Fixing member and heat fixing device
By uniformly distributing thermal conductive filler particles in the elastic layer of a fixing member, the delamination issue is resolved, maintaining high thermal conductivity and ensuring stable image quality in electrophotographic devices.
Patent Information
- Application Number
- JP2022136307
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Fixing members in electrophotographic image forming machines experience delamination at the interface between the base layer and the elastic layer due to uneven distribution of thermal conductive filler particles, leading to reduced thermal conductivity and poor image quality over time.
A fixing member with a base layer, elastic layer, and surface layer, where the elastic layer contains uniformly distributed thermal conductive filler particles, with controlled coefficient of variation in Voronoi regions, ensuring high thermal conductivity and preventing delamination.
The solution provides a fixing member with stable thermal conductivity in the thickness direction and prevents peeling between layers, enabling high-quality electrophotographic image formation.
Smart Images

Figure 0007955102000003 
Figure 0007955102000004 
Figure 0007955102000005
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a fixing member and a heating fixing apparatus used in a heating fixing apparatus of an electrophotographic image forming apparatus. [Background technology]
[0002] Fixing components used in the heating and fixing devices of electrophotographic image forming machines such as printers, copiers, and facsimile machines come in film or roller forms. These fixing components are known to have an elastic layer formed on a heat-resistant resin or metal film or roller-shaped substrate, with the elastic layer being made of heat-resistant rubber or the like as needed, and the surface layer containing a fluororesin that has excellent release properties from toner. The elastic layer of the fixing component is required to have high elasticity and high thermal conductivity. Therefore, the elastic layer is blended with an inorganic filler with high thermal conductivity as a thermal conductive filler in rubber such as silicone rubber. In recent years, there has been a growing demand to further improve the thermal conductivity of fixing materials in order to increase print speed and improve image quality. Patent Document 1 discloses a fixing material in which a heat channel is formed within an elastic layer by a thermal conductive filler, thereby improving thermal conductivity. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Patent No. 5054924 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] According to the inventors' studies, the fixing member described in Patent Document 1 may experience delamination at the interface between the base layer and the elastic layer after long-term use. One aspect of the present disclosure is directed to providing a fixing member having high thermal conductivity in the thickness direction and being free from peeling between a base layer and an elastic layer even after long-term use. Another aspect of the present disclosure is directed to providing a heat fixing device capable of stably forming high-quality electrophotographic images. [Means for solving the problem]
[0005] According to one aspect of the present disclosure, there is provided a fixing member including at least an endless base layer, an elastic layer provided on an outer peripheral surface of the base layer, and a surface layer provided on an outer peripheral surface of the elastic layer, wherein the base layer contains at least one selected from the group consisting of aluminum, iron, copper, nickel, stainless steel, brass, polyimide, polyamide-imide, and polyether ether ketone, wherein the elastic layer contains rubber and thermally conductive filler particles dispersed in the rubber, wherein the elastic layer has a thickness of 200 μm or more, wherein the elastic layer has a thermal conductivity in a thickness direction of 0.40 W / m·K or more, wherein the elastic layer contains the thermally conductive filler particles in an amount of 40% by volume or more and 60% by volume or less, wherein, in a cross section of the elastic layer in a direction orthogonal to a circumferential direction, a region from an interface between the base layer and the elastic layer to a thickness of 50 μm in the thickness direction of the elastic layer is defined as a region A, and an arithmetic average value of each area of Voronoi regions formed by performing Voronoi division using, as mother points, the thermally conductive filler particles exposed in the region A of the cross section is defined as A ave and a standard deviation is defined as Aσ, and a coefficient of variation calculated by the following formula (1) is defined as Av, and an arithmetic average value of the coefficient of variation Av is defined as Av ave wherein the arithmetic average value Av of the coefficient of variation ave is 1.2 or less The arithmetic mean of the areas of each Voronoi region formed by Voronoi tessellation using the heat-conducting filler particles exposed in region B other than region A of the cross-section as the parent points is B. ave Let Bσ be the standard deviation, let Bv be the coefficient of variation calculated by the following equation (2), and let Bv be the arithmetic mean of the coefficient of variation Bv. ave In this case, the arithmetic mean of the coefficient of variation is Bv ave The value is between 1.5 and 4.0. A fixing member is provided. Av = (Aσ / A ave ) (1) Bv=(Bσ / B ave )(2) Further, according to another aspect of the present disclosure, there is provided a heat fixing device including the above-described fixing member, and a pressure member disposed to face the fixing member. Advantageous Effects of Invention
[0006] According to an aspect of the present disclosure, it is possible to obtain a fixing member which is high in thermal conductivity in the thickness direction and in which peeling does not occur between the base layer and the elastic layer even after long-term use. In addition, according to an aspect of the present disclosure, it is possible to obtain a heat fixing device capable of stably forming a high-quality electrophotographic image. Brief Description of Drawings
[0007] [Figure 1] FIG. 1 is a schematic view of an image forming apparatus in a first exemplary embodiment. [Figure 2] FIG. 2 is a schematic view of a fixing device in the first exemplary embodiment. [Figure 3] FIG. 3 is a schematic view of a fixing film in the first exemplary embodiment. [Figure 4] FIG. 4 are views each illustrating a first section and a second section of an elastic layer of a fixing member in a belt form. [Figure 5] FIG. 5 is a schematic view of a section of a fixing member. [Figure 6] FIG. 6 are schematic views of binarization and Voronoi division of a section image of an elastic layer. Description of Embodiments
[0008] In the present specification, the expression "from XX or more to XX or less" or "XX to XX" representing a numerical range means a numerical range including lower and upper limits which are endpoints unless otherwise specified. In addition, in the case where the numerical ranges are described stepwise, arbitrary combinations of the upper limit and the lower limit of each numerical range are disclosed. Hereinafter, a fixing belt having an endless belt shape according to at least one embodiment of the present disclosure will be described in detail. It should be noted that the technical scope of the present disclosure is not limited to the following description.
[0009] The inventors speculate that the reason for delamination occurring at the interface between the base layer and the elastic layer when the fixing member described in Patent Document 1 is used over a long period of time is as follows: For example, a heating element is pressed against the inner circumferential surface of the base layer. On the other hand, in the fixing process, since moving paper is in contact with the surface of the fixing member, the surface side of the elastic layer tries to follow the transport of the paper. As a result, a large shear force is applied to the interface between the base layer and the elastic layer. Regarding adhesion between the base layer and the elastic layer, "adhesion force" and "peel force" are related, and adhesion can be ensured when the relationship "adhesion force > peel force" holds, but delamination occurs when "adhesion force < peel force". The above shear force functions as a peel force. According to the inventors' investigation, it was found that when the microscopic strain generated between the heat-conducting filler particles in the elastic layer due to the shear force is large, the peel force becomes high. This microscopic strain depends on the distance between the thermally conductive filler particles. If the distance between the thermally conductive filler particles is uneven, the magnitude of the microscopic strain will be uneven, leading to increased localized delamination forces and making delamination between the base layer and the elastic layer more likely.
[0010] Therefore, it is thought that by making the distance between heat-conducting filler particles uniform, the unevenness of microscopic strain can be reduced, thereby suppressing the occurrence of delamination between the base layer and the elastic layer. However, if the distance between heat-conducting filler particles is made uniform, it becomes difficult to form heat channels in the thickness direction of the elastic layer, leading to a decrease in the thermal conductivity in the thickness direction of the elastic layer. Here, the inventors found that shear stress tends to concentrate particularly in a 50 μm thickness region (hereinafter also referred to as "region A") from the surface facing the base layer of the elastic layer toward the opposite surface. Therefore, they found that by improving the dispersibility of the thermally conductive filler in region A and making the distance between thermally conductive filler particles uniform, while agglomerating the thermally conductive filler in regions other than region A, it is possible to suppress delamination between the base layer and the elastic layer while maintaining a thermal conductivity of 0.40 W / mK or higher in the thickness direction of the elastic layer.
[0011] Specifically, a fixing member according to one aspect of the present disclosure includes at least a base layer having an endless shape, an elastic layer provided on the outer peripheral surface of the base layer, and a surface layer on the outer peripheral surface of the elastic layer. The base layer includes at least one selected from the group consisting of aluminum, iron, copper, nickel, stainless steel, brass, polyimide, polyamide-imide, and polyether ether ketone. The elastic layer contains rubber and thermally conductive filler particles dispersed in the rubber, and the elastic layer has a thickness of 200 μm or more. The content of the thermally conductive filler particles in the elastic layer is 40% by volume or more and 60% by volume or less. Furthermore, in a cross-section of the elastic layer in a direction orthogonal to the circumferential direction, when Voronoi division is performed using the thermally conductive filler particles exposed in the cross-section as generating points to form Voronoi regions, the coefficient of variation Av of the area of the Voronoi regions in region A ave is 1.2 or less. Furthermore, the thermal conductivity of the elastic layer in the thickness direction is 0.40 W / mK or more.
[0012] FIG. 1 is a cross-sectional view of a color electrophotographic printer as an image forming apparatus according to an aspect of the present disclosure, taken along the conveyance direction of the recording material. In the present embodiment, the color electrophotographic printer is simply referred to as a "printer". The printer shown in FIG. 1 includes image forming units 10 for each color of Y (yellow), M (magenta), C (cyan), and Bk (black). A photosensitive drum (photoconductor) 11 is pre-charged by a charger 12. Thereafter, the photosensitive drum 11 is exposed by a laser scanner 13 to form an electrostatic latent image. The electrostatic latent image is developed into a toner image by a developing device 14. The toner image on the photosensitive drum 11 is sequentially transferred onto an image carrier, such as an intermediate transfer belt 31, by a primary transfer blade 17. After transfer, the toner remaining on the photosensitive drum 11 is removed by a cleaner 15. As a result, the surface of the photosensitive drum 11 is cleaned and prepared for the next image formation.
[0013] Meanwhile, the recording material P is fed one sheet at a time from the paper feed cassette 20 or the multi-feed tray 25 and delivered to the registration roller pair 23. The registration roller pair 23 receives the recording material P and straightens it if it is skewed. Then, the registration roller pair 23 synchronizes with the toner image on the intermediate transfer belt 31 and delivers the recording material P between the intermediate transfer belt 31 and the secondary transfer roller 35. The color toner image on the intermediate transfer belt is transferred to the recording material P by a transfer body, such as the secondary transfer roller 35. Subsequently, the toner image on the recording material P is fixed to the recording material P by heating and pressurizing the recording material P by the fuser 40.
[0014] Next, a fixing device according to one aspect of the present disclosure will be described. Figure 2 shows a schematic configuration diagram of the fixing device 40, which uses a film heating type heating device (tensionless type). In this embodiment, such a heating device was used, but it can also be implemented with a roller pair type or a film type heating device.
[0015] 43 is a ceramic heater (hereinafter referred to as "heater") used as a heating element. Heater 43 basically consists of a long, narrow ceramic substrate with its length perpendicular to the drawing and an electrically conductive heat-generating resistor layer on the surface of this substrate. It is a low-heat-capacity heater that heats up with a steep rise characteristic when current is passed through the heat-generating resistor layer. Furthermore, it is configured to switch the energized area according to the length width size of the recording material.
[0016] 41 is a cylindrical (endless) heat-resistant fixing film that serves as a heating element for transferring heat, and is loosely fitted onto the support member (heater holder) including the heater 43. The structure of the fixing film 41 in this embodiment is as shown in Figure 3, and is a fixing film having a three-layer composite structure including at least a surface layer 41a, an elastic layer 41c, and a base layer 41b.
[0017] Reference numeral 44 denotes a heat-resistant elastic pressure roller as a pressurizing member, consisting of a core metal and an elastic layer made of heat-resistant rubber such as silicone rubber or fluororubber, or silicone rubber foam, with both ends of the core metal supported by bearings so as to be freely rotatable. The fixing film 41 and heater 43 are placed above the pressure roller 44, parallel to the pressure roller 44, and pressed with a pressing member (not shown). In this way, the lower surface of the heater 43 and the upper surface of the pressure roller 44 are pressed together against the elasticity of the roller's elastic layer via the fixing film 41, forming a fixing nip portion T of a predetermined width which serves as a heating portion.
[0018] The pressure roller 44 is driven to rotate at a predetermined peripheral speed in the counterclockwise direction indicated by the arrow by a driving means (not shown). Due to the rotational drive of the pressure roller 44, a rotational force is applied to the cylindrical fixing film 41 by the pressure friction force at the fixing nip portion T between the pressure roller 44 and the fixing film 41. The fixing film 41 then slides in close contact with the downward surface of the heater 43 and enters a state of driven rotation in the clockwise direction indicated by the arrow. The support member (heater holder) 46 also serves as a rotation guide member for the cylindrical fixing film 41.
[0019] The pressure roller 44 is driven to rotate, causing the cylindrical fixing film 41 to rotate along with it. Power is also supplied to the heater 43, causing it to rapidly heat up to a predetermined temperature and reach a temperature-controlled state. In this state, recording material P carrying an unfixed toner image T is introduced between the fixing film 41 and the pressure roller 44 in the fixing nip section T. The toner image-carrying side of the recording material P then adheres closely to the outer surface of the fixing film 41 in the fixing nip section T, and the fixing nip section T is clamped and conveyed together with the fixing film 41. During this clamping and conveying process, the recording material P is heated by the heat of the fixing film 41 heated by the heater 43, and the unfixed toner image T on the recording material P is heated and pressurized, melting and fixing it onto the recording material P. The recording material P that has passed through the fixing nip section T is separated from the surface of the fixing film 41 by curvature and discharged and conveyed. 45 is a contact thermometer (thermistor) that measures the temperature of the fixing film 41 heated by the heater 43 and passes the detection result to a temperature control means (not shown). 46 is a heater holder, a component that holds the heater 43 which has been heated to a high temperature.
[0020] An anchoring member according to one aspect of the present disclosure comprises a base layer having an endless shape, an elastic layer provided on the outer circumferential surface of the base layer, and a surface layer on the outer circumferential surface of the elastic layer. The fixing member 41 in this disclosure is as shown in Figure 3. The fixing member has a base layer 41b, an elastic layer 41c covering its outer surface, and a surface layer 41a covering the surface of the elastic layer 41c opposite to the side facing the base layer. The surface layer 41a may be bonded to the surface of the elastic layer 41c opposite to the side facing the base layer 41b with an adhesive layer (not shown).
[0021] (1) Surface layer The surface layer 41a can be made of a fluororesin material with a thickness of 100 μm or less, preferably 10 to 70 μm. Examples of fluororesin layers include polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA).
[0022] (2) Base layer The material of the base layer 41b includes at least one selected from the group consisting of aluminum, iron, copper, nickel, stainless steel, brass, polyimide, polyamide-imide, and polyetheretherketone. The thickness is not particularly limited, but for example, from the viewpoint of strength, flexibility, and heat capacity, it is preferably 20 μm to 100 μm. The outer surface of the base layer 41b may be subjected to a surface treatment to provide adhesion to the elastic layer 41b. The surface treatment can be one or more types of physical treatments such as blasting, lapping, and polishing, or chemical treatments such as oxidation, coupling agent treatment, and primer treatment.
[0023] When an elastic layer 41c containing silicone rubber is provided on the surface of the base layer 41b, it is preferable to apply a primer treatment to the surface of the base layer 41b in order to improve the adhesion between the base layer 41b and the elastic layer 41c. Examples of primers used for the primer treatment include paints in which a silane coupling agent, a silicone polymer, methyl siloxane hydrogenation, an alkoxysilane, a reaction-accelerating catalyst, and a coloring agent such as red iron oxide are appropriately blended and dispersed in an organic solvent. The primer can be appropriately selected depending on the material of the base layer, the type of elastic layer, or the form of the crosslinking reaction. In particular, when the elastic layer contains a large amount of unsaturated aliphatic groups, a primer containing hydrosilyl groups is preferably used to impart adhesion through reaction with the unsaturated aliphatic groups. Other types of primers include those containing alkoxy groups. Commercially available primers can be used. The priming process also includes applying the primer to the outer surface of the base layer (the surface that adheres to the elastic layer) and drying or firing it.
[0024] (3) Elastic layer The elastic layer 41c is sandwiched between the surface layer 41a and the base layer 41b, and has a thickness of 200 μm or more. A thickness of 200 μm or more in the elastic layer ensures a sufficient nip width when the fixing belt is incorporated into the fixing device. While there is no particular upper limit to the thickness of the elastic layer, it is preferably, for example, 5 mm or less. That is, a preferred thickness range for the elastic layer is 200 μm or more and 5 mm or less, and a particularly preferred thickness range is 200 μm or more and 500 μm or less. The elastic layer may have a multilayer structure and may include rubber and heat-conducting filler particles dispersed in the rubber. The elastic layer 41c preferably contains silicone rubber with excellent heat resistance. Furthermore, addition-curing liquid silicone rubber is preferably used as the raw material for the silicone rubber.
[0025] High thermal conductivity is required for the thermal conductive filler particles, and inorganic materials, especially metals and metal compounds, are preferred. Specifically, the following can be listed, and these can be used individually or in mixtures of two or more: High thermal conductivity fine powders such as silicon carbide (SiC), silicon nitride (Si3N4), boron nitride (BN), aluminum nitride (AlN), alumina (Al2O3), zinc oxide (ZnO), magnesium oxide (MgO), silica (SiO2), copper (Cu), aluminum (Al), silver (Ag), iron (Fe), nickel (Ni), carbon black (C), carbon fiber (C), and carbon nanotubes (C).
[0026] The content of thermally conductive filler particles in the elastic layer is between 40% by volume and 60% by volume. A content of 40% by volume or more ensures sufficient thermal conductivity of the elastic layer. A content of 60% by volume or less prevents the elastic layer from becoming excessively hard. The method for measuring the content of thermally conductive filler particles in the elastic layer is shown below.
[0027] <Method for measuring the content of thermally conductive filler particles in an elastic layer> The content of thermally conductive filler particles in the elastic layer can be confirmed using a thermogravimetric analyzer (TGA) (e.g., product name: TGA851, manufactured by Mettler-Toledo). Cut out a portion of the elastic layer with a razor or similar tool, accurately weigh approximately 20 mg, and place it in an alumina sample pan used with the apparatus. Set the sample pan containing the sample in the apparatus and heat it in a nitrogen atmosphere from room temperature to 800°C at a heating rate of 20°C per minute, and then maintain a constant temperature of 800°C for 1 hour. In a nitrogen atmosphere, as the temperature rises, components other than thermally conductive filler particles are decomposed and removed by cracking without oxidation, thus reducing the mass of the sample. By comparing the mass before and after measurement, the weight of thermally conductive filler particles contained in the elastic layer can be calculated. The content of thermally conductive filler particles in the elastic layer can be calculated from the specific gravity of the thermally conductive filler particles used.
[0028] In this disclosure, when a Voronoi partition is performed in a cross-section perpendicular to the circumferential direction of an elastic layer, with heat-conducting filler particles exposed in the cross-section as parent points, a Voronoi region is formed, and the coefficient of variation of the area of the Voronoi region Av in region A is... ave The coefficient of variation Av is 1.2 or less. ave By keeping the value below 1.2, the uneven distribution of thermally conductive fillers in region A is suppressed, preventing shear stress from concentrating in specific areas. As a result, delamination at the interface between the base layer and the elastic layer can be prevented.
[0029] In regions other than region A of the elastic layer, i.e., regions adjacent to region A and located closer to the surface layer than region A (hereinafter also referred to as "region B"), the coefficient of variation of the Voronoi region area Bv ave It is preferable that the coefficient of variation Bv is between 1.5 and 4.0. ave A value of 1.5 or higher makes it possible to set the thermal conductivity in the thickness direction of the elastic layer to 0.4 W / m·K or higher. Also, the coefficient of variation Bv ave By keeping the value below 4.0, variations in the hardness of the elastic layer can be suppressed.
[0030] <Formation of Voronoi domains> This section describes the formation of a Voronoi region by Voronoi tessellation using heat-conducting filler particles exposed in a cross-section perpendicular to the circumferential direction of an elastic layer, with the heat-conducting filler particles exposed in the cross-section as parent points. When multiple points (hereinafter also referred to as generator points) exist within an image region, all adjacent generator points are connected by straight lines, and perpendicular bisectors are created for each of the basic lines connecting two adjacent generator points. When the perpendicular bisectors extending from adjacent basic lines are connected, a region is created in which a single generator point is enclosed by these perpendicular bisectors. This region enclosed by perpendicular bisectors is called a Voronoi region. The points where the lines connecting two adjacent generator points intersect with their perpendicular bisectors represent the shortest distance from each generator point, and the size (area) of the Voronoi region formed by these perpendicular bisectors represents the distance between adjacent generator points. In other words, if the distance between adjacent generator points is large, the area of the Voronoi region will also be large.
[0031] In this disclosure, the generating point for the above Voronoi partition is a heat-conducting filler particle. There are two partitioning methods: one based on the centroid of the heat-conducting filler particle and another based on the edges of the heat-conducting filler particle. In this disclosure, the partitioning method based on the edges is used. In the partitioning method based on the edges, the shortest distance between the edges of two adjacent heat-conducting filler particles is selected, and the region enclosed by the perpendicular bisector of this line becomes the Voronoi region. Specifically, this is done in the following way.
[0032] <Coefficient of variation of the area of the Voronoi domain in region A: Av ave Calculation > (1) First, prepare cross-sectional observation samples. For example, if the fixing member is a fixing belt 400 as shown in Figure 4A, take a total of 10 samples 401, each 5 mm long, 5 mm wide, and with a thickness equal to the total thickness of the fixing belt, from 10 arbitrary locations on the fixing belt, as shown in Figure 4B. Sample 401 consists of the surface layer 6, adhesive layer 5, elastic layer 4, and base layer 3 of the cut sample, with the elastic layer having a first cross-section 401-1 in the thickness-circumferential direction and a second cross-section 401-2 in the thickness-axial direction. Five of the 10 obtained samples are polished using an ion beam at the cross-section in the circumferential direction of the fixing belt, i.e., the cross-section including the first cross-section 401-1 of the elastic layer in the thickness-circumferential direction. The remaining five samples are polished using an ion beam at the cross-section perpendicular to the circumferential direction of the fixing belt, i.e., the cross-section including the second cross-section 401-2 of the elastic layer in the thickness-axial direction. For polishing the cross-section with an ion beam, for example, a cross-section polisher can be used. Ion beam polishing of cross-sections prevents the detachment of filler particles from the sample and the inclusion of abrasives, and also allows for the formation of cross-sections with fewer polishing marks.
[0033] (2) Next, the first and second cross-sections of the elastic layer are observed using a laser microscope or scanning electron microscope (SEM) for five samples in which the first cross-section 401-1 of the elastic layer has been polished, and for five samples in which the second cross-section 401-2 of the elastic layer has been polished. For example, when the cross-section is as shown in Figure 5A, a 50 μm × 50 μm square cross-sectional image is obtained at any location within a 50 μm thickness region A (Figure 5A 403) from the surface facing the base layer of the elastic layer toward the opposite surface.
[0034] (3) Next, the obtained image, as shown in Figure 6A, is subjected to black and white binarization using commercially available image software so that the filler particles 61 appear white and the elastic layer appears black (Figure 6B). For example, the Otsu method can be used as a binarization method. (4) Next, the white areas of the created binarized image are segmented using the watershed algorithm. This process is necessary because if fillers are close together, multiple fillers may stick together and be recognized as a single filler.
[0035] (5) Finally, Voronoi partitioning is performed on the regions that have been partitioned using the watershed algorithm. Specifically, Voronoi partitioning is performed using the following procedure: Calculate the position of the centroid (point A in Figure 6C) of each white region. Connect all the centroids of adjacent white regions with straight lines to create a base line, and calculate the position of the intersection (point F in Figure 6C) of the base line with the outer perimeter of each partitioned white region. Usually, two of these intersection points F are created on a single straight line connecting the centroids, and the perpendicular bisector between these two intersection points is created and used as the partition line. When adjacent regions are touching, sometimes only one intersection point F is created, in which case a line perpendicular to the base line and passing through intersection point F is created and used as the partition line. When the partition lines created from adjacent white regions are connected, a region enclosed by the partition lines is created so as to surround the white region (Figure 6D). In this embodiment, this is defined as the Voronoi region. This Voronoi region can be used as a region that represents the distribution of distances between fillers. Calculate the area of each Voronoi region and take their arithmetic mean as A. ave, if the standard deviation is Aσ, then Aσ is A ave The coefficient of variation Av (= Aσ / A) is obtained by dividing the value by Aσ / A. ave ) is defined as follows.
[0036] (6)Calculate the coefficient of variation Av for each of the 10 images obtained in (2), and then average them to get Av ave As a result, the coefficient of variation of the Voronoi region of the filler in region A of this embodiment is derived. One method for controlling the coefficient of variation Avave of the area of the Voronoi region of the thermally conductive filler in region A is to adjust the particle size distribution of the filler particles.
[0037] <Coefficient of variation Bv of the area of the Voronoi domain in region B> ave Calculation > (1) Following the same procedure as in region A, for example, if the fixing member is a fixing belt 400 as shown in Figure 4A, then, as shown in Figure 4B, a total of 10 samples 401, each measuring 5 mm in length, 5 mm in width, and having a thickness equal to the total thickness of the fixing belt, were taken from 10 arbitrary locations on the fixing belt. Five of the obtained samples were polished using an ion beam to form a cross-section in the circumferential direction of the fixing belt, i.e., a cross-section including the thickness of the elastic layer minus the first cross-section 401-1 in the circumferential direction. The remaining five samples were polished using an ion beam to form a cross-section perpendicular to the circumferential direction of the fixing belt, i.e., a cross-section including the thickness of the elastic layer minus the second cross-section 401-2 in the axial direction.
[0038] (2) Next, for five samples in which the first cross-section 401-1 of the elastic layer has been polished, the first cross-section 401-1 is observed using a laser microscope or scanning electron microscope (SEM), and cross-sectional images are obtained for region B other than region A (Figure 5B 404). Next, for five samples in which the second cross-section 401-2 of the elastic layer has been polished, the second cross-section 401-2 is observed using a laser microscope or scanning electron microscope (SEM), and cross-sectional images are obtained for region B other than region A (Figure 5B 404). For the cross-sectional images, a total of three 50 μm × 50 μm square images are obtained at arbitrary locations in each of the three regions B1, B2, and B3 (Figure 5 404-1, 404-2, 404-3), which are obtained by dividing region B into three equal parts in the thickness direction.
[0039] (3) The acquired image is subjected to the same procedure as in region A: grayscale binarization, region segmentation using the watershed algorithm, and Voronoi segmentation. For the images acquired in regions B1, B2, and B3, the area of each Voronoi region is calculated, and the arithmetic mean of these areas is taken as B1. ave B2 ave B3 ave And the standard deviations of each were set to B1σ, B2σ, and B3σ. Then, B1σ was set to B1 ave The value obtained by dividing by is the coefficient of variation B1v, and B2σ is B2 ave The value obtained by dividing by is the coefficient of variation B2v, and B3σ is B3 ave The value obtained by dividing by is defined as the coefficient of variation B3v, and the average of B1v, B2v, and B3v is taken as the coefficient of variation Bv.
[0040] (4) For the 10 samples obtained in (2), calculate the coefficient of variation Bv for each, and then average them to obtain Bv ave This was used as the coefficient of variation of the Voronoi region of the filler within region B of this embodiment. In addition to rubber and thermally conductive filler particles, other additives may be added to the elastic layer according to desired properties. Examples of other additives include flocculants.
[0041] In this disclosure, the coefficient of variation Bv of the Voronoi region area in region B of the elastic layer other than region A. ave It is preferable that the ratio is between 1.5 and 4.0, and as a method to achieve this, it is preferable to add a flocculant in region B of the elastic layer and adjust the amount added. In region B, the adhesion of the flocculant to the surface of the thermally conductive filler particles reduces the dispersibility of the thermally conductive filler particles in the rubber, and the coefficient of variation of the Voronoi region area Bv ave It can improve.
[0042] As a flocculant, it is preferable to use a compound that has high affinity for thermally conductive filler particles and, conversely, low compatibility with rubber, possessing multiple alcohol groups (alcoholic hydroxyl groups, or functional groups derived from alcoholic hydroxyl groups), and that does not produce unwanted side reactions during rubber curing. Specifically, the following are examples: ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), propylene glycol (PG), glycerin (GLC), etc. These flocculants can be used individually or in combination.
[0043] The thermal conductivity of the elastic layer in the thickness direction is 0.40 W / mK or higher. This range ensures good adhesion. The measurement method is shown below.
[0044] <Method for measuring the thermal conductivity in the thickness direction of an elastic layer> The thermal conductivity λ in the thickness direction of the elastic layer is calculated using the following formula. λ = α × Cp × ρ In the formula, λ is the thermal conductivity in the thickness direction of the elastic layer (W / (m·K)), and α is the thermal diffusivity in the thickness direction (m 2 / s), Cp is constant-pressure specific heat (J / (kg·K)), ρ is density (kg / m³). 3 ) Here, the values of the thermal diffusivity α in the thickness direction, the specific heat at constant pressure Cp, and the density ρ are determined by the following method.
[0045] ·Thermal diffusivity α The thermal diffusivity α in the thickness direction of the elastic layer is measured at room temperature (25°C) using a periodic heating method thermophysical property measuring device (product name: FTC-1, manufactured by Advance Riko Co., Ltd.). Five rectangular sample pieces measuring 8 mm × 12 mm are cut from the elastic layer using a cutter, and the thickness of each sample piece is measured using a digital length measuring device (product name: DIGIMICRO® MF-501 flat measuring probe φ4 mm; manufactured by Nikon Corporation). Next, the thermal diffusivity α is measured five times for each sample piece using the periodic heating method thermophysical property measuring device, and the average value (m 2 The time ( / s) is calculated. The measurement is performed while applying pressure to the sample piece using a 1 kg weight.
[0046] • Constant pressure specific heat CP The constant-pressure specific heat of the elastic layer is measured using a differential scanning calorimetry system (product name: DSC823e, manufactured by Mettler-Toledo Co., Ltd.). Specifically, aluminum pans are used as the sample pan and the reference pan. First, as a blank measurement, both pans are kept at a constant temperature of 15°C for 10 minutes with no pans inside, then the temperature is increased to 215°C at a rate of 10°C / min, and the pan is kept at a constant temperature of 215°C for another 10 minutes. Next, 10 mg of synthetic sapphire, whose low-pressure specific heat is known, is used as the reference material, and the measurement is performed using the same program. Then, 10 mg of the sample, the same amount as the reference synthetic sapphire, is cut from the elastic layer, placed in the sample pan, and the measurement is performed using the same program. These measurement results are analyzed using the specific heat analysis software attached to the differential scanning calorimetry device, and the constant-pressure specific heat CP at 25°C is calculated from the average value of the five measurement results.
[0047] ·Density ρ The density of the elastic layer is measured using a dry automatic densimeter (product name: Accupic 1330-01, manufactured by Shimadzu Corporation). Specifically, 10 cm 3Using a sample cell, a sample piece is cut from the elastic layer to fill approximately 80% of the cell volume. After measuring the mass of this sample piece, it is placed in the sample cell. This sample cell is then set in the measuring section of the apparatus, and helium is used as the measuring gas. After gas replacement, volume measurements are performed 10 times. For each measurement, the density of the elastic layer is calculated from the mass of the sample piece and the measured volume, and the average value is determined. Based on the above, the constant-pressure specific heat Cp (J / (kg·K)) and density ρ (kg / m³) of the elastic layer, converted to units, are obtained. 3 ), and the measured thermal diffusivity α(m 2 The thermal conductivity λ in the thickness direction of the elastic layer is calculated from ( / s). [Examples]
[0048] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the embodiments of this disclosure are not limited thereto. Unless otherwise specified, commercially available Grade 1 or Special Grade reagents were used.
[0049] <Preparation of Fillers 1-3> Spherical alumina (product name: Alnabeads CB-A30S, manufactured by Showa Denko Corporation) was classified using a sieve to prepare fillers 1-3 having 50% particle size (D50), 5% particle size (D5), and 95% particle size (D95) values as shown in Table 1. For fillers 1-3, measurements and analyses were performed using a Coulter Multisizer III (manufactured by Beckman Coulter) according to the instrument's operating manual, and the 50% particle size (D50), 5% particle size (D5), and 95% particle size (D95) were determined from the particle size distribution.
[0050] [Table 1]
[0051] <Example 1> In this example, a fixing film as shown in Figure 3 was prepared. As the base layer, a substrate made of stainless steel with an endless belt shape, measuring 25 mm in inner diameter, 400 mm in width, and 40 μm in thickness, was prepared. The outer surface of this substrate was treated with a primer. As a raw material for forming the elastic layer, an addition-curing liquid silicone rubber (product name: SE1886, manufactured by Toray Dow Corning Co., Ltd.) without fillers was prepared. To 100 parts by volume of this liquid silicone rubber, 100 parts by volume of filler 2 was added as thermal conductive filler particles, and the mixture was stirred using a universal mixing and stirring machine (Dalton Co., Ltd.). In this way, an addition-curing silicone rubber composition for forming the elastic layer was prepared. These were applied to the outer surface of the above base layer using the ring coating method to form an uncured elastic layer 1 with a thickness of 50 μm.
[0052] Next, 9.0 wt% ethylene glycol was uniformly mixed and stirred with the liquid silicone rubber as a flocculant to prepare a mixture. To 100 parts by volume of the mixture, 100 parts by volume of filler 1 was added as thermal conductive filler particles. These were then applied to the outer surface of the uncured elastic layer 1 using the ring coating method to form an uncured elastic layer 2 with a thickness of 300 μm. The uncured elastic layer 1 and uncured elastic layer 2 were crosslinked by heating at 200°C for 4 hours to form an elastic layer with a thickness of 350 μm.
[0053] The base layer on which the elastic layer was formed was rotated circumferentially at a speed of 20 mm / second, and ultraviolet light was irradiated onto the surface of the elastic layer in an atmospheric environment using an ultraviolet lamp positioned 10 mm away from the surface of the elastic layer. A low-pressure mercury ultraviolet lamp (product name: GLQ500US / 11, manufactured by Toshiba Lighting & Technology Corporation) was used as the ultraviolet lamp, and the integrated light amount at a wavelength of 185 nm on the irradiated surface was 800 mJ / cm². 2 The irradiation was applied in such a manner that it resulted in the following:
[0054] Next, an addition-curing silicone rubber adhesive (product name: SE1819CV, a mixture of equal parts of "liquid A" and "liquid B" manufactured by Toray Dow Corning) was applied to the surface of the elastic layer in a nearly uniform manner to a thickness of approximately 20 μm. Next, a fluororesin tube with a hydrophilic inner surface was placed over the belt, and the belt surface was uniformly rubbed over the fluororesin tube to remove excess adhesive from between the elastic layer and the fluororesin tube. • Fluoropolymer tubing (Product name: 959HP-Plus, manufactured by Mitsui Chemours Fluoroproducts, 20 μm thick, melting point 306°C)
[0055] Then, the base layer, which was covered with an elastic layer and a surface layer, was placed in an electric furnace set to a temperature of 200°C, heated for 1 hour to cure the adhesive and bond the fluororesin tube onto the elastic layer, and both ends were cut to obtain a fixing film with a width of 350 mm. Next, the thermal conductivity in the thickness direction of the elastic layer of the fabricated fixing film and the coefficient of variation of the Voronoi region were determined. Furthermore, hardness uniformity, peel durability, and fixing performance were evaluated based on the following evaluation methods. These results are shown in Table 2.
[0056] <Evaluation of hardness variations> Using a micro rubber hardness tester (MD-1TYPE-C hardness tester, manufactured by Polymer Instruments Co., Ltd.), measurements were taken at three points in total: both ends and the center, located 15 mm to 25 mm from the edge of the fixing film. A total of four measurements were taken at 90° intervals around each point in the circumferential direction. The standard deviation of the 12 rubber hardness measurements obtained was calculated.
[0057] (Evaluation Criteria) Rank A: Standard deviation is less than 2.0°. Rank B: Standard deviation is between 2.0° and less than 3.5°. Rank C: Standard deviation is between 3.5° and less than 5.0°. Rank D: Standard deviation is 5.0° or greater.
[0058] <Evaluation of peeling durability> Using the fixing device shown in Figure 2, the total pressure was set to 300 N, the rotation speed of the pressure roller to 200 mm / s, and the temperature of the outer periphery of the fixing film in contact with the recording material was controlled to 130°C. GF-C081 (manufactured by Nippon Paper Industries Ltd.) was used as the recording material. If the evaluation was A to C, it was determined that the effects of this disclosure were obtained.
[0059] (Evaluation Criteria) Rank A: No delamination between the base layer and the elastic layer was observed even after continuous use up to 900,000 sheets. Rank B: If the number of sheets exceeds 800,000 but falls below 900,000, delamination will occur between the base layer and the elastic layer. Rank C: If the number of sheets exceeds 700,000 but falls below 800,000, delamination will occur between the base layer and the elastic layer. Rank D: If the number of sheets remains below 700,000, delamination will occur between the base layer and the elastic layer.
[0060] <Evaluation of retention> A modified Canon imageRUNNER ADVANCE C5560 digital commercial printer was used as the unfixed image forming apparatus. The modifications included allowing free setting of the fixing temperature, process speed, DC voltage VDC of the developer carrier, charging voltage VD of the electrostatic latent image carrier, and laser power. For image output evaluation, an FFh image (solid image) with the desired image ratio was output, and the VDC, VD, and laser power were adjusted so that the amount of toner on the FFh image on the paper was as desired, and an unfixed image was output under the following conditions.
[0061] FFh is a hexadecimal value representing 256 gradations, where 00h is the first gradation (white area) of the 256 gradations, and FFh is the 256th gradation (solid area). Paper: GF-C081 (81.0g / m 2 (Sold by Canon Marketing Japan Inc.) Toner coverage on paper: 0.70 mg / cm² 2 (Adjusted by the DC voltage VDC of the developer carrier, the charging voltage VD of the electrostatic latent image carrier, and the laser power) Evaluation image: A 2cm x 5cm rectangular solid blue image is placed in the center of the A4 paper shown above.
[0062] Next, using the fixing device shown in Figure 2, the total pressure was set to 300 N, the rotation speed of the pressure roller to 200 mm / s, and the temperature of the outer edge of the fixing film in contact with the recording material was controlled to 130°C. GF-C081 (manufactured by Nippon Paper Industries Ltd.) was used as the recording material. The above unfixed images were passed through five consecutive sheets of paper, and the fixation of the fifth image was evaluated. The percentage decrease in image density was used as the evaluation index for fixation.
[0063] The image density reduction rate is determined using an X-Rite color reflectance densitometer (500 series: manufactured by X-Rite). First, the image density of the central area is measured. Next, 4.9 kPa (50 g / cm³) is applied to the area where the image density was measured. 2 Apply a load and rub the fixed image with Silbon paper (5 back-and-forth motions), then measure the image density again. Then, the percentage decrease in image density before and after friction was calculated using the following formula. The obtained percentage decrease in image density was evaluated according to the following evaluation criteria. Image density reduction rate = (Image density before friction - Image density after friction) / Image density before friction × 100 If the evaluation criteria below result in an A to C rating, it is determined that the effects of this disclosure have been achieved.
[0064] (Evaluation Criteria) Rank A: Image density reduction rate is less than 3% Rank B: Image density reduction rate is 3% or more, but less than 5%. Rank C: Image density reduction rate is 5% or more, but less than 8%. Rank D: Image density reduction rate is 8% or more.
[0065] <Example 2> A fixed film was obtained in the same manner as in Example 1, except that the thickness of the uncured elastic layer 2 was changed to 150 μm. <Example 3> A fixed film was obtained in the same manner as in Example 1, except that the thickness of the uncured elastic layer 2 was changed to 2950 μm.
[0066] <Example 4> The amount of filler 2 was changed from 100 parts by volume to 67 parts by volume. The amount of filler 1 was changed from 100 parts by volume to 67 parts by volume. A fixed film was obtained in the same manner as in Example 1, except that the amount of ethylene glycol was changed from 9.0 wt% to 6.0 wt%.
[0067] <Example 5> The amount of filler 2 was changed from 100 parts by volume to 150 parts by volume. The amount of filler 1 was changed from 100 parts by volume to 150 parts by volume. A fixing film was obtained in the same manner as in Example 1, except that ethylene glycol was not used.
[0068] <Example 6> A fixing film was obtained in the same manner as in Example 1, except that filler 2 was changed to filler 3. <Example 7> A fixing film was obtained in the same manner as in Example 1, except that ethylene glycol was not used.
[0069] <Example 8> The amount of filler 2 was changed from 100 parts by volume to 122 parts by volume. The filler ratio of 1:100 parts by volume was changed to filler ratio 4 (silicon carbide (SiC) powder (product name: GC-1000J, manufactured by Yakushima Electric Co., Ltd.)):122 parts by volume. A fixing film was obtained in the same manner as in Example 1, except that ethylene glycol: 9.0 wt% was changed to glycerin: 6.3 wt%.
[0070] <Example 9> A fixed film was obtained in the same manner as in Example 1, except that the amount of ethylene glycol was changed to 8.6 wt%. <Example 10> A fixed film was obtained in the same manner as in Example 1, except that the amount of ethylene glycol was changed to 3.9 wt%. <Example 11> A fixed film was obtained in the same manner as in Example 1, except that the amount of ethylene glycol was changed to 7.1 wt%.
[0071] <Comparative Example 1> A fixed film was obtained in the same manner as in Example 1, except that the thickness of the uncured elastic layer 2 was changed to 130 μm. <Comparative Example 2> The amount of filler 2 was changed from 100 parts by volume to 54 parts by volume. The amount of filler 1 was changed from 100 parts by volume to 54 parts by volume. A fixed film was obtained in the same manner as in Example 1, except that the amount of ethylene glycol was changed from 9.0 wt% to 4.9 wt%.
[0072] <Comparative Example 3> The amount of filler 2 was changed from 100 parts by volume to 185 parts by volume. The amount of filler 1 was changed from 100 parts by volume to 185 parts by volume. A fixing film was obtained in the same manner as in Example 1, except that ethylene glycol was not used. <Comparative Example 4> A fixing film was obtained in the same manner as in Example 1, except that filler 2 was changed to filler 1.
[0073] <Comparative Example 5> A fixed film was obtained in the same manner as in Example 1, except that filler 2 was changed to filler 3, the thickness of the uncured elastic layer 1 was changed to 350 μm, and the uncured elastic layer 2 was not formed. In Examples 2-11 and Comparative Examples 1-5, the thermal conductivity in the thickness direction of the elastic layer of the fabricated fixing film and the coefficient of variation of the Voronoi region were determined. Furthermore, hardness uniformity, peel durability, and fixing performance were evaluated based on the same evaluation method as in Example 1. These results are shown in Table 2.
[0074] [Table 2]
[0075] This disclosure includes the following components. [Configuration 1] A fixing member comprising at least a base layer having an endless shape, an elastic layer provided on the outer circumferential surface of the base layer, and a surface layer provided on the outer circumferential surface of the elastic layer, The base layer comprises at least one selected from the group consisting of aluminum, iron, copper, nickel, stainless steel, brass, polyimide, polyamide-imide, and polyetheretherketone. The elastic layer comprises rubber and heat-conducting filler particles dispersed in the rubber. The thickness of the elastic layer is 200 μm or more. The content of the thermal conductive filler particles in the elastic layer is 40% by volume or more and 60% by volume or less. In a cross-section of the elastic layer in a direction perpendicular to the circumferential direction, Region A is defined as the region from the interface between the base layer and the elastic layer to a thickness of 50 μm in the thickness direction of the elastic layer. The arithmetic mean of the areas of each Voronoi region formed by Voronoi tessellation using the heat-conducting filler particles exposed in region A of the cross-section as the parent point is A. ave Let Aσ be the standard deviation, and let Av be the coefficient of variation calculated by the following formula. The arithmetic mean of the coefficient of variation Av is Av ave In that case, Arithmetic mean of coefficient of variation (Av) ave A fixing member characterized by having a value of 1.2 or less: Av=(Aσ / A ave ). [Configuration 2] The arithmetic mean of the areas of each Voronoi region formed by Voronoi tessellation using the heat-conducting filler particles exposed in region B other than region A of the cross-section as the parent point is B. ave Let Bσ be the standard deviation, and let Bv be the coefficient of variation calculated by the following formula. The arithmetic mean of the coefficient of variation Bv is Bv ave In this case, the arithmetic mean of the coefficient of variation is Bv ave The fixing member described in configuration 1, wherein the value is 1.5 or more and 4.0 or less: Bv=(Bσ / B ave ). [Configuration 3] A thermal fixing apparatus comprising a fixing member as described in configuration 1 or 2, and a pressurizing member disposed opposite to the fixing member. [Explanation of Symbols]
[0076] 10: Image forming unit 11: Photosensitive drum 12: Charger 13: Laser Scanner 14: Developer 15: Cleaner 17: Primary transfer blade 20: Paper feed cassette 25: Multi-purpose paper tray 23: Resistola vs. 31: Intermediate transfer belt 35: Secondary transfer roller 40: Fuser 41: Fixing film 41a: Surface layer 41b: Base layer 41c: Elastic layer 43: Heating body 44: Pressure roller 45: Contact type thermistor 46: Heater holder P: Recording material T: Toner 401-1: 1st cross section 401-2:Second cross section 402: Cross-section 403: Area A 404: Area B 404-1: Area B1 404-2: Area B2 404-3: Area B3 61: Filler particles A: Center of gravity F: Intersection
Claims
1. A fixing member comprising at least a base layer having an endless shape, an elastic layer provided on the outer circumferential surface of the base layer, and a surface layer provided on the outer circumferential surface of the elastic layer, The base layer comprises at least one selected from the group consisting of aluminum, iron, copper, nickel, stainless steel, brass, polyimide, polyamide-imide, and polyetheretherketone. The elastic layer comprises rubber and heat-conducting filler particles dispersed in the rubber. The thickness of the elastic layer is 200 μm or more. The thermal conductivity of the elastic layer in the thickness direction is 0.40 W / mK or higher. The content of the thermal conductive filler particles in the elastic layer is 40% by volume or more and 60% by volume or less. In a cross-section perpendicular to the circumferential direction of the elastic layer, the region from the interface between the base layer and the elastic layer to a thickness of 50 μm in the thickness direction of the elastic layer is defined as region A, and the arithmetic mean of the areas of each Voronoi region formed by Voronoi tessellation using the heat-conducting filler particles exposed in region A of the cross-section as the parent points is defined as A. ave Let Aσ be the standard deviation, let Av be the coefficient of variation calculated by the following formula (1), and let Av be the arithmetic mean of the coefficient of variation Av. ave In this case, the arithmetic mean of the coefficient of variation is Av. ave The fixing member is characterized in that when the coefficient of variation is 1.2 or less, and the arithmetic mean of the areas of each Voronoi region formed by Voronoi tessellation using the heat-conducting filler particles exposed in region B other than region A of the cross-section as the parent point is Bave, the standard deviation is Bσ, the coefficient of variation calculated by the following formula (2) is Bv, and the arithmetic mean of the coefficient of variation Bvave is Bv, then the arithmetic mean of the coefficient of variation Bvave is 1.5 or more and 4.0 or less: A=(Aσ / A) ave )(1) Bv=(Bσ / B ave ) (2).
2. A thermal fixing apparatus characterized by comprising a fixing member as described in claim 1 and a pressing member disposed opposite to the fixing member.
Citation Information
Patent Citations
JP1975054924A
Fixing member
JP2007219371A
Heating rotating body and image heating device equipped with the same
JP2009300593A
Fixing belt
JP2011186127A