Positive electrode active material layer, positive electrode, and all-solid-state secondary battery

The core-shell structured positive electrode active material layer with a lithium transition metal oxide core and halogen-containing shell, combined with a halide-based electrolyte, addresses the self-discharge issue in all-solid-state batteries by stabilizing the interface and reducing side reactions.

JP7955156B2Active Publication Date: 2026-11-24TDK CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022205482
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2026-11-24
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Conventional all-solid-state secondary batteries, particularly those using a halide-based solid electrolyte, suffer from significant self-discharge when left in an open circuit state, leading to cell voltage drop.

Method used

A positive electrode active material layer with a core-shell structure is developed, where the core is made of a lithium transition metal oxide and the shell is composed of a compound containing oxygen and a halogen element, combined with a halide-based solid electrolyte, which forms a strong covalent bond to suppress reactions between the core and electrolyte.

Benefits of technology

This structure significantly reduces side reactions and enhances self-discharge characteristics by stabilizing the interface, preventing cell voltage drop when the battery is left standing in an open circuit state.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955156000003
    Figure 0007955156000003
  • Figure 0007955156000004
    Figure 0007955156000004
  • Figure 0007955156000001
    Figure 0007955156000001
Patent Text Reader

Abstract

To provide a positive electrode active material layer capable of forming a positive electrode of an all-solid-state secondary battery in which self-discharge is suppressed.SOLUTION: A positive electrode active material layer 1B includes a positive electrode active material, and a solid electrolyte 11, the positive electrode active material includes particles 10 having a core-shell structure with a core portion 10a and a shell portion 10b covering at least a part of the surface of the core portion 10a, and the core portion 10a is made of a lithium transition metal oxide, the shell portion 10b is made of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I, and the solid electrolyte 11 includes a halide-based solid electrolyte.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a positive electrode active material layer, a positive electrode, and an all-solid-state secondary battery. [Background Art]

[0002] In recent years, the electronics industry has developed remarkably, and portable electronic devices have been made smaller, lighter, thinner, and more multifunctional. Along with this, there is a strong demand for batteries serving as power sources for electronic devices to be smaller, lighter, thinner, and more reliable. Accordingly, all-solid-state secondary batteries using a solid electrolyte as the electrolyte have attracted attention. Conventionally, oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, halide-based solid electrolytes, and the like are known as solid electrolytes for all-solid-state secondary batteries.

[0003] As a negative electrode active material for all-solid-state batteries, one including a core part containing a carbon material and a shell part covering at least a part of the surface of the core part has been proposed (see Patent Document 1). Patent Document 1 describes that the shell part contains a metal oxide. [Prior Art Documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent No. 7038951 [Summary of Invention] [Problem to be Solved by the Invention]

[0005] However, conventional all-solid-state secondary batteries have insufficient self-discharge characteristics, and have had a problem of capacity degradation in an open circuit state. In particular, in all-solid-state secondary batteries using a halide-based solid electrolyte as the solid electrolyte, the cell voltage drop when left standing in an open circuit state is remarkable, and improvement of self-discharge characteristics has been required.

[0006] The present invention was made in view of the above problems, and aims to provide a positive electrode active material layer capable of forming a positive electrode of an all-solid secondary battery with suppressed self-discharge, as well as a positive electrode and an all-solid secondary battery comprising the same. [Means for Solving the Problems]

[0007] In order to solve the above problems, the following means are provided. A positive electrode active material layer according to an aspect of the present invention includes a positive electrode active material and a solid electrolyte, the positive electrode active material includes particles having a core-shell structure comprising a core portion and a shell portion covering at least a part of the surface of the core portion, the core portion is made of a lithium transition metal oxide represented by the following formula (1), the shell portion is made of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I, the solid electrolyte includes a halide-based solid electrolyte represented by the following formula (2).

[0008] Li x MO y ···(1) (In formula (1), M is one or more transition metals. 0.1<x<1.1, 1.8<y<2.2) A a E b G c X d ···(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , Si6O 18 , PO3, PO4, P2O7, P3O 10, is at least one group selected from the group consisting of O, SO, SO2, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB. X is at least one element selected from the group consisting of F, Cl, Br, I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1) [Effects of the Invention]

[0009] The positive electrode active material layer of the present invention comprises a positive electrode active material and a solid electrolyte. The positive electrode active material includes particles having a core-shell structure comprising a core portion made of a lithium transition metal oxide represented by formula (1) and a shell portion made of a compound containing oxygen and a halogen element, covering at least a portion of the surface of the core portion. The solid electrolyte includes a halide-based solid electrolyte represented by formula (2). Therefore, a shell portion made of a compound containing oxygen and a halogen element is arranged in a portion between the core portion and the solid electrolyte of the particles having a core-shell structure. Halogen elements are elements with high electronegativity. For this reason, the oxygen and halogen element in the compound containing oxygen and a halogen element forming the shell portion form a strong covalent bond. Therefore, the compound containing oxygen and a halogen element forming the shell portion is electrochemically stable. As a result, in an all-solid-state secondary battery having a positive electrode equipped with the positive electrode active material layer of the present invention, the reaction between the core portion and the solid electrolyte is suppressed by the shell portion. As a result, this all-solid-state secondary battery is less prone to cell voltage drop due to side reactions when left standing in an open-circuit state and has excellent self-discharge characteristics. [Brief explanation of the drawing]

[0010] [Figure 1] This is a schematic cross-sectional view showing an all-solid-state secondary battery according to the first embodiment. [Figure 2] Figure 2(a) is a schematic cross-sectional view showing an enlarged portion of the positive electrode active material layer 1B of the all-solid-state secondary battery 100 shown in Figure 1. Figure 2(b) is a schematic cross-sectional view showing an enlarged portion of Figure 2(a). [Modes for carrying out the invention]

[0011] In order to solve the above problems, the inventors focused on the reaction between the positive electrode active material and the solid electrolyte in a positive electrode active material layer containing a halogen element, and conducted extensive research. As a result, we found that by forming an all-solid-state secondary battery structure having a positive electrode active material layer comprising a positive electrode active material made of a specific lithium transition metal oxide and a solid electrolyte containing a specific halide-based solid electrolyte, and performing the initial charge and discharge at a high temperature of 60°C to 85°C, the positive electrode active material and the solid electrolyte react in the positive electrode active material layer to generate a compound containing oxygen and halogen elements along at least a portion of the surface of the particles of the positive electrode active material.

[0012] Compounds containing oxygen and halogen elements, formed along at least a portion of the surface of the positive electrode active material particles, are presumed to be formed by the reaction of oxygen released from the positive electrode active material and halogen elements diffused from the solid electrolyte when the all-solid-state secondary battery is charged and discharged at high temperatures of 60°C to 85°C. Compounds containing oxygen and halogen elements are electrochemically stable because they have a strong covalent bond between the highly electronegative halogen element and oxygen. Therefore, compounds containing oxygen and halogen elements, formed along at least a portion of the surface of the positive electrode active material particles, are difficult to decompose, reduce the contact area between the positive electrode active material and the solid electrolyte, and suppress the reaction between the positive electrode active material and the solid electrolyte when left standing in an open circuit state.

[0013] Based on the above findings, the inventors conducted further investigations. As a result, they found that an all-solid-state secondary battery structure may be formed having a positive electrode active material layer comprising a positive electrode active material made of a specific lithium transition metal oxide, a solid electrolyte containing a specific halide-based solid electrolyte, and a compound containing a halogen element different from the halogen element contained in the solid electrolyte, and that by performing the initial charge and discharge at a high temperature of 60°C to 85°C, the positive electrode active material and the compound containing the halogen element may react in the positive electrode active material layer to generate a compound containing oxygen and a halogen element along at least a portion of the surface of the particles of the positive electrode active material.

[0014] In this way, compounds containing oxygen and halogen elements, formed along at least a portion of the surface of the positive electrode active material particles, are electrochemically stable and therefore difficult to decompose, reducing the contact area between the positive electrode active material and the solid electrolyte, and suppressing the reaction between the positive electrode active material and the solid electrolyte when left standing in an open circuit state.

[0015] Based on these findings, it is presumed that a positive electrode comprising a positive electrode active material layer containing a specific lithium transition metal oxide and a solid electrolyte containing a specific halide-based solid electrolyte, wherein at least a portion of the surface of the particles of the positive electrode active material is coated with a compound containing oxygen and halogen elements, will be less prone to cell voltage drop due to side reactions when an all-solid-state secondary battery having this electrode is left standing in an open circuit state, and will have excellent self-discharge characteristics.

[0016] The present invention includes the following embodiments. [1] comprising a positive electrode active material and a solid electrolyte, The positive electrode active material includes particles having a core-shell structure comprising a core portion and a shell portion covering at least a part of the surface of the core portion. The core portion is made of a lithium transition metal oxide represented by the following formula (1), The shell portion is made of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I. The solid electrolyte is a positive electrode active material layer containing a halide-based solid electrolyte represented by the following formula (2).

[0017] Li x MO y ...(1) (In equation (1), M is one or more transition metals. 0.1 <x<1.1、1.8<y<2.2) A a E b G c X d ...(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 Si6O 18 PO3, PO4, P2O7, P3O 10 , is at least one group selected from the group consisting of O, SO, SO2, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB. X is at least one element selected from the group consisting of F, Cl, Br, I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1)

[0018] [2] The positive electrode active material layer according to [1], wherein the average thickness of the shell portion is 0.1 μm to 1.0 μm. [3] The positive electrode active material layer according to [1] or [2], wherein the ratio of the area of ​​the shell portion to the cross-sectional area of ​​the particles having the core-shell structure is 1% to 40%. [4] The positive electrode active material layer according to any one of [1] to [3], wherein the halogen element contained in the shell portion and the halogen element contained in the solid electrolyte are the same element. [5] The positive electrode active material layer according to any one of [1] to [4], wherein the ratio of halogen element content at the interface between the shell portion and the solid electrolyte and the interface between the shell portion and the core portion is 0.6 or more and less than 1.0.

[0019] A positive electrode comprising a positive electrode active material layer as described in any of [6] [1] to [5]. [7] [6] An all-solid-state secondary battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer.

[0020] [8] The all-solid-state secondary battery according to [7], wherein the solid electrolyte layer comprises a halide-based solid electrolyte represented by the following formula (2). A a E b G cX d ...(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 Si6O 18 PO3, PO4, P2O7, P3O 10 , is at least one group selected from the group consisting of O, SO, SO2, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB. X is at least one element selected from the group consisting of F, Cl, Br, I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1)

[0021] [9] The all-solid-state secondary battery according to [8], wherein the solid electrolyte layer comprises Li2ZrSO4Cl4.

[0022] The positive electrode active material layer, positive electrode, and all-solid-state secondary battery of this embodiment will be described in detail below with reference to the drawings as appropriate. In the drawings used in the following description, characteristic parts may be enlarged for convenience in order to make the features of the present invention easier to understand. Therefore, the dimensional ratios of each component may differ from those of the actual components. The materials, dimensions, etc. exemplified in the following description are examples only, and the present invention is not limited to them, and can be implemented with appropriate modifications without changing the essence of the invention.

[0023] [All-solid-state secondary battery] Figure 1 is a schematic cross-sectional view of the all-solid-state secondary battery 100 of this embodiment. The all-solid-state secondary battery 100 can be used, for example, in laminated batteries, prismatic batteries, cylindrical batteries, coin-type batteries, button-type batteries, etc. As shown in Figure 1, the all-solid-state secondary battery 100 has a laminate 4. The laminate 4 has a positive electrode layer 1 (positive electrode), a negative electrode layer 2 (negative electrode), and a solid electrolyte layer 3 sandwiched between the positive electrode layer 1 and the negative electrode layer 2. The number of positive electrode layer 1 and negative electrode layer 2 included in the laminate 4 may be one layer each, as shown in Figure 1, or it may be two or more layers.

[0024] The positive electrode layer 1 shown in Figure 1 is connected at one end to a first external terminal (not shown). The negative electrode layer 2 is connected at one end to a second external terminal (not shown). The first and second external terminals are made of a conductive material and are electrically connected to the outside. The all-solid-state secondary battery 100 shown in Figure 1 is charged or discharged by the exchange of ions between the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3.

[0025] "Positive electrode layer" As shown in Figure 1, the positive electrode layer 1 comprises a positive electrode current collector 1A and a positive electrode active material layer 1B. The positive electrode active material layer 1B may be formed on only one side of the positive electrode current collector 1A, or on both sides of the positive electrode current collector 1A, as shown in Figure 1.

[0026] (Positive electrode current collector) The positive electrode current collector 1A has excellent conductivity. The positive electrode current collector 1A is made of metals such as silver, palladium, gold, platinum, aluminum, copper, nickel, stainless steel, and iron, and their alloys. The positive electrode current collector 1A may also contain a positive electrode active material such as a lithium vanadium compound (LiV2O5, Li3V2(PO4)3, LiVOPO4).

[0027] (Cathode active material layer) Figure 2(a) is a schematic cross-sectional view showing an enlarged portion of the positive electrode active material layer 1B of the all-solid-state secondary battery 100 shown in Figure 1. Figure 2(b) is a schematic cross-sectional view showing an enlarged portion of Figure 2(a). As shown in Figures 2(a) and 2(b), the positive electrode active material layer 1B includes particles 10 having a core-shell structure, which are the positive electrode active material, and a solid electrolyte 11. The positive electrode active material layer 1B of this embodiment may also include a conductive additive 12, as shown in Figures 2(a) and 2(b).

[0028] (Cathode active material) The positive electrode active material reversibly facilitates the release and intercalation of ions (e.g., lithium ions), as well as the desorption and insertion of ions. As shown in Figure 2(b), the positive electrode active material includes a plurality of particles 10 having a core-shell structure, each particle comprising a particulate core portion 10a and a shell portion 10b covering at least a part of the core portion 10a. As shown in Figure 2(b), the shell portion 10b may cover only a part of the surface of the core portion 10a, or it may cover the entire surface of the core portion 10a. Ions such as lithium ions can diffuse into the shell portion 10b. Therefore, even when particles 10 in which the entire surface of the core portion 10a is covered with the shell portion 10b are used as the positive electrode active material, the all-solid-state secondary battery 100 having a positive electrode active material layer 1B containing these particles can be charged and discharged.

[0029] The multiple particles 10 contained in the positive electrode active material may consist only of particles in which a portion of the surface of the core portion 10a is covered by the shell portion 10b, or only of particles in which the entire surface of the core portion 10a is covered by the shell portion 10b, or both may be mixed in any proportion. The core-shell structure particles 10 contained in the positive electrode active material may be of only one type, or they may contain two or more different materials forming the core portion 10a and / or the shell portion 10b.

[0030] The core portion 10a is made of a lithium transition metal oxide represented by the following formula (1). Li x MO y ...(1) (In formula (1), M represents one or more transition metals. 0.1<x<1.1, 1.8<y<2.2)

[0031] M in formula (1) is one or more transition metals. M preferably contains at least one selected from Co, Ni, Mn, Fe, Mg, V, Ti, Al, Nb, Ti, Cu, and Cr, and more preferably contains at least one selected from Co, Ni, Mn, and Al. By performing initial charge and discharge at a high temperature of 60°C to 85°C, the core portion 10a reacts with the halogen element in the compound containing a halogen element included in the positive electrode active material layer (the halogen element included in the solid electrolyte 11, and / or the halogen element included in the compound containing a halogen element different from that included in the solid electrolyte 11), a shell portion 10b having a sufficient thickness and a sufficiently high area ratio relative to the cross-sectional area of the particle 10 is easily formed.

[0032] x in formula (1) satisfies 0.1<x<1.1, and preferably satisfies 0.2<x<0.6. This is because the lithium transition metal oxide represented by formula (1) forming the core portion 10a has a stable crystal structure.

[0033] y in formula (1) satisfies 1.8<y<2.2, and preferably satisfies 1.9<y<2.1. This is because the lithium transition metal oxide represented by formula (1) forming the core portion 10a has a stable crystal structure.

[0034] Specific examples of the lithium transition metal oxide represented by formula (1) include lithium cobaltate (LiCoO2 (LCO)), lithium nickelate (LiNiO2), LiNi x Co y Mn z M a O2 (x+y+z+a=1, 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦a≦1, M is one or more elements selected from Al, Mg, Nb, Ti, Cu, Cr), and LiNi x Co y Alz O2 (0.9 < x + y + z < 1.1), and other composite metal oxides. Among these lithium transition metal oxides, LiCoO2 (LCO), LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 (NCM), LiNi 0.85 Co 0.10 Al 0.05 O2 (NCA), and preferably includes any one selected from these, and most preferably LiCoO2 (LCO). When the core part 10a is LiCoO2 (LCO), LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 (NCM), LiNi 0.85 Co 0.10 Al 0.05 O2 (NCA), secondary reactions when left in an open circuit state are even less likely to occur, and particles 10 having a core-shell structure that can form an all-solid secondary battery 100 with even better self-discharge characteristics are obtained.

[0035] As shown in FIG. 2(a) and FIG. 2(b), the core part 10a is in the form of particles. The particle size of the core part 10a can be, for example, 5 μm to 30 μm, and is preferably 10 μm to 25 μm. When the particle size of the core part 10a is within the above range, using a method in which initial charge and discharge are performed at a high temperature of 60°C to 85°C, the halogen element in the compound containing the halogen element contained in the core part 10a and the positive electrode active material layer is reacted, thereby easily forming a shell part 10b having a sufficient thickness and an appropriate ratio of the area occupied by the cross-sectional area of the particle 10.

[0036] The shell part 10b is composed of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I. The halogen element contained in the shell part 10b is at least one selected from the group consisting of F, Cl, Br, and I, and preferably contains Br and / or Cl. This is because the shell part 10b is made of a compound with an appropriate covalent bonding force with oxygen, and the particles 10 can effectively suppress secondary reactions when left in an open circuit state.

[0037] The halogen element contained in the shell portion 10b may be the same as or different from the halogen element contained in the solid electrolyte of the positive electrode active material layer 1B. If the particles 10 having a core-shell structure include particles 10 having multiple types of core-shell structures, the halogen element contained in the shell portion 10b may be a mixture of particles with the same halogen element as the halogen element contained in the solid electrolyte of the positive electrode active material layer 1B and particles with different halogen elements, in any proportion.

[0038] In this embodiment, it is preferable that all particles 10 having a core-shell structure have the same halogen element contained in the shell portion 10b as the halogen element contained in the solid electrolyte of the positive electrode active material layer 1B. This is because it makes side reactions less likely to occur when left standing in an open circuit state, and the positive electrode active material layer 1B can form an all-solid-state secondary battery 100 with even better self-discharge characteristics. Furthermore, if the halogen element contained in the shell portion 10b and the halogen element contained in the solid electrolyte of the positive electrode active material layer 1B are the same element, the positive electrode active material layer 1B, which includes particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b, and a solid electrolyte 11, can be easily manufactured by using a method that performs the initial charge and discharge at a high temperature of 60°C to 85°C, without using a compound containing a different halogen element from the halogen element contained in the solid electrolyte 11.

[0039] Preferably, the shell portion 10b consists of oxygen, at least one halogen element selected from the group consisting of F, Cl, Br, and I, Li, and M (one or more transition metals) in formula (1) that forms the core portion 10a. This is because a positive electrode active material layer 1B containing a positive electrode active material including particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b, and a solid electrolyte 11 can be easily manufactured by using a method that performs the initial charge and discharge at a high temperature of 60°C to 85°C without using a compound containing a halogen element different from the halogen element contained in the solid electrolyte 11.

[0040] The shell portion 10b preferably has an average thickness of 0.1 μm to 1.0 μm, and more preferably 0.3 μm to 0.8 μm. When the average thickness of the shell portion 10b is 0.1 μm or more, the desorption of oxygen from the core portion 10a can be effectively suppressed in the all-solid-state secondary battery 100 having a positive electrode layer 1 with a positive electrode active material layer 1B. As a result, the reaction between the core portion 10a and the solid electrolyte 11 can be suppressed more effectively. Consequently, the all-solid-state secondary battery 100 having a positive electrode layer 1 with a positive electrode active material layer 1B of this embodiment is less prone to side reactions when left standing in an open-circuit state, and exhibits even better self-discharge characteristics. If the average thickness of the shell portion 10b is 1.0 μm or less, a positive electrode active material layer 1B containing a positive electrode active material including particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b, and a solid electrolyte 11 can be easily manufactured by using a method that performs the initial charge and discharge at a high temperature of 60°C to 85°C.

[0041] (Average thickness of shell section 10b) The average thickness of the shell portion 10b in this embodiment is the value measured by the method shown below. A cross-section of the positive electrode active material layer 1B is observed at a magnification of 30kx using a scanning electron microscope (SEM) to obtain a 256-level grayscale image of the core-shell structure particle 10. For the core-shell structure particle 10 in the obtained image, the lighter colored region (whitish region (average lightness of grayscale 193-207)) is designated as the core portion 10a, and the darker colored region (blackish region (average lightness of grayscale 174-187)) is designated as the shell portion 10b. For any one core-shell structure particle 10 in the field of view, the thickness of the shell portion 10b along the diameter direction of the particle 10 is measured at five arbitrary locations, and the average value is taken as the average thickness of the shell portion 10b.

[0042] The ratio of the shell portion 10b area to the cross-sectional area of ​​the core-shell structured particle 10 is preferably 1% to 40%, and more preferably 15% to 30%. When the ratio of the shell portion 10b area is 1% or more, the shell portion 10b can effectively reduce the contact area between the core portion 10a and the solid electrolyte 11. As a result, the desorption of oxygen from the core portion 10a to the solid electrolyte 11 of the all-solid-state secondary battery 100 is suppressed, and the reaction between the core portion 10a and the solid electrolyte 11 is more effectively suppressed. This makes it even less likely for side reactions to occur when left standing in an open circuit state, and allows for the formation of an all-solid-state secondary battery 100 with even better self-discharge characteristics.

[0043] If the ratio of the shell portion 10b area to the cross-sectional area of ​​the core-shell structure particle 10 is 40% or less, the diffusion of ions such as lithium ions within the particle 10 will not be hindered due to an excessively high ratio of the shell portion 10b area. Furthermore, if the ratio of the shell portion 10b area is 40% or less, a positive electrode active material layer 1B containing a positive electrode active material including a core-shell structure particle 10 comprising a core portion 10a and a shell portion 10b, and a solid electrolyte 11 can be easily manufactured by using a method that performs the initial charge and discharge at a high temperature of 60°C to 85°C.

[0044] (The ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the particle 10 having a core-shell structure) In this embodiment, the ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the core-shell structured particle 10 is a value measured by the method described below. A 256-level grayscale image of the core-shell structure particle 10 is obtained in the same manner as when the average thickness of the shell portion 10b was measured. For the core-shell structure particle 10 in the obtained image, the lighter colored areas are designated as the core portion 10a and the darker colored areas as the shell portion 10b, in the same manner as when the average thickness of the shell portion 10b was measured. Then, for any five core-shell structure particle 10 within the field of view, the area of ​​the core portion 10a and the area of ​​the shell portion 10b are determined for each. Using the obtained values, the ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the core-shell structure particle 10 ({area of ​​shell portion 10b / (area of ​​core portion 10a + area of ​​shell portion 10b)} × 100 (%)) is calculated for each of the five core-shell structure particle 10, and the average value of this is taken as the ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the core-shell structure particle 10.

[0045] In the particle 10 having the core-shell structure shown in Figure 2(b), the ratio of halogen element content at the interface 14 between the shell portion 10b and the solid electrolyte 11 and the interface 13 between the shell portion 10b and the core portion 10a (interface between shell portion 10b and core portion 10a / interface between shell portion 10b and solid electrolyte 11) is preferably 0.6 or more and less than 1.0, and more preferably 0.6 to 0.9. When the particle 10 having the core-shell structure is produced by using a method in which the initial charge and discharge is performed at a high temperature of 60°C to 85°C, the portion of the shell portion 10b closer to the interface 14 with the solid electrolyte 11 will have a higher halogen element content diffused from the halogen element compound contained in the positive electrode active material layer. On the other hand, the portion of the shell portion 10b closer to the interface 13 with the core portion 10a will have a lower halogen element content.

[0046] When the ratio of halogen element content at the above interface 14 and the above interface 13 is 0.6 or more, the entire shell portion 10b is sufficiently filled with halogen elements. Therefore, strong covalent bonds between halogen elements and oxygen are sufficiently formed in the shell portion 10b. Thus, a positive electrode active material layer 1B with an electrochemically more stable shell portion 10b is obtained. As a result, side reactions when left standing in an open circuit state are less likely to occur, and particles 10 having a core-shell structure can be formed to create an all-solid-state secondary battery 100 with even better self-discharge characteristics. Furthermore, when the ratio of the above interfaces is less than 1.0, a positive electrode active material layer 1B containing particles 10 having a core-shell structure with a shell portion 10b covering a part of the core portion 10a can be easily manufactured by using a method in which the initial charge and discharge is performed at a high temperature of 60°C to 85°C. Furthermore, if the ratio of the above interfaces is less than 1.0, the particle 10 will have suppressed excessive covalent bonding between the halogen element and oxygen at the interface 13 with the core portion 10a within the shell portion 10b, resulting in a more stable crystal structure of the core portion 10a. As a result, the particle 10 will be able to form an all-solid-state secondary battery 100 with even better self-discharge characteristics.

[0047] (Ratio of halogen element content) In this embodiment, the ratio of halogen element content at the interface 14 between the shell portion 10b and the solid electrolyte 11, and at the interface 13 between the shell portion 10b and the core portion 10a in the core-shell structured particle 10, is a value measured by the method described below. For any five particles 10 having a core-shell structure in the cross-section of the positive electrode active material layer 1B, a scanning transmission electron microscope (STEM) energy-dispersive X-ray spectroscopy (EDS) instrument is used to perform a mapping analysis of halogen elements in a 3 μm x 3 μm square measurement area (measurement interval 0.1 μm). Then, for each of the five particles 10 having a core-shell structure within the field of view, the ratio of the halogen element content (interface 13 between shell portion 10b and core portion 10a / interface 14 between shell portion 10b and solid electrolyte 11) is calculated using the measurement value closest to the interface between the thickest shell portion 10b along the diameter direction of the particle 10 and the core portion 10a, and the measurement value closest to the interface with the solid electrolyte 11, and the average value is calculated.

[0048] The positive electrode active material contained in the positive electrode active material layer 1B of this embodiment may consist only of particles 10 having a core-shell structure, as shown in Figure 2(a), or it may contain, together with the particles 10 having a core-shell structure, a positive electrode active material used in known all-solid-state secondary batteries, to the extent that the effects of the present invention can be obtained. Examples of positive electrode active materials that may be contained together with the particles 10 having a core-shell structure include particles consisting of a core portion 10a that is not covered by a shell portion 10b.

[0049] (solid electrolyte) The solid electrolyte 11 contained in the positive electrode active material layer 1B improves the ionic conductivity within the positive electrode active material layer 1B. The solid electrolyte 11 contained in the positive electrode active material layer 1B includes a halide-based solid electrolyte represented by the following formula (2).

[0050] A a E b G c X d ...(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 Si6O 18 PO3, PO4, P2O7, P3O 10 , is at least one group selected from the group consisting of O, SO, SO2, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB. X is at least one element selected from the group consisting of F, Cl, Br, I. 0.5≦a<6, 0 <b<2、0≦c≦6、0<d≦6.1)

[0051] In formula (2), A is an essential component and is at least one element selected from Li and Cs, preferably Li, or both Li and Cs, and more preferably Li.

[0052] In equation (2), a satisfies 0.5 ≤ a < 6, preferably 2.0 ≤ a ≤ 4.0, and more preferably 2.5 ≤ a ≤ 3.5. When a is 0.5 ≤ a < 6, the content of A in the halide-based solid electrolyte represented by equation (2) becomes appropriate, and the ionic conductivity of the solid electrolyte 11 becomes sufficiently high.

[0053] In formula (2), E is an essential component for improving the ionic conductivity of the solid electrolyte 11. In formula (2), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). E is preferably at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and La, more preferably containing Al and / or Zr, and most preferably being Zr.

[0054] In formula (2), b satisfies 0 < b < 2. b is preferably 0.6 ≤ b ≤ 1, because the effect of including E in improving the ionic conductivity of the solid electrolyte 11 becomes more pronounced.

[0055] In formula (2), G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , Si6O 18 , PO3, PO4, P2O7, P3O 10 , O, SO, SO2, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, or BOB, and is at least one group selected from the group consisting of these. G is preferably at least one group selected from the group consisting of O, SO, SO2, SO3, and SO4, and particularly preferably O and / or SO4.

[0056] In formula (2), c satisfies 0 ≤ c ≤ 6. When the halide-based solid electrolyte represented by formula (2) contains G (0 < c), the potential window on the reduction side of the solid electrolyte 11 is widened, making it less prone to reduction. c is preferably 0.5 ≤ c, because the effect of including G in widening the potential window on the reduction side becomes more pronounced. c is preferably c ≤ 3, to prevent a decrease in the ionic conductivity of the solid electrolyte caused by an excessively high G content.

[0057] In formula (2), X is an essential component for improving the ionic conductivity of the solid electrolyte 11. X in formula (2) is at least one selected from the group consisting of F, Cl, Br, and I, and preferably contains Br and / or Cl, because the effect of the positive electrode active material layer 1B containing particles 10 having a core-shell structure becomes more pronounced.

[0058] d in formula (2) satisfies 0<d≦6.1. d is preferably 1≦d. When d is 1≦d, the ionic conductivity of the solid electrolyte 11 becomes higher. Further, d is preferably d≦5 so that the potential window of the solid electrolyte 11 does not become narrow due to the excessive content of X.

[0059] Specific examples of the halide-based solid electrolyte represented by formula (2) include Li2ZrSO4Cl4 (LZSOC), Li2ZrCCl4 (LZOC), Li2ZrCl6 (LZC), Li2ZrBr6 (LZBr), Li2ZrBO2Cl5, Li2ZrBF4Cl5, Li3YSO4Cl4, Li3YCO3Cl4, Li3YBO2Cl5, Li3YBF4Cl5, and the like. Among these halide-based solid electrolytes, it is preferably any one selected from Li2ZrSO4Cl4 (LZSOC), Li2ZrCCl4 (LZOC), Li2ZrCl6 (LZC), and Li2ZrBr6 (LZBr), and most preferably Li2ZrSO4Cl4 (LZSOC). When the halide-based solid electrolyte is any one selected from Li2ZrSO4Cl4 (LZSOC), Li2ZrCCl4 (LZOC), Li2ZrCl6 (LZC), and Li2ZrBr6 (LZBr), a positive electrode active material layer 1B can be formed that is less likely to cause side reactions when left standing in an open circuit state, and can form an all-solid secondary battery 100 with further excellent self-discharge characteristics.

[0060] The solid electrolyte 11 contained in the positive electrode active material layer 1B of the present embodiment may be only one type, or may contain two or more types of solid electrolytes having different compositions. When the solid electrolyte 11 contains two or more types of solid electrolytes having different compositions, all may be halide-based solid electrolytes represented by formula (2), or together with the halide-based solid electrolyte represented by formula (2), may contain solid electrolytes used in known all-solid secondary batteries within a range where the effects of the present application can be obtained. The solid electrolyte 11 contained in the positive electrode active material layer 1B of the present embodiment may be the same as the solid electrolyte contained in the solid electrolyte layer 3 described later.

[0061] (Conductive auxiliary agent) The conductive additive 12 is not particularly limited as long as it improves the electronic conductivity within the positive electrode active material layer 1B, and known conductive additives can be used. The conductive additive 12 may be in the form of a powder or fibers. Examples of conductive additives 12 include carbon-based materials such as graphite, carbon black, graphene, and carbon nanotubes; metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron; conductive oxides such as ITO (indium tin oxide); or mixtures thereof. Among these, the conductive additive 12 is preferably a carbon-based material such as carbon nanotubes because it can improve the physical strength of the positive electrode active material layer 1B.

[0062] When the positive electrode active material layer 1B contains a sufficient amount of the conductive additive 12, the electronic conductivity within the positive electrode active material layer 1B becomes good. Furthermore, when generating particles 10 having a core-shell structure by performing the initial charge-discharge at a high temperature of 60°C to 85°C, the conductive additive 12 coats at least a portion of the surface of the particulate material made of lithium transition metal oxide represented by formula (1), thereby preventing the diffusion of halogen elements from the solid electrolyte 11 into the lithium transition metal oxide represented by formula (1). As a result, the generation of excess shell portion 10b is suppressed, and the ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the particles 10 having a core-shell structure becomes appropriate.

[0063] In this embodiment, when the positive electrode active material layer 1B contains a sufficient amount of particles 10 having a core-shell structure, the release and intercalation of ions (e.g., lithium ions), and the desorption and insertion of ions can be sufficiently performed. Furthermore, if the positive electrode active material layer 1B contains a sufficient amount of solid electrolyte 11 consisting of a halide-based solid electrolyte represented by formula (2), the ionic conductivity within the positive electrode active material layer 1B will be good. In addition, by performing the initial charge and discharge at a high temperature of 60°C to 85°C, a sufficiently large amount of halogen elements will diffuse from the solid electrolyte 11 when generating particles 10 having a core-shell structure, and the shell portion 10b will be sufficiently formed.

[0064] In this embodiment, the positive electrode active material layer 1B may contain, in addition to particles 10 having a core-shell structure, a solid electrolyte 11, and a conductive additive 12 which may be included as needed, a compound containing the same halogen element as the halogen element contained in the shell portion 10b of the particles 10 having a core-shell structure. Examples of halogen-containing compounds include sodium chloride and sodium bromide.

[0065] "Negative electrode layer" As shown in Figure 1, the negative electrode layer 2 comprises a negative electrode current collector 2A and a negative electrode active material layer 2B. The negative electrode active material layer 2B may be formed on only one side of the negative electrode current collector 2A, or on both sides of the negative electrode current collector 2A, as shown in Figure 1.

[0066] (Negative electrode current collector) The negative electrode current collector 2A is the same as the positive electrode current collector 1A. (Negative electrode active material layer) The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may also contain a conductive additive and a solid electrolyte.

[0067] (Negative electrode active material) The negative electrode active material is a compound capable of intercalating and releasing ions. The negative electrode active material is a compound exhibiting a lower potential than the positive electrode active material. Known materials can be used as the negative electrode active material, and the same material as the positive electrode active material may also be used. The negative electrode active material and positive electrode active material used in the all-solid-state secondary battery 100 are determined by considering the potentials of the negative electrode active material and the positive electrode active material.

[0068] (Conductive additive) The conductive additive improves the electronic conductivity of the negative electrode active material layer 2B. The conductive additive can be the same material used for the positive electrode active material layer 1B.

[0069] (solid electrolyte) The solid electrolyte contained in the negative electrode active material layer 2B improves the ionic conductivity within the negative electrode active material layer 2B. One or more known solid electrolytes can be used as a mixture. Examples of solid electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, and halide-based solid electrolytes. The same solid electrolyte 11 used in the positive electrode active material layer 1B described above may also be used as the solid electrolyte.

[0070] "Solid electrolyte layer" The solid electrolyte layer 3 can move ions by an externally applied electric field. One or more known solid electrolytes can be used as the solid electrolyte forming the solid electrolyte layer 3. Examples of solid electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, complex hydride-based solid electrolytes, and halide-based solid electrolytes. The solid electrolyte layer 3 preferably contains a halide-based solid electrolyte represented by formula (2), similar to the solid electrolyte 11 contained in the positive electrode active material layer 1B, and preferably contains Li2ZrSO4Cl4. This is because when the solid electrolyte layer 3 contains Li2ZrSO4Cl4, the reaction between the solid electrolyte layer 3 and the layer that becomes the positive electrode active material layer 1B proceeds more easily at the interface between the solid electrolyte layer 3 and the layer that becomes the positive electrode active material layer 1B when the initial charge and discharge is performed at a high temperature of 60°C to 85°C.

[0071] (Exterior) In the all-solid-state secondary battery 100 of this embodiment, the laminate 4 having a positive electrode layer 1, a solid electrolyte layer 3, and a negative electrode layer 2 is preferably housed in an outer casing (not shown) and sealed. The outer casing can be any known material that can prevent moisture and other elements from entering from the outside, and is not particularly limited. For example, as an outer casing, a metal laminate film, which is made by coating both sides of a metal foil with a polymer film, can be formed into a bag shape. Such an outer casing can be sealed by heat sealing the opening.

[0072] As the metal foil forming the metal laminate film, for example, aluminum foil or stainless steel foil can be used. As the polymer film placed on the outside of the outer casing, it is preferable to use a polymer with a high melting point, for example, polyethylene terephthalate (PET) or polyamide can be used. As the polymer film placed on the inside of the outer casing, for example, polyethylene (PE) or polypropylene (PP) can be used.

[0073] [Manufacturing method for all-solid-state rechargeable batteries] Next, a method for manufacturing the all-solid-state secondary battery 100 of this embodiment will be described. In this embodiment, we will explain using as an example the case in which particles 10 having a core-shell structure are produced, and the particles 10 have a shell portion 10b that contains the same halogen element as the halogen element contained in the solid electrolyte 11 of the positive electrode active material layer 1B.

[0074] The all-solid-state secondary battery 100 of this embodiment can be manufactured, for example, using a powder molding method. First, prepare a resin holder with a through hole in the center, a lower punch, and an upper punch. Furthermore, a powdered positive electrode mixture, which is the material for the positive electrode active material layer 1B, a powdered negative electrode mixture, which is the material for the negative electrode active material layer 2B, and a powdered solid electrolyte, which is the material for the solid electrolyte layer 3, are prepared separately.

[0075] In this embodiment, a mixed powder is prepared as the positive electrode mixture, comprising a powder (particles) made of a lithium transition metal oxide represented by formula (1), a powder of a solid electrolyte containing a halide-based solid electrolyte represented by formula (2), and a powder of a conductive additive as needed. The composition of the powder (particles) made of the lithium transition metal oxide represented by formula (1) corresponds to the composition of the core portion 10a. The composition of the powder of the solid electrolyte containing a halide-based solid electrolyte represented by formula (2) corresponds to the composition of the solid electrolyte 11.

[0076] Next, the lower punch is inserted from below the through-hole in the resin holder, and the powdered materials—the positive electrode mixture, the solid electrolyte, and the negative electrode mixture—are fed in that order from the opening side of the resin holder. Then, the upper punch is inserted on top of the fed powdered materials, and the press is placed on the press machine and pressed. The pressing pressure is, for example, 20 kPa. The powdered material placed in the resin holder is pressed by an upper punch and a lower punch within the resin holder. This results in a molded body in which the positive electrode active material layer 1B, the solid electrolyte layer 3, and the negative electrode active material layer 2B are laminated together.

[0077] Next, a positive electrode current collector 1A is placed on the positive electrode active material layer 1B of the molded body by a known method, and a negative electrode current collector 2A is placed below the negative electrode active material layer 2B. After the above procedure, a laminate 4 is obtained in which the positive electrode current collector 1A, positive electrode active material layer 1B, solid electrolyte layer 3, negative electrode active material layer 2B, and negative electrode current collector 2A are stacked in that order.

[0078] Next, external terminals are welded to the positive electrode current collector 1A of the positive electrode layer 1 and the negative electrode current collector 2A of the negative electrode layer 2, respectively, which form the laminate 4, by known methods, thereby electrically connecting the positive electrode current collector 1A or the negative electrode current collector 2A to the external terminals. After that, the laminate 4 connected to the external terminals is housed in an outer casing. The opening of the outer casing is then sealed by heat sealing to form an all-solid-state secondary battery structure.

[0079] In this embodiment, the all-solid-state secondary battery structure formed in this manner is subjected to its first charge and discharge at a high temperature of 60°C to 85°C. When the temperature during the first charge and discharge is 60°C or higher, oxygen released from the lithium transition metal oxide and halogen elements diffused from the halide-based solid electrolyte react at the interface between the powder (particles) made of lithium transition metal oxide represented by formula (1) and the powder of the solid electrolyte containing a halide-based solid electrolyte represented by formula (2). This generates particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b.

[0080] If the temperature during the initial charge and discharge is 60°C or lower, particles 10 having a core-shell structure will not be formed. The temperature during the initial charge and discharge is 60°C or higher, preferably 70°C or higher, and can be appropriately determined depending on the time required for charge and discharge. Furthermore, if the temperature during the initial charge and discharge is 85°C or lower, the oxygen released from the lithium transition metal oxide and the halogen elements diffused from the halide-based solid electrolyte will not react excessively, and particles 10 with a stable crystal structure in the core portion 10a can be obtained. Preferably, the temperature difference between the charging temperature and the discharging temperature during the initial charge-discharge cycle is 25°C or less.

[0081] Conventionally, charging and discharging of all-solid-state secondary battery structures has been performed at room temperature (in the range of 20°C to 30°C). Therefore, conventional manufacturing methods did not involve heating the all-solid-state secondary battery structure. Furthermore, since it is not necessary to heat the all-solid-state secondary battery structure for the initial charging and discharging, devices for heating the all-solid-state secondary battery structure, such as a constant-temperature bath, were unnecessary. Conventionally, the all-solid-state secondary battery structure sometimes generated heat during charging and discharging. However, even when the all-solid-state secondary battery structure generated heat, the temperature of the entire all-solid-state secondary battery structure did not exceed 60°C during the initial charging and discharging.

[0082] Other conditions for the all-solid-state secondary battery structure, such as current and voltage during the initial charge and discharge, can be known conditions and can be appropriately determined according to the application of the all-solid-state secondary battery 100 to be manufactured, within the range in which particles 10 having a core-shell structure are generated. For the initial charge and discharge of an all-solid-state secondary battery structure, the following methods can be used. The all-solid-state secondary battery structure is placed in a constant temperature bath at 60°C to 85°C and charged with a constant current at 0.01°C to 2.00°C until the battery voltage reaches 2.75V to 2.85V. Then, constant voltage charging is performed at that battery voltage for 0.5 hours to 8.0 hours. After that, constant current discharge is performed at 0.05°C until the battery voltage reaches 1.3V.

[0083] When the constant current charging conditions during the initial charge are changed, the ratio of the shell portion 10b area to the cross-sectional area of ​​the core-shell structure particle 10 changes. Specifically, when the constant current charging conditions during the initial charge are 0.02C or higher, particles 10 in which the shell portion 10b area ratio is 40% or less are more likely to be produced, and when they are 0.04C or higher, particles 10 in which the shell portion 10b area ratio is 30% or less are more likely to be produced. When the constant current charging conditions during the initial charge are 2.00C or lower, particles 10 in which the shell portion 10b area ratio is 1% or more are more likely to be produced, and when they are 0.50C or lower, particles 10 in which the shell portion 10b area ratio is 15% or more are more likely to be produced.

[0084] Furthermore, increasing the upper limit of the battery voltage during the initial charge tends to decrease the ratio of halogen element content at the interface 14 between the shell portion 10b and the solid electrolyte 11, and at the interface 13 between the shell portion 10b and the core portion 10a in the core-shell structured particle 10. Lowering the upper limit of the battery voltage during the initial charge tends to increase the ratio of halogen element content. When the upper limit of the battery voltage during the initial charge is within the range of 2.75V to 2.84V, particles 10 with a halogen element content ratio of 0.6 or more and less than 1.0 are more likely to be generated, and when it is within the range of 2.80V to 2.84V, particles 10 with a halogen element content ratio of 0.6 or more and 0.9 or less are more likely to be generated.

[0085] If the constant voltage charging time during the initial charge is increased, the average thickness of the shell portion 10b increases, and if the constant voltage charging time is shortened, the average thickness of the shell portion 10b decreases. If the constant voltage charging time during the initial charge is 1.0 hour or longer, particles 10 with an average thickness of 0.1 μm or more in the shell portion 10b are more likely to be generated, and if it is 3.0 hours or longer, particles 10 with an average thickness of 0.3 μm or more in the shell portion 10b are more likely to be generated. If the constant voltage charging time during the initial charge is 7.0 hours or less, particles 10 with an average thickness of 1.0 μm or less in the shell portion 10b are more likely to be generated, and if it is 6.0 hours or less, particles 10 with an average thickness of 0.8 μm or less in the shell portion 10b are more likely to be generated.

[0086] When the initial charge and discharge is performed at a high temperature as described above for the all-solid-state secondary battery structure, a reaction occurs between the lithium transition metal oxide represented by formula (1) and the halide-based solid electrolyte represented by formula (2) in the layer that becomes the positive electrode active material layer 1B. Then, a compound containing oxygen and halogen elements is formed along at least a portion of the surface of the particles made of the lithium transition metal oxide represented by formula (1), and particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b are generated. By following the above steps, an all-solid-state secondary battery 100 can be manufactured.

[0087] Next, we will explain using an example of generating particles 10 having a core-shell structure, which include a shell portion 10b containing a halogen element different from the halogen element contained in the solid electrolyte 11 of the positive electrode active material layer 1B. In this case, the all-solid-state secondary battery 100 can be manufactured in the same manner as described above, except that a mixed powder is used as the positive electrode compound, comprising a powder (particles) made of a lithium transition metal oxide represented by formula (1), a solid electrolyte powder containing a halide-based solid electrolyte represented by formula (2), a compound powder containing a halogen element to be included in the shell portion 10b, and a conductive additive powder as needed.

[0088] The above positive electrode mixture is preferably manufactured by mixing a powder (particles) made of a lithium transition metal oxide represented by formula (1) with a compound containing a halogen element to be included in the shell portion 10b to form a mixture, and then mixing the resulting mixture with a powder of a solid electrolyte containing a halide-based solid electrolyte represented by formula (2) and, if necessary, a powder of a conductive additive. This is because, in a positive electrode mixture manufactured by such a method, the contact area between the powder (particles) made of lithium transition metal oxide and the compound containing a halogen element to be included in the shell portion 10b is sufficiently larger than the contact area between the powder (particles) made of lithium transition metal oxide and the solid electrolyte. As a result, when the all-solid-state secondary battery structure manufactured using this positive electrode mixture undergoes its first charge and discharge at a high temperature as described above, the reaction between the powder (particles) made of lithium transition metal oxide and the compound containing a halogen element takes precedence over the reaction between the powder (particles) made of lithium transition metal oxide and the solid electrolyte.

[0089] As a compound containing a halogen element to be included in the shell portion 10b of the positive electrode mixture, a compound containing the same halogen element as the one contained in the shell portion 10b described above can be used.

[0090] When the all-solid-state secondary battery structure manufactured using the above positive electrode mixture undergoes its first charge and discharge at a high temperature as described above, the lithium transition metal oxide represented by formula (1) and the compound containing the halogen element to be included in the shell portion 10b preferentially react in the layer that becomes the positive electrode active material layer 1B. Then, a compound containing oxygen and the halogen element is formed along at least a portion of the surface of the particles made of the lithium transition metal oxide represented by formula (1), and particles 10 having a core-shell structure comprising a core portion 10a and a shell portion 10b are generated. By following the above steps, an all-solid-state secondary battery 100 can be manufactured.

[0091] The positive electrode active material layer 1B of this embodiment includes a positive electrode active material and a solid electrolyte 11. The positive electrode active material includes particles 10 having a core-shell structure, comprising a core portion 10a made of a lithium transition metal oxide represented by formula (1), and a shell portion 10b made of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I, covering at least a part of the surface of the core portion 10a. The solid electrolyte 11 includes a halide-based solid electrolyte represented by formula (2). Therefore, the shell portion 10b is arranged in a part between the core portion 10a and the solid electrolyte 11 of the particles 10 having a core-shell structure. The compound containing oxygen and a halogen element forming the shell portion 10b is electrochemically stable. As a result, in the all-solid-state secondary battery 100 having a positive electrode layer 1 equipped with the positive electrode active material layer 1B of this embodiment, the reaction between the core portion 10a and the solid electrolyte 11 is suppressed by the shell portion 10b, making it less likely for side reactions to occur when left standing in an open circuit state, and resulting in excellent self-discharge characteristics.

[0092] Although embodiments of the present invention have been described in detail above with reference to the drawings, the configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications to the configurations are possible without departing from the spirit of the present invention. [Examples]

[0093] "Example 1" (Preparation of positive electrode mixture) As a positive electrode mixture, the lithium transition metal oxide powder (particles) that will form the core as shown in Table 1, the solid electrolyte powder as shown in Table 1, and the graphite powder that will act as a conductive additive were prepared. These were weighed and mixed in a ratio of 50% by mass: 40% by mass: 10% by mass (lithium transition metal oxide: solid electrolyte: conductive additive).

[0094] (Preparation of negative electrode mixture) As a negative electrode mixture, lithium titanate powder, which is the negative electrode active material, solid electrolyte powder as shown in Table 1, and graphite powder, which is a conductive additive, were prepared and weighed out in the following proportions: 40% by mass: 50% by mass: 10% by mass (negative electrode active material: solid electrolyte: conductive additive), and then mixed.

[0095] (Fabrication of molded parts) A resin holder with a 12mm diameter through-hole in the center, and a lower punch and upper punch made of SKD11 material with a diameter of 11.99mm were prepared. The lower punch was inserted from below the through-hole of the resin holder, and the powdered materials, the positive electrode mixture, the solid electrolyte Li2ZrSO4Cl4 (LZSOC), and the negative electrode mixture, were added in that order from the opening side of the resin holder.

[0096] Next, an upper punch was inserted onto the powdered material that had been fed in, and the unit, which included the upper punch, a resin holder for containing the powdered material, and a lower punch, was placed in a press machine and pressed at a pressure of 20 kPa to produce a molded body. Next, a positive electrode current collector made of aluminum foil, with a diameter of 12 mm and a thickness of 15 μm, was placed on top of the positive electrode active material. In addition, a negative electrode current collector made of copper foil, with a diameter of 12 mm and a thickness of 9 μm, was placed below the negative electrode active material layer. Following the above procedure, a laminate 4 was obtained in which positive electrode current collector 1A, positive electrode active material layer 1B, solid electrolyte layer 3, negative electrode active material layer 2B, and negative electrode current collector 2A were stacked in that order.

[0097] Next, external terminals were welded to the positive electrode current collector 1A of the positive electrode layer 1 and the negative electrode current collector 2A of the negative electrode layer 2, respectively, using a known method, thereby electrically connecting the positive electrode current collector 1A or the negative electrode current collector 2A to the external terminals. Subsequently, the laminated body 4, connected to the external terminals, was housed in an outer casing made of aluminum laminate material. The opening of the outer casing was then sealed by heat sealing, creating an all-solid-state secondary battery structure.

[0098] Next, the all-solid-state secondary battery structure formed in this manner was subjected to its first charge and discharge using the method described below. The all-solid-state secondary battery structure was placed in a constant temperature bath at 60°C and charged with a constant current of 0.05C using a charge / discharge machine SD8 (manufactured by Hokuto Denko Co., Ltd.) until the battery voltage reached 2.80V. Subsequently, constant voltage charging at 2.8V was performed for 6.0 hours. The conditions for the initial charge are shown in Table 2. After that, constant current discharge was performed at 0.05C until the battery voltage reached 1.3V. By following the above steps, the all-solid-state secondary battery 100 of Example 1 was obtained.

[0099] [Table 1]

[0100] [Table 2]

[0101] The lithium transition metal oxides shown in Table 1 are as follows: (LCO); LiCoO2 (NCM);LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 (NCA);LiNi 0.85 Co 0.10 Al 0.05 O2

[0102] The solid electrolytes shown in Table 1 are as follows: (LZSOC);Li2ZrSO4Cl4 (LZOC);Li2ZrCCl4 (LZC);Li2ZrCl6 (LZBr);Li2ZrBr6 (LGPS); Li 10 GeP2S 12

[0103] Example 2 , Reference example 3 ~ Reference example 4" As shown in Table 2, the upper limit of the battery voltage during the initial charge is 2.84V in Example 2. Reference example 3 is 2.85V, Reference example Example 2 was constructed in the same manner as Example 1, except that 4 was set to 2.79V. , Reference example 3, Reference example A solid-state secondary battery 100 was obtained using method 4.

[0104] " Reference example 5. Reference example 6" Aside from the fact that the positive electrode mixture was prepared using the solid electrolyte shown in Table 1, Reference example In the same manner as in 4, Reference example 5. Reference example A solid-state secondary battery 100 was obtained using method 6.

[0105] " Reference example 7" Aside from the fact that the positive electrode mixture was prepared by mixing the lithium transition metal oxide powder (particles) that forms the core as shown in Table 1 with sodium chloride to make a mixture, and then mixing the solid electrolyte powder shown in Table 1 with graphite powder, which is a conductive additive, the positive electrode mixture was prepared by mixing these two components together. Reference example In the same manner as in 4, Reference example A total solid-state secondary battery 100 was obtained. The proportions of each component in the positive electrode mixture were 50% by mass: 40% by mass: 10% by mass (lithium transition metal oxide: solid electrolyte: conductive additive), and the proportion of sodium chloride was 2 parts by mass per 100 parts by mass of the total of lithium transition metal oxide, solid electrolyte and conductive additive.

[0106] " Reference example 8" Aside from the fact that the positive electrode mixture was prepared by mixing the lithium transition metal oxide powder (particles) that forms the core as shown in Table 1 with sodium bromide to make a mixture, and then mixing the solid electrolyte powder shown in Table 1 with graphite powder, which is a conductive additive, the positive electrode mixture was prepared by mixing these two components together. Reference example In the same manner as in 4, Reference example A total solid-state secondary battery 100 was obtained. The proportions of each component in the positive electrode mixture were 50% by mass: 40% by mass: 10% by mass (lithium transition metal oxide: solid electrolyte: conductive additive), and the proportion of sodium bromide was 2 parts by mass per 100 parts by mass of the total of lithium transition metal oxide, solid electrolyte and conductive additive.

[0107] " Reference example 9~ Reference example 13" The constant current charging conditions during the initial charge are as shown in Table 2: Reference example 9 is 1.00C, Reference example 10 is 0.80C. Reference example 11 is 0.10C, Reference example 12 is 0.02C, Reference exampleAside from setting 13 to 0.01C, Reference example As with 8, Reference example 9~ Reference example 13 all-solid-state secondary batteries 100 were obtained.

[0108] " Reference example 14~ Reference example 18" The constant voltage charging time during the initial charge is as shown in Table 2. Reference example 14 is 0.5 hours. Reference example 15 is 1.0 hour. Reference example 16 is 4.0 hours, Reference example 17 is 7.0 hours, Reference example Aside from setting 18 to 8.0 hours, Reference example As with 8, Reference example 14~ Reference example 18 all-solid-state secondary batteries 100 were obtained.

[0109] " Reference example 19 Except for setting the constant current charging conditions during the initial charge to 2.00C and the constant voltage charging time during the initial charge to 0.3 hours, as shown in Table 2, Reference example As with 8, Reference example 19 all-solid-state secondary batteries 100 were obtained.

[0110] " Reference example 20 Aside from the fact that the positive electrode mixture was prepared using the solid electrolyte shown in Table 1, Reference example As with 8, Reference example 20 all-solid-state secondary batteries 100 were obtained. " Reference example twenty one, Reference example twenty two" Aside from the fact that the positive electrode mixture was prepared using lithium transition metal oxides shown in Table 1, Reference example As with 8, Reference example twenty one, Reference example 22 all-solid-state secondary batteries 100 were obtained.

[0111] "Comparative Example 1" A comparative example 1 all-solid-state secondary battery 100 was obtained in the same manner as in Example 1, except that the temperature during the initial charging was set to 20°C, as shown in Table 1. "Comparative Example 2" Aside from the fact that the positive electrode mixture was prepared using the solid electrolyte shown in Table 1, Reference example In the same manner as in 7, an all-solid-state secondary battery 100 for Comparative Example 2 was obtained.

[0112] Example 1 obtained in this manner Example 2, Reference Example 3 ~ Reference example 22. For the all-solid-state secondary batteries of Comparative Example 1 and Comparative Example 2, the following were measured using the methods described below: "average particle size of the core," "halogen elements" contained in the shell of particles having a core-shell structure, "average thickness of the shell," "ratio of the shell area to the cross-sectional area of ​​particles having a core-shell structure," "ratio of halogen element content at the interface between the shell and the solid electrolyte and the interface between the shell and the core (interface with core / interface with solid electrolyte)," and "self-discharge characteristics (self-discharge)." The results are shown in Table 1.

[0113] "Average particle size of the core" The cross-section of the positive electrode active material layer 1B was observed at a magnification of 30kx using a scanning electron microscope (SEM) (product name: SU3800; manufactured by Hitachi High-Tech Corporation). The obtained image was converted into an 8-bit (256-level grayscale) black and white image using image analysis software (imageJ) to obtain a 256-level grayscale image of the core-shell structure particle 10. For the core-shell structure particle 10 in the obtained image, the lighter colored region (whitish region (average lightness of grayscale 193-207)) was designated as the core portion 10a, and the darker colored region (blackish region (average lightness of grayscale 174-187)) was designated as the shell portion 10b. For all core-shell structure particle 10 contained within a 100 μm x 100 μm square measurement area in the field of view, the diameter of the core portion 10a was measured, and the average value was taken as the average particle size of the core portion 10a.

[0114] "Halogen elements contained in the shell portion of particles having a core-shell structure" For particles 10 having an arbitrary core-shell structure in the cross-section of the positive electrode active material layer 1B, halogen element mapping analysis was performed using a scanning transmission electron microscope (STEM) energy-dispersive X-ray spectroscopy (EDS) system (product name: HD-2700; manufactured by Hitachi High-Tech Corporation) (measurement area: 3 μm x 3 μm square, measurement interval: 0.1 μm). This allowed for the identification of halogen elements in the shell portion 10b of the core-shell structured particles 10.

[0115] "Average thickness of the shell" A cross-section of the positive electrode active material layer 1B was observed at a magnification of 30kx using a scanning electron microscope (SEM) (product name: SU3800; manufactured by Hitachi High-Tech Corporation). The obtained image was converted into an 8-bit (256-level grayscale) black and white image using image analysis software (imageJ) to obtain a 256-level grayscale image of the particle 10 having a core-shell structure. For the particle 10 having a core-shell structure in the obtained image, the lighter colored region (whitish region (average lightness of grayscale 193-207)) was designated as the core portion 10a, and the darker colored region (blackish region (average lightness of grayscale 174-187)) was designated as the shell portion 10b. For any one particle 10 having a core-shell structure in the field of view, the thickness of the shell portion 10b along the diameter direction of the particle 10 was measured at five arbitrary locations, and the average value was taken as the average thickness of the shell portion 10b.

[0116] "The ratio of the shell area to the cross-sectional area of ​​a particle having a core-shell structure." A 256-level grayscale image of the core-shell structure particle 10 was obtained in the same manner as when the average thickness of the shell portion 10b was measured. For the core-shell structure particle 10 in the obtained image, the lighter colored areas were designated as the core portion 10a and the darker colored areas as the shell portion 10b, in the same manner as when the average thickness of the shell portion 10b was measured. Then, for any five core-shell structure particle 10 within the field of view, the area of ​​the core portion 10a and the area of ​​the shell portion 10b were determined. Using the obtained values, the ratio of the shell portion 10b to the cross-sectional area of ​​the core-shell structure particle 10 ({area of ​​shell portion 10b / (area of ​​core portion 10a + area of ​​shell portion 10b)} × 100 (%)) was calculated for each of the five core-shell structure particle 10, and the average value was taken as the ratio of the area of ​​the shell portion 10b to the cross-sectional area of ​​the core-shell structure particle 10.

[0117] "The ratio of halogen element content at the interface between the shell and the solid electrolyte, and at the interface between the shell and the core (interface with core / interface with solid electrolyte)." For particles 10 having any five core-shell structures in the cross-section of the positive electrode active material layer 1B, a scanning transmission electron microscope (STEM) energy-dispersive X-ray spectroscopy (EDS) system (product name: HD-2700; manufactured by Hitachi High-Tech Corporation) was used to perform a mapping analysis of halogen elements (measurement area: 3 μm x 3 μm square, measurement interval: 0.1 μm). For each of the five core-shell structures in the field of view, the ratio of halogen element content (interface between shell portion 10b and core portion 10a / interface between shell portion 10b and solid electrolyte 11) was calculated using the measurement value closest to the interface between the thickest shell portion 10b along the diameter direction of the particle 10 and the core portion 10a, and the measurement value closest to the interface with the solid electrolyte 11. The average value of this ratio was then calculated.

[0118] "Self-discharge characteristics (self-discharge)" For all-solid-state secondary batteries, a secondary battery charge / discharge test device (manufactured by Hokuto Denko Co., Ltd.) was used to charge the batteries at a constant current charge rate of 1.0C (the current value at which charging is completed in 1 hour when constant current charging is performed at 25°C) until the battery voltage reached 2.8V. After charging was complete, the voltage after being left at room temperature for 24 hours was defined as V1, and then the voltage after being left at a 40°C environment for 5 days was defined as V2. Using the obtained values ​​of V1 and V2, the self-discharge was calculated using the following equation (I). Self-discharge (mV / day)=V1-V2 (I)

[0119] As shown in Table 1, Example 1 Example 2, Reference Example 3 ~ Reference example The 22 all-solid-state secondary batteries exhibited suppressed self-discharge compared to the all-solid-state secondary batteries of Comparative Example 1 and Comparative Example 2. In particular, the all-solid-state secondary batteries of Examples 1 and 2, in which the ratio of halogen element content at the interface is 0.6 or more and less than 1.0, have a ratio of halogen element content at the interface of 0.5. Reference example 3. The ratio of halogen element content at the interface is 1.0. Reference example Compared to models 4-22, self-discharge was significantly suppressed.

[0120] Furthermore, the halogen element contained in the shell portion 10b is Cl. Reference example 4 is a case where the halogen element contained in the shell portion 10b is Br. Reference example Compared to version 8, self-discharge was significantly suppressed. Furthermore, the halogen elements in the shell portion 10b are the same as the halogen elements contained in the solid electrolyte 11 of the positive electrode active material layer 1B. Reference example 6 is different from the halogen elements contained in the solid electrolyte 11 of the positive electrode active material layer 1B. Reference example Compared to the 7, self-discharge was significantly suppressed.

[0121] Furthermore, the ratio of the shell portion 10b to the cross-sectional area of ​​the particle having a core-shell structure is 1% to 40%. Reference example In cases 10-12, the area ratio of the shell portion 10b is less than 1%. Reference example 9% and over 40% Reference example Compared to version 13, self-discharge was suppressed. Furthermore, the thickness of the shell portion 10b is 0.1 μm to 1.0 μm. Reference example In samples 15-17, the thickness of the shell portion 10b is less than 0.1 μm. Reference example 14. The thickness of the shell portion 10b is greater than 1.0 μm. Reference example Compared to version 18, self-discharge was suppressed. [Explanation of Symbols]

[0122] 1...Positive electrode layer, 1A...Positive electrode current collector, 1B...Positive electrode active material layer, 2...Negative electrode layer, 2A...Negative electrode current collector, 2B...Negative electrode active material layer, 3...Solid electrolyte layer, 4...Laminate, 10...Particles having a core-shell structure, 10a...Core part, 10b...Shell part, 11...Solid electrolyte, 12...Conductive additive, 100...All-solid-state secondary battery.

Claims

1. It comprises a positive electrode active material and a solid electrolyte, The positive electrode active material includes particles having a core-shell structure comprising a core portion and a shell portion covering at least a part of the surface of the core portion. The core portion is made of a lithium transition metal oxide represented by the following formula (1), The shell portion is made of a compound containing oxygen and at least one halogen element selected from the group consisting of F, Cl, Br, and I. The solid electrolyte includes a halide-based solid electrolyte represented by the following formula (2): A positive electrode active material layer in which the ratio of halogen element content at the interface between the shell portion and the solid electrolyte and the interface between the shell portion and the core portion is 0.6 or more and less than 1.

0. Li x MO y ・・・(1) (In equation (1), M is one or more transition metals. 0.1 < x < 1.1, 1.8 < y < 2.2) A a E b G c X d ・・・(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G represents OH, BO 2 , BO 3 , BO 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , PO 3 , PO 4 , P 2 O 7 , P 3 O 10 , O, SO, SO 2 , SO 3 , SO 4 , SO 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , BF 4 , PF 6 , and BOB. X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≤a<6, 0<b<2, 0≤c≤6, 0<d≤6.1)

2. The positive electrode active material layer according to claim 1, wherein the average thickness of the shell portion is 0.1 μm to 1.0 μm.

3. The positive electrode active material layer according to claim 1, wherein the ratio of the area of ​​the shell portion to the cross-sectional area of ​​the particles having the core-shell structure is 1% to 40%.

4. The positive electrode active material layer according to claim 1, wherein the halogen element contained in the shell portion and the halogen element contained in the solid electrolyte are the same element.

5. A positive electrode comprising a positive electrode active material layer according to any one of claims 1 to 4.

6. An all-solid-state secondary battery comprising the positive electrode, the negative electrode, and the solid electrolyte layer described in Claim 5.

7. The all-solid-state secondary battery according to claim 6, wherein the solid electrolyte layer includes a halide-based solid electrolyte represented by the following formula (2). A a E b G c X d ・・・(2) (In formula (2), A is at least one element selected from Li and Cs. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is OH, BO 2 , BO 3 , BO 4 , B 3 O 6 , B 4 O 7 , CO 3 , NO 3 , AlO 2 , SiO 3 , SiO 4 , Si 2 O 7 , Si 3 O 9 , Si 4 O 11 , Si 6 O 18 , PO 3 , PO 4 , P 2 O 7 , P 3 O 10 , O, SO, SO 2 , SO 3 , SO 4 , SO 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 , BF 4 , PF 6 , and BOB. X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5 ≤ a < 6, 0 < b < 2, 0 ≤ c ≤ 6, 0 < d ≤ 6.1)

8. The solid electrolyte layer is Li 2 ZrSO 4 Cl 4 The all-solid-state secondary battery according to claim 7, including the above.

Citation Information

Patent Citations

  • Anode active material and anode for all-solid-state battery containing the same

    JP7038951B2

  • Electrode material and battery

    WO2019146308A1

  • Coated positive electrode active material and battery using same

    WO2021199618A1

  • Positive electrode material, and battery

    WO2021220924A1

  • Positive electrode material and battery

    WO2021221001A1