Fiber sheet

A fiber sheet with controlled orthogonal elongation rates and specific fiber diameters in layers addresses the lack of elasticity and durability in ultrafine fiber sheets, achieving improved adhesion and resistance to tearing and abrasion.

JP7955185B2Active Publication Date: 2026-11-24KAO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023026742
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2026-11-24
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Fiber sheets containing ultrafine fibers lack sufficient elasticity, resistance to tearing, and abrasion, while maintaining adhesion to objects like skin, which conventional nonwoven fabrics do not adequately address.

Method used

A fiber sheet composed of a first layer with a median fiber diameter of 0.3 μm to 5 μm and a second layer with a median fiber diameter of 5 μm to 50 μm, both made from the same material system of olefin, diene, or urethane resins, with controlled elongation rates in orthogonal directions, enhancing directional elasticity and resistance to tearing and abrasion.

Benefits of technology

The fiber sheet exhibits directional elasticity, high resistance to tearing and abrasion, and improved adhesion to surfaces, with enhanced handling properties and durability during stretching and contracting movements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955185000002
    Figure 0007955185000002
  • Figure 0007955185000003
    Figure 0007955185000003
  • Figure 0007955185000004
    Figure 0007955185000004
Patent Text Reader

Abstract

To provide a fiber sheet that includes ultra fine fibers, expresses elasticity with directivity, and has high tolerance to break or abrasion.SOLUTION: A fiber sheet has a first fiber layer having the median fiber diameter of 0.3 μm or more and 5 μm or less and a second fiber layer which is adjacent to the first fiber layer and has the median fiber diameter of 5 μm or more and 50 μm or less, where the first fiber layer and the second fiber layer contain a material of the same series, a material of the same series is selected from olefin-based resin, diene-based resin, and urethane-based resin and a copolymer thereof, an elongation rate in one direction of the fiber sheet is 20 or more and 100 or less, and an elongation rate in a direction orthogonal to the one direction is 0 or more and 30 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a fiber sheet. [Background technology]

[0002] Sheets containing fibers (hereinafter referred to as fiber sheets) include, for example, nonwoven fabrics, and come with a variety of structures. For example, Patent Document 1 describes a multilayer stretchable nonwoven fabric in which an adhesive meltblown nonwoven fabric is laminated and bonded onto a non-adhesive meltblown nonwoven fabric. Both of these meltblown nonwoven fabrics are made of thermoplastic elastomers and possess stretchable properties. In this multilayer stretchable nonwoven fabric, even if it is adhesive during manufacturing, the occurrence of adhesion to manufacturing equipment is suppressed without reducing the aforementioned stretchable properties. Patent Document 2 describes a nonwoven fabric mainly composed of thermoplastic resin fibers, in which the elongation rate differs in one direction and in a direction perpendicular to it. This eliminates the need for post-processing of the nonwoven fabric when it is desired to have elasticity in only one direction.

[0003] In addition to the general nonwoven fabrics mentioned above, fiber sheets have recently attracted attention for their ability to deposit ultrafine fibers (e.g., fiber diameter of 5 μm or less). One example of a spinning technology for uniformly producing fiber sheets made of such fine fibers is the electrospinning method. Fiber sheets containing such ultrafine fibers have high adhesion to objects such as skin, and are expected to be used in a variety of applications in the future, and are being actively studied for industrialization. For example, the nanofiber sheet described in Patent Document 3 is shown as something to be applied to the skin for cosmetic purposes. Here, a technology is described for controlling the rigidity and slipperiness of the nanofiber sheet itself against the skin, from the viewpoint of maintaining the smooth state of the nanofiber sheet itself even when wrinkles occur on the skin surface due to changes in facial expression, etc., and maintaining its ability to conceal skin wrinkles. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-237752 [Patent Document 2] Japanese Patent Application Publication No. 9-279460 [Patent Document 3] Japanese Patent Publication No. 2021-54734 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] With regard to fiber sheets containing ultrafine fibers, such as those described in Patent Document 3, there has been a growing need to impart elasticity to them in order to further improve their adhesion to objects such as skin. On the other hand, the aforementioned fiber sheet is softer than conventional nonwoven fabrics due to the fineness of its constituent fibers. Therefore, the fiber sheet needs to have improved resistance to tearing and abrasion, in addition to its elasticity, without compromising the aforementioned adhesion. This point is not demonstrated in the conventional nonwoven fabrics with general fiber diameters described in Patent Documents 1 and 2.

[0006] In view of the above, the present invention relates to a fiber sheet containing ultrafine fibers that exhibits directional elasticity while simultaneously having high resistance to tearing and abrasion. [Means for solving the problem]

[0007] The present invention provides a fiber sheet having a first fiber layer with a median fiber diameter of 0.3 μm or more and 5 μm or less, and an adjacent second fiber layer with a median fiber diameter of 5 μm or more and 50 μm or less, wherein the first fiber layer and the second fiber layer contain the same material system, and the same material system is selected from olefin resins, diene resins, urethane resins, and copolymers thereof, and the fiber sheet has an elongation rate of 20 or more and 100 or less in one direction, and an elongation rate of 0 or more and 30 or less in the direction perpendicular to the said one direction. [Effects of the Invention]

[0008] The fiber sheet of the present invention contains ultrafine fibers, exhibiting directional elasticity while simultaneously possessing high resistance to tearing and abrasion. [Brief explanation of the drawing]

[0009] [Figure 1] This is a schematic cross-sectional view showing one embodiment of the fiber sheet according to the present invention. [Figure 2] (A) is a substitute photograph showing the first fiber layer being held between the fingers, and (B) is a substitute photograph showing the fiber sheet of the present invention being held between the fingers. [Figure 3] This is a schematic diagram illustrating the fusion points at the intersections of ultrafine fibers in the first fiber layer. [Figure 4] Figure 4 is a photograph used as a substitute for a diagram, showing an example of an observation image used when measuring the ratio of the number of fusion points to the number of fiber intersections. [Figure 5] This schematic diagram shows an example where fusion points are included at the intersection of the fibers in both layers at the interface between the first and second fiber layers, with (A) showing the state before stretching and (B) showing the state after stretching. [Figure 6] Figures (A) to (C) are schematic diagrams illustrating the procedure for measuring the compressive strength of a fiber sheet. [Modes for carrying out the invention]

[0010] A preferred embodiment of the fiber sheet of the present invention will be described below with reference to the drawings.

[0011] As shown in Figure 1, the fiber sheet 10 of the present invention is a laminated sheet having a first fiber layer 1 and a second fiber layer 2 adjacent thereto. The first fiber layer 1 is arranged on one surface side 10T of the front and back surfaces of the fiber sheet 10, and the second fiber layer 2 is arranged on the other surface side 10B opposite to the one surface side 10T. The fiber sheet 10 of the present invention may further include another fiber layer in addition to the first fiber layer 1 and the second fiber layer 2. In this case, from the viewpoint of allowing the later-described characteristics of the first fiber layer 1 to significantly exert their effects and not impairing the cooperative action between the first fiber layer 1 and the second fiber layer 2, the other fiber layer is preferably located on the other surface side 10B of the second fiber layer 2. That is, the first fiber layer 1 is preferably arranged as the outermost layer of the fiber sheet 10.

[0012] The first fiber layer 1 contains ultrafine fibers having a median fiber diameter (P1) of 0.3 μm or more and 5 μm or less. It can be formed, for example, by an electrospinning method. Due to the fineness of the fibers, such a first fiber layer 1 has suppressed unevenness per fiber unit compared to conventional fiber layers such as non-woven fabrics, resulting in a larger contact area with an object (e.g., skin surface) and higher adhesion to the object. For this reason, in the fiber sheet 10, it is preferable that the side of the first fiber layer 1 serves as the surface facing the object.

[0013] The median fiber diameter (P1) of the first fiber layer 1 is preferably 5 μm or less, more preferably 3 μm or less, further preferably 2 μm or less, and particularly preferably 1 μm or less, from the viewpoint of further enhancing adhesion to an object such as a skin surface. Further, the median fiber diameter (P1) of the first fiber layer 1 is preferably 0.3 μm or more, more preferably 0.4 μm or more, and further preferably 0.5 μm or more, from the viewpoint of imparting durability to withstand repeated stretching and contracting operations.

[0014] The second fiber layer 2 contains fibers with a median fiber diameter (P2) of 5 μm or more and 50 μm or less. By having the above median fiber diameter, the second fiber layer 2 provides sheet strength or rigidity to the entire fiber sheet 10, including the first fiber layer 1, without impairing the aforementioned adhesion properties of the first fiber layer 1, thereby increasing resistance to tearing and abrasion. Such a second fiber layer 2 can be obtained by appropriately setting the median fiber diameter using methods commonly used in this type of article. For example, nonwoven fabrics obtained using the spunbond method can be used.

[0015] The median fiber diameter (P2) of the second fiber layer 2 is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 25 μm or less, from the viewpoint of making the entire fiber sheet 10 thinner and easier to stretch. Furthermore, the median fiber diameter (P2) of the second fiber layer 2 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more, from the viewpoint of increasing resistance to tearing and abrasion.

[0016] Furthermore, the ratio (P2 / P1) of the median fiber diameter (P2) of the second fiber diameter 2 to the median fiber diameter (P1) of the first fiber diameter 1 is preferably 1.5 or higher, more preferably 10 or higher, and even more preferably 20 or higher, from the viewpoint of increasing the overall strength of the fiber sheet 10 while maintaining the adhesion characteristics of the first fiber layer 1 to the skin surface. Furthermore, the ratio (P2 / P1) is preferably 170 or less, more preferably 150 or less, and even more preferably 100 or less, from the viewpoint of reducing the overall thickness of the fiber sheet and improving its elasticity.

[0017] (Method for measuring median fiber diameter) (1) Separate the fiber sheet 10 between the fiber layers and take out the fiber layer to be measured. Cut this fiber layer into 10 mm x 10 mm pieces. Attach these pieces to a scanning electron microscope sample stage (manufactured by Oken Shoji Co., Ltd.) using conductive carbon double-sided tape (manufactured by Oken Shoji Co., Ltd.). (2) The sample stage to which the fiber layer is attached is placed in a sputtering apparatus (Hitachi High-Tech Corporation, Ion Sputter E-1030). Platinum-palladium (Pt-Pd) deposition is performed under an argon gas atmosphere with a reduced pressure of 6 Pa. The distance between the fiber layer mounting surface and the Pt-Pd electrode is set to 30 mm, the deposition time to 80 seconds, and the deposition current to 30 mA. (3) A sample stage is provided to a scanning electron microscope (SEM) (Hitachi High-Tech Corporation, S-4300SE / N), and observation images are acquired in high-resolution mode (acceleration voltage: 5kV, workpiece distance: 10mm, observation magnification: 500x or 1000x). Observation images are acquired from a total of 15 locations by changing the observation position for the same sample. (4) Using the observation images obtained in (3) above, the fiber diameter of the fiber layer is measured using image analysis software (WinRooF2015 manufactured by Mitani Corporation). From the measured fiber diameters of a total of 600 fibers, the number mean diameter, the several-tenths percent diameter (D10), the several-fifths percent diameter (median diameter), and the several-nineths percent diameter (D90) are compiled (starting from the smallest diameter side). Of these, the median diameter is used as the representative value of the fiber diameter.

[0018] The first fiber layer 1 and the second fiber layer 2 contain the same material system. This same material system refers to a material having a polymer structure with identical repeating units (monomer structures). Specifically, the same material system is selected from olefin resins, diene resins, urethane resins, and copolymers thereof. Because the first fiber layer 1 and the second fiber layer 2 contain the same material, the molecular structures of their respective resin components are similar, resulting in high compatibility between their fibers. Therefore, the first fiber layer 1 and the second fiber layer 2 are easily fused together, enhancing the overall integrity of the fiber sheet 10. Furthermore, the same material is selected from olefin resins, diene resins, urethane resins, and copolymers thereof, and both the first fiber layer 1 and the second fiber layer 2 contain elastomers and are elastic.

[0019] (Method for measuring whether the first fiber layer 1 and the second fiber layer 2 contain the same material system) To determine whether the first fiber layer 1 and the second fiber layer 2 contain the same material, the fiber layers are separated and the resin composition contained in each fiber layer is measured. The resin composition is subjected to various analyses such as nuclear magnetic resonance (NMR) analysis and infrared spectroscopy (IR) analysis, and the structure of the molecular skeleton and the functional group structure at the ends of the molecular structure are identified based on the signals and spectral positions obtained from these analyses. This identifies and specifies the type of resin contained in each fiber layer. The resin compositions identified for each fiber layer are compared to determine whether they contain the same material.

[0020] The fiber sheet of the present invention has high unity while both the adjacent first fiber layer 1 and second fiber layer 2 possess elasticity. This unity makes it difficult for delamination to occur at the interface between the first fiber layer 1 and the second fiber layer 2 when the fiber sheet 10 is stretched or contracted. By suppressing delamination, the fiber sheet 10 gains overall sheet strength or rigidity, and becomes more resilient. Furthermore, the first fiber layer 1 becomes more easily stretched or contracted together with the second fiber layer 2. As a result, the fiber sheet 10 as a whole has durability that can withstand repeated stretching and contracting movements. In other words, the fiber sheet 10 of the present invention is designed to stretch or contract with high overall sheet strength or rigidity due to the high unity of the first fiber layer 1 and the second fiber layer 2. Therefore, twisting and abrasion of the first fiber layer 1 are less likely to occur during the stretching and contracting behavior of the fiber sheet 10. In addition, shedding of fibers in the first fiber layer 1 is suppressed. In this way, the fiber sheet 10 as a whole exhibits improved elasticity and sheet strength, and even when elasticity is achieved, resistance to tearing and abrasion is enhanced. Furthermore, due to the overall stretching and contraction of the fiber sheet 10, the first fiber layer 1 can follow the shape and various changes (movements) of an object such as the skin surface, and can fully exhibit the aforementioned adhesive properties even under these changes.

[0021] The fiber sheet 10 of the present invention is given rigidity due to the integration of the first fiber layer 1 and the second fiber layer 2, and its handling properties are improved. In other words, it has more stiffness than a fiber sheet consisting of only the first fiber layer 1 made of ultrafine fibers (Figures 2(A) and (B)), and it also has the effect of being easier to handle. For example, when taking out a single fiber sheet 10 from a stack of fiber sheets 10 or from storage in a packaging bag or container and using it (for example, applying it to the skin surface), the stiffness significantly affects how easy it is to take out. Furthermore, even when taken out, the fiber sheet 10 of the present invention is less likely to curl up than a fiber sheet consisting of only the first fiber layer 1 (for example, Figure 2(A)), and its handling properties are improved. As a result, it is possible to apply it neatly to an object such as the skin surface without wrinkles.

[0022] Of the above-mentioned materials, olefin resins are preferred from the viewpoint of increasing the integrity of the first fiber layer 1 and the second fiber layer 2, and improving the elasticity of the fiber sheet 10 containing them. By using an olefin resin, the first fiber layer 1 and the second fiber layer 2 become less likely to peel off when the fiber sheet 10 is stretched or contracted. Furthermore, from a similar viewpoint, it is preferable that the first fiber layer 1 contains a low-crystallinity olefin resin. The term "low-crystallinity" means that the degree of crystallinity is 10.5% or less, and this can be measured by the method described below. By containing a low-crystallinity olefin resin in the first fiber layer 1, the first fiber layer 1 itself becomes more flexible. When the first fiber layer 1 contains a low-crystallinity olefin resin, the mass percentage of the low-crystallinity olefin resin in the first fiber layer 1 is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 92% by mass or more, and even more preferably 94% by mass or more.

[0023] (Method for measuring whether the first fiber layer 1 contains a low-crystallinity olefin resin) The resin composition constituting the first fiber layer 1 is subjected to various analyses such as NMR analysis and IR analysis. Based on the signals and spectral positions obtained from these analyses, the structure of the molecular skeleton and the functional group structure at the ends of the molecular structure are identified. This allows for the identification and specification of the type of resin contained. Next, crystallinity is measured using differential scanning calorimetry. The total heat of fusion obtained when the resin composition is heated is divided by the heat of fusion of a perfect crystal. If this value is less than 10.5%, it is determined that the resin contains a low-crystallinity olefin resin.

[0024] From the viewpoint of enhancing the integrity of the first fiber layer 1 and the second fiber layer 2 and improving the elasticity of the fiber sheet 10 containing them, the following specific examples can be given of the above-mentioned identical material system. In other words, examples of olefin resins include polypropylene (hereinafter referred to as PP) and polyethylene. Examples of low-crystallinity olefin resins include α-olefins, such as polypropylene with controlled stereoregularity (polypropylene polymerized with controlled stereoregularity using a metallocene catalyst). Examples of diene resins include polybutadiene and polyisoprene. Examples of urethane-based resins include polyurethane. Examples of copolymers of olefin resins, diene resins, and urethane resins include ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-octene copolymer, propylene-1-butene copolymer, propylene-1-octene copolymer, ethylene-isoprene copolymer, ethylene-butadiene copolymer, propylene-isoprene copolymer, propylene-butadiene copolymer, ethylene-propylene-isoprene copolymer, and ethylene-propylene-butadiene copolymer.

[0025] In the fiber sheet 10, in a structure in which a first fiber layer 1 and a second fiber layer are integrated and both possess elasticity, it is preferable that the elongation rate in one direction Y (also called the Y direction) in the planar direction is 20 to 100, and the elongation rate in the direction X (also called the X direction) perpendicular to the said direction is 0 to 30. The difference in elongation rates between these two mutually orthogonal directions gives the fiber sheet 10 directional elasticity. This one direction Y and the direction X perpendicular to the said direction Y are appropriately determined according to the intended use of the fiber sheet 10. For example, the longitudinal direction of the fiber sheet 10 may be the one direction Y, and the width direction may be the direction X perpendicular to the one direction Y. In this case, it is preferable that the longitudinal direction of the fiber sheet 10 aligns with the direction of elasticity required in the article to which it is applied.

[0026] (Method for measuring elongation rate) The elongation rate in the fiber sheet 10 is calculated by fixing a test specimen with a width of 20 mm and a length of 70 mm with a gripping distance of 50 mm, and expressing the elongation of the test specimen under a tensile load of 1.2 N as a percentage of the gripping distance of 50 mm. More specifically, the elongation rate can be calculated by setting the length between the grips of the test specimen before the elongation test as L0, and the length between the grips of the test specimen at the time of fracture elongation as LB, and then using the formula: Elongation rate (%) = 100 × (LB - L0) / L0. The measurement is performed along any two mutually orthogonal directions within the sheet plane of the fiber sheet 10, for example, the longitudinal direction and the width direction perpendicular to the longitudinal direction.

[0027] Because the fiber sheet 10 has a directional elasticity due to the difference in elongation rates, its elasticity can be suitably controlled to suit the intended use, thereby reducing excessive stretching in directions where elasticity is not needed and reducing excessive load associated with stretching. This makes it possible to more effectively suppress twisting, abrasion, and tearing of the first fiber layer 1. For example, when the fiber sheet 10 is made into a glove, it is preferable to make the elasticity in the length direction of the finger large and the elasticity in the width direction perpendicular to the length direction small. This makes it possible to provide a glove that fits closely to the fingertips and webbing of the user's fingers. On the other hand, when the fiber sheet 10 is made into a glove, it is also preferable to make the elasticity in the length direction of the finger small and the elasticity in the width direction perpendicular to the length direction large. This makes it possible to provide a glove that fits snugly according to the thickness of the user's fingers when wearing a glove made of the fiber sheet 10.

[0028] As described above, the fiber sheet 10 of the present invention contains ultrafine fibers, exhibits directional elasticity, and simultaneously has high resistance to tearing and abrasion.

[0029] The elongation rate (T1) of the fiber sheet 10 in one direction Y is preferably 20% or more, more preferably 25% or more, and even more preferably 30% or more, from the viewpoint of further enhancing the aforementioned effects. From the viewpoint of processing and attaching the fiber sheet to an arbitrary shape, the elongation rate (T1) is preferably 100% or less, more preferably 80% or less, and even more preferably 60% or less. The elongation rate (T2) of the fiber sheet 10 in the direction X perpendicular to the one direction Y is preferably 0% or greater from the viewpoint of continuous conveying of the fiber sheet. The elongation rate (T2) is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less, from the viewpoint of continuously conveying the fiber sheet.

[0030] The absolute value |T1-T2| of the difference between the elongation rate of the fiber sheet 10 in one direction Y (T1) and the elongation rate of the fiber sheet 10 in the direction X perpendicular to the one direction Y (T2) is preferably 0 or greater, more preferably 10 or greater, and even more preferably 20 or greater, from the viewpoint of more clearly defining the directionality of the elasticity of the fiber sheet 10 and more effectively suppressing twisting, abrasion, and tearing of the first fiber layer 1. The absolute value of the difference |T1-T2| is preferably 70 or less, more preferably 60 or less, and even more preferably 50 or less, from the viewpoint of improving the adherence of the fiber sheet to objects such as skin. This makes it possible to balance the elongation rates in two orthogonal directions in the glove, for example, when the fiber sheet 10 is applied to a glove, making it easier to put on.

[0031] The directionality of the stretchability in the fiber sheet 10 is mainly determined by the second fiber layer 2 rather than the first fiber layer 1. The first fiber layer 1 contains the aforementioned ultrafine fibers and is formed by directly spinning and depositing a resin solution or resin melt using, for example, electrospinning, making it difficult to form a directionality of stretchability. Therefore, it is preferable to mainly impart the directionality of stretchability to the fiber sheet 10 in the second fiber layer 2. Furthermore, by mainly determining the directionality of stretchability in the fiber sheet 10 in the second fiber layer 2, it is possible to suitably control the stretching of the fiber sheet 10 so that the second fiber layer 2 stops stretching before the first fiber layer 1 breaks. The directionality of stretchability in the second fiber layer 2 can be formed, for example, by stretching it in the transport direction and allowing it to cool and solidify during the transport process, so that the second fiber layer does not have stretchability in the transport direction but has stretchability in the perpendicular direction.

[0032] From the viewpoint of further increasing the strength of the first fiber layer 1 itself in the fiber sheet 10, it is preferable that the ratio of the number of fusion points (for example, the enclosed areas labeled D4, D14, and D1 in Figure 4) to the number of fiber intersections in a 0.128 mm × 0.096 mm field of view of the SEM image of the first fiber layer 1 be 50% or more, and more preferably 70% or more. This increases the strength by fixing each individual ultrafine fiber of the first fiber layer 1 at the intersection. In other words, the integrity of the first fiber layer 1 itself is strengthened. For example, when the surface of the first fiber layer 1 on one side 10T of the fiber sheet 10 is traced with a finger, the fibers are less likely to fray and fiber shedding is suppressed. Also, because the bonding area is suppressed at the fusion points at the fiber intersections, compared to surface fusion, an excessive increase in the rigidity of the first fiber layer 1 itself is suppressed, maintaining its softness and making it easier for the aforementioned adhesion characteristics to be expressed.

[0033] (The ratio of the number of fusion points to the number of fiber intersections) Perform the same procedure as in (1), (2), and (3) above in the section (Method for Measuring Median Fiber Diameter) and acquire an SEM observation image of the fiber layer to be measured at an observation magnification of 1000x. For the same sample, measurements are taken at a total of 5 locations, changing the observation site each time. Focus on the surface side of the sample at each location and acquire a total of 5 observation images. The image quality should be 0.128 mm in width and 0.096 mm in height. From the acquired observation images, mark the fiber intersections using image analysis software (WinRooF2015 manufactured by Mitani Corporation) and record the number of fusion points at the fiber intersections. Calculate the ratio of the number of fusion points to the total number of fiber intersections using the following formula (I). This evaluation is performed by two people: an observer and a recorder. The number of fiber intersections is tallied by the observer's marking process on the image analysis software. For fusion points, the recorder tally the fiber intersections that the observer designated as fusion points according to the definition of fusion points below. Percentage of fusion points [%] = Number of fusion points / Total number of fiber intersections × 100 (Equation (I)) Furthermore, the definitions of fiber intersections and fusion points of said fiber intersections are defined as follows. (Fiber intersection) In the SEM observation image of the fiber layer to be measured, the image itself is magnified three times (300%) on a 410mm x 260mm monitor. In this case, a focus is selected within a range where the width between the boundaries of the fiber shapes (fiber width observed in the observation image) does not exceed 1 mm. Fiber intersections are defined as points where they intersect, points where they do not intersect but are in contact, or points where a single fiber branches off midway (for example, the enclosed areas labeled D4, D14, and D1 in Figure 4). If two or more fibers visible in the image are in contact along the longitudinal direction in the entire or partial area of ​​the image acquisition region, forming a fiber bundle, these are also defined as fiber intersections (for example, the enclosed area labeled D5 in Figure 4). For example, if there is a point in the observation image where four fibers are lined up without gaps, the number of fiber intersections is determined to be 3. Furthermore, due to the characteristics of the fibrous layer, SEM observation involves a depth difference caused by the thickness of the fibrous layer, with the side closer to the detector (surface side in the sample thickness direction) and the side further away (sample stage side in the sample thickness direction). Therefore, even if fibers appear to intersect in the observation image, they may not actually be in contact with each other. As mentioned above, when the image itself is magnified three times (300%) on a 410mm x 260mm monitor, multiple fibers that are in focus within a range where the width of the fiber shape boundary does not exceed 1mm are considered to be in a similar positional relationship in the thickness direction (depth) of the sample. The intersection points of these selected fibers are defined as fiber intersections according to the definition above. (Fusion point at fiber intersection) Of the intersections defined above, (i) locations where the boundary lines of two or more related fibers at the intersection are not clearly discernible (for example, the area enclosed by the symbol D4 in Figure 4), and (ii) locations where the width between the boundary lines of one or more related fibers at the intersection is wider than the width between boundary lines outside the intersection (for example, the area enclosed by the symbol D16 in Figure 4) are defined as fiber intersection fusion points. When the sheets are laminated, the fiber layers are separated and the fiber layer to be measured is removed and subjected to the above procedure.

[0034] The fiber sheet 10 possesses the elasticity described above, while maintaining the integrity of the first fiber layer 1 and the second fiber layer 2, and possessing high strength. This strength is expressed as the breaking strength. In relation to the aforementioned elasticity and the resistance of the first fiber layer 1 to abrasion and tearing during stretching behavior, it is preferable that the breaking strength be within the following range in the two directions X and Y that show the aforementioned elongation rate. The breaking strength in the Y direction is preferably 1 N / 20 mm or more, more preferably 2 N / 20 mm or more, and even more preferably 2.5 N / 20 mm or more, from the viewpoint of obtaining resistance to elongation. The breaking strength in the X direction is preferably 1 N / 20 mm or more, more preferably 3 N / 20 mm or more, and even more preferably 5 N / 20 mm or more, from the viewpoint of facilitating the transport of the fiber sheet.

[0035] (Method for measuring the breaking strength of fiber sheet 10) The breaking strength of the fiber sheet 10 is determined by fixing a test specimen with a width of 20 mm and a length of 70 mm with a gripping distance of 50 mm, stretching it at a tensile speed of 300 mm / min, and recording the maximum load until it breaks as the breaking strength. The measurement temperature is 23°C.

[0036] In the fiber sheet 10, it is preferable from the viewpoint of improving integrity that the fibers of both the first fiber layer 1 and the second fiber layer 2 are fused together at the interface (for example, fusion point 32 in Figure 5(A)). Furthermore, it is preferable that the fibers of both layers at the interface are joined by fusion points at the intersection of the fibers while maintaining the shape of the fibers, as this can suppress an excessive increase in the rigidity of the fiber sheet 10. The aforementioned fusion means that the resin components contained in the first fiber layer 1 and the second fiber layer 2 melt due to heat and adhere to each other (e.g., thermal bonding). As mentioned above, since the first fiber layer 1 and the second fiber layer 2 contain the same material with high compatibility, the fusion at the interface becomes stronger. This enhances the integration of the first fiber layer 1 and the second fiber layer 2 while maintaining the softness and adhesion to skin surfaces, etc., on one side 10T of the first fiber layer 1 itself. In particular, delamination at the interface between the first fiber layer 1 and the second fiber layer 2 can be more effectively suppressed during the stretching and contracting behavior of the fiber sheet 10, resulting in better followability between the two layers (for example, Figures 5(A) to (B)). By suppressing delamination, twisting, wrinkles, abrasion, and tearing of the first fiber layer 1 caused by delamination can be more effectively prevented. Furthermore, the improved integration leads to better handling of the fiber sheet 10.

[0037] From the viewpoint of further improving the above effect, the fusion strength at the interface is preferably 0.01 N / 20 mm or more, more preferably 0.1 N / 20 mm or more, and even more preferably 0.2 N / 20 mm or more. Furthermore, the strength of fusion at the interface is practically 10 N / 20 mm or less.

[0038] (Method for measuring the strength of fusion at the interface between the first fiber layer and the second fiber layer 2) Measurement will be performed using the following methods. An adhesive tape is applied to the surface of the first fiber layer 1 of a fiber sheet, and the tape is peeled off in a T-shape using a tensile testing machine. This allows for the measurement of the fusion strength between the fibers of both layers at the interface between the first fiber layer 1 and the second fiber layer 2. The more fusion points there are at the interface between the first and second fiber layers, the greater the resistance when peeled off in a T-shape. After applying an adhesive tape (adhesion strength: 4.4 N / 10 mm) to the surface side of the first fiber layer 1, a test specimen with a width of 20 mm and a length of 100 mm is prepared. The tape end on the longitudinal side is peeled off, and the tape end and the fiber sheet are gripped and pulled at a distance of 50 mm and a tensile speed of 100 mm / min, and the test force at which the tape peels off from the fiber sheet is measured. Of the obtained test forces, the average value of the test forces during which the gripping distance from the initial point is between 30 mm and 80 mm is taken as the fusion strength, i.e., the fusion force.

[0039] The fusion points at the fiber intersections in the first fiber layer 1, and the fusion points between the fibers at the interface between the first fiber layer 1 and the second fiber layer 2, are easily formed when the first and second fiber layers contain the same material as described above. They can be formed as follows. On the surface of the second fiber layer 2, a resin solution or resin melt using the same material as described above is discharged from a nozzle, for example, by electrospinning. The spun fibers formed by the discharge (the constituent fibers of the first fiber layer 1) are collected on the second fiber layer 2 while they are at a high temperature and fluid. This allows the spun fibers to be collected in a state where they are fused at their intersections, and the spun fibers and the fibers of the second fiber layer 2 are integrated in a fused state. By collecting these spun fibers, the first fiber layer 1 is formed, which has a network with fusion points at the aforementioned fiber intersections. At the same time, fusion points between the fibers of both the first fiber layer 1 and the second fiber layer 2 can be formed at the interface between them. The temperature at which the spun fibers become fluid is appropriately set depending on the resin raw material used. For example, when low-crystallinity PP resin is used as the resin raw material for the first fiber layer 1, it is preferable to collect the spun fibers in a range of 40°C to 70°C where they change to a rubbery state. Furthermore, it is preferable to heat and maintain such a temperature for the second fiber layer 2, which serves as the collection tray. In addition to the methods described above, the aforementioned fusion points can also be formed by heat sealing. From the viewpoint of preventing thermal shrinkage of the elastomer of the fibers and film formation due to the melting of the resin, as mentioned above, fusion during spinning, which involves less exposure to heat in terms of time and number of times, is more preferable.

[0040] In the fiber sheet 10, the basis weight of the first fiber layer 1 is 1 g / m². 2and 8 g / m 2 or less. When the basis weight of the first fiber layer 1 is within this range, the first fiber layer 1 maintains the aforementioned softness, adhesion to the skin surface, etc., and uniformity of the formulation liquid film accompanied by capillary force, and can be provided with strength without impairing these. Further, in the first fiber layer 1 whose basis weight is suppressed within the above range, the number of ultrafine fibers having the aforementioned median fiber diameter is reduced by that amount, and the number of fiber voids is also reduced. As a result, light scattering due to the presence of the fiber voids is suppressed, and the first fiber layer 1 is likely to be transparentized. From the viewpoint of further increasing the capillary force and further increasing the strength, the basis weight of the first fiber layer 1 is 1 g / m 2 or more is preferable, and 1.5 g / m 2 or more is more preferable, and 2 g / m 2 or more is even more preferable. From the viewpoint of further enhancing softness and adhesion to the skin surface, etc., the basis weight of the first fiber layer 1 is 8 g / m 2 or less is preferable, and 6 g / m 2 or less is more preferable, and 5 g / m 2 or less is even more preferable.

[0041] In the fiber sheet 10, the basis weight of the second fiber layer 2 is 8 g / m 2 or more and 50 g / m 2 or less is preferable. When the basis weight of the second fiber layer 2 is within this range, the strength of the entire fiber sheet 10 can be further enhanced, and the resistance to tearing and abrasion can be further increased. Further, in the second fiber layer 2 having a basis weight within the above range, the number of fibers having the aforementioned median fiber diameter is reduced. From the viewpoint of further increasing the strength of the entire fiber sheet 10, the basis weight of the second fiber layer 2 is 8 g / m 2 or more is preferable, and 15 g / m 2 or more is more preferable, and 20 g / m 2 or more is even more preferable. From the viewpoint of preventing the softness of the first fiber layer 1 and the adhesion to the skin surface, etc. from being impaired, the basis weight of the second fiber layer 2 is 50 g / m 2 or less is preferable, and 40 g / m 2 or less is more preferable, and 30 g / m 2 or less is even more preferable.

[0042] Such fiber sheets 10 can be used in a variety of articles. For example, they can be used in adhesive bandages, dressings, tubular bodies, gloves, etc., which are used in contact with the skin surface. Specific examples of the tubular bodies include supports and finger cots. In such articles, it is preferable that the article has unidirectional stretchability. That is, it is preferable that the fiber sheet 10 is applied to the article such that it stretches along the unidirectional stretch direction Y. Furthermore, the aforementioned "unidirectional stretchability" refers to the direction in which the difference in elongation rates between two mutually orthogonal directions is 20 percentage points or more, obtained by applying a 1.2N load to the sample based on the (method for measuring elongation rate) described above, and the elongation rate is greater. In the case of the fiber sheet 10, these two mutually orthogonal directions are one direction Y and the direction X that is orthogonal to that direction Y. [Examples]

[0043] The present invention will be described in more detail below based on examples, but the present invention is not to be interpreted as being limited thereto. In these examples, "parts" and "%" used to express mass are both based on mass unless otherwise specified. "←" means that it is the same as the column on the left. "-" means that there is no value corresponding to that item.

[0044] (Example 1) Using PP as the resin raw material, a second fiber layer 2 with the median fiber diameter and basis weight shown in Table 1 was formed by the spunbond method. A resin molten solution was prepared using the resin raw material PP, and spun by electrospinning. During this process, the space between the spinning nozzle and the collection device was heated to over 40°C by hot air ejected from around the spinning nozzle, and the spun fibers were collected on the second fiber layer 2 in a fluid state. The distance between the nozzle and the collection device was set to 300 mm. This resulted in the formation of the first fiber layer 1 with the median fiber diameter and basis weight shown in Table 1. With the above manufacturing method, fusion points were formed at the fiber intersections within the first fiber layer 1, and fusion points were formed between the fibers of both layers at the interface between the first fiber layer 1 and the second fiber layer 2. As a result, the first fiber layer 1 and the second fiber layer 2 were firmly integrated, and a fiber sheet sample of Example 1 with elasticity was produced. The obtained fiber sheet sample of Example 1 was cut into rectangular pieces with dimensions of 100 mm along the machine flow direction (MD) during the manufacturing of the long second fiber layer 2, and 20 mm along the width direction (Cross Direction (CD)) perpendicular to the MD direction. That is, the MD direction and the CD direction correspond to the above-mentioned directions X and Y. In the obtained fiber sheet sample, as shown in Table 1, there was a 25 percentage point difference between the elongation rate in the MD direction and the elongation rate in the CD direction. In other words, the direction of elasticity in Example 1 was in the MD direction.

[0045] (Example 2) The fiber sheet sample for Example 2 was prepared in the same manner as in Example 1, except that the basis weight of the first fiber layer 1 was as shown in Table 1.

[0046] (Comparative Example 1) The first fiber layer 1 prepared in Example 1 was used alone as the fiber sheet sample for Comparative Example 1.

[0047] (Comparative Example 2) The second fiber layer 2 prepared in Example 1 was used alone as the fiber sheet sample for Comparative Example 2.

[0048] The following tests were performed on the fiber sheet samples of each example and each comparative example. (1) Elongation rate (under 1.2N load) Based on the aforementioned (method for measuring elongation), the elongation was measured for each fiber sheet sample under a load of 1.2 N. The elongation was measured in each fiber sheet sample along two directions: the MD direction and the width direction perpendicular to the MD direction. (2) Breaking strength The measurement was performed based on the aforementioned (method for measuring the breaking strength of the fiber sheet 10). (3) Fusion strength The measurement was performed based on the aforementioned method for measuring the strength of fusion at the interface between the first fiber layer 1 and the second fiber layer 2. (4) Compression strength Ten test pieces S, each 20 mm wide and 100 mm long, were stacked to create a ring-shaped test piece Q, with the ends S1 and S2 overlapping by 20 mm (Figures 6(A) and (B)). S1 and S2 were fixed together using staples or similar. A compression test was performed on the width X of the above test piece Q using two flat plates W1 and W2 with a diameter of 30 mm or more at a compression speed of 10 mm / min (Figure 6(C)). The maximum compressive load in the compression test was recorded as the compressive strength. A higher compressive strength indicates higher sheet rigidity and better sheet handling.

[0049] [Table 1]

[0050] In Comparative Example 1, the elongation could not be measured because the breaking strength of the fiber sheet was 1.2 N or less. In other words, it broke when a load of about 1.2 N was applied, and it could not maintain its elongation. In contrast, in Examples 1 and 2, the elongation rates were as shown in Table 1, and the material exhibited elasticity. Furthermore, both Examples 1 and 2 exhibited higher breaking strength compared to Comparative Example 1. Therefore, it can be seen that they have higher resistance to tearing compared to Comparative Example 1. Furthermore, Examples 1 and 2 exhibit fusion strength between the first and second fiber layers, resulting in high resistance to abrasion. In addition, Examples 1 and 2 both exhibited higher compressive strength compared to Comparative Examples 1 and 2. This, along with the aforementioned fusion strength and integrated laminated structure, demonstrates that Examples 1 and 2 have superior handling properties compared to Comparative Example 1, which consists of only the first fiber layer 1, and Comparative Example 2, which consists of only the second fiber layer 2. From the above, it was found that the fiber sheet of the present invention exhibits elasticity while also having high resistance to tearing and abrasion. In addition, it was found that the fiber sheet of the present invention also has excellent handling properties. [Explanation of Symbols]

[0051] 1. First fiber layer 2. Second fiber layer 10 Fiber Sheets

Claims

1. A fiber sheet having a first fiber layer with a median fiber diameter of 0.3 μm or more and 5 μm or less, and a second fiber layer adjacent thereto with a median fiber diameter of 5 μm or more and 50 μm or less. The first fiber layer and the second fiber layer contain the same material system, and this same material system is selected from olefin resins, diene resins, urethane resins, and copolymers thereof. A fiber sheet having an elongation rate of 20 to 100 in one direction, and an elongation rate of 0 to 30 in a direction perpendicular to the said one direction.

2. The aforementioned identical material is an olefin resin. The fiber sheet according to claim 1, wherein the first fiber layer comprises a low-crystalline olefin resin.

3. The fiber sheet according to claim 1 or 2, wherein the first fiber layer has a ratio of 50% or more of the number of fusion points to the number of fiber intersections in a scanning electron microscope image of 0.128 mm × 0.096 mm.

4. The basis weight of the first fiber layer is 1 g / m². 2 8g / m or more 2 The fiber sheet according to claim 1 or 2, which is as follows:

5. The basis weight of the second fiber layer is 8 g / m². 2 50g / m or more 2 The fiber sheet according to claim 1 or 2, which is as follows:

6. A bandage, dressing, tubular body, or glove comprising the fiber sheet described in claim 1 or 2.

7. The adhesive bandage, dressing, tubular body, or glove according to claim 6, having unidirectional stretchability.

Citation Information

Patent Citations

  • Unidirectionally stretchable nonwoven fabric and its production, and diaper, sanitary article using the nonwoven fabric

    JP1997279460A

  • Multi-layered nonwoven stretch fabric and its production

    JP1998237752A

  • Nanofiber sheet

    JP2021054734A