Sound-absorbing structure construction method, laminate, method for manufacturing laminate, sound-absorbing material

The laminate construction method using a hot-melt resin with controlled viscosity and thermoplastic resin components addresses the performance gaps in conventional sound-absorbing materials, achieving superior sound absorption and ease of application on complex surfaces.

JP7955103B2Active Publication Date: 2026-11-24INOAC TECHN CENT
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022137300
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-27
Filing Date
2022-08-30
Publication Date
2026-11-24
Estimated Expiration
2042-08-30

AI Technical Summary

Technical Problem

Conventional sound-absorbing materials and construction methods do not meet sufficient performance requirements.

Method used

A laminate is formed by spray-coating a target object with a hot-melt resin in a molten state having a melt viscosity of 200,000 mPa·s or less to create a resin fiber layer, which is then fused onto a base material, using specific thermoplastic resin components and conditions to enhance sound absorption and adhesion.

Benefits of technology

The method provides a sound-absorbing structure with excellent performance, enabling effective sound absorption and ease of application on complex shapes without peeling, while maintaining sound absorption properties over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955103000003
    Figure 0007955103000003
  • Figure 0007955103000001
    Figure 0007955103000001
  • Figure 0007955103000002
    Figure 0007955103000002
Patent Text Reader

Abstract

To provide a sound absorption structure construction method having superior performance, a laminate, a method of manufacturing the laminate, and a sound absorber.SOLUTION: A sound absorption structure construction method is a method that uses a base material of a laminate as an object to be given sound absorbency in a method of manufacturing the laminate, and comprises spraying and applying hot-melt resin of 200,000 mPa s or less in melt viscosity at 180°C on the object or base material to form a resin fiber layer as a sound absorber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a method for constructing a sound-absorbing structure, a laminate, a method for manufacturing a laminate, and a sound-absorbing material. [Background technology]

[0002] Automobiles are designed with sound-absorbing materials placed in various locations to suppress noise (external noise and noise caused by vibrations during driving).

[0003] For example, Patent Document 1 discloses a technology for using a nonwoven web as a sound-absorbing material. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2017-160575 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] However, conventional sound-absorbing materials and construction methods for sound-absorbing structures did not meet sufficient performance requirements.

[0006] Therefore, the object of the present invention is to provide a method for constructing a sound-absorbing structure with excellent performance.

[0007] Furthermore, the present invention aims to provide a laminate that is preferably usable as a sound-absorbing material, a method for manufacturing the laminate, and a sound-absorbing material. [Means for solving the problem]

[0008] The inventors of this invention have conducted diligent research and discovered that the above problem can be solved by a laminate having a structure (layer) formed from specific components, and have completed the present invention. That is, the present invention is as follows.

[0009] One aspect of the present invention provides a sound-absorbing structure construction method, characterized by spray-coating a target object with a hot-melt resin in a molten state having a melt viscosity at 180°C of 200,000 mPa·s or less, to form a resin fiber layer serving as a sound-absorbing material.

[0010] Further, another aspect of the present invention provides a method for producing a laminate including a base material and a resin fiber layer, the method including a step of spray-coating the base material with a hot-melt resin in a molten state having a melt viscosity at 180°C of 200,000 mPa·s or less, to form the resin fiber layer. The resin fiber layer may be a sound-absorbing material.

[0011] Further, another aspect of the present invention provides a sound-absorbing material including a resin fiber layer formed of a hot-melt resin having a melt viscosity at 180°C of 200,000 mPa·s or less.

[0012] Further, another aspect of the present invention provides a laminate including: a resin fiber layer formed of a hot-melt resin having a melt viscosity at 180°C of 200,000 mPa·s or less; and a base material, wherein the resin fiber layer is fused onto the base material. [[Effects of the Invention]]

[0013] According to the present invention, it is possible to provide a sound-absorbing structure construction method having excellent performance.

[0014] Further, according to the present invention, it is possible to provide a laminate that can be preferably used as a sound-absorbing material, a method for producing the laminate, and a sound-absorbing material. [[Brief Description of the Drawings]]

[0015] [Figure 1] It is a conceptual side view of the laminate according to the present embodiment. [Modes for carrying out the invention]

[0016] The following will specifically describe laminates suitable for use as sound-absorbing materials, as well as methods for manufacturing laminates and constructing sound-absorbing structures, but the present invention is not limited to these.

[0017] In this specification, if multiple upper limits and multiple lower limits are described separately, all numerical ranges that can be set by freely combining these upper and lower limits are described herein.

[0018] <<<<Laminate>>>> The laminate according to this embodiment comprises a resin fiber layer and a substrate (see Figure 1).

[0019] <<<Resin fiber layer>>> <<Ingredients>> The resin fiber layer is a fibrous structure formed from hot-melt resin (also called hot-melt adhesive). The resin fiber layer (hot-melt resin) is fixed to the substrate by fusing it onto the substrate.

[0020] Hot melt resin primarily contains thermoplastic resin components. It may also contain other components.

[0021] <Thermoplastic resin component> Examples of thermoplastic resin components that make up the hot melt resin of the resin fiber layer include polyolefins, polyesters, polyurethanes, polyamides, and polyvinyl alcohols.

[0022] The thermoplastic resin component can be selected considering its compatibility with the material of the substrate (object). For example, if the substrate is a polyolefin such as polypropylene, including polyolefin in the thermoplastic resin component can increase the bonding strength between the substrate and the fibrous structure.

[0023] From the viewpoint of improving the sound absorption effect and workability of the fiber structure, it is preferable that the thermoplastic resin component be polyolefin.

[0024] Examples of polyolefins include polyethylene, polypropylene, polybutene-1, ethylene-propylene copolymers, ethylene-α-olefin copolymers, and polymer blends thereof.

[0025] From the viewpoint of improving sound absorption and adhesion to the substrate, the polyolefin is preferably poly-αolefin, and more preferably amorphous poly-αolefin.

[0026] Poly-α-olefins refer to polymers obtained by polymerizing α-olefins. Amorphous poly-α-olefins, on the other hand, refer to poly-α-olefins that do not have a clearly defined melting point.

[0027] Amorphous poly-α-olefins can be those that are known, such as those described in Japanese Patent Publication No. 6001685 and Japanese Patent Publication No. 3153648. Amorphous poly-α-olefins can be, for example, amorphous olefin resins obtained by polymerizing (or copolymerizing) propylene, ethylene, and 1-butene individually or in combination.

[0028] <Other ingredients> Other known additives include tackifiers, plasticizers, fillers, pigments, dyes, antioxidants, antioxidants, antistatic agents, flame retardants, antibacterial agents, light stabilizers, stabilizers, dispersants, solvents, and hydrophilicity-imparting agents.

[0029] Other components may be present in amounts of, for example, 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, 5 parts by mass or less, 1 part by mass or less, or 0.1 parts by mass or less per 100 parts by mass of hot melt resin.

[0030] <<<Physical properties / properties>>> <<Melting viscosity>> The melt viscosity of the hot-melt resin constituting the resin fiber layer at 180°C is preferably 200,000 mPa·s or less, 100,000 mPa·s or less, 50,000 mPa·s or less, 20,000 mPa·s or less, 15,000 mPa·s or less, or 10,000 mPa·s or less. Furthermore, the melt viscosity of the hot melt resin at 180°C is preferably 1,000 mPa·s or more, 2,000 mPa·s or more, or 5,000 mPa·s or more.

[0031] The melt viscosity of the hot-melt resin constituting the resin fiber layer at 200°C is preferably 100,000 mPa·s or less, 50,000 mPa·s or less, 25,000 mPa·s or less, 15,000 mPa·s or less, or 10,000 mPa·s or less. Furthermore, the melt viscosity of the hot melt resin at 200°C is preferably 500 mPa·s or higher, 1,000 mPa·s or higher, 1,500 mPa·s or higher, or 3,000 mPa·s or higher.

[0032] By setting the melt viscosity of the hot melt resin within this range, spray application of the hot melt resin becomes easy, and a resin fiber layer with excellent sound absorption properties can be easily obtained.

[0033] The melt viscosity was measured using a parallel plate rheometer with a swing angle of 10% and an angular frequency of 1 rad / s for a hot melt resin heated to a predetermined temperature.

[0034] <<Crystallization Temperature / Crystallization Energy>> The crystallization temperature of the hot-melt resin constituting the resin fiber layer is preferably 50-150°C, 75-125°C, or 90-110°C. By setting the temperature within this range, it is possible to achieve a good balance of ease of workability, sound absorption, and other properties.

[0035] The crystallization energy (heat of crystallization) of the hot melt resin is preferably 0.1 to 50 mJ / mg, 0.5 to 25 mJ / mg, or 5 to 15 mJ / mg. By setting it within this range, it is possible to achieve a good balance of ease of workability, sound absorption, and other properties.

[0036] Furthermore, from the viewpoint of achieving a good balance in terms of sound absorption and shape retention (for example, the thickness reduction rate described later), the crystallization energy (heat of crystallization) of the hot melt resin is preferably 0.1 to 150 mJ / mg, 20 to 140 mJ / mg, 50 to 130 mJ / mg, or 60 to 120 mJ / mg.

[0037] The crystallization temperature and crystallization energy shall be measured in accordance with JIS K 7121.

[0038] <<Storage modulus, loss modulus, loss tangent, glass transition temperature>> The lower limit of the storage modulus G' of the hot melt resin is preferably 10 MPa or more, 20 MPa or more, 50 MPa or more, 75 MPa or more, 90 MPa or more, 100 MPa or more, 200 MPa or more, or 500 MPa or more. The upper limit of the storage modulus G' of the hot melt resin is, for example, 2000 MPa or less, 1500 MPa or less, 1000 MPa or less, or 750 MPa or less.

[0039] The loss modulus G'' of the hot melt resin is preferably 50 MPa or less, or 40 MPa or less.

[0040] The loss tangent tanδ (loss modulus G'' / storage modulus G') of the hot melt resin is preferably 1.00 or less, or 0.50 or less.

[0041] The hot melt resin preferably has a glass transition temperature of -30 to 60°C or -25 to 40°C.

[0042] The storage modulus G' and the loss modulus G'' are measured as follows. Measurement method: rheometer Device name: MCR302 (Anton Paar) Amplitude: 0.8° Frequency: 10 Hz Deformation mode: shear mode Temperature: -50 to 110°C Sample size: width 5 mm × length 20 mm × thickness 1 mm The storage modulus G' and loss modulus G'' are values at 23°C.

[0043] The temperature corresponding to the peak value of the loss tangent tanδ described above is defined as the glass transition temperature.

[0044] By setting the storage modulus G', loss modulus G'', loss tangent tanδ, or glass transition temperature of the hot melt resin within such ranges, it is easy to obtain a resin fiber layer excellent in sound absorption, shape retention, workability, and the like. In particular, by setting the storage modulus G' of the hot melt resin within such a range, it is easy to obtain a resin fiber layer that has high sound absorption and is extremely excellent in shape retention.

[0045] <<Air permeability>> The air permeability of the resin fiber layer is 10.0 cm 3 / cm 2 / s or more, 15.0 cm 3 / cm 2 / s or more, 20.0 cm 3 / cm 2 / s or more, 30.0 cm 3 / cm 2 / s or more, 40.0 cm 3 / cm 2 / s or more, 50.0 cm 3 / cm 2 / s or more, 52.5 cm 3 / cm 2 / s or more, or 55.0 cm 3 / cm 2 / s or more is preferable. Further, the air permeability of the resin fiber layer is 200 cm 3 / cm 2 / s or less, 150 cm 3 / cm2 / s or less, 100cm 3 / cm 2 / s or less, 95.0cm 3 / cm 2 / s or less, 85.0cm 3 / cm 2 / s or less, or 80.0cm 3 / cm 2 It is preferable that the value be less than or equal to / s. By setting the air permeability of the resin fiber layer within this range, excellent sound absorption effects can be obtained.

[0046] In particular, in a resin fiber layer formed by hot-melt resin, by using fibers with a preferred fiber diameter while maintaining the air permeability within this range, the distribution of voids and fibers becomes appropriate, resulting in a very excellent sound absorption effect.

[0047] The air permeability of the resin fiber layer was measured according to the air permeability test specified in JIS L 1096.

[0048] Furthermore, if the resin fiber layer is bonded to the substrate, the air permeability of the resin fiber layer can be measured by forming an identical resin fiber layer (a resin fiber layer with the same composition, structure, thickness, etc.) on a release film, removing the release film to produce a single layer of resin fiber, and then measuring the value of this resin fiber layer.

[0049] <<<structure>>> <<Fiber diameter>> The fiber diameter of the fibers constituting the resin fiber layer can be, for example, 1-100 μm, 5-50 μm, or 10-40 μm. When the fiber diameter is within this range, excellent sound absorption effects can be obtained. The method for calculating the fiber diameter is as follows: First, the resin fiber layer is photographed with a scanning electron microscope (SEM), and the fiber diameter (width along the short axis) of 10 fibers included in the obtained image is measured and averaged to determine the fiber diameter.

[0050] <<Thickness>> The thickness of the resin fiber layer can be, for example, 0.1 to 500 mm, 1 to 100 mm, 5 to 50 mm, or 10 to 30 mm. By setting the thickness of the resin fiber layer within this range, excellent sound absorption can be obtained while maintaining ease of manufacturing.

[0051] The reduction in thickness of the resin fiber layer is preferably 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less. When the reduction in thickness of the resin fiber layer falls within these ranges, high sound absorption is more easily achieved over a long period of time. Here, the thickness reduction rate of the resin fiber layer is measured by the following method. The thickness of the resin fiber layer immediately after manufacturing (provided that the hot melt resin has fully solidified) is defined as the initial thickness T. A Let's assume that. The thickness of the resin fiber layer after being held under constant temperature and humidity conditions (25°C, 50%RH) for one week (168 hours) is defined as the post-holding thickness T. B Let's assume that. The thickness reduction rate is [(T A -T B ) / T A It is calculated as ].

[0052] Furthermore, when a resin fiber layer is used as a sound-absorbing material, the frequency range that is easily absorbed changes depending on the thickness of the resin fiber layer (for example, increasing the thickness of the resin fiber layer shifts the peak of the sound absorption frequency to the lower frequency side). Therefore, it is possible to adjust the thickness of the resin fiber layer according to its intended use (the environment in which it is used).

[0053] <<Inspection>> The basis weight of the resin fiber layer is, for example, 100 to 2,000 g / m². 2 200-1,000 g / m 2 , or 300-750g / m 2 This can be achieved. By setting the basis weight of the resin fiber layer within this range, excellent sound absorption effects can be obtained.

[0054] Fiber diameter, basis weight, thickness, air permeability, etc., can be adjusted by the melt viscosity of the hot melt resin, the type of nozzle used when spraying the hot melt resin, and the spray application conditions (pressure, time, etc.).

[0055] The resin fiber layer according to this embodiment has excellent sound absorption properties and can therefore be preferably used as a sound-absorbing material.

[0056] <<<Base material>>> The shape of the base material is not particularly limited, and any suitable shape can be used. In particular, since the resin fiber layer according to this embodiment can be formed simply by spray-coating hot-melt resin, it is possible to provide excellent sound absorption even when using a base material with a complex shape (such as a member with a bent portion).

[0057] Furthermore, the material of the base material is not particularly limited, and any suitable material can be used. For example, the base material may be a composite of two or more materials (e.g., resin and metal).

[0058] << The following describes the manufacturing method of the laminate and the method for constructing the sound-absorbing structure. Note that in the manufacturing method of the laminate, a method in which the base material of the laminate is the object to which sound absorption properties are to be imparted can be considered the method for constructing the sound-absorbing structure.

[0059] The laminate is obtained by directly spray-coating a hot-melt resin, held in a molten state, onto a substrate. The hot-melt resin, which has become fibrous due to the spray coating, comes into contact with the substrate in a molten or softened state and fuses with the substrate. As the hot-melt resin cools and solidifies, a resin fiber layer is formed.

[0060] As for the spraying method, known methods such as curtain spray, omega spray, spiral spray, summit spray, etc., can be applied.

[0061] The hot melt resin used for spray coating can be manufactured by known methods. For example, the aforementioned raw materials can be put into a continuous mixer such as a single-screw or twin-screw extruder, or a batch mixer such as a roll mixer, Banbury mixer, kneader, planetary mixer, or high-shear Z-wing mixer, and mixed at a predetermined temperature for a predetermined time.

[0062] Surface treatment (such as cleaning, smoothing, roughening, electrical discharge treatment, or UV treatment) may be performed on the substrate for purposes such as increasing the bonding strength of the resin fiber layer to the substrate.

[0063] According to the manufacturing method of the laminate and the sound-absorbing structure construction method of this embodiment, unlike the case in which a laminate is manufactured by heat welding fiber sheets, there is no need to perform heat treatment or the like after the resin layer fibers are formed.

[0064] In conventional techniques, where fiber sheets made of thermoplastic resin are laminated onto a substrate and the layers are bonded by applying heat and pressure, the fiber structure is crushed by the heat and pressure, making it difficult to obtain the desired sound absorption effect.

[0065] Furthermore, when fiber sheets are joined to a substrate in a spot manner using adhesives or heat welding, the fiber structure is crushed at the joint, making it impossible to obtain the desired sound absorption effect, and delamination is prone to occur in the non-jointed areas.

[0066] Furthermore, these methods involve not only the process of laminating the resin fiber layer onto the substrate by predetermined means, but also processes such as die-cutting to shape the fiber sheet to suit the substrate, making the work complicated, and the sound absorption performance decreases due to the sagging of the fiber sheet during storage.

[0067] According to the sound-absorbing structure construction method of this embodiment, construction is completed by only a simple process of spraying hot melt resin onto a substrate to form a resin fiber layer, and the hot melt resin itself has the function of adhering to the substrate (there is no need for the process of heating and welding the nonwoven fabric or the process of applying adhesive to the nonwoven fabric). Therefore, a resin fiber layer with excellent sound absorption properties derived from the hot melt resin can be easily formed, and peeling is unlikely to occur because the resin fiber layer is uniformly adhered to the surface.

[0068] Here, we will further compare the method for manufacturing a laminate or constructing a sound-absorbing structure according to this embodiment with the conventional method for constructing a sound-absorbing structure disclosed in Japanese Patent Application Publication No. 2017-160575, etc. (a method for constructing a sound-absorbing structure that uses a nonwoven fabric web formed by the meltblown method as a sound-absorbing material). The meltblown method described in Japanese Patent Publication No. 2017-160575 requires an accumulation device to collect the sprayed resin fibers after spraying. Such an accumulation device generally includes a suction device consisting of a rotating roll or belt conveyor with holes to prevent scattering. The method for manufacturing a laminate or constructing a sound-absorbing structure according to this embodiment can be carried out using only simple equipment, without the use of accumulation devices or suction devices. Furthermore, by not using accumulation devices or suction devices, the sound-absorbing material can be directly applied to the target object to obtain a laminate. Therefore, it becomes possible to directly apply the material to complex shapes (e.g., 3D shapes) by, for example, attaching a spray nozzle to the tip of a robot arm.

[0069] As mentioned above, the laminate obtained by spray-coating hot-melt resin onto a substrate according to this embodiment and the laminate obtained by spot-welding a pre-prepared fiber sheet to a substrate are thought to have different bonding areas.

[0070] More specifically, in the laminate according to this embodiment, the adhesive area of ​​the resin fiber layer to the substrate is 50% or more, 60% or more, 70% or more, or 80% or more. The adhesive area of ​​the resin fiber layer to the substrate can be, for example, 99% or less, 95% or less, or 90% or less. In the laminate according to this embodiment, the substrate and the resin fiber layer are sufficiently bonded while maintaining the fiber structure, and excellent sound absorption properties can be exhibited.

[0071] On the other hand, laminates obtained by spot welding fiber sheets typically have a bonding area of ​​1% or less of the fiber sheets, making them easily peeled off and making it difficult to exhibit excellent sound absorption.

[0072] The adhesive area of ​​the resin fiber layer can be calculated by peeling off the fibers other than those in the adhesive area from the substrate and analyzing the adhesive area (the part remaining after peeling off the fibers) using a microscope.

[0073] The application location (the location to which the resin fiber layer is applied or the base material of the laminate) of the sound-absorbing structure construction method according to this embodiment is not particularly limited and can be any location where sound absorption is required. For example, it can be applied to interior and exterior components of vehicles such as airplanes, ships, and automobiles (rail cars), in addition to buildings.

[0074] In particular, the sound-absorbing structure construction method according to this embodiment can impart sound absorption to members with complex shapes, is less prone to peeling due to vibration, and has good workability. Therefore, the resin fiber layer obtained by the sound-absorbing structure construction method can be suitably applied to components that make up an automobile (pillars, deck sides, floor silencers, back door trims, etc.). [Examples]

[0075] The laminates of the present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0076] <<Manufacturing of laminates / resin fiber layers>> The following materials were used as the hot-melt resins that make up the resin fiber layer. VESTOPLAST 807 (manufactured by Evonik, poly-alpha-olefin) PES120L (manufactured by Toagosei Co., Ltd., polyester) PPET (Polyolefin, manufactured by Toagosei Co., Ltd.) Diabond DH-672 (manufactured by Diabond, polyamide) PP (manufactured by Tosho Chemical Co., Ltd., polypropylene, MFR: 1500g / 10min) PP (Xiamen Keyuan Plastic Co., Ltd., polypropylene, MFR: 1500g / 10min)

[0077] A hot-melt resin, held at 180°C and molten, was spray-coated onto a polypropylene (PP) substrate, and the hot-melt resin was cooled and solidified at room temperature to obtain laminates according to Examples 1 to 5, comprising the substrate and a resin fiber layer.

[0078] The table shows the composition (hot melt resin), thickness, basis weight, fiber diameter, air permeability, storage modulus G', loss modulus G'', loss tangent tanδ, and glass transition temperature of the resin fiber layer in each example. SEM images of the fibers in the resin fiber layer for each example are also shown in each table. The thickness, basis weight, fiber diameter, and air permeability of the resin fiber layer were adjusted by changing the spray application conditions (application time) and nozzle diameter. The thickness of the resin fiber layer is determined according to the method described above, with an initial thickness T. A And, thickness T after holding B The following measurements were taken, and the thickness reduction rate was calculated accordingly.

[0079] Comparative Example 1 was a single layer consisting only of the base material, without the resin fiber layer.

[0080] <<Rating>> For each laminate in Examples 1 to 5, the adhesion between the substrate and the resin fiber layer and the sound absorption coefficient were evaluated. The sound absorption coefficient of Comparative Example 1 was also evaluated.

[0081] <Adhesion between the base material and the resin fiber layer (adhesion to PP)> The fibers (hot melt resin) other than the adhesive portion were peeled off the substrate, and the area of ​​the adhesive portion (the part remaining after peeling off the fibers) was calculated using a microscope and evaluated as follows. A: Adhesion area of ​​80% or more B: Adhesion area is 50% or more but less than 80% C: Adhesion area is 10% or more but less than 50% D: Bonding area is less than 10%

[0082] <Sound absorption coefficient> In accordance with JIS A 1405-2, the sound absorption coefficient was measured as the average value for n=2, with a sample size of 28.9φ, incident surface: fiber surface, target frequency: 4000Hz, and evaluated as follows. A: 0.6 or more and 1.0 or less B: 0.5 or higher, less than 0.6 C: 0.1 or greater, less than 0.5 D: Less than 0.1

[0083] [Table 1]

[0084] [Table 2]

[0085] From the above results, it can be understood that the laminates comprising the resin fiber layer according to each embodiment have excellent sound absorption properties. Furthermore, since this resin fiber layer with excellent sound absorption properties is obtained simply by spraying molten hot melt resin onto the object, it can be understood that this is a sound-absorbing structure construction method with excellent workability.

Claims

1. A sound-absorbing structure construction method characterized by spray-coating a hot-melt resin in a molten state, having a melt viscosity of 200,000 mPa·s or less at 180°C, onto a target object to form a resin fiber layer that is a sound-absorbing material, The thickness of the aforementioned resin fiber layer is 1 mm or more. A method for constructing a sound-absorbing structure, wherein the basis weight of the resin fiber layer is 200 g / m² or more.

2. The sound-absorbing structure construction method according to Claim 1, satisfying (A) and / or (B) below. (A) The object in question is a location where sound absorption is required. (B) The object is made of metal.

3. A method for manufacturing a laminate comprising a base material and a resin fiber layer, A method for manufacturing a laminate, characterized by including the step of spray-coating a molten hot-melt resin having a melt viscosity of 200,000 mPa·s or less at 180°C onto the substrate to form the resin fiber layer, The thickness of the aforementioned resin fiber layer is 1 mm or more. A method for manufacturing a laminate, wherein the basis weight of the resin fiber layer is 200 g / m² or more.

4. A method for manufacturing a laminate according to claim 3, satisfying one or more of the following (A) to (C). (A) The substrate is a location where sound absorption is required. (B) The base material is a metal. (C) The base material is a member having a bent portion.

5. The method for manufacturing a laminate according to claim 3, wherein the resin fiber layer is a sound-absorbing material.

6. A sound-absorbing material characterized by comprising a resin fiber layer formed from a hot-melt resin having a melt viscosity of 200,000 mPa·s or less at 180°C, The thickness of the aforementioned resin fiber layer is 1 mm or more. The basis weight of the resin fiber layer is 200 g / m² or more. A sound-absorbing material that satisfies the following conditions (1) and / or (2). (1) The melt viscosity of the hot melt resin at 200°C is 11,800 mPa·s or more. (2) The fiber diameter of the fibers constituting the resin fiber layer is 10 μm or more.

7. The material comprises a resin fiber layer formed from a hot-melt resin having a melt viscosity of 200,000 mPa·s or less at 180°C, and a base material. A laminate characterized in that the resin fiber layer is fused onto the substrate, The thickness of the aforementioned resin fiber layer is 1 mm or more. The basis weight of the resin fiber layer is 200 g / m² or more. A laminate that satisfies (A) and / or (C) below, and satisfies one or more of (1) to (4) below. (A) The substrate is required to absorb sound. (C) The base material is a member having a bent portion. (1) The melt viscosity of the hot melt resin at 200°C is 11,800 mPa·s or more. (2) The fiber diameter of the fibers constituting the resin fiber layer is 10 μm or more. (3) The adhesive area of ​​the resin fiber layer to the substrate is 50% or more. (4) The base material is made of polyolefin, and the hot melt resin is made of polyolefin.

8. A resin fiber layer formed from a hot melt resin having a melt viscosity of 200,000 mPa·s or less at 180°C, and a metal substrate, The thickness of the aforementioned resin fiber layer is 1 mm or more. The basis weight of the resin fiber layer is 200 g / m² or more. A laminate characterized in that the resin fiber layer is fused onto the substrate.

Citation Information

Patent Citations

  • Sound absorbing material component, sound absorbing material and manufacturing method of sound absorbing material

    JP2010064361A

  • Vehicle component

    JP2017160575A

  • Laminate and sound absorbing material using the same

    JP2019193980A

  • Sound-absorbing material, sound-absorbing panel in which same is used, and method for manufacturing sound-absorbing material