Connecting material, connecting structure, and method for manufacturing a connecting structure

A connecting material with an ionic polymerizable compound and caprolactone derivative balances high glass transition temperature for reliability with repairability by reducing crosslink density, addressing the challenge of removing cured materials from electronic components.

JP7955133B2Active Publication Date: 2026-11-24DEXERIALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022171252
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2026-11-24
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

Existing connection materials for connecting electronic components, such as LCD driver ICs to display panels, face challenges in achieving both high connection reliability and repairability due to the difficulty in removing cured materials with high elastic modulus and glass transition temperature, which compromises repairability when trying to maintain reliability.

Method used

A connecting material comprising an ionic polymerizable compound, an ionic polymerization initiator, and a caprolactone derivative, with specific ratios and properties, is used to create a connection structure that balances high glass transition temperature for reliability with repairability by incorporating caprolactone derivatives into the crosslink structure to reduce density and control Tg.

Benefits of technology

The solution achieves excellent connection reliability and repairability by controlling the glass transition temperature and crosslink density, allowing for easy removal of the connection material while maintaining strong bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955133000002
    Figure 0007955133000002
  • Figure 0007955133000003
    Figure 0007955133000003
  • Figure 0007955133000004
    Figure 0007955133000004
Patent Text Reader

Abstract

To provide a connection material with which it is possible to obtain excellent connection reliability and repairability, a connection structure, and a method for producing a connection structure.SOLUTION: A connection material contains an ionically polymerizable compound, an ionic polymerization initiator, and a caprolactone derivative. The content of the caprolactone derivative is 5-40 pts.mass relative to 100 pts.mass of the total mass of the ionically polymerizable compound and the caprolactone derivative. This enables adjustment in the glass transition temperature of the cured product, enabling excellent connection reliability and repairability.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This technology relates to a connecting material for applications such as COG (Chip On Glass), a connecting structure using the same, and a method for manufacturing the connecting structure. [Background technology]

[0002] Conventionally, in connection materials used to connect, for example, an LCD (Liquid Crystal Display) driver IC (Integrated Circuit) to a display panel, epoxy compounds and oxetane compounds have been used to achieve high elastic modulus and high glass transition temperature (Tg) in order to maintain high reliability. On the other hand, in order to reuse expensive display panels and driver ICs, repairability is also required, which allows for easy removal of the cured connection material (see, for example, Patent Documents 1-4).

[0003] However, epoxy resin cured by cationic polymerization, for example, is difficult to remove due to its high modulus of elasticity and high glass transition temperature (Tg). Generally, lowering the glass transition temperature of the cured material improves repairability, but this also raises concerns about a decrease in connection reliability, making it difficult to achieve both excellent connection reliability and repairability simultaneously. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2016-079313 [Patent Document 2] Japanese Patent Publication No. 2010-102859 [Patent Document 3] Japanese Patent Application Publication No. 10-204153 [Patent Document 4] Japanese Patent Publication No. 2001-093939 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] This technology solves the aforementioned problems and provides a connection material, a connection structure, and a method for manufacturing the connection structure that can achieve excellent connection reliability and repairability. [Means for solving the problem]

[0006] As a result of diligent research, the inventors have discovered that the following connecting material, connecting structure, and method for manufacturing the connecting structure can achieve the above objective, and have completed this technology.

[0007] [1] It contains an ionic polymerizable compound, an ionic polymerization initiator, and a caprolactone derivative. A connecting material wherein the content of the caprolactone derivative is 5 to 40 parts by mass per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative. [2] The connecting material according to [1], wherein the content of the caprolactone derivative is 5 to 25 parts by mass per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative. [3] The connecting material according to [1], wherein the glass transition temperature of the connecting material after curing is 170 to 195°C. [4] It further contains a thermoplastic resin and an insulating filler, The connecting material according to [1], wherein the total content of the ionic polymerizable compound and the caprolactone derivative is 10 to 50 wt%. [5] The ionic polymerizable compound includes an epoxy compound or an oxetane compound. The connecting material according to [1], wherein the ionic polymerization initiator is a cationic polymerization initiator. [6] The connecting material according to [1], wherein the molecular weight per functional group of the caprolactone derivative is 100 to 3000. [7] The connecting material according to [1], wherein the molecular weight per functional group of the caprolactone derivative is 100 to 1000. [8] The connection material according to [1], wherein the caprolactone derivative is one or more selected from the group consisting of polycaprolactone diol, polycaprolactone triol, and polycaprolactone tetraol. [9] The connection material according to [1], further containing conductive particles.

[10] A first electronic component, a second electronic component, and an adhesive cured film in which the first electronic component and the second electronic component are bonded to each other, The adhesive cured film contains an ion polymerizable compound, an ion polymerization initiator, and a caprolactone derivative, and the content of the caprolactone derivative is 5 to 40 parts by mass with respect to 100 parts by mass in total of the ion polymerizable compound and the caprolactone derivative. A connected structure formed by curing a connecting material.

[11] The connected structure according to

[10] , wherein the connection material further contains conductive particles.

[12] It contains an ion polymerizable compound, an ion polymerization initiator, and a caprolactone derivative, and the content of the caprolactone derivative is 5 to 40 parts by mass with respect to 100 parts by mass in total of the ion polymerizable compound and the caprolactone derivative. An arrangement step of arranging the first electronic component and the second electronic component via a certain connection material, A curing step of crimping the second electronic component to the first electronic component with a crimping tool and curing the connection material A method for manufacturing a connected structure having

[13] The method for manufacturing a connected structure according to

[12] , wherein the connection material further contains conductive particles.

Effect of the invention

[0008] According to this technique, excellent connection reliability and repairability can be obtained. [[Brief description of drawings]]

[0009] [Figure 1]FIG. 1(A) is a diagram for explaining a crosslinked structure after cationic polymerization of an ion-polymerizable compound, and FIG. 1(B) is a diagram for explaining a crosslinked structure after ionic polymerization of an ion-polymerizable compound and a caprolactone derivative. [Figure 2] FIG. 2 is a diagram for explaining a method for manufacturing a connection structure according to the present embodiment, FIG. 2(A) shows an arrangement step (S1), and FIG. 2(B) shows a curing step (S2). [Figure 3] FIG. 3 is a graph showing a glass transition temperature (Tg) with respect to a content of a caprolactone derivative. [Mode for Carrying Out the Invention]

[0010] Hereinafter, an embodiment of the present technology will be described in detail in the following order with reference to the drawings. 1. Connection material 2. Connection structure and method for manufacturing connection structure 3. Examples

[0011] <1. Connection material> A connection material according to the present embodiment contains an ion-polymerizable compound, an ion polymerization initiator, and a caprolactone derivative. The connection material may be either in a film form or a paste form. The film form is preferable from the viewpoint of easy handling, and the paste form is preferable from the viewpoint of cost. Examples of a curing type of the connection material include a thermal curing type, a photocuring type, and a photothermal combined curing type, and these can be appropriately selected according to applications. In addition, as an ionic polymerization type of the connection material, cationic polymerization or anionic polymerization can be appropriately selected according to applications.

[0012] (Ion-polymerizable compound) Examples of the ion-polymerizable compound include an epoxy compound and an oxetane compound. The ion-polymerizable compound preferably has 2 or more and 5 or less epoxy groups at a terminal in order to obtain a crosslinked structure by a curing reaction.

[0013] Epoxy compounds preferably have two to five epoxy groups at their terminal ends. For example, one or more of the following can be used individually or in combination: alicyclic epoxy compounds, glycidyl ether type epoxy compounds, glycidyl ester type epoxy compounds, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, dicyclopentadiene type epoxy compounds, novolacphenol type epoxy compounds, biphenyl type epoxy compounds, naphthalene type epoxy compounds, etc. Specific examples of alicyclic epoxy compounds having a cycloalkene oxide structure include, for example, Daicel Corporation's product names "Celoxide 8010 ((3,3',4,4'-diepoxy)bicyclohexyl)" and "Celoxide 2021P (3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate)".

[0014] The oxetane compound preferably has two to five oxetane groups at its terminal end. For example, one or more of the following can be used individually or in combination: biphenyl-type oxetane compounds, xylylene-type oxetane compounds, silsesquioxane-type oxetane compounds, ether-type oxetane compounds, phenol novolac-type oxetane compounds, silicate-type oxetane compounds, etc. A specific example of a biphenyl-type oxetane compound is the product name "OXBP (4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl)" from Ube Industries, Ltd.

[0015] The content of the ionic polymerizable compound is preferably 11 to 48 wt%, more preferably 15 to 43 wt%, and even more preferably 19 to 38 wt%, of the binder, which is a resin component. If the content of the cationic polymerizable compound is too high, curing shrinkage tends to increase.

[0016] Depending on the type of ionic polymerization, cationic polymerization initiators or anionic polymerization initiators are used as ionic polymerization initiators.

[0017] (Cationic polymerization initiator) Cationic polymerization initiators can be used individually or in combination of two or more, from among onium salt-type acid generators such as sulfonium salts, ammonium salts, and phosphonium salts. Among these, it is preferable to use a quaternary ammonium salt-based thermal acid generator to improve storage life. Examples of quaternary ammonium salt-based thermal acid generators include salts of a quaternary ammonium cation with an antimony hexafluoride anion, hexafluoride phosphate anion, trifluoromethanesulfonic acid anion, perfluorobutanesulfonic acid anion, dinonylnaphthalenesulfonic acid anion, dinonylnaphthalenesulfonic acid anion, p-toluenesulfonic acid anion, dodecylbenzenesulfonic acid anion, or tetrakis(pentafluorophenyl)borate anion. Examples of quaternary ammonium cations include NR1R2R3R4 + Examples of cations represented by the formula are shown. Here, R1, R2, R3, and R4 are linear, branched, or cyclic alkyl or aryl groups having 1 to 12 carbon atoms, and may each have a hydroxyl group, halogen, alkoxyl group, amino group, ester group, etc. An example of a quaternary ammonium salt-based thermal acid generator is King Industries' product "K-PURE CXC-1821".

[0018] (Anionic polymerization initiator) Anionic polymerization initiators can be selected individually or in combination of two or more from among, for example, organic acid dihydrazides, dicyandiamides, amine compounds, polyamidoamine compounds, cyanate ester compounds, phenolic resins, acid anhydrides, carboxylic acids, tertiary amine compounds, imidazoles, Lewis acids, Brønsted salts, polymer captan curing agents, urea resins, melamine resins, isocyanate compounds, and blocked isocyanate compounds. Among these, it is preferable to use a microencapsulated latent curing agent that has an imidazole modified material as a core and its surface coated with polyurethane. A specific example available on the market is Asahi Kasei E-Materials Corporation's product name "NovaCure 3941HP".

[0019] The content of the ionic polymerization initiator is preferably 1 to 20 wt%, more preferably 3 to 15 wt%, and even more preferably 5 to 10 wt%, of the binder, which is a resin component.

[0020] (Caprolactone derivative) Caprolactone derivatives are, for example, polycaprolactone polyols obtained by ring-opening polymerization of ε-caprolactone with an alcohol compound, and it is preferable that they have two or more hydroxyl groups at the terminal end. Examples of polycaprolactone polyols include polycaprolactone diols having two hydroxyl groups at the terminal end, polycaprolactone triols having three hydroxyl groups at the terminal end, and polycaprolactone tetraols having four hydroxyl groups at the terminal end. One of these can be used alone, or two or more can be used in combination. Specific examples of polycaprolactone polyols include, for example, the "Praxel" series of products from Daicel Corporation.

[0021] The molecular weight per functional group of the caprolactone derivative is preferably 100 to 3000, more preferably 100 to 2000, and even more preferably 100 to 1000. As the molecular weight per functional group of the caprolactone derivative decreases, the change in glass transition temperature (Tg) with respect to the caprolactone derivative content tends to increase.

[0022] The total content of the ionic polymerizable compound and the caprolactone derivative is preferably 15 to 50 wt%, more preferably 20 to 45 wt%, and even more preferably 25 to 40 wt%, of the binder, which is a resin component. The content of the caprolactone derivative is preferably 5 to 40 parts by mass, more preferably 5 to 30 parts by mass, and even more preferably 5 to 25 parts by mass, per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative. Increasing the content of the caprolactone derivative per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative tends to lower the glass transition temperature (Tg) and improve repairability.

[0023] Furthermore, the content of the caprolactone derivative is preferably 1 to 10 wt%, more preferably 1 to 8 wt%, and even more preferably 2 to 6 wt%, of the binder, which is a resin component. Adding a small amount of the caprolactone derivative allows for precise control of the glass transition temperature (Tg).

[0024] The glass transition temperature (Tg) of the connecting material after curing is preferably 150-195°C, more preferably 155-195°C, and even more preferably 160-195°C. A higher glass transition temperature (Tg) tends to result in better connection reliability.

[0025] Figure 1(A) is a diagram illustrating the crosslinking structure of an ionic polymerizable compound after cationic polymerization, and Figure 1(B) is a diagram illustrating the crosslinking structure of an ionic polymerizable compound and a caprolactone derivative after ionic polymerization. As shown in Figure 1(A), the crosslinking structure of an ionic polymerizable compound after cationic polymerization consists of (a) a network derived from epoxy compounds or oxetane compounds. On the other hand, as shown in Figure 1(A), the crosslinking structure of an ionic polymerizable compound and a caprolactone derivative after ionic polymerization consists of (a) a network derived from epoxy compounds or oxetane compounds into which (b) a polycaprolactone polyol is incorporated.

[0026] Generally, the denser the crosslink structure, the higher the Tg and elastic modulus of the cured product. However, caprolactone derivatives have hydroxyl groups at their ends, so they react as monomers during ionic polymerization and are incorporated into the crosslink structure. Caprolactone derivatives have the effect of reducing the crosslink density of flexible long-chain alkyl structures, so the Tg can be lowered with the addition of a small amount, enabling precise Tg control and achieving both excellent connection reliability and repairability.

[0027] (polymer) The connecting material may further contain a polymer as a binder to improve film-forming properties, connection reliability, etc. Examples of polymers include bisphenol A type phenoxy resin, phenoxy resin having a fluorene skeleton, polystyrene, polyacrylonitrile, polyphenylene sulfide, polytetrafluoroethylene, and polycarbonate, which can be used individually or in combination of two or more. Among these, it is preferable to use a thermoplastic resin such as phenoxy resin from the viewpoint of film-forming properties and connection reliability. Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin. Specific examples of phenoxy resins include Nippon Steel & Sumitomo Metal Chemical Co., Ltd.'s product names "FX293," "YP50," and "YP70." While using a polymer with a flexible skeleton can be considered as a way to lower Tg, polymers affect various physical properties such as film-forming properties and connection reliability, making it difficult to precisely control Tg by selecting a polymer while considering these properties.

[0028] The polymer content is preferably 10 to 50 wt%, more preferably 15 to 45 wt%, and even more preferably 20 to 30 wt%, of the binder, which is a resin component.

[0029] (Insulating filler) The connecting material may further contain insulating fillers as a binder to adjust the minimum melt viscosity. Examples of insulating fillers include inorganic fillers such as silica, alumina, calcium carbonate, and titanium oxide, and organic fillers such as acrylic rubber and silicone, which can be used individually or in combination of two or more. Among these, silica is preferred. Specific examples of silica include "AEROSIL R202" from Nippon Aerosil Co., Ltd. and "Admanano" from Admatex Co., Ltd.

[0030] The content of the insulating filler is preferably 5 to 60 wt%, more preferably 10 to 55 wt%, and even more preferably 20 to 50 wt%, of the binder, which is a resin component. A higher filler content tends to result in a higher minimum melt viscosity, while a lower filler content tends to result in a lower minimum melt viscosity. The average particle size of the filler is preferably 1 to 500 nm, more preferably 10 to 300 nm, and even more preferably 20 to 100 nm.

[0031] (Silane coupling agent) The connecting material may further contain a silane coupling agent as a binder to improve adhesion at the interface with the inorganic material. Examples of silane coupling agents include epoxy, methacryloxy, amino, vinyl, mercapto-sulfide, and ureid types, which may be used individually or in combination of two or more types. Specific examples of epoxy silane coupling agents include product name "A-187" from Momentive Performance Materials Japan LLC and product name "KBM-4803" from Shin-Etsu Chemical Co., Ltd.

[0032] The content of the silane coupling agent is preferably 0.1 to 10 wt%, more preferably 0.1 to 5 wt%, and even more preferably 0.5 to 3 wt%, of the binder, which is a resin component.

[0033] (Conductive adhesive) The connecting material may be a conductive adhesive containing conductive particles in a binder. The conductive adhesive may be either a film-like conductive film or a paste-like conductive paste. The conductive adhesive may also be used as an anisotropic conductive adhesive. The anisotropic conductive adhesive may be either a film-like anisotropic conductive film (ACF) or a paste-like anisotropic conductive paste (ACP). A film-like form is preferred for ease of handling, while a paste-like form is preferred from a cost perspective.

[0034] As conductive particles, those used in known anisotropic conductive films can be appropriately selected and used. Examples include metal particles such as nickel (melting point 1455°C), copper (melting point 1085°C), silver (melting point 961.8°C), gold (melting point 1064°C), palladium (melting point 1555°C), tin (melting point 231.9°C), nickel boride (melting point 1230°C), ruthenium (melting point 2334°C), and tin alloys such as solder. Also, for example, metal-coated metal particles are obtained in which the surface of metal particles is coated with a metal such as nickel, copper, silver, gold, palladium, tin, nickel boride, or ruthenium. Furthermore, for example, metal-coated resin particles are obtained in which the surface of resin particles, such as polymers containing at least one monomer selected from polyamide, polybenzoguanamine, styrene, and divinylbenzene as monomer units, is coated with a metal such as nickel, copper, silver, gold, palladium, tin, nickel boride, or ruthenium. Furthermore, examples include metal-coated inorganic particles in which the surface of inorganic particles such as silica, alumina, barium titanate, zirconia, carbon black, silicate glass, borosilicate glass, lead glass, soda-lime glass, and alumina silicate glass is coated with a metal such as nickel, copper, silver, gold, palladium, tin, nickel boride, or ruthenium. The metal coating layer of the metal-coated resin particles and metal-coated inorganic particles may be a single layer or a multi-layer of dissimilar metals. In addition, these conductive particles may be subjected to an insulating coating treatment by coating them with, for example, a resin layer or insulating particles such as resin particles or inorganic particles. In this case, the particle size of the conductive particles does not include the portion that has been treated with the insulating coating.

[0035] The particle size of the conductive particles is appropriately changed depending on the optical elements to be mounted, the electrodes of the wiring board, the area of ​​the bumps, etc., but is preferably 1 to 30 μm, more preferably 1 to 10 μm, and particularly preferably 1 to 5 μm. The particle size can be determined by measuring 200 or more particles using a microscope (optical microscope, metallurgical microscope, electron microscope, etc.) and taking the average value.

[0036] The conductive particles may have any shape, such as spherical, ellipsoidal, spiky, or irregular. Among these, spherical conductive particles are preferred because they facilitate easy control of particle size and particle size distribution. The conductive particles may also have protrusions on their surface to improve connectivity.

[0037] The anisotropic conductive film is preferably configured with conductive particles aligned in the plane direction. By configuring the conductive particles to be aligned in the plane direction, the particle surface density becomes uniform, and conductivity and insulation can be improved. The state in which the conductive particles are aligned in the plane direction includes, for example, a planar lattice pattern having at least one array axis in which the conductive particles are arranged in a predetermined direction at a predetermined pitch, such as an orthorhombic lattice, a hexagonal lattice, a square lattice, a rectangular lattice, or a parallelepiped lattice. The arrangement of the conductive particles in the plane direction may be random, or may have a plurality of regions with different planar lattice patterns.

[0038] The particle surface density of the anisotropic conductive film can be appropriately designed according to the size of the electrodes to be connected, and the lower limit of the particle surface density is 500 particles / mm 2 or more, 20,000 particles / mm 2 or more, 40,000 particles / mm 2 or more, 50,000 particles / mm 2 or more, and the upper limit of the particle surface density is 1,500,000 particles / mm 2 or less, 1,000,000 particles / mm 2 or less, 500,000 particles / mm 2 or less, 100,000 particles / mm 2 or less. This makes it possible to obtain excellent conductivity and insulation even when the size of the electrodes to be connected is small. The particle surface density of the anisotropic conductive film refers to the density in the aligned portion of the conductive particles when the film is formed during manufacturing. When determining the particle number density from a plurality of individual pieces, the particle surface density can be determined from the area obtained by subtracting the space between the individual pieces from the area including the individual pieces and the space, and the number of particles.

[0039] By forming the anisotropic conductive film into a film, it becomes easier to apply the anisotropic conductive film to the substrate. From the viewpoint of ease of handling, the anisotropic conductive film may have a release film such as polyethylene terephthalate film on one or both sides. Furthermore, the anisotropic conductive film may have an adhesive layer or tack layer that does not contain conductive particles laminated over it, and the number of layers and the lamination surface can be appropriately selected according to the target and purpose.

[0040] The thickness of the anisotropic conductive film can be appropriately changed depending on the height of the electrodes and bumps of the mounted optical element or wiring substrate, and should be within 1 to 10 times the particle diameter, preferably 1 μm to 10 μm, more preferably 1 μm to 6 μm, and even more preferably 2 μm to 4 μm. The film thickness can be measured using a known micrometer or digital thickness gauge. The film thickness can be determined by measuring at, for example, 10 or more locations and averaging the results.

[0041] Methods for manufacturing anisotropic conductive films include, for example, applying a solution of anisotropic conductive adhesive onto a substrate and drying it, or forming an adhesive layer without conductive particles on a substrate and then fixing conductive particles to the resulting adhesive layer.

[0042] <2. Connecting structure and method for manufacturing the connecting structure> The connecting structure according to this embodiment comprises a first electronic component, a second electronic component, and an adhesive curing film on which the first electronic component and the second electronic component are bonded.

[0043] Furthermore, the manufacturing method of the connecting structure according to this embodiment includes an arrangement step of arranging a first electronic component and a second electronic component via a connecting material, and a curing step of pressing the second electronic component to the first electronic component with a crimping tool and curing the connecting material.

[0044] The connection structure and method for manufacturing the connection structure according to this embodiment use a connection material containing an ionic polymerizable compound, an ionic polymerization initiator, and a caprolactone derivative, thereby providing excellent connection reliability and repairability.

[0045] The following describes a method for manufacturing a connecting structure using a thermosetting anisotropic conductive film as the connecting material. Note that the anisotropic conductive film is the same as described above, so its explanation will be omitted here.

[0046] Figure 2 is a diagram illustrating the manufacturing method of the connecting structure according to this embodiment, where Figure 2(A) shows the arrangement step (S1) and Figure 2(B) shows the curing step (S2).

[0047] [Placement process (S1)] As shown in Figure 1(A), in the placement step (S1), the second electronic component 20 is placed on the first electronic component 10 via an anisotropic conductive film 30 containing an ionic polymerizable compound, an ionic polymerization initiator, and a caprolactone derivative.

[0048] The first electronic component 10 comprises a first terminal row 11, and the second electronic component 20 comprises a second terminal row 21 facing the first terminal row 11. The first electronic component 10 and the second electronic component 20 are not particularly limited and can be appropriately selected according to the purpose. Examples of the first electronic component 10 include LCD (Liquid Crystal Display) panels, flat panel display (FPD) applications such as organic EL (OLED), and touch panel applications, as well as printed circuit boards (PWB). The material of the printed circuit board is not particularly limited and may be glass epoxy such as FR-4 substrate, or plastics such as thermoplastic resins, ceramics, etc. Examples of the wiring board include glass substrates and plastic substrates. Examples of the second electronic component 20 include ICs (Integrated Circuits), flexible printed circuits (FPCs), tape carrier package (TCP) substrates, and COFs (Chip On Film) with ICs mounted on FPCs.

[0049] [Curing process (S2)] In the curing step (S2), the second electronic component 20 is pressed against the first electronic component 10 using the crimping tool 40, and heat is applied while pressing. In the curing step (S2), the crimping tool 40 is used to press at a temperature preferably of 200°C or lower, more preferably of 180°C or lower, and even more preferably of 150°C or lower. As a result, the binder of the anisotropic conductive film melts due to the heat from the crimping tool, the second electronic component is sufficiently pressed in by the crimping tool 40, and conductive particles 31 are sandwiched between the first terminal row 11 and the second terminal row 21. Furthermore, the binder hardens due to heat curing, bonding the first electronic component 10 and the second electronic component 20 together.

[0050] Furthermore, in the curing process (S2), a cushioning material may be used between the crimping tool 40 and the second electronic component 20. Examples of cushioning materials include polytetrafluoroethylene (PTFE), polyimide, glass cloth, and silicone rubber. [Examples]

[0051] <3. Examples> In this example, a cationic polymerized anisotropic conductive film was fabricated as one form of the connecting material. An IC chip was then thermocompressed onto a glass substrate using the anisotropic conductive film to create a connecting structure. The conductivity resistance of the connecting structure was measured initially and after a High Accelerated Stress Test (HAST) to evaluate the connection reliability. Furthermore, the die shear strength of the IC chip was measured to evaluate the repairability of the anisotropic conductive film after the IC chip was removed.

[0052] [Fabrication of a two-layer anisotropic conductive film] As shown in Table 1, a thermoplastic resin, filler, ionic polymerizable compound, caprolactone derivative, silane coupling agent, and cationic polymerization initiator were blended in predetermined parts by mass to prepare a first adhesive layer with a thickness of 10 μm. Furthermore, as shown in Table 1, a second adhesive layer with a thickness of 5 μm was prepared by blending a thermoplastic resin, filler, ionic polymerizable compound, caprolactone derivative, silane coupling agent, and cationic polymerization initiator in predetermined parts by mass. Conductive particles with an average particle size of 3.2 μm were then added to the second adhesive layer at a surface density of 28,000 particles / mm². 2 The materials were aligned to create an anisotropic conductive layer. Then, the first adhesive layer and the anisotropic conductive layer were bonded together to create a two-layer anisotropic conductive film.

[0053] [Fabrication of single-layer anisotropic conductive films] As shown in Table 1, a resin composition was prepared by blending a thermoplastic resin, filler, ionic polymerizable compound, caprolactone derivative, silane coupling agent, and cationic polymerization initiator in predetermined parts by mass. Conductive particles (average particle size 3.2 μm) were added to the resin composition to a concentration of 15 wt% relative to the total of the resin mixture and conductive particles, and an anisotropic conductive film with a thickness of 7 μm was prepared.

[0054] Thermoplastic: Phenoxy resin FX293 (Nippon Steel Chemical & Material Co., Ltd.) Filler: Fumed Silica AEROSIL R202 (Nippon Aerosil Co., Ltd.) Ionic polymerizable compound: Alicyclic epoxy compound Celoxide 8010 (Daicel Corporation, bifunctional) Caprolactone derivatives: Polycaprolactone diol L205AL (Daicel Corporation, bifunctional, molecular weight 500), polycaprolactone diol L220AL (Daicel Corporation, bifunctional, molecular weight 2000), polycaprolactone triol PCL305 (Daicel Corporation, trifunctional, molecular weight 550), polycaprolactone triol PCL312 (Daicel Corporation, trifunctional, molecular weight 1250), polycaprolactone triol PCL320 (Daicel Corporation, trifunctional, molecular weight 2000) Silane coupling agents: A-187 (Momentive Performance Materials Japan LLC) Cationic polymerization initiator: Onium salt type thermal acid generator using quaternary ammonium salts: K-PURE CXC-1821 (King Industries Co.)

[0055] [Measurement of glass transition temperature (Tg)] A sample of a two-layer anisotropic conductive film (size: 2.0 mm x 20 mm) was cured at a temperature of 200°C for 10 minutes, and the glass transition temperature (°C) was measured by dynamic mechanical analysis (DMA) at a heating rate of 10°C / min.

[0056] [Creating connection structures] The IC chip had an outer dimension (X) of 29.8 mm, an outer dimension (Y) of 0.84 mm, and a thickness of 0.15 mm. The output side bumps had a width of 18 μm, a length of 100 μm, a spacing of 18 μm, and 1424 bumps. The input side bumps had a width of 34 / 24 μm, a length of 100 μm, a spacing of 10 / 8 μm, and 823 bumps, with a bump height of 9 μm.

[0057] The glass substrate had an outer dimension of 60 mm (X) and 80 mm (Y), with a thickness of 0.3 mm. The electrode film composition was a-ITO / Mo / Al, and a measuring TEG was used with 30 channels for continuity measurement on the output side and 11 channels on the input side.

[0058] A first connection structure was fabricated by thermocompressing an IC chip onto a glass substrate using a two-layer anisotropic conductive film. A second connection structure was then fabricated by thermocompressing an IC chip onto a glass substrate using a single-layer anisotropic conductive film. The thermocompression conditions were 145°C, 60 MPa pressure, and 5 seconds.

[0059] [Evaluation of connection reliability] (Measurement of conductivity resistance) The conductivity resistance values ​​of the first and second connection structure samples, both initially and after the High Accelerated Stress Test (HAST), were measured using a digital multimeter with a 1mA current applied via the 4-terminal method. The HAST test was conducted under conditions of 110°C, 85% humidity, and 12 hours.

[0060] (Evaluation metrics) Based on whether or not non-conductive channels occurred from the initial stage to after HAST, and whether or not component delamination occurred, the following indicators were used for evaluation. A: No non-conductive channels or material delamination occurred. B: Either a non-conductive channel or delamination of the material occurs. C: Both non-conductive channels and material delamination occur.

[0061] [Measurement of die shear strength] The first connection structure sample was heated on a stage at 250°C for 20 seconds, after which the IC chip was peeled off using a die shear tester, and the die shear strength (kgf) was measured.

[0062] [Evaluation of repairability] The glass substrates of the first and second connection structure samples, after the IC chips were removed, were heated on a hot plate at 85°C while methyl ethyl ketone (MEK) was continuously dripped onto the remaining anisotropic conductive film for 1 minute, ensuring it did not dry out. The remaining anisotropic conductive film after immersion in MEK was scraped off with a wooden bar, and the time it took for it to disappear was measured.

[0063] (Evaluation metrics) The following indicators were used to evaluate the process based on the time it took from the start of scraping with the wood bar until the remaining portion of the anisotropic conductive film was completely removed. A: Less than 20 seconds B: 20 ​​seconds or more, less than 60 seconds C: 60 seconds or more

[0064] Table 1 shows the glass transition temperature, connection reliability evaluation results, die shear strength, and repairability evaluation results for the examples and comparative examples.

[0065] [Table 1]

[0066] As shown in Table 1, the evaluation of connection reliability and repairability of the first connection structure using a two-layer anisotropic conductive film and the second connection structure using a single-layer anisotropic conductive film yielded similar results.

[0067] Comparative Example 1 did not contain a caprolactone derivative, and therefore did not provide good repairability. Examples 1 to 13 contained 5 to 40 parts by mass of caprolactone derivative per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative, and thus achieved excellent connection reliability and repairability. In particular, Examples 1, 2, 4, 5, 7, 8, 10, 11, and 12 contained 5 to 25 parts by mass of caprolactone derivative per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative, which allowed for improved repairability while maintaining a high glass transition temperature.

[0068] Figure 3 is a graph showing the glass transition temperature (Tg) as a function of caprolactone derivative content. The graph in Figure 3 shows the glass transition temperatures as a function of the added amounts of polycaprolactone diol with a molecular weight of 500, polycaprolactone diol with a molecular weight of 2000, polycaprolactone triol with a molecular weight of 500, and polycaprolactone triol with a molecular weight of 2000. From the graph in Figure 3, it was found that the change in glass transition temperature as a function of caprolactone derivative content was greater for bifunctional polycaprolactone than for trifunctional polycaprolactone. It was also found that the change in glass transition temperature as a function of caprolactone derivative content was greater for low molecular weight polycaprolactone than for high molecular weight polycaprolactone. It is thought that incorporating a large amount of low molecular weight caprolactone derivative into the crosslinking structure is more effective in lowering the glass transition temperature than reducing the crosslinking density with long molecular chains. [Explanation of Symbols]

[0069] 10 First electronic component, 11 First terminal row, 20 Second electronic component, 21 Second terminal row, 30 Anisotropic conductive adhesive, 31 Conductive particles, 40 Crimping tool

Claims

1. A thermoplastic resin, an ionic polymerizable compound, an ionic polymerization initiator, a caprolactone derivative, and conductive particles, The content of the caprolactone derivative is 5 to 25 parts by mass per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative. The total content of the ionic polymerizable compound and the caprolactone derivative is 10 to 50 wt%, The glass transition temperature of the connecting material after curing is 170 to 195°C. A connecting material that is in the form of a film.

2. The connecting material according to claim 1, further containing an insulating filler.

3. The ionic polymerizable compound includes an epoxy compound or an oxetane compound. The connecting material according to claim 1, wherein the ionic polymerization initiator is a cationic polymerization initiator.

4. The connecting material according to claim 1, wherein the molecular weight per functional group of the caprolactone derivative is 100 to 3000.

5. The connecting material according to claim 1, wherein the molecular weight per functional group of the caprolactone derivative is 100 to 1000.

6. The connecting material according to claim 1, wherein the caprolactone derivative is one or more selected from the group consisting of polycaprolactone diol, polycaprolactone triol, and polycaprolactone tetraol.

7. The device comprises a first electronic component, a second electronic component, and an adhesive curing film on which the first electronic component and the second electronic component are bonded together. The adhesive cured film contains a thermoplastic resin, an ionic polymerizable compound, an ionic polymerization initiator, a caprolactone derivative, and conductive particles, wherein the content of the caprolactone derivative is 5 to 25 parts by mass per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative, the total content of the ionic polymerizable compound and the caprolactone derivative is 10 to 50 wt%, the glass transition temperature after curing of the connecting material is 170 to 195°C, and the connecting structure is formed by curing a film-like connecting material.

8. A connecting material comprising a thermoplastic resin, an ionic polymerizable compound, an ionic polymerization initiator, a caprolactone derivative, and conductive particles, wherein the content of the caprolactone derivative is 5 to 25 parts by mass per 100 parts by mass of the total of the ionic polymerizable compound and the caprolactone derivative, the total content of the ionic polymerizable compound and the caprolactone derivative is 10 to 50 wt%, the glass transition temperature after curing of the connecting material is 170 to 195°C, and the arrangement step of arranging a first electronic component and a second electronic component via a connecting material which is in the form of a film, The second electronic component is pressed against the first electronic component using a crimping tool, and the connecting material is cured in a curing step. A method for manufacturing a connecting structure having the following characteristics.

Citation Information

Patent Citations

  • Adhesive

    JP1998204153A

  • Adhesive composition, adherend, adhering method, and production of optical disk

    JP1999061078A

  • Connection method

    JP2001093939A

  • Curable resin composition and method for producing the same

    JP2007169337A

  • Heat or active energy ray-curable adhesive

    JP2008214449A