat storage material composition retained its shape at 40°C (in other words, whether it was fluid): ○ (Pass): It takes 90 seconds or more for the sample to exceed the mark. A ○ in the shape retention test means that the heat storage material composition maintains its shape (does not have fluidity) at 40°C. × (Fail): The sample exceeds the mark within 90 seconds. An evaluation of × in the shape retention test means that the heat storage material composition does not retain its shape (is fluid) at 40°C.
[0126] Furthermore, a heat storage material composition that is judged to "maintain its shape at 40°C" (a ○ rating) in the above shape retention test will be judged to "not be liquid at 40°C" in a test based on the Class 4 and designated combustible material judgment flowchart prescribed by the Fire and Disaster Management Agency of the Ministry of Internal Affairs and Communications. Therefore, a heat storage material composition that is judged to "maintain its shape at 40°C" in the above shape retention test will be judged to "be liquid at 40°C" in a test based on the Class 4 and designated combustible material judgment flowchart prescribed by the Fire and Disaster Management Agency of the Ministry of Internal Affairs and Communications, and will be judged to be a Class 4 combustible material under the Fire and Disaster Management Agency of Japan.
[0127] [Evaluation of the coagulation process] A heat storage material composition at 40°C was filled into a polypropylene cryovial and left to stand for 1 hour in a constant temperature bath [Cryoporter® CS-80CP, ultra-low temperature aluminum block constant temperature bath manufactured by Cynics Co., Ltd.] which was conditioned to 50°C. After that, the temperature inside the constant temperature bath was lowered at a rate of 1.0°C / min within a temperature range of 50°C to -25°C.
[0128] In the above temperature decrease process, a graph was created plotting the temperature of the heat storage material composition in the constant temperature bath against time (elapsed time from the start of temperature decrease). Figure 1 is a schematic graph showing the temperature change of the heat storage material composition in the above temperature decrease process. In the temperature decrease process, while the temperature of the constant temperature bath decreased at a constant rate, the temperature of the heat storage material composition changed in the following order (1) to (5), as shown in Figure 1 (solid line): (1) The temperature of the heat storage material composition decreased at a constant or approximately constant rate from 50°C to a certain temperature (let's call it temperature T1); (2) With temperature T1 as the boundary, the temperature of the heat storage material composition rose, rising from temperature T1 to a certain temperature (let's call it temperature T2); (3) At this point, the temperature of the heat storage material composition decreased again as the temperature dropped, falling at a constant or nearly constant rate from temperature T2 to a certain temperature (let's call it temperature T4); (4) From temperature T4 to a certain temperature (let's call it temperature T5), the temperature of the heat storage material composition remained almost unchanged due to latent heat, despite the temperature of the constant temperature bath being lowered; (5) At temperature T5, the temperature of the heat storage material composition decreased again, falling at a constant or nearly constant rate to -25°C.
[0129] As another example, the temperature of the heat storage material composition changed in the following order (1') to (4'), as shown in Figure 1 (dashed line): (1') The temperature of the heat storage material composition decreased at a constant or near-constant rate from 50°C to a certain temperature (let's call it temperature T3); (2') With temperature T3 as the boundary, the temperature of the heat storage material composition increased, rising from temperature T3 to a certain temperature (let's call it temperature T4); (3') From temperature T4 to a certain temperature (let's call it temperature T5), the temperature of the heat storage material composition hardly changed due to latent heat, despite the temperature of the constant temperature bath decreasing; (4') With temperature T5 as the boundary, the temperature of the heat storage material composition decreased again, falling at a constant or near-constant rate to -25°C.
[0130] In this specification, temperature T2 is referred to as the "crystal nucleation temperature," temperature T3 as the "supercooling temperature," temperature T4 as the "solidification start temperature," and temperature T5 as the "solidification end temperature." Furthermore, temperature T6, which is the midpoint between temperatures T4 and T5, is defined as the "solidification temperature" of the heat storage material composition. In evaluating the solidification process of the heat storage material composition, the solidification temperature (T6), supercooling temperature (T3), solidification start temperature (T4), and crystal nucleation temperature (T2) of the heat storage material composition were measured based on the temperature change graph obtained by the above method during temperature decrease of the heat storage material composition. Note that if the supercooling temperature (T3) is not clearly observed, as shown in the solid line graph of Figure 1, the supercooling temperature (T3) and the solidification start temperature (T4) are considered to be the same, and the solidification start temperature (T4) is adopted as the supercooling temperature (T3). Furthermore, if the nucleation temperature (T2) cannot be clearly identified as shown in the dashed graph of Figure 1, (i) if the supercooling temperature (T3) of the heat storage material composition under evaluation is higher than the supercooling temperature of tetradecane alone (4.3°C in this specification), the supercooling temperature (T3) of the heat storage material composition under evaluation will be adopted as the nucleation temperature (T2) of the heat storage material composition under evaluation. (i) if the supercooling temperature (T3) of the heat storage material composition under evaluation is lower than the supercooling temperature of tetradecane alone (4.3°C in this specification), "less than the supercooling temperature of tetradecane (×)" will be adopted as the nucleation temperature (T2). In addition, although not shown in the figures, there may be cases in the temperature decrease process of the heat storage material composition where a constant temperature is maintained (a region corresponding to (4) or (3') above) does not exist. In this case, since it is difficult to determine the temperature T5, the temperature T4 will be defined as the "solidification temperature".
[0131] The crystal nucleation temperature (T2) measured from the solidification process evaluation results was used for evaluation according to the following criteria: ○ (Good): Above the supercooling temperature of tetradecane and below 8°C. △ (Too high): Above 8℃. × (Too low): Below the supercooling temperature of tetradecane.
[0132] [Evaluation of the melting process] In a constant temperature bath [Cryoporter® CS-80CP, ultra-low temperature aluminum block constant temperature bath manufactured by Cynics Co., Ltd.], the temperature of a heat storage material composition filled in a polypropylene cryovial, also heated to -25°C, was increased within a temperature range of -25°C to 50°C at a heating rate of 1.0°C / minute.
[0133] In the above temperature rise process, a graph was created plotting the temperature of the heat storage material composition in the constant temperature bath against time (elapsed time from the start of the temperature rise). Figure 2 is a schematic graph showing the above graph illustrating the temperature change of the heat storage material composition in the above temperature rise process. In the temperature rise process, while the temperature of the constant temperature bath rose at a constant rate, the temperature of the heat storage material composition changed in the following order (1) to (5), as shown in Figure 1 (solid and dashed lines): (1) The temperature of the heat storage material composition rose at a constant or approximately constant rate from -25°C to a certain temperature (let's call it temperature T7); (2) At temperature T7, the temperature of the heat storage material composition hardly changed due to latent heat, despite the rising temperature of the constant temperature bath; (3) At temperature T8, the temperature of the heat storage material composition rose again and then fell at a constant or approximately constant rate down to 50°C.
[0134] In this specification, the temperature T7 is referred to as the "melting start temperature," and the temperature T8 is referred to as the "melting end temperature." Furthermore, the temperature T9, which is the midpoint between temperatures T7 and T8, is defined as the "melting temperature" of the heat storage material composition. In evaluating the solidification process of the heat storage material composition, the melting temperature (T9) was measured based on the temperature change graph obtained by the above method during the temperature rise of the heat storage material composition.
[0135] [The difference between the supercooling temperature and the solidification initiation temperature] Using the value obtained by subtracting the supercooling temperature (T3) from the solidification start temperature (T4) of the heat storage material composition obtained from the solidification process evaluation results, the "difference between the supercooling temperature and the solidification start temperature" of the heat storage material composition was evaluated based on the following criteria. ○ (Good): The difference between the supercooling temperature and the solidification start temperature is 1°C or less. △ (Poor): The difference between the supercooling temperature and the solidification start temperature exceeds 1°C.
[0136] [Difference between melting temperature and solidification temperature] Based on the results of the solidification process evaluation and the melting process evaluation, the difference between the melting temperature and solidification temperature of the heat storage material composition was evaluated using the value obtained by subtracting the melting temperature (T9) from the solidification temperature (T6) of the heat storage material composition, according to the following criteria. ○ (Good): The difference between the solidification temperature and the melting temperature is 1°C or less. × (Poor): The difference between the solidification temperature and the melting temperature exceeds 1°C.
[0137] [Whether or not freezing occurred in a 4°C constant temperature bath] A heat storage material composition (heat storage material) sealed in a PVC container was placed in a constant temperature bath (CH43-15P, manufactured by Nagano Science) set to 4.0°C and left to stand for 48 hours. After standing, the container containing the heat storage material composition was removed from the constant temperature bath and its appearance was checked. Based on the appearance of the heat storage material composition inside the container, a determination of "freezing in a 4°C constant temperature bath" was made based on the following criteria. ◎(Good): The entire heat storage material composition is uniformly frozen. ○ (Pass): Although there are variations in color intensity in the heat storage material composition in some areas, the entire heat storage material composition is frozen (unevenly frozen). △ (Fail): Part of the heat storage material composition is frozen, but there are unfrozen portions. × (Defective): The entire heat storage material composition is not frozen.
[0138] [Crystal precipitation after melting / solidification evaluation] After repeating the solidification process evaluation and melting process evaluation three times, the heat storage material composition filled in the cryovial, i.e., the heat storage material composition heated to 50°C, was subjected to a cooling operation from 50°C to -25°C and a heating operation from -25°C to 50°C, repeated three times. The heat storage material composition filled in the cryovial was then left to stand in a constant temperature bath heated to 23°C for at least one hour. After that, the cryovial was removed from the constant temperature bath, and the appearance of the heat storage material composition filled in the cryovial was checked. Based on the appearance of the checked heat storage material composition, a determination of "crystal precipitation after melting / solidification evaluation" was made based on the following criteria. ○ (Pass): The heat storage material composition is a transparent liquid, and no crystal precipitation is observed inside the cryovial. △(Note): The heat storage material composition is cloudy, but no crystal precipitation is observed inside the cryovial. × (Defective): Crystal precipitation is observed inside the cryovial.
[0139] [Examples 1-7] (Preparation of heat storage material composition (i)) Tetradecane (Tetradecane (A)) heated to 40°C was mixed with myristyl alcohol (B1), which had been heated to 50°C and dissolved, in the proportions shown in Table 1. This liquid mixture was mixed and stirred for 30 minutes while cooling to a liquid temperature of 18°C. After confirming that the liquid temperature of the above mixture was 18°C, aluminum 2-ethylhexanoate was added as a gelling agent (C) in the proportions shown in Table 1, and the mixture was stirred at 18°C for 10 minutes to obtain a heat storage material composition (preparation step). The obtained heat storage material composition was heated in a 40°C constant temperature bath (CH43-15P, manufactured by Nagano Science) for 6 hours (gelling step) to complete the gelling of the heat storage material composition and obtain a gelled heat storage material composition.
[0140] (Preparation of a heat storage material comprising a heat storage material composition (i)) 1000g of the heat storage material composition obtained in the above process, immediately after manufacturing (immediately after adding the gelling agent (C) and stirring at 18°C for 10 minutes), was filled into a 1L capacity PVC container using a liquid transfer pump (Hyoshin Equipment Co., Ltd. NHL-15FN). Furthermore, the cap and container were integrated and sealed by heat fusion, thereby obtaining a heat storage material (equipped with) the heat storage material composition (heat storage material composition (i) of Examples 1 to 7) inside the container (filling process). In the above preparation and filling processes, gelation of the heat storage material composition did not proceed, and it was confirmed that gelation was completed by heating in a constant temperature bath (Nagano Science Co., Ltd. CH43-15P) set to 40°C for 6 hours.
[0141] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 1.
[0142] [Reference example 1] Tetradecane (Tetradecane (A)) heated to 40°C was mixed with myristyl alcohol (B1), which had been heated to 50°C and dissolved, in the proportions shown in Table 1. This liquid mixture was mixed and stirred for 30 minutes while being heated to maintain a liquid temperature of 40°C. After stirring, aluminum 2-ethylhexanoate was added as a gelling agent (C) in the proportions shown in Table 1, and the mixture was mixed and stirred while being heated to maintain a liquid temperature of 40°C to obtain a heat storage material composition (preparation step). 1000g of this heat storage material composition was filled into a 1L capacity PVC container using a liquid transfer pump (Hyoshin Equipment Co., Ltd. NHL-15FN) while maintaining the liquid temperature at 40°C. Furthermore, the cap and container were integrated and sealed by heat fusion to produce a heat storage material filled into a container (filling step). However, approximately one hour after the start of the filling process, the heat storage material composition began to gel, making liquid transport difficult, and the filling operation was stopped.
[0143] [Examples 8-10] (Preparation of heat storage material composition (ii)) Tetradecane (Tetradecane (A)) heated to 40°C was mixed with cetyl alcohol (powdered) at room temperature as a higher alcohol (B2) in the proportions shown in Table 1. This liquid mixture was mixed and stirred for 30 minutes while cooling to a liquid temperature of 18°C. Then, aluminum 2-ethylhexanoate was added as a gelling agent (C) in the proportions shown in Table 1, and after stirring at 18°C for 10 minutes, the mixture was heated in a 40°C constant temperature bath (CH43-15P, manufactured by Nagano Science) for 6 hours to obtain a heat storage material composition.
[0144] (Preparation of a heat storage material comprising heat storage material composition (ii)) 1000g of the heat storage material composition obtained in the above process was immediately filled into a 1L PVC container (immediately after adding the gelling agent (C) and stirring at 18°C for 10 minutes). The cap and container were then integrated and sealed by heat fusion to obtain a heat storage material (equipped with) the heat storage material composition (heat storage material composition (ii) of Examples 8-10) inside the container.
[0145] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 1.
[0146] [Table 1]
[0147] [Comparative Examples 1-6] Myristyl alcohol, dissolved at 50°C, or cetyl alcohol (powdered) at room temperature was mixed with tetradecane heated to 40°C in the proportions shown in Table 2. This liquid mixture was mixed and stirred for 30 minutes while cooling to a liquid temperature of 18°C. Then, aluminum 2-ethylhexanoate was added in the proportions shown in Table 2, and the mixture was stirred at 18°C for 10 minutes to obtain a heat storage material composition.
[0148] 1000g of the heat storage material composition obtained in the above process was immediately filled into a 1L PVC container using the same procedure as in Example 1, immediately after production (immediately after adding aluminum 2-ethylhexanoate and stirring at 18°C for 10 minutes), to obtain a heat storage material containing the heat storage material compositions of Comparative Examples 1 to 6.
[0149] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 2.
[0150] [Table 2]
[0151] [Reference example 2] A heat storage material composition consisting solely of tetradecane, and a heat storage material obtained by filling a 1L PVC container with 1000g of tetradecane were obtained.
[0152] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 3.
[0153] [Reference examples 3 to 15] In tetradecane heated to 40°C, tridecyl alcohol, myristyl alcohol, lauryl alcohol (liquid) at room temperature, or cetyl alcohol (powder) at room temperature, all heated / dissolved at 50°C, were mixed in the proportions shown in Table 3, and the mixture was stirred at 50°C for 10 minutes to obtain the heat storage material compositions of Reference Examples 3 to 15.
[0154] Furthermore, 1000g of the obtained heat storage material composition was filled into a 1L capacity PVC container to obtain a heat storage material that is filled with (or contains) the heat storage material compositions of Reference Examples 3 to 15.
[0155] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 3.
[0156] [Table 3]
[0157] [Reference examples 16-21] In tetradecane heated to 40°C, room temperature Octadecanol The heat storage material compositions of Reference Examples 16 to 21 were obtained by mixing (in powder form) or eicosyl alcohol (in pellet form) in the proportions shown in Table 3 and stirring at 60°C for 60 minutes.
[0158] Furthermore, 1000g of the obtained heat storage material composition was filled into a 1L capacity PVC container to obtain a heat storage material that is filled with (or equipped with) the heat storage material compositions of Reference Examples 16 to 21.
[0159] The obtained heat storage material compositions and heat storage materials were subjected to measurement and evaluation of their physical properties. The results are shown in Table 4.
[0160] [Table 4]
[0161] As is clear from Tables 1-4, the heat storage material compositions of Examples 1-10 (heat storage material composition (i) and heat storage material composition (ii)) (1) passed the shape retention test at 40°C, meaning they do not fall under the category of Class 4 hazardous materials under the Fire Service Act of Japan; (2) the difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is less than 1.0°C, indicating that supercooling is suppressed, and the crystal nucleation temperature derived from the higher alcohol (B1) or (B2) is within the range of above the supercooling temperature of tetradecane (A) and below 8°C, meaning that the temperature of temperature-controlled items can be stably maintained between 2°C and 8°C; and (3) the entire heat storage material composition is frozen after being left standing in a 4°C constant temperature bath for 48 hours, indicating that it can be stably frozen at a 4°C temperature.
[0162] These results indicate that the present heat storage material composition (either the present heat storage material composition (i) or the present heat storage material composition (ii)) does not fall under the category of Class 4 hazardous materials under the Fire Service Act of Japan, can stably maintain the temperature of temperature-controlled items between 2°C and 8°C, and can stably freeze at a temperature of 4°C.
[0163] On the other hand, the results from Comparative Examples 1-3 and the Reference Examples show that if the heat storage material composition does not contain a gelling agent, or if the gelling agent content is 3% by weight or less, the heat storage material composition will not gel, or the gelling will be insufficient, and it will not be able to maintain its shape at 40°C, resulting in a heat storage material composition that falls under Class 4 of hazardous materials under Japan's Fire Service Act.
[0164] From the results of Comparative Examples 4 and 5, it can be seen that when the content of higher alcohol (B1) in the main component of the heat storage material composition (i) is 1.0 mol% or less, the crystal nucleation temperature drops below the supercooling temperature of tetradecane, and the crystal nuclei derived from the higher alcohol (B1) are unable to suppress the supercooling of the cold storage material composition. From this, it can be seen that when the content of higher alcohol (B1) in the heat storage material composition (i) is 1.0 mol% or less, it becomes difficult to stably freeze the heat storage material composition at a temperature of 2°C.
[0165] From the results of Comparative Example 6, when the content of higher alcohol (B2) in the main component of the heat storage material composition (ii) is less than 1.0 mol%, the crystal nucleation temperature drops below the supercooling temperature of tetradecane, and the crystal nuclei derived from the higher alcohol (B2) are unable to suppress the supercooling of the cold storage material composition. From this, it can be seen that when the content of higher alcohol (B2) in the heat storage material composition (ii) is less than 1.0 mol%, it becomes difficult to stably freeze the heat storage material composition at a temperature of 2°C. [Industrial applicability]
[0166] The heat storage material composition according to one embodiment of the present invention can be suitably used as a heat storage material, particularly as a heat storage material (5°C type heat storage material) for maintaining a temperature of 2 to 8°C.
Claims
1. The main component contains tetradecane (A) and a higher alcohol with 14 carbon atoms (B1), A heat storage material composition comprising a gelling agent (C), The main component contains, in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B1), the higher alcohol (B1) in an amount greater than 1.0 mol% and less than or equal to 5.0 mol%, A heat storage material composition comprising more than 3.0% and 10.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition.
2. The heat storage material composition according to claim 1, wherein the difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is 1.0°C or less, and the crystal nucleation temperature derived from the higher alcohol (B1) is above the supercooling temperature of tetradecane (A) and 8.0°C or less.
3. The heat storage material composition according to claim 1, wherein the difference (ΔT) between the melting temperature and the solidification temperature is 1.0°C or less.
4. The heat storage material composition according to claim 1, wherein the higher alcohol (B1) is myristyl alcohol.
5. The heat storage material composition according to claim 1, wherein the gelling agent (C) is aluminum 2-ethylhexanoate.
6. The main component contains tetradecane (A) and a higher alcohol (B2) having 15 to 18 carbon atoms, A heat storage material composition comprising a gelling agent (C), The main component contains 1.0 mol% to 5.0 mol% of the higher alcohol (B2) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B2). A heat storage material composition comprising more than 3.0% and 10.0% by weight of the gelling agent (C) in 100% by weight of the heat storage material composition.
7. The heat storage material composition according to claim 6, wherein the difference between the supercooling temperature and the solidification start temperature of the heat storage material composition is 1.0°C or less, and the crystal nucleation temperature derived from the higher alcohol (B2) is above the supercooling temperature of tetradecane (A) and 8.0°C or less.
8. The heat storage material composition according to claim 6, wherein the difference (ΔT) between the melting temperature and the solidification temperature is 1.0°C or less.
9. The heat storage material composition according to claim 6, wherein the higher alcohol (B2) is cetyl alcohol or octadecanol.
10. The heat storage material composition according to claim 6, wherein the gelling agent (C) is aluminum 2-ethylhexanoate.
11. A heat storage material comprising the heat storage material composition according to any one of claims 1 to 10.
12. A preparation step for preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol having 14 carbon atoms (B1), and a gelling agent (C), The process includes a filling step in which the heat storage material composition obtained in the preparation step is filled into a container, The main component contains, in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B1), higher alcohol (B1) in an amount greater than 1.0 mol% and less than or equal to 5.0 mol%. The heat storage material composition contains more than 3.0% by weight and 10.0% by weight or less of the gelling agent (C) in 100% by weight, A method for manufacturing a heat storage material, wherein in the preparation step and the filling step, the heat storage material composition is maintained at a temperature of 20.0°C or lower.
13. A preparation step for preparing a heat storage material composition comprising a main component containing tetradecane (A) and a higher alcohol having 15 to 18 carbon atoms (B2), and a gelling agent (C), The process includes a filling step in which the heat storage material composition obtained in the preparation step is filled into a container, The main component contains 1.0 mol% to 5.0 mol% of the higher alcohol (B2) in a total amount of 100 mol% of the tetradecane (A) and the higher alcohol (B2). The heat storage material composition contains more than 3.0% by weight and 10.0% by weight or less of the gelling agent (C) in 100% by weight, A method for manufacturing a heat storage material, wherein in the preparation step and the filling step, the heat storage material composition is maintained at a temperature of 20.0°C or lower.
Citation Information
Patent Citations
Microcapsule for heat accumulating material
JP1993237368A
Thermal storage medium and its dispersion
JP1997031451A
Heat storage material composition
JP2009120734A
Heat storage material composition and heat storage material using the same
JP2018154796A
Method for producing heat storage material
JP2021123638A