Manufacturing method for semiconductor devices
Patent Information
- Application Number
- JP2023031776
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-03-02
Smart Images

Figure 0007955187000001 
Figure 0007955187000002 
Figure 0007955187000003
Abstract
Description
[Technical Field]
[0001] This embodiment relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] In the manufacturing of semiconductor devices, two substrates are sometimes joined together, and then one of the substrates is separated (laser delamination) by irradiating it with laser light. Improving the throughput of this laser delamination process is desirable. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2021-103725 [Patent Document 2] Japanese Patent Publication No. 2021-106197 [Patent Document 3] International Publication No. 2020 / 213478 [Patent Document 4] International Publication No. 2021 / 010284 [Patent Document 5] International Publication No. 2021 / 131710 [Patent Document 6] International Publication No. 2021 / 131711 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] One embodiment aims to provide a method for manufacturing a semiconductor device that can improve the throughput of laser peeling. [Means for solving the problem]
[0005] According to one embodiment, a method for manufacturing a semiconductor device is provided. The method for manufacturing a semiconductor device includes preparing a first substrate on which a plurality of two-dimensionally distributed protrusions are formed. The method for manufacturing a semiconductor device includes laminating a first film onto the plurality of protrusions on the first substrate. The method for manufacturing a semiconductor device includes laminating a second film onto a second substrate. The method for manufacturing a semiconductor device includes joining the main surface of the first film opposite to the first substrate to the main surface of the second film opposite to the second substrate. The method for manufacturing a semiconductor device includes irradiating the first substrate with laser light from the side. The method for manufacturing a semiconductor device includes peeling off the first substrate. The diameter of the spot area of the laser light is greater than the average arrangement pitch of the protrusions on the main surface of the first substrate. [Brief explanation of the drawing]
[0006] [Figure 1] A flowchart illustrating a method for manufacturing a semiconductor device according to the first embodiment. [Figure 2] A cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 3] An enlarged cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 4] A plan view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 5] A cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 6] An enlarged cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 7] A plan view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 8] A cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 9] A cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 10] A cross-sectional view showing a method for manufacturing a semiconductor device according to the first embodiment. [Figure 11] A cross-sectional view showing the generation of stress in the first embodiment. [Figure 12] Sectional view illustrating a method for manufacturing a semiconductor device according to a first embodiment. [Figure 13] Enlarged sectional view illustrating a method for manufacturing a semiconductor device according to the first embodiment. [Figure 14] Plan view illustrating a method for manufacturing a semiconductor device according to a first modification of the first embodiment. [Figure 15] Sectional view illustrating a method for manufacturing a semiconductor device according to a second modification of the first embodiment. [Figure 16] Sectional view illustrating a method for manufacturing a semiconductor device according to a third modification of the first embodiment. [Figure 17] Flowchart illustrating a method for manufacturing a semiconductor device according to a second embodiment. [Figure 18] Sectional view illustrating a method for manufacturing a semiconductor device according to the second embodiment. [Figure 19] Sectional view illustrating a method for manufacturing a semiconductor device according to the second embodiment. [Figure 20] Plan view illustrating a divided irradiation pattern in the second embodiment. [Figure 21] Sectional view illustrating a method for manufacturing a semiconductor device according to the second embodiment. [Figure 22] Sectional view illustrating a method for manufacturing a semiconductor device according to the second embodiment. [Figure 23] Plan view illustrating a divided irradiation pattern in a first modification of the second embodiment. [Figure 24] Plan view illustrating a divided irradiation pattern in a second modification of the second embodiment. [Figure 25] Plan view illustrating generation of stress in the second modification of the second embodiment. [Figure 26] Plan view illustrating a divided irradiation pattern in a third modification of the second embodiment. [Figure 27] Plan view illustrating generation of stress in the third modification of the second embodiment. [Embodiments for Carrying Out the Invention]
[0007] The method for manufacturing a semiconductor device according to the embodiments will be described in detail below with reference to the attached drawings. However, the present invention is not limited to these embodiments.
[0008] (First embodiment) In the semiconductor device manufacturing method according to the first embodiment, two substrates are joined together, and then one of the two substrates is peeled off (laser peeling) by irradiating it with laser light. Measures are taken to ensure that this laser peeling is performed efficiently.
[0009] In the following, the other substrate that remains unseparated from the two substrates being joined is used as the reference, the direction perpendicular to the main surface of the other substrate is defined as the Z direction, and the two mutually orthogonal directions within the plane perpendicular to the Z direction are defined as the X and Y directions.
[0010] For example, the manufacturing method of semiconductor device 1 can be as shown in Figures 1 to 12. Figure 1 is a flowchart of the manufacturing method of semiconductor device 1. Figures 2(a) to 2(f), 3(a), 3(b), 5(a) to 5(b), 6, 7(a) to 7(c), 9(a) to 9(c), 10, 12(a) to 12(e), and 13 are YZ cross-sectional views showing the manufacturing method of semiconductor device 1. Figure 3(a) is an enlarged cross-sectional view of Figure 2(a). Figure 3(b) is an enlarged cross-sectional view of Figure 2(e). Figure 6 is an enlarged cross-sectional view of Figure 5(a). Figure 13 is an enlarged cross-sectional view of Figure 12(e). Figure 11 is a YZ cross-sectional view showing the generation of stress. Figures 4 and 8 are XY plan views showing the manufacturing method of semiconductor device 1.
[0011] In the manufacturing method of semiconductor device 1, as shown in Figure 1, the processing of the lower substrate (S1-S2) and the processing of the upper substrate (S3-S5) are carried out in parallel, for example. The lower substrate is the substrate that is placed on the -Z side at the time of joining of the two substrates to be joined. The upper substrate is the substrate that is placed on the +Z side at the time of joining of the two substrates to be joined.
[0012] In the preparation of the lower substrate (S1), the substrate (lower substrate) 2 is prepared as shown in Figure 2(a). The substrate 2 may be formed from a material mainly composed of a semiconductor (e.g., silicon) that is substantially free of impurities.
[0013] During film deposition (S2), a predetermined device structure is formed on the main surface 2a side (+Z side) of the substrate 2, as shown in Figure 2(b).
[0014] For example, a peripheral circuit structure PHC as shown in Figure 3(a) may be formed. An impurity is introduced near the main surface 2a on the +Z side of the substrate 2 to form a semiconductor region SR. A conductive pattern GT is formed on the main surface 2a of the substrate 2. This forms a plurality of transistors TR, each containing a semiconductor region SR and a conductive pattern GT. The peripheral circuit structure PHC containing the plurality of transistors TR functions as a peripheral circuit to the memory cell array structure MAR, which will be described later.
[0015] After a predetermined device structure is formed, film 3 is formed by CVD or the like. For example, the interlayer insulating film 40 may be formed from a material mainly composed of an insulator, or from a material mainly composed of a semiconductor oxide (e.g., silicon oxide). In addition, as the interlayer insulating film 40 is deposited, holes are processed in the interlayer insulating film 40, conductive material is embedded, or conductive patterns are formed, thereby forming a wiring structure WR that is electrically connected to the transistor TR. On the main surface 40a on the +Z side of the interlayer insulating film 40, an electrode PD1 that is electrically connected to the wiring structure WR is formed by plating or the like. In Figure 2(b) and subsequent figures, for simplification, the film including the conductive pattern GT, wiring structure WR, electrode PD1, and interlayer insulating film 40 is illustrated and described as film 3. Also, since the interlayer insulating film 40 accounts for the majority of the volume of film 3, it is treated as if it may be formed from a material mainly composed of a semiconductor oxide (e.g., silicon oxide). Note that the device structure shown in Figure 3(a) is just an example and is not particularly limited.
[0016] In the preparation of the upper substrate (S3), the substrate (upper substrate) 100 is prepared as shown in Figure 2(c). The substrate 100 may be formed from a material mainly composed of a semiconductor (e.g., silicon) that is substantially free of impurities.
[0017] In the convex portion formation (S4), the main surface 100b of the substrate 100 is processed as shown in Figure 2(d). Multiple convex portions 101 are formed on the main surface 100b side (-Z side) of the substrate 100 by dry etching such as the RIE method. For example, a photosensitive agent is applied to the main surface 100b of the substrate 100, and a resist pattern RP (not shown) is formed by exposure and development to selectively cover multiple regions corresponding to the multiple convex portions 101 on the main surface 100b. Using the resist pattern RP as a mask, etching is performed under anisotropic etching conditions using the RIE method or the like to form multiple convex portions 101 on the main surface 100b of the substrate 100.
[0018] As shown in Figure 4, the multiple protrusions 101 are formed on the main surface 100b so as to be distributed in the XY direction. The arrangement direction of the multiple protrusions 101 may be random within the XY plane.
[0019] The XY distance between the centers of adjacent protrusions 101 in a plurality of protrusions 101 will be called the arrangement pitch. The arrangement pitch P of the plurality of protrusions 101 may be approximately constant or may vary within a predetermined range. Figure 4 illustrates a layout configuration in which the arrangement pitches P_1 to P_k of the plurality of protrusions 101 vary within a first range. The average arrangement pitch P of the protrusions 101 may be a value within a second range (for example, 0.1 μm to 10 μm). The average arrangement pitch P of the protrusions 101 may be the summation average of the arrangement pitches P_1 to P_k of the plurality of protrusions 101.
[0020] The Z distance from the main surface 100b at the tip surface of each protrusion 101 will be called the height. The height h of each protrusion 101 may be approximately constant, or it may vary within a third range. Figure 2(d) illustrates a configuration in which the height h of each protrusion 101 is approximately constant. The average height h of the protrusions 101 may be a value within a fourth range. The average height h of the protrusions 101 may be the sum of the heights h of multiple protrusions 101.
[0021] The maximum width in the XY direction at the tip surface of each protrusion 101 is called the tip width. The tip width W of each protrusion 101 may be approximately constant, or it may vary within the fifth range. Figure 4 illustrates a configuration in which the tip width W of each protrusion 101 is approximately constant. The average tip width W of the protrusions 101 may be a value within the sixth range. The average tip width W of the protrusions 101 may be the sum of the tip widths W of multiple protrusions 101.
[0022] The value obtained by dividing the height h of the protrusion 101 by the tip width W will be called the aspect ratio h / W. The aspect ratio h / W of each protrusion 101 may be approximately constant, or it may vary within the seventh range. Figure 2(d) illustrates a configuration in which the aspect ratio h / W of each protrusion 101 is approximately constant. The average aspect ratio h / W of the protrusions 101 may be a value within the eighth range (for example, 0.01 to 100). The average aspect ratio h / W of the protrusions 101 may also be the value obtained by dividing the average height h of the protrusions 101 by the average tip width W of the protrusions 101.
[0023] In film formation (S5), as shown in Figure 2(e), a film 4 covering multiple protrusions 101 is formed on the main surface 100b of the substrate 100 by a CVD method or the like.
[0024] For example, a film 4 including a memory cell array structure MAR as shown in Figure 3(b) may be formed. After depositing an insulating film 60 covering a plurality of protrusions 101 on the main surface 100b of the substrate 100, a conductive film is deposited, and the conductive film is patterned to form a conductive layer SL. The insulating film 60 may be made of an insulator such as silicon oxide. The conductive layer SL may be made of a conductive semiconductor such as polysilicon containing impurities. Subsequently, an insulating layer and a sacrificial layer (not shown) are deposited alternately multiple times on the +Z side of the conductive layer SL to form a laminate LM. The insulating layer may be made of an insulator such as silicon oxide. The sacrificial layer may be made of an insulator capable of ensuring an etching selectivity ratio with respect to the insulating layer, such as silicon nitride. Each insulating layer and each sacrificial layer may be deposited with generally similar film thicknesses.
[0025] A resist pattern with linear openings extending in the Y direction is formed on the -Z side of the laminate. Anisotropic etching, such as RIE (Reactive Ion Etching), is performed using the resist pattern as a mask to form grooves penetrating the laminate LM in the YZ direction. A dividing film (not shown) is then embedded in the grooves. The dividing film may be formed from a material mainly composed of an insulator (e.g., silicon oxide). The dividing film extends in the YZ direction on the -X side of the laminate LM. The dividing film separates the laminate LM from other laminate LMs on the -X side. In each laminate LM, insulating layers and sacrificial layers are stacked alternately multiple times. Each laminate LM has a substantially rectangular shape with the Y direction as the longitudinal direction in an XY plan view.
[0026] A resist pattern with openings for memory hole formation is formed on the Z side of each laminate. Anisotropic etching, such as RIE, is performed using the resist pattern as a mask to form memory holes that penetrate the laminate LM and reach the conductive layer SL.
[0027] A block insulating film, a charge storage film, and a tunnel insulating film are deposited sequentially on the sides and bottom of the memory hole. The block insulating film may be formed from an insulator such as silicon oxide. The portion of the tunnel insulating film on the bottom of the memory hole is selectively removed.
[0028] A semiconductor film is deposited on the sides and bottom of the memory holes. The semiconductor film may be made of a material mainly composed of a semiconductor (e.g., polysilicon). Then, a core member is embedded in the memory hole. The core member may be made of an insulator such as silicon oxide. This forms a plurality of columnar bodies PL that penetrate the laminate LM in the Z direction. The plurality of columnar bodies PL are formed to be arranged in the XY direction.
[0029] The sacrificial layer of the laminate LM is removed. A block insulating film is formed on the exposed surface of the void created by the removal. The block insulating film may be made of an insulator such as aluminum oxide. A conductive layer WL is then embedded in the void. The conductive layer WL may be made of a material mainly composed of a conductor (e.g., a metal such as tungsten). This forms a laminate LM in which conductive layers WL and insulating layers are repeatedly stacked alternately. Memory cells are formed at the intersection of the conductive layer WL and the semiconductor film of the columnar body PL. That is, a memory cell array structure MAR is formed in which multiple memory cells are arranged three-dimensionally.
[0030] Furthermore, an interlayer insulating film 50 is formed to cover the laminate LM. By repeatedly forming a resist pattern, slimming, and etching, a stepped structure is formed in which conductive layers WL are drawn out in a stepped manner on both sides of the laminate LM in the Y direction. Conductive plugs CC are formed that are electrically connected to each conductive layer WL by forming holes in the interlayer insulating film 50 and embedding conductive material. In addition, as the interlayer insulating film 50 is deposited, holes are processed in the interlayer insulating film 50 and conductive material is embedded or conductive patterns are formed, thereby forming a wiring structure WR2 that is electrically connected to the conductive plugs CC. On the main surface 50a on the -Z side of the interlayer insulating film 50, electrodes PD2 that are electrically connected to the wiring structure WR2 are formed by plating or the like. In Figure 2(e) and subsequent figures, for simplification, the film including the memory cell array structure MAR, conductive plugs CC, wiring structure WR2, electrodes PD2, and interlayer insulating films 50 and 60 is illustrated and described as film 4. Furthermore, since the part of film 4 that is of interest in this embodiment is the interlayer insulating film 60, the material of film 4 is treated as mainly being the material of the interlayer insulating film 60. Note that the device structure shown in Figure 3(b) is just an example and is not particularly limited. Also, although one memory cell array structure (MAR) is shown in Figure 3(b), there may be multiple MARs.
[0031] The film 4 can be formed from any material with a greater infrared light absorption rate than the substrate 100. The film 4 may also be formed from any material with a greater absorption rate than the substrate 100 at laser wavelengths suitable for the film 4 to function as a laser absorption layer (e.g., 9200 nm or higher, and 10800 nm or lower). The film 4 may be formed from a material mainly composed of an insulator, or from a material mainly composed of a semiconductor oxide (e.g., silicon oxide).
[0032] As shown in Figure 1, once the processing of the lower substrate (S1-S2) and the upper substrate (S3-S5) is completed, the upper and lower substrates are joined together (S6). The main surface 3a on the +Z side of film 3 (see Figure 2(b)) and the main surface 4b on the -Z side of film 4 (see Figure 2(e)) are activated by plasma irradiation or the like, and as shown in Figure 2(f), substrates 2 and 100 are positioned opposite each other in the Z direction so that the main surfaces 3a and 4b face each other. As shown in Figures 2(f), 5(a), and 6, the XY positions of substrate 2 and substrate 100 are aligned so that the XY positions of electrode PD1 on main surface 3a correspond to the XY positions of electrode PD2 on main surface 4b. As shown in Figures 5(a) and 6, substrates 2 and 100 are brought closer to each other in the Z direction, and the main surface 3a on substrate 2 and the main surface 4b on substrate 100 are joined by direct bonding. At this time, the atoms on the main surface 3a and the atoms on the main surface 4b are bonded by hydrogen bonds or the like, and the substrate 2 and the substrate 100 are in a state of temporary bonding.
[0033] Therefore, as shown in Figure 1, a heat treatment (annealing) is performed at a relatively low temperature (S7). During the heat treatment (annealing), substrates 2 and 100 are heated as a whole, as shown by the dotted arrows in Figure 5(b). During the heat treatment, for example, substrates 2 and 100 are heated to a relatively low temperature (i.e., the allowable temperature of the device structure, for example, around 200°C) for a predetermined time. At this time, due to the removal of water molecules from the interface, the atoms on the main surface 3a and the atoms on the main surface 4b are bonded by covalent bonds, etc., and substrates 2 and 100 become fully bonded. This forms the bonded body CB of substrates 2 and 100. At this time, electrodes PD1 and PD2 are directly bonded, and the peripheral circuit structure PHC and the memory cell array structure MAR can be electrically connected.
[0034] Once S7 shown in Figure 1 is completed, laser light 200 is shone from the substrate 100 side so that the focal point is located near the film 4 (S8).
[0035] In this embodiment, one irradiation of the laser beam 200 includes the irradiation of the entire substrate by the first laser beam 200 to the Nth laser beam 200. N is any integer of 2 or more.
[0036] The laser light irradiation is performed with laser light 200 whose wavelength band is greater than that of the substrate 100 (preferably 1117 nm or higher, more preferably around 9300 nm or 10600 nm, etc., when the laser absorption layer is a silicon oxide film). A pulsed laser is used for the laser light 200. An infrared laser may be used for the laser light 200. A carbon dioxide laser (CO2 laser) may be used for the laser light 200. The absorption of the laser light 200 depends on the absorption coefficient and thickness of the substrate or film, and in this structure, the greatest laser absorption occurs in the film 4, which is the laser absorption layer.
[0037] In this case, the laser beam 200 is irradiated in a two-dimensional manner within the film 4, with a spot area 201 having a diameter larger than the average arrangement pitch P of the protrusions 101, as shown in Figure 7. This reduces the number of irradiations N in a single laser beam 200 irradiation compared to the case where the diameter of the spot area 201 is equal to the average arrangement pitch P of the protrusions 101, thereby shortening the time required for the laser irradiation process to peel off the substrate 100.
[0038] The spot region 201 refers to the area illuminated by the beam of laser light 200 at its focal plane. In Figure 7, the spot region 201 is shown enclosed by a dashed line.
[0039] The spot area 201 of the laser beam 200 may have a substantially circular shape in an XY plane view. When the spot area 201 has a substantially circular shape, the diameter of the spot area 201 will be called the spot diameter. The spot diameter D of the laser beam 200 is greater than the average arrangement pitch P of the protrusions 101 on the main surface 100b of the substrate 100 (see Figure 4). The spot diameter D of each spot area 201 may be approximately constant or may vary within the 9th range. Figure 7 illustrates an irradiation pattern in which the spot diameter D of each spot area 201 is approximately constant. The average spot diameter D of the spot areas 201 may be a value within the 10th range (for example, 10 μm to 1000 μm). The average spot diameter D of the spot areas 201 may be the summation average of the spot diameters D of multiple spot areas 201.
[0040] The XY distance between the centers of adjacent spot regions 201 in multiple spot regions 201 is called the irradiation pitch. The irradiation pitch LP of multiple spot regions 201 may be approximately constant or may vary within the 11th range. Figure 7 illustrates an irradiation pattern in which the irradiation pitches LP_1 to LP_n of multiple spot regions 201 are approximately constant. The average irradiation pitch LP of a spot region 201 may be a value within the 12th range (e.g., 10 μm to 1000 μm). The average irradiation pitch LP of a spot region 201 may be the summation average of the irradiation pitches LP_1 to LP_n of multiple spot regions 201.
[0041] The spot area 201 of the laser beam 200 overlaps with two or more protrusions 101 when viewed from the Z direction. The spot area 201 of the laser beam 200 may contain two or more protrusions 101 inside when viewed from the Z direction. The number of protrusions 101 contained in each of the multiple spot areas 201 may be approximately constant or may vary within the 13th range. Figure 7 illustrates an irradiation pattern in which the number of protrusions 101 contained in each of the multiple spot areas 201 is approximately constant (e.g., 3). The average number of protrusions 101 contained in the spot area 201 may be a value within the 14th range (e.g., 100 to 1000). The average number of protrusions 101 contained in the spot area 201 may be the summation average of the number of protrusions 101 contained in each of the multiple spot areas 201. The pitch P of the protrusions 101 is preferably constant, and accordingly, the spot region 201 may move while overlapping so that a certain number of protrusions 101 are included in the spot region 201.
[0042] The irradiation of the laser light 200 may be performed while the spot area 201 moves along a helical trajectory OB shown by a dotted line in Figure 7. In a laser irradiation apparatus (not shown) having a stage and a light source, the bonded body CB of the substrate 2 and the substrate 100 (see Figure 5(b)) is placed on the stage, and as the stage rotates, the light source gradually moves from the outer periphery to the center of the substrate, thereby realizing an irradiation pattern of the spot area 201 moving from the outer periphery to the center along the helical trajectory OB.
[0043] Furthermore, in a laser irradiation device having a stage and a light source, the light source may gradually move from the center position of the substrate to the outer periphery position while the stage is rotated. In this case, it is possible to realize an irradiation pattern of a spot region 201 that moves from the center position to the outer periphery position along a helical trajectory OB.
[0044] For example, as shown in Figure 8(a), the XY plane position to which the first laser beam 200-1 should be irradiated is determined, and the focal point of the laser beam 200-1 is adjusted to be located within the film 4. The XY plane position to be irradiated may also be the starting position of the helical trajectory OB (see Figure 7). The absorption rate of the laser beam 200-1 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200-1 irradiated onto the film 4 through the substrate 100 is efficiently absorbed at the irradiated location within the film 4, causing localized heating of the film 4 at that XY plane position.
[0045] The localized heat generated by the film 4 is transferred to the interface between the film 4 and the substrate 100, as shown in Figure 8(b). The thermal expansion coefficient of the substrate 100 is greater than that of the film 4, and therefore the substrate 100 expands toward the film 4 at its XY plane position.
[0046] At this time, as shown in Figure 9(c), the interface between the film 4 and the substrate 100 contains multiple protrusions 101 within the spot region 201. The tips of the protrusions 101 are in three-dimensional contact with the film 4 on the -Z side and the outer circumference in the XY direction, while the bottom surfaces of the recesses 102 located around the protrusions 101 are in planar contact with the film 4 on the -Z side. As shown by the dotted arrows in Figure 9(c), the amount of heat transferred from the film 4 to the tips of the protrusions 101 is greater than the amount of heat transferred from the film 4 to the bottom surfaces of the recesses 102.
[0047] As shown in Figure 9(d), the expansion amount Δh is the amount by which the tip of the protrusion 101a expands toward the film 4. 101 This is the amount of expansion Δh, which is the amount by which the bottom surface of the recess 102 expands toward the side of the film 4. 102 It becomes larger. As a result, compressive stress is generated at the interface between the tip of the protrusion 101a and the film 4, while tensile stress is generated at the interface between the bottom surface of the recess 102 and the film 4.
[0048] Expansion amount Δh 101 and expansion amount Δh 102 The difference occurs at multiple locations in the XY direction within the spot region 201. As a result, tensile stress at the interface between the bottom surface of the recess 102 and the film 4 occurs at multiple locations in the XY direction within the spot region 201.
[0049] Furthermore, the height ha of the protrusion 101a within the spot region 201 is higher than the height h of the protrusion 101 outside the spot region 201 (ha > h).
[0050] As shown in Figure 8(c), the XY plane position to which the second laser beam 200-2 should be irradiated is determined to be a position shifted in the XY plane direction from the XY plane position in Figure 8(a), and the focal point of the laser beam 200-2 is adjusted to be located within the film 4. The position shifted in the XY plane direction from the XY plane position in Figure 8(a) may also be a position shifted from its starting position along the helical trajectory OB (see Figure 7). The absorption rate of the laser beam 200-2 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200-2 irradiated into the film 4 through the substrate 100 is efficiently absorbed at the irradiated location within the film 4, causing local heating of the film 4 at that XY plane position.
[0051] The localized heat generated by the film 4 is transferred to the interface between the film 4 and the substrate 100, as shown in Figure 10(a). The thermal expansion coefficient of the substrate 100 is greater than that of the film 4, and therefore the substrate 100 expands toward the film 4 at its XY plane position.
[0052] At this time, as shown in Figure 9(c), the interface between the film 4 and the substrate 100 contains multiple protrusions 101 within the spot region 201. The tips of the protrusions 101 are in three-dimensional contact with the film 4 on the -Z side and the outer circumference in the XY direction, while the bottom surfaces of the recesses 102 located around the protrusions 101 are in planar contact with the film 4 on the -Z side. As shown by the dotted arrows in Figure 9(c), the amount of heat transferred from the film 4 to the tips of the protrusions 101 is greater than the amount of heat transferred from the film 4 to the bottom surfaces of the recesses 102.
[0053] As shown in Figure 9(d), the expansion amount Δh is the amount by which the tip of the protrusion 101a expands toward the film 4. 101 This is the amount of expansion Δh, which is the amount by which the bottom surface of the recess 102 expands toward the side of the film 4. 102It becomes larger. As a result, compressive stress is generated at the interface between the tip of the protrusion 101a and the film 4, while tensile stress is generated at the interface between the bottom surface of the recess 102 and the film 4.
[0054] Expansion amount Δh 101 and expansion amount Δh 102 The difference occurs at multiple locations in the XY direction within the spot region 201. As a result, tensile stress at the interface between the bottom surface of the recess 102 and the film 4 occurs at multiple locations in the XY direction within the spot region 201.
[0055] Furthermore, the height ha of the protrusion 101a within the spot region 201 is higher than the height h of the protrusion 101 outside the spot region 201 (ha > h).
[0056] As shown in Figure 10(b), the final XY plane position to which the Nth laser beam 200-N should be irradiated is determined, and the focal point of the laser beam 200-N is adjusted to be located within the film 4. The final XY plane position may also be the final position along the helical trajectory OB (see Figure 7). The absorption rate of the laser beam 200-N in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200-N irradiated onto the film 4 through the substrate 100 is efficiently absorbed at the irradiated location within the film 4, causing localized heating of the film 4 at the final XY plane position.
[0057] The localized heat generated by the film 4 is transferred to the interface between the film 4 and the substrate 100, as shown in Figure 10(c). The thermal expansion coefficient of the substrate 100 is greater than that of the film 4, and therefore, at the final XY plane position, the substrate 100 expands toward the film 4.
[0058] At this time, as shown in FIG. 9(c), the spot region 201 includes a plurality of protrusions 101 at the interface between the film 4 and the substrate 100. The tip of each protrusion 101 three-dimensionally contacts the film 4 on the −Z side and on the outer peripheral side in the XY directions, while the bottom surface of each recess 102 located around the protrusion 101 planarly contacts the film 4 on the −Z side. As indicated by dotted arrows in FIG. 9(c), the amount of heat transferred from the film 4 to the tip of the protrusion 101 is larger than the amount of heat transferred from the film 4 to the bottom surface of the recess 102.
[0059] As shown in FIG. 9(d), an expansion amount Δh by which the tip of the protrusion 101a expands toward the film 4 101 is larger than an expansion amount Δh by which the bottom surface of the recess 102 expands toward the film 4 102 . As a result, compressive stress is generated at the interface between the tip of the protrusion 101a and the film 4, while tensile stress is generated at the interface between the bottom surface of the recess 102 and the film 4.
[0060] A difference between the expansion amount Δh 101 and the expansion amount Δh 102 occurs at a plurality of positions in the XY directions within the spot region 201. As a result, the tensile stress at the interface between the bottom surface of the recess 102 and the film 4 is generated at a plurality of positions in the XY directions within the spot region 201.
[0061] Further, the height ha of the protrusion 101a within the spot region 201 is larger than the height h before expansion (ha>h).
[0062] The laser light 200 is applied such that the plurality of spot regions 201 are two-dimensionally distributed in the film 4, so that, as indicated by dotted arrows in FIG. 11, tensile stress is generated at the bottom surfaces of the plurality of recesses 102 that are two-dimensionally distributed.
[0063] As a result, delamination occurs at the interface between the film 4 and the substrate 100 (S9). During delamination, as shown in Figure 12(a), the substrate 100 is peeled off the laminate 6 in which the films 3 and 4 are laminated on the substrate 2. For example, since tensile stress is generated at the bottom surfaces of the multiple recesses 102 which are distributed in two dimensions, the substrate 100 is easily peeled off the laminate 6 starting from the bottom surfaces of the multiple recesses 102.
[0064] Considering subsequent processing, the laminate 6 is treated at the delamination surface as shown in Figure 1 (S10). In the laminate 6, as shown in Figure 12(b), multiple protrusions 4a2 are distributed in the XY direction on the main surface 4a on the +Z side of the film 4. The main surface 4a is polished and flattened by CMP or the like.
[0065] As a result, as shown in Figure 12(c), films 3 and 4 are laminated on the substrate 2, and a semiconductor device 1 is obtained in which the main surface 4a of film 4 is flattened.
[0066] For example, as shown in Figure 13, after planarization, a conductive plug PG is formed that is electrically connected to the conductive layer SL by creating a hole in the main surface 60a on the +Z side of the interlayer insulating film 60 and embedding a conductive material. An electrode pattern EL that is electrically connected to the conductive plug PG is formed on the main surface 60a of the interlayer insulating film 60 by plating or the like. In addition, although not shown, an electrode pattern EL that is connected to the peripheral circuit structure PHC by bypassing the memory cell array structure MAR is also formed on the main surface 60a of the interlayer insulating film 60. This makes it possible to supply power, signals, etc. from the outside to the memory cell array structure MAR and the peripheral circuit structure PHC.
[0067] Furthermore, the film 4 containing the memory cell array structure MAR can be considered as a chip region for the memory cell array, and the film 3 containing the peripheral circuit structure PHC and the substrate 2 can be considered as chip regions for the peripheral circuits. The semiconductor device 1 has a structure obtained by directly bonding a chip region for the memory cell array and a chip region for the peripheral circuits. This structure is also called CBA (CMOS directly bonded to array). In CBA, the number of chip regions for the memory cell array bonded to the +Z side of the chip region for the peripheral circuits is not limited to one, but may be two or more.
[0068] On the other hand, the peeled substrate 100 is reused as shown in Figure 1 (S11). The substrate 100 may also be reused as the upper substrate 100, as shown by the solid arrows in Figure 2.
[0069] Immediately after peeling, the substrate 100 has multiple protrusions 101a distributed in the XY direction on the main surface 100b on the -Z side, as shown in Figure 12(d). The main surface 100b is polished and flattened by a CMP method or the like. As a result, a substrate 100 with a flattened main surface 100b is obtained, as shown in Figure 12(e). Since the main surface 100b of the substrate 100 shown in Figure 12(e) is flattened, it can be easily reused, for example, as a top substrate 100.
[0070] Alternatively, the peeled substrate 100 may be reused as the lower substrate 2, as shown by the dotted arrow in Figure 1, instead of being reused as the upper substrate 100.
[0071] As described above, in the first embodiment, in the method for manufacturing the semiconductor device 1, a plurality of protrusions are formed on the main surface 100b of the upper substrate 100, distributed two-dimensionally. Subsequently, the laser light 200 is irradiated in a spot region 201 with a diameter larger than the average arrangement pitch P of the protrusions 101, so as to be distributed two-dimensionally within the film 4, and peeling is performed. As a result, the irradiation of the laser light 200 can generate a difference in the amount of thermal expansion between the tip of the protrusion and the bottom surface of the surrounding recess, and tensile stress can be efficiently generated at the bottom surface of the recess. Furthermore, since a difference in the amount of thermal expansion and the resulting tensile stress can be generated at multiple locations within the spot region 201 with a single laser irradiation, the number of irradiations N in a single laser light 200 can be reduced compared to the case where the diameter of the spot region 201 is equal to the average arrangement pitch P, and the time required for the laser irradiation process to peel the substrate 100 can be shortened. Therefore, the throughput of laser peeling can be efficiently improved.
[0072] Furthermore, according to the first embodiment, the number of irradiations N in a single laser beam 200 can be reduced. This reduces the amount of heat reaching the device structure (for example, the device structure shown in Figure 6) within the film 4 and / or film 3 during the laser irradiation process until the substrate 100 is peeled off, thereby suppressing thermal damage to the device structure.
[0073] For example, as a comparative example, consider a manufacturing method for semiconductor device 1 in which, as shown in Figure 9(a), multiple protrusions distributed two-dimensionally on the main surface 800a of the upper substrate 800 are not formed before irradiation with laser light 900. In this case, by irradiating each of the desired multiple locations with laser light 900 having a spot diameter equal in size to each of the desired multiple locations, approximately the same number of protrusions 901 as the number of irradiations are formed, as shown in Figure 9(b). Compressive stress is generated at the interface between the tip of the protrusion 901 and the film 704, but tensile stress is generated at the interface between the recess 902 located around the protrusion 901 and the film 704. That is, since the same number of irradiations of laser light 900 as the number of locations where tensile stress is to be generated are performed, the time required for the laser irradiation process to peel off the substrate 800 tends to be prolonged.
[0074] In this regard, our investigation revealed that when the time interval between laser beam 900 irradiations is shortened (or the irradiation frequency is increased) in accordance with the increase in the number of laser beam 900 irradiations, the substrate is less likely to be cooled due to thermal interference between multiple points irradiated by the laser beam 900, disrupting the periodicity of the shape that expands toward the film 704 at each point, and making it difficult to form recesses 902. In this case, since almost no tensile stress is generated at the interface between the substrate 900 and the film 704, it becomes difficult to peel off the substrate 800 itself. In other words, it is difficult to shorten the laser irradiation process by shortening the time interval between laser beam 900 irradiations.
[0075] On the other hand, in the first embodiment, as shown in Figure 9(c), multiple protrusions distributed two-dimensionally are formed on the surface of the upper substrate 100 before irradiation with the laser beam 200. As a result, as shown in Figures 9(c) and 9(d), a single irradiation of the laser beam can generate differences in thermal expansion and the resulting tensile stress at multiple locations within the spot region 201. This means that fewer irradiations of the laser beam 900 are required than the number of locations where tensile stress is to be generated. For example, if there are five locations where tensile stress is to be generated, in Figure 9(a), five irradiations of laser beams 900-1 to 900-5 are performed, but in Figure 9(c), only two irradiations of laser beams 200-1 and 200-2 are required. As a result, the number of irradiations N of the laser beam 200 can be reduced, and the time required for the laser irradiation process to peel off the substrate 100 can be shortened.
[0076] Furthermore, in the manufacturing method of the semiconductor device 1, if multiple protrusions distributed two-dimensionally are not formed on the surface of the upper substrate 800 before irradiation with laser light 900, the amount of heat transferred to the substrate 800 when irradiated with laser light 900 is limited, as shown by the dotted arrow in Figure 9(a). For this reason, as shown in Figure 9(b), the thermal expansion amount Δh of the tip of the protrusion 901 is limited. 901 The difference between the thermal expansion of the recess 902 and the amount of thermal expansion of the bottom surface (≒0) becomes relatively small, and the tensile stress at the bottom surface of the recess tends to be small.
[0077] On the other hand, in the first embodiment, as shown in Figure 9(d), a plurality of protrusions 101 are formed on the surface of the upper substrate 100 in a two-dimensional manner, so the expansion amount Δh of the tip of the protrusion 101a 101 and the amount of expansion Δh of the bottom surface of the recess 102 102 This makes it easier to secure a large difference. As a result, tensile stress can be efficiently generated on the bottom surface of the recess 102.
[0078] (First modification of the first embodiment) As a first modification of the first embodiment, the shape of the spot area 201 of the laser light 200 may be a shape other than a substantially circular shape in an XY plane view, and may include any shape suitable for laser peeling. The shape of the spot area 201p of the laser light 200p may not be constant during a single irradiation of the laser light 200p, and may change between the first irradiation of the laser light 200p and the Nth irradiation of the laser light 200p.
[0079] For example, if N is a multiple of 3, as shown in Figure 14, the spot area 201p of the first laser beam 200p-1 to (1 / 3)N laser beam 200p-(1 / 3)N may be a relatively large trapezoidal shape, the spot area 201p of the {(1 / 3)N+1} laser beam 200p-(1 / 3)N to (2 / 3)N laser beam 200p-(2 / 3)N may be a slightly smaller trapezoidal shape, and the spot area 201p of the {(2 / 3)N+1} laser beam 200p-(2 / 3)N to N laser beam 200p-N may be a small triangular shape. In the case shown in Figure 14, one irradiation of laser beam 200p can be performed in a manner in which the spot area 201p is efficiently spread across the substrate 100.
[0080] (Second modification of the first embodiment) As a second modification of the first embodiment, the formation of the protrusion (S4) may be performed by processing the film 5 disposed on the substrate 100, instead of by processing the main surface 100b of the substrate 100, as shown in Figure 15. Figures 15(a) to 15(f) are YZ cross-sectional views showing a method for manufacturing the semiconductor device 1 according to the second modification of the first embodiment.
[0081] The preparation of the lower substrate (S1) shown in Figure 15(a) and the film deposition (S2) shown in Figure 15(b) are carried out in the same manner as in the first embodiment.
[0082] In the preparation of the upper substrate (S3), as shown in Figure 15(c), the substrate (upper substrate) 100 is prepared, and a film 5 is deposited on the main surface 100b of the substrate 100 by CVD or the like. The film 5 may be formed from a material mainly composed of a semiconductor nitride (e.g., silicon nitride), or from a material mainly composed of a semiconductor (e.g., polysilicon). Alternatively, the film 5 may be epitaxially grown on the main surface 100b of the substrate 100. The film 5 may be formed from a material mainly composed of a semiconductor (e.g., silicon).
[0083] In the formation of the protrusions (S4), the process may be carried out by processing the film 5, as shown in Figure 15(d). Multiple protrusions 51 are formed on the film 5 by dry etching such as the RIE method. For example, a photosensitive agent is applied to the main surface 5b of the film 5, and a resist pattern RP (not shown) is formed by exposure and development, which selectively covers multiple regions on the main surface 5b corresponding to the multiple protrusions 51. Using the resist pattern RP as a mask, etching is performed under anisotropic etching conditions using the RIE method or the like to form multiple protrusions 51 on the main surface 100b of the substrate 100.
[0084] Similar to the first embodiment, the multiple protrusions 51 are formed so as to be distributed in the XY direction on the main surface 100b, as shown in Figure 4.
[0085] In film formation (S5), as shown in Figure 15(e), a film 4 covering multiple protrusions 51 is deposited by CVD or the like.
[0086] Once the processing of the lower substrate (S1-S2) and the upper substrate (S3-S5) is completed, the upper and lower substrates are joined together (S6). The main surface 3a on the +Z side of film 3 and the main surface 4b on the -Z side of film 4 are activated by plasma irradiation or the like, and as shown in Figure 15(f), substrates 2 and 100 are positioned facing each other in the Z direction so that the main surfaces 3a and 4b face each other. As shown in Figure 5(a), substrates 2 and 100 are brought closer to each other in the Z direction, and the main surface 3a on the substrate 2 side and the main surface 4b on the substrate 100 side are joined together.
[0087] Then, the process from S7 onwards shown in Figure 1 is carried out in the same manner as in the first embodiment.
[0088] This process can also form multiple protrusions 51 that are distributed two-dimensionally on the main surface 100b of the upper substrate 100.
[0089] (Third modification of the first embodiment) As a third modification of the first embodiment, the formation of the protrusion (S4) may be performed by processing the film 5 disposed on the substrate 100 via the film 7, instead of by processing the main surface 100b of the substrate 100, as shown in Figure 16. Figures 16(a) to 16(g) are YZ cross-sectional views showing a method for manufacturing the semiconductor device 1 according to the third modification of the first embodiment.
[0090] The preparation of the lower substrate (S1) shown in Figure 16(a) and the film deposition (S2) shown in Figure 16(b) are carried out in the same manner as in the first embodiment.
[0091] In the preparation of the upper substrate (S3), as shown in Figure 16(c), the substrate (upper substrate) 100 is prepared, and a film 7 is deposited on the main surface 100b of the substrate 100 by CVD or the like. The film 7 may be formed from a material mainly composed of semiconductor nitride (for example, silicon nitride).
[0092] As shown in Figure 16(d), film 5 is deposited on the main surface 7b of film 7 by CVD or the like. Film 5 may be formed from a material mainly composed of a semiconductor (for example, polysilicon).
[0093] In the formation of the protrusions (S4), the film 5 may be processed as shown in Figure 16(e). Multiple protrusions 51 are formed on the film 5 by dry etching such as the RIE method. For example, a photosensitive agent is applied to the main surface 5b of the film 5, and a resist pattern RP (not shown) is formed by exposure and development, which selectively covers multiple regions on the main surface 5b corresponding to the multiple protrusions 51. Using the resist pattern RP as a mask, etching is performed under anisotropic etching conditions using the RIE method or the like to form multiple protrusions 51 on the main surface 7b of the film 7.
[0094] Similar to the first embodiment, the multiple protrusions 51 are formed so as to be distributed in the XY direction on the main surface 100b, as shown in Figure 4.
[0095] In film formation (S5), as shown in Figure 16(f), a film 4 covering multiple protrusions 51 is deposited on the main surface 7b of the film 7 by a method such as CVD.
[0096] Once the processing of the lower substrate (S1-S2) and the upper substrate (S3-S5) is completed, the upper and lower substrates are joined together (S6). The main surface 3a on the +Z side of film 3 and the main surface 4b on the -Z side of film 4 are activated by plasma irradiation or the like, and as shown in Figure 16(g), substrates 2 and 100 are positioned opposite each other in the Z direction so that the main surfaces 3a and 4b face each other. As shown in Figure 5(a), substrates 2 and 100 are brought closer to each other in the Z direction, and the main surface 3a on substrate 2 and the main surface 4b on substrate 100 are joined together.
[0097] Then, the process from S7 onwards shown in Figure 1 is carried out in the same manner as in the first embodiment.
[0098] Even through this process, multiple protrusions 51 distributed two-dimensionally on the main surface 100b side of the upper substrate 100 can be formed.
[0099] (Second embodiment) Next, a method for manufacturing the semiconductor device 1 according to the second embodiment will be described. The following description will focus on the differences from the first embodiment.
[0100] As mentioned above, when the time interval between laser beam 900 irradiations is shortened in response to an increase in the number of laser beam irradiations as shown in Figure 9(a), the substrate is less likely to be cooled due to thermal interference between multiple locations irradiated by the laser beam 900, disrupting the periodicity of the shape that expands toward the film 704 at each location, and making it difficult to form recesses 902. In this case, since almost no tensile stress is generated at the interface between the substrate 900 and the film 704, it becomes difficult to peel off the substrate 800 itself.
[0101] Therefore, in the second embodiment, as shown in Figure 20 described later, the laser beam 200i is irradiated in a segmented irradiation along the trajectory OB1, aiming to improve the throughput of laser delamination while suppressing thermal interference between irradiation points.
[0102] In this embodiment, one irradiation of laser light 200i includes the irradiation of the first laser light 200 onto the entire substrate to the irradiation of the K × Nth laser light 200. K is any integer of 2 or more. N is any integer of 2 or more. Divided irradiation means dividing one irradiation of laser light 200i into K irradiations of laser light, each including the irradiation of the first laser light 200 onto the entire substrate to the irradiation of the Nth laser light 200.
[0103] For example, the method for manufacturing the semiconductor device 1 differs from the first embodiment in the following respects, as shown in Figures 17 to 22. Figure 17 is a flowchart of the method for manufacturing the semiconductor device 1. Figures 18(a) to 18(f), 19(a) to 19(b), 21(a) to 21(c), and 22 are YZ cross-sectional views showing the method for manufacturing the semiconductor device 1. Figures 20(a) to 20(c) are XY plan views showing the divided irradiation pattern.
[0104] In the manufacturing method of semiconductor device 1, as shown in Figure 17, S4 (see Figure 1) is omitted, and S21 to S22 are added in place of S8 (see Figure 1).
[0105] The preparation of the lower substrate (S1) shown in Figure 18(a) and the film deposition (S2) shown in Figure 18(b) are carried out in the same manner as in the first embodiment.
[0106] The preparation of the upper substrate (S3) shown in Figure 18(c) is carried out in the same manner as in the first embodiment, but the film deposition (S5) differs from the first embodiment in that the film 4 is deposited on the flat main surface 100b of the substrate 100, as shown in Figure 18(d).
[0107] Once the processing of the lower substrate (S1-S2) and the upper substrate (S3-S5) is completed, the upper and lower substrates are joined together (S6). The main surface 3a on the +Z side of film 3 and the main surface 4b on the -Z side of film 4 are activated by plasma irradiation or the like, and as shown in Figure 18(e), substrates 2 and 100 are positioned opposite each other in the Z direction so that the main surfaces 3a and 4b face each other. As shown in Figure 19(a), substrates 2 and 100 are brought closer to each other in the Z direction, and the main surface 3a on substrate 2 and the main surface 4b on substrate 100 are joined together.
[0108] Subsequently, as shown in Figure 1, a heat treatment (annealing) is performed at a relatively low temperature (S7). During the heat treatment (annealing), substrates 2 and 100 are heated overall, as indicated by the dotted arrows in Figure 19(b). This forms the bond CB of substrates 2 and 100.
[0109] Once S7 shown in Figure 17 is completed, laser light 200i is irradiated from the substrate 100 side so that the focal point is located near the film 4 (S21).
[0110] In this case, the irradiation of the laser beam 200i may be performed in K fractions along the trajectory OB1, where K is an integer greater than or equal to 2. A parameter may be provided to count the number of fractions. For example, for the first fraction, the parameter may be set to an initial value of 1, and the parameter may be incremented each time the number of fractions increases.
[0111] The K-division irradiation pattern may be such that the starting positions are offset from each other by a distance corresponding to the dimensions of the spot area of one irradiation, and the spot areas are aligned along the trajectory OB1 at a pitch corresponding to K times the dimensions of the spot area of one irradiation. The trajectory OB1 may be helical when viewed from the Z direction.
[0112] For example, when K=3, irradiation patterns as shown in Figures 20(a) to 20(c) may be realized. Figure 20(a) illustrates the first fractionated irradiation pattern, Figure 20(b) illustrates the second fractionated irradiation pattern, and Figure 20(c) illustrates the third fractionated irradiation pattern. Figures 20(a) to 20(c) illustrate the case where each spot region 201i has a circular shape.
[0113] As shown in Figures 20(a) to 20(c), the first, second, and third fractionated irradiation patterns are offset from each other by a distance corresponding to the spot diameter Di of the spot area 201i of the first irradiation.
[0114] As shown in Figure 20(a), in the first fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB1 at a pitch equivalent to three times the spot diameter Di of one irradiation. As shown in Figure 20(b), in the second fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB1 at a pitch equivalent to three times the spot diameter Di of one irradiation. As shown in Figure 20(c), in the third fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB1 at a pitch equivalent to three times the spot diameter Di of one irradiation.
[0115] This allows for increasing the spatial distance between temporally adjacent spot regions 201i during each fractional irradiation, thereby shortening the time interval between irradiations of laser light 900 (or increasing the irradiation frequency) while suppressing thermal interference between temporally adjacent spot regions 201i.
[0116] The number of laser beams 200i (i.e., the number of spot regions 201i) included in each divided irradiation pattern may be equal to each other. Furthermore, while an example of an irradiation pattern of spot regions 201i moving from the outer position to the central position along a helical trajectory OB1 is given, an irradiation pattern of spot regions 201i moving from the central position to the outer position along a helical trajectory OB1 may also be used.
[0117] For example, as shown in Figure 21(a), the XY plane position to which the first laser beam 200i-1 should be irradiated is determined, and the focal point of the laser beam 200i-1 is adjusted to be located within the film 4. The XY plane position to be irradiated may be the starting position shown in Figure 20(a) for the first split irradiation pattern. For the second split irradiation pattern, it may be the starting position shown in Figure 20(b). For the third split irradiation pattern, it may be the starting position shown in Figure 20(c). The absorption rate of the laser beam 200-1 in the film 4 is greater than that of the substrate 100. As a result, the laser beam 200-1 irradiated onto the film 4 through the substrate 100 is efficiently absorbed at the irradiated location within the film 4, causing local heating of the film 4 at that XY plane position.
[0118] As shown in Figure 21(b), the localized heat generation of the film 4 is transferred to the interface between the film 4 and the substrate 100. The thermal expansion coefficient of the substrate 100 is greater than that of the film 4, and therefore the substrate 100 expands toward the film 4 at its XY plane position. As a result, a convex portion 101i protruding toward the -Z side is formed on the main surface 100b of the substrate 100 at its XY plane position. Consequently, compressive stress is generated at the interface between the tip of the convex portion 101i and the film 4, while tensile stress is generated at the interface between the bottom surface of the recess 102i located around the convex portion 101i and the film 4.
[0119] As shown in Figure 21(c), the XY plane position to which the second laser beam 200i-2 should be irradiated is determined to be a position shifted in the XY plane direction from the XY plane position in Figure 21(a), and the focal point of the laser beam 200i-2 is adjusted to be located within the film 4. The position shifted in the XY plane direction from the XY plane position in Figure 21(a) may be a position shifted along the trajectory OB1 from the starting position shown in Figure 20(a) at a pitch corresponding to three times the spot diameter Di for the first split irradiation pattern. For the second split irradiation pattern, it may be a position shifted along the trajectory OB1 from the starting position shown in Figure 20(b) at a pitch corresponding to three times the spot diameter Di for the second split irradiation pattern. For the third split irradiation pattern, it may be a position shifted along the trajectory OB1 from the starting position shown in Figure 20(c) at a pitch corresponding to three times the spot diameter Di for the third split irradiation pattern. The absorption rate of the laser beam 200i-2 in the film 4 is greater than the absorption rate of the laser beam 200i-2 in the substrate 100. As a result, the laser light 200i-2 irradiated onto the film 4 through the substrate 100 is efficiently absorbed at the irradiated location within the film 4, causing localized heating of the film 4 at that XY plane position.
[0120] The localized heat generated by the film 4 is transferred to the interface between the film 4 and the substrate 100, as shown in Figure 21(d). The thermal expansion coefficient of the substrate 100 is greater than that of the film 4, and therefore the substrate 100 expands toward the film 4 at its XY plane position.
[0121] In this case, the XY plane position in Figure 21(d) is separated from the XY plane position in Figure 21(b) by a pitch corresponding to three times the spot diameter Di, and thermal interference from the XY plane position in Figure 21(b) is suppressed.
[0122] Accordingly, at the XY plane position shown in Figure 21(d), the substrate 100 expands toward the film 4, and a convex portion 101i protruding toward the -Z side is formed on the main surface 100b of the substrate 100 at that XY plane position. As a result, compressive stress is generated at the interface between the tip of the convex portion 101i and the film 4, while tensile stress is generated at the interface between the bottom surface of the recess 102i located around the convex portion 101i and the film 4.
[0123] Similarly, once the laser beam 200i has been irradiated up to the Nth fraction, it is determined whether the current fraction is the Kth fraction (S22). For example, a parameter for counting the number of fractions is checked, and if the value of the parameter is less than K, it is determined that the current fraction is not the Kth fraction (No in S22), and the process returns to S21.
[0124] As a result of the laser beam 200i being irradiated in the Kth fractional irradiation so that multiple spot regions 201i are distributed two-dimensionally within the film 4, tensile stress is generated at the bottom surface of multiple two-dimensionally distributed recesses 102i, as shown by the dotted arrows in Figure 22.
[0125] For example, a parameter for counting the number of fractional irradiations is checked, and if the value of the parameter is K or greater, the current fractional irradiation is considered to be the Kth fractional irradiation (Yes in S22), and delamination is performed at the interface between the film 4 and the substrate 100 (S9). Delamination is performed in the same manner as in the first embodiment.
[0126] On the other hand, the peeled substrate 100 is reused as shown in Figure 17 (S11). The substrate 100 may be reused as the upper substrate 100, as shown by the solid arrows in Figure 17. The reuse is carried out in the same manner as in the first embodiment.
[0127] Alternatively, the peeled substrate 100 may be reused as the lower substrate 2, as shown by the dotted arrow in Figure 17, instead of being reused as the upper substrate 100.
[0128] As described above, in the second embodiment, in the manufacturing method of the semiconductor device 1, the irradiation of the laser light 200i is performed by segmented irradiation along the start OB1. This makes it possible to shorten the time interval of irradiation of the laser light 200i (or increase the irradiation frequency) while suppressing thermal interference between irradiation points. As a result, the throughput of laser peeling can be improved.
[0129] As shown in Figures 20(a) to 20(c), in the helical trajectory OB1, as the radius decreases from the outer periphery to the center, the XY distance to the spot region 201i that is temporally close (for example, 1 to 3 times earlier) tends to decrease. Consequently, as the laser beam approaches the center from the outer periphery, it becomes more difficult to shorten the irradiation time interval of the laser beam 200i while keeping it constant, potentially complicating the control of the irradiation time interval of the laser beam 200i.
[0130] (First modification of the second embodiment) Taking this into consideration, as a first modification of the second embodiment, the K-fold divided irradiation may be performed using a linear trajectory OB2, as shown in Figure 23. Figure 23 is an XY plan view showing the divided irradiation pattern in the first modification of the second embodiment.
[0131] For example, when K=3, irradiation patterns as shown in Figures 23(a) to 23(c) may be realized. Figure 23(a) illustrates the first fractionated irradiation pattern, Figure 23(b) illustrates the second fractionated irradiation pattern, and Figure 23(c) illustrates the third fractionated irradiation pattern. Figures 23(a) to 23(c) illustrate the case where each spot region 201i has a circular shape.
[0132] As shown in Figures 23(a) to 23(c), multiple orbitals OB2-1 to OB2-M are used for K fractional irradiation. M is any integer of 2 or more. The multiple orbitals OB2-1 to OB2-M extend approximately parallel to each other and are arranged at approximately constant intervals in a direction perpendicular to the direction of their extension. In the case of Figures 23(a) to 23(c), each orbital OB2-1 to OB2-M extends in the Y direction. The multiple orbitals OB2-1 to OB2-M are arranged at approximately constant intervals in the X direction. The spacing of the arrangement of the multiple orbitals OB2-1 to OB2-M may correspond to the spot diameter Di of the spot region 201i.
[0133] The laser beam 200i may be irradiated in one direction, sequentially along the orbits OB2-1 to OB2-M. Figures 23(a) to 23(c) illustrate the case where the laser beam 200i is irradiated along each orbit OB2 from the +Y side to the -Y side, but the laser beam 200i may also be irradiated along each orbit OB2 from the -Y side to the +Y side.
[0134] As shown in Figures 23(a) to 23(c), the first, second, and third fractionated irradiation patterns are offset from each other by a distance corresponding to the spot diameter Di of the spot area 201i of the first irradiation.
[0135] As shown in Figure 23(a), in the first fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Di of one irradiation. As shown in Figure 23(b), in the second fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Di of one irradiation. As shown in Figure 23(c), in the third fractionated irradiation pattern, the spot regions 201i are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Di of one irradiation.
[0136] This also allows for increasing the spatial distance between temporally adjacent spot regions 201i during each fractional irradiation, thereby shortening the time interval between irradiations of the laser beam 200i (or increasing the irradiation frequency) while suppressing thermal interference between temporally adjacent spot regions 201i.
[0137] (Second modification of the second embodiment) Alternatively, as a second modification of the second embodiment, the K-stage irradiation may be performed in a linear spot region 201j using a linear trajectory OB2, as shown in Figure 24. Figure 24 is an XY plan view showing the irradiation pattern in the second modification of the second embodiment.
[0138] For example, when K=3, irradiation patterns as shown in Figures 24(a) to 24(c) may be realized. Figure 24(a) illustrates the first segmented irradiation pattern, Figure 24(b) illustrates the second segmented irradiation pattern, and Figure 24(c) illustrates the third segmented irradiation pattern. Figures 24(a) to 24(c) illustrate cases where each spot region 201j has a line shape. Note that the size of the line-shaped irradiation pattern shown in Figure 24 is just an example; for example, the length in the longitudinal direction of the line shape may be approximately the same as the spot diameter shown in Figure 23, or larger than the spot diameter.
[0139] As shown in Figures 24(a) to 24(c), multiple orbitals OB2-1 to OB2-M are used for K fractional irradiation. M is any integer of 2 or more. The multiple orbitals OB2-1 to OB2-M extend approximately parallel to each other and are arranged at approximately constant intervals in a direction perpendicular to their extension. In the case of Figures 24(a) to 24(c), each orbital OB2-1 to OB2-M extends in the Y direction. The multiple orbitals OB2-1 to OB2-M are arranged at approximately constant intervals in the X direction. The spot region 201j extends in the X direction. The spacing of the arrangement of the multiple orbitals OB2-1 to OB2-M may correspond to the Y-direction width of the spot region 201j.
[0140] The laser beam of 200j may be irradiated in one direction, sequentially along the orbits OB2-1 to OB2-M. Figures 24(a) to 24(c) illustrate the case where the laser beam of 200j is irradiated along each orbit OB2 from the +Y side to the -Y side, but the laser beam of 200j may also be irradiated along each orbit OB2 from the -Y side to the +Y side.
[0141] As shown in Figures 24(a) to 24(c), the first, second, and third split irradiation patterns are offset from each other by a distance corresponding to the Y-direction width of the spot area 201j of the first irradiation. The Y-direction width of the spot area 201j may correspond to two locations where tensile stress is to be generated.
[0142] As shown in Figure 24(a), in the first fractionated irradiation pattern, the spot areas 201j are arranged along the trajectory OB2 at a pitch corresponding to three times the Y-direction width of the spot area 201j of one irradiation. As shown in Figure 24(b), in the second fractionated irradiation pattern, the spot areas 201j are arranged along the trajectory OB2 at a pitch corresponding to three times the Y-direction width of the spot area 201j of one irradiation. As shown in Figure 24(c), in the third fractionated irradiation pattern, the spot areas 201j are arranged along the trajectory OB2 at a pitch corresponding to three times the Y-direction width of the spot area 201j of one irradiation.
[0143] For example, as shown in Figure 25, consider an irradiation pattern in which spot regions 201j extending linearly in the X direction are arranged along the trajectory OB2-2 in the X direction at a pitch corresponding to three times the Y-direction width of the spot regions 201j.
[0144] When the spot region 201j of the laser beam 200j-k of any k irradiation time is irradiated, compressive stress is generated on the main surface 100b of the substrate 100 in the region overlapping with the spot region 201j when viewed from the Z direction, as shown by the dotted line in Figure 25. k is an arbitrary integer. On the main surface 100b of the substrate 100, tensile stress is generated on both sides of the spot region 201j in the Y direction when viewed from the Z direction, as shown by the dashed line in Figure 25.
[0145] When the spot area 201j of the k+1th laser beam 200j-(k+1) is irradiated, compressive stress is generated on the main surface 100b of the substrate 100 in the region overlapping with the spot area 201j when viewed from the Z direction, as shown by the dotted line in Figure 25. Tensile stress is generated on the main surface 100b of the substrate 100 in the regions adjacent to the spot area 201j on both sides in the Y direction, as shown by the dashed line in Figure 25.
[0146] When the spot region 201j of the k+4th laser beam 200j-(k+4) is irradiated, compressive stress is generated on the main surface 100b of the substrate 100 in the region overlapping with the spot region 201j when viewed from the Z direction, as shown by the dotted line in Figure 25. Tensile stress is generated on the main surface 100b of the substrate 100 in the regions adjacent to the spot region 201j on both sides in the Y direction, as shown by the dashed line in Figure 25.
[0147] This also allows for increasing the spatial distance between temporally adjacent spot regions 201j during each fractional irradiation, thereby shortening the time interval between irradiations of the 200j laser beam (or increasing the irradiation frequency) while suppressing thermal interference between temporally adjacent spot regions 201j.
[0148] (Third modified example of the second embodiment) Alternatively, as a third modification of the second embodiment, the K-stage irradiation may be performed in a ring-shaped spot region 201n using a linear trajectory OB2, as shown in Figure 26. Figure 26 is an XY plan view showing the irradiation pattern in the third modification of the second embodiment.
[0149] For example, when K=3, irradiation patterns as shown in Figures 26(a) to 26(c) may be realized. Figure 26(a) illustrates the first segmented irradiation pattern, Figure 26(b) illustrates the second segmented irradiation pattern, and Figure 26(c) illustrates the third segmented irradiation pattern. Figures 26(a) to 26(c) illustrate cases where each spot region 201n has a ring shape. Note that the size of the ring-shaped irradiation pattern shown in Figure 26 is just an example; for example, the outer diameter of the ring shape may be approximately the same as the spot diameter shown in Figure 23, or larger than the spot diameter.
[0150] As shown in Figures 26(a) to 26(c), multiple orbitals OB2-1 to OB2-M are used for K fractional irradiation. M is any integer of 2 or more. The multiple orbitals OB2-1 to OB2-M extend approximately parallel to each other and are arranged at approximately constant intervals in a direction perpendicular to the direction of their extension. In the case of Figures 26(a) to 26(c), each orbital OB2-1 to OB2-M extends in the Y direction. The multiple orbitals OB2-1 to OB2-M are arranged at approximately constant intervals in the X direction. The spacing of the arrangement of the multiple orbitals OB2-1 to OB2-M may correspond to the spot diameter Dn of the spot region 201j.
[0151] The laser beam 200n may be irradiated in one direction, sequentially along the orbits OB2-1 to OB2-M. Figures 26(a) to 26(c) illustrate the case where the laser beam 200n is irradiated along each orbit OB2 from the +Y side to the -Y side, but the laser beam 200n may also be irradiated along each orbit OB2 from the -Y side to the +Y side.
[0152] As shown in Figures 26(a) to 26(c), the first, second, and third split irradiation patterns are offset from each other by a distance corresponding to the spot diameter Dn of the spot region 201n of the first irradiation. The spot diameter Dn of the spot region 201n may correspond to two locations where tensile stress is to be generated.
[0153] As shown in Figure 26(a), in the first fractionated irradiation pattern, the spot regions 201n are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Dn of the spot region 201n of one irradiation. As shown in Figure 24(b), in the second fractionated irradiation pattern, the spot regions 201n are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Dn of the spot region 201n of one irradiation. As shown in Figure 24(c), in the third fractionated irradiation pattern, the spot regions 201n are arranged along the trajectory OB2 at a pitch equivalent to three times the spot diameter Dn of the spot region 201n of one irradiation.
[0154] For example, as shown in Figure 25, consider an irradiation pattern in which ring-shaped spot regions 201n are arranged along the trajectory OB2-2 in the X direction at a pitch corresponding to three times the spot diameter Dn of the spot regions 201n.
[0155] When the spot area 201n of the second laser beam 200n-2 is irradiated, compressive stress is generated on the main surface 100b of the substrate 100 in the area overlapping the spot area 201n when viewed from the Z direction, as shown by the dotted line in Figure 27. Tensile stress is generated on the main surface 100b of the substrate 100 in the area adjacent to the spot area 201n in the XY direction and the area adjacent to it in the XY direction in the XY direction, as shown by the dashed line in Figure 27.
[0156] When the spot area 201n of the third laser beam 200n-3 is irradiated, compressive stress is generated on the main surface 100b of the substrate 100 in the area overlapping with the spot area 201n when viewed from the Z direction, as shown by the dotted line in Figure 27. Tensile stress is generated on the main surface 100b of the substrate 100 in the area adjacent to the spot area 201n in the XY direction and the area adjacent to it in the XY direction, as shown by the dashed line in Figure 27, when viewed from the Z direction.
[0157] This also allows for increasing the spatial distance between temporally adjacent spot regions 201n during each fractional irradiation, thereby shortening the time interval between irradiations of the laser light 200n (or increasing the irradiation frequency) while suppressing thermal interference between temporally adjacent spot regions 201n.
[0158] The embodiments 1 and 2 described above, and their respective modifications, may be carried out in combination with each other.
[0159] Furthermore, while the embodiments 1 and 2 described above and their respective modifications were illustrated as examples of manufacturing a semiconductor device 1 using a bonding (joining) substrate peeling technique, the bonding (joining) substrate peeling method may also be used in the manufacture of SOI (Silicon On Insulator) substrates and the like.
[0160] While several embodiments of the present invention have been described, these embodiments are presented as examples only and are not intended to limit the scope of the invention. These novel embodiments can be carried out in a variety of other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their variations are included in the scope and spirit of the invention, as well as in the claims of the invention and its equivalents. [Explanation of Symbols]
[0161] 1 semiconductor device, 2,100,800 substrates, 3-5,7,704 films.
Claims
1. A first substrate is prepared on which multiple protrusions are formed that are distributed in two dimensions. The first film is laminated onto the plurality of protrusions of the first substrate, A second film is laminated onto the second substrate. The main surface of the first film opposite to the first substrate and the main surface of the second film opposite to the second substrate are joined together. The first substrate is irradiated with laser light from the side, The first substrate is peeled off. Equipped with, The diameter of the spot area of the laser beam is greater than the average arrangement pitch of the protrusions on the main surface of the first substrate. A method for manufacturing a semiconductor device.
2. The spot area of the laser beam overlaps with two or more of the multiple protrusions when viewed from a direction perpendicular to the main surface of the first substrate. A method for manufacturing a semiconductor device according to claim 1.
3. The spot region of the laser beam includes the two or more protrusions on its interior when viewed from a direction perpendicular to the main surface of the first substrate. The method for manufacturing a semiconductor device according to claim 2.
4. The aforementioned multiple protrusions are, The main surface of the first substrate is processed to form: A method for manufacturing a semiconductor device according to claim 1.
5. The aforementioned multiple protrusions are, A third film is deposited on the main surface of the first substrate. The third film is processed to form: A method for manufacturing a semiconductor device according to claim 1.
6. The thermal expansion coefficient of the first substrate is greater than the thermal expansion coefficient of the first film. A method for manufacturing a semiconductor device according to claim 1.
Citation Information
Patent Citations
Substrate processing method and substrate processing system
JP2021103725A
Substrate processing device and substrate processing method
JP2021106197A
Method for manufacturing semiconductor device
JP2022049603A
Processing device and processing method
WO2020213478A1
Processing device and processing method
WO2021010284A1