Electrophotographic component, process cartridge, and electrophotographic image forming apparatus

The use of a urethane elastomer-based conductive elastic layer with specific viscoelastic properties addresses the issues of high hardness and compression set in electrophotographic components, enabling stable and high-quality image formation.

JP7955132B2Active Publication Date: 2026-11-24CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022170590
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2026-11-24
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Existing electrophotographic components face issues with high micro-rubber hardness and compression set, leading to uneven development and charging, which affect the quality of electrophotographic images.

Method used

An electrophotographic component with a conductive elastic layer composed of a urethane elastomer and conductive filler, where the urethane elastomer has a matrix and dispersed domains, with specific viscoelastic properties and chemical bonding between the matrix and domains, ensuring low hardness and rapid deformation recovery.

Benefits of technology

The solution provides high conductivity, low hardness, and excellent deformation recovery, resulting in stable formation of high-quality electrophotographic images.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955132000017
    Figure 0007955132000017
  • Figure 0007955132000018
    Figure 0007955132000018
  • Figure 0007955132000019
    Figure 0007955132000019
Patent Text Reader

Abstract

To provide an electrophotographic member that is quickly restored from deformation despite inclusion of urethane elastomer with low hardness, has good wear resistance, and can prevent a streak-like image defect.SOLUTION: An electrophotographic member is provided, and the electrophotographic member has an elastic layer having conductivity. The elastic layer includes urethane elastomer and conductive filler. The urethane elastomer has a matrix and a plurality of domains dispersed in the matrix. A parameter A indicating the viscoelasticity term of the domain and a parameter B indicating the viscoelasticity term of the matrix, which are measured in a predetermined viscoelasticity image of a cross section of the elastic layer from which the domains and the matrix are exposed, have a relationship of A<B. The elastic layer has a micro rubber hardness of 20 to 50 degrees at a temperature of 23°C. Distortion of the elastic member five seconds after removal of load measured at a temperature of 23°C by a predetermined method is 1.00 μm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure is intended for use in electrophotographic image forming apparatuses (hereinafter also simply referred to as "image forming apparatuses") such as electrophotographic copiers and printers. This disclosure is also intended for process cartridges and electrophotographic image forming apparatuses. [Background technology]

[0002] Image forming apparatus employing the electrophotographic method (such as photocopiers, fax machines, and printers using the electrophotographic method) mainly consists of an electrophotographic photoreceptor (hereinafter also referred to as "photoreceptor"), a charging device, an exposure device, a developing device, a transfer device, and a fixing device. In an image forming apparatus, the photoreceptor is first charged by a charging member (hereinafter also referred to as the "charging roller"), and then exposed to light to form an electrostatic latent image on the photoreceptor. The toner in the toner container is applied to the toner carrier (hereinafter also referred to as the "developing roller") by a toner regulating member and transported to the developing area by the developing roller. The toner transported to the developing area then develops the electrostatic latent image on the photoreceptor at the contact point between the photoreceptor and the developing roller. After that, the toner on the photoreceptor is transferred to the recording paper by a transfer means and fixed by heat and pressure. Any toner remaining on the photoreceptor is removed by a cleaning member.

[0003] Conventionally, the elastic layer of such developing rollers and charging rollers is required to have high recovery from deformation, that is, low compression set, and low micro-rubber hardness. For this reason, vulcanized rubbers with high electrical resistance, such as silicone rubber, acrylonitrile butadiene rubber, and epichlorohydrin rubber, have been used as materials for the elastic layer. On the other hand, the elastic layer is also required to be electrically conductive. Because the vulcanized rubber described above has high electrical resistance, conductive fillers such as carbon black are sometimes included to make the elastic layer conductive. However, conductive fillers can lead to an increase in the micro-rubber hardness of the elastic layer and an increase in compression set. An increase in the micro-rubber hardness of the elastic layer can, for example, increase the stress that the developing roller places on the toner. Furthermore, an increase in the compression set of the elastic layer can lead to phenomena such as the deformation of the contact point between the developing roller and the toner regulating member not easily recovering when the developing roller is in contact with the toner regulating member for a long period of time while stationary. Partial deformation of the developing roller can cause uneven development. Similarly, an increase in the compression set of the elastic layer can lead to phenomena such as the deformation of the contact point between the charging roller and the photosensitive drum not easily recovering when the charging roller is in contact with the photosensitive drum for a long period of time while stationary. Partial deformation of the charging roller can cause uneven charging of the photosensitive drum.

[0004] Patent Document 1 discloses a conductive member for electrophotographic equipment comprising an elastic layer composed of a conductive first polymer phase containing one or more polymers, a non-conductive second polymer phase containing one or more polymers and existing separately from the first polymer phase, and an interface phase existing between the first polymer phase and the second polymer phase, which contains a compatibilizer made of a polymer containing either or both of the polymer components contained in the first polymer phase and the polymer components contained in the second polymer phase. Patent Document 1 states that, according to this conductive member for electrophotographic equipment, the presence of a non-conductive phase in the conductive elastic layer provides low hardness and low deformation that cannot be obtained with a conductive phase alone, and that the uniform fine dispersion of both phases enables charge control at the toner size level, suppresses resistance unevenness, and exhibits excellent chargeability. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2017-116685 [Non-patent literature]

[0006] [Non-Patent Document 1] IEEE Transactions on SYSTEMS, MAN, AND CYBERNETICS, Vol. SMC-9, No. 1, January 1979, pp. 62-66 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] The present inventors investigated the conductive member for electrophotographic equipment described in Patent Document 1. As a result, they found that the conductive member for electrophotographic equipment described in Patent Document 1 still has room for improvement in terms of its recovery from deformation.

[0008] At least one aspect of this disclosure is toward providing an electrophotographic component that has high conductivity, low hardness, and excellent recovery from deformation. At least one aspect of this disclosure is toward providing a process cartridge that contributes to the stable formation of high-quality electrophotographic images. Furthermore, at least one aspect of this disclosure is toward providing an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images. [Means for solving the problem]

[0009] According to at least one aspect of this disclosure, An electrophotographic component, wherein the electrophotographic component has a conductive elastic layer, The elastic layer comprises a urethane elastomer and a conductive filler. The urethane elastomer has a matrix and a plurality of domains dispersed in the matrix, The relationship between parameter A, which represents the viscoelastic term of the domain, and parameter B, which represents the viscoelastic term of the matrix, as measured in a viscoelastic image obtained by scanning probe microscopy of a cross-section of the elastic layer in which the domain and the matrix are exposed, is A <Bであり、 The microrubber hardness of the elastic layer at a temperature of 23°C is 20 to 50 degrees. Provided is an electrophotographic member having a strain of 1.00 μm or less 5 seconds after unloading when a Vickers indenter is brought into contact with the matrix on the outer surface of the elastic layer at a temperature of 23° C., the Vickers indenter is pressed into the elastic layer at a load rate of 10 mN / 30 seconds, held at a load of 10 mN for 60 seconds, and then unloaded.

[0010] Also, according to at least one aspect of the present disclosure, there is provided a process cartridge configured to be attachable to and detachable from an image forming apparatus, the process cartridge including the electrophotographic member of the present disclosure.

[0011] Further, according to at least one aspect of the present disclosure, there is provided an electrophotographic image forming apparatus including the electrophotographic member of the present disclosure. [[Effects of the Invention]]

[0012] According to at least one aspect of the present disclosure, it is possible to obtain an electrophotographic member that has high conductivity, low hardness, and excellent recoverability against deformation. In addition, according to at least one aspect of the present disclosure, it is possible to obtain a process cartridge that contributes to formation of high-quality electrophotographic images. Further, according to at least one aspect of the present disclosure, it is possible to obtain an electrophotographic image forming apparatus capable of forming high-quality electrophotographic images. [[Brief Description of the Drawings]]

[0013] [Figure 1] A schematic cross-sectional view illustrating an example of an electrophotographic member according to an aspect of the present disclosure. [Figure 2] A schematic cross-sectional view of an embodiment of an elastic layer of an electrophotographic member according to an aspect of the present disclosure. [Figure 3] A diagram illustrating deformation of an elastic layer according to the present disclosure. [Figure 4] A diagram illustrating a cutout position and direction of a cross-section. [Figure 5] A schematic diagram illustrating a method for manufacturing an electrophotographic member according to an embodiment of the present disclosure. [Figure 6] A schematic cross-sectional view of an example of an image forming apparatus according to an embodiment of the present disclosure. [Figure 7] A schematic cross-sectional view of an example of a process cartridge according to one embodiment of the present disclosure. [Modes for carrying out the invention]

[0014] In this disclosure, unless otherwise specified, the expressions "XX or greater and YY or less" and "XX to YY" that represent numerical ranges mean numerical ranges that include the lower and upper limits. Furthermore, when numerical ranges are described in steps, any combination of the upper and lower limits of each numerical range is disclosed.

[0015] The inventors speculated that the reason why the deformation recovery of the conductive member for electrophotographic equipment described in Patent Document 1 is insufficient is as follows. That is, the low hardness and low deformation characteristics of the conductive member for electrophotographic equipment described in Patent Document 1 are achieved by separating the functions of the conductive elastic layer into a conductive phase and a flexible phase (paragraph

[0030] of Patent Document 1, etc.). Here, the conductive phase and the flexible phase are formed by the phase separation of two types of polymers that are incompatible with each other. Therefore, there is no chemical bond between the conductive phase and the flexible phase. As a result, it is thought that the recovery behavior from deformation of the conductive elastic layer when a load is applied to the conductive elastic layer and then removed occurs independently of the conductive phase and the flexible phase. The inventors speculated that this is one of the reasons why the deformation recovery of the conductive elastic layer is insufficient. Based on this consideration, the inventors conducted further investigations and found that a urethane elastomer having a specific structure can achieve an extremely high level of both flexibility and deformation recovery, even when a conductive filler is included. The electrophotographic components and the like related to this disclosure will be described in detail below with reference to preferred embodiments.

[0016] <Electrophotographic components> Figures 1(a) and 1(b) are schematic circumferential cross-sectional views of two embodiments of an electrophotographic member having a roller shape according to the present disclosure (hereinafter also referred to as "electrophotographic roller"). The electrophotographic roller 1A shown in Figure 1(a) has a conductive shaft 2 and a conductive elastic layer (hereinafter also simply referred to as the "elastic layer") 3 covering the surface (outer surface) of the shaft 2. The electrophotographic roller 1B shown in Figure 1(b) has an additional surface layer 4 on the surface (hereinafter also referred to as the "outer surface") of the elastic layer 3 on the side opposite to the shaft 2. The electrophotographic roller according to this disclosure is not limited to these configurations, and for example, it may have an adhesive layer (not shown) between each layer.

[0017] (Core body) The core body 2 is preferably conductive in order to supply power to the surface of the electrophotographic member through the core body. The electrical resistance of the core body is preferably lower than that of the elastic layer, and the volume resistivity of the core body is 10 3 It is preferable that the value is Ω·cm or less. The conductive core can be appropriately selected from those known in the field of electrophotographic components, and is preferably made of a metal such as aluminum, aluminum alloy, stainless steel, or iron. Furthermore, to improve corrosion resistance and abrasion resistance, these metals may be plated with chromium, nickel, or the like. The shape of the shaft core can be selected from either a hollow (cylindrical) or solid (columnar) shape. For example, a cylindrical shaft core made of carbon steel alloy with a nickel plating of about 5 μm thickness can be used. The outer diameter of the cylindrical or columnar shaft core can be appropriately selected depending on the image forming apparatus to which it is mounted.

[0018] (Elastic layer) The elastic layer 3 satisfies the following requirements (1-1) to (1-4). Requirement (1-1): The elastic layer comprises a urethane elastomer and a conductive filler, the urethane elastomer having a matrix and a plurality of domains dispersed in the matrix. Requirement (1-2): The relationship between parameter A, which represents the viscoelastic term of the domain, and parameter B, which represents the viscoelastic term of the matrix, as measured in a viscoelastic image obtained by scanning probe microscopy of a cross-section of the elastic layer in which the domains and matrix are exposed, is A <Bである。 In other words, in the cross-section along the thickness of the elastic layer, the matrix domain structure of the urethane elastomer is observed. Furthermore, the elastic modulus of the urethane elastomer matrix observed in the cross-section along the thickness of the elastic layer is greater than the elastic modulus of the domains.

[0019] Requirements (1-3): The microrubber hardness of the elastic layer at a temperature of 23°C is 20-50. Requirements (1-4): At a temperature of 23°C, a Vickers indenter is brought into contact with the matrix on the outer surface of the elastic layer, the Vickers indenter is pressed into the elastic layer at a loading rate of 10 mN / 30 seconds, the load is maintained at 10 mN for 60 seconds, and then the load is removed. The strain 5 seconds after unloading is 1.00 μm or less. In a urethane elastomer, the matrix primarily plays a role in enabling the urethane elastomer to exhibit high recovery from deformation, while the domains primarily play a role in enabling the urethane elastomer to have low hardness. Furthermore, as will be described later, in the urethane elastomer according to this disclosure, it is considered that the domains and matrix are chemically bonded by urethane bonds at the boundary between the domains and the matrix. Therefore, it is considered that the recovery of the domains from deformation when the load applied to the urethane elastomer is removed proceeds in conjunction with the recovery of the matrix from deformation. As a result, the elastic layer according to this disclosure is considered to have extremely high recovery from deformation. By employing such an elastic layer, the elastic layer exhibits the softness specified in requirement (1-3) above and the extremely high recovery from deformation specified in requirement (1-4) above. It should be noted that general urethane elastomers also have a difference in elastic modulus between the so-called hard segments and soft segments. However, in general urethane elastomers, the soft segments constitute the matrix and the hard segments constitute the domains, and it is considered that while they possess the flexibility related to requirement (1-3) above, they do not exhibit a fast recovery rate from deformation as specified in requirement (1-4).

[0020] Figure 2(a) is a partial cross-sectional view in the circumferential direction of an electrophotographic roller 1A according to one embodiment of the present disclosure. Figure 2(b) is a partial cross-sectional view of the electrophotographic roller 1A along the longitudinal direction of the axial core 2. Figures 2(a) and 2(b) schematically show the matrix 31 of the urethane elastomer, the multiple domains 32 dispersed in the matrix 31, and the conductive filler 33 contained in the elastic layer, as observed in a cross-section in the thickness direction of the elastic layer 3. As described above, the urethane elastomer has a matrix 31 and a plurality of domains 32 dispersed within the matrix. The matrix exhibits higher elasticity than the domains. Furthermore, it is preferable that at least a portion of the outer surface of the elastic layer is composed of a matrix. Figures 2(a) and 2(b) show an example in which the entire outer surface of the elastic layer 3 is composed of a matrix.

[0021] Figures 3(a) and 3(b) are explanatory diagrams illustrating the recovery from deformation of the elastic layer 3 according to this disclosure. As shown in Figure 3(a), multiple domains 32 are dispersed within the matrix 31. Furthermore, since domain 32 is less elastic than matrix 31, when the elastic layer 3 is compressed in the direction of arrow F, as shown in Figure 3(b), domain 32 deforms preferentially. For this reason, even if matrix 31 is highly elastic, the micro-rubber hardness of the elastic layer can be kept low. Also, when the elastic layer is released from compression, the elasticity of the continuous phase matrix 31 allows the thickness of the elastic layer to quickly return to its original thickness. In other words, high recovery from deformation of matrix 31 is achieved.

[0022] (Microrubber hardness of the elastic layer) The microrubber hardness of the elastic layer at a temperature of 23°C is 20 to 50 degrees. By setting the microrubber hardness to 50 degrees or less, the nip width between the developing roller and the toner regulating member, and between the charging roller and the photoreceptor, increases, preventing excessive contact pressure. This makes it less likely for toner on the developing roller to fuse to the developing roller, and for toner that has slipped through the cleaning member and adhered to the charging roller to fuse to the charging roller. Furthermore, by setting the microrubber hardness to 20 degrees or more, the mechanical strength increases, making it less likely for the edges of the elastic layer to wear down even when used in high-life image forming machines. The microrubber hardness is preferably 20 to 40 degrees, and more preferably 22 to 38 degrees. Microrubber hardness can be adjusted by, for example, the elastic modulus of the matrix, the amount of conductive filler contained in the matrix, and the ratio of the matrix to the domains. Specifically, increasing the elastic modulus of the matrix, increasing the proportion of conductive filler in the matrix, and decreasing the proportion (volume) of domains relative to the matrix all act to increase microrubber hardness. Microrubber hardness can be determined, for example, as follows: The locations for measuring microrubber hardness are three in total: the center of the elastic layer in the longitudinal direction, and two locations L / 4 from both ends of the elastic layer toward the center, where L is the length of the elastic layer in the longitudinal direction. At each measurement location, the surface is measured for microrubber hardness at a temperature of 23°C using a microrubber hardness tester (product name: MD-1capa; manufactured by Polymer Instruments Co., Ltd., indenter: type A (indenter shape: cylindrical, diameter 0.16 mm, height 0.5 mm, pressure leg dimensions: outer diameter 4 mm, inner diameter 1.5 mm), measurement mode: peak hold mode).

[0023] (Parameters indicating the viscoelastic term) The matrix 31 and domain 32 are measured in a viscoelastic image obtained by scanning probe microscopy, and the relationship between parameter A, which represents the viscoelastic term of the domain, and parameter B, which represents the viscoelastic term of the matrix, is such that A <Bである。 Parameters A and B can be determined by preparing sections from the elastic layer and measuring the sections with a scanning probe microscope (SPM / AFM). For example, the "S-Image" (product name) manufactured by Hitachi High-Tech Science Corporation can be used as a scanning probe microscope. Furthermore, while methods for sectioning include, for example, a sharp razor, a microtome, and focused ion beam (FIB), this disclosure uses a microtome. The sections are prepared at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center, where L is the length of the elastic layer in the longitudinal direction. Then, as shown in Figure 4, a total of three sections are prepared from cross-sections 41-43 in the thickness direction of the elastic layer. As a result, the obtained sections have cross-sections in which the domains and matrix are exposed. Furthermore, the region in which the electrophotographic component deforms when it comes into contact with another component is mainly the thickness region from the outer surface of the elastic layer to a depth of 100 μm. Therefore, the observation region is the thickness region from the surface of the elastic layer to a depth of 100 μm. Specifically, for sections 41 to 43, a square observation region with sides of 50 μm is selected within the thickness region from the outer surface to a depth of 100 μm for each section, and the viscoelastic image is observed in a total of three observation regions.

[0024] The measurement mode for viscoelastic images using SPM is the microviscoelastic dynamic force mode. The system will be in Viscoelastic Dynamic Force Mode (VE-DFM). A silicon microcantilever for DFM ("SI-DF3" (product name), manufactured by Hitachi High-Tech Science, with a spring constant of 1.9 N / m) will be used as the cantilever. Furthermore, the scanning frequency will be 0.5 Hz. VE-DFM is one of the measurement modes of SPM (Scanning Probe Microscopy). In VE-DFM, a surface topographic image can be obtained by controlling the distance between the probe and the sample to be measured so that the vibration and amplitude of the cantilever remain constant while the cantilever is resonating. In VF-DFM, the viscoelastic distribution can be imaged from the deflection amplitude of the cantilever when a periodic force is applied by making the sample vibrate slightly in the Z direction. If the sample is hard, the cantilever amplitude will be large because the sample deformation is small, and if the sample is soft, sample deformation vibration will be induced and the cantilever amplitude will be small. The obtained amplitude, converted to displacement in mV, becomes the parameter representing the viscoelastic term. Therefore, parameters A and B serve as indicators of the relationship between the hardness of the domains and the hardness of the matrix present in a single observed sample. In VF-DFM, the magnitude of the cantilever amplitude is output as voltage, so the units of parameters A and B are in mV. Furthermore, a larger value indicates higher elasticity.

[0025] After acquiring the viscoelastic image, 10 parameters representing the viscoelastic term are determined for both the matrix and the domain in each observation region. The arithmetic mean of these parameters is defined as parameter A representing the viscoelastic term in the domain and parameter B representing the viscoelastic term in the matrix. The measurement procedure will be described later.

[0026] The ratio (A / B) of parameter A(mV) to parameter B(mV) is preferably 0.65 or less, more preferably 0.60 or less, and even more preferably 0.50 or less. The smaller A / B, the greater the difference in viscoelasticity between the matrix and the domain, making it easier to achieve both hardness and deformation recovery. There is no particular lower limit to A / B, but a smaller value is preferable. Specifically, for example, it is 0.10. Preferred ranges for A / B are, for example, 0.10 to 0.65, 0.10 to 0.60, 0.10 to 0.50, particularly 0.10 to 0.40, and even more preferably 0.10 to 0.30. Parameters A and B can be adjusted, for example, by the elastic moduli of the domains and the matrix. The elastic moduli of the matrix can be increased, for example, by increasing the crosslinking density of the matrix using polyisocyanate trimer compounds or polymer compounds as raw materials for matrix formation. The elastic moduli of the domains can be lowered, for example, by increasing the molecular weight of the polyether polyol used as a raw material for domain formation, which reduces the crosslinking density of the domains and thus lowers the elastic moduli.

[0027] (Recovery from deformation) When the elastic layer 3 is subjected to a Vickers indenter being brought into contact with the matrix on the outer surface of the elastic layer at a temperature of 23°C, and the Vickers indenter being pressed into the elastic layer at a loading rate of 10 mN / 30 seconds, and the load being maintained at 10 mN for 60 seconds before being unloaded, the strain 5 seconds after unloading is 1.00 μm or less. By reducing the strain after 5 seconds of unloading under the above conditions to 1.00 μm or less, streaky image defects can be suppressed when applied as a developing roller in a high-speed printer. This is because, in the short time between the operation of the high-speed printer and the development of the electrostatic latent image, the deformation of the developing roller can recover to a size less than that of a single normal toner cartridge. Furthermore, even when applied to a charging roller, the recovery from deformation is fast, making it less likely for uneven discharge to occur on the photoreceptor, thus preventing the occurrence of streaky image defects caused by uneven charging of the photoreceptor. As described above, in the elastic layer according to this disclosure, it is considered that the domains and matrix are chemically bonded by urethane bonds at the boundary between the domains and the matrix. Therefore, it is considered that the recovery from deformation of the domains when the load applied to the urethane elastomer is removed is linked to the recovery from deformation of the matrix. As a result, the elastic layer according to this disclosure The material layer exhibits extremely high recovery from deformation, and it is believed that the strain after 5 seconds of unloading can be kept within the above range. The strain after 5 seconds of unloading can be adjusted, for example, by the modulus of elasticity of the matrix, assuming that the matrix and domains are chemically bonded. Specifically, for example, the modulus of elasticity of the matrix can be increased by increasing the crosslinking density of the urethane elastomer matrix using a trimer or polymer compound of polyisocyanate as at least one of the raw materials of the urethane elastomer. The strain after 5 seconds of unloading is preferably 0.90 μm or less, and more preferably 0.80 μm or less. The lower limit of the strain after 5 seconds of unloading is not particularly limited, but is usually 0.00 μm, may be 0.05 μm, or may be 0.10 μm. For example, preferred values ​​include 0.00 to 1.00 μm, 0.00 to 0.90 μm, and 0.00 to 0.80 μm. The strain value 5 seconds after unloading shall be the value obtained by an indentation test using a microhardness tester (nanoindenter). The measurement temperature shall be 23°C. A Vickers indenter with a square pyramidal shape and a face angle of 136° shall be used for the measurement. The measurement method shall be to bring the Vickers indenter into contact with the matrix portion of the surface of the elastic layer, and to indent the Vickers indenter into the elastic layer at a speed of 10 mN / 30 seconds, maintaining a load of 10 mN for 60 seconds. Then, the load shall be removed at a speed of 10 mN / 1 second (unloading), and the strain of the elastic layer 5 seconds after unloading shall be measured. Furthermore, the measurement positions shall be a total of three locations, with the length of the elastic layer being L, being the center in the longitudinal direction of the elastic layer, and two locations at L / 4 from both ends of the elastic layer toward the center.

[0028] (Matrix modulus) The elastic modulus of the matrix 31 present in the observation area at a temperature of 23°C is preferably 1 to 13 MPa. A higher elastic modulus of the matrix increases its spring effect, allowing for faster deformation recovery. A lower elastic modulus of the matrix (13 MPa or less) reduces its hardness, further lowering the micro-rubber hardness of the elastic layer. A higher elastic modulus of the matrix (2 MPa or more) is preferable because it further increases the matrix's spring effect, accelerating deformation recovery. A lower elastic modulus of the matrix (8 MPa or less) is even more preferable because it further reduces its hardness, lowering the micro-rubber hardness of the elastic layer. As a result, image defects and edge wear caused by toner fusion are easily prevented. Specifically, the elastic modulus of the matrix is ​​more preferably 2 to 8 MPa, and even more preferably 5 to 8 MPa. The elastic modulus of the matrix can be adjusted, for example, by increasing the crosslinking density using polyisocyanate trimer compounds or polymer compounds. Normally, increasing the elastic modulus also increases the microrubber hardness of the elastic layer, but in this disclosure, since multiple low-elasticity domains are dispersed in the matrix, excessive hardening can be suppressed.

[0029] The elastic modulus of the matrix can be calculated by preparing sections of the elastic layer and measuring the sections with a scanning probe microscope (SPM / AFM). For example, the "MFP-3D-Origin" (product name) manufactured by Oxford Instruments Ltd. can be used as a scanning probe microscope. Other methods for sectioning include, for example, using a sharp razor, a microtome, or focused ion beam (FIB) spectroscopy. The sections are prepared at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center, where L is the length of the elastic layer in the longitudinal direction. Then, as shown in Figure 4, a total of three sections are prepared from cross-sections 41-43 in the thickness direction of the elastic layer. As a result, the obtained sections have cross-sections in which the domains and matrix are exposed. Furthermore, for the same reasons as the measurement of parameters indicating the viscoelastic term, the observation area of ​​sections 41-43 is any area within the thickness region corresponding to the outer surface to a depth of 100 μm of each section. Select a 50 μm square observation area and perform phase image observation in a total of three observation areas. The phase image measurement mode for SPM will be AM-AFM. A dynamic mode silicon cantilever, such as the "OMCL-AC-160TS" (product name, manufactured by Olympus Corporation, spring constant = 47.08 N / m), will be used as the cantilever. Furthermore, the scanning frequency will be 0.5 Hz. After acquiring the phase image, the force curve is measured using SPM to determine the elastic modulus of the matrix. The force curve measurement mode is set to contact mode. The distance will be 500 nm and the trigger point will be 0.01 V. The cantilever will be a silicon cantilever for dynamic mode, such as the "OMCL-AC-160TS" (product name, manufactured by Olympus Corporation, spring constant = 47.08 N / m), as described above. The scanning frequency will be 1 Hz. Ten elastic moduli of the matrix were calculated for each of the three observation areas, for a total of 30 points. The arithmetic mean of these points was used as the elastic modulus of the matrix.

[0030] (Conductive fillers contained in the matrix) The elastic layer contains a conductive filler. The conductive filler is preferably unevenly distributed within the matrix. That is, the matrix preferably contains a conductive filler. Electrophotographic components require that the elastic layer have low electrical resistance. If the electrical resistance is not sufficiently low, image defects such as low density will occur in solid images. In the elastic layer, including conductive fillers in the matrix makes it easier to achieve a low-electrical-resistance elastic layer. Furthermore, the uneven distribution of conductive fillers within the matrix makes it easier for them to exhibit the function of suppressing the increase in micro-rubber hardness of the domains.

[0031] Conductive fillers can be used without particular limitations as long as they exhibit conductivity. Examples include solid carbon materials such as carbon black, graphite, carbon nanotubes, fullerenes, graphene, and carbon nanowalls; metal powders such as silver, copper, aluminum, nickel, and iron; conductive metal oxides such as conductive tin oxide and conductive titanium oxide; and inorganic ionic substances such as lithium perchlorate, sodium perchlorate, and calcium perchlorate. These can be used individually or in combination of two or more types. Among these, solid carbon materials such as carbon black, graphite, carbon nanotubes, fullerenes, graphene, and carbon nanowalls are preferred from the viewpoint that conductivity can be imparted with only a small amount of addition. More preferably, conductive carbon blacks such as furnace black, thermal black, acetylene black, Ketjen black, PAN (polyacrylonitrile) carbon, and pitch carbon are preferred because they can be easily adjusted to the desired resistance range by appropriately selecting the particle size, structure, etc. Furthermore, carbon nanotubes are preferred from the viewpoint that conductivity can be imparted with an extremely small amount of addition.

[0032] Preferred conductive carbon blacks include Denka Black from Denka Corporation, the Ketjenblack series from Lion Corporation, and NIPex160IQ from Orion Engineered Carbons. Examples of the Ketjenblack series include Ketjenblack EC600JD, Ketjenblack EC300J, Carbon ECP, and Carbon ECP600JD.

[0033] The mechanism by which carbon black exhibits conductivity is explained by percolation theory. When the carbon black packing density is low, the electrical conductivity does not change. However, beyond a certain critical packing density, the carbon black forms conductive paths with intervals below a certain level, resulting in a rapid increase in electrical conductivity (decrease in volume resistivity), which then tends to reach a constant value.

[0034] Furthermore, in addition to conductive fillers, ionic conductive agents can also be used in the elastic layer to adjust the electrical resistance. As the ionic conductive agent, ionic conductive agents that can be used in the surface layer, as described later, can be used.

[0035] (Percentage of conductive fillers in the matrix) This section describes the proportion of conductive filler 33 contained in the matrix, as observed in a cross-section in the thickness direction of the elastic layer. The proportion of conductive filler contained in the matrix refers to the ratio of the area of ​​conductive filler contained in the matrix to the total area of ​​conductive filler present in the observation region described later. The proportion of conductive filler in the matrix can be calculated by preparing sections of the elastic layer and measuring them with a scanning electron microscope. For example, Thermo Fisher Scientific's "Helios" (trade name) can be used as a scanning electron microscope. Alternatively, measurements can also be performed using a transmission electron microscope (TEM) or a scanning probe microscope (SPM / AFM). Furthermore, examples of equipment for sectioning include sharp razors, microtomes, and focused ion beam (FIB) methods. Among the above-mentioned equipment, ultramicrotomes, which can prepare ultrathin sections, are particularly suitable for use. The sections are prepared at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center, where L is the length of the elastic layer in the longitudinal direction. Then, as shown in Figure 4, a total of three sections are prepared from cross-sections 41-43 in the thickness direction of the elastic layer. As a result, the obtained sections have cross-sections in which the domains and matrix are exposed. Furthermore, for the same reasons as the measurement of parameters indicating the viscoelastic term, the observation areas of sections 41-43 are divided into three sections: a 50 μm square observation area in the thickness region from the outer surface to a depth of 100 μm, and the proportion of conductive filler contained in the matrix is ​​calculated using these three observation areas. The detailed calculation method will be described later.

[0036] In other words, when the longitudinal length of the elastic layer is L, it is preferable that each of the three cross-sections where the domains and matrix in the thickness direction of the elastic layer are exposed—the center of the elastic layer in the longitudinal direction and two locations L / 4 from both ends of the elastic layer toward the center—is observed in a square area with sides of 50 μm in the thickness region from the outer surface of the elastic layer to a depth of 100 μm, and that each of the observation areas satisfies requirement (3). Requirement (3): The ratio of the area of ​​conductive filler contained in the matrix present in the observation region to the total area of ​​conductive filler present in the observation region is 95% or more.

[0037] The proportion of the area of ​​conductive filler contained in the matrix may be 85% or more, or 90% or more. Furthermore, there is no particular upper limit to the proportion of conductive filler contained in the matrix, but it may be 100% or 99%. For example, preferred values ​​include 85-100%, 90-100%, and 95-100%. By keeping the proportion of conductive fillers in the matrix within the above range, it is possible to prevent an increase in domain hardness, thereby achieving both low microrubber hardness and high recovery from deformation. The proportion of conductive fillers in the matrix can be increased by preparing a dispersion in step (ii) described later. Because the interface between the matrix and the domains is strongly phase-separated by the urethane reactive emulsifier, even if conductive fillers are added after step (ii), it is possible to suppress the inclusion of a large amount of conductive fillers into the domains, thereby increasing the proportion of conductive fillers in the matrix. Furthermore, the proportion of conductive fillers in the matrix can be increased by improving the dispersibility between the conductive fillers and the matrix material used. Conversely, the proportion of conductive fillers in the matrix can be decreased by improving the dispersibility between the conductive fillers and the domain material used. Specifically, by reducing the amount of hydrophilic functional groups on the surface of the conductive fillers, the proportion of conductive fillers in the matrix can be increased. The proportion of - can be increased. Also, by increasing the amount of hydrophilic functional groups on the conductive filler surface, the proportion of conductive filler contained in the matrix can be reduced.

[0038] The content of conductive filler in the elastic layer is preferably 0.02 to 5.0 mass%, based on the mass of the elastic layer. When the content of conductive filler is 0.02 mass or more, the conductivity of the elastic layer is better. Furthermore, when the content of conductive filler is 5.0 mass or less, it is easier to achieve both conductivity, low hardness, and low compression set. The content of the conductive filler is more preferably 0.05 to 4.5% by mass, and even more preferably 0.1 to 4.0% by mass. Specifically, the specific surface area is 500 m². 2 For carbon black with a concentration of less than 1 / g (for example, Denka Black manufactured by Denka Co., Ltd.), the content is preferably 1.0 to 4.5% by mass, and more preferably 1.5 to 4.0% by mass. Specific surface area of ​​500 m² 2 For carbon black with a concentration of 1 / g or more (for example, Lion's Ketjenblack series), the content is preferably 0.2 to 4.0 mass%, and more preferably 0.5 to 3.5 mass%. Also, the specific surface area is 500 m². 2In the case of tubular carbon fibers (carbon nanotubes) or needle-shaped carbon fibers (carbon nanofibers) of 1 / g or more (for example, single-walled carbon nanotubes (TUBALL®) manufactured by Oxial Corporation), the content is preferably 0.05 to 3.0 mass%, and more preferably 0.1 to 2.5 mass%. If the conductive filler is a solid carbon material, its content can be calculated using a differential thermogravimetric analyzer (TG-DTA).

[0039] Specifically, the measurement is performed using the following procedure. Using TG-DTA, a sample placed in a designated container is heated to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min and held for 10 minutes. Then, it is cooled to 400°C at a cooling rate of 10°C / min, and the weight loss W1 (%) from the start of measurement is measured. Next, the temperature is heated again to 800°C in an air atmosphere at a heating rate of 10°C / min, and the weight loss W2 (%) from the start of measurement is measured. The content of conductive filler (solid carbon material) can be calculated as the difference between W2 and W1 (W2 - W1 (%)).

[0040] (Cross-sectional area and number of domains) This paper describes the cross-sectional area and number of domains 32 of the urethane elastomer observed in the cross-section in the thickness direction of the elastic layer. When the longitudinal length of the elastic layer is L, it is preferable that each of the following requirements (2-1) and requirements (2-2) are met when an observation area of ​​a square with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm for each of the cross-sections in the thickness direction of the elastic layer where the domains and matrix are exposed, at a total of three locations: the center of the elastic layer in the longitudinal direction and two locations L / 4 from both ends of the elastic layer toward the center. Requirement (2-1): The total area of ​​the domains present within the observation area is between 15% and 45% of the total area of ​​the observation area. Requirement (2-2): The proportion of domains within the observation area that have a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation area is 70% or more.

[0041] Regarding requirement (2-1), the microrubber hardness of the elastic layer can be kept lower by making the total cross-sectional area of ​​the domains within the observation area equal to 15% or more. Furthermore, the recovery of the deformation of the elastic layer can be made faster by making the total cross-sectional area of ​​the domains equal to 45% or less. Furthermore, the total area ratio of the cross-sectional areas of the domains present within the observation area is more preferably 20-40 area%, and even more preferably 25-35 area%. The proportion of the sum of the cross-sectional areas of the domains is, for example, the poly(1) matrix represented by equation (1). If a carbonate structure is included and the domains include a polyether structure represented by formula (2), this can be adjusted by changing the ratio of the polycarbonate structure represented by formula (1) in the matrix to the polyether structure represented by formula (2) in the domains. For example, increasing the ratio of the polyether structure represented by formula (2) increases the proportion of the total cross-sectional area of ​​the domains. Also, by keeping the ratio of the polyether structure represented by formula (2) within the above range, reversal of the matrix and domains becomes less likely, and the polyether structure represented by formula (2) is less likely to become the main component of the matrix. Furthermore, the cross-sectional area of ​​the domain can be increased, for example, by increasing the number-average molecular weight of the polyether polyol that forms the polyether structure represented by formula (2).

[0042] Regarding requirement (2-2), by setting the ratio of domains with a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation region to 70% or more of the total number of domains in the observation region, a sufficient number of domains of a size that can deform sufficiently when the elastic layer is pressed is ensured. Therefore, the microrubber hardness of the elastic layer can be made lower. In addition, because there are fewer large domains that deform excessively when a load is applied to the elastic layer, it is possible to prevent the microrubber hardness of the elastic layer from becoming too low. Furthermore, the ratio of domains having a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation region is preferably 70 to 100%, more preferably 80 to 100%, and even more preferably 90 to 100%. The ratio of domains with a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation region can be adjusted by the size of the domain's cross-sectional area. The closer the size of the domain's cross-sectional area is to the center of the above requirement range, the higher the ratio of domains meeting the above requirement. As mentioned above, the size of the domain's cross-sectional area can be adjusted by the number-average molecular weight of the polyether polyol that forms the polyether structure represented by formula (2), and it increases as the number-average molecular weight of the polyether polyol increases. In addition, the domain's cross-sectional area can be reduced by increasing the isocyanate index in the process of obtaining the first polyether, as described later, or by increasing the shear force when mixing the materials. The measurement of the total cross-sectional area of ​​domains present within the observation region, and the ratio of the number of domains with a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation region, can be performed following the method used for the proportion of conductive fillers contained in the matrix described in the previous section, and details will be described later.

[0043] Furthermore, the average cross-sectional area of ​​the domains present within the observation area is preferably 0.08 to 16.00 area%, more preferably 0.10 to 15.00 area%, and even more preferably 0.10 to 13.00 area% of the area of ​​the observation area. The above range makes it easier to adjust the ratio of domains with a cross-sectional area of ​​0.10 to 13.00% of the area of ​​the observed region. As mentioned above, the average cross-sectional area of ​​the domain can be adjusted by the number-average molecular weight of the polyether polyol that forms the polyether structure represented by equation (2), and increases as the number-average molecular weight of the polyether polyol increases. In addition, the average cross-sectional area of ​​the domain can be reduced by increasing the isocyanate index in the process of obtaining the first polyether, which will be described later, or by increasing the shear force when mixing the materials.

[0044] (Circularity of the domain) In a cross-section of the elastic layer in the thickness direction where the domains and matrix are exposed, the domains of the urethane elastomer observed in the observation area preferably have a ratio of 70% or more, more preferably 80% or more, and even more preferably 90% or more. The upper limit may be 100% or less, or 98% or less. For example, preferred ratios include 70-98%, 80-100%, and 90-100%. Domains whose circularity falls within the above range are less likely to exhibit anisotropy in the direction of shape recovery when they recover from deformation. Furthermore, a larger number (proportion) of domains with circularity within the above range leads to less anisotropy in the recovery of the elastic layer from deformation. In other words, the recovery from deformation can be made into a more isotropic elastic layer. As a result, wrinkles and other defects caused by anisotropy in deformation recovery are less likely to occur in the elastic layer after it has recovered from deformation. However, if wrinkles or other defects do occur, circumferential streak-like image defects may randomly appear along the length of the wrinkles. The circularity of the domains and the ratio of the number of domains can be measured by the method described below. The proportion of domains with a circularity of 0.60 to 0.95 can be adjusted, for example, by the rate at which the material is injected into the mold. Slowing down the injection rate reduces the shear force applied to the material, allowing it to be heat-cured while maintaining a high circularity.

[0045] When the longitudinal length of the elastic layer is L, and a square observation area with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm for each of the three cross-sections in the thickness direction of the elastic layer where the domains and matrix are exposed, at the center of the elastic layer in the longitudinal direction and at two locations L / 4 from both ends toward the center of the elastic layer, it is preferable that the average circularity of the domains present in the observation area is 0.55 to 1.00. It is more preferable that it is 0.60 to 0.98, and even more preferable that it is 0.60 to 0.95. By keeping the values ​​within the above range, it becomes easier to adjust the proportion of domains with a circularity of 0.60 to 0.95 within that range. The average circularity of a domain can be adjusted, for example, by the rate at which the material is injected into the mold. A slower injection rate reduces the shear force applied to the material, allowing for heat curing while maintaining high circularity.

[0046] (Materials for the elastic layer) The urethane elastomer will now be described. As previously mentioned, the elastic layer comprises a urethane elastomer and a conductive filler, and the urethane elastomer has a matrix 31 and a plurality of domains 32 dispersed in the matrix. In other words, the urethane elastomer has a matrix-domain structure. In this case, it is preferable that the matrix 31 has a structure that can enhance recovery from deformation, and the domain 32 has a structure that contributes to suppressing the increase in microrubber hardness. The presence of a urethane elastomer in the elastic layer can be analyzed, for example, using a spectroscopic analyzer such as a micro-infrared spectrometer or a mass spectrometer.

[0047] The matrix 31 preferably includes a polycarbonate structure represented by the following formula (1). Polyurethane obtained by reacting a polyol having a polycarbonate structure (polycarbonate polyol) with a polyisocyanate exhibits high elasticity due to strong intermolecular forces between carbonate groups. Therefore, it is preferable as a structure contained in the matrix. The matrix has at least one polycarbonate structure represented by formula (1), and preferably has a plurality thereof. When the matrix has a plurality of polycarbonate structures represented by formula (1), the polycarbonate structures can be repeating structural units. [Chemical Formula] (In formula (1), R 1 represents an alkylene group having 3 to 9 carbon atoms (preferably 3 to 6).)

[0048] R in formula (1) 1 The alkylene group having 3 to 9 carbon atoms represented by may have a linear structure or a branched structure, but more preferably has a branched structure. R 1 is an alkylene group having 3 to 9 carbon atoms, which ensures incompatibility with the domain containing the polyether structure represented by the following formula (2) described later, and allows clear phase separation between the matrix and the domain. This makes it possible to more reliably exhibit the two functions of the urethane elastomer: softness and quick recovery from deformation. Furthermore, R 1 is an alkylene group having a branched structure with 3 to 9 carbon atoms (preferably 4 to 9), which appropriately suppresses intermolecular forces between carbonate groups and prevents the matrix from becoming excessively highly elastic. R 1 Examples include -(CH2) m -(m=3~9, preferably 3~6), -CH2C(CH3)2CH2-, -CH2CH(CH3)CH2-, -(CH2)2CH(CH3)(CH2)2-, and the like. These can be used alone or in combination of two or more. The matrix contains the polycarbonate structure represented by formula (1), and R1 However, the fact that it is an alkylene group having 3 to 9 carbon atoms can be analyzed using, for example, a spectroscopic analyzer such as a micro-infrared spectrometer or a mass spectrometer.

[0049] Domain 32 preferably contains a polyether structure represented by the following formula (2). Polyethers exhibit a low modulus of elasticity due to weak intermolecular forces between ether groups. Therefore, they are preferred as structures to be included in the domain. The domain has at least one polyether structure represented by formula (2), and preferably more than one. When the domain has more than one polyether structure represented by formula (2), the polyether structure can be a repeating structural unit. [ka] (In formula (2), R 2 This represents an alkylene group having 3 to 5 carbon atoms (preferably 4 to 5).

[0050] R in equation (2) 2 The alkylene group having 3 to 5 carbon atoms, represented by , may have a linear structure or a branched structure, but it is preferable to have a branched structure. R 2 The presence of an alkylene group with 3 to 5 carbon atoms ensures incompatibility with the matrix containing the polycarbonate structure represented by formula (1), allowing for clear phase separation of the matrix and domains. This enables the urethane elastomer to more reliably exhibit its two functions: softness and rapid recovery from deformation. Also, R 2 Because the alkylene group has a branched structure with 3 to 5 carbon atoms (preferably 4 to 5), crystallization of the domains can be suppressed, and the hardness of the domains can be more easily reduced. As a result, the domains tend to have a lower elastic modulus. R 2 For example, -(CH2) mExamples include -(m=3~5, preferably 4~5), -CH2CH(CH3)-, -CH2C(CH3)2CH2-, -CH2CH(CH3)CH2-, and -(CH2)2CH(CH3)CH2-. These can be used individually or in combination of two or more types. The domain contains a polyether structure represented by formula (2), and R 2 However, the fact that it is an alkylene group having 3 to 5 carbon atoms can be analyzed using, for example, a spectroscopic analyzer such as a micro-infrared spectrometer, or a mass spectrometer.

[0051] (Method of manufacturing urethane elastomer) An example of the manufacturing method for the above-mentioned urethane elastomer is the following steps (i) to (iii) A method having the following characteristics is an example. Step (i): A step of reacting a first polyether having at least two isocyanate groups with a first polycarbonate polyol having at least two hydroxyl groups to obtain a urethane reactive emulsifier having at least two hydroxyl groups. Step (ii): A step of mixing a urethane reactive emulsifier and a second polycarbonate polyol to obtain a dispersion in which droplets containing at least a portion of the urethane reactive emulsifier are dispersed in the second polycarbonate polyol. Step (iii): A mixture for forming an elastic layer is prepared, comprising the dispersion obtained in step (ii) and a polyisocyanate having at least two isocyanate groups; and then the urethane reactive emulsifier, the second polycarbonate polyol, and the polyisocyanate having at least two isocyanate groups in the mixture for forming the elastic layer are reacted.

[0052] Each step of the above manufacturing method will be explained using Figure 5 (conductive filler not shown). In step (i), a first polyether 51 having at least two isocyanate groups is mixed with a first polycarbonate polyol 52 having at least two hydroxyl groups. The isocyanate groups and hydroxyl groups in the mixture are reacted in the presence of a catalyst, and the two are linked via urethane bonds to obtain a urethane reactive emulsifier 53 having at least two hydroxyl groups. The urethane reactive emulsifier is a reactive emulsifier having urethane bonds.

[0053] In step (ii), the urethane-reactive emulsifier 53 obtained in step (i) is dispersed in the second polycarbonate polyol 55. Here, the urethane-reactive emulsifier can be mixed with the second polycarbonate polyol newly added in this step. Alternatively, any excess unreacted material from the first polycarbonate polyol in step (i) can also be used as the second polycarbonate polyol. The first polyether 51 contained in the urethane reactive emulsifier 53 is incompatible with the second polycarbonate polyol 55 and forms droplets 54. On the other hand, the first polycarbonate polyol 52 contained in the urethane reactive emulsifier 53 is compatible with the second polycarbonate polyol 55. Therefore, droplets 54 containing the first polyether, which constitutes a part of the urethane reactive emulsifier, are uniformly and stably dispersed in the second polycarbonate polyol 55 via the first polycarbonate polyol 52. As a result, a dispersion is obtained in which droplets 54 containing the first polyether 51 of the urethane reactive emulsifier 53 are dispersed in the second polycarbonate polyol 55. For explanatory purposes, steps (i) and (ii) are described separately, but these steps may be a series of continuous steps.

[0054] In order to incorporate the conductive filler into the matrix, it is preferable to add and disperse the conductive filler after step (ii). That is, the method for producing the urethane elastomer preferably includes a step of adding and dispersing the conductive filler to the dispersion obtained in step (ii). Alternatively, the conductive filler may be added and dispersed in step (ii). If the conductive filler is added to the second polycarbonate polyol beforehand, the viscosity of the polycarbonate polyol increases due to the high intermolecular forces, which may reduce the workability in step (ii). On the other hand, if it is added after step (ii), the viscosity does not increase excessively even if the conductive filler is added because the first polyether, which has low intermolecular forces and low viscosity, is present. Furthermore, in step (ii), the interface between the matrix and the domains is strongly phase-separated by the urethane reactive emulsifier, so even if the conductive filler is added and stirred after step (ii), a large amount of conductive filler will not enter the domains.

[0055] In step (ii), the second polycarbonate polyol 55 that disperses the droplet 54 can be the unreacted product of the first polycarbonate polyol used in step (i) with the first polyether. That is, in step (i), the first polyether By using an excess amount of the first polycarbonate polyol, a dispersion can be obtained in which the urethane reactive emulsifier 53, as described in step (ii), is dispersed in the excess first polycarbonate polyol (i.e., the second polycarbonate polyol 55). Even when an excess amount of the first polycarbonate polyol is used, additional polycarbonate polyol (the second polycarbonate polyol) can be added as a dispersion medium for the urethane reactive emulsifier. In this case, the additional polycarbonate polyol may have the same chemical composition as the first polycarbonate polyol used in step (i), or it may have a different chemical composition.

[0056] On the other hand, if in step (i) the first polycarbonate polyol and the first polyether are reacted in equivalent amounts and all of the first polycarbonate polyol is consumed, then in step (ii) a new polycarbonate polyol is used as the second polycarbonate polyol to prepare a dispersion. In this case as well, the polycarbonate polyol used as the second polycarbonate polyol may have the same chemical composition as the first polycarbonate polyol or a different one.

[0057] Finally, in step (iii), a mixture for forming an elastic layer is prepared, which includes the dispersion prepared in step (ii) and a polyisocyanate 56 having at least two isocyanate groups. Next, the hydroxyl groups of the urethane reactive emulsifier 53 or the hydroxyl groups of the second polycarbonate polyol 55 in the mixture for forming the elastic layer are reacted with the isocyanate groups of the polyisocyanate 56. In this way, the mixture for forming the elastic layer is cured by forming a network structure via urethane bonds to obtain a urethane elastomer. The urethane elastomer 500 thus obtained has a matrix domain structure in which domains 32 containing the polyether structure of the first polyether 51 are dispersed in a matrix 31 containing the polycarbonate structures of the unreacted first polycarbonate polyol 52 and the second polycarbonate polyol 55. Furthermore, the domains 32 are mainly composed of polyether structures, and the inside of the domains can be substantially free of crosslinking structures. In other words, domain 32 can exist in the matrix in a nearly liquid state. This allows the domain to have a low elastic modulus in the urethane elastomer.

[0058] Furthermore, it is believed that the domains are not simply confined within the matrix, but rather chemically bonded to the matrix by urethane bonds at the boundary between the domains and the matrix. Therefore, the recovery of the domains from deformation when the load applied to the urethane elastomer is removed can be linked to the recovery of the matrix from deformation. As a result, the elastic layer according to this disclosure is considered to have extremely high recovery properties from deformation. Moreover, because the recovery of the domains from deformation is linked to the recovery of the matrix from deformation, the elastic layer can recover from deformation more stably even when the loading and unloading of loads are repeated. Here, as described above, the domains can be substantially liquid in nature, having virtually no cross-linking structure internally. This makes the urethane elastomer even more flexible. In this case, since the substantially liquid domains that are deformed by the application of a load to the urethane elastomer have a low elastic modulus, it is considered difficult for them to recover from deformation spontaneously. However, in the urethane elastomer according to this disclosure, as described above, it is considered that the domains and the matrix are chemically bonded at the boundary with the matrix. Due to the presence of this chemical bond, even substantially liquid domains can recover well from deformation along with the deformation recovery of the matrix. Therefore, the urethane elastomer according to this disclosure, having substantially liquid domains, can achieve an even higher level of flexibility and recovery from deformation.

[0059] Furthermore, steps (i) to (ii) above are intended to disperse materials that are inherently miscible in a stable and uniform manner. This process involves stably dispersing polyethers, which are difficult to handle, in a polycarbonate polyol. Specifically, a first polyether 51 is reacted with a first polycarbonate polyol 52 to form a urethane-reactive emulsifier 53. This process yields a dispersion in which segments of the polyether corresponding to the first polyether 51 are stably and uniformly dispersed in the second polycarbonate polyol. This makes it easy to produce a urethane elastomer in which domains 32 with high circularity, small size on the order of micrometers, and a relatively uniform size distribution are dispersed in the matrix 31.

[0060] Another method for mixing materials with low compatibility is, for example, mixing and dispersing them with high shear force. However, in this method, the high shear force applied to the polyether can result in the domain shape becoming irregular and the circularity decreasing, and the size of the domains may also become non-uniform. Furthermore, the dispersion state is unstable, and aggregation of domains progresses relatively quickly. In addition, the incompatibility between the polyether and the polycarbonate polyol is not guaranteed, and the phase separation between the matrix and domains of the resulting urethane elastomer becomes unclear. For these reasons, it is difficult to obtain a urethane elastomer that provides an elastic body that is flexible and has excellent recovery from deformation, as described in this disclosure.

[0061] The first polyether has at least two isocyanate groups. Preferably, the first polyether is a polyether containing the polyether structure represented by formula (2). The first polyether can be obtained, for example, by reacting a polyether polyol having at least two hydroxyl groups and containing the polyether structure represented by formula (2) with a polyisocyanate having at least two isocyanate groups. Examples of polyether polyols include alkylene-containing polyether polyols such as polypropylene glycol, polytetramethylene glycol, copolymers of tetrahydrofuran and neopentyl glycol, and copolymers of tetrahydrofuran and 3-methyltetrahydrofuran, as well as random or block copolymers of these polyalkylene glycols. These can be used individually or in combination of two or more types.

[0062] Among polyether polyols, amorphous polyether polyols are preferred from the viewpoint of achieving incompatibility with the second polycarbonate polyol and low hardness. More preferably, the product contains at least one selected from the group consisting of polypropylene glycol, a copolymer of tetrahydrofuran and neopentyl glycol, and a copolymer of tetrahydrofuran and 3-methyltetrahydrofuran.

[0063] The number-average molecular weight of the polyether polyol is preferably 1,000 to 50,000. More preferably, it is 1,200 to 30,000. A number-average molecular weight of 1,000 or more is preferable because it ensures incompatibility with the polycarbonate polyol and clarifies the phase separation between the matrix and domains of the resulting urethane elastomer. A number-average molecular weight of 50,000 or less is preferable because it facilitates domain formation and stabilizes the phase separation morphology.

[0064] The number-average molecular weight of a polyether polyol can be calculated using the following formula (3), with respect to the hydroxyl value (mgKOH / g) and the valency of the polyether polyol. For example, the number-average molecular weight of a polyether polyol with a hydroxyl value of 56.1 mgKOH / g and a valency of 2 can be calculated to be 2000. Number-average molecular weight = 56.1 × 1000 × valency ÷ hydroxyl value (3)

[0065] Examples of polyisocyanates that react with polyether polyols include pentamethylene diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate. Examples include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, or trimer compounds (isocyanurates) or polymer compounds of these polyisocyanates, allophanate-type polyisocyanates, biuret-type polyisocyanates, and aqueous-dispersible polyisocyanates. These polyisocyanates can be used individually or in combination of two or more types. Among polyisocyanates, difunctional isocyanates (diisocyanates) having two isocyanate groups are preferred due to their high compatibility with the first polyether and ease of adjusting physical properties such as viscosity. More preferably, the polyisocyanate contains at least one selected from the group consisting of hexamethylene diisocyanate, isophorone diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, and diphenylmethane diisocyanate. Xylene diisocyanate is even more preferred.

[0066] In the process of reacting a polyether polyol with a polyisocyanate, the isocyanate index is preferably 1.2 to 5.0. Having the isocyanate index within this range reduces the amount of the first polyether-derived component that remains without forming a network structure, thereby suppressing the seepage of liquid substances from the urethane elastomer. The isocyanate index is the ratio ([NCO] / [OH]) of the number of moles of isocyanate groups in the isocyanate compound to the number of moles of hydroxyl groups in the polyol compound. The first polyether obtained by the reaction of a polyether polyol and a polyisocyanate has a structure linked via urethane bonds formed by the reaction of hydroxyl groups and isocyanate groups. Its number-average molecular weight is preferably 1,000 to 50,000, more preferably 1,200 to 30,000. The number-average molecular weight of the first polyether can be calculated using the standard polystyrene molecular weight conversion, or using the hydroxyl value (mgKOH / g) and valency. The number-average molecular weight conversion using polystyrene molecular weight conversion can be measured using high-performance liquid chromatography. For example, a high-performance GPC instrument (product name: HLC-8220GPC, manufactured by Tosoh Corporation) can be used with a column: Shodex GPCLF-804 (exclusion limit molecular weight: 2 × 10⁻¹⁶). 6 Separation range: 3 × 10 2 ~2×10 6 The measurement can be performed using two of these in series. When using the hydroxyl value and valency, it can be calculated using the following formula. For example, the number-average molecular weight of a polyol with 56.1 mg KOH / g and a valency of 2 can be calculated as 2000. Number-average molecular weight = 56.1 × 1000 × valency ÷ hydroxyl value The number-average molecular weight of the first polyether can be adjusted by changing the number-average molecular weight of the polyether polyol or polyisocyanate used, or by changing the reaction temperature and reaction time in the process of reacting the polyether polyol with the polyisocyanate.

[0067] The first polycarbonate polyol has at least two hydroxyl groups. Preferably, the first polycarbonate polyol is a polycarbonate polyol containing a polycarbonate structure represented by formula (1). Examples of the first polycarbonate polyol include a reaction product of a polyhydric alcohol and phosgene, and a ring-opening polymerization product of a cyclic carbonate ester (such as alkylene carbonate).

[0068] Examples of polyhydric alcohols include propylene glycol, dipropylene glycol, trimethylene glycol, 1,4-tetramethylenediol, 1,3-tetramethylenediol, 2-methyl-1,3-trimethylenediol, 1,5-pentamethylenediol, neopentyl glycol, 1,6-hexamethylenediol, 3-methyl-1,5-pentamethylenediol, 2,4-diethyl-1,5-pentamethylenediol, and glyceryl Examples include trimethylolpropane, trimethylolethane, cyclohexanediols (such as 1,4-cyclohexanediol), and sugar alcohols (such as xylitol and sorbitol).

[0069] Examples of alkylene carbonates include trimethylene carbonate, tetramethylene carbonate, and hexamethylene carbonate.

[0070] The number-average molecular weight of the first polycarbonate polyol is preferably 500 to 10,000, more preferably 700 to 8,000. When the number-average molecular weight is 500 or more, incompatibility with the domain is ensured when the domain contains a polyether structure represented by formula (2), and the phase separation between the matrix and the domain can be made clearer. Furthermore, by setting the number-average molecular weight to 10,000 or less, an excessive increase in the viscosity of the first polycarbonate polyol can be prevented. The number-average molecular weight of the first polycarbonate polyol can be calculated using the same method as the method for calculating the number-average molecular weight of the polyether polyol described above.

[0071] As the second polycarbonate polyol used in step (ii), the polycarbonate polyols listed above as the first polycarbonate polyols can be used. As stated above, the first polycarbonate polyol and the second polycarbonate polyol may have the same chemical composition, or they may have different compositions.

[0072] The amounts of the first polyether and the first polycarbonate polyol used are not particularly limited, and should be sufficient to disperse the droplet 54 in the second polycarbonate polyol 55 and form distinct domains. For example, the ratio of the first polyether to the first polycarbonate polyol is preferably 10:90 to 50:50 by mass, and more preferably 15:85 to 45:55.

[0073] The polyisocyanate 56 having at least two isocyanate groups used in step (iii) can be the same as the polyisocyanate reacted with the polyether polyol as exemplified above as a raw material for the first polyether. These polyisocyanates can be used individually or in combination of two or more types. As for polyisocyanate 56, from the viewpoint of increasing the elastic modulus of the matrix, it is preferable to include polyisocyanates having at least three isocyanate groups, such as polyisocyanate trimer compounds (isocyanurates) or polymer compounds, allophanate-type polyisocyanates, or biuret-type polyisocyanates, among the polyisocyanates exemplified above. More preferably, the product contains at least one selected from the group consisting of a trimer compound (isocyanurate) of pentamethylene diisocyanate, a trimer compound (isocyanurate) of hexamethylene diisocyanate, a polymer compound of diphenylmethane diisocyanate, and polymeric MDI.

[0074] Among the above, polymeric MDI is preferred. Here, polymeric MDI is a mixture of monomeric MDI and high molecular weight polyisocyanate, and is represented by the following formula (A). In formula (A), n is preferably between 0 and 4. Polymeric MDI can be commercially available, such as the Millionate MR series (manufactured by Tosoh Corporation), including the Millionate MR200 (product name). [ka]

[0075] As the polyisocyanate 56 having at least two isocyanate groups, it is preferable to use a combination of a polyisocyanate having at least three isocyanate groups, such as polymeric MDI, and a difunctional isocyanate having two isocyanate groups. This combination is preferable from the viewpoint of achieving both low hardness and low compression set, as it allows for adjustment of the crosslinking density of the matrix.

[0076] The amounts of polyisocyanate having at least three isocyanate groups and difunctional isocyanate having two isocyanate groups are not particularly limited. When mixed into the dispersion in step (iii), the ratio of difunctional isocyanate to polyisocyanate having at least three isocyanate groups is preferably 3:1 to 1:10, and more preferably 1:1 to 1:6. The amount of polyisocyanate per 100 parts by mass of the dispersion in step (iii) is also not particularly limited, and examples include 1 to 10 parts by mass and 3 to 8 parts by mass.

[0077] As catalysts, known urethane catalysts or isocyanurate catalysts (isocyanate trimerization catalysts) can be used. These may be used individually or in combination. Examples of urethane catalysts include tin-based urethane catalysts such as dibutyltin dilaurate and stanus octoate, and amine-based urethane catalysts such as triethylenediamine, tetramethylguanidine, pentamethyldiethylenetriamine, diethylimidazole, tetramethylpropanediamine, N,N,N'-trimethylaminoethylethanolamine, and 1,4-diazabicyclo[2.2.2]octane-2-methanol. These may be used individually or in combination. Among these urethane catalysts, triethylenediamine and 1,4-diazabicyclo[2.2.2]octane-2-methanol are particularly preferred in that they promote the urethane reaction.

[0078] Examples of isocyanurate catalysts include metal oxides such as Li2O,(Bu3Sn)2O, hydride compounds such as NaBH4, alkoxide compounds such as NaOCH3, KO-(t-Bu), and borates, amine compounds such as N(C2H5)3, N(CH3)2CH2C2H5, and 1,4-ethylenepiperazine (DABCO), alkaline carboxylate salt compounds such as HCOONa, Na2CO3, PhCOONa / DMF, CH3COOK, (CH3COO)2Ca, alkaline soaps, and naphthenates, alkaline formate compounds, and quaternary ammonium salt compounds such as ((R)3-NR'OH)-OCOR''. Here, Bu represents a butyl group, Ph represents a phenyl group, and R, R', and R'' represent any alkyl group. Furthermore, examples of combination catalysts (co-catalysts) used as isocyanurate catalysts include amine / epoxide, amine / carboxylic acid, and amine / alkyleneimide. These isocyanurate catalysts and combination catalysts may be used individually or in combination.

[0079] As a catalyst for urethane synthesis, N,N,N'-trimethylaminoethylethanolamine (hereinafter referred to as ETA), which acts as a urethane catalyst on its own and also exhibits isocyanurate catalyst activity, may be used.

[0080] In the method for producing urethane elastomers, a chain extender (a polyfunctional low molecular weight polyol) may be used as needed. Examples of chain extenders include glycols with a number average molecular weight of 1000 or less. Examples of glycols include ethylene glycol (EG), diethylene glycol (DEG), propylene glycol (PG), dipropylene glycol (DPG), 1,4-butanediol (1,4-BD), 1,6-hexanediol (1,6-HD), 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, xylylene glycol (terephthalyl alcohol), and triethylene glycol. Other chain extenders besides glycols include, for example, polyhydric alcohols with a valency of three or higher. Examples of polyhydric alcohols with a valency of three or higher include trimethylolpropane, glycerin, pentaerythritol, and sorbitol. These may be used individually or in combination. Additionally, additives such as pigments, plasticizers, waterproofing agents, antioxidants, conductive agents, UV absorbers, and light stabilizers can be used as needed.

[0081] (Method for manufacturing an elastic layer) The elastic layer can be formed, for example, by performing the reaction step in step (iii) of the above-described method for manufacturing urethane elastomer on the circumferential surface of the axial core. Other conditions can be the same as those for manufacturing urethane elastomer. Specifically, for example, a method is to prepare a mixture containing the dispersion prepared in step (ii) and a polyisocyanate having at least two isocyanate groups, and then cure it on the circumferential surface of the axial core. That is, a method for producing the elastic layer is, for example, a method having the following steps (2-i) to (2-iv). Step (2-i): A step of reacting a first polyether having at least two isocyanate groups with a first polycarbonate polyol having at least two hydroxyl groups to obtain a urethane reactive emulsifier having at least two hydroxyl groups. Step (2-ii): A step of mixing a urethane reactive emulsifier and a second polycarbonate polyol to obtain a dispersion in which droplets containing at least a portion of the urethane reactive emulsifier are dispersed in the second polycarbonate polyol. Step (2-iii): A step of mixing the dispersion obtained in step (2-ii) with a polyisocyanate having at least two isocyanate groups to obtain a mixture for forming an elastic layer. Step (2-iv): A step of reacting a urethane reactive emulsifier, a second polycarbonate polyol, and a polyisocyanate having at least two isocyanate groups in the elastic layer forming mixture on the circumferential surface of the core body.

[0082] As a method for curing the elastic layer-forming mixture on the circumferential surface of the shaft core, for example, a method can be used in which the elastic layer material containing the elastic layer-forming mixture is injected into a mold in which a cylindrical pipe, a piece for holding the shaft core, and the shaft core are arranged, and then heated and cured (casting method). Alternatively, a method can be used in which the elastic layer material containing the elastic layer-forming mixture is applied to the circumferential surface of the shaft core to form a coating film, and then the coating film is heated and cured. Furthermore, it is preferable to perform aging after curing the elastic layer-forming mixture on the circumferential surface of the shaft core.

[0083] (Surface layer) A surface layer may be provided on the surface of the elastic layer as needed. Examples of materials for forming the surface layer include resins, natural rubber, and synthetic rubber. Examples of resins include thermosetting resins. A fluororesin or thermoplastic resin can be used. In particular, fluororesins, polyamide resins, acrylic resins, polyurethane resins, silicone resins, or butyral resins are preferred as resins because they allow for easy control of the viscosity of the paint. These resins can be used individually or in combination of two or more types. Copolymers are also acceptable. Conductive agents can be incorporated into the surface layer to adjust the electrical resistance of the electrophotographic roller. The volume resistivity of the surface layer can be adjusted using ionic or electronic conductive agents.

[0084] Examples of ionic conductive agents include: inorganic ionic substances such as lithium perchlorate, sodium perchlorate, and calcium perchlorate; cationic surfactants such as lauryltrimethylammonium chloride, stearyltrimethylammonium chloride, octadecyltrimethylammonium chloride, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, trioctylpropylammonium bromide, and modified aliphatic dimethylethylammonium ethosulfate; amphoteric surfactants such as lauryl betaine, stearyl betaine, and dimethylalkyl lauryl betaine; quaternary ammonium salts such as tetraethylammonium perchlorate, tetrabutylammonium perchlorate, and trimethyloctadecylammonium perchlorate; and lithium organic acid salts such as lithium trifluoromethanesulfonate. These can be used individually or in combination of two or more types.

[0085] Examples of electronically conductive agents include: Metallic fine particles and fibers such as aluminum, palladium, iron, copper, and silver; conductive metal oxides such as titanium dioxide, tin oxide, and zinc oxide; composite particles obtained by surface treatment of the aforementioned metallic fine particles, fibers, or metal oxides by electrolytic treatment, spray coating, or mixed shaking; and carbon powders such as furnace black, thermal black, acetylene black, Ketjen black, PAN (polyacrylonitrile) carbon, and pitch carbon.

[0086] Other particles can also be included in the surface layer. Examples of other particles include insulating particles. Examples of insulating particles include: polyamide resins, silicone resins, fluororesins, (meth)acrylic resins, styrene resins, phenolic resins, polyester resins, melamine resins, urethane resins, olefin resins, epoxy resins, copolymers, modified products, and derivatives thereof. Rubbers such as ethylene-propylene-diene copolymer (EPDM), styrene-butadiene copolymer rubber (SBR), silicone rubber, urethane rubber, isoprene rubber (IR), butyl rubber, acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), epichlorohydrin rubber, polyolefin-based thermoplastic elastomers, urethane-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, fluororubber-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, polybutadiene-based thermoplastic elastomers, ethylene vinyl acetate-based thermoplastic elastomers, polyvinyl chloride-based thermoplastic elastomers, and chlorinated polyethylene-based thermoplastic elastomers. Among these, (meth)acrylic resin, styrene resin, urethane resin, fluororesin, and silicone resin are particularly preferred.

[0087] The materials constituting these surface layers can be dispersed using known dispersion devices that utilize beads from a sand mill, paint shaker, dyno mill, or pearl mill. The method for coating the resulting dispersion is not particularly limited, but the dipping method is preferred due to its ease of operation.

[0088] <Electrophotographic image forming apparatus> Figure 6 shows a schematic configuration of an example of an electrophotographic image forming apparatus equipped with an electrophotographic component according to one embodiment of the present disclosure. In Figure 6, the image forming apparatus consists of a photoreceptor 61, a charging device, a latent image forming device, a developing device, and a transfer device. It consists of a device, a cleaning device, and a fixing device. The photoreceptor 61 is a rotating drum having a photosensitive layer on a conductive substrate. The photoreceptor 61 is driven to rotate at a predetermined peripheral speed (process speed) in the direction of the arrow. The charging device has the function of charging the photoreceptor 61 and includes a contact-type charging roller 62 that is positioned in contact with the photoreceptor 61 by being pressed against it with a predetermined pressure. The charging roller 62 rotates in the direction of the arrow in accordance with the rotation of the photoreceptor 61. The charging roller 62 charges the photoreceptor 61 to a predetermined potential by applying a predetermined DC voltage from a charging power supply 63. A latent image forming device (not shown) performs exposure to form an electrostatic latent image on the photoreceptor 61. An exposure device such as a laser beam scanner is used as the latent image forming device. The latent image forming device forms an electrostatic latent image by irradiating the uniformly charged photoreceptor 61 with exposure light 64 corresponding to the image information. The developing device has a function to develop a toner image and includes a developing roller 65 that is positioned close to or in contact with the photoreceptor 61. The developing roller 65 develops the electrostatic latent image by reverse development using toner that has been electrostatically treated to have the same polarity as the charge polarity of the photoreceptor 61, thereby forming a toner image on the photoreceptor 61. The transfer device has the function of transferring the developed toner image onto the recording material P, and has a contact-type transfer roller 66. The transfer roller 66 rotates in the direction of the arrow in accordance with the rotation of the photoreceptor 61, and transfers the toner image from the photoreceptor 61 onto the recording material P, such as plain paper. The recording material P is transported in the direction of the arrow by a paper feeding system (not shown) having a transport member. The cleaning device has the function of recovering residual toner on the photoreceptor 61 and includes a blade-shaped cleaning member 68 and a recovery container 69. After transferring the toner image to the recording material P, the cleaning device mechanically scrapes off and recovers any residual toner remaining on the photoreceptor 61. Here, by adopting a development-simultaneous cleaning method in which residual toner is recovered in the developing device, it is possible to eliminate the need for a separate cleaning device. The fixing device has the function of fixing the toner image and consists of a fixing belt 67 having a heated roll. By rotating in the direction of the arrow, it fixes the toner image transferred onto the recording material P and discharges the recording material P outside the machine. In an image forming apparatus, the electrophotographic member described above can be suitably used as a charging roller 62 or a developing roller 65. That is, an electrophotographic image forming apparatus can be equipped with the electrophotographic member of this disclosure.

[0089] <Processing Cartridge> Figure 7 shows a schematic configuration of one embodiment of a process cartridge according to one embodiment of the present disclosure. The process cartridge integrates a photoreceptor 71, a charging roller 72, a developing roller 73, and a cleaning member 74, and is configured to be detachable from the main body of an electrophotographic image forming apparatus. The process cartridge comprises the electrophotographic members according to the above embodiment of the present disclosure, and such electrophotographic members can be suitably used as the charging roller 72 and the developing roller 73 in particular. In other words, the process cartridge is a process cartridge configured to be detachably attached to the main body of an electrophotographic image forming apparatus, and may be a process cartridge comprising the electrophotographic component of this disclosure. [Examples]

[0090] One embodiment of this disclosure will be described in more detail below with reference to examples. However, this disclosure is not limited to the examples described below.

[0091] <Example 1> (Preparation of mixture for forming an elastic layer) Polypropylene glycol (product name: PREMINOL S 4013F, manufactured by AGC Inc.) 20.1 parts by mass, Polypropylene glycol (product name: UNIOL D-400 19.2 parts by mass of (0, manufactured by NOF Corporation), 2.5 parts by mass of xylylene diisocyanate (XDI) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 500 ppm of 1,4-diazabicyclo[2.2.2]octane-2-methanol (trade name: RZETA, manufactured by Tosoh Corporation) as a curing catalyst were added to a sealed mixer and stirred for 4 hours in a sealed mixer adjusted to 100°C to synthesize a first polyether having two isocyanate groups. In addition, the amount of curing catalyst in the following examples and comparative examples is expressed in ppm by mass, based on the mass of the elastic layer-forming mixture other than the curing catalyst. 50.4 parts by mass of polycarbonate diol (product name: Duranol G3452, manufactured by Asahi Kasei Corporation) was mixed with this. The mixture was then stirred for a further 2 hours in a sealed mixer adjusted to 100°C to synthesize a urethane reactive emulsifier having two hydroxyl groups (step (2-i)), and a dispersion was obtained in which droplets containing at least a portion of the urethane reactive emulsifier were dispersed in the polycarbonate diol (step (2-ii)). 2.0 parts by mass of carbon black (product name: Denka Black Powder, manufactured by Denka Co., Ltd.) was added to this dispersion, and the mixture was stirred for 3 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to obtain a dispersion in which the carbon black was dispersed. Next, 1.0 part by mass of xylylene diisocyanate (manufactured by Tokyo Chemical Industry Co., Ltd., hereafter sometimes referred to as "XDI") and 5.0 parts by mass of polyisocyanate (product name: Millionate MR-200, manufactured by Tosoh Corporation, hereafter sometimes referred to as "MR-200") were added to the dispersion containing carbon black, and the mixture was stirred for 2 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to obtain a mixture for forming an elastic layer (step (2-iii)).

[0092] (Fabrication of electrophotographic rollers) A SUS304 stainless steel shaft with a diameter of 6 mm and a length of 250 mm was coated with a primer (product name: Metalock N-33, manufactured by Toyo Chemical Research Institute Co., Ltd.) and baked at 130°C for 30 minutes. Next, this shaft was placed concentrically in a cylindrical mold with an inner diameter of 11.5 mm, and an elastic layer forming mixture was injected into the cylindrical mold, which had been preheated to 130°C, over a period of 10 seconds. A cylindrical mold was heated at 130°C for 1 hour, then demolded, and aged at 80°C for 2 days to obtain an elastic layer (step 2-iv). Furthermore, by removing the edges of the elastic layer, an electrophotographic roller with a length of 225 mm and an elastic layer thickness of 2.0 mm was obtained. The obtained electrophotographic roller was evaluated as follows.

[0093] <Evaluation method for electrophoto rollers> (Evaluation 1: Confirmation and analysis of the matrix and domain) Ultrathin sections (500 μm × 500 μm × 5 μm) were prepared from the elastic layer of an electrophotographic roller using a freeze-cutting system (product name: EM FC6, Leica Microsystems) and an ultramicrotome (product name: EM UC6, Leica Microsystems). Sections were prepared at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center. The sections prepared exposed the cross-section in the thickness direction of the elastic layer, where the domains and matrix are exposed. Mapping measurements were performed on the prepared sections using an infrared microscope and imaging system (product names: Spectrum400 (analyzer), Spotlight400 (scanner), and PerkinElmer), and mapping images were created. ATR imaging accessories were used for the measurements, with a pixel size of 1.56 μm and a resolution of 16 cm². -1 Mapping measurements were performed under the conditions of a field of view of 300 μm × 300 μm and a scan speed of 1.0 cm / s. The above mapping image is an image of the magnitude of the integrated value of the infrared absorption spectrum for each pixel. From the obtained mapping image, the presence of the matrix and domains was confirmed. Furthermore, from the infrared absorption spectrum of the matrix in the mapping image, it was confirmed that the matrix contains a structure corresponding to a polycarbonate diol. Furthermore, from the infrared absorption spectra of the domains in the mapping images, it was confirmed that the domains contain structures corresponding to polypropylene glycol. Specifically, it was confirmed that the matrix contains a carbonate structure represented by formula (1), and the domains contain an ether structure represented by formula (2).

[0094] (Evaluation 2: Measurement of micro-rubber hardness) The microrubber hardness of the elastic layer was measured using a microrubber hardness tester (product name: MD-1capa, manufactured by Polymer Instruments Co., Ltd.). For the measurement, the electrophotographic roller was left in an environment of 23°C for more than 24 hours, and the measurement was performed using a measuring device placed in the same environment. A type A indenter (indenter shape: height 0.50 mm, diameter 0.16 mm, cylindrical, pressure leg dimensions: outer diameter 4 mm, inner diameter 1.5 mm) was used, and the measurement mode was set to peak hold mode. The micro-rubber hardness was measured at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center. The micro-rubber hardness was measured once at each measurement location at a temperature of 23°C.

[0095] (Evaluation 3: Measurement of parameters indicating the viscoelastic term) In the same manner as in Evaluation 1, ultrathin sections were prepared with exposed domains and matrix in cross-sections from a total of three locations: the center of the elastic layer in the longitudinal direction, and two locations L / 4 extending from both ends of the elastic layer toward the center. Within the thickness region of each section, from the outer surface to a depth of 100 μm, an arbitrary square observation area with sides of 50 μm was selected, and viscoelastic images were measured in a total of three observation areas using a scanning probe microscope (product name: S-Image, manufactured by SII Nanotechnology Co., Ltd.). The measurement mode for viscoelastic images was set to VE-DFM. The cantilever used was "SI-DF3" (product name, manufactured by Hitachi High-Tech Science Corporation, spring constant = 1.9 N / m). Furthermore, the scanning frequency was set to 0.5 Hz. From the obtained viscoelastic images, 10 parameters representing the viscoelastic term were calculated for both the matrix and the domain in each observation region. From the arithmetic mean of these parameters, parameter A(mV) representing the viscoelastic term in the domain and parameter B(mV) representing the viscoelastic term in the matrix were determined. Furthermore, the exposure of domains and the matrix in the cross-section was confirmed by viscoelastic imaging using SPM.

[0096] (Evaluation 4: Measurement of the recovery from deformation of the elastic layer) The recovery from deformation of the elastic layer was evaluated by an indentation test using a nanoindenter (product name: HM2000, manufactured by Fischer Instruments Co., Ltd.) at a temperature of 23°C. For the measurement, the electrophotographic roller was left in an environment of 23°C for more than 24 hours, and the measurement was performed using a measuring device placed in the same environment. The measurement locations were set at the center of the elastic layer in the longitudinal direction, and at two locations L / 4 from both ends of the elastic layer toward the center, for a total of three locations. In the indentation test, a Vickers indenter was brought into contact with the matrix on the outer surface of the elastic layer, and the Vickers indenter (square pyramidal type, face angle 136°) was pressed into the elastic layer at a loading rate of 10 mN / 30 seconds, and the load of 10 mN was maintained for 60 seconds. After that, the load was removed at a removal rate of 10 mN / second, and the strain 5 seconds after the completion of removal was measured once at each measurement location.

[0097] (Rating 5: Measurement of the matrix's elastic modulus) In the same manner as in Evaluation 1, ultrathin sections were prepared from a total of three locations: the center of the elastic layer in the longitudinal direction, and two locations L / 4 extending from both ends of the elastic layer toward the center. These sections exposed the cross-sections in which the domains and matrix were exposed. A 50 μm square observation area was placed at an arbitrary position within the region corresponding to the thickness range from the outer surface of the elastic layer to a depth of 100 μm in each section. Then, a scanning probe microscope (product name: MFP-3D-Origin, Oxford) was used to examine a total of three observation areas. Phase images were observed using a D Instruments Corporation (D Instruments Corporation) scanner. The phase image measurement mode was AM-AFM. The cantilever used was the "OMCL-AC-160TS" (product name, manufactured by Olympus Corporation, spring constant = 47.08 N / m). The scanning frequency was set to 0.5 Hz. The elastic modulus of the matrix was determined from the obtained phase image by measuring the force curve using the scanning probe microscope described above. The force curve measurement mode was contact mode, the force distance was 500 nm, and the trigger point was 0.01 V. A cantilever, "OMCL-AC-160TS" (product name, manufactured by Olympus Corporation, spring constant = 47.08 N / m), was used. Furthermore, the scanning frequency was set to 1 Hz. For each observation area, the elastic modulus of the matrix was calculated at 10 points, and the arithmetic mean of each was calculated. Furthermore, the exposure of domains and matrices in the cross-section was confirmed by SPM phase imaging.

[0098] (Evaluation 6: Evaluation of the area ratio of conductive fillers present in each of the matrix and domains) Sections (500 μm × 500 μm × 100 nm) were prepared from an electrophotographic roller using a freeze-cutting system (product name: EM FC6, Leica Microsystems) and an ultramicrotome (product name: EM UC6, Leica Microsystems). Sections were prepared at three locations: the center of the elastic layer in the longitudinal direction, and two locations at L / 4 from both ends of the elastic layer toward the center. These sections exposed the cross-section of the elastic layer in the thickness direction, where the domains and matrix are exposed. A 50 μm square observation area was placed at an arbitrary position within the region corresponding to the thickness range from the outer surface of the elastic layer to a depth of 100 μm in each section. Then, using a high-resolution electron energy loss spectroscopy microscope (product name: H-7100FA, Hitachi High-Technologies Corporation) that combines transmission electron microscopy (TEM) and electron energy loss spectroscopy (EELS), TEM images and oxygen atom mapping images (hereinafter also simply referred to as "mapping images") of the observation areas were obtained under the conditions of an acceleration voltage of 100 kV, observation magnification of 3,000x, and beam diameter of 2 nm.

[0099] TEM images confirmed the presence of both a matrix and domains in the observed region. Furthermore, the mapping images allowed for the identification of regions without oxygen atoms, i.e., carbon black (conductive filler), as distinct from the urethane elastomer regions. Based on the TEM and mapping images, the carbon black present in the matrix and the carbon black present in the domains were identified. Next, the mapping image was binarized using image processing software (product name: ImageProPlus, manufactured by MediaCybernetics) to obtain a binarized image for analysis, separating the carbon black portion from the urethane elastomer portion. The threshold for binarization was determined from the brightness distribution of the mapping image based on Otsu's algorithm described in Non-Patent Document 1. Next, using the counting function of the image processing software, the total area of ​​carbon black (conductive filler) present in the matrix within the observation region and the total area of ​​carbon black (conductive filler) present in the domains within the observation region were calculated from the obtained binarized image. Then, the ratio (area ratio) of the total area of ​​carbon black present in the matrix to the total area of ​​carbon black present in the observation region was calculated.

[0100] (Evaluation 7: Measurement of domain cross-sectional area and number) For each of the three viscoelastic images obtained in Evaluation 3, 256 grayscale levels were applied using image processing software (product name: ImageProPlus, manufactured by MediaCybernetics). The image was converted to a grayscale image, and then binarized to obtain a binarized image for analysis. The threshold for binarization was determined from the luminance distribution of the monochrome image based on Otsu's algorithm described in Non-Patent Document 1. Furthermore, from the obtained binarized images, the cross-sectional area of ​​the domains, the number of domains, and the average cross-sectional area of ​​the domains were calculated using the counting function of the image processing software mentioned above. However, among those identified as domains by the counting function, domains with a cross-sectional area of ​​less than 0.05% of a 50 μm square observation area were considered noise and removed from the data. Then, the ratio (area %) of the total cross-sectional area of ​​the domains in each observation area to the area of ​​the observation area was calculated. Furthermore, within each observation region, the number of domains whose cross-sectional area is between 0.1% and 13.0% of the area of ​​the observation region was determined, and the ratio (area %) of the number of domains with a cross-sectional area between 0.1% and 13.0% of the area of ​​the observation region was calculated.

[0101] (Evaluation 8: Measurement of domain circularity and number) From the binarized images obtained in Evaluation 7, the circularity of the domains and the mean circularity were calculated using the counting function of the image processing software described above. However, noise was removed from the data in the same manner as in Evaluation 7. Then, the number of domains with a circularity of 0.60 to 0.95 within each observation area was counted, and the ratio (number %) of the number of domains with a circularity of 0.60 to 0.95 to the total number of domains within each observation area was calculated.

[0102] (Rating 9: Evaluation for streaky image defects) A color laser printer (product name: LBP7700C, manufactured by Canon Inc.) and a process cartridge incorporating an electrophotographic roller as a developing roller were exposed to an environment of 23°C / 50% RH for 24 hours, after which image evaluation was performed. Specifically, a process cartridge incorporating an electrophotographic roller as a developing roller was installed in the color laser printer described above. Then, ten halftone images (images with horizontal lines of 1 dot width and 2 dot spacing perpendicular to the rotation direction of the photoreceptor) were printed in succession, and the resulting images were visually inspected to determine streaky image defects according to the following two criteria. <Evaluation of streaky image defects 9-1> Rank A: No streaky image defects were observed from the first image. Rank B: Only the first image shows a streaky image defect. Rank C: Streaky image defects are also observed in the second and subsequent images. <Evaluation of streaky image defects 9-2> Rank A: No streaky image defects are observed along the entire longitudinal direction of the electrophotographic roller. Rank B: Streaky image defects are observed in a portion of the longitudinal region of the electrophotographic roller. Rank C: Streaky image defects are observed over a wide area in the longitudinal direction of the electrophotographic roller and are noticeable.

[0103] (Rating 10: Evaluation of edge wear, toner fusion, and image defects caused by toner fusion) The above-mentioned color laser printer and a process cartridge incorporating an electrophotographic roller as a developing roller were allowed to acclimate for 24 hours in an environment of 23°C / 50% RH. Subsequently, the electrophotographic roller was mounted on the aforementioned color laser printer as a developing roller, and 10,000 images were continuously printed, each depicting horizontal lines with a width of 2 dots and a spacing of 50 dots. During the continuous printing of 10,000 sheets, the developing roller was removed every 1,000 sheets and visually inspected. The wear on the edges of the developing roller and the fusion of toner were judged according to the following criteria. <Evaluation 10-1: Evaluation of wear on the edges> The number of prints produced when wear was observed on the edge of the developing roller was defined as the number of prints produced. <Evaluation 10-2: Evaluation of toner fusion> The number of printed pages at which toner fusion was observed on the developing roller was defined as the number of pages produced.

[0104] <Evaluation 10-3: Evaluation of image defects caused by toner fusion> During the continuous printing of 10,000 images, the printed images were checked every 10 images. If image defects were found, such as toner being transferred to the paper at intervals equivalent to one rotation of the electrophotographic roller in areas other than the horizontal lines, printing was paused and the electrophotographic roller was removed from the process cartridge. If the location of the image defect matched the location and size of the toner fusion on the electrophotographic roller, the number of printed images at the time of the pause was considered the number of images with image defects caused by toner fusion.

[0105] (Rating 11: Solid Image Density Evaluation) A color laser printer (product name: LBP7700C, manufactured by Canon Inc.) and a process cartridge incorporating an electrophotographic roller as a developing roller were exposed to an environment of 15°C / 10%RH for 24 hours. After that, one full-surface solid image was printed in the same environment, and the density was evaluated. Density was measured using a spectrophotometer: X-Rite504 (product name, S.D.G. Corporation). The image density was calculated as the average value of 15 measurements taken at arbitrary points on each full-screen image. Images meeting the following criteria were classified as "OK," and those not meeting them were classified as "NG." If a full-screen image meets the following criteria, it can be judged that the image density is sufficient. Criterion: The average value of 15 measurements taken at arbitrary points on a single full-screen image must be 1.3 or higher.

[0106] <Examples 2-7, 9-12, 14, 15, 18> An elastic layer was formed in the same manner as in Example 1, except that the materials shown in Table 4 were used in the proportions shown in Table 4 to prepare the mixture for forming the elastic layer. Electrophotographic rollers according to each example were then fabricated. The obtained electrophotographic rollers were evaluated in the same manner as in Example 1. Details of the materials in Table 4 are shown in Tables 1, 2, and 3. The same applies to the following examples.

[0107] <Example 8> An electrophotographic roller according to Example 8 was fabricated in the same manner as in Example 1, except that the materials shown in Table 4 were used in the proportions shown in Table 4 to prepare the elastic layer forming mixture, and the mixture was injected into the cylindrical mold for 5 seconds. The resulting electrophotographic roller was evaluated in the same manner as in Example 1.

[0108] <Examples 13, 16, 17> An elastic layer was formed in the same manner as in Example 1, except that the materials shown in Table 4 were used in the proportions shown in Table 4 to prepare the elastic layer forming mixture, and the mixture was injected into the cylindrical tube for 3 seconds. Electrophotographic rollers according to each example were then manufactured. The obtained electrophotographic rollers were evaluated in the same manner as in Example 1. [Table 1]

[0109] In the table, the tetrahydrofuran-neopentyl glycol copolymer is a polyether glycol represented as HO-(CH2CH2CH2CH2O)m-(CH2C(CH3)2CH2O)n-OH. That is, regarding the number of carbon atoms in the tetrahydrofuran-neopentyl glycol copolymer, the notation 4 (straight chain) + 5 (branched) means R 2 This shows that it contains both a straight-chain structure with 4 carbon atoms and a branched structure with 5 carbon atoms. [Table 2]

[0110] In the table, Kuraray Polyol C-2090 (manufactured by Kuraray Co., Ltd.) has a number-average molecular weight of 2000 and a hydroxyl value of 56.3 mgKOH / g, and is a polycarbonate polyol having a structure corresponding to 1,6-hexanediol and a structure corresponding to 3-methyl-1,5-pentanediol. That is, regarding the number of carbon atoms in polycarbonate diols and polycarbonate polyols, for example, the notation 6 (linear) + 6 (branched) is R 1This indicates that it contains both a linear structure with 6 carbon atoms and a branched structure with 6 carbon atoms. Furthermore, Kuraray Polyol P-2050 is a polyester polyol that has a structure corresponding to adipic acid and a structure corresponding to 3-methyl-1,5-pentanediol. [Table 3] [Table 4]

[0111] <Comparative Example 1> (Preparation of mixture for forming an elastic layer) Polyether having two isocyanate groups was synthesized by adding 24.9 parts by mass of polypropylene glycol (product name: PREMINOL S 4013F, manufactured by AGC Inc.), 24.0 parts by mass of polypropylene glycol (product name: UNIOL D-4000, manufactured by NOF Corporation), 3.1 parts by mass of xylylene diisocyanate (XDI) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 500 ppm of 1,4-diazabicyclo[2.2.2]octane-2-methanol (product name: RZETA, manufactured by Tosoh Corporation) as a curing catalyst to a sealed mixer and stirring for 4 hours in a sealed mixer adjusted to 100°C. 41.5 parts by mass of polycarbonate diol (product name: Duranol G3452, manufactured by Asahi Kasei Corporation) was mixed with this. Subsequently, the mixture was stirred for a further 2 hours in a sealed mixer adjusted to 100°C to synthesize a urethane reactive emulsifier having two hydroxyl groups, and a dispersion was obtained in which droplets containing at least a portion of the urethane reactive emulsifier were dispersed in the polycarbonate diol. 2.0 parts by mass of carbon black (product name: Denka Black Powder, manufactured by Denka Co., Ltd.) was added to this dispersion, and the mixture was stirred for 3 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to obtain a dispersion in which the carbon black was dispersed. Next, 0.1 parts by mass of xylylene diisocyanate (XDI) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4.6 parts by mass of polyisocyanate (product name: Millionate MR-200, manufactured by Tosoh Corporation) are added to the dispersion containing carbon black, and the mixture is stirred for 2 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to form an elastic layer. A mixture was obtained. An electrophotographic roller according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the elastic layer-forming mixture obtained in this manner was used. The obtained electrophotographic roller was evaluated in the same manner as in Example 1.

[0112] Regarding the results of Evaluation 1, the matrix and domains were clearly phase-separated. Furthermore, it was confirmed that the matrix contained structures corresponding to polypropylene glycol, and the domains contained structures corresponding to polycarbonate diol. In other words, the relationship between domains and matrix was reversed compared to the urethane elastomer in Example 1.

[0113] <Comparative Example 2> (Preparation of mixture for forming an elastic layer) 20.1 parts by mass of polypropylene glycol (product name: PREMINOL S 4013F, manufactured by AGC Inc.), 19.2 parts by mass of polypropylene glycol (product name: UNIOL D-4000, manufactured by NOF Corporation), and 500 ppm of 1,4-diazabicyclo[2.2.2]octane-2-methanol (product name: RZETA, manufactured by Tosoh Corporation) as a curing catalyst were added to a sealed mixer and stirred for 2 hours in a sealed mixer adjusted to 100°C. 50.4 parts by mass of polycarbonate diol (product name: Duranol G3452, manufactured by Asahi Kasei Corporation) was mixed into this. Then, the mixture was stirred for a further 2 hours in a sealed mixer adjusted to 100°C. Furthermore, 2.0 parts by mass of carbon black (product name: Denka Black Powder, manufactured by Denka Co., Ltd.) was added, and the mixture was stirred for 3 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm. To this, 3.5 parts by mass of xylylene diisocyanate (XDI) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5.0 parts by mass of polyisocyanate (product name: Millionate MR-200, manufactured by Tosoh Corporation) were added. The resulting mixture was stirred for 2 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to obtain a mixture for forming an elastic layer. An elastic layer was formed in the same manner as in Example 1, except that this elastic layer-forming mixture was used, and an electrophotographic roller according to Comparative Example 2 was prepared. The obtained electrophotographic roller was evaluated in the same manner as in Example 1. In this comparative example, the same raw materials as in Example 1 were used. However, a urethane reactive emulsifier was not synthesized, and therefore, a dispersion in which droplets containing at least a portion of the urethane reactive emulsifier were dispersed in polycarbonate diol was not formed. Regarding the results of Evaluation 1 of the electrophotographic roller obtained by this comparative example, a matrix and domains were observed, but the boundary between the matrix and domains was extremely unclear. The reason for this is not clear, but the elastic layer according to this comparative example was manufactured without going through the process of forming a dispersion in which droplets containing at least a portion of the urethane reactive emulsifier were dispersed in polycarbonate diol. Therefore, during the formation process of the elastic layer, although the polycarbonate diol and polypropylene glycol undergo phase separation due to the difference in compatibility between polypropylene glycol and polycarbonate diol, a region where polycarbonate diol and polypropylene glycol are mixed is formed around the droplet containing the polycarbonate diol, which is thought to have resulted in an unclear boundary between the matrix and the domains. Furthermore, in the elastic layer of this comparative example, it is thought that almost no urethane bonds are formed at the interface between the domains and the matrix. As a result, the result of Evaluation 4 is thought to have become larger at 3.00 μm.

[0114] <Comparative Example 3> (Preparation of mixture for forming an elastic layer) 46.6 parts by mass of polycarbonate diol (product name: Kuraray Polyol C-2090, manufactured by Kuraray Co., Ltd.), 44.8 parts by mass of flexible resin particles, silicone particles (product name: KMP-598, manufactured by Shin-Etsu Chemical Co., Ltd.), and 1,4-diazabicyclo as a curing catalyst. [2.2.2] 500 ppm of octane-2-methanol (product name: RZETA, manufactured by Tosoh Corporation) was added to a sealed mixer and stirred for 4 hours in a sealed vacuum mixer adjusted to 100°C. Furthermore, 2.0 parts by mass of carbon black (product name: Denka Black, manufactured by Denka Co., Ltd.) was added, and the mixture was stirred for 3 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm. To this, 2.6 parts by mass of xylylene diisocyanate (XDI) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4.2 parts by mass of polyisocyanate (product name: Millionate MR-200, manufactured by Tosoh Corporation) were added. The resulting mixture was stirred for 2 minutes in a self-rotating vacuum degassing mixer at a rotational speed of 800 rpm and an orbital speed of 1600 rpm to obtain a mixture for forming an elastic layer. An elastic layer was formed in the same manner as in Example 1, except that this elastic layer-forming mixture was used, and an electrophotographic roller according to Comparative Example 3 was fabricated. The obtained electrophotographic roller was evaluated in the same manner as in Example 1. In the evaluation of the electrophotographic roller according to this comparative example, the silicone particles were considered as domains for evaluation.

[0115] <Comparative Example 4> (Preparation of mixture for forming an elastic layer) 100.0 parts by mass of NBR (product name: N230SV, manufactured by JSR Corporation), 50.0 parts by mass of carbon black (product name: Toka Black #7360, manufactured by Tokai Carbon Co., Ltd.), 70.0 parts by mass of calcium carbonate (product name: Nanox #30, manufactured by Maruo Calcium Co., Ltd.), 7.0 parts by mass of zinc oxide (product name: Zinc Oxide, manufactured by Sakai Chemical Industry Co., Ltd.), and 2.8 parts by mass of zinc stearate (product name: SZ-2000, manufactured by Sakai Chemical Industry Co., Ltd.) were mixed in a pressurized kneader for 16 minutes under conditions of a filling rate of 70 vol% and a blade rotation speed of 30 rpm to obtain unvulcanized rubber for matrix formation. Next, 100.0 parts by mass of SBR (product name: Toughden 2003, manufactured by Asahi Kasei Corporation), 5.0 parts by mass of zinc oxide (product name: Zinc Oxide, manufactured by Sakai Chemical Industry Co., Ltd.), and 2.0 parts by mass of zinc stearate (product name: SZ-2000, manufactured by Sakai Chemical Industry Co., Ltd.) were mixed in a pressurized kneader for 16 minutes under conditions of a filling rate of 70 vol% and a blade rotation speed of 30 rpm to obtain unvulcanized rubber for domain formation.

[0116] Furthermore, 65.0 parts by mass of unvulcanized rubber for matrix formation and 35.0 parts by mass of unvulcanized rubber for domain formation were mixed in a pressurized kneader for 16 minutes under conditions of a filling rate of 70 vol% and a blade rotation speed of 30 rpm to obtain an unvulcanized rubber mixture. The obtained unvulcanized rubber mixture (100.0 parts by mass), sulfur (trade name: Sulfac PMC, manufactured by Tsurumi Chemical Industries, Ltd.), and tetrabenzylthioram disulfide (trade name: TBZTD, manufactured by Sanshin Chemical Industries, Ltd.) were passed through an open roll with the front roll rotation speed at 10 rpm, the rear roll rotation speed at 8 rpm, and the roll gap at 2 mm for a total of 20 turns from left to right. Then, with the roll gap at 0.5 mm, the mixture was passed through 10 times to obtain a mixture for forming an elastic layer.

[0117] (Fabrication of electrophotographic rollers) A SUS304 stainless steel shaft with a diameter of 6 mm and a length of 250 mm was coated with a primer (product name: Metalock N-33, manufactured by Toyo Chemical Research Institute Co., Ltd.) and baked at 130°C for 30 minutes. Next, a die with an inner diameter of 14.0 mm was attached to the tip of a crosshead extruder, which had a core supply mechanism and an unvulcanized rubber roller discharge mechanism, and the crosshead extruder was preheated to 80°C. The conveying speed of the core was adjusted to 60 mm / sec, and an elastic layer forming mixture was supplied from the extruder to coat the outer circumference of the core with the elastic layer forming mixture inside the crosshead, thereby obtaining an unvulcanized rubber roller. The obtained unvulcanized rubber roller was heated in a 170°C hot air vulcanization furnace for 60 minutes to obtain a roller in which an elastic layer was formed on the outer circumference of the shaft. Then, the edges of the elastic layer were removed and the surface of the elastic layer was rotated. By polishing with a grinding wheel, an electrophotographic roller with a length of 225 mm and an elastic layer thickness of 2.0 mm was obtained. The obtained electrophotographic roller was evaluated in the same manner as in Example 1.

[0118] The evaluation results for Examples 1-18 and Comparative Examples 1-3 are shown in Tables 5-1 to 5-4 and Table 6. [Table 5-1] [Table 5-2] [Table 5-3] [Table 5-4] In Tables 5-1 to 5-4, M represents the matrix, D represents the domain, A and B represent the parameters A and B that indicate the viscoelastic term, respectively, and PPG represents polypropylene glycol. [Table 6]

[0119] The electrophotographic rollers in Examples 1-18 had low microrubber hardness in the elastic layer, and multiple domains were dispersed in the matrix containing urethane elastomer. Furthermore, parameter B, which represents the viscoelastic term of the matrix, was larger than parameter A, which represents the viscoelastic term of the domains, and the circularity of the domains was high, as was the elastic modulus of the matrix, resulting in good results in evaluating streak-like image defects. In addition, although toner fusion was observed in some electrophotographic rollers, no image defects caused by toner fusion occurred.

[0120] On the other hand, in the electrophotographic roller according to Comparative Example 1, parameter A, which represents the viscoelastic term of the domain, was larger than parameter B, which represents the viscoelastic term of the matrix. As a result, since A > B was not satisfied, an excessive decrease in microrubber hardness occurred, and edge wear occurred. The electrophotographic roller in Comparative Example 2 formed a matrix domain structure by mechanically separating the phases of the polyether and urethane reactive emulsifier without going through the process of synthesizing the polyether. As a result, the phase separation was unclear, and the circularity of the domains was reduced. Consequently, the microrubber hardness was less than 20 degrees, the strain was 3 μm, and edge wear and streaky images occurred.

[0121] In Comparative Example 3, the electrophotographic roller used flexible particles as domains, but in order to maintain the shape of the particles, parameter A, which represents the viscoelastic term, was much larger than that of the domains in this disclosure, and parameter B, which represents the viscoelastic term of the matrix, also had to be increased. As a result, the microrubber hardness became 60. Then, toner fusion occurred. In image evaluation, image defects caused by toner fusion occurred in 8,410 images. The electrophotographic roller in Comparative Example 4 used vulcanized rubber as the material for the elastic layer, resulting in low wear resistance and edge abrasion.

[0122] This disclosure relates to the following configuration. (Composition 1) An electrophotographic component, wherein the electrophotographic component has a conductive elastic layer, The elastic layer comprises a urethane elastomer and a conductive filler. The urethane elastomer has a matrix and a plurality of domains dispersed in the matrix, The relationship between parameter A, which represents the viscoelastic term of the domain, and parameter B, which represents the viscoelastic term of the matrix, as measured in a viscoelastic image obtained by scanning probe microscopy of a cross-section of the elastic layer in which the domain and the matrix are exposed, is A <Bであり、 The microrubber hardness of the elastic layer at a temperature of 23°C is 20 to 50 degrees. An electrophotographic member characterized in that, at a temperature of 23°C, a Vickers indenter is brought into contact with the matrix on the outer surface of the elastic layer, the Vickers indenter is pressed into the elastic layer at a loading rate of 10 mN / 30 seconds, the load of 10 mN is maintained for 60 seconds, and then the load is removed, and the strain 5 seconds after unloading is 1.00 μm or less. (Configuration 2) The electrophotographic member according to configuration 1, wherein the conductive filler is conductive carbon black. (Composition 3) When the longitudinal length of the elastic layer is L, and a total of three locations: the center of the elastic layer in the longitudinal direction and two locations L / 4 from both ends of the elastic layer toward the center, a total of three locations, in the thickness direction of the elastic layer where the domain and the matrix are exposed, an observation area with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm, such that each of the observation areas satisfies requirements (1) and (2), the electrophotographic member according to configuration 1 or 2. Requirement (1): The total cross-sectional area of ​​the domains present within the observation area is 15 to 45% of the area of ​​the observation area. Requirement (2): The proportion of domains within the observation region that have a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation region is 70% or more. (Composition 4) An electrophotographic member according to any one of configurations 1 to 3, wherein the proportion of domains with a circularity of 0.60 to 0.95 in the observation area is 70 percent or more. (Composition 5) The matrix includes a polycarbonate structure represented by formula (1), and The electrophotographic member according to any one of configurations 1 to 4, wherein the domain includes a polyether structure represented by formula (2). TIFF0007955132000013.tif26170(In formula (1), R 1 This represents an alkylene group with 3 to 9 carbon atoms. TIFF0007955132000014.tif16170(In formula (2), R 2This represents an alkylene group with 3 to 5 carbon atoms. (Composition 6) The aforementioned R 1 The electrophotographic component according to configuration 5, wherein the alkylene group has a branched structure with 3 to 9 carbon atoms. (Composition 7) The aforementioned R 2 The electrophotographic component according to configuration 5 or 6, wherein the alkylene group has a branched structure with 3 to 5 carbon atoms. (Composition 8) When the longitudinal length of the elastic layer is L, and a total of three locations where the domain and matrix in the thickness direction of the elastic layer are exposed, namely at the center of the elastic layer in the longitudinal direction and at two locations L / 4 from both ends of the elastic layer toward the center, an observation area with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm, the electrophotographic member according to any of configurations 1 to 7, wherein each of the observation areas satisfies requirement (3). Requirement (3): The ratio of the area of ​​conductive filler contained in the matrix present in the observation region to the total area of ​​conductive filler present in the observation region is 95% or more. (Composition 9) An electrophotographic member according to any one of configurations 1 to 8, wherein the ratio value of parameter A to parameter B (A / B) is 0.65 or less. (Composition 10) A process cartridge configured to be detachably attached to the main body of an electrophotographic image forming apparatus, comprising an electrophotographic component as described in any of configurations 1 to 9. (Composition 11) An electrophotographic image forming apparatus comprising an electrophotographic component described in any of configurations 1 to 9.

Claims

1. An electrophotographic component, wherein the electrophotographic component has a conductive elastic layer, The elastic layer comprises a urethane elastomer and a conductive filler. The urethane elastomer has a matrix and a plurality of domains dispersed in the matrix, In a viscoelastic image of a cross-section of the elastic layer where the domain and the matrix are exposed, measured using a scanning probe microscope, the relationship between parameter A, which represents the viscoelastic term of the domain, and parameter B, which represents the viscoelastic term of the matrix, is A < B. The microrubber hardness of the elastic layer at a temperature of 23°C is 20 to 50 degrees. An electrophotographic member characterized in that, at a temperature of 23°C, a Vickers indenter is brought into contact with the matrix on the outer surface of the elastic layer, the Vickers indenter is pressed into the elastic layer at a loading rate of 10 mN / 30 seconds, the load of 10 mN is maintained for 60 seconds, and then the load is removed, and the strain 5 seconds after unloading is 1.00 μm or less.

2. The electrophotographic member according to claim 1, wherein the conductive filler is conductive carbon black.

3. When the longitudinal length of the elastic layer is L, and a total of three locations: the center of the elastic layer in the longitudinal direction and two locations L / 4 from both ends of the elastic layer toward the center, a total of three locations, in which the domain and the matrix are exposed in the thickness direction of the elastic layer, a square observation area with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm, each of the observation areas satisfies requirement (1) and requirement (2), as described in claim 1. Requirement (1): The total cross-sectional area of ​​the domains present within the observation area is 15 to 45% of the area of ​​the observation area. Requirement (2): The proportion of domains within the observation area that have a cross-sectional area of ​​0.1 to 13.0% of the area of ​​the observation area is 70% or more.

4. The electrophotographic member according to claim 3, wherein the proportion of domains having a circularity of 0.60 to 0.95 in the observation area is 70 percent or more.

5. The matrix includes a polycarbonate structure represented by formula (1), and The electrophotographic member according to claim 1, wherein the domain includes a polyether structure represented by formula (2). (In formula (1), R 1 (This indicates an alkylene group with 3 to 9 carbon atoms.) (In formula (2), R 2 (This indicates an alkylene group with 3 to 5 carbon atoms.)

6. The aforementioned R 1 The electrophotographic member according to claim 5, wherein the alkylene group has a branched structure with 3 to 9 carbon atoms.

7. The aforementioned R 2 The electrophotographic member according to claim 5, wherein the alkylene group has a branched structure with 3 to 5 carbon atoms.

8. When the longitudinal length of the elastic layer is L, and a total of three locations where the domain and matrix in the thickness direction of the elastic layer are exposed, such as the center of the elastic layer in the longitudinal direction and two locations L / 4 from both ends of the elastic layer toward the center, an observation area with sides of 50 μm is placed in the thickness region from the outer surface of the elastic layer to a depth of 100 μm, then each of the observation areas satisfies requirement (3), as described in claim 1. Requirement (3): The ratio of the area of ​​conductive filler contained in the matrix present in the observation region to the total area of ​​conductive filler present in the observation region is 95% or more.

9. The electrophotographic member according to claim 1, wherein the ratio of parameter A to parameter B (A / B) is 0.65 or less.

10. A process cartridge configured to be detachably attached to the main body of an electrophotographic image forming apparatus, comprising an electrophotographic member as described in any one of claims 1 to 9.

11. An electrophotographic image forming apparatus comprising an electrophotographic member according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Developing roller

    JP1998111599A

  • Developing roller, process cartridge and electrophotographic apparatus

    JP2005266500A

  • Elastic member for electrophotography, manufacturing method thereof, electrophotographic device, and process cartridge

    JP2006039031A

  • Conductive member for electrophotographic apparatus

    JP2017116685A

  • Process cartridge and image forming apparatus

    JP2021067740A