toner
A toner formulation with crystalline vinyl resin and metal-complexed units addresses low-temperature fixing and heat resistance issues, ensuring stable electrostatic charging in varying humidity conditions.
Patent Information
- Application Number
- JP2022209748
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing toners struggle with low-temperature fixing performance, heat resistance, and electrostatic stability, particularly in varying humidity conditions, due to shell layer inhibition and unstable electrostatic properties.
A toner formulation containing crystalline vinyl resin, crystalline polyester, and wax components, with specific metal-complexed crystalline resin units, enhances crystallization and electrostatic stability, improving low-temperature fixability and heat-resistant storage.
The toner achieves improved low-temperature fixability, heat-resistant storage, and stable electrostatic charging across different humidity environments, reducing image defects.
Smart Images

Figure 0007955159000001 
Figure 0007955159000002 
Figure 0007955159000003
Abstract
Description
[Technical Field]
[0001] This disclosure relates to toner used in recording methods utilizing electrophotography, electrostatic recording, and toner jet recording. [Background technology]
[0002] In recent years, in electrophotography, energy conservation in various electrophotographic processes has been required to reduce power consumption. In laser beam printers, the thermal energy of the fuser unit accounts for a large proportion of the toner fixing process, and efforts are being made to lower the fuser temperature. Improving the low-temperature fixing properties of the toner is effective in lowering the fuser temperature. Furthermore, the toner is also required to have storage properties (heat resistance) to withstand high-temperature storage environments such as during transportation. To achieve both high low-temperature fixation and heat-resistant storage properties in toner, Patent Document 1 describes studies involving the addition of a large amount of crystalline organic material as a binder resin and coating it with an amorphous shell. Furthermore, Patent Document 2 describes studies to improve the electrostatic properties in low-temperature, low-humidity environments in toners containing a large amount of crystalline polyester resin. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2015-36723 [Patent Document 2] Japanese Patent Publication No. 2017-181576 [Patent Document 3] Japanese Patent Publication No. 2017-67925 [Overview of the project] [Problems that the invention aims to solve]
[0004] However, it has been found that toner coated with a shell layer, such as that described in Patent Document 1, cannot achieve the desired low-temperature fixing performance when fixed at a lower fixing temperature due to inhibition by the shell layer. On the other hand, adding large amounts of crystalline organic materials tends to worsen the electrostatic stability at low temperatures and low humidity, as well as at high temperatures and high humidity. However, in technologies such as those described in Patent Document 2, when attempting to control electrostatic properties using highly leaky additives such as surfactants, it has been found that it is difficult to maintain stable electrostatic properties over long periods, especially in high-temperature and high-humidity environments, when printing is repeated for extended periods (Patent Document 3 will be discussed later). Therefore, the present invention aims to provide a toner with improved low-temperature fixability, heat resistance for storage, and electrostatic stability in both low-temperature, low-humidity and high-temperature, high-humidity environments. [Means for solving the problem]
[0005] The present invention relates to a toner having toner particles containing a crystalline organic material, The crystalline organic material contains crystalline vinyl resin as an essential component, and further contains crystalline polyester and wax components as optional components. The total content of the crystalline vinyl resin, the crystalline polyester, and the wax component is 10.0% by mass or more and 90.0% by mass or less, based on the toner particles. The crystalline vinyl resin is (i) Unit A represented by formula (1), and (ii) Unit B represented by equation (2) It contains a crystalline resin A having the following characteristics: The toner particles contain a metal capable of forming a complex in the acetylacetonate portion of unit B of the crystalline resin A, in an amount of 0.0020% by mass or more and 0.0500% by mass or less, based on the mass of the toner particles. At least a portion of the unit B in the crystalline resin A forms a complex with the metal in the acetylacetonate portion. The present invention relates to a toner, wherein the content of the unit B in the crystalline resin A is from 0.50% by mass to 10.0% by mass.
[0006] [Chemical Formula] [In Formula (1), R1 represents a hydrogen atom or a methyl group, L1 represents a single bond, an ester bond, or an amide bond, and m represents an integer of 15 to 30.]
[0007] [Chemical Formula] [In Formula (2), R2 represents an alkylene group having 1 to 5 carbon atoms which may have a branched structure, L2 represents a single bond, an ester bond, or an amide bond, and R3 represents a hydrogen atom or a methyl group.] [Advantageous Effects of Invention]
[0008] According to the present invention, it is possible to obtain a toner having improved low-temperature fixability, heat-resistant storage stability, and charging stability in both low-temperature low-humidity and high-temperature high-humidity environments. [Description of Embodiments]
[0009] Hereinafter, the pigment dispersion and toner of the present invention will be specifically described.
[0010] [Features of the Present Invention] The toner of the present invention is a toner having toner particles containing a crystalline organic material, (I) the crystalline organic material contains a crystalline vinyl resin as an essential component, and further contains a crystalline polyester and a wax component as optional components, and the total content of the crystalline vinyl resin, the crystalline polyester, and the wax component is from 10.0% by mass to 90.0% by mass based on the toner particles, (II) the crystalline vinyl resin contains (i) a unit A represented by the following formula (1), and (ii) Unit B represented by the following formula (2) and a crystalline resin A having
[0011] [Chemical Formula] [In formula (1), R 1 represents a hydrogen atom or a methyl group, L1 represents a single bond, an ester bond, or an amide bond, and m represents an integer of 15 or more and 30 or less.]
[0012] [Chemical Formula] [In formula (2), R 2 represents an alkylene group having 1 to 5 carbon atoms which may have a branched structure, L2 represents a single bond, an ester bond, or an amide bond, and R 3 represents a hydrogen atom or a methyl group.]
[0013] (III) The toner particles contain a metal capable of forming a complex in the acetylacetonate moiety of the unit B contained in the crystalline resin A, in an amount of 0.0020 mass% or more and 0.0500 mass% or less based on the mass of the toner particles, and at least a part of the unit B in the crystalline resin A forms a complex with the metal in the acetylacetonate moiety, and (IV) in the crystalline resin A, the content of the unit B is 0.50 mass% or more and 10.0 mass% or less .
[0014] The toner of the present invention contains the aforementioned crystalline organic material, and by exhibiting sharp-melt thermal melting characteristics, the toner can improve low-temperature fixing performance. Generally, the crystallization state (crystallinity) of crystalline organic materials changes depending on the composition, manufacturing method, and whether or not thermal annealing is performed. If crystallization is insufficient, amorphous components tend to develop a low glass transition temperature (Tg), and the thermal stability of the toner over time (heat resistance) tends to deteriorate. One method to further increase crystallinity is to use a site that acts as a starting point for crystallization (nucleating site or nucleating agent) in combination with the crystalline organic material. The crystalline resin A of the present invention has unit A, which allows long-chain alkyl units to be arranged and crystallized. Furthermore, since at least a part of unit B has metal, it can promote the crystallization of unit A and thus act as a nucleating agent. A more detailed mechanism for this reason will be described below.
[0015] When at least a portion of unit B in crystalline resin A forms a complex with the metal in the acetylacetonate portion, the metal of one polymer chain acts as a driving force that facilitates proximity to the acetylacetonate portion of the other polymer chain through coordination bonding. As a result, both polymer chains become closer in the toner, and the units A incorporated into the same polymer chain also become more likely to crystallize. Therefore, it is expected that crystalline resin A itself will easily form aggregates (nuclei) of highly crystallized polymers in the toner. It is thought that this acts as a nucleating agent, promoting the crystallization of organic crystalline materials. Therefore, it is believed that the toner of the present invention has improved heat resistance and storage properties.
[0016] On the other hand, when Unit B of the present invention forms a complex with a metal, a moderate degree of leakiness is imparted. Therefore, significant charge-up can be suppressed, especially in low-temperature, low-humidity (LL) environments. Furthermore, since it does not contain acid-dissociable functional groups and can suppress moisture absorption, it can exhibit good charging properties in high-temperature, high-humidity (HH) environments. As a result, it is possible to exhibit stable charging properties in a variety of environments, from high-temperature, high-humidity (HH) to low-temperature, low-humidity (LL), thereby suppressing image defects.
[0017] It should be noted that controlling electrostatic properties by introducing a low-molecular-weight compound having an acetoacetoxy structure in Unit B and a metal into toner has been done in the past (for example, Patent Document 3). However, introducing a metal-coordinating site like Unit B into a crystalline material (crystalline resin A) like the present invention, and using them in combination with a metal as a nucleating agent to promote crystallization, is an effect that the manufacturer could not have anticipated.
[0018] [Regarding each component material of the present invention] The materials of the present invention will be described in detail below.
[0019] <Crystalline organic materials> In this invention, the term "crystalline" in expressions such as crystalline resins and crystalline organic materials refers to resins or organic materials that exhibit a clear endothermic peak (melting point) in differential scanning calorimeter (DSC) measurements.
[0020] The crystalline organic material in this invention is an organic compound having a high or low molecular weight melting point. The crystalline organic material in this invention may contain elements other than organic elements. When used as an electrophotographic toner, it is preferable to use one with a melting point of 250°C or lower from the viewpoint of adhesion to paper.
[0021] The crystalline organic material contains crystalline vinyl resin as an essential component, but may also contain crystalline polyester and wax components as optional components. When these components are present, low-temperature fixability tends to improve. In this invention, wax refers to a compound in the crystalline organic material having a weight-average molecular weight of 3000 or less.
[0022] The crystalline organic material of the present invention is characterized in that the total content of the crystalline vinyl resin, the crystalline polyester, and the wax component is 10.0% by mass or more and 90.0% by mass or less, based on the toner particles. When the content is 10.0% by mass or more, low-temperature fixability can be improved. When the content is 90.0% by mass or less, the decrease in heat-resistant storage, which is a problem of crystalline resins as described above, can be suppressed. More preferably, the content is 30.0% by mass or more and 70.0% by mass or less.
[0023] The crystalline organic material of the present invention may contain an ester wax as an optional wax component. Ester waxes generally have a plasticizing effect on amorphous resins. When ester wax is present, it is preferable to satisfy the following requirements in order to enhance the plasticizing effect during toner melting: that is, it contains an amorphous resin C, the amorphous resin C is a styrene-acrylic resin or a polyester resin, and the content of the ester wax in the crystalline organic material is preferably 70.0% by mass or more. Known materials can be used as the ester wax.
[0024] Ester waxes only need to have at least one ester bond in each molecule, and either natural or synthetic ester waxes may be used. There are no particular limitations on the ester wax, but examples include the following:
[0025] Esters of monohydric alcohols and monocarboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate; Esters of divalent carboxylic acids and monoalcohols, such as dibehenyl sebacate; Esters of dihydric alcohols such as ethylene glycol distearate and hexanediol dibehenate with monocarboxylic acids; Esters of trihydric alcohols such as glycerol tribehenate and monocarboxylic acids; Esters of tetrahydric alcohols such as pentaerythritol tetrastearate and pentaerythritol tetrapalmitate with monocarboxylic acids; Esters of hexahydritol alcohols such as dipentaerythritol hexastearate, dipentaerythritol hexapalmitate, and dipentaerythritol hexabéhenate with monocarboxylic acids; Esters of polyfunctional alcohols such as polyglycerin behenates and monocarboxylic acids; natural ester waxes such as carnauba wax and rice wax; Among these, ethylene glycol distearate is preferred from the viewpoint of plasticizing effect.
[0026] Another optional component in the crystalline organic material of the present invention, the crystalline polyester, can be obtained by polycondensation of a polycarboxylic acid and a polyhydric alcohol, and among these, polymers having a melting point can be used. For example, the following monomers can be used. Examples of polycarboxylic acids include the following compounds: dibasic acids such as succinic acid, adipic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, malonic acid, and dodecenylsuccinic acid, and their anhydrides or lower alkyl esters, as well as aliphatic unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, and citraconic acid.
[0027] Other examples include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, and their anhydrides or lower alkyl esters. These may be used individually or in combination of two or more.
[0028] Examples of polyhydric alcohols include the following compounds: alkylene glycols (ethylene glycol, 1,2-propylene glycol, and 1,3-propylene glycol); alkylene ether glycols (polyethylene glycol and polypropylene glycol); alicyclic diols (1,4-cyclohexanedimethanol); bisphenols (bisphenol A); and alkylene oxide (ethylene oxide and propylene oxide) adducts of alicyclic diols. The alkyl portions of alkylene glycols and alkylene ether glycols may be linear or branched.
[0029] Furthermore, examples include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. These may be used individually or in combination of two or more.
[0030] Furthermore, monohydric acids such as acetic acid and benzoic acid, and monohydric alcohols such as cyclohexanol and benzyl alcohol may be used as needed to adjust the acid value and hydroxyl value.
[0031] The method for producing the polyester resin is not particularly limited, but for example, the transesterification method or the direct polycondensation method can be used alone or in combination.
[0032] In the organic crystalline material of the present invention, hydrocarbon waxes may be used to improve mold release properties. In the toner, the content of the mold release agent in the toner particles is preferably 1.0% by mass or more and 30.0% by mass or less, more preferably 2.0% by mass or more and 25.0% by mass or less. Having the content of the mold release agent in the toner particles within the above range makes it easier to ensure mold release properties during fixing. The melting point of the mold release agent is preferably 60°C or more and 120°C or less. Having the melting point of the mold release agent within the above range makes it easier to melt during fixing and seep out onto the surface of the toner particles, thus making it easier to exhibit mold release properties. More preferably 70°C or more and 100°C or less. Examples of hydrocarbon waxes that can be used include aliphatic hydrocarbon waxes: low molecular weight polyethylene, low molecular weight polypropylene, low molecular weight olefin copolymer, Fischer-Tropsch wax, or waxes obtained by oxidation or acid addition of these.
[0033] Furthermore, in the crystalline organic material, as a crystalline vinyl resin, together with the crystalline resin A having the above characteristics, • The weight-average molecular weight (Mw) is between 5000 and 50000. The content of unit A represented by formula (1) above is 40.0% by mass or more and 90.0% by mass or less, • The content of Unit B is less than 0.50% by mass. It is preferable that the material contains 80.0% by mass or more of crystalline resin B that satisfies the following conditions. When these requirements are met, low-temperature fixability, heat resistance, and electrostatic stability in an HH environment can be improved.
[0034] When the weight-average molecular weight (Mw) of crystalline resin B is 5000 or more, the low molecular weight components make it easier to improve heat-resistant storage properties. When it is 50000 or less, it is easier to wet and spread during fixing, making it easier to improve low-temperature fixing properties. When the content of unit A in crystalline resin B is 40.0% by mass or more and 90.0% by mass or less, it is easier to achieve both low-temperature fixing and heat-resistant storage properties because the degree of crystallinity is maintained at a high level and the amount of crystals in the polymer is large. A unit A content of 60.0% by mass or more and 90.0% by mass or less is more preferable. When crystalline resin B contains 80% by mass or more of crystalline resin B with a unit B content of less than 0.50% by mass, hygroscopicity in an HH environment can be reduced and electrostatic stability can be improved.
[0035] (Crystalline resin A) The crystalline resin A of the present invention will be described further.
[0036] The crystalline resin vinyl resin of the present invention contains a crystalline resin A having (i) a unit A represented by formula (1) above, and (ii) a unit B represented by formula (2) above, wherein the toner particles contain a metal capable of forming a complex in the acetylacetonate portion of the unit B of the crystalline resin A in an amount of 0.0020% by mass or more and 0.0500% by mass or less, based on the mass of the toner particles, wherein at least a portion of the unit B in the crystalline resin A forms a complex with the metal in the acetylacetonate portion, and the content of the unit B in the crystalline resin A is 0.50% by mass or more and 10.0% by mass or less.
[0037] As mentioned above, meeting these requirements improves heat resistance and electrostatic stability.
[0038] "Unit B": When the content of unit B in crystalline resin A is 0.50% by mass or more, the effects described above are easily obtained, and heat resistance and electrostatic stability can be improved. When it is 10.0% by mass or less, hygroscopicity in an HH environment can be suppressed, so electrostatic stability is easily improved.
[0039] In this case, the acetylacetonate moiety in unit B exhibits keto-enol tautomerism and can form complexes with metals, for example, as shown in formula (3).
[0040] [ka] (In equation (3), M represents a metallic element.)
[0041] One method for introducing unit B into crystalline resin A is by copolymerizing the following monomers.
[0042] Examples include acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, acetoacetoxybutyl (meth)acrylate, 2-[(1-oxo-2-propen-1-yl)amino]ethyl 3-oxobutanoate, and 4-[(1-oxo-2-propen-1-yl)amino]butyl 3-oxobutanoate.
[0043] In formula (2) of unit B, when R2 has 1 to 5 carbon atoms, the nucleation effect is easily exhibited because of its close proximity to the polymer main chain. More preferably, the number of carbon atoms is 2 to 4.
[0044] When L2 is an ester bond, it is preferable because the electrostatic stability in an HH environment is easily improved.
[0045] "Unit A": On the other hand, it is preferable that the content of unit A in the crystalline resin A is 40.0% by mass or more and 90.0% by mass or less. When it is 40.0% by mass or more, the crystallinity tends to be high, so the heat resistance to storage tends to improve. When it is 90.0% by mass or less, the nucleation sites in the toner particles tend to be finer, so this also tends to improve the heat resistance to storage. More preferably, it is 60.0% by mass or more and 80.0% by mass or less.
[0046] In formula (1) of unit A, when m is between 15 and 30, it indicates the presence of a long-chain alkyl group, which makes the resin more likely to exhibit crystallinity. A more preferable value for m is between 17 and 23, and more preferably between 19 and 23.
[0047] One method for introducing unit A into crystalline resin A is to polymerize the following (meth)acrylic acid esters. For example, (meth)acrylic acid esters having a linear alkyl group with 16 to 36 carbon atoms [stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myricyl (meth)acrylate, dotriacontyl (meth)acrylate, etc.] and (meth)acrylic acid esters having a branched alkyl group with 18 to 36 carbon atoms [2-decyltetradecyl (meth)acrylate, etc.]. The monomers forming unit A may be used individually or in combination of two or more.
[0048] "Other Units": The crystalline resin A may be copolymerized with monomers capable of forming units A and B, as well as other monomers capable of forming the units shown below.
[0049] (Meth)acrylic acid esters such as styrene, α-methylstyrene, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0050] Monomers having a urea group: For example, monomers obtained by reacting the following amines having 3 to 22 carbon atoms [primary amines (n-butylamine, t-butylamine, propylamine, and isopropylamine, etc.), secondary amines (di-normal ethylamine, di-normal propylamine, di-normal butylamine, etc.), aniline, and cycloxylamine, etc.] with isocyanates having 2 to 30 carbon atoms and having an ethylenically unsaturated bond, by known methods.
[0051] Monomers having a carboxyl group; for example, methacrylic acid, acrylic acid, and 2-carboxyethyl (meth)acrylate.
[0052] Monomers having a hydroxyl group; for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.
[0053] Monomers having an amide group; for example, acrylamide, monomers obtained by reacting an amine having 1 to 30 carbon atoms with a carboxylic acid having 2 to 30 carbon atoms having an ethylenically unsaturated bond (such as acrylic acid and methacrylic acid) by known methods.
[0054] Monomers having a nitrile group; for example, acrylonitrile, methacrylonitrile.
[0055] In particular, it is preferable to use styrene, methacrylic acid, acrylic acid, methyl (meth)acrylate, t-butyl (meth)acrylate, acrylonitrile, and methacrylonitrile.
[0056] "Physical properties of crystalline resin A": The crystalline resin A preferably has a melting point of 55.0°C or higher and 70.0°C or lower.
[0057] If the melting point is 70.0°C or lower, it melts at a lower temperature, which easily improves low-temperature fixability. If it is 55.0°C or higher, it easily improves heat resistance for storage. More preferably, it is between 58.0°C and 68.0°C. The melting point of crystalline resin A can be controlled by changing the amount of unit A or the number of carbon atoms in m within unit A.
[0058] The crystalline resin A preferably has an acid value (Av) and a hydroxyl value (OHv) of 5.0 mgKOH / g or less. When the values are 5.0 mgKOH / g or less, hygroscopicity can be suppressed in an HH environment, thus improving electrostatic stability. One method for controlling the acid value is copolymerizing a polymer having an acid group, such as acrylic acid. Another method for controlling the hydroxyl value is copolymerizing a monomer having a hydroxyl group, such as 2-hydroxyethyl methacrylate.
[0059] The content of the crystalline resin A in the crystalline organic material is preferably 1.0% by mass or more and 70.0% by mass or less. When it is 1.0% by mass or more, the effect as a nucleating agent is easily obtained. When it is 70.0% by mass or less, leakage in an HH environment is easily suppressed, and thus the electrostatic stability is easily improved. More preferably it is 5.0% by mass or more and 30.0% by mass or less.
[0060] From the viewpoint of achieving both low-temperature fixability and heat-resistant storage, the weight-average molecular weight (Mw) of the THF-soluble component of the crystalline resin A is preferably 10,000 or more and 50,000 or less.
[0061] For obtaining the crystalline vinyl resin of the present invention, known polymerization initiators can be used.
[0062] Examples of azo or diazo polymerization initiators include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitride), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile; and peroxide polymerization initiators such as benzoyl peroxide, t-butyl peroxy 2-ethylhexanoate, t-butyl peroxypivalate, t-butyl peroxyisobutyrate, t-butyl peroxyneodecanoate, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumenehydroperoxide, 2,4-dichlorobenzoyl peroxide, and lauroyl peroxide. Known chain transfer agents and polymerization inhibitors may also be used.
[0063] "Metals capable of forming complexes with Unit B": Regarding the metal capable of forming a complex in the acetylacetonate portion of unit B of the crystalline resin A described above, when its content is 0.0020% by mass or more, based on the mass of the toner particles, the complex formation efficiency is improved, which tends to improve heat resistance and electrostatic stability in an LL environment. When it is 0.0500% by mass or less, charge leakage in an HH environment can be suppressed, which tends to improve electrostatic stability in an HH environment. A metal content of 0.0100% by mass or more and 0.0400% by mass or less is more preferable.
[0064] The metal bonded to unit B can be any metal capable of coordinating with unit B, but it is preferable that the metal is one of Al, Zn, Fe, Cu, Co, Ni, Ti, Mg, or Mn. Using these metals enhances the effect as a nucleating agent and improves heat resistance during storage. More preferably, it is Al, Zn, Fe, Co, Ti, Mg, or Mn, and even more preferably aluminum. Unit B may form any complex with these metals. The metal compound used to introduce these metals into the toner can be in any form, but it is preferable to use an oil-soluble metal compound for more effective introduction into the toner. An example of an oil-soluble metal compound that can be used is the metal compound represented by formula (4).
[0065] [ka] (In equation (4), M represents a metallic element, x is an integer between 2 and 17 (inclusive), and n is an integer between 1 and 3 (inclusive).)
[0066] Specific examples of metal compounds represented by formula (4) above include aluminum laurate (M=Al, x=10, n=3), aluminum distearate (M=Al, x=16, n=2), cobalt distearate (M=Co, x=16, n=2), magnesium distearate (M=Mg, x=16, n=2), and iron tristearate (M=Fe, x=16, n=3).
[0067] <Coloring agent> The toner may contain a colorant. Examples of colorants include known organic pigments, organic dyes, inorganic pigments, and carbon black as a black colorant. Other colorants conventionally used in toners may also be used.
[0068] Examples of yellow colorants include: condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specifically, CI Pigment Yellows 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 150, 155, 168, and 180 are preferably used.
[0069] Examples of magenta colorants include: condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolon compounds, thioindigo compounds, and perylene compounds. Specifically, CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 236, and 254 are preferably used.
[0070] Examples of cyanide colorants include: copper phthalocyanine compounds and their derivatives, anthraquinone compounds, and basic dye lake compounds. Specifically, CI pigment blues 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66 are preferably used.
[0071] The colorants are selected based on their hue angle, saturation, brightness, lightfastness, and dispersibility in the toner.
[0072] The colorant content is preferably 3.0% by mass or more and 20.0% by mass or less in the toner particles.
[0073] <External additives> The toner particles can be used as is as toner, or, if necessary, external additives can be mixed in and attached to the surface of the toner particles to create toner.
[0074] Examples of external additives include inorganic fine particles selected from the group consisting of silica fine particles, alumina fine particles, and titania fine particles, or composite oxides thereof. Examples of composite oxides include silica-aluminum fine particles and strontium titanate fine particles.
[0075] The content of the external additive is preferably 0.01 parts by mass or more and 8.0 parts by mass or less per 100 parts by mass of toner particles, and more preferably 0.1 parts by mass or more and 4.0 parts by mass or less.
[0076] <Toner manufacturing method> Toner particles may be manufactured by any known method, such as suspension polymerization, emulsification and agglutination, dissolution and suspension, or pulverization, as long as they are within the scope of the present configuration, but are preferably manufactured by suspension polymerization.
[0077] I will now describe the suspension polymerization method in detail.
[0078] For example, a polymerizable monomer composition is prepared by mixing crystalline resin A, optionally crystalline resin B, crystalline polyester, wax, amorphous resin C or polymerizable monomers that produce amorphous resin C, colorants, release agents, charge control agents, and other materials, and uniformly dissolving or dispersing them.
[0079] Subsequently, the polymerizable monomer composition is dispersed in an aqueous medium using a stirrer or the like to prepare suspended particles of the polymerizable monomer composition. Then, toner particles are obtained by polymerizing the polymerizable monomers contained in the particles with an initiator or the like.
[0080] After polymerization is complete, the toner particles should be filtered, washed, and dried by known methods, and external additives may be added as needed to obtain toner.
[0081] As the polymerization initiator, the same type of polymerization initiator used to obtain the aforementioned crystalline vinyl resin can be used. Alternatively, known chain transfer agents and polymerization inhibitors may also be used.
[0082] The aqueous medium may contain an inorganic or organic dispersion stabilizer. Known dispersion stabilizers can be used as the dispersion stabilizer.
[0083] Examples of inorganic dispersion stabilizers include phosphates such as hydroxyapatite, tricalcium phosphate, dicalcium phosphate, magnesium phosphate, aluminum phosphate, and zinc phosphate; carbonates such as calcium carbonate and magnesium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide; sulfates such as calcium sulfate and barium sulfate; calcium metasilicate; bentonite; silica; and alumina.
[0084] Examples of organic dispersion stabilizers include polyvinyl alcohol, gelatin, methylcellulose, methylhydroxypropylcellulose, ethylcellulose, sodium salts of carboxymethylcellulose, polyacrylic acid and its salts, and starch.
[0085] When using inorganic compounds as dispersion stabilizers, commercially available compounds may be used as is, but to obtain finer particles, the inorganic compounds may be generated in an aqueous medium before use. For example, in the case of calcium phosphate such as hydroxyapatite or tricalcium phosphate, it is preferable to mix the aqueous phosphate solution with the aqueous calcium salt solution under high stirring.
[0086] The aqueous medium may contain a surfactant. Known surfactants can be used as the surfactant. Examples include anionic surfactants such as sodium dodecylbenzene sulfate and sodium oleate; cationic surfactants; amphoteric surfactants; and nonionic surfactants.
[0087] On the other hand, the method for producing toner by pulverization is not particularly limited, but preferably includes a step of melting and kneading raw materials containing crystalline resin A, amorphous resin C, and optionally a colorant, a mold release agent, etc., and a step of pulverizing the resulting melted mixture to obtain toner particles. Known equipment can be used for melting and kneading and pulverization.
[0088] [Methods for Measuring Physical Properties] Hereinafter, methods for measuring various physical properties of the toner will be described.
[0089] <Method for Measuring Weight Average Particle Diameter (D4) of Toner Particles and Toner> The weight average particle diameter (D4) of the toner particles and the toner is measured using a precision particle size distribution measuring device "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.). The measurement is performed under the following conditions. Effective measurement channel count: 25,000 channels Total control motor count: 50,000 Aperture: 100 μm Current: 1600 μA Gain: 2 The Kd value is measured using a value obtained with "standard particle 10.0 μm" (manufactured by Beckman Coulter, Inc.). The measurement data is analyzed using dedicated software included with the device to calculate the weight average particle diameter (D4). When the graph / volume % is set using the aforementioned dedicated software, the "average diameter" on the "analysis / volume statistical value (arithmetic mean)" screen is the weight average particle diameter (D4).
[0090] <Method for Measuring Molecular Weight (Mw) of THF Soluble Fraction> The molecular weight (weight average molecular weight Mw) of the THF soluble fraction of the toner is measured by gel permeation chromatography (GPC) as follows.
[0091] First, the toner is dissolved in tetrahydrofuran (THF) at 50° C. over 2 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Maishori Disc" (manufactured by Tosoh Corporation) with a pore diameter of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is 0.8 mass %. Using this sample solution, measurement is performed under the following conditions.
[0092] · Device: HLC8120 GPC (detector: RI) (manufactured by Tosoh Corporation) • Columns: Shodex KF-801, 802, 803, 804, 805, 806, 807 (7 columns, manufactured by Showa Denko) • Eluent: Tetrahydrofuran (THF) ·Flow rate: 1.0ml / min Oven temperature: 40.0℃ • Sample injection volume: 0.10 ml To calculate the molecular weight of the sample, a molecular weight calibration curve created using standard polystyrene resin (for example, "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.
[0093] <Method for separating crystalline resin A and crystalline polyester from toner> The separation of crystalline resin A and crystalline polyester from toner can be done by known methods, and one example is shown below.
[0094] Gradient LC is used as a method for separating resin components from toner. This analysis allows for separation based on the polarity of the resin in the binder resin, regardless of molecular weight.
[0095] First, the toner was dissolved in chloroform. The sample was adjusted to a sample concentration of 0.1% by mass using chloroform, and the solution was filtered through a 0.45 μm PTFE filter before being used for measurement. The measurement conditions for gradient polymer LC are shown below.
[0096] Equipment: UlTIMATE3000 (manufactured by Thermo Fisher Scientific) Mobile phase: A. Chloroform (HPLC), B. Acetonitrile (HPLC) Gradient: 2 min (A / B=0 / 100) → 25 min (A / B=100 / 0) (Note that the gradient of the mobile phase change was made to be a straight line.) Flow rate: 1.0mL / min Injection: 0.1% by mass x 20μL Column: Tosoh TSKgel ODS (4.6mmφ x 150mm x 5μm) Column temperature: 40℃ Detector: Corona Charged Particle Detector (Corona-CAD) (manufactured by Thermo Fisher Scientific) For the time-intensity graph obtained from the measurement, the peak detection position is identified, and when repeating the measurement, the peak position is fractionated using a fraction collector or similar device. DSC measurement is performed on the fractionated resins, and the resins with melting point peaks are designated as crystalline resin A and crystalline polyester. NMR measurement is performed on the fractionated resins with melting points to identify the resin species.
[0097] <Method for separating wax from toner> If the toner contains wax, it is necessary to separate the release agent from the toner. The release agent is separated by recycled HPLC, which separates components with a molecular weight of 3000 or less as release agents. The measurement method is as follows. First, a chloroform solution of the toner is prepared using the method described above. Then, the obtained solution is filtered through a solvent-resistant membrane filter "Myshoridisk" (manufactured by Tosoh Corporation) with a pore diameter of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in chloroform is 1.0% by mass. This sample solution is used for measurement under the following conditions.
[0098] ·Equipment: LC-Sakura NEXT (manufactured by Nippon Analytical Industry Co., Ltd.) • Columns: JAIGEL2H, 4H (manufactured by Nippon Analytical Engineering Co., Ltd.) • Eluent: Chloroform ·Flow rate: 10.0ml / min Oven temperature: 40.0℃ • Sample injection volume: 1.0 ml To calculate the molecular weight of the sample, a molecular weight calibration curve created using standard polystyrene resin (for example, "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.
[0099] From the molecular weight curve obtained in this way, components with a molecular weight of 3000 or less were separated. The DSC of the obtained components was measured, and those with a melting point were designated as wax.
[0100] <Method for measuring the melting point of crystalline resin A> The melting point of crystalline resin A is measured using a DSC Q2000 (manufactured by TA Instruments) under the following conditions. Heating rate: 10℃ / min Measurement start temperature: 20℃ Measurement end temperature: 180℃ The temperature correction for the device's detection unit uses the melting points of indium and zinc, while the heat of fusion of indium is used for heat quantity correction.
[0101] Specifically, 5 mg of the sample is accurately weighed, placed in an aluminum pan, and differential scanning calorimetry is performed. An empty silver pan is used as a reference. The heating process involves raising the temperature to 180°C at a rate of 10°C / min. Then, the peak temperature is calculated from each peak and used as the melting point.
[0102] <Method for identifying resin types and quantifying the content ratios of Unit A and Unit B> The measurement of the content ratio of various monomer units in the resin is performed as follows: 1 The procedure is performed using H-NMR under the following conditions.
[0103] Measuring device: FT NMR device JNM-EX400 (manufactured by JEOL Ltd.) Measurement frequency: 400MHz Pulse condition: 5.0 μs Frequency range: 10500Hz Total number of times: 64 Measurement temperature: 30°C Sample: Prepared by placing 50 mg of the measurement sample into a sample tube with an inner diameter of 5 mm, adding deuterated chloroform (CDCl₃) as a solvent, and dissolving the mixture in a constant temperature bath at 40°C. The obtained 1 H-NMR chart is analyzed to identify the structure of each monomer unit. Here, as an example, the measurement of the content ratios of unit A and unit B in the crystalline resin A is described. The obtained 1 In the H-NMR chart, a peak independent of peaks attributed to components of other monomer units is selected from peaks attributed to components of unit A and unit B, and the integrated value S₁ of this peak is calculated. Integrated values are similarly calculated for other monomer units contained in the crystalline resin A.
[0104] When a polymerizable monomer whose components other than the vinyl group do not contain hydrogen atoms is used, 13 the measurement nucleus is set to 13 C using C-NMR, measurement is performed in single pulse mode, and the value is calculated in the same manner as in 1 H-NMR. The proportion (mol%) of each monomer unit calculated by the above method is multiplied by the molecular weight of each monomer unit to convert the content ratio of each monomer unit into mass %.
[0105] <Method for Quantifying Metal Content in Toner Particles> The metal content in the toner is measured by fluorescent X-ray analysis and determined using a calibration curve method. Fluorescent X-ray measurement conforms to JIS K 0119-1969, and the specific procedure is as follows.
[0106] The measurement equipment used will be the wavelength-dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and its accompanying software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh will be used as the anode of the X-ray tube, the measurement atmosphere will be vacuum, and the measurement diameter (collimator mask diameter) will be 27 mm. A proportional counter (PC) will be used for measuring light elements, and a scintillation counter (SC) will be used for measuring heavy elements. During measurement, the acceleration voltage and current values of the X-ray generator will be set to 24 kV and 100 mA, respectively.
[0107] First, pellets are prepared to create a calibration curve for determining the metal content in the toner. Binder [Product name: Spectro Blend, Composition: C 81.0, O 2.9, H 13.5, N 2.6 (mass%), Chemical formula: C 19 H 38 [ON, Shape: Powder (44 μm); Manufactured by Rigaku Corporation] Add 1.0 ppm of a metal compound with a known metal content to 100 parts by mass. Mix thoroughly using a coffee mill, then place 4 g into a dedicated aluminum ring for pressing and flatten it. Then, using a tablet molding compressor "BRE-32" (manufactured by Maekawa Testing Machinery Co., Ltd.), pressurize at 20 MPa for 60 seconds to prepare pellets with a thickness of 2 mm and a diameter of 39 mm. Similarly, prepare mixtures and pellets with known metal compounds at 10.0 ppm, 50.0 ppm, 200.0 ppm, and 500.0 ppm by mass.
[0108] A linear calibration curve is obtained by plotting the resulting X-ray count rate on the vertical axis and the aluminum concentration calculated from the amount of aluminum hydroxide added to each calibration sample on the horizontal axis.
[0109] Toner particles were measured under similar tableting and measurement conditions, and the metallic elements were quantified based on the created calibration curve.
[0110] <Method for identifying the metal that complexes with the acetylacetonate moiety of Unit B> In the above method for isolating crystalline resin A, the isolated crystalline resin A is recovered and measured using the same method as the above method for quantifying the amount of metal in toner particles to identify the type of metal.
[0111] <Method for measuring the acid value of resins> The acid value is the weight (mg) of potassium hydroxide required to neutralize the acid contained in 1 g of the sample. The acid value of resin A in this invention is measured in accordance with JIS K 0070-1992, and specifically, it is measured according to the following procedure.
[0112] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), add deionized water to make a total volume of 100 mL, and obtain a phenolphthalein solution.
[0113] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water and add ethyl alcohol (95 vol%) to make 1 L. Place the solution in an alkali-resistant container, taking care not to allow it to come into contact with carbon dioxide, etc., and leave it for 3 days. After that, filter the solution to obtain potassium hydroxide solution. Store the obtained potassium hydroxide solution in an alkali-resistant container. The factor of the above potassium hydroxide solution is determined by taking 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of the above phenolphthalein solution, titrating with the above potassium hydroxide solution, and determining the amount of potassium hydroxide solution required for neutralization. The above 0.1 mol / L hydrochloric acid should be prepared in accordance with JIS K 8001-1998.
[0114] (2) Operation (A) Main examination 2.0 g of melt-kneaded and pulverized toner sample is accurately weighed into a 200 mL Erlenmeyer flask, and 100 mL of a toluene / ethanol (2:1) mixture is added. The mixture is dissolved over 5 hours. Then, a few drops of the phenolphthalein solution are added as an indicator, and the sample is titrated with the potassium hydroxide solution. The endpoint of the titration is when the indicator turns a pale pink color for 30 seconds. (B) Blank test The titration procedure is the same as described above, except that no sample is used (i.e., only a mixed solution of toluene / ethanol (2:1) is used).
[0115] (3) Substitute the obtained results into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A: acid value (mgKOH / g), B: amount of potassium hydroxide solution added in the blank test (mL), C: amount of potassium hydroxide solution added in the main test (mL), f: factor of the potassium hydroxide solution, and S: sample (g).
[0116] [Method for measuring hydroxyl value] The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl groups when acetylating 1 g of a sample. The hydroxyl value of the binder resin is measured according to JIS K 0070-1992, and specifically, it is measured according to the following procedure.
[0117] (1) Preparation of reagents Place 25g of special grade acetic anhydride into a 100ml volumetric flask, add pyridine to bring the total volume to 100ml, and shake thoroughly to obtain the acetylation reagent. Store the obtained acetylation reagent in a brown bottle, keeping it away from moisture, carbon dioxide, etc.
[0118] Dissolve 1.0 g of phenolphthalein in 90 ml of ethyl alcohol (95 vol%), add deionized water to make a total volume of 100 ml, and obtain a phenolphthalein solution.
[0119] Dissolve 35 g of special grade potassium hydroxide in 20 ml of water and add ethyl alcohol (95 vol%) to make 1 liter. Place the solution in an alkali-resistant container, taking care not to allow contact with carbon dioxide, etc., and leave it for 3 days. After filtration, obtain the potassium hydroxide solution. Store the obtained potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is determined by taking 25 ml of 0.5 mol / l hydrochloric acid in an Erlenmeyer flask, adding a few drops of the phenolphthalein solution, titrating with the potassium hydroxide solution, and determining the amount of potassium hydroxide solution required for neutralization. The 0.5 mol / l hydrochloric acid used is prepared in accordance with JIS K 8001-1998.
[0120] (2) Operation (A) Main examination Accurately weigh 1.0 g of the sample into a 200 ml round-bottom flask, and precisely add 5.0 ml of the acetylation reagent to it using a volumetric pipette. If the sample is difficult to dissolve in the acetylation reagent, add a small amount of special grade toluene to dissolve it.
[0121] Place a small funnel over the mouth of the flask and immerse about 1 cm of the bottom of the flask in a glycerin bath at approximately 97°C and heat. At this time, it is preferable to cover the base of the flask's neck with a piece of cardboard with a round hole cut out to prevent the temperature of the flask's neck from rising due to the heat of the bath.
[0122] After 1 hour, remove the flask from the glycerin bath and allow it to cool. After cooling, add 1 ml of water from the funnel and shake to hydrolyze the acetic anhydride. To further complete hydrolysis, heat the flask again in the glycerin bath for 10 minutes. After cooling, wash the funnel and the walls of the flask with 5 ml of ethyl alcohol.
[0123] Add a few drops of the phenolphthalein solution as an indicator, and titrate with the potassium hydroxide solution. The titration endpoint is reached when the indicator remains faintly pink for approximately 30 seconds. (B) Blank test Perform the titration in the same manner as described above, except that no sample is used.
[0124] (3) Substitute the obtained results into the following formula to calculate the hydroxyl value. A = [{(BC) × 28.05 × f} / S] + D Here, A: hydroxyl value (mgKOH / g), B: amount of potassium hydroxide solution added in the blank test (ml), C: amount of potassium hydroxide solution added in the main test (ml), f: factor of the potassium hydroxide solution, S: sample (g), D: acid value of the sample (mgKOH / g).
[0125] [Configurations included in embodiments of the present invention] This embodiment includes the following configuration. (Configuration 1) A toner having toner particles containing a crystalline organic material, The crystalline organic material contains crystalline vinyl resin as an essential component, and further contains crystalline polyester and wax components as optional components. The total content of the crystalline vinyl resin, the crystalline polyester, and the wax component is 10.0% by mass or more and 90.0% by mass or less, based on the toner particles. The crystalline vinyl resin is (i) Unit A represented by the above formula (1), and (ii) Unit B represented by formula (2) above It contains a crystalline resin A having the following characteristics: The toner particles contain a metal capable of forming a complex in the acetylacetonate portion of unit B of the crystalline resin A, in an amount of 0.0020% by mass or more and 0.0500% by mass or less, based on the mass of the toner particles. At least a portion of the unit B in the crystalline resin A forms a complex with the metal in the acetylacetonate portion. A toner characterized in that the crystalline resin A contains 0.50% by mass or more and 10.0% by mass or less of the unit B. (Configuration 2) The toner according to Configuration 1, wherein the total content of the crystalline organic material is 30.0% by mass or more and 70.0% by mass or less, based on the toner particles. (Configuration 3) The toner according to Configuration 1 or 2, wherein the content of unit A in the crystalline resin A is 40.0% by mass or more and 90.0% by mass or less. (Configuration 4) The toner according to any of Configurations 1 to 3, wherein the metal bonded to Unit B is one of Al, Zn, Fe, Cu, Co, Ni, Ti, Mg, or Mn. (Configuration 5) The toner according to any one of Configurations 1 to 3, wherein the metal bonded to Unit B is aluminum. (Configuration 6) The toner according to any one of Configurations 1 to 5, wherein the content of the crystalline resin A in the crystalline organic material is 1.0% by mass or more and 70.0% by mass or less. (Configuration 7) The toner according to any one of Configurations 1 to 6, wherein the crystalline resin A has an acid value (Av) and a hydroxyl value (OHv) of 5.0 mgKOH / g or less, respectively. (Configuration 8) The toner according to any one of Configurations 1 to 7, wherein the crystalline resin A has a melting point of 55.0°C or higher and 70.0°C or lower. (Configuration 9) The toner according to any one of Configurations 1 to 8, wherein the crystalline organic material contains 80.0% by mass or more of crystalline resin B as a crystalline vinyl resin, having a weight-average molecular weight (Mw) of 5,000 or more and a content of unit A represented by formula (1) of 40.0% by mass or more and a content of unit B less than 0.50% by mass. (Configuration 10) The toner particles contain amorphous resin C, and the amorphous resin C is styrene acrylic resin or polyester resin. The toner according to any one of configurations 1 to 9, wherein the wax component in the crystalline organic material has an ester wax, and the content of the ester wax in the crystalline organic material is 70.0% by mass or more. (Configuration 11) The toner according to any one of Configurations 1 to 10, wherein the metal bonded to Unit B is one of Al, Zn, Fe, Co, Ti, Mg, or Mn. [Examples]
[0126] The present invention will be described in detail below with reference to examples, but these examples are not intended to limit the present invention in any way.
[0127] <Example of manufacturing crystalline resin A1> The following materials were added to a reaction vessel equipped with a reflux condenser, stirrer, thermometer, and nitrogen inlet tube under a nitrogen atmosphere. Toluene 100.0 parts by mass Behenyl acrylate 80.0 parts by mass Styrene 18.5 parts by mass Acetoacetoxyethyl methacrylate 1.5 parts by mass Polymerization initiator t-butyl peroxypivalate (manufactured by NOF Corporation: Perbutyl PV) 2.0 parts by mass
[0128] The reaction vessel was heated to 70°C while stirring at 200 rpm, and the polymerization reaction was carried out for 12 hours to obtain a solution in which the monomer polymer was dissolved in toluene. Subsequently, the solution was cooled to 25°C, and then added to 1000.0 parts by mass of methanol while stirring to precipitate the methanol-insoluble components. The obtained methanol-insoluble components were filtered off, washed with methanol, and then vacuum-dried at 40°C for 24 hours to obtain crystalline resin A1. The physical properties of the obtained crystalline resin A1 are shown in Table 2.
[0129] <Manufacturing examples of crystalline resins A2 to A15> Crystalline resins A2 to A15 were obtained in the same manner as in the example of producing crystalline resin A1, except that the monomer was changed as shown in Table 1.
[0130] [Table 1]
[0131] In Table 1, BEA represents behenyl acrylate, STA represents stearyl acrylate, AAEM represents acetoacetoxyethyl methacrylate, AAPM represents acetoacetoxypropyl methacrylate, AAEAA represents 2-[(1-oxo-2-propen-1-yl)amino]ethyl 3-oxobutanoate, and HEMA represents 2-hydroxyethyl methacrylate.
[0132] [Table 2]
[0133] <Manufacturing examples of crystalline resins B1-B8> Crystalline resins B1 to B8 were obtained in the same manner as in the production example of crystalline resin A, except that the type and amount of monomer added and the amount of initiator were changed, as shown in Table 3 below. The physical properties of the obtained crystalline resins B1 to B8 are shown in Table 3.
[0134] [Table 3]
[0135] In Table 3, BEA represents behenyl acrylate and MAN represents methacrylonitrile.
[0136] <Manufacturing of Crystalline Polyester 1> In a reaction vessel equipped with a stirrer, thermometer, nitrogen inlet tube, dehydration tube, and vacuum device, 100.0 parts by mass of 1,10-decanedicarboxylic acid and 120.0 parts by mass of 1,12-dodecanediol were added and heated to 130°C while stirring. After adding 0.7 parts by mass of titanium(IV) isopropoxide as an esterification catalyst, the temperature was raised to 160°C and condensation polymerization was carried out over 5 hours. Thereafter, the temperature was raised to 180°C and the reaction was carried out under reduced pressure until the desired molecular weight was obtained to obtain crystalline polyester 1.
[0137] <Example of Amorphous Resin C1 Production> In an automatic reaction vessel equipped with a depressurization device, a water separation device, a nitrogen gas introduction device, a temperature measuring device, and a stirring device, Terephthalic acid 29.9 parts by mass • Bisphenol A-propylene oxide 2 molar adduct 40.0 parts by mass Isosorbide 10.0 parts by mass • Ethylene glycol 4.5 parts by mass • Tetrabutoxytitanate 0.125 parts by mass The above monomers and catalyst were charged, and a polycondensation reaction was carried out under a nitrogen atmosphere, atmospheric pressure, and at -200°C for 5 hours to obtain amorphous resin C1.
[0138] <Example of Amorphous Resin C2 Production> • Styrene 80.0 parts by mass Butyl acrylate (n-BA) 18.0 parts by mass • Acrylic acid 2.0 parts by mass • Toluene 50.0 parts by mass The above materials were mixed and heated to 70°C. While stirring, 1.0 part by mass of t-butyl peroxypivalate was added as a polymerization initiator. Polymerization was then carried out at 70°C for 5 hours, and the temperature was further increased to 85°C and heated and held for 2 hours. After cooling, the mixture was reprecipitated in methanol, filtered, and dried to obtain amorphous resin C2.
[0139] <Example of toner particle 1 manufacturing> [Toner manufacturing by suspension polymerization method] Butyl acrylate (n-BA) 10.4 parts by mass • Styrene 31.3 parts by mass • Coloring agent: Pigment Blue 15:3 5.0 parts by mass A mixture consisting of the above materials was prepared. The above mixture was placed in an attritor (manufactured by Nippon Coke Co., Ltd.) and dispersed using 5 mm diameter zirconia beads at 200 rpm for 2 hours to obtain a dispersion of raw materials.
[0140] Meanwhile, 735.0 parts by mass of deionized water and 16.0 parts by mass of trisodium phosphate (dodecahydrate) were added to a container equipped with a high-speed stirring device homomixer (Primix Corporation) and a thermometer, and the temperature was raised to 60°C while stirring at 12,000 rpm. Then, an aqueous calcium chloride solution, prepared by dissolving 9.0 parts by mass of calcium chloride (dihydrate) in 65.0 parts by mass of deionized water, was added, and the mixture was stirred at 12,000 rpm for 30 minutes while maintaining the temperature at 60°C. Then, 10% hydrochloric acid was added to adjust the pH to 6.0, and an aqueous medium in which an inorganic dispersion stabilizer containing hydroxyapatite was dispersed in water was obtained.
[0141] Next, the above raw material dispersion was transferred to a container equipped with a stirring device and a thermometer, and the temperature was raised to 60°C while stirring at 100 rpm.
[0142] ·Crystalline resin A1: 5.0 parts by mass ·Crystalline resin B1: 40.0 parts by mass • Aluminum distearate 0.30 parts by mass • Hydrocarbon wax: 5.0 parts by mass (Hydrogen wax; Paraffin wax HNP-9, manufactured by Nippon Seiro Co., Ltd.) ·Amorphous resin C2 3.0 parts by mass The above materials were added and stirred at 100 rpm for 30 minutes while maintaining a temperature of 60°C. Then, 9.0 parts by mass of t-butyl peroxypivalate (manufactured by NOF Corporation: Perbutyl PV) was added as a polymerization initiator and stirred for another minute. The mixture was then added to an aqueous medium being stirred at 12,000 rpm in the high-speed stirring device. Stirring was continued at 12,000 rpm for 20 minutes while maintaining a temperature of 60°C in the high-speed stirring device to obtain a granulated liquid.
[0143] The granulated liquid described above was transferred to a reaction vessel equipped with a reflux condenser, stirrer, thermometer, and nitrogen inlet tube, and heated to 70°C while stirring at 150 rpm under a nitrogen atmosphere. The polymerization reaction was carried out at 150 rpm for 12 hours while maintaining the temperature at 70°C to obtain a toner particle dispersion.
[0144] The obtained toner particle dispersion was cooled to 45°C while stirring at 150 rpm, and then heat-treated for 5 hours while maintaining the temperature at 45°C. Afterward, while maintaining stirring, dilute hydrochloric acid was added until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid components were filtered off, thoroughly washed with deionized water, and then vacuum-dried at 30°C for 24 hours to obtain toner particles 1. The weight-average particle size of the obtained toner particles 1 was 6.9 μm. The properties of the obtained toner particles 1 are shown in Table 5.
[0145] <Manufacturing examples of toner particles 2-46 and comparative toner particles 1-3> In the manufacturing example of toner particle 1 described above, toner particles 2-46 and comparative toner particles 1-3 were obtained in the same manner, except that the type and amount of added material were changed as shown in Table 4. The properties of the obtained toner particles 2-46 and comparative toner particles 1-3 are shown in Table 5.
[0146] [Table 4]
[0147] In Table 4, "parts" represents parts by mass, and EG18 represents ethylene glycol distearate, di-STAl represents aluminum distearate, di-STCo represents cobalt distearate, di-STMg represents magnesium distearate, di-STCu represents copper distearate, di-STZn represents zinc distearate, di-STCa represents calcium distearate, tri-STFe represents iron tristearate, di-STNi represents nickel distearate, Ti-ipr represents titanium tetraisopropoxide, and di-STMn represents manganese distearate.
[0148] <Example of toner particle 47 manufacturing> [Toner manufacturing using the grinding method] ·Crystalline resin A 5.0 parts by mass ·Amorphous resin C1 59.7 parts by mass • Ethylene glycol distearate 25.0 parts by mass • Hydrocarbon wax: 5.0 parts by mass (Hydrogen wax; Paraffin wax HNP-9, manufactured by Nippon Seiro Co., Ltd.) • Coloring agent: Pigment Blue 15:3 5.0 parts by mass • Aluminum distearate 0.30 parts by mass The raw materials shown in the above formula were mixed using a Henschel mixer (FM-75 model, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 seconds. -1 After mixing for 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30 model, manufactured by Ikegai Co., Ltd.) set to a temperature of 125°C. The resulting mixture was cooled and coarsely ground to less than 1 mm in a hammer mill to obtain coarse material. The obtained coarse material was finely ground in a mechanical pulverizer (T-250, manufactured by Turbo Kogyo Co., Ltd.). Further classification was performed using a rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) to obtain toner particles 47. The weight-average particle size of the obtained toner particles 47 was 7.5 μm. The properties are shown in Table 5.
[0149] <Example of toner particle 48 manufacturing> In the manufacturing example of toner particles 47, the raw materials were changed as follows. ·Crystalline resin A 5.0 parts by mass ·Amorphous resin C1 64.7 parts by mass Crystalline polyester 1 20.0 parts by mass • Hydrocarbon wax: 5.0 parts by mass (Hydrogen wax; Paraffin wax HNP-9, manufactured by Nippon Seiro Co., Ltd.) • Coloring agent: Pigment Blue 15:3 5.0 parts by mass • Aluminum distearate 0.30 parts by mass
[0150] Toner particles 48 were obtained by performing the same processing as in the manufacturing example of toner particles 47. The weight-average particle size of the obtained toner particles 48 was 7.8 μm. Their properties are shown in Table 5.
[0151] [Table 5]
[0152] <Example of Toner 1 manufacturing> For the above toner particles in a ratio of 1:98.0 parts by mass, silica microparticles (hydrophobized with hexamethyldisilazane, primary particle number average particle size: 10 nm, BET specific surface area: 170 m²) are added as an external additive. 2 2.0 parts by mass of ( / g) were added and mixed using a Henschel mixer (manufactured by Nippon Coke Co., Ltd.) at 3000 rpm for 15 minutes to obtain Toner 1.
[0153] <Manufacturing examples for toners 2-48 and comparative toners 1-3> Toner particles 2-48 and comparative toner particles 1-3 were obtained using the same method as described in the manufacturing example of toner 1 above.
[0154] [Examples 1-48] The following evaluations were performed using toners 1 through 48.
[0155] [Comparative Examples 1-3] The following evaluations were performed using comparative toners 1-3.
[0156] The toner evaluation method is shown below.
[0157] <Method for evaluating low-temperature fixation properties> Process cartridges filled with toner used for evaluation were left at 25°C and 40% RH for 48 hours. Using a modified LBP-712Ci (manufactured by Canon Inc.) that could operate even without the fuser, an unfixed image of an image pattern with 10mm x 10mm squares evenly distributed at 9 points across the entire transfer paper was printed. The amount of toner adhering to the transfer paper was 0.80 mg / cm². 2 The fixing start temperature was evaluated. The transfer paper was... • A4 standard paper ("Proverbond paper": 105g / m²) 2 (Manufactured by Fox River Corporation) The following was used: For the fuser, an external fuser was used, which was created by removing the fuser from the LBP-712Ci and allowing it to operate outside the laser beam printer.
[0158] The fixing temperature of the external fuser was increased in 5°C increments from 100°C, and the paper was fixed at a process speed of 330 mm / sec using standard paper. Kimwipes (S-200, manufactured by Crecia Co., Ltd.) were used, with a pressure of 7.35 kPa (75 g / cm²). 2 The fixed image was rubbed 10 times under a load of ) and the temperature at which the reduction in image density before and after rubbing was less than 5% was defined as the fixing start temperature. The fixing start temperature was evaluated based on the following criteria, and a value of C or higher was considered good. The evaluation results are shown in Table 6. [Evaluation Criteria] A: Fixation start temperature is 110°C or lower B: Fixation start temperature is between 115°C and 120°C. C: Fixing start temperature is between 125°C and 130°C. D: Fixing start temperature is 135°C or higher
[0159] <Method for evaluating heat resistance and storage properties> 5 g of each toner was placed in a 50 cc polycup and allowed to stand for 72 hours at a temperature of 50°C / humidity of 10%RH and at a temperature of 55°C / humidity of 10%RH, respectively. The presence or absence of agglomerates in the toner after standing was examined and evaluated. In the present invention, a C rank or higher provides good heat-resistant storage stability. The results are shown in Table 6. [Evaluation Criteria] A: No agglomerates generated B: Minor agglomerates generated, which crumble when lightly pressed with a finger C: Agglomerates generated, which do not crumble even when lightly pressed with a finger D: Completely agglomerated
[0160] <Evaluation of Charging Stability in HH and LL Environments> As the image forming apparatus, a modified version of LBP-712Ci (manufactured by Canon Inc.), which is a commercially available laser printer, was used. As modifications, the apparatus was connected to an external high-voltage power supply so that potentials for charging, transfer, etc. could be reversed, and images could be formed even with negatively or positively charged toners. The process speed was set to 210 mm / sec.
[0161] As the process cartridge, a commercially available toner cartridge 040H (cyan) (manufactured by Canon Inc.) was used. The product toner was removed from the inside of the cartridge, and after cleaning by air blowing, 165 g of the toner used for evaluation was filled therein.
[0162] For each of the yellow, magenta, and black stations, the product toner was removed, and yellow, magenta, and black cartridges with the toner remaining amount detection mechanism disabled were inserted for evaluation.
[0163] Images with a printing rate of 1% were continuously output in a low-temperature, low-humidity (LL) environment at a temperature of 15°C and a humidity of 10%RH and in a high-temperature, high-humidity (HH) environment at a temperature of 30°C and a humidity of 85%RH. Finally, 10,000 images were output, and the fog density of the solid white portions at that time was evaluated by the following method.
[0164] A solid white image was output, and the worst-case reflection density of the white area was defined as Ds, and the average reflection density of the transfer material before image formation was defined as Dr(%). [Dr-Ds(%)] was defined as the fogging value. The reflection density of the white area was measured using a reflectometer (Reflectometer Model TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.), and an amber light filter was used as the filter. A smaller value indicates a better evaluation. The evaluation criteria are as follows. The evaluation results are shown in Table 6.
[0165] [Evaluation Criteria] A: Less than 0.5% B: 0.5% or more and less than 1.5% C: 1.5% or more and less than 3.0% D: 3.0% or more
[0166] [Table 6]
Claims
1. A toner having toner particles containing a crystalline organic material, The crystalline organic material contains crystalline vinyl resin as an essential component, and further contains crystalline polyester and wax components as optional components. The total content of the crystalline vinyl resin, the crystalline polyester, and the wax component is 10.0% by mass or more and 90.0% by mass or less, based on the toner particles. The crystalline vinyl resin is (i) Unit A represented by the following formula (1), and (ii) Unit B represented by the following formula (2) It contains a crystalline resin A having the following characteristics: The toner particles contain a metal capable of forming a complex in the acetylacetonate portion of unit B of the crystalline resin A, in an amount of 0.0020% by mass or more and 0.0500% by mass or less, based on the mass of the toner particles. At least a portion of the unit B in the crystalline resin A forms a complex with the metal in the acetylacetonate portion. A toner characterized in that the crystalline resin A contains 0.50% by mass or more and 10.0% by mass or less of the unit B. 【Chemistry 1】 [In formula (1), R 1 L represents a hydrogen atom or a methyl group. 1 [where m represents a single bond, ester bond, or amide bond, and m represents an integer between 15 and 30.] 【Chemistry 2】 [In formula (2), R 2 L represents an alkylene group which may have a branched structure with 1 to 5 carbon atoms. 2 R represents a single bond, ester bond, or amide bond. 3 [This represents a hydrogen atom or a methyl group.]
2. The toner according to claim 1, wherein the total content of the crystalline organic material is 30.0% by mass or more and 70.0% by mass or less, based on the toner particles.
3. The toner according to claim 1 or 2, wherein the content of unit A in the crystalline resin A is 40.0% by mass or more and 90.0% by mass or less.
4. The toner according to claim 1 or 2, wherein the metal bonded to unit B is one of Al, Zn, Fe, Cu, Co, Ni, Ti, Mg, or Mn.
5. The toner according to claim 1 or 2, wherein the metal bonded to the unit B is aluminum.
6. The toner according to claim 1 or 2, wherein the content of the crystalline resin A in the crystalline organic material is 1.0% by mass or more and 70.0% by mass or less.
7. The toner according to claim 1 or 2, wherein the crystalline resin A has an acid value (Av) and a hydroxyl value (OHv) of 5.0 mgKOH / g or less, respectively.
8. The toner according to claim 1 or 2, wherein the crystalline resin A has a melting point of 55.0°C or higher and 70.0°C or lower.
9. The toner according to claim 1 or 2, wherein the crystalline organic material contains 80.0% by mass or more of crystalline resin B as a crystalline vinyl resin, having a weight-average molecular weight (Mw) of 5,000 or more and 50,000 or less, a content of unit A represented by formula (1) of 40.0% by mass or more and a content of unit B less than 0.50% by mass.
10. The toner particles contain amorphous resin C, and the amorphous resin C is styrene acrylic resin or polyester resin. The toner according to claim 1 or 2, wherein the wax component in the crystalline organic material has an ester wax, and the content of the ester wax in the crystalline organic material is 70.0% by mass or more.
11. The toner according to claim 1 or 2, wherein the metal bonded to the unit B is one of Al, Zn, Fe, Co, Ti, Mg, or Mn.
Citation Information
Patent Citations
Wet developer for developing electrostatic latent image
JP1994019216A
Resin composition for electrophotographic toner
JP1996095297A
Toner, developer composition containing toner and production process
JP2009064013A
Electrostatic charge image developing toner
JP2011118260A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2015036723A