Electrophotographic image forming apparatus

By integrating a cage-type silsesquioxane structure into the molecular chain of an acrylic resin surface layer, the electrophotographic belt prevents crystallization, reducing noise and ensuring stable, high-quality image formation in image forming apparatuses.

JP7955101B2Active Publication Date: 2026-11-24CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022134522
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-25
Publication Date
2026-11-24
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

Existing electrophotographic belts in image forming apparatuses suffer from abnormal noise during cleaning due to phase separation and crystallization of cage silsesquioxane structures, leading to instability and reduced durability.

Method used

Incorporating a cage-type silsesquioxane structure into the molecular chain of an acrylic resin surface layer, ensuring no crystallization peaks are observed, thereby preventing phase separation and enhancing hardness and durability.

Benefits of technology

The solution reduces abnormal noise and ensures stable, high-quality image formation over an extended period by preventing crystallization of the cage-type silsesquioxane structure, maintaining consistent friction and reducing noise from cleaning blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955101000004
    Figure 0007955101000004
  • Figure 0007955101000005
    Figure 0007955101000005
  • Figure 0007955101000006
    Figure 0007955101000006
Patent Text Reader

Abstract

To provide an electrophotographic belt which is less likely to cause noise from a cleaning blade and allows good electrophotographic images to be formed over a prolonged period.SOLUTION: An electrophotographic belt disclosed herein comprises a base layer and a surface layer containing an acrylic resin having a cage silsesquioxane structure in a molecule, where no crystallization peak caused by the cage silsesquioxane structure is observed in X-ray diffraction measurement of a surface of the surface layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to electrophotographic image forming apparatus such as photocopiers and printers. [Background technology]

[0002] In electrophotographic image forming apparatuses, a tandem method is widely used to obtain a full-color image by superimposing toner images of each color of YMCK on an intermediate transfer belt and then transferring them to paper in one go. Semiconductive belts are generally used as intermediate transfer belts, and typical examples include belts formed by dispersing carbon black in resins such as polyimide and polyetheretherketone. In this context, electrophotographic apparatuses that require high speed and high durability are seeking further improvements in the transfer characteristics of the intermediate transfer belt. One such effort is to reduce the surface free energy of the outer periphery, i.e., the surface layer. Patent Document 1 discloses an intermediate transfer member having a surface layer containing polyimide to which polyfaceted silsesquioxane is bonded. Patent Document 2 discloses an intermediate transfer body having an elastic layer on the surface of an elastic layer, in which a plurality of protrusions are uniformly distributed on the surface of spherical matrix particles, and the surface irregularities are formed by silicone fine particles in which the matrix particles and the protrusions are polymethylsilsesquioxane. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2011-034083 [Patent Document 2] Japanese Patent Publication No. 2014-215470 [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] However, according to the inventors' research, the electrophotographic belt described in Patent Document 1 sometimes produced abnormal noises from the cleaning blade after prolonged use. Furthermore, the intermediate transfer material described in Patent Document 2 had insufficient surface hardness and was not yet sufficiently durable. One aspect of this disclosure aims to provide an electrophotographic belt that is less prone to generating abnormal noise from the cleaning blade and contributes to the stable formation of high-quality electrophotographic images over a long period of time. Furthermore, other aspects of this disclosure are aimed at providing an electrophotographic image forming apparatus capable of stably forming high-quality electrophotographic images. [Means for solving the problem]

[0005] According to one aspect of this disclosure, The device comprises an image carrier for holding a toner image, an intermediate transfer belt for carrying and transporting the toner image, which has been primarily transferred from the image carrier, to a transfer material for secondary transfer, and a cleaning blade for removing residual toner from the surface of the intermediate transfer belt. The intermediate transfer belt is An electrophotographic belt having a base layer and a surface layer, The surface layer comprises an acrylic resin and a compound containing a cage-type silsesquioxane structure. A key feature is that, in X-ray diffraction measurements of the surface layer, no crystallization peaks attributable to the cage-type silsesquioxane structure are observed. Electrophotographic image forming apparatus It will be provided. [Effects of the Invention]

[0006] According to one aspect of this disclosure, abnormal noise is less likely to occur from the cleaning blade, and good electrophotographic images can be formed over a long period of time. Electrophotographic image forming apparatus You can obtain this. [Brief explanation of the drawing]

[0007] [Figure 1] This is a schematic cross-sectional view of the image forming apparatus relating to this disclosure. [Figure 2] This is a schematic cross-sectional view of the intermediate transfer belt related to this disclosure. [Figure 3] This is a three-dimensional diagram of the cage-type silsesquioxane structure of Si8O12. [Figure 4]FIG. 1 is a three-dimensional view of a cage silsesquioxane structure of Si₁₀O₁₅. [Figure 5] FIG. 2 is a structural formula of a compound having a cage silsesquioxane structure as a raw material used in Examples and Comparative Examples. [Figure 6] FIG. 3 is an XRD spectrum of a surface layer according to Example 1. [Description of Embodiments]

[0008] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the drawings. However, dimensions, materials, shapes, relative arrangements, and the like of components described in the following embodiments should be appropriately changed depending on configurations of devices to which the present disclosure is applied and various conditions, and the scope of the present disclosure is not intended to be limited only thereto. In the present specification, descriptions of “XX or more and YY or less” and “XX to YY” representing numerical ranges mean numerical ranges including lower and upper limits that are endpoints, unless otherwise specified. In addition, when numerical ranges are described stepwise, any combination of upper and lower limits of each numerical range is disclosed.

[0009] The present inventors presume the reason why the intermediate transfer member disclosed in Patent Document 1 generates abnormal noise during surface cleaning by a cleaning blade as follows. Specifically, in the polyimide disclosed in Patent Document 1, a cage silsesquioxane structure is bonded to the terminal of a molecular chain or a side chain portion. For this reason, the cage silsesquioxane structure is considered to be in a relatively movable state. Since cage silsesquioxane has high stereoregularity, cage silsesquioxanes easily aggregate with each other to form a crystalline state. Therefore, in the intermediate transfer member disclosed in Patent Document 1, the cage silsesquioxanes bonded to the polyimide aggregate and crystallize, causing phase separation between the main chain portion of the polyimide and the cage silsesquioxane structure. That is, on the surface of the intermediate transfer member, there are regions where the cage silsesquioxane structure contributing to reduction in surface energy is present sparsely and densely, and the coefficient of friction is considered to locally vary. As a result, when the surface of the intermediate transfer member is cleaned with a cleaning blade, a stick-slip phenomenon occurs, and this is considered to cause abnormal noise.

[0010] Thus, the present inventors have considered that, in order to reduce surface free energy by introducing a cage silsesquioxane structure and prevent generation of abnormal noise during cleaning, it is effective to prevent generation of a crystalline state due to aggregation between cage silsesquioxane structures. As a result of further studies based on such consideration, the present inventors have arrived at the electrophotographic belt according to the present disclosure, which has high hardness and hardly generates abnormal noise even during cleaning with a cleaning blade.

[0011] [Image Forming Apparatus] An electrophotographic image forming apparatus 100 illustrated in Figure 1 is a schematic cross-sectional view of an electrophotographic image forming apparatus including an electrophotographic belt according to an embodiment of the present invention. In this electrophotographic image forming apparatus, image forming units Py, Pm, Pc, and Pk for yellow (Y), magenta (M), cyan (C), and black (K) are arranged in order along the flat portion of the intermediate transfer belt 7, which is an intermediate transfer body, in the direction of movement. Here, 1Y, 1M, 1C, and 1K represent electrophotographic photoreceptors (photosensitive drums), and 2Y, 2M, 2C, and 2K represent charging rollers. Furthermore, 3Y, 3M, 3C, and 3K represent laser exposure devices, 4Y, 4M, 4C, and 4K represent developers, and 5Y, 5M, 5C, and 5K represent primary transfer rollers. Since the basic configuration of each image forming unit is the same, only the yellow image forming unit Py will be described in detail.

[0012] The yellow image forming unit Py has a drum-shaped electrophotographic photoreceptor (hereinafter also referred to as the "photosensitive drum" or "first image carrier") 1Y as an image carrier. The photosensitive drum 1Y is formed by sequentially laminating a charge generation layer, a charge transport layer, and a surface protection layer on an aluminum cylinder as the base. Furthermore, the yellow image forming unit Py is equipped with a charging roller 2Y as a charging means. By applying a charging bias to the charging roller 2Y, the surface of the photosensitive drum 1Y is uniformly charged.

[0013] A laser exposure device 3Y, which serves as an image exposure means, is positioned above the photosensitive drum 1Y. The laser exposure device 3Y scans and exposes the surface of the uniformly charged photosensitive drum 1Y according to image information, thereby forming an electrostatic latent image of the yellow component on the surface of the photosensitive drum 1Y. The electrostatic latent image formed on the photosensitive drum 1Y is developed by a developer unit 4Y using toner, which is the developer. The developer unit 4Y is equipped with a developer roller 4Ya, which is the developer carrier, and a regulating blade 4Yb, which is the developer amount regulating member, and also contains yellow toner, which is the developer. The developer roller 4Ya, to which the yellow toner has been supplied, is in light contact with the photosensitive drum 1Y in the developing section and rotates in the forward direction with a speed difference from the photosensitive drum 1Y. The yellow toner conveyed to the developing section by the developer roller 4Ya adheres to the electrostatic latent image formed on the photosensitive drum 1Y by applying a development bias to the developer roller 4Ya. This causes a visible image (yellow toner image) to be formed on the photosensitive drum 1Y.

[0014] The intermediate transfer belt 7 is stretched over the drive roller 71, tension roller 72, and driven roller 73, and is moved (rotationally driven) in the direction of the arrow in the figure when in contact with the photosensitive drum 1Y. The yellow toner image formed on the photosensitive drum (on the first image carrier) upon reaching the primary transfer section Ty is primary transferred onto the intermediate transfer belt 7 by a primary transfer body (primary transfer roller 5Y) positioned opposite the photosensitive drum 1Y via the intermediate transfer belt 7. Similarly, the above image formation operations are performed in the magenta (M), cyan (C), and black (K) units Pm, Pc, and Pk as the intermediate transfer belt 7 moves, stacking toner images of four colors—yellow, magenta, cyan, and black—on the intermediate transfer belt 7. The four toner layers are transported as the intermediate transfer belt 7 moves, and in the secondary transfer section T', they are transferred collectively onto the transfer material S (hereinafter also referred to as the "second image carrier"), which is transported at a predetermined timing by the secondary transfer roller 8, which acts as a secondary transfer means. In such secondary transfers, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate.

[0015] The transfer material S is supplied to the transport path from the cassette 12 in which the transfer material S is stored by the pickup roller 13. The transfer material S supplied to the transport path is transported to the secondary transfer section T' in synchronization with the four-color toner image transferred to the intermediate transfer belt 7 by the transport roller pair 14 and the registration roller pair 15. The toner image transferred to the transfer material S is fixed by the fuser 9 to become, for example, a full-color image. The fuser 9 has a fixing roller 91 equipped with a heating means and a pressure roller 92, and fixes the unfixed toner image on the transfer material S by heating and pressurizing it. After that, the transfer material S is discharged from the machine by a transport roller pair 16, a discharge roller pair 17, etc.

[0016] The cleaning unit 11 for the intermediate transfer belt 7 is positioned downstream of the secondary transfer section T' in the driving direction of the intermediate transfer belt 7. The cleaning blade in the cleaning unit 11 removes the remaining transfer toner that was not transferred to the transfer material S in the secondary transfer section T' and remains on the surface of the intermediate transfer belt 7. As explained above, the electrical transfer process of the toner image is repeatedly performed from the photoreceptor to the intermediate transfer belt, and from the intermediate transfer belt to the transfer material. Furthermore, the electrical transfer process is repeated even more by repeatedly recording onto multiple transfer materials.

[0017] [Electrophotographic belt] As illustrated in Figure 2, the electrophotographic belt of this embodiment is a laminate composed of at least two layers: a base layer 21 and an outermost layer 22. However, it is not limited to these two layers, and a primer layer to improve adhesion, a stress relaxation layer to suppress cracking of the surface layer 22, or an intermediate layer to suppress bleeding may be added between each layer. The electrophotographic belt can be used, for example, as an intermediate transfer belt.

[0018] (base layer) The base layer 21 has a cylindrical shape that is either roll-shaped or belt-shaped, forming an endless loop. Suitable materials for the base layer 21 include, for example, the following: polyether ether ketone, polyethylene terephthalate, polybutylene naphthalate, polyester, polyimide, polyamide, polyamide-imide, polyacetal, polyphenylene sulfide, polyvinylidene fluoride, etc. Furthermore, conductive compounds such as metal powder, conductive oxide powder, conductive carbon, lithium salt, and ionic liquid may be added to the resin for the base layer 21 to impart conductivity. In the following examples, polyimide with added carbon black was used from the viewpoint of obtaining excellent conductivity and environmental stability, but other combinations of resins and other conductive compounds may also be used. The thickness of the base layer 21 is preferably 10 μm or more and 500 μm or less. A thickness of 10 μm or more ensures sufficient strength as an electrophotographic belt. A thickness of 500 μm or less prevents the base layer from becoming too rigid, making it easier to create an endless shape for the electrophotographic belt.

[0019] (Surface layer) The surface 22-1 of the surface layer 22, opposite to the side facing the base layer, constitutes one of the outermost surfaces of the electrophotographic belt. When the electrophotographic belt is used as an intermediate transfer belt, surface 22-1 becomes the toner-carrying surface and also the surface to be cleaned by a cleaning member such as a cleaning blade. The thickness of the surface layer 22 is preferably 1 μm or more and 20 μm or less. By making the thickness of the surface layer 22 1 μm or more, durability can be ensured by achieving both low toner adhesion and suppression of peeling. By making the thickness of the surface layer 22 20 μm or less, it becomes easier to make the electrophotographic belt into an endless shape. The surface layer relating to this disclosure includes an acrylic resin. Furthermore, the surface layer 22 has at least a cage-type silsesquioxane structure.

[0020] <Acrylic resin> As the acrylic resin, acrylic resin, methacrylic resin, and mixed resins thereof can be used. Acrylic resins are used to ensure adhesion to the base layer 21 and to ensure mechanical strength. Examples of polymerizable monomers for forming acrylic resins include (i) or (ii) below. It is also possible to use polymerizable monomers that are commercially available as paints.

[0021] (i) At least one acrylate selected from the group consisting of pentaerythritol triacrylate, pentaerythritol tetraacrylate, trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol hexaacrylate, alkyl acrylate, benzyl acrylate, phenyl acrylate, ethylene glycol diacrylate, and bisphenol A diacrylate.

[0022] (ii) At least one methacrylate selected from the group consisting of pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, trimethylolpropane trimethacrylate, ditrimethylolpropane tetramethacrylate, dipentaerythritol hexamethacrylate, alkyl methacrylate, benzyl methacrylate, phenyl methacrylate, ethylene glycol dimethacrylate, and bisphenol A dimethacrylate.

[0023] Among these, high hardness is preferable, considering friction with other components such as photoreceptors and cleaning blades. For this reason, it is preferable to use a bifunctional or higher polymerizable monomer for the acrylic resin. Examples of bifunctional or higher polymerizable monomers include, for example, at least one polymerizable monomer selected from the group consisting of pentaerythritol triacrylate, pentaerythritol trimethacrylate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate. It is also preferable to use two or more polymerizable monomers selected from the above four polymerizable monomers in any combination. Furthermore, to form acrylic resins from such polymerizable monomers, one method involves adding a photopolymerization initiator and polymerizing it using electron beams or ultraviolet light.

[0024] Examples of photopolymerization initiators include: radical-generating photopolymerization initiators such as benzophenone, thioxanthone derivatives, benzyldimethyl ketal, α-hydroxyketone, α-hydroxyalkylphenone, α-aminoketone, α-aminoalkylphenone, monoacylphosphine oxide, bisacylphosphine oxide, hydroxybenzophenone, aminobenzophenone, titanocene derivatives, oxime esters, and oxyphenyl acetate. The acrylic resin content in the surface layer is preferably 20% by mass or more and 90% by mass or less, relative to the total solid content of the surface layer 22, in order to provide the surface layer with excellent strength and to support excellent toner release properties on the outer surface of the surface layer.

[0025] (Cage-type silsesquioxane structure) A cage-type silsesquioxane structure is a polyhedral structure in which Si atoms and O atoms are regularly arranged. For example, a cage-type silsesquioxane structure has 8 Si atoms and 12 oxygen atoms (RSiO 1.5 )8 (cage-type octasylsesquioxane, hereafter also called "T8"), having 10 Si atoms and 15 oxygen atoms, (RSiO 1.5 ) 10 (Cage-type decasilsesquioxane, hereafter also referred to as "T10"), and (RSiO2) having 12 Si atoms and 18 oxygen atoms. 1.5 ) 12 It is derived from at least one cage-type silsesquioxane selected from the group consisting of (cage-type dodecacilsesquioxane, hereafter also called "T12"). Figures 3 and 4 show non-restrictive examples of cage-type silsesquioxane structures. Figure 3 shows T8, Si8O 12Figure 4 shows a three-dimensional diagram of the cage-like silsesquioxane structure formed by (large spheres represent Si atoms, small spheres represent O atoms, and rod-shaped structures represent bonds). Also, Figure 4 shows the Si of T10. 10 O 15 This shows a three-dimensional diagram of the cage-like silsesquioxane structure formed by the two (large spheres represent Si atoms, small spheres represent O atoms, and rod-shaped structures represent bonds).

[0026] Because cage-type silsesquioxane has high stereoregularity, it readily aggregates with other cage-type silsesquioxanes to form a crystalline state. Therefore, even if cage-type silsesquioxane is simply incorporated into an acrylic resin binder in the surface layer, the cage-type silsesquioxanes readily aggregate to form crystals and undergo phase separation in the surface layer. As mentioned earlier, a surface layer having a phase separation structure derived from the cage-type silsesquioxane crystals is prone to generating abnormal noise when in contact with a cleaning blade. Therefore, the surface layer according to this disclosure has at least a cage-type silsesquioxane structure, but in X-ray diffraction measurements of its surface, no crystallization peak derived from the cage-type silsesquioxane structure is observed. One possible method to prevent the cage-type silsesquioxane structure from aggregating and forming a crystalline state in the surface layer is to reduce the symmetry of the cage-type silsesquioxane structure, creating an incomplete cage-type structure that makes crystallization less likely. However, if the symmetry of the cage-type silsesquioxane structure is reduced and made incomplete, the effect of introducing the cage-type silsesquioxane structure, such as improving the hardness of the surface layer, may be impaired. Therefore, in the present disclosure, as a material (raw material) for forming the surface layer, for example, a raw material composition containing the aforementioned polymerizable monomer and a compound having at least 2, preferably 3 or more functional groups (hereinafter simply referred to as "functional groups") capable of reacting with the raw material of the acrylic resin in the molecule, and having a cage-type silsesquioxane structure is used. Examples of the functional group include an acryloyl group and a methacryloyl group. Then, by reacting this raw material composition, an acrylic resin in which a cage-type silsesquioxane structure is three-dimensionally incorporated in the molecular chain can be obtained as a reactant. The cage-type silsesquioxane structure incorporated in the molecular chain of such an acrylic resin becomes difficult to move in the surface layer, and crystallization due to aggregation of the cage-type silsesquioxane structures is less likely to occur. As a result, a surface layer having a cage-type silsesquioxane structure and having no crystallization peak derived from the cage-type silsesquioxane structure in the reflection X-ray diffraction measurement of the surface can be obtained. As the compound having a cage-type silsesquioxane structure with a functional group, it is preferable to use a compound having 3 or more of the functional groups. The cage-type silsesquioxane structure can be more firmly incorporated into the molecular chain of the acrylic resin, and crystallization derived from the cage-type silsesquioxane structure can be more reliably suppressed. The crystallization peak derived from the cage-type silsesquioxane structure is observed under the conditions of X-ray source: Cu-Kα ray, tube voltage / current: 30 kv / 20 mA, scanning range: 5° to 15°, scan speed: 2.0° / min, sampling angle: 0.01°, when measured by the θ-fixed 2θ scanning method, it can be observed in the range of 2θ=7.0° or more and 9.0° or less. The criteria for the presence or absence of the crystallization peak derived from the cage-type silsesquioxane structure will be described in Examples below.

[0027] The cage-type silsesquioxane having at least two functional groups capable of reacting with the raw material of the acrylic resin in the molecule is not particularly limited, and examples thereof include the following. (C6H9O2)n(SiO with one acrylic group attached to one Si atom 1.5 )n, (C7H with one methacryl group attached to one Si atom11 O2)n(SiO 1.5 (CH2CH)n(SiO2) has one vinyl group attached to each Si atom. 1.5 )n, one epoxy group is attached to each Si atom (C6H 11 O2)n(SiO 1.5 )n. n represents 8, 10, or 12.

[0028] Examples of such compounds include those commercially available as "POSS" (trade name; Hybrid Plastics Inc.). More specifically, examples include "METHACRYL POSS Cage Mixture MA0735" having the structure shown in Figure 5(a), and "ACRYLO POSS Cage Mixture MA0736" having the structure shown in Figure 5(b) (both manufactured by Hybrid Plastics Inc.). The surface layer 22 may contain, in addition to the acrylic resin described above, a photopolymerization initiator, a conductive substance, and the like. [Examples]

[0029] <Preparation of coatings A to E for surface layer formation> (Paint A) The following materials were mixed in a homogenizer to obtain paint A. Pentaerythritol triacrylate 70 parts by mass Methyl ethyl ketone (MEK) 100 parts by mass 10 parts by mass of 1-hydroxycyclohexylphenyl ketone • Polyfunctional methacrylate containing a cage-type silsesquioxane structure (MA0735, made of hybrid plastics) 20 parts by mass

[0030] (Paint B) Paint B was prepared in the same manner as Paint A, except that the cage-type silsesquioxane structure-containing polyfunctional methacrylate in Paint A was replaced with a cage-type silsesquioxane structure-containing polyfunctional acrylate (MA0736, manufactured by Hybrid Plastics).

[0031] (Paint C) Paint C was prepared in the same manner as Paint B, except that the pentaerythritol triacrylate in Paint B was replaced with trimethylolpropane trimethacrylate.

[0032] (Paint D) The following materials were mixed in a homogenizer to obtain paint D. Pentaerythritol triacrylate 45 parts by mass Methyl ethyl ketone (MEK) 100 parts by mass 10 parts by mass of 1-hydroxycyclohexylphenyl ketone • Cage-type silsesquioxane structure-containing polyfunctional methacrylate (MA0735, made of hybrid plastics) 45 parts by mass

[0033] (Paint E) The following materials were mixed in a homogenizer to obtain paint E. • Macromonomer (AA-6, manufactured by Toagosei) 70 parts by mass Methyl ethyl ketone (MEK) 100 parts by mass 10 parts by mass of 1-hydroxycyclohexylphenyl ketone • Monofunctional methacrylate containing a cage-type silsesquioxane structure (PSS-(1-propylmethacrylate)-heptisobutyl substituted compound, manufactured by Sigma-Aldrich) 20 parts by mass

[0034] (Paint F) The following materials were mixed in an N-methylpyrrolidone solvent and polymerized at room temperature to obtain a polyamic acid containing a cage-type silsesquioxane structure. 30 parts by mass of 3,3′,4,4′-bifeltetracarboxylic acid dianhydride 15 parts by mass of p-phenylenediamine Double-decker cage-type silsesquioxane monomer 55 parts by mass The obtained cage-type silsesquioxane structure-containing polyamic acid was diluted with N,N-dimethylacetamide to a viscosity of 50 Pa·s or less to obtain paint F.

[0035] (Example 1) An electrophotographic belt according to this embodiment was fabricated using an endless intermediate transfer belt, which is installed in a full-color electrophotographic image forming apparatus (product name: imageRUNNER ADVANCE C5051; manufactured by Canon Inc.), as the base layer. Specifically, the outer surface of the intermediate transfer belt was subjected to corona treatment. After that, paint A was applied to the corona-treated outer surface and dried at a temperature of 70°C for 3 minutes to form a coating film with a thickness of 5 μm. Next, a high-pressure mercury lamp was used to irradiate the surface at a peak illuminance of 200 mW / cm² at 365 nm. 2 , cumulative light intensity 2 J / cm 2 The coating film was irradiated with ultraviolet light under these conditions to form a surface layer, thereby obtaining the electrophotographic belt 1 according to this embodiment.

[0036] (Examples 2-4) As shown in Table 1, electrophotographic belts 2 to 4 having a surface layer were obtained in the same manner as in Example 1, except that paint A was changed to paints B to D.

[0037] (Comparative Example 1) As shown in Table 1, an electrophotographic belt 5 was fabricated in the same manner as in Example 1, except that paint A was changed to paint E.

[0038] (Comparative Example 2) Corona treatment was performed on the outer surface of a polyimide seamless belt containing dispersed carbon black, which was installed in the imageRUNNER ADVANCE C5051. Subsequently, a polyamic acid solution containing a cage-type silsesquioxane structure was applied to the outer surface under conditions that resulted in a dry film thickness of 5 μm, and dried at 120°C for 30 minutes. Then, the polyamic acid was heated at 280°C for 2 hours to promote the ring-closing reaction and imidization, obtaining an electrophotographic belt 6 having a polyimide surface layer containing a cage-type silsesquioxane structure. Table 2 shows a list of CAS numbers for the materials used in the examples.

[0039] [Table 1]

[0040] [Table 2] In Table 2, the structure of the DDSQ monomer (silsesquioxane alicyclic acid dianhydride) is shown in Figure 5(c).

[0041] <Rating> X-ray diffraction measurement X-ray diffraction of the surface layers of electrophotographic belts 1-6 was measured using an X-ray diffractometer (e.g., product name: Ultima series, manufactured by Rigaku Corporation) with a fixed θ 2θ scanning method. Specifically, the measurement was performed with the following settings: X-ray source: Cu-Kα rays, tube voltage / current: 30kV / 20mA, scanning range: 5°~15°, scan speed: 2.0° / min, sampling angle: 0.01°, and number of integrations: 3. Under these conditions, a peak due to crystallization of the cage-type silsesquioxane structure can be observed in the range of 2θ = 7.0° to 9.0°. The presence or absence of this crystallization peak due to the cage-type silsesquioxane structure (hereinafter also referred to as the crystallization peak) is shown in Table 3. The determination of the presence or absence of the crystallization peak was made based on the spectrum obtained by smoothing and background removal using polynomial fitting smoothing processing on the obtained X-ray pattern with analysis software (product name: PDXL2, manufactured by Rigaku Corporation). Furthermore, if no peak with a peak top in 2θ = 7.0° to 9.0° was observed in the spectrum, it was determined that there were "no" crystallization peaks originating from the silsesquioxane structure. Also, if a peak with a peak top in 2θ = 7.0° to 9.0° was observed, and the intensity at the peak top of that peak was less than twice the difference between the maximum and minimum observed intensities in the range of 2θ = 5.0° to less than 7.0°, it was determined that there were "no" peaks originating from the silsesquioxane structure. Here, the peak top refers to the position where the positive and negative signs reverse in the differential curve of the diffraction intensity curve. In addition, peaks with peak tops appearing in the range of 2θ = 5.0° to less than 7.0° are due to measurement noise. Figure 6 shows the XRD spectrum of the surface layer according to Example 1.

[0042] ·Hardness measurement The hardness of the intermediate transfer belts obtained in Examples 1-4 and Comparative Examples 1-2 was measured by nanoindentation. Specifically, nanoindentation tests were performed using a Fischer Instruments PICODENTOR HM500 with a Vickers indenter, under conditions where the indentation depth was 100-200 nm, and the indentation hardness (MPa) was determined.

[0043] • Evaluation of whether or not abnormal noise occurs during cleaning with the cleaning blade. The electrophotographic properties of the intermediate transfer belts obtained in Examples 1-4 and Comparative Examples 1-2 were evaluated. Specifically, the obtained intermediate transfer belt was mounted in an electrophotographic image forming apparatus (product name: imageRUNNER ADVANCE C5760F; manufactured by Canon Corporation), and 30,000 electrophotographic images were formed continuously under the following conditions. Temperature: 25℃, relative humidity: 55% • Paper used: GF-C081 A3 size (basis weight 81.4g / m²) 2 (Thickness 97μm, whiteness approximately 100%, manufactured by Canon Inc.) • Printed image: The amount of CMYK toner on the intermediate transfer belt is 0.4 mg / cm² each. 2 After printing 97 images at 100% aspect ratio, the amount of CMYK toner on the intermediate transfer belt was 0 mg / cm². 2 Three copies were printed with an image ratio of 100%. This cycle of 100 copies was repeated 30,000 times (300 cycles). During the printing of 30,000 sheets, we checked for any abnormal noises caused by the cleaning blade in contact with the intermediate transfer belt. If no noise occurred, it was recorded as "no noise," and if noise occurred, it was recorded as "abnormal noise occurred." The evaluation results are shown in Table 3. In addition, Table 3 also shows the types and number of functional groups of the cage-type silsesquioxane structure compounds used as raw materials in the examples and comparative examples.

[0044] [Table 3]

[0045] As shown in Table 3, the indentation hardness of the surface layers of Examples 1-4 by the nanoindentation method was 450 MPa or higher. In Comparative Example 1, the compound having a cage-type silsesquioxane structure used as a raw material for forming the surface layer had only one functional group. Therefore, it is thought that the cage-type silsesquioxane structure was not incorporated into the molecular chain of the acrylic resin, but rather existed as a side chain of the acrylic resin molecular chain. As a result, the cage-type silsesquioxane structure was in a state where it could move relatively freely, and it is thought that the formation of a crystalline structure derived from the cage-type silsesquioxane structure could not be prevented. Consequently, it is presumed that phase separation occurred in the surface layer due to the crystallization of the cage-type silsesquioxane structure, forming areas where the cage-type silsesquioxane structure was aggregated and areas where it was sparse, and that the coefficient of friction on the surface of the electrophotographic belt changed locally, causing abnormal noise from the cleaning blade. Furthermore, in Comparative Example 2, it is believed that the cage-type silsesquioxane structure was incorporated into the linear polymer of polyimide. Since the linear polymer is in a state where the molecular chains can move relatively freely, it is thought that it was not able to prevent the formation of the crystal structure originating from the cage-type silsesquioxane structure. As a result, it is presumed that, similar to Comparative Example 1, phase separation occurred in the surface layer due to the crystallization of the cage-type silsesquioxane structure.

[0046] This disclosure includes the following components: [Configuration 1] An electrophotographic belt having a base layer and a surface layer containing an acrylic resin, The surface layer has at least a cage-type silsesquioxane structure, An electrophotographic belt in which no crystallization peak originating from the cage-type silsesquioxane structure is observed in reflection X-ray diffraction measurements of the surface of the surface layer. [Configuration 2] The electrophotographic belt according to configuration 1, wherein the cage-type silsesquioxane structure is incorporated into the molecular chain of the acrylic resin. [Configuration 3] The electrophotographic belt according to configuration 1 or 2, wherein the indentation hardness of the surface layer by the nanoindentation method is 450 MPa or more. [Structure 4] The aforementioned acrylic resin, At least one polymerizable monomer selected from the group consisting of pentaerythritol triacrylate, pentaerythritol trimethacrylate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate, An electrophotographic belt according to any one of configurations 1 to 3, comprising a reaction product with a compound having the cage-type silsesquioxane structure within its molecule and having at least two functional groups. [Composition 5] The electrophotographic belt according to configuration 4, wherein the functional group is at least one selected from the group consisting of an acryloyl group and a methacryloyl group. [Composition 6] An electrophotographic image forming apparatus comprising an image carrier for carrying a toner image, and an intermediate transfer belt for carrying and transporting the toner image, which has been primary transferred from the image carrier, to a transfer material for secondary transfer, wherein the intermediate transfer belt is an electrophotographic belt as described in any of configurations 1 to 5. [Explanation of Symbols]

[0047] Py: Yellow image forming unit Pm: Magenta Image Forming Unit Pc: Cyan image forming unit Pk: Black image forming unit 1Y: Yellow Photosensitive Drum 1M: Magenta photosensitive drum 1C: Cyan photosensitive drum 1K: Black photosensitive drum 4Y: Yellow Developer 4M: Magenta Developer 4C: Cyan Developer 4K: Black Developer 5Y, 5M, 5C, 5K: Primary transfer rollers Ty, Tm, Tc, Tk: Primary transfer area 71: Drive roller 72: Tension Roller 73: Driven roller 100: Image forming apparatus 2Y, 2M, 2C, 2K: Electrostatic rollers 3Y, 3M, 3C, 3K: Laser exposure equipment 11: Transfer belt cleaning unit 12: Paper feed cassette 15: Resistola vs. 7: Intermediate transfer belt 8:2nd secondary transfer outer roller 9: Fuser 91: Fixing film 92: Pressure roller S: Transfer material 21: Base layer of the intermediate transfer belt 22: Surface layer of the intermediate transfer belt

Claims

1. The device comprises an image carrier for holding a toner image, an intermediate transfer belt for carrying and transporting the toner image, which has been primarily transferred from the image carrier, to a transfer material for secondary transfer, and a cleaning blade for removing residual toner from the surface of the intermediate transfer belt. The intermediate transfer belt is an electrophotographic belt having a base layer and a surface layer containing an acrylic resin, The surface layer has at least a cage-type silsesquioxane structure, An electrophotographic image forming apparatus characterized in that, in reflection X-ray diffraction measurements of the surface of the surface layer, no crystallization peak originating from the cage-type silsesquioxane structure is observed.

2. The electrophotographic image forming apparatus according to claim 1, wherein the cage-type silsesquioxane structure is incorporated into the molecular chain of the acrylic resin.

3. The electrophotographic image forming apparatus according to claim 1, wherein the indentation hardness of the surface layer by the nanoindentation method is 450 MPa or more.

4. The aforementioned acrylic resin, At least one polymerizable monomer selected from the group consisting of pentaerythritol triacrylate, pentaerythritol trimethacrylate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate, The electrophotographic image forming apparatus according to claim 1, comprising a reaction product with a compound having the cage-type silsesquioxane structure within its molecule and having at least two functional groups.

5. The electrophotographic image forming apparatus according to claim 4, wherein the functional group is at least one selected from the group consisting of acryloyl groups and methacryloyl groups.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor

    JP2010008753A

  • Polyhedral silsesquioxane modified polyimide-containing intermediate transfer member

    JP2011034083A

  • Electrophotographic photoreceptor, intermediate transfer member, process cartridge, and electrophotographing apparatus

    JP2013029812A

  • Intermediate transfer body and image forming apparatus using the same

    JP2014215470A

  • Image carrier for electrophotography, electrophotographic image forming apparatus, and process cartridge

    JP2017049530A