Nickel self-fluxing alloy and its powder, and a component coated therewith
A nickel self-fluxing alloy with controlled composition and particle size addresses the inadequacies of existing materials by providing robust hydrochloric acid corrosion and wear resistance, suitable for large-scale applications.
Patent Information
- Application Number
- JP2022161405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-06
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-06
AI Technical Summary
Existing materials and methods for providing hydrochloric acid corrosion resistance and wear resistance are inadequate, especially in severe environments, and existing coating methods are limited to small areas due to sintering requirements.
A nickel self-fluxing alloy composition with specific mass percentages of Mo, B, Si, Cr, Cu, Fe, Nb, and C, combined with a particle size distribution of 45 to 106 μm, applied through thermal spraying and fusing, to form a dense coating with enhanced corrosion and wear resistance.
The alloy provides high resistance to hydrochloric acid corrosion and wear, suitable for large areas, with improved adhesion and durability in harsh environments.
Smart Images

Figure 0007955125000005 
Figure 0007955125000006 
Figure 0007955125000001
Abstract
Description
Technical Field
[0001] The present invention relates to surface modification materials used in various construction processes employing powders, such as flame spraying, high-velocity flame spraying, plasma spraying, and plasma powder overlay welding. In particular, the present invention relates to nickel self-fluxing alloys used for components requiring durability in hydrochloric acid corrosion environments and wear resistance, powders thereof, and components coated therewith.
Background Art
[0002] Conventionally, for parts requiring corrosion resistance against halogen-based corrosive environments such as hydrochloric acid, bulk materials of Ni-Cu-based alloys (MONEL (registered trademark)), Ni-Mo-Cr-based alloys (HASTELLOY (registered trademark)), or Ni-Cr-Mo-based alloys (INCONEL (registered trademark)) have been used, or overlay members obtained by cladding steel materials with these alloys have been used. For example, Patent Document 1 can be cited.
[0003] However, when bulk materials of Ni-Cu-based alloys, Ni-Mo-Cr-based alloys, or Ni-Cr-Mo-based alloys are used as they are, the product cost becomes high, and satisfactory durability may not be obtained in environments with severe wear. In addition, when overlay members made of Ni-Cu-based alloys, Ni-Mo-Cr-based alloys, or Ni-Cr-Mo-based alloys are used, the overlay member is diluted by the penetration of molten steel, resulting in reduced corrosion resistance and, similar to bulk materials, poor wear resistance.
[0004] Therefore, for imparting hydrochloric acid corrosion resistance and wear resistance, for example, high-Mo-based alloys described in Patent Documents 2 to 6 have been applied or studied for coating on the surface of steel materials or the like by thermal spraying or overlay welding. Although hydrochloric acid corrosion resistance is not described, Patent Documents 7 to 12 list alloy compositions similar to those in Patent Documents 2 to 6.
[0005] Although not thermal spray or overlay materials, Patent Documents 13 to 17 and the like can be cited as high-Mo-based sintered materials.
Prior Art Documents
[0006] [Patent Document 1] Patent No. 6918114 [Patent Document 2] Japanese Patent Publication No. 2000-45058 [Patent Document 3] Patent No. 3987129 [Patent Document 4] Patent No. 5855357 [Patent Document 5] Japanese Patent Publication No. 2004-263260 [Patent Document 6] Japanese Patent Publication No. 2014-111265 [Patent Document 7] Japanese Patent Publication No. 2008-291300 [Patent Document 8] Patent No. 2628317 [Patent Document 9] Patent No. 3430498 [Patent Document 10] Patent No. 4762583 [Patent Document 11] Japanese Patent Application Publication No. 9-31576 [Patent Document 12] Japanese Patent Publication No. 2000-239860 [Patent Document 13] Japanese Patent Application Publication No. 1-79338 [Patent Document 14] Patent No. 2995597 [Patent Document 15] Japanese Patent Publication No. 2003-155527 [Patent Document 16] WO2013-058074 publication [Patent Document 17] Patent No. 4121694 [Overview of the Initiative] [Problems that the invention aims to solve]
[0007] However, in recent years, operating environments have become more severe, and there is a demand for further improvements in hydrochloric acid corrosion resistance and wear resistance. However, the coating materials described in Patent Documents 2 to 12 sometimes have insufficient properties, and Patent Documents 13 to 17 require sintering or HIP processing, making it impossible to apply surface coatings to large areas and limiting their applications. Therefore, the challenge is to develop thermal spray and build-up materials that possess further hydrochloric acid corrosion resistance and wear resistance. [Means for solving the problem]
[0008] In this invention, when considering alloy compositions that possess excellent hydrochloric acid corrosion resistance and wear resistance, the following target values were set, and it was a condition that all of these be satisfied. (1) Hydrochloric acid corrosion resistance: Under specified conditions, corrosion loss is 15.0 mg / m². 2 Less than s (2) Abrasion resistance → Rockwell hardness of 45 HRC or higher (3) Melting temperature range in which remelting (fusing) is possible → Solidus temperature of 1150°C or less, melting temperature range of 250°C or higher
[0009] In other words, the nickel self-fluxing alloy and its powder composition of the present invention that satisfy the above objectives (1) to (3) is characterized by containing 18.0 to 30.0 mass% of Mo, 1.8 to 4.0 mass% of B, and 2.5 to 5.0 mass% of Si, with the total of B and Si being 5.5 mass% or more, the Cr content being 22.0 mass% or less, the Cu content being 5.0 mass% or less, and the remainder consisting of 43.0 to 75.0 mass% of Ni and unavoidable impurities.
[0010] Furthermore, the nickel self-fluxing alloy of the present invention contains 18.0 to 30.0 mass% of Mo, 1.8 to 4.0 mass% of B, and 2.5 to 5.0 mass% of Si, with the total content of B and Si being 5.5 mass% or more, the Cr content being 22.0 mass% or less, the Cu content being 5.0 mass% or less, and further contains at least one selected from the group consisting of 5.0 mass% or less of Fe, 3.0 mass% or less of Nb, and 0.3 mass% or less of C, with the total content of Fe, Nb, and C being 5.0 mass% or less, and the balance being 43.0 to 75.0 mass% of Ni and unavoidable impurities.
[0011] Furthermore, the present invention also provides a nickel self-fluxing alloy having the above characteristics, wherein the Cr content is 13.0 mass% or less, the Cu content is 0.1 mass% or more and less than 1.0 mass%, the B content is 2.6 to 4.0 mass%, the Si content is 3.6 to 5.0 mass%, and the total content of B and Si is 6.5 mass% or more.
[0012] Furthermore, the nickel self-fluxing alloy powder of the present invention contains 18.0 to 30.0 mass% of Mo, 1.8 to 4.0 mass% of B, and 2.5 to 5.0 mass% of Si, with the total content of B and Si being 5.5 mass% or more, the Cr content being 22.0 mass% or less, the Cu content being 5.0 mass% or less, and the balance being 43.0 to 75.0 mass% of Ni and unavoidable impurities, and contains 80 mass% or more of powder with a particle size of 45 to 106 μm in a particle size distribution measurement according to the method specified in JIS Z 2510.
[0013] In addition, the nickel self-fluxing alloy powder of the present invention contains 18.0 to 30.0 mass% of Mo, 1.8 to 4.0 mass% of B, and 2.5 to 5.0 mass% of Si, with the total content of B and Si being 5.5 mass% or more, the Cr content being 22.0 mass% or less, the Cu content being 5.0 mass% or less, and further contains at least one of 5.0 mass% or less of Fe, 3.0 mass% or less of Nb, and 0.3 mass% or less of C, with the total content of Fe, Nb, and C being 5.0 mass% or less, and the balance being 43.0 to 75.0 mass% of Ni and inevitable impurities. In a particle size distribution measurement according to the method specified in JIS Z 2510, it is characterized in that it contains 80 mass% or more of powder with a particle size of 45 to 106 μm.
[0014] The above nickel self-fluxing alloy powder can be produced by pulverizing a nickel self-fluxing alloy having the above composition by an atomization method, and then adjusting the particle size.
[0015] In addition, the present invention also relates to a coated member, characterized in that a coating made of the above nickel self-fluxing alloy is provided on the surface.
[0016] Furthermore, the present invention is also a method for producing various coated members on which a dense coating having excellent hydrochloric acid corrosion resistance is formed, and the method is characterized in that thermal spraying is performed on a blasted steel material using the above nickel self-fluxing alloy powder to form a coating, and then fusing is performed in a torch or a furnace.
[0017] Next, the reasons for limiting each component of the alloy of the present invention will be described.
[0018] Mo contributes to imparting corrosion resistance to halogen-based corrosive environments such as hydrochloric acid, and combines with B to form intermetallic compounds in the metal structure, improving wear resistance. However, if the content is less than 18.0 mass%, the effect is small, and if it exceeds 30.0 mass%, the amount of intermetallic compounds increases, making the alloy brittle, and the melting temperature (solidus temperature) increases, which deteriorates the fluidity of the molten metal and makes fusing after thermal spraying difficult. Therefore, the content is limited to the range of 18.0 to 30.0 mass%.
[0019] While chromium (Cr) is undesirable for corrosion resistance in halogen-based corrosive environments such as hydrochloric acid, its addition improves high-temperature corrosion properties and enhances wear resistance by bonding with boron (B) to form intermetallic compounds in the metal structure. Exceeding 22.0% by mass significantly reduces corrosion resistance in halogen-based corrosive environments such as hydrochloric acid, increases the amount of intermetallic compounds, makes the metal brittle, raises the melting temperature, worsens molten metal flow, and makes fusing after thermal spraying difficult; therefore, the Cr content was limited to 22.0% by mass or less. Furthermore, limiting the Cr content to 13.0% by mass or less reduces the negative effect on corrosion resistance in halogen-based corrosive environments such as hydrochloric acid, thereby improving corrosion resistance.
[0020] While Cu contributes to corrosion resistance in halogen-based corrosive environments such as hydrochloric acid, exceeding 5.0% by mass causes coarsening of Mo-based intermetallic compounds, leading to a decrease in toughness; therefore, it was limited to 5.0% by mass or less. Furthermore, adding 0.1% by mass or more improves hydrochloric acid corrosion resistance by 25% or more, and up to 70%, compared to no addition (0% Cu by mass), making addition of 0.1% by mass or more more preferable. Moreover, adding 1.0% by mass or more does not further improve hydrochloric acid corrosion resistance, and the Mo-based compounds tend to coarseen, leading to a decrease in toughness, i.e., a decrease in impact resistance; therefore, a range of 0.1% by mass or more to less than 1.0% by mass is more preferable.
[0021] In addition to imparting self-fluxability and lowering the melting temperature to improve fusing workability, B also contributes to improved wear resistance by forming intermetallic compounds with Mo and Cr in the metal structure. However, below 1.8 mass%, self-fluxability is insufficient, making fusing difficult, and the amount of intermetallic compounds decreases, resulting in reduced wear resistance. Furthermore, above 4.0 mass%, the intermetallic compounds become coarser, and the amount of intermetallic compounds increases, leading to a decrease in toughness, i.e., a decrease in impact resistance. For this reason, the range was limited to 1.8 to 4.0 mass%. Moreover, considering self-fluxability, melting temperature, and the amount of intermetallic compounds, the range of 2.6 to 4.0 mass% is more preferable.
[0022] Si imparts self-fluxability and lowers the melting temperature, improving the workability of fusing. However, below 2.5 mass%, self-fluxability is insufficient, making fusing difficult. Furthermore, above 5.0 mass%, corrosion resistance to halogen-based corrosive environments such as hydrochloric acid decreases, so the range was limited to 2.5 to 5.0 mass%. Moreover, considering corrosion resistance, self-fluxability, and melting temperature, the range of 3.6 to 5.0 mass% is more preferable.
[0023] Furthermore, the combined addition of B and Si provides a purifying effect on the molten metal, improves workability during fusing after thermal spraying, and contributes to densifying the coating layer by reducing oxides and voids in the film. However, if the total amount is less than 5.5% by mass, the purifying effect on the molten metal and the workability during fusing are not obtained. Therefore, the total amount of B and Si is specified to be 5.5% by mass or more. In addition, the effect is greater with higher amounts of B and Si added, and more preferably 6.5% by mass or more.
[0024] When the base material used for thermal spraying or overlaying is Fe-based steel, Fe promotes metallurgical bonding (diffusion) during fusing, improving adhesion strength. However, exceeding 5.0% by mass leads to a decrease in corrosion resistance to halogen-based corrosive environments such as hydrochloric acid, so it was limited to 5.0% or less.
[0025] Nb forms intermetallic compounds with Mo, Cr, Si, and C in the metal structure, imparting wear resistance and further improving high-temperature corrosion properties (oxidation and sulfidation). However, if the amount added is too high, the amount of intermetallic compounds increases, leading to a decrease in toughness, i.e., a decrease in impact resistance. Therefore, the amount was limited to 3.0 mass% or less.
[0026] Carbon (C) lowers the melting temperature, improving the workability of fusing. It also forms intermetallic compounds with Mo and Cr in the metal structure, improving wear resistance. However, if the amount exceeds 0.3 mass%, the amount of angular intermetallic compounds increases and becomes coarser, leading to a decrease in toughness, i.e., a decrease in impact resistance. Therefore, the amount was limited to 0.3 mass% or less.
[0027] The nickel self-fluxing alloy of the present invention may contain at least one of Fe, Nb, and C, but if the total amount is large (exceeding 5.0 mass%), the melting temperature range becomes narrow, leading to a decrease in corrosion resistance and toughness. Therefore, the total amount is limited to 5.0 mass% or less.
[0028] Furthermore, if all additive elements such as Mo, Cr, B, Si, Cu, and Fe are at their upper limits, the main component Ni will be 29.0 mass%, but in that case, the amount of Ni as the main component will be small, and the amount of intermetallic compounds formed in the metal structure will be large, leading to a decrease in toughness, i.e., a decrease in impact resistance. Also, if all additive elements are at their lower limits, the amount of Ni as the main component will be 77.7 mass%, but in that case, the amount of Ni as the main component will be large, and the amount of intermetallic compounds formed in the metal structure will be small, making it impossible to obtain the desired hardness (wear resistance). For this reason, Ni was limited to the range of 43.0 to 75.0 mass%.
[0029] Furthermore, by atomizing the alloy having the above alloy composition into powder and adjusting the resulting powder particles to a predetermined particle size, it can be applied to various surface modification processes such as thermal spraying and plasma powder cladding. [Effects of the Invention]
[0030] The nickel self-fluxing alloy and its powder of the present invention possess high resistance to hydrochloric acid corrosion, as well as high-temperature corrosion resistance and wear resistance, making them suitable for use as surface modification materials in high-temperature environments accompanied by halogen corrosion. In particular, in thermal spraying, fusing after film formation densifies the coating layer, further improving corrosion resistance and wear resistance. In addition, a metallurgical bond is obtained with substrates such as steel, improving adhesion and enabling application to a wide range of applications in high-temperature environments. [Brief explanation of the drawing]
[0031] [Figure 1] This is a schematic diagram of a component obtained by thermal spraying the nickel self-fluxing alloy of the present invention onto a roll member. [Figure 2]This is the cross-sectional structure of a component obtained by fusing the nickel self-fluxing alloy of the present invention after thermal spraying. [Modes for carrying out the invention]
[0032] The base metal Ni and the additive components Mo, Cr, Cu, B, Si, Fe, Nb, and C are each adjusted and blended to a predetermined mass percentage. This base metal is heated and melted in a crucible in a melting furnace to form a liquid alloy, and then the powder of the alloy of the present invention can be obtained by atomization.
[0033] Furthermore, by adjusting the particle size of the alloy powder produced by the atomization method to suit the desired construction method, it can be applied to surface modification constructions such as thermal spraying and plasma powder cladding. By coating with this powder, it is possible to impart hydrochloric acid corrosion resistance (or corrosion resistance to halogen-based corrosive environments) and further improve wear resistance.
[0034] For example, in the roll member 1 shown in Figure 1, a SUS347 tube with an inner diameter of 35.6 mm, an outer diameter of 45 mm, and a length of 2000 mm was used as the base material 2, and a thermal spray coating 3 was applied to the base material 2 to a thickness of approximately 1 mm. Figure 2, which shows a cross-section, is an example in which fusing was performed after thermal spraying. A diffusion layer 7 is formed at the interface between the base material 2 and the thermal spray coating 3, and it can be seen that the molybdenum compound 5, which contributes to wear resistance, is homogeneously dispersed in the nickel solid solution 4 that forms the matrix within the thermal spray coating 3, and that the coating has few voids 6 due to fusing. [Examples]
[0035] The target alloy composition was achieved by melting and blending the metal, and its resistance to hydrochloric acid corrosion, Rockwell hardness (an indicator of wear resistance), and melting temperature range were evaluated using the methods described below. Furthermore, the properties of coatings produced by thermal spraying and fusing using alloy powders prepared by atomization were also evaluated.
[0036] (1) Hydrochloric acid corrosion resistance; 100g of metal having the alloy composition of each alloy was heated to approximately 1650°C in an electric furnace under an argon gas stream, melted, and cast into a shell mold. This cast piece was then machined to approximately 10 × 10 × 20 mm, and the surface roughness was adjusted using #240 waterproof abrasive paper to prepare the test piece. Next, a 30% hydrochloric acid aqueous solution was prepared in a 200cc beaker, and the test piece was placed in it to perform a corrosion test using the total immersion method. The test conditions were a test temperature of 60°C and a test time of 6 hours. The unit surface area and the mass loss per unit time before and after the test were calculated to determine the corrosion weight loss (mg / m²). 2 The corrosion resistance to hydrochloric acid was evaluated using the following method (s). The corrosion loss was 15.0 mg / m². 2 A score below 's' was considered a passing grade.
[0037] (2) Rockwell hardness; A Rockwell hardness test was conducted in accordance with JIS Z 2245:2005 using a cast slab that was melted using the same method as in (1) above, machined to the same shape, and had its surface roughness adjusted. The hardness measurement was performed on the C scale, and a Rockwell hardness of 45 or higher was considered acceptable as a standard for wear resistance.
[0038] (3) Melting temperature range; 100g of metal having the composition of each alloy was heated to approximately 1650°C in an argon stream using an electric furnace and melted. After melting, an alumina protective tube with an R thermocouple was inserted into the molten metal and slow cooling was performed to obtain a time-temperature curve during cooling. From this time-temperature curve, the inflection point associated with the endothermic reaction that occurs during solidification was read, and the final solidification temperature (solidus temperature) and the range between the solidification start temperature (liquidus temperature) and the final solidification temperature (solidus temperature) (melting temperature range) were read. A solidus temperature of 1150°C or less and a melting temperature range of 250°C or more were considered acceptable.
[0039] Table 1 shows examples of the alloy of the present invention, and Table 2 shows comparative examples.
[0040] [Table 1]
[0041] [Table 2]
[0042] Comparative alloys No. 13 to No. 19 shown in Table 2 did not satisfy the targets for hydrochloric acid corrosion resistance, hardness, solidus temperature, and melting temperature range. No. 13 had less than 18.0 mass% Mo and less than 5.5 mass% total B and Si, resulting in poor hydrochloric acid corrosion resistance. No. 14 had more than 30.0 mass% Mo and less than 1.8 mass% B, resulting in a relatively high solidus temperature and low hardness. No. 15 had more than 23.0 mass% Cr, resulting in a high solidus temperature and a narrow melting temperature range, resulting in poor hydrochloric acid corrosion resistance. No. 16 had more than 4.0 mass% B and more than 0.3 mass% C, resulting in poor hydrochloric acid corrosion resistance. No. 17 had less than 2.5 mass% Si and more than 5.0 mass% Fe, resulting in poor hydrochloric acid corrosion resistance and a narrow melting temperature range. No. 18 has a Si content exceeding 5.0 mass%, resulting in poor hydrochloric acid corrosion resistance. No. 19 has a combined Fe and Nb content exceeding 5.0 mass%, resulting in a narrow melting temperature range.
[0043] In contrast, as shown in Table 1, Examples No. 1 to 12, which are alloys of the present invention, satisfy all the targets of hydrochloric acid corrosion resistance, hardness, solidus temperature, and melting temperature range, and can be expected to be thermal spray materials that possess hydrochloric acid corrosion resistance and wear resistance.
[0044] Furthermore, 100 kg of metal having the compositions of Examples No. 1, No. 2, No. 4, No. 6, No. 9, and No. 10 listed in Table 1 was heated and melted to approximately 1650°C in an air atmosphere using a high-frequency induction melting furnace, pulverized by gas atomization, and the particle size was adjusted to 45-106 μm using a vibrating screen. This alloy powder was coated onto the surface of blast-treated steel (S15C) using a powder flame spraying method. Subsequently, furnace fusing (remelting treatment using a vacuum furnace, at an arbitrary temperature of 1000-1200°C) was performed to obtain a coating. The corrosion weight loss of the coating after fusing was evaluated in a hydrochloric acid vapor exposure test (under two conditions: room temperature and 220°C) to assess its resistance to hydrochloric acid corrosion. Furthermore, a high-temperature molten salt corrosion test (67% NaCl + 33% Na2SO4, held at 650°C for 5 hours, followed by cooling to room temperature, repeated 10 times, with the depth of corrosion degradation evaluated from cross-sectional observation) and a Vickers hardness test were used to evaluate the surface hardness of the coating. The following criteria were deemed acceptable. <Evaluation Criteria> [Table 3]
[0045] For comparison, we used NiCrCuMoBSi 67 15 3 3A (formerly JIS symbol: SFNi4) and NiCrBSi 70 20A (formerly JIS symbol: SFNi5) described in JIS H 8303, as well as thermal spray and fusing coatings of alloys described in Patent Document 9 (Patent No. 3430498), and INCONEL 625 (registered trademark), applied as a single-layer and double-layer TIG weld on blast-treated steel (S15C). SFNi5 was applied by high-velocity flame spraying, and the test specimens were made without fusing, with the raw material powder adjusted to 10-45 μm. For the TIG-welded INCONEL 625, a φ5 welding rod was used. The results are shown in Table 4.
[0046] Furthermore, when adjusting the particle size of the powder used for thermal spraying, if there is a large amount of fine powder, problems such as spitting during application and pulsation due to impaired powder flowability can occur. On the other hand, if there is a large amount of coarse powder, in addition to impaired flowability, unmelted particles are produced, making it impossible to form a dense coating. Therefore, in particle size distribution measurement using the method specified in JIS Z 2510, the powder was adjusted so that 80% by mass or more of the powder was within the desired particle size range (45-106 μm).
[0047] [Table 4]
[0048] Examples No. A to F are coatings using the alloy of the present invention and satisfy all of the following tests: hydrochloric acid vapor exposure test, high-temperature molten salt corrosion test, and hardness test. On the other hand, comparative examples No. G to K failed to satisfy all of the following tests: hydrochloric acid vapor exposure test, high-temperature molten salt corrosion test, and hardness test. [Industrial applicability]
[0049] As described above, the nickel self-fluxing alloy according to the present invention possesses not only excellent hydrochloric acid corrosion resistance but also high hardness. Therefore, for components that require hydrochloric acid corrosion resistance and wear resistance, coating the surface with atomized powder by thermal spraying can be expected to extend the lifespan of the component.
[0050] By separating the powder particles into sizes of 10-45 μm, or 20-53 μm, 45-106 μm, 45-150 μm, or 75-150 μm using a vibrating screen or airflow classifier, and selecting the appropriate particle size, the powder of the alloy of the present invention can be applied not only to flame spraying but also to high-speed flame spraying, plasma spraying, plasma powder cladding, etc. Furthermore, by forming a cast piece having the alloy composition of the present invention, it can be used to create machine parts with excellent hydrochloric acid corrosion resistance and wear resistance. [Explanation of Symbols]
[0051] 1 Roll Member 2 Base material 3. Thermal spray coating 4. Nickel solid solution 5. Molybdenum compounds 6 void 7. Diffusion layer
Claims
1. A nickel self-fluxing alloy characterized by containing 18.0 to 30.0 mass% of Mo, 2.6 to 4.0 mass% of B, and 3.6 to 5.0 mass% of Si, with the total of B and Si being 6.5 mass% or more, the Cr content being 13.0 mass% or less, the Cu content being 0.1 mass% or more and less than 1.0 mass%, and the remainder consisting of 43.0 to 75.0 mass% Ni and unavoidable impurities.
2. A nickel self-fluxing alloy characterized by containing 18.0 to 30.0 mass% of Mo, 2.6 to 4.0 mass% of B, and 3.6 to 5.0 mass% of Si, with the total of B and Si being 6.5 mass% or more, a Cr content of 13.0 mass% or less, a Cu content of 0.1 mass% or more and less than 1.0 mass%, and further containing at least one of Fe (5.0 mass% or less), Nb (3.0 mass% or less), and C (0.3 mass% or less), with the total of Fe, Nb, and C being 5.0 mass% or less, and the remainder consisting of 43.0 to 75.0 mass% Ni and unavoidable impurities.
3. Nickel self-fluxing alloy powder characterized by having a composition containing 18.0 to 30.0 mass% of Mo, 2.6 to 4.0 mass% of B, and 3.6 to 5.0 mass% of Si, with the total of B and Si being 6.5 mass% or more, a Cr content of 13.0 mass% or less, a Cu content of 0.1 mass% or more and less than 1.0 mass%, and the remainder consisting of 43.0 to 75.0 mass% of Ni and unavoidable impurities, and containing 80 mass% or more of powder with a particle size of 45 to 106 μm.
4. Nickel self-fluxing alloy powder characterized by having a composition comprising 18.0 to 30.0 mass% of Mo, 2.6 to 4.0 mass% of B, and 3.6 to 5.0 mass% of Si, with the total of B and Si being 6.5 mass% or more, a Cr content of 13.0 mass% or less, a Cu content of 0.1 mass% or more and less than 1.0 mass%, and further comprising at least one of Fe (5.0 mass% or less), Nb (3.0 mass% or less), and C (0.3 mass% or less), with the total of Fe, Nb, and C being 5.0 mass% or less, and the remainder consisting of 43.0 to 75.0 mass% Ni and unavoidable impurities, and containing 80 mass% or more of powder with a particle size of 45 to 106 μm.
5. A method for producing self-fluxing alloy powder, characterized by atomizing the nickel self-fluxing alloy described in claim 1 or 2 into powder and then adjusting the particle size.
6. A coating member characterized in that a film made of the nickel self-fluxing alloy described in claim 1 or 2 is provided on its surface.
7. A method for manufacturing a coated member, characterized by forming a coating on a blast-treated steel material by thermal spraying using the nickel self-fluxing alloy powder described in claim 3 or 4, and then fusing it in a torch or furnace.
Citation Information
Patent Citations
High-speed laser cladding method of boiler pipe and boiler pipe
CN110616425A
Cold insulating roll
JP1982058965A
Concrete retarder
JP1983055357A
Wear-resistant alloy excellent in corrosion resistance to halogen gas and its production
JP1989079338A
Corrosion and wear resistant high strength nickel-based alloy
JP1996134569A