Method for carbon dioxide fixation, and cement hardened body

By adjusting the water content of cementitious bodies and carbonating them at low pressures and temperatures, the method effectively immobilizes carbon dioxide in cement, addressing energy inefficiencies in existing technologies and contributing to carbon neutrality.

JP7955186B2Active Publication Date: 2026-11-24MITSUBISHI UBE CEMENT CORP +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023027518
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2026-11-24
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

Existing methods for fixing carbon dioxide in cementitious bodies require high temperatures, necessitating significant energy input to heat low-temperature carbon dioxide-containing gases.

Method used

A method involving a pretreatment step to adjust the water content of a hardened cement body to 10-70% followed by a carbonation step at pressures of 9 MPa or less and temperatures of 60°C or less to immobilize carbon dioxide.

Benefits of technology

Sufficient carbon dioxide immobilization in cementitious bodies is achieved at lower temperatures, reducing energy consumption and equipment constraints while promoting carbon neutrality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955186000004
    Figure 0007955186000004
  • Figure 0007955186000005
    Figure 0007955186000005
  • Figure 0007955186000006
    Figure 0007955186000006
Patent Text Reader

Abstract

To provide a method for immobilizing carbon dioxide, capable of sufficiently immobilizing carbon dioxide in a cement hardened body even at a relatively low temperature.SOLUTION: A method for immobilizing carbon dioxide includes: a pretreatment step of adjusting the moisture content of a cement hardened body (A) to obtain a cement hardened body (B) having a moisture content W of 10 to 70%, as calculated by formulas (1) to (3); and a carbonation step of contacting the hardened cement body (B) with carbon dioxide under a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which carbon dioxide is immobilized. (1) W=100-Δw2 / Δw1×100; (2) Δw1=(WA-WD) / WA×100; (3) Δw2=(WA-WB) / WA×100 [In the formulae (1)-(3), WA and WB are the weights of the cement hardened bodies (A) and (B), respectively; and WD is the weight of the cement hardened body (A) when it is dried at 105°C under atmospheric pressure until it reaches a constant weight].SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to a method for fixing carbon dioxide and a cement hardened body. [Background technology]

[0002] To achieve carbon neutrality, technological development is underway to reduce carbon dioxide emissions. One such technology is the fixation of CO2 as CaCO3 in calcium-rich materials such as cementitious bodies. For example, Patent Document 1 proposes a technology in which carbon dioxide contained in a carbon dioxide-containing gas with a temperature of 350°C or higher, such as factory exhaust gas, is brought into contact with a cementitious body, thereby fixing the carbon dioxide contained in the carbon dioxide-containing gas into the cementitious body. Patent Document 2 proposes a method in which carbon dioxide is fixed in contact with a cementitious body by bringing it into contact with a carbon dioxide-containing gas with a moisture content of 1.5% or higher and a temperature of 75 to 175°C. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2020-131074 [Patent Document 2] Japanese Patent Publication No. 2020-15659 [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] In the technologies described in Patent Documents 1 and 2, the temperature of the carbon dioxide-containing gas needs to be high in order to fix carbon dioxide in the cement hardened body. Therefore, when using a low-temperature carbon dioxide-containing gas, a lot of energy is required to heat the gas.

[0005] Accordingly, the present disclosure provides a method for immobilizing carbon dioxide that can sufficiently immobilize carbon dioxide in a hardened cement body even at a relatively low temperature. Also provided are a hardened cement body capable of sufficiently immobilizing carbon dioxide even at a relatively low temperature, and a hardened cement body in which carbon dioxide is sufficiently immobilized and which is useful for achieving carbon neutrality. [Means for Solving the Problems]

[0006] One aspect of the present disclosure is a pretreatment step of adjusting the water content of a hardened cement body (A) to obtain a hardened cement body (B) having a water ratio W calculated by the following formulas (1) to (3) of 10 to 70%, and a carbonation step of bringing the hardened cement body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a hardened cement body (C) in which the carbon dioxide is immobilized. A method for immobilizing carbon dioxide. W = 100 - Δw2 / Δw1 × 100 (1) Δw1 = (W A - W D ) / W A × 100 (2) Δw2 = (W A - W B ) / W A × 100 (3) However, in the above formulas (1) to (3), W A and W B represent the weights of the hardened cement body (A) and the hardened cement body (B), respectively, and W D represents the weight when the hardened cement body (A) is dried at 105°C under atmospheric pressure until it reaches a constant weight.

[0007] In this method for immobilizing carbon dioxide, carbon dioxide is brought into contact with a hardened cement body (B) having a water content W of 10 to 70%. This allows carbon dioxide to be sufficiently immobilized in the hardened cement body even at a relatively low temperature of 60°C or less.

[0008] One aspect of the present disclosure provides a method for immobilizing carbon dioxide, the method comprising: a pretreatment step of holding a hardened cement body (A) in an environment at a temperature of 5 to 55° C. and a relative humidity of 10 to 95% RH to obtain a hardened cement body (B); and a carbonation step of bringing the hardened cement body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60° C. or less to obtain a carbon dioxide-immobilized hardened cement body (C).

[0009] In this method for immobilizing carbon dioxide, the hardened cement body (B) with an adjusted water content can be obtained by performing the pretreatment step of holding the hardened cement body in a predetermined environment. Such a hardened cement body (B) can sufficiently immobilize carbon dioxide at a relatively low temperature of 60° C. or lower.

[0010] One aspect of the present disclosure provides a hardened cement body for immobilizing carbon dioxide, the hardened cement body containing water in at least a part of pores, and being capable of immobilizing 20 parts by weight or more of carbon dioxide with respect to 100 parts by weight of oxides contained in the hardened cement body when coexisting with carbon dioxide at a pressure of 9 MPa or less and a temperature of 60° C. or less. The weight of the “oxides contained in the hardened cement body” in the present specification is a weight obtained by excluding the amount of H2O and the amount of CO2 generated at room temperature to 1000° C. from the weight of the hardened cement body when thermogravimetric-mass spectrometry is performed on the hardened cement body.

[0011] This hardened cement body contains water in at least a part of pores, and can sufficiently immobilize carbon dioxide at a relatively low temperature of 60° C. or lower.

[0012] One aspect of the present disclosure provides a hardened cement body having a surface porosity of 7 to 18 area% and an immobilization amount of carbon dioxide of 20% by weight or more. This hardened cement body sufficiently immobilizes carbon dioxide, and is useful for achieving carbon neutrality. In addition, since components such as calcium carbonate constitute a dense structure, the hardened cement body is excellent in durability. [Advantageous Effects of Invention]

[0013] This disclosure provides a method for fixing carbon dioxide in a cementite, which is capable of sufficiently fixing carbon dioxide in a cementite even at relatively low temperatures. Furthermore, it provides a cementite capable of sufficiently fixing carbon dioxide even at relatively low temperatures, and a cementite in which carbon dioxide is sufficiently fixed, making it useful for achieving carbon neutrality. [Brief explanation of the drawing]

[0014] [Figure 1] (A), (B), (C), (D), (E), and (F) are magnified SEM images showing the surface of the hardened cement bodies of Examples 1, 2, 3, 4, 5 and Comparative Example 7. [Figure 2] (A), (B), (C), (D), (E), and (F) are magnified SEM images showing the surface of the hardened cement bodies of Examples 6, 7, 8, 9, 10 and Comparative Example 9. [Figure 3] (A), (B), (C), (D), (E), and (F) are magnified SEM images showing the surface of the cement hardened body (C) of Comparative Examples 1, 2, 3, 4, 5, and 6. [Modes for carrying out the invention]

[0015] Embodiments of this disclosure will be described below, with reference to the drawings as appropriate. However, the following embodiments are illustrative for the purpose of illustrating this disclosure and are not intended to limit this disclosure to the following. The numerical ranges illustrated by "a~b" are numerical ranges that include a and b, with a lower limit being a and b as the upper limit. The disclosure also includes the case in which the upper or lower limit of each numerical range is replaced with the numerical values ​​of any embodiment. If multiple materials are illustrated, one of them may be used alone or in combination with others.

[0016] <First Embodiment of a Method for Carbon Dioxide Fixation> The carbon dioxide fixation method according to this embodiment includes a pretreatment step of adjusting the moisture content of a cement hardened body (A) to obtain a cement hardened body (B) in which the moisture content W calculated by the following formulas (1) to (3) is 10 to 70%, and a carbonation step of contacting the cement hardened body (B) with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which carbon dioxide has been fixed. W = 100 - Δw² / Δw1 × 100 (1) Δw1=(W A -W D ) / W A ×100 (2) Δw²=(W A -W B ) / W A ×100 (3) However, in equations (1) to (3), W A and W B The values ​​shown are the weights of cement hardened body (A) and cement hardened body (B), respectively. D This indicates the weight of the cement hardened body (A) after drying at 105°C under atmospheric pressure until a constant weight is reached. That is, W D This is the weight of the hardened cement (D) after the moisture contained in the voids has been removed by drying. A >W B >W D The relationship between magnitudes is W A >W B >W D That's fine.

[0017] Δw1 corresponds to the weight change rate when the cement hardened body (A) is dried at 105°C under atmospheric pressure until it reaches a constant weight, as shown in equation (2) above. Δw2 corresponds to the weight change rate calculated by subtracting the weight of cement hardened body (B) from the weight of cement hardened body (A), as shown in equation (3) above. Δw1 may be 3-90%, 5-70%, 8-50%, or 10-30%. Δw2 may be 1-80%, 2-65%, 3-45%, or 5-25%.

[0018] The cementite (A) used in the above-described fixation method is a hardened body obtained by hardening a composition containing cement and water. The cementite may be a hardened cement paste, a hardened mortar, or a hardened concrete. Examples of cement include Portland cement, blended cement, and eco-cement.

[0019] The age of the cement hardened body (A) is not particularly limited; for example, it may be 1 day or older, or 1 year or older. The cement hardened body (A) contains voids, and at least some of these voids are filled with water. The cement hardened body (A) may be, for example, waste materials from building materials made of concrete or mortar, waste materials from cement paste hardening, or waste materials such as sludge generated in ready-mixed concrete. By using such waste materials, the effective utilization of resources can be achieved. The shape and size of the cement hardened body (A) are not particularly limited.

[0020] The hardened cement (A) may contain moisture. The moisture content W in the hardened cement (A) may be, for example, 15% or more, or 20% or more. This allows for the smooth production of a hardened cement (B) with a high moisture content W. The moisture content W in the hardened cement (A) may be, for example, 90% or less, or 80% or less. In the pretreatment step, the moisture content of the hardened cement (A) is adjusted, for example, using a constant temperature and humidity chamber.

[0021] The cementitious body (B) obtained by adjusting the moisture content of cementitious body (A) has a moisture content W of 10-70%. This range of moisture content W allows for sufficient carbon dioxide fixation under relatively mild conditions, such as a pressure of 9 MPa or less and a temperature of 60°C or less. From the viewpoint of further increasing the amount of carbon dioxide fixed, the moisture content W of cementitious body (B) may be 15% or more, or even 20% or more. Similarly, from the same viewpoint, the moisture content W may be 65% or less.

[0022] The moisture content W is calculated using equation (1) above, with respect to the weight loss rate Δw1 calculated by equation (2) above and the weight change rate Δw2 calculated by equation (3) below. For this reason, the weight loss rate Δw1 may be determined by performing a drying process in which the cement hardened body (A) is heated at 105°C for 48 hours, and then the weight change rate Δw2 may be determined by performing a pretreatment process in which it is held in a predetermined environment. Alternatively, multiple cement hardened bodies (A) with the same moisture content may be prepared, and the weight loss rate Δw1 may be determined using one cement hardened body (A), and the weight change rate Δw2 may be determined using another cement hardened body (A), and the moisture content W may be derived using equation (1) above using these values. In this case, the carbonation process is performed using the cement hardened body (B) obtained by pretreatment of the other cement hardened body (A).

[0023] The moisture content W in the hardened cement body (B) may be, for example, 10-70% or 25-65%. This moisture content W can be adjusted by changing the temperature, relative humidity, or holding time in the pretreatment process.

[0024] The moisture content of the cement hardened body (A) in the pretreatment process may be adjusted in a gas atmosphere at a temperature of 55°C or lower and a relative humidity of 95% RH or lower. This makes it possible to obtain a cement hardened body (B) with a high moisture content and sufficiently suppressed deterioration. Such a cement hardened body (B) can sufficiently fix carbon dioxide. The ambient temperature when adjusting the moisture content of the cement hardened body (A) may be 50°C or lower, or 45°C or lower, from the viewpoint of further sufficiently suppressing deterioration of the cement hardened body. The ambient temperature when adjusting the moisture content of the cement hardened body (A) may be 5°C or higher, 10°C or higher, or 15°C or higher, from the viewpoint of quickly adjusting the moisture content.

[0025] The relative humidity of the environment when adjusting the moisture content of the cementite (A) may be 95% RH or less, 80% RH or less, 65% RH or less, or 62% RH or less, from the viewpoint of further sufficiently suppressing deterioration of the cementite. The relative humidity of the environment when adjusting the moisture content of the cementite (A) may be 10% RH or more, 15% RH or more, 20% RH or more, or 25% RH or more, from the viewpoint of quickly adjusting the moisture content.

[0026] In the pretreatment step, the cement hardened body (A) is kept in the above-described environment for a predetermined period of time (for example, 1 minute or more, 1 hour or more, 1 day or more, 3 days or more, or 5 days or more). This makes it possible to obtain a cement hardened body (B) with a highly precise moisture content. The predetermined period for keeping the cement hardened body (A) in the above-described environment may be 30 days or less, 20 days or less, or 10 days or less.

[0027] The atmosphere in the pretreatment process is not particularly limited and can include, for example, air and inert gases such as nitrogen gas and argon gas. The atmosphere in the pretreatment process may contain carbon dioxide. In this case, carbon dioxide can be fixed during the pretreatment process. The pressure of the environment in the pretreatment process is not particularly limited as long as the moisture content of the cement hardened body (A) can be adjusted, and the pretreatment may be carried out under atmospheric pressure, reduced pressure, or increased pressure.

[0028] The pretreatment process is not limited to being performed in the gas phase; the moisture content of the cementite (A) may be adjusted by immersing the cementite (A) in water. This makes it possible to obtain a cementite (B) with a high moisture content and sufficiently suppressed deterioration in a short time.

[0029] In the carbonation process, the cement hardened body (B) is brought into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which carbon dioxide is fixed. The carbon dioxide may be in gaseous, liquid, supercritical, or subcritical form. The carbon dioxide may also be a mixture with other components. For example, the cement hardened body (C) may be obtained by bringing the cement hardened body (B) into contact with exhaust gas containing carbon dioxide and other components. When bringing the cement hardened body (B) into contact with a gas containing carbon dioxide, from the viewpoint of efficiently fixing carbon dioxide, the concentration of carbon dioxide in the gas may be 1 volume% or more, 3 volume% or more, 5 volume% or more, 10 volume% or more, 20 volume% or more, 30 volume% or more, 50 volume% or more, 70 volume% or more, or 90 volume% or more at standard conditions (1 atm, 273.15 K).

[0030] In the carbonation process, components contained in the hardened cement (B) react with carbon dioxide, for example, in the following reaction equations (4) and (5). Through these reactions, carbon dioxide is carbonated and fixed to the hardened cement. In reaction equation (5), x is any positive number, and z and t are any positive numbers that satisfy z + t = 1. Note that the reaction that fixes carbon dioxide is not limited to the following two reactions. Ca(OH)2 + CO2 → CaCO3 + H2O (4) (CaO) x (SiO2)(H2O)+xCO2→ xCaCO3+SiO2(H2O) t +(zt)H2O (5)

[0031] Since the hardened cement body (B) has a predetermined moisture content W, the reaction shown in reaction equation (4) above is promoted among the carbon dioxide fixation reactions. Therefore, carbon dioxide can be sufficiently fixed even under relatively mild conditions of a pressure of 9 MPa or less and a temperature of 60°C or less. Consequently, equipment constraints can be reduced, and energy consumption can be significantly lowered.

[0032] The pressure in the carbonation process may be 8 MPa or less, 7 MPa or less, 6 MPa or less, 5 MPa or less, 4 MPa or less, or 3 MPa or less, from the viewpoint of further reducing the load on the equipment and further reducing energy consumption. The pressure may be 0.2 MPa or more, 0.5 MPa or more, 1 MPa or more, or 1.5 MPa or more, from the viewpoint of sufficiently fixing carbon dioxide.

[0033] The temperature in the carbonation process may be 55°C or lower, 50°C or lower, 45°C or lower, 40°C or lower, or 35°C or lower, from the viewpoint of reducing equipment load and energy consumption. The temperature may also be 5°C or higher, 10°C or higher, or 15°C or higher, from the viewpoint of sufficiently fixing carbon dioxide.

[0034] The holding time under the above-mentioned pressure and temperature conditions may be 10 minutes or more, 1 hour or more, 10 hours or more, 15 hours or more, or 20 hours or more, from the viewpoint of sufficient carbon dioxide fixation. From the viewpoint of efficiency, the holding time under the above-mentioned pressure and temperature conditions may be 100 hours or less, or 50 hours or less.

[0035] In the carbonation process, the cement hardened body (B) can fix 20 parts by weight or more, preferably 25 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 35 parts by weight or more, and particularly preferably 40 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the cement hardened body (B). In this way, the cement hardened body (B) can sufficiently fix carbon dioxide. Therefore, it can greatly contribute to the realization of carbon neutrality. The amount of carbon dioxide fixed per 100 parts by weight of oxide contained in the cement hardened body (B) may be 60 parts by weight or less. The amount of carbon dioxide fixed per 100 parts by weight of oxide contained in the cement hardened body (B) can be determined by performing thermogravimetric-mass spectrometry on the cement hardened body (C) after fixation. This analysis quantifies the amount of carbon dioxide generated at room temperature to 1000°C. The weight of oxide contained in the cement hardened body (B) is the value obtained by subtracting the amount of H2O and CO2 generated at room temperature to 1000°C in the above analysis from the weight of the test specimen used for the analysis. By converting the amount of carbon dioxide obtained from the analysis into a value based on 100 parts by weight of oxides contained in the hardened cement (B), the amount of carbon dioxide fixed as described above can be determined.

[0036] The amount of carbon dioxide fixed in the cement hardened body (C) obtained by fixing carbon dioxide in the carbonation process is 20% by weight or more, preferably 25% by weight or more, more preferably 30% by weight or more, even more preferably 35% by weight or more, and particularly preferably 40% by weight or more. Such a cement hardened body (C) has sufficient carbon dioxide fixed. Therefore, it is useful for achieving carbon neutrality. The amount of carbon dioxide fixed in the cement hardened body (C) may be 50% by weight or less.

[0037] The amount of carbon dioxide fixed in the cementitious body (C) can be determined by multiplying the weight of carbon dioxide quantified by the thermogravimetric-mass spectrometry described above by 100, divided by the weight of oxides contained in the cementitious body (C). The weight of oxides contained in the cementitious body (C) is the value obtained by subtracting the amount of H2O and CO2 generated at room temperature to 1000°C in the above analysis from the weight of the test specimen used for the analysis.

[0038] <Second Embodiment of a Method for Carbon Dioxide Fixation> The carbon dioxide fixation method according to this embodiment includes a pretreatment step of obtaining a cement hardened body (B) by holding a cement hardened body (A) in an environment with a temperature of 5 to 55°C and a relative humidity of 10 to 70% RH, and a carbonation step of obtaining a cement hardened body (C) in which carbon dioxide is fixed by bringing the cement hardened body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less. In this embodiment, the pretreatment step is performed in a specific environment. This makes it possible to obtain a cement hardened body (B) in which carbon dioxide can be sufficiently fixed. As the cement hardened body (A), the one described in the first embodiment above can be used. The resulting cement hardened body (B) may also be the same as the one described in the first embodiment above.

[0039] The ambient temperature when adjusting the moisture content of the cement hardened body (A) in the pretreatment process may be 50°C or lower, or 45°C or lower, from the viewpoint of sufficiently suppressing deterioration of the cement hardened body. The ambient temperature when adjusting the moisture content of the cement hardened body (A) may be 10°C or higher, or 15°C or higher, from the viewpoint of quickly adjusting the moisture content.

[0040] The relative humidity of the environment when adjusting the moisture content of the cement hardened body (A) in the pretreatment process may be 95% RH or 62% RH or less, from the viewpoint of further sufficiently suppressing deterioration of the cement hardened body. The relative humidity of the environment when adjusting the moisture content of the cement hardened body (A) may be 15% RH or higher, 20% RH, or 25% RH or higher, from the viewpoint of quickly adjusting the moisture content.

[0041] In the pretreatment step, the period for holding the material under the above temperature and relative humidity conditions may be 1 minute or more, 1 hour or more, 3 days or more, or 5 days or more. This allows for highly accurate adjustment of the moisture content W of the hardened cement (A). The period for holding the hardened cement (A) under the above conditions may be 30 days or less, 20 days or less, or 10 days or less.

[0042] The carbonation process may be the same as in the above embodiment. The resulting cement hardened body (C) may also be the same as that described in the above embodiment. The carbon dioxide fixation method of this embodiment can also sufficiently fix carbon dioxide under relatively mild conditions of a pressure of 9 MPa or less and a temperature of 60°C or less. Therefore, it is possible to reduce equipment constraints and significantly reduce energy consumption. By further lowering the pressure and temperature, equipment load and energy consumption can be further reduced.

[0043] <First embodiment of a hardened cement body> The cement hardened body for carbon dioxide fixation according to this embodiment contains water in at least a portion of its voids and, when coexisting with carbon dioxide at a pressure of 9 MPa or less and a temperature of 60°C or less, can fix 20 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the cement hardened body. Such a cement hardened body may be the cement hardened body (B) obtained in the first and second embodiments of the carbon dioxide fixation method described above. Therefore, the contents of the cement hardened body (B) and its manufacturing method in each of the above embodiments of the fixation method also apply to this embodiment. Because the moisture content of this cement hardened body is within a predetermined range, carbon dioxide can be sufficiently fixed under relatively mild conditions of a temperature of 60°C or less and a pressure of 9 MPa or less.

[0044] The moisture content W of the hardened cement may be, for example, 10-70%, or 25-65%. This moisture content W can be calculated using the above formulas (1) to (3).

[0045] When a hardened cement body is in the presence of carbon dioxide at a pressure of 9 MPa or less and a temperature of 60°C or less, it can fix 20 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the hardened cement body. The hardened cement body can preferably fix 25 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 35 parts by weight or more, and particularly preferably 40 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the hardened cement body. Thus, the hardened cement body can sufficiently fix carbon dioxide. Therefore, it can greatly contribute to the realization of carbon neutrality. The amount of carbon dioxide fixed per 100 parts by weight of oxide contained in the hardened cement body may be 70 parts by weight or less. The amount of carbon dioxide fixed can be determined in the same manner as the method for determining the amount of carbon dioxide per 100 parts by weight of oxide contained in the hardened cement body (B) described above.

[0046] The conditions under which the hardened cement coexists with carbon dioxide may be the same as those described in each embodiment of the carbon dioxide fixation method described above. The age of the hardened cement may be one day or more. The shape and size of the hardened cement are not particularly limited.

[0047] <Second embodiment of the cement hardened body> The hardened cement body according to this embodiment has a surface porosity of 7 to 18 area percent and a carbon dioxide fixation amount of 20% by weight or more. This hardened cement body has sufficient carbon dioxide fixation and is useful for achieving carbon neutrality. A hardened cement body with a surface porosity within the above range has excellent durability because components such as calcium carbonate constitute a dense structure. Such a hardened cement body may be the hardened cement body (C) obtained in the first and second embodiments of the carbon dioxide fixation method described above. Therefore, the contents of the hardened cement body (C) and its manufacturing method in each of the above embodiments of the fixation method also apply to this embodiment.

[0048] The porosity on the surface of the hardened cement can be determined by using a scanning electron microscope to magnify the surface 500 times and then binarizing the image using image processing software. The amount of carbon dioxide fixed in the hardened cement is preferably 25% by weight or more, more preferably 30% by weight or more. Such a hardened cement has sufficient carbon dioxide fixed. Therefore, it is useful for achieving carbon neutrality. The amount of carbon dioxide fixed in the hardened cement may be 50% by weight or less. The amount of carbon dioxide fixed can be determined in the same manner as the method for determining the amount of carbon dioxide fixed in the hardened cement (C) described above.

[0049] The amount of carbon dioxide fixed in the cementitious body (cementitious body (C)) can be determined by dividing the weight of fixed carbon dioxide by the weight of oxides contained in the cementitious body (cementitious body (C)), and multiplying the resulting value by 100. The age of the cementitious body may be one day or more. The shape and size of the cementitious body are not particularly limited.

[0050] Although embodiments of the present disclosure have been described above, the present disclosure is not limited in any way to the embodiments described above. For example, each of the contents described in each embodiment may also be applicable to other embodiments.

[0051] This disclosure includes the following: [1] A pretreatment step to obtain a cement hardened body (B) in which the moisture content W calculated by the following formulas (1) to (3) is 10 to 70%, A method for fixing carbon dioxide, comprising a carbonation step of bringing the cement hardened body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which the carbon dioxide has been fixed. W = 100 - Δw² / Δw1 × 100 (1) Δw1=(W A -W D ) / W A ×100 (2) Δw²=(W A -WB ) / W A ×100 (3) [However, in formulas (1) to (3) above, W A and W B The values ​​of the cement hardened body (A) and the cement hardened body (B) are shown, respectively, and W D This indicates the weight obtained when the cement hardened body (A) is dried at 105°C under atmospheric pressure until it reaches a constant weight. [2] The carbon dioxide fixation method according to [1], wherein the moisture content of the cement hardened body (A) in the pretreatment step is adjusted in an environment with a temperature of 55°C or less and a relative humidity of 95%RH or less. [3] A pretreatment step to obtain a cement hardened body (B) by holding the cement hardened body (A) in an environment with a temperature of 5 to 55°C and a relative humidity of 10 to 95% RH, A method for fixing carbon dioxide, comprising a carbonation step of bringing the cement hardened body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which the carbon dioxide has been fixed. [4] The carbonation step is carried out under the conditions of a temperature of 55°C or lower, as described in any one of [1] to [3], for the fixation of carbon dioxide. [5] The carbon dioxide fixation method according to any one of [1] to [4], wherein the amount of carbon dioxide fixed in the cement hardened body (C) is 20% by weight or more. [6] The carbon dioxide fixation method according to any one of [1] to [5], wherein the age of the cement hardened body (A) is 1 day or more. [7] A cementitious body for carbon dioxide fixation, The void contains water in at least part of it. A cementitious body that, when coexisting with carbon dioxide at a pressure of 9 MPa or less and a temperature of 60°C or less, fixes 20 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the cementitious body. [8] A cementitious body having a surface void ratio of 7 to 18 area percent and a carbon dioxide fixation amount of 20% by weight or more. [9] A cementitious body according to [7] or [8], wherein the age of the material is 1 day or more. [Examples]

[0052] The contents of this disclosure will be described in more detail with reference to examples and comparative examples, but this disclosure is not limited to the following examples.

[0053] (Comparative Examples 1-6) A paste-hardened body of ordinary Portland cement (aged for more than one year) was prepared. This was cut to the desired size using an isomet cutter to produce multiple rectangular cement bodies (A) with dimensions of 1.7cm x 1.7cm x 0.3cm. The cement bodies (A) were dried in a drying oven (atmosphere: air) at atmospheric pressure for 48 hours at a temperature controlled to 105°C to obtain cement bodies (D). The weight of the cement bodies (A) before drying was W. A [g], weight W of the hardened cement body (D) after drying D The amount [g] of each was measured. Since the weight of the hardened cement body (D) was constant, the water content was considered to be 0. The weight loss rate Δw1[%] due to drying of each hardened cement body (A) was calculated using the following formula (2). As a result, the average value of Δw1 was 17.3%. Δw1=(W A -W D ) / W A ×100 (2)

[0054] The dried cementite (D) was placed in a reaction vessel, and carbon dioxide gas was filled into the pressure vessel using dry ice. The pressure vessel was then adjusted to the conditions shown in Table 1 and maintained for 24 hours in a carbonation process. The temperature of the pressure vessel was adjusted using a water bath. Subsequently, the sample (cementite (C)) was removed from the pressure vessel, and the amount of CO2 fixed in the sample (CO2 fixation amount) was measured using a thermogravimetric-mass spectrometer (manufactured by Rigaku Corporation, model: Thermo Mass Photo). The measurement results are shown in Table 1. Note that the CO2 fixation amount shown in Table 1 is a value based on the weight of oxides contained in the cementite (D) (100 wt%).

[0055] The surface of the hardened material was observed using a scanning electron microscope (SEM, magnification: 500x). The resulting SEM images were processed to determine the area ratio of voids (porosity). Image processing involved binarization using image processing software (Image J). The porosity was then calculated by dividing the total void area by the total area. The results are shown in Table 1.

[0056] [Table 1]

[0057] Figures 3(A), (B), (C), (D), (E), and (F) are magnified SEM images of the surface of the cementitious bodies (C) of Comparative Examples 1, 2, 3, 4, 5, and 6. As shown in Table 1, in the case of the dried cementitious body (D), the amount of CO2 fixed could be increased by sufficiently increasing the temperature and pressure in the carbonation process. However, it was confirmed that the amount of CO2 fixed decreased significantly when the pressure in the carbonation process was reduced.

[0058] (Examples 1-5, Comparative Example 7) Multiple rectangular cementite-shaped cementite bodies (A) with dimensions of length × width × height = 1.7 cm × 1.7 cm × 0.3 cm were prepared by cutting out the same paste-hardened material (aged for more than one year) as in Comparative Examples 1-6 using the same procedure as in Comparative Examples 1-5. These were placed in a constant temperature and humidity chamber and held for 7 days under pretreatment conditions of air, temperature 40°C, and relative humidity 30% RH (pretreatment process). The weight W of each cementite-hardened body (A) before pretreatment was... A [g] and the weight W of each cement hardened body (B) after the above pretreatment. B The weight [g] was measured, and the weight change rate Δw2 resulting from the pretreatment was calculated using the following formula (3). Δw²=(W A -W B ) / W A ×100 (3)

[0059] The water content W of the hardened cement (B) was calculated using the following formula (1), and the average water content W was 22.7%. The average value of the weight loss rate Δw1[%] obtained in Comparative Examples 1 to 6 was used as Δw1[%] in formula (1). W = 100 - Δw² / Δw1 × 100 (1)

[0060] The cementite (B) obtained after the above-described pretreatment was placed in the same reaction vessel as in Comparative Examples 1-6, and carbon dioxide gas was filled into the reaction vessel using dry ice. The reaction vessel was then adjusted to the conditions shown in Table 2 and maintained for 24 hours in a carbonation process. Subsequently, the sample (cementite (C)) was removed from the reaction vessel, and the amount of CO2 fixed in each sample (CO2 fixation amount) was measured using a thermogravimetric-mass spectrometer (manufactured by Rigaku Corporation, model: Thermo Mass Photo). The measurement results are shown in Table 2. Note that the CO2 fixation amount shown in Table 2 is a value based on the weight of oxides contained in cementite (B) (100 wt%).

[0061] The surface of the hardened cement body (C) was observed using the same procedure as in Comparative Examples 1-6, and the area ratio of voids (porosity) was determined by image processing. The porosity results are shown in Table 2.

[0062] (Comparative Example 8) A cementitious body was obtained using the same procedure as in Example 1, except that the carbonation step was omitted. In other words, the cementitious body (B) from Example 1 was used as the cementitious body (C) from Comparative Example 8. The amount of CO2 fixed in this cementitious body (C) was measured in the same manner as in Example 1. The measurement results are shown in Table 2.

[0063] [Table 2]

[0064] Figures 1(A), (B), (C), (D), and (E) are magnified SEM images showing the surface of the cementitious bodies (C) of Examples 1, 2, 3, 4, and 5. Figure 1(F) is a magnified SEM image showing the surface of the cementitious body (C) of Comparative Example 7. According to the results in Table 2, the cementitious bodies (C) of Examples 1 to 5 fixed the same amount of CO2 as or more than that of Comparative Example 7, which had the most severe temperature and pressure conditions in the carbonation process. Thus, it was confirmed that the cementitious bodies (C) can efficiently fix CO2 even under mild conditions by containing moisture in their voids. It should be noted that even in Comparative Example 7, which did not undergo a carbonation process, a small amount of CO2 was fixed. This is thought to be due to the incorporation of CO2 in the pretreatment process.

[0065] (Examples 6-10, Comparative Example 9) Except for setting the temperature of the constant temperature and humidity chamber in the pretreatment step to 20°C and the relative humidity to 60%RH, cement hardened bodies (C) of Examples 1-5 and Comparative Example 7 were prepared using the same procedure as in Comparative Examples 6-10 and Comparative Example 9. The temperature and pressure inside the reaction vessel during the carbonation step were as shown in Table 3. The average value of the water content W of the cement hardened body (B), calculated using the above formula (1), was 62.7% by weight. Here again, the average value of the weight loss rate Δw1[%] obtained in Comparative Examples 1-6 was used as Δw1[%] in formula (1). The amount of CO2 fixed and the porosity of each cement hardened body (C) were determined using the same procedure as in Examples 1-5 and Comparative Example 7. The results are shown in Table 3.

[0066] (Comparative Example 10) A cementitious body was obtained using the same procedure as in Example 6, except that the carbonation step was omitted. In other words, the cementitious body (B) from Example 6 was used as the cementitious body (C) from Comparative Example 10. The amount of CO2 fixed in this cementitious body (C) was measured in the same manner as in Example 6. The measurement results are shown in Table 3.

[0067] [Table 3]

[0068] Figures 2(A), (B), (C), (D), and (E) are magnified SEM images showing the surface of the cementitious bodies (C) of Examples 6, 7, 8, 9, and 10. Figure 2(F) is a magnified SEM image showing the surface of the cementitious body (C) of Comparative Example 9. According to the results in Table 3, the cementitious bodies (C) of Examples 6 to 10 fixed CO2 at a level equivalent to or greater than that of Comparative Example 9, which had the most severe temperature and pressure conditions in the carbonation process. Thus, it was confirmed that the cementitious bodies (C) can efficiently fix CO2 under mild conditions by containing moisture. In addition, a small amount of CO2 was fixed even in Comparative Example 10, which did not undergo a carbonation process. This is thought to be due to the incorporation of CO2 in the pretreatment process.

[0069] As shown in Tables 2 and 3, the cement hardened bodies (C) of Examples 1 to 10 were able to sufficiently fix CO2 under mild conditions of a pressure of 9 MPa or less and a temperature of 60°C or less. [Industrial applicability]

[0070] This disclosure provides a method for fixing carbon dioxide in a cementite body under mild conditions. Furthermore, it provides a cementite body capable of sufficiently fixing carbon dioxide under mild conditions, and a cementite body in which carbon dioxide is sufficiently fixed, making it useful for achieving carbon neutrality.

Claims

1. A pretreatment step to obtain a cementite (B) in which the water content of a cementite (A) obtained by hardening a composition containing cement and water is adjusted so that the water content W calculated by the following formulas (1) to (3) is 10 to 70%, A method for fixing carbon dioxide, comprising a carbonation step of bringing the cement hardened body (B) into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which the carbon dioxide has been fixed. W=100-Δw 2 / Δw 1 ×100 (1) Δw 1 =(W A -W D ) / W A ×100 (2) Δw 2 =(W A -W B ) / W A ×100 (3) [However, in formulas (1) to (3) above, W A and W B The values ​​of the cement hardened body (A) and the cement hardened body (B) are shown, respectively, and W D This indicates the weight of the cement hardened body (A) after it has been dried at 105°C under atmospheric pressure until it reaches a constant weight.

2. The carbon dioxide fixation method according to claim 1, wherein the adjustment of the moisture content of the cement hardened body (A) in the pretreatment step is performed in an environment with a temperature of 55°C or less and a relative humidity of 95% RH or less.

3. A pretreatment step to obtain a cement hardened body (B) by holding a cement hardened body (A) obtained by hardening a composition containing cement and water in an environment with a temperature of 5 to 55°C and a relative humidity of 10 to 95% RH, The process includes a carbonation step in which the cement hardened body (B) is brought into contact with carbon dioxide under conditions of a pressure of 9 MPa or less and a temperature of 60°C or less to obtain a cement hardened body (C) in which the carbon dioxide is immobilized. A method for fixing carbon dioxide, wherein the amount of carbon dioxide fixed in the cement hardened body (C) is 20% by weight or more.

4. The carbonation step is carried out under the conditions of a temperature of 55°C or lower, the method for fixing carbon dioxide according to any one of claims 1 to 3.

5. The carbon dioxide fixation method according to claim 1 or 2, wherein the amount of carbon dioxide fixed in the cement hardened body (C) is 20% by weight or more.

6. The carbon dioxide fixation method according to any one of claims 1 to 3, wherein the age of the cement hardened body (A) is one day or more.

7. A cementitious body for carbon dioxide fixation, The void contains water in at least part of it. A cementitious body that, when coexisting with carbon dioxide at a pressure of 9 MPa or less and a temperature of 60°C or less, fixes 20 parts by weight or more of carbon dioxide per 100 parts by weight of oxide contained in the cementitious body.

8. A cementitious body having a surface void ratio of 7 to 18 area percent and a carbon dioxide fixation amount of 20% by weight or more.

9. A cementitious body according to claim 7 or 8, wherein the age of the material is one day or more.

Citation Information

Patent Citations

  • Method and device for fixing carbon dioxide by using cement-based material

    CN112191090A

  • Method of manufacturing high-strength cement hardened body utilizing carbonation reaction

    JP2002080285A

  • Curing apparatus for hardened body

    JP2006143531A

  • Mortar or concrete having compacted surface layer and its manufacturing method

    JP2006182583A

  • Carbon dioxide fixing retaining wall

    JP2007177586A