Rubber composition for tire treads and tires

A rubber composition with modified butadiene rubber, silica, and terpene resin achieves both low-temperature and wet grip performance by promoting phase separation and improving compatibility, addressing the dual performance challenge in tire treads.

JP7955146B2Active Publication Date: 2026-11-24TOYO TIRE CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022192173
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2026-11-24
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

Existing rubber compositions for tire treads struggle to simultaneously achieve both low-temperature performance and wet grip performance, as adding butadiene rubber for low-temperature performance worsens wet grip, and adding resin for wet grip worsens low-temperature performance.

Method used

A rubber composition comprising 100 parts by mass of a diene rubber component with 40 parts by mass or more of modified butadiene rubber, 60 to 200 parts by mass of silica, and 20 to 60 parts by mass of a terpene resin with a β-pinene unit content of 40% by mass or more, which promotes phase separation and improves compatibility, thereby enhancing both low-temperature and wet grip performance.

Benefits of technology

The composition achieves improved low-temperature performance and wet grip performance while maintaining processability by using modified butadiene rubber and terpene resin, with silica dispersion enhancing compatibility and reducing tackiness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955146000001
    Figure 0007955146000001
  • Figure 0007955146000002
    Figure 0007955146000002
  • Figure 0007955146000003
    Figure 0007955146000003
Patent Text Reader

Abstract

To achieve both low-temperature performance and wet grip performance.SOLUTION: A rubber composition for a tire tread according to an embodiment contains: 100 pts.mass of a diene rubber component containing 40 pts.mass or more of a modified butadiene rubber; 60-200 pts.mass of silica; and 20-60 pts.mass of a terpene-based resin having a β-pinene unit content of 40 mass% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber composition for a tire tread, and a tire using the same.

Background Art

[0002] One performance required for tires is grip performance on wet road surfaces (i.e., wet grip performance). In order to improve wet grip performance, it is known to incorporate silica as a filler and also incorporate a resin.

[0003] For example, Patent Document 1 discloses a tire tread containing 100 parts by mass of a diene rubber component including a modified diene rubber having a silanol functional group (specifically, modified SBR), 120 to 140 parts by mass of silica, and 5 to 60 parts by mass of a hydrocarbon resin. According to Patent Document 1, this improves wet grip performance, grip performance on dry road surfaces, and rolling resistance.

[0004] Patent Document 2 discloses a rubber composition for a tread in which a specific butadiene rubber and a terpene-based resin are blended, and silica is further blended. According to Patent Document 2, this improves fuel efficiency, wear resistance, and wet grip performance.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Summary of Invention

Problem to be Solved by the Invention

[0006] For example, all-season tires, which can be driven not only on wet roads but also on snowy winter roads, require both wet grip performance and low-temperature performance. Low-temperature performance refers to the ability to maintain softness in low-temperature environments below 0°C, enabling driving on snowy roads. If butadiene rubber, which has a low glass transition temperature, is added to impart low-temperature performance, the glass transition temperature of the entire rubber composition tends to decrease, worsening wet grip performance. On the other hand, if resin is added to a rubber composition containing butadiene rubber to improve wet grip performance, the glass transition temperature tends to increase, worsening low-temperature performance. Thus, low-temperature performance and wet grip performance are mutually exclusive, and it is difficult to achieve both simultaneously.

[0007] Patent documents 1 and 2 describe combining butadiene rubber with terpene resins, but they do not describe combining a rubber component containing 40% or more by mass of modified butadiene rubber with β-pinene resin, nor do they describe how this can achieve both low-temperature performance and wet grip performance.

[0008] The embodiments of the present invention aim to provide a rubber composition for tire treads that can achieve both low-temperature performance and wet grip performance, and a tire using the same. [Means for solving the problem]

[0009] The present invention includes embodiments shown below. [1] A rubber composition for tire treads comprising 100 parts by mass of a diene rubber component containing 40 parts by mass or more of modified butadiene rubber, 60 to 200 parts by mass of silica, and 20 to 60 parts by mass of a terpene resin having a β-pinene unit content of 40% by mass or more. [2] The rubber composition for tire treads according to [1], wherein the total content of the terpene resin and oil is less than 60 parts by mass per 100 parts by mass of the diene rubber component. [3] The tire tread rubber composition according to [1] or [2], wherein 100 parts by mass of the diene rubber component comprises 60 parts by mass or more of the modified butadiene rubber. [4] A tire having a tread made using a rubber composition for tire treads described in any one of the items [1] to [3]. [Effects of the Invention]

[0010] According to embodiments of the present invention, it is possible to achieve both low-temperature performance and wet grip performance, and processability can be improved by using modified butadiene rubber. [Modes for carrying out the invention]

[0011] The rubber composition for tire treads according to the embodiment (hereinafter also referred to as the rubber composition) comprises: (A) 100 parts by mass of a diene-based rubber component containing 40 parts by mass or more of modified butadiene rubber; (B) 60 to 200 parts by mass of silica; and (C) 20 to 60 parts by mass of a terpene-based resin having a β-pinene unit content of 40% by mass or more.

[0012] Butadiene rubber generally has a low glass transition temperature. By increasing the proportion of butadiene rubber with such a low glass transition temperature, low-temperature performance can be improved. On the other hand, terpene resins with a β-pinene unit content of 40% by mass or more have low compatibility with butadiene rubber. Therefore, by adding such terpene resins to a diene rubber component with a higher proportion of butadiene rubber, the diene rubber component and the terpene resin enter a phase-separated state. This allows for the improvement of wet grip performance by the terpene resin while maintaining the good low-temperature performance provided by butadiene rubber, thus achieving both low-temperature and wet grip performance.

[0013] However, as described above, it was found that when a considerable amount of silica and terpene resin is added, the tackiness of the unvulcanized rubber composition increases, and the processability deteriorates. This is thought to be because, when butadiene rubber is unmodified, it has poor compatibility with silica, causing the silica to aggregate and become unevenly distributed. According to this embodiment, by using modified butadiene rubber, the dispersibility of silica can be improved. By uniformly dispersing silica, the inherent tackiness of butadiene rubber is suppressed, and the processability can be improved. Therefore, it is possible to improve processability while achieving both low-temperature performance and wet grip performance.

[0014] [(A) Diene-based rubber component] In this embodiment, the diene rubber component includes modified butadiene rubber (modified BR). Modified butadiene rubber is butadiene rubber (BR) in which the terminals and / or main chain have been modified. Here, butadiene rubber is a polymer of 1,3-butadiene and is also called polybutadiene.

[0015] As the modified butadiene rubber, a butadiene rubber modified by introducing a functional group to the ends and / or main chain is used. Examples of functional groups include those that interact (have reactivity or affinity) with the silanol groups on the silica surface, and include those containing heteroatoms. As the heteroatom, at least one selected from the group consisting of oxygen atoms, nitrogen atoms, and silicon atoms is preferred. Specific examples of functional groups include at least one selected from the group consisting of polyorganosiloxane groups, alkoxysilyl groups, hydroxyl groups, aldehyde groups, carboxyl groups, alkoxy groups, amino groups, imino groups, epoxy groups, and amide groups. As the modified butadiene rubber, it is preferable to use a terminally modified butadiene rubber having the above functional groups on both or one of its molecular ends.

[0016] In the present embodiment, 100 parts by mass of the diene rubber component contains 40 parts by mass or more of the modified butadiene rubber. That is, 40% by mass or more of the diene rubber component is the modified butadiene rubber. By increasing the proportion of the modified butadiene rubber, the diene rubber component and the terpene-based resin can be brought into a phase-separated state, thereby achieving both low-temperature performance and wet grip performance. From the viewpoint of enhancing the above-mentioned compatibility effect, 100 parts by mass of the diene rubber component preferably contains 60 parts by mass or more of the modified butadiene rubber, and more preferably contains 65 parts by mass or more of the modified butadiene rubber. The diene rubber component may be composed of only the modified butadiene rubber. The amount of the modified butadiene rubber may be 60 to 90 parts by mass, or 65 to 85 parts by mass, based on 100 parts by mass of the diene rubber component.

[0017] In one embodiment, the modified butadiene rubber preferably has a glass transition temperature (Tg) of -85°C or lower. The glass transition temperature of the modified butadiene rubber may be -90°C to -110°C.

[0018] In the present specification, the glass transition temperature (Tg) is a value measured by a differential scanning calorimetry (DSC) method in accordance with JIS K7121:2012 at a heating rate of 20°C / min (measurement temperature range: -150°C to 50°C).

[0019] In one embodiment, the diene rubber component may contain other diene rubbers in addition to the modified butadiene rubber. The diene rubber refers to a rubber having a repeating unit corresponding to a diene monomer having a conjugated double bond. Specific examples of the other diene rubbers include natural rubber (NR), synthetic isoprene rubber (IR), styrene-butadiene rubber (SBR), unmodified butadiene rubber, nitrile rubber (NBR), chloroprene rubber (CR), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, and other various diene rubbers commonly used in rubber compositions. These other diene rubbers, excluding unmodified butadiene rubber, may also include those whose terminal or main chain is modified as needed, or those modified to impart desired properties (e.g., modified NR), which are also encompassed by the concept.

[0020] The styrene-butadiene rubber as another diene rubber may be solution-polymerized SBR (SSBR) or emulsion-polymerized SBR (ESBR). The styrene-butadiene rubber may also be a modified SBR that is modified by functional groups introduced into its terminal and / or main chain. Similar to the modified butadiene rubber, the functional groups of the modified SBR include those that interact (have reactivity or affinity) with silanol groups on the silica surface, and specific examples thereof are as described above.

[0021] In one embodiment, 100 parts by mass of the diene rubber component may include 40 to 90 parts by mass of the modified butadiene rubber and 10 to 60 parts by mass of at least one selected from the group consisting of natural rubber, synthetic isoprene rubber, and styrene-butadiene rubber. 100 parts by mass of the diene rubber component may include 60 to 85 parts by mass (more preferably 65 to 80 parts by mass) of the modified butadiene rubber and 15 to 40 parts by mass (more preferably 20 to 35 parts by mass) of at least one selected from the group consisting of natural rubber, synthetic isoprene rubber, and styrene-butadiene rubber.

[0022] [(B) Silica] The rubber composition according to the present embodiment contains silica as a filler. Examples of silica include wet silica and dry silica. Wet silica such as wet-precipitated silica and wet-gelled silica is preferably used.

[0023] The nitrogen adsorption specific surface area (N2SA) of silica is not particularly limited, and may be, for example, 100 to 300 m 2 / g, 150 to 250 m 2 / g, or 160 to 220 m 2 / g. The nitrogen adsorption specific surface area of silica is the BET specific surface area measured according to the BET method described in JIS K6430:2008.

[0024] The silica content is 60 to 200 parts by mass per 100 parts by mass of the diene-based rubber component. A silica content of 60 parts by mass or more can improve wet grip performance. Preferably, the silica content is 80 to 180 parts by mass, more preferably 90 to 160 parts by mass, and may also be 110 to 160 parts by mass per 100 parts by mass of the diene-based rubber component.

[0025] The filler used in the rubber composition may be silica alone, or it may be silica mixed with carbon black. The filler preferably contains 80% by mass or more silica, and more preferably 90% by mass or more. The carbon black content is not particularly limited and may be 15 parts by mass or less, or 1 to 10 parts by mass, per 100 parts by mass of the rubber component.

[0026] The carbon black used is not particularly limited, and various known varieties can be used. Specifically, these include SAF grade (N100 series), ISAF grade (N200 series), HAF grade (N300 series), FEF grade (N500 series), and GPF grade (N600 series) (all ASTM grades). One or more of these grades of carbon black can be used in combination.

[0027] [(C) Terpene resin] The rubber composition according to this embodiment contains a terpene resin having a β-pinene unit content of 40% by mass or more.

[0028] Terpene resins are resins obtained by polymerizing terpene compounds such as α-pinene, β-pinene, limonene, and dipentene, and have units derived from the terpene compounds. Examples of terpene resins include polyterpene resins obtained by polymerizing only terpene compounds, and modified terpene resins obtained by polymerizing terpene compounds with monomers other than terpenes. Examples of modified terpene resins include aromatic modified terpene resins obtained by polymerizing terpene compounds with aromatic compounds. Preferably, the terpene resin is a polyterpene resin with a β-pinene unit content of 40% by mass or more, and more preferably a pinene resin with a β-pinene unit content of 40% by mass or more.

[0029] The β-pinene unit content refers to the content of β-pinene units in 100% by mass of the terpene resin. A β-pinene unit is a unit derived from β-pinene. In terpene resins, the β-pinene unit content is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and may also be 100% by mass, from the viewpoint of lowering compatibility with modified butadiene rubber and improving the effect of achieving both low-temperature performance and wet grip performance.

[0030] The α-pinene unit content of the terpene resin is 60% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, even more preferably 5% by mass or less, and may even be 0% by mass. The α-pinene unit content is the content of α-pinene units in 100% by mass of the terpene resin. An α-pinene unit is a unit derived from α-pinene.

[0031] The softening point of terpene resins is not particularly limited and may be, for example, 100°C to 150°C or 110°C to 130°C. Here, the softening point is measured in accordance with ASTM D6090 (published in 1997).

[0032] The method for synthesizing terpene resins is not particularly limited. For example, terpene resins can be synthesized by cationic polymerization of a monomer containing β-pinene using a Lewis acid catalyst. Specific examples of Lewis acid catalysts are not particularly limited and include metal halides (e.g., BF3, BBr3, AlF3, AlBr3, TiCl4, TiBr4, FeCl3, FeCl2, SnCl4, WCl6, MoCl5, ZrCl4, SbCl3, SbCl5, TeCl2, and ZnCl2), metal alkyl compounds (e.g., Et3Al, Et2AlCl, EtAlCl2, Et3Al2Cl3, (iBu)3Al, (iBu)2AlCl, (iBu)AlCl2, Me4Sn, Et4Sn, Bu4Sn, and Bu3SnCl), and metal alkoxy compounds (e.g., Al(OR) 3-x Cl x and Ti(OR) 4-y Cl y (In the formula, R represents an alkyl group or aryl group, x represents an integer of 1 or 2, and y represents an integer of 1 to 3)). Here, Et represents an ethyl group, iBu represents an isobutyl group, Me represents a methyl group, and Bu represents a butyl group.

[0033] The terpene resin content is 20 to 60 parts by mass per 100 parts by mass of the diene rubber component. A terpene resin content of 20 parts by mass or more can improve wet grip performance. A terpene resin content of 60 parts by mass or less can suppress deterioration of low-temperature performance. The terpene resin content per 100 parts by mass of the diene rubber component is preferably 25 parts by mass or more. Furthermore, this content is preferably less than 60 parts by mass, more preferably 50 parts by mass or less, even more preferably 45 parts by mass or less, and may even be 40 parts by mass or less.

[0034] [oil] The rubber composition according to this embodiment may contain oils. Examples of oils include mineral oils such as paraffinic oils, naphthenic oils, and aromatic oils, and vegetable oils such as linseed oil, safflower oil, soybean oil, corn oil, castor oil, rapeseed oil, and cottonseed oil. Any one or more of these can be used in combination.

[0035] The oil content is preferably 0 to 40 parts by mass, more preferably 5 to 38 parts by mass, more preferably 10 to 35 parts by mass, and even more preferably 15 to 30 parts by mass, per 100 parts by mass of the diene-based rubber component. Note that, if oil-expandable rubber is used as the diene-based rubber, the oil content also includes the amount of oil contained in the oil-expandable rubber.

[0036] In the rubber composition according to this embodiment, it is preferable that the total content of terpene resin and oil is less than 60 parts by mass per 100 parts by mass of diene rubber component. By reducing the total amount of terpene resin and oil, the tackiness of the unvulcanized rubber composition can be reduced and processability can be improved. The total content of terpene resin and oil is more preferably 25 to 58 parts by mass, even more preferably 30 to 57 parts by mass, and may also be 40 to 56 parts by mass per 100 parts by mass of diene rubber component.

[0037] [Other ingredients] In addition to the above-mentioned components, the rubber composition according to this embodiment may also contain various additives commonly used in rubber compositions, such as silane coupling agents, zinc oxide, stearic acid, antioxidants, waxes, vulcanizing agents, and vulcanization accelerators.

[0038] Examples of silane coupling agents include sulfide silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)disulfide, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropyl Examples of mercaptosilane coupling agents include pyrtriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyldimethylmethoxysilane, and mercaptoethyltriethoxysilane; and thioester group-containing silane coupling agents include 3-octanoylthio-1-propyltriethoxysilane, 3-propionylthiopropyltrimethoxysilane, 3-hexanoylthio-1-propyltriethoxysilane, and 3-octanoylthio-1-propyltrimethoxysilane. These can be used individually or in combination of two or more.

[0039] The content of the silane coupling agent is not particularly limited, but is preferably 2 to 25% by mass of the silica amount, that is, 2 to 25 parts by mass per 100 parts by mass of silica. More preferably, the content of the silane coupling agent is 5 to 20% by mass of the silica amount, and even more preferably 5 to 15% by mass.

[0040] The zinc oxide content is not particularly limited; for example, it may be 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass per 100 parts by mass of the diene rubber component.

[0041] The stearic acid content is not particularly limited; for example, it may be 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass per 100 parts by mass of the diene rubber component.

[0042] Examples of anti-aging agents include amine-ketone, aromatic secondary amine, monophenol, bisphenol, and benzimidazole-based anti-aging agents, and one or more of these can be used in combination. The content of the anti-aging agent is not particularly limited and may be 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass per 100 parts by mass of the diene-based rubber component.

[0043] Sulfur is preferably used as the vulcanizing agent. The amount of vulcanizing agent is not particularly limited, but may be 0.1 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 3 parts by mass per 100 parts by mass of the diene rubber component.

[0044] Examples of vulcanization accelerators include sulfenamide-based, guanidine-based, thiuram-based, and thiazole-based vulcanization accelerators, which can be used individually or in combination of two or more. The content of the vulcanization accelerator is not particularly limited, but is preferably 0.1 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, and may also be 1 to 3 parts by mass, per 100 parts by mass of the diene-based rubber component.

[0045] [Method for preparing rubber composition] The rubber composition according to this embodiment can be prepared by kneading in accordance with conventional methods using a commonly used mixer such as a Banbury mixer, kneader, or roll. That is, for example, in the first mixing stage (non-progressive kneading stage), additives other than the vulcanizing agent and vulcanization accelerator are added and mixed with silica and terpene resin to the diene rubber component. Then, in the final mixing stage (progressive kneading stage), the vulcanizing agent and vulcanization accelerator are added and mixed to the resulting mixture. This makes it possible to prepare an unvulcanized rubber composition.

[0046] [Uses of rubber compositions] The rubber composition according to this embodiment can be used as a rubber composition for tire treads. Examples of tires include passenger car tires, heavy-duty tires for trucks and buses, and pneumatic tires of various sizes and applications.

[0047] As described above, the rubber composition according to this embodiment can achieve both low-temperature performance and wet grip performance, and is therefore preferably used in the tread rubber that constitutes the contact surface of all-season tires. All-season tires are tires that can be used throughout the year, from summer roads to snowy winter roads, and are also called all-weather tires.

[0048] A tire according to one embodiment is a tire having a tread made using the above-mentioned rubber composition. That is, a tire according to one embodiment is equipped with a tread rubber made of the above-mentioned rubber composition.

[0049] The tread rubber of a tire may have a two-layer structure consisting of a cap rubber and a base rubber, or a single-layer structure in which both are integrated. In the case of a single-layer structure, the tread rubber may be formed from the above-mentioned rubber composition. In the case of a two-layer structure, the outer cap rubber that contacts the road surface may be formed from the above-mentioned rubber composition, the base rubber placed inside the cap rubber may be formed from the above-mentioned rubber composition, or both the cap rubber and the base rubber may be formed from the above-mentioned rubber composition.

[0050] The method for manufacturing the tire is not particularly limited. For example, the rubber composition described above can be molded into a predetermined shape by extrusion according to a conventional method to obtain an unvulcanized tread rubber member. By combining this tread rubber member with other tire members, an unvulcanized tire (green tire) can be produced. Subsequently, the tire can be manufactured by vulcanization molding at, for example, 140°C to 180°C. [Examples]

[0051] The following are examples, but the present invention is not limited to these examples.

[0052] The components used in the examples and comparative examples are as follows: • Unmodified BR: Unmodified butadiene rubber polymerized using a neodymium-based catalyst, Tg = -102°C, manufactured by JSR Corporation, "BR730" • Modified BR: Terminally modified butadiene rubber with polyorganosiloxane groups at the ends, Tg = -92℃, manufactured by Nippon Zeon Co., Ltd. "Nipol BR1261" • SBR1: Modified SSBR, Tg = -60℃, styrene content 10% by mass, microstructure of butadiene portion; vinyl content 42%, manufactured by JSR Corporation as "HPR840". • SBR2: Unmodified SSBR, Tg = -68℃, 37.5 parts by mass of oil per 100 parts by mass of rubber, manufactured by Asahi Kasei Corporation as "Toughden 1834" • SBR3: Modified SSBR, Tg = -24℃, Styrene content 20.5% by mass, Microstructure of the butadiene portion; Vinyl content 55.5%, manufactured by JSR Corporation as "HPR350" • NR: RSS#3

[0053] • Carbon Black: "Seast 3" manufactured by Tokai Carbon Co., Ltd. • Silica: Evonik Industries' "Ultrasil VN3" (N2SA=180m) 2 / g) • Silane coupling agent 1: Bis(3-triethoxysilylpropyl)tetrasulfide, Evonik Industries "Si69" • Silane coupling agent 2:3-octanoylthio-1-propyltriethoxysilane, manufactured by Momentive Performance Materials, Inc. "NXT"

[0054] • Oil: ENEOS Corporation's "Process NC140" • Zinc oxide: "Zinc Oxide Type 2" manufactured by Mitsui Mining & Smelting Co., Ltd. • Stearic acid: "Lunaq S-20" manufactured by Kao Corporation • Anti-aging agent: "Antigen 6C" manufactured by Sumitomo Chemical Co., Ltd.

[0055] ·Terpene resin 1: β-pinene unit content = 100% by mass, softening point = 115℃, "DERCOLYTE S 115" manufactured by DRT ·Terpene resin 2: β-pinene unit content = 98% by mass or more, softening point = 115℃, "Sylvatraxx4150" manufactured by KRATON • Terpene resin 3: α-pinene unit content = 100% by mass, softening point = 115°C, DRT "DERCOLYTE A 115" • Hydrocarbon resin: Styrene monomer / aliphatic monomer copolymer resin, softening point = 110°C, manufactured by Mitsui Chemicals, Inc. "FTR6110"

[0056] • Sulfur: Tsurumi Chemical Industries Co., Ltd. "Powdered Sulfur" • Vulcanization accelerator CBS: Sulfenamide type, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. "Noxellar CZ-G (CZ)" • Vulcanization accelerator DPG: Guanidine-based, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., "Noxellar D"

[0057] The evaluation methods in the examples and comparative examples are as follows. (1) Wet grip performance Four prototype tires were mounted on a 2000cc 4WD vehicle, and the vehicle was driven on a road surface with 2-3mm of water. The braking distance was measured when decelerating from 90km / h to 20km / h with ABS activated (average value for n=10). The reciprocal of the braking distance is shown as an index, with the values ​​for Comparative Example 1 (Table 1), Comparative Example 11 (Table 2), and Comparative Example 21 (Table 3) set to 100. A larger index indicates a shorter braking distance and superior wet grip performance.

[0058] (2) Low temperature performance In accordance with JIS K6253:2012, hardness was measured at -5°C using a Type A durometer. The reciprocal of hardness is shown as an index, with the values ​​for Comparative Example 1 (Table 1), Comparative Example 11 (Table 2), and Comparative Example 21 (Table 3) set to 100. A larger index indicates softer material and superior low-temperature performance in a low-temperature environment (-5°C).

[0059] (3) Processability (unvulcanized viscosity) In accordance with JIS K6300-1:2013, a rotaryless Mooney viscosity measuring instrument manufactured by Toyo Seiki Co., Ltd. was used to preheat unvulcanized rubber compositions at 100°C for 1 minute, and then measure the torque value in Mooney units after 4 minutes. Table 1 shows the values ​​for Comparative Example 1, Table 2 shows the values ​​for Comparative Example 11, and Table 3 shows the values ​​for Comparative Example 21, all of which are shown as indices with a base of 100. A higher index indicates higher Mooney viscosity, resulting in lower tackiness of the rubber composition and superior processability.

[0060] (4) Processability (ease of discharge) After mixing the rubber composition in a Banbury mixer, the ease of discharge of the mixture from the Banbury mixer was evaluated using the following methods 1-3. 1: Discharges smoothly without any problems. 2: A small amount of the mixture was found adhering to the mixer wall. 3: The mixed material adheres to the mixer walls, making it difficult to discharge.

[0061] [First Experimental Example] Using a Banbury mixer, according to the formulation (parts by mass) shown in Table 1 below, first, in the first mixing stage, compounding agents excluding sulfur and vulcanization accelerator were added to the diene-based rubber component and kneaded (discharge temperature = 160°C). Next, in the final mixing stage, sulfur and vulcanization accelerator were added to the resulting knead and kneaded (discharge temperature = 90°C) to prepare the rubber composition.

[0062] In Table 1, the amounts in parentheses for SBR2 represent the amount as rubber, and the remainder represents the amount of oil. In Table 1, "Resin + Oil (parts by mass)" is the total amount of resin and oil per 100 parts by mass of diene-based rubber component (the same applies to Tables 2 and 3), and the oil includes the oil contained in oil-spreading rubber.

[0063] The processability (ease of discharge) was evaluated during discharge at the final mixing stage, and the processability (unvulcanized viscosity) of the unvulcanized rubber composition was also evaluated. Furthermore, test specimens were prepared by vulcanizing the unvulcanized rubber composition at 160°C for 20 minutes, and the low-temperature performance was evaluated. In addition, a pneumatic radial tire (all-season tire, tire size: 215 / 45ZR17) was manufactured by using the unvulcanized rubber composition as the tread rubber and vulcanizing it according to a conventional method. The wet grip performance of the resulting prototype tire was evaluated.

[0064] [Table 1]

[0065] The results are shown in Table 1. In the first experimental example, 40% by mass of the diene rubber component is butadiene rubber. In Comparative Example 1, a terpene resin with a high α-pinene unit content was blended with unmodified butadiene rubber as the resin. In this case, the compatibility between the resin and the butadiene rubber was high, making it difficult to achieve both low-temperature performance and wet grip performance.

[0066] In Comparative Example 2, a terpene-based resin with a high β-pinene unit content was used as the resin, resulting in phase separation between the rubber component and the resin. Compared to Comparative Example 1, this improved wet grip performance while suppressing deterioration of low-temperature performance. However, because the butadiene rubber was unmodified, the processability was poor.

[0067] In Comparative Example 3, a terpene-based resin with a high α-pinene unit content was blended with modified butadiene rubber. In this case, an improvement in low-temperature performance was observed, but wet grip performance was inferior, making it difficult to achieve both. In Comparative Example 4, a petroleum-based hydrocarbon resin was used as the resin, and, similar to Comparative Example 3, it was difficult to achieve both low-temperature performance and wet grip performance.

[0068] In contrast, in Examples 1 to 4, a terpene-based resin with a high β-pinene unit content was used as the resin, resulting in phase separation between the rubber component and the resin. Compared to Comparative Example 1, this improved wet grip performance while maintaining or improving low-temperature performance. Furthermore, by using modified butadiene rubber, processability was improved compared to Comparative Example 2 while maintaining the effect of achieving both wet grip performance and low-temperature performance.

[0069] In Comparative Example 5, the amount of terpene resin was too low, resulting in insufficient improvement in wet grip performance. In Comparative Example 6, the amount of terpene resin was too high, leading to a deterioration in low-temperature performance and processability compared to Comparative Example 1.

[0070] [Second Experimental Example] Rubber compositions were prepared according to the formulations (parts by mass) shown in Table 2 below, with the rest being the same as in the first experimental example. For each rubber composition, wet grip performance, low-temperature performance, processability (unvulcanized viscosity), and processability (ease of discharge) were evaluated in the same manner as in the first experimental example. The results are shown in Table 2.

[0071] [Table 2]

[0072] The second experimental example is one in which 70% by mass of the diene rubber component is butadiene rubber. In the second experimental example, as in the first experimental example, Examples 11 to 14, which incorporated a terpene resin with a high β-pinene unit content, showed improved wet grip performance and low-temperature performance compared to Comparative Example 11, which incorporated a terpene resin with a high α-pinene unit content. Furthermore, by using modified butadiene rubber, processability was improved compared to Comparative Example 12, which used unmodified butadiene rubber, while maintaining the effect of balancing wet grip performance and low-temperature performance. In addition, since the proportion of modified butadiene rubber in the diene rubber component was higher in the second experimental example than in the first experimental example, a tendency for a higher effect of balancing wet grip performance and low-temperature performance was observed compared to the first experimental example.

[0073] [Third experimental example] Rubber compositions were prepared according to the formulations (parts by mass) shown in Table 3 below, with the rest of the preparation being the same as in the first experimental example. For each rubber composition, wet grip performance, low-temperature performance, processability (unvulcanized viscosity), and processability (ease of discharge) were evaluated in the same manner as in the first experimental example. The results are shown in Table 3.

[0074] [Table 3]

[0075] The third experimental example is one in which 75% by mass of the diene rubber component is butadiene rubber. In the third experimental example, as in the first experimental example, Examples 21 to 24, which incorporated a terpene resin with a high β-pinene unit content, showed improved wet grip performance and low-temperature performance compared to Comparative Example 21, which incorporated a terpene resin with a high α-pinene unit content. Furthermore, by using modified butadiene rubber, processability was improved compared to Comparative Example 22, which used unmodified butadiene rubber, while maintaining the effect of balancing wet grip performance and low-temperature performance. In addition, since the proportion of modified butadiene rubber in the diene rubber component was higher in the third experimental example than in the first experimental example, a tendency for a higher effect of balancing wet grip performance and low-temperature performance was observed compared to the first experimental example.

[0076] Furthermore, the various numerical ranges described in this specification can be any combination of their upper and lower limits, and all such combinations are described herein as preferred numerical ranges. Also, the description of a numerical range as "X~Y" means X or greater and Y or less.

[0077] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their omissions, substitutions, and modifications are included in the scope and spirit of the invention, as well as in the claims and their equivalents.

Claims

1. 100 parts by mass of a diene rubber component containing 40 parts by mass or more of modified butadiene rubber having a functional group that interacts with silanol groups on the silica surface, 60 to 200 parts by mass of silica, and 20 to 58 parts by mass of a terpene resin having a β-pinene unit content of 40% by mass or more and a softening point of 100°C to 150°C. Includes, The total content of the terpene resin and oil is 58 parts by mass or less per 100 parts by mass of the diene rubber component. Rubber composition for tire treads.

2. The rubber composition for tire treads according to claim 1, wherein 100 parts by mass of the diene-based rubber component contains 60 parts by mass or more of the modified butadiene rubber.

3. A tire having a tread made using the rubber composition for tire treads described in claim 1 or 2.

Citation Information

Patent Citations

  • Tire tread

    JP2017500402A

  • Rubber composition for tread and pneumatic tire

    JP2018083932A

  • Cap tread rubber composition for studless tire

    JP2018177980A

  • Tread rubber composition and pneumatic tire

    JP2020041077A

  • Winter tire

    JP2021195000A