Method for manufacturing resin compositions

JP7955190B2Active Publication Date: 2026-11-24YKK AP INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023034295
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2026-11-24
Estimated Expiration
2043-03-07

AI Technical Summary

Benefits of technology

【0008】 本発明によれば、硬質ポリ塩化ビニルを主成分とする樹脂形材をリサイクルして、軟質ポリ塩化ビニルの樹脂組成物を容易に製造することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955190000002
    Figure 0007955190000002
  • Figure 0007955190000003
    Figure 0007955190000003
  • Figure 0007955190000004
    Figure 0007955190000004
Patent Text Reader

Abstract

To easily produce a soft polyvinyl chloride resin composition by recycling a resin profile mainly composed of a hard polyvinyl chloride.SOLUTION: There is provided a method for producing a resin composition in which a soft polyvinyl chloride resin composition is produced by using a resin profile mainly composed of a hard polyvinyl chloride as a raw material. The method for producing the resin composition comprises: a crushing step of crushing a resin profile to form a crushed material; a kneading step of kneading a first powder material mainly composed of a hard polyvinyl chloride, a second powder material mainly composed of calcium carbonate and a plasticizer while heating to obtain a kneaded material; and a mixing step of kneading the crushed material and the kneaded material while heating to produce a resin composition in which the crushed material and the kneaded material are mixed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a resin composition for producing a resin composition of flexible polyvinyl chloride.

Background Art

[0002] In fittings such as resin windows, resin profiles mainly composed of rigid polyvinyl chloride are used. The resin profile is manufactured by heating and melting a rigid polyvinyl chloride resin material, and extrusion-molding the molten resin material. When such a resin profile is recycled to produce a resin composition of flexible polyvinyl chloride, for example, a pulverized material obtained by pulverizing the resin profile and a liquid plasticizer are kneaded, and the rigid polyvinyl chloride of the pulverized material is softened with the plasticizer to produce a resin composition of flexible polyvinyl chloride.

[0003] However, in the resin profile after production, the resin particles are crushed by extrusion molding, and the voids in the resin particles that existed before extrusion molding are almost eliminated. Along with this, during kneading of the pulverized material of the resin profile and the plasticizer, the plasticizer becomes difficult to penetrate into the pulverized material, and the pulverized materials also become slippery due to the plasticizer. Therefore, it becomes difficult to knead the pulverized material of the resin profile and the plasticizer, and it becomes difficult to soften the rigid polyvinyl chloride of the pulverized material with the plasticizer. On the other hand, conventionally, a method for producing a flexible vinyl chloride resin composition is known in which a pulverized product having a particle size of 3 mm or less obtained by pulverizing a rigid vinyl chloride resin molded product, a plasticizer, and a filler are mixed with a mixer (see Patent Document 1).

[0004] In the conventional method for producing flexible polyvinyl chloride resin compositions described in Patent Document 1, a plasticizer is absorbed by a filler and then mixed with the filler into the pulverized material. However, since the amount of plasticizer that is mainly absorbed by the filler is mixed into the pulverized material, the amount of plasticizer that can be added is limited, which may make it difficult to produce a soft, flexible polyvinyl chloride resin composition. In addition, it is necessary to make the particle size of all the pulverized material 3 mm or less, which may affect the efficiency of recycling rigid polyvinyl chloride resin molded products. Therefore, there is room for improvement in the conventional method for producing flexible polyvinyl chloride resin compositions from the viewpoint of easily producing flexible polyvinyl chloride resin compositions. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Patent No. 5446105 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] The present invention has been made in view of the above-mentioned conventional problems, and its purpose is to easily produce a flexible polyvinyl chloride resin composition by recycling a resin profile mainly composed of rigid polyvinyl chloride. [Means for solving the problem]

[0007] The present invention A method for producing a resin composition of flexible polyvinyl chloride using a resin profile mainly composed of rigid polyvinyl chloride as a raw material, A grinding step of crushing the aforementioned resin profile to form a crushed material, A kneading process in which a first powder material mainly composed of rigid polyvinyl chloride, a second powder material mainly composed of calcium carbonate, and a plasticizer are kneaded while heating to obtain a kneaded product, A mixing step of kneading the kneaded mixture and the pulverized material while heating them to produce the resin composition in which the kneaded mixture and the pulverized material are mixed, This is a method for producing a resin composition having [a certain characteristic]. [Effects of the Invention]

[0008] According to the present invention, a resin composition of flexible polyvinyl chloride can be easily produced by recycling a resin profile mainly composed of rigid polyvinyl chloride. [Brief explanation of the drawing]

[0009] [Figure 1] This flowchart shows the manufacturing procedure for the flexible polyvinyl chloride resin composition of this embodiment. [Figure 2] This diagram schematically shows the state of each stage in the manufacturing process of the flexible polyvinyl chloride resin composition of this embodiment. [Figure 3] This figure shows examples of the compound and the crushed material to be mixed in this embodiment. [Figure 4] This figure shows another example of the resin profile of this embodiment. [Modes for carrying out the invention]

[0010] One embodiment of a method for producing the resin composition of the present invention will be described with reference to the drawings. In the resin composition manufacturing method of this embodiment, a resin profile mainly composed of rigid polyvinyl chloride is used as a raw material to manufacture a resin composition of flexible polyvinyl chloride. This allows the manufactured resin profile to be reused, recycled into a new resin composition, and then a new resin composition to be generated.

[0011] Figure 1 is a flowchart showing the manufacturing procedure (process) of the flexible polyvinyl chloride resin composition of this embodiment. Figure 2 is a schematic diagram showing the state of each stage in the manufacturing process of the flexible polyvinyl chloride resin composition of this embodiment.

[0012] As shown in the figure, the discarded resin profile 10 (see Figure 2A) is recovered (S101 in Figure 1). The resin profile 10 is a profile (extruded profile) formed by resin extrusion molding. The resin is rigid polyvinyl chloride, and the resin profile 10 is a rigid polyvinyl chloride profile made of rigid polyvinyl chloride. The rigid polyvinyl chloride is polyvinyl chloride (PVC) without plasticizers, although other components (for example, various stabilizers and modifiers) may be mixed with the polyvinyl chloride. Note that Figure 2A shows a cross-section perpendicular to the longitudinal direction of the resin profile 10.

[0013] Here, the resin profile 10 is a molded resin product used in resin windows, which are building fixtures. A resin window has a resin frame and a sash that includes a resin frame, and the resin frame and resin frame are each made of the resin profile 10. In addition, the resin profile 10 is made from scraps of resin profile 10 from resin windows. The scraps of resin profile 10 are, for example, scraps from the resin window manufacturing site or scraps collected as market waste. On the other hand, the resin profile 10 may also be discarded resin profile 10.

[0014] Next, the recovered resin profile 10 is crushed by a crusher to form crushed resin profile 10 material 20 (see Figure 2B) (S102 in Figure 1). The crusher is, for example, an impact crusher. If the resin profile 10 is long or large, it is cut or otherwise modified to a size that can be crushed by the crusher before being crushed by the crusher. Alternatively, the resin profile 10 may be crushed in two stages. In this case, the resin profile 10 is roughly crushed by a first-stage coarse crusher, and then the coarse crushed material 20 is crushed into fine crushed material 20 by a second-stage fine crusher. In this way, crushed resin profile 10 material 20 is produced.

[0015] The resin profile 10 is part of the raw materials for the flexible polyvinyl chloride resin composition. Flexible polyvinyl chloride is polyvinyl chloride mixed with a plasticizer, and therefore contains a plasticizer. The resin composition is a composition mainly composed of flexible polyvinyl chloride and serves as a raw material for molded products of flexible polyvinyl chloride. The plasticizer is an additive that gives flexibility to rigid polyvinyl chloride, and softens the rigid polyvinyl chloride.

[0016] Examples of plasticizers include phthalate ester plasticizers such as dibutyl phthalate (DBP), diisodecyl phthalate (DIDP), bis(2-ethylhexyl) phthalate (DOP), butyl benzyl phthalate (BBP), and diisononyl phthalate (DINP); aliphatic dibasic acid ester plasticizers such as tris(2-ethylhexyl) trimellitate (TOTM), bis(2-ethylhexyl) adipate (DOA), diisononyl adipate (DINA), disisodecyl adipate (DIDA), and dibutyl sebacate (DBS); phosphate ester plasticizers such as tris(2-ethylhexyl) phosphate (TOP) and triphenyl phosphate (TPP); or plasticizers such as polyesters and epoxidized soybean oil.

[0017] Before mixing the crushed resin material 10 20 (see Figure 2C), a first powder material 30 mainly composed of rigid polyvinyl chloride, a second powder material 40 mainly composed of calcium carbonate, and a liquid plasticizer 50 are heated and mixed in a heated kneader (S103 in Figure 1). This mixes the first powder material 30, the second powder material 40, and the plasticizer 50 to obtain a kneaded mixture 60 (see Figure 2D). The heated kneader is, for example, a Banbury mixer, a kneader, or a Brabender, and applies shear force to the kneaded mixture 60 during mixing. The first powder material 30, the second powder material 40, and the plasticizer 50 are heated to a predetermined temperature and kneaded at that temperature in the heated kneader.

[0018] The first powder material 30 is a powder of rigid polyvinyl chloride formed in a powder form (rigid polyvinyl chloride powder), and is a powder (fine powder) smaller than the pulverized material 20. Further, the first powder material 30 is an unused rigid polyvinyl chloride powder or a recycled rigid polyvinyl chloride powder. When the recycled rigid polyvinyl chloride powder is used as the first powder material 30, the resin profile 10 is pulverized by a pulverizer until it becomes a powder smaller than the pulverized material 20, and the rigid polyvinyl chloride powder obtained by pulverizing the resin profile 10 (first powder material 30) is produced. In this way, the first powder material 30 is formed from the resin profile 10.

[0019] The second powder material 40 is a powder of calcium carbonate formed in a powder form (calcium carbonate powder), and is a powder (fine powder) smaller than the pulverized material 20. The particle diameter of the first powder material 30 and the particle diameter of the second powder material 40 are each 500 μm or less. Here, the particle diameter is a particle diameter sieved using a sieve having a nominal mesh opening conforming to Japanese Industrial Standards (JIS Z 8801-1:2019), and the particle diameter being 500 μm or less means a particle diameter that passes through a sieve having a nominal mesh opening of 500 μm. The first powder material 30 and the second powder material 40 having a particle diameter of 500 μm or less are kneaded with the plasticizer 50 to produce a kneaded product 60 of the first powder material 30, the second powder material 40, and the plasticizer 50.

[0020] When the first powder material 30 of rigid polyvinyl chloride is 100 parts by weight (phr), the second powder material 40 of calcium carbonate is 50 to 150 parts by weight, and the plasticizer 50 is 100 to 250 parts by weight. As described above, when the kneaded product 60 is kneaded, 50 to 150 parts by weight of the second powder material 40 and 100 to 250 parts by weight of the plasticizer 50 are added to 100 parts by weight of the first powder material 30 and kneaded. Further, the kneaded product 60 (the first powder material 30, the second powder material 40, and the plasticizer 50) is kneaded while being heated at a temperature in the range of 160 to 170° C., and the kneading of the kneaded product 60 is completed.

[0021] During the mixing of the compound 60, the plasticizer 50 is absorbed by the first powder material 30 and the second powder material 40. At this time, since the rigid polyvinyl chloride and calcium carbonate used in the mixing are in powder form (first powder material 30 and second powder material 40), the plasticizer 50 is easily absorbed by the first powder material 30 and the second powder material 40, and the plasticizer 50 is efficiently mixed into the first powder material 30 and the second powder material 40. While the plasticizer 50 is absorbed into the first powder material 30 and the second powder material 40, the first powder material 30, the second powder material 40, and the plasticizer 50 are completely mixed.

[0022] The compound 60 is an intermediate mixture obtained by mixing the first powder material 30, the second powder material 40, and the plasticizer 50, and is produced in an intermediate stage in the production of the final mixture, a flexible polyvinyl chloride resin composition. The compound 60 also contains rigid polyvinyl chloride, calcium carbonate, and the plasticizer 50, with flexible polyvinyl chloride as its main component. When the rigid polyvinyl chloride contained in the first powder material 30 is mixed with the plasticizer 50, the rigid polyvinyl chloride contained in the first powder material 30 is softened by the plasticizer 50. As a result, flexible polyvinyl chloride is produced, and the compound 60 of flexible polyvinyl chloride containing calcium carbonate contained in the second powder material 40 is produced.

[0023] Next, a heating kneader is used to heat and knead the mixture 60 of the first powder material 30, the second powder material 40, and the plasticizer 50, and the crushed material 20 of the resin profile 10, in order to produce a flexible polyvinyl chloride resin composition in which the mixture 60 and the crushed material 20 are mixed (S104 in Figure 1). The heating kneader applies shear force to the mixture 60 and the crushed material 20 (the mixture of the mixture 60 and the crushed material 20) during kneading. The heating kneader heats the mixture 60 and the crushed material 20 to a predetermined temperature and kneads them at that temperature. The mixture 60 and the crushed material 20 are completely mixed to produce a flexible polyvinyl chloride resin composition.

[0024] Here, the compound 60 is processed to form pellets 61 of the compound 60 (see Figure 2E). When mixing the compound 60 and the crushed material 20, the pellets 61 of the compound 60 and the crushed material 20 are mixed while being heated. The pellets 61 are granular material of the compound 60, mainly composed of flexible polyvinyl chloride and containing calcium carbonate. For example, the pellets 61 are formed from the compound 60 by a molding process including extrusion molding.

[0025] The resin composition is a mixture of a compound 60 (pellets 61) containing flexible polyvinyl chloride and a crushed material 20 containing rigid polyvinyl chloride, with flexible polyvinyl chloride as the main component. When the compound 60 and the crushed material 20 are kneaded together, the flexible polyvinyl chloride contained in the compound 60 and the rigid polyvinyl chloride contained in the crushed material 20 are mixed. In addition, the plasticizer 50 contained in the flexible polyvinyl chloride of the compound 60 and the rigid polyvinyl chloride contained in the crushed material 20 are mixed together, and the rigid polyvinyl chloride contained in the crushed material 20 is softened by the plasticizer 50. As a result, flexible polyvinyl chloride is produced, and a resin composition of flexible polyvinyl chloride containing calcium carbonate contained in the compound 60 is produced.

[0026] During the mixing of the compound 60 and the crushed material 20 (see Figure 2F), the solid calcium carbonate 62 (e.g., calcium carbonate crystals) contained in the compound 60 penetrates the crushed material 20. In addition, the calcium carbonate 62 causes the crushed material 20 to catch on the compound 60, and also causes the crushed material 20 to catch on each other. As a result, the friction acting on the compound 60 and the crushed material 20 during mixing increases, making it easier for the compound 60 and the crushed material 20 to mix. Consequently, the mixing of the compound 60 and the crushed material 20 is promoted.

[0027] When the amount of crushed resin material 20 is 100 parts by weight, the amount of kneaded material 60 (pellets 61) is 80 parts by weight or more. Thus, when kneading the kneaded material 60 and the crushed material 20, 80 parts by weight or more of the kneaded material 60 are added to 100 parts by weight of the crushed material 20 and kneaded. Furthermore, the kneading of the kneaded material 60 and the crushed material 20 is completed by heating them at a temperature in the range of 160 to 170°C.

[0028] The compound 60 and the crushed material 20 can be kneaded and mixed in any ratio. Furthermore, the hardness of the flexible polyvinyl chloride resin composition changes depending on the concentration (e.g., mass percentage concentration) of the plasticizer 50 it contains, resulting in a hardness corresponding to the concentration of the plasticizer 50. By adjusting the amount of compound 60 added to the crushed material 20 based on the amount of plasticizer 50 kneaded into the compound 60, the concentration of the plasticizer 50 in the flexible polyvinyl chloride resin composition and the hardness of the resin composition are adjusted. The hardness of the resin composition is adjusted to the target hardness by adjusting the concentration of the plasticizer 50 in the resin composition to the target concentration.

[0029] Figure 3 shows an example of the kneaded mixture 60 and the crushed material 20 to be kneaded according to this embodiment. As shown in the figure, crushing the resin profile 10 forms crushed material 20 of various shapes and with a maximum dimension R. The maximum dimension R of the crushed material 20 is the dimension of the largest part of the outer shape of each crushed material 20. The maximum dimension R of the crushed material 20 used for mixing with the compound 60 is 15 mm or less. Therefore, when crushing the resin profile 10, the resin profile 10 is crushed so that the maximum dimension R of the crushed material 20 is 15 mm or less. Alternatively, after crushing the resin profile 10, crushed material 20 with a maximum dimension R greater than 15 mm is separated and removed using a separation device or the like, and crushed material 20 with a maximum dimension R of 15 mm or less is selected. The crushed material 20 with a maximum dimension R of 15 mm or less is mixed with the compound 60 to produce a flexible polyvinyl chloride resin composition.

[0030] As the mixing of the compound 60 and the crushed material 20 progresses, the resulting mixture gradually softens, its viscosity gradually decreases, and it becomes difficult to mix. This slows down the mixing process. Therefore, during the mixing of the mixture, the heating temperature of the mixture is reduced while mixing. In response to the decrease in viscosity of the mixture, the heating temperature is gradually reduced to adjust the viscosity of the mixture and suppress the decrease in viscosity. By reducing the heating temperature, the viscosity of the mixture is adjusted to a viscosity suitable for mixing, and the mixing process progresses.

[0031] The mixture of the kneaded material 60 and the crushed material 20 is kneaded using a heating kneader while gradually lowering the heating temperature of the mixture from a first temperature to a second temperature. The first temperature is the temperature before the heating temperature of the mixture is lowered. The mixture is kneaded while being heated at the first temperature, and at an intermediate stage of kneading, the heating temperature of the mixture is started to decrease from the first temperature. The mixture is then kneaded while gradually lowering the heating temperature from the first temperature to the second temperature, and when the heating temperature of the mixture reaches the second temperature, the decrease in heating temperature is stopped. After that, the heating temperature of the mixture is maintained at the second temperature, and the mixture is kneaded while being heated at the second temperature until the kneading is complete.

[0032] After the manufacturing of the flexible polyvinyl chloride resin composition is completed, the molten resin composition is discharged from the heating kneader and passed between parallel rolls (S105 in Figure 1). At this time, the resin composition is compressed by passing it between the outer surfaces of two or more opposing rolls. Subsequently, the resin composition is extruded using an extrusion molding machine, and the extruded resin composition is sequentially cut to form flexible polyvinyl chloride pellets (S106 in Figure 1). After that, flexible polyvinyl chloride molded products are formed using the flexible polyvinyl chloride pellets (S107 in Figure 1). Flexible polyvinyl chloride molded products are, for example, airtight materials and gaskets used in building fixtures.

[0033] In the resin composition manufacturing method described above, a second powder material 40, mainly composed of calcium carbonate, is added when kneading a first powder material 30, mainly composed of rigid polyvinyl chloride, and a plasticizer 50. By absorbing the plasticizer 50 into the second powder material 40, the amount of plasticizer 50 that can be contained in the kneaded mixture 60 can be increased. Furthermore, by making the rigid polyvinyl chloride and calcium carbonate into powders (first powder material 30, second powder material 40), the plasticizer 50 can be more easily absorbed into the first powder material 30 and the second powder material 40. This allows for an increase in the amount of plasticizer 50 that can be added. In addition, the plasticizer 50 can be efficiently kneaded into the first powder material 30 and the second powder material 40, increasing the amount of plasticizer 50 contained in the kneaded mixture 60. The plasticizer 50 can be more easily incorporated into the kneaded mixture 60, which can also shorten the time required for kneading the mixture 60.

[0034] A resin composition of flexible polyvinyl chloride is produced by kneading the crushed material 20 of the resin profile 10 with a compound 60. In this way, the resin composition can be produced using the crushed material 20, which can be formed relatively easily, and the resin profile 10 can be recycled efficiently. The calcium carbonate 62 contained in the compound 60 allows the compound 60 and the crushed material 20 to be kneaded smoothly, and the time required for kneading the compound 60 and the crushed material 20 can also be shortened.

[0035] Therefore, a resin composition of flexible polyvinyl chloride can be easily manufactured by recycling a resin profile 10 mainly composed of rigid polyvinyl chloride. Furthermore, the concentration of the plasticizer 50 in the resin composition can be increased, thereby broadening the range of hardness of the resin composition that can be manufactured. A soft resin composition can also be manufactured. Even if the amount of calcium carbonate added is increased, the hardness of the resin composition can be lowered by increasing the concentration of the plasticizer 50. This suppresses a deterioration in the physical properties of the resin composition. As a result, the amount of calcium carbonate added can be increased, thereby reducing the cost of the materials for the resin composition.

[0036] Pellet 61 is formed from the mixture 60, and the pellet 61 of the mixture 60 and the crushed material 20 are mixed together. Therefore, during mixing, the pellet 61 of the mixture 60 and the crushed material 20 are dispersed, allowing the mixture 60 and the crushed material 20 to be mixed smoothly.

[0037] When the particle size of the first powder material 30 is larger than 500 μm, there is a risk that the absorption of the plasticizer 50 into the first powder material 30 will be affected. When the particle size of the second powder material 40 is larger than 500 μm, there is a risk that the absorption of the plasticizer 50 into the second powder material 40 will be affected. On the other hand, when the particle size of the first powder material 30 is 500 μm or less, the plasticizer 50 is more easily absorbed into the first powder material 30, and the plasticizer 50 can be efficiently absorbed into the first powder material 30. Also, when the particle size of the second powder material 40 is 500 μm or less, the plasticizer 50 is more easily absorbed into the second powder material 40, and the plasticizer 50 can be efficiently absorbed into the second powder material 40. As a result, the kneading of the mixture 60 can be easily performed.

[0038] When the amount of the second powder material 40 is less than 50 parts by weight relative to 100 parts by weight of the first powder material 30, the amount of plasticizer 50 absorbed by the second powder material 40 will be small, which may make it difficult for the plasticizer 50 to be kneaded into the mixture 60. Also, when the amount of the second powder material 40 is more than 150 parts by weight relative to 100 parts by weight of the first powder material 30, the concentration of calcium carbonate in the flexible polyvinyl chloride resin composition will be high, which may affect the hardness of the resin composition. On the other hand, when the amount of the second powder material 40 is in the range of 50 to 150 parts by weight (50 parts by weight or more and 150 parts by weight or less) relative to 100 parts by weight of the first powder material 30, the plasticizer 50 will be easier to knead into the mixture 60, and the effect of calcium carbonate on the hardness of the resin composition can also be reduced. It is more preferable that the amount of the second powder material 40 is 80 to 120 parts by weight relative to 100 parts by weight of the first powder material 30. This makes it possible to easily mix the plasticizer 50 into the mixture 60 while further reducing the influence of calcium carbonate on the hardness of the resin composition.

[0039] When the amount of plasticizer 50 is less than 100 parts by weight relative to 100 parts by weight of the first powder material 30, the amount of plasticizer 50 contained in the kneaded product 60 will be small, which may result in a small amount of crushed material 20 that can be kneaded with the kneaded product 60. Also, when the amount of plasticizer 50 is more than 250 parts by weight relative to 100 parts by weight of the first powder material 30, the plasticizer 50 may be difficult to knead into the kneaded product 60. On the other hand, when the amount of plasticizer 50 is in the range of 100 to 250 parts by weight (100 parts by weight or more and 250 parts by weight or less) relative to 100 parts by weight of the first powder material 30, the plasticizer 50 is easily kneaded into the kneaded product 60, and a sufficient amount of crushed material 20 that can be kneaded with the kneaded product 60 can be secured. It is more preferable that the amount of plasticizer 50 is 130 to 220 parts by weight relative to 100 parts by weight of the first powder material 30. This ensures a sufficient amount of the kneaded material 60 and the kneadable crushed material 20, while allowing the plasticizer 50 to be smoothly mixed into the kneaded material.

[0040] When the amount of kneaded material 60 is less than 80 parts by weight relative to 100 parts by weight of crushed material 20, the amount of plasticizer 50 added to the kneaded material 60 will be reduced, which may affect the hardness of the flexible polyvinyl chloride resin composition. On the other hand, when the amount of kneaded material 60 is 80 parts by weight or more relative to 100 parts by weight of crushed material 20, the hardness of the resin composition can be sufficiently reduced. It is more preferable that the amount of kneaded material 60 is 100 parts by weight or more relative to 100 parts by weight of crushed material 20. This allows for stable softening of the resin composition.

[0041] When the maximum dimension R of the crushed material 20 of the resin profile 10 is greater than 15 mm, the larger size of the crushed material 20 may make it difficult to mix the crushed material 20 with the compound 60 and pellets 61. In contrast, when the maximum dimension R of the crushed material 20 is 15 mm or less, the crushed material 20 can be dispersed during mixing, allowing it to be smoothly mixed with the compound 60 and pellets 61. It is more preferable that the maximum dimension R of the crushed material 20 be 8 mm or less. This allows the crushed material 20 to be mixed with the compound 60 and pellets 61 more smoothly.

[0042] By kneading the mixture of the compound 60 and the crushed material 20 while lowering the heating temperature, the decrease in viscosity of the mixture can be suppressed, allowing the compound 60 and the crushed material 20 to mix smoothly. Furthermore, a flexible polyvinyl chloride resin composition can be produced efficiently. When the resin profile 10 used as a raw material for the resin composition is scrap of resin profile 10 (in this case, resin profile 10 for a resin window), the scrap of resin profile 10 can be recycled, thereby reducing the cost of the resin composition.

[0043] Furthermore, either unused rigid polyvinyl chloride powder or recycled rigid polyvinyl chloride powder, or both, may be used as the first powder material 30. Alternatively, instead of forming pellets 61 from the kneaded mixture 60, the kneaded mixture 60 may be kneaded with the crushed material 20.

[0044] Figure 4 shows another example of the resin profile 10 of this embodiment, and shows a cross-section perpendicular to the longitudinal direction of the resin profile 10. As shown in the figure, the resin profile 10 here has a main body 11 mainly composed of rigid polyvinyl chloride and an attachment 12 mainly composed of flexible polyvinyl chloride. The attachment 12 is a flexible part attached to the rigid main body 11, and is formed to be smaller than the main body 11 and protrudes from the main body 11. When crushing the resin profile 10 (S102 in Figure 1), the resin profile 10 with the attachment 12 attached to the main body 11 is crushed without removing the attachment 12 from the main body 11 to form crushed resin profile 10 material 20.

[0045] The resulting crushed material 20 includes crushed material 20 of only the main body 11, crushed material 20 of only the accessory part 12, and crushed material 20 containing both the main body 11 and the accessory part 12. The crushed material 20 is kneaded with the compound 60 to produce a flexible polyvinyl chloride resin composition. In this way, the resin profile 10 can be easily recycled without separating the main body 11, which is made of rigid polyvinyl chloride, from the accessory part 12, which is made of flexible polyvinyl chloride.

[0046] Next, examples of methods for producing a flexible polyvinyl chloride resin composition will be described, but the present invention is not limited to the following examples. In the examples, a flexible polyvinyl chloride resin composition was produced according to the flowchart shown in Figure 1.

[0047] [Table 1]

[0048] Table 1 shows the parts by weight of each material at each stage of the embodiment. When kneading the compound 60, 80 parts by weight of the second powder material 40 and 200 parts by weight of the plasticizer 50 were added to 100 parts by weight of the first powder material 30. The plasticizer 50 is diisononyl adipate (DINA). When kneading the crushed material 20 and the compound 60, 114 parts by weight of the compound 60 were added to 100 parts by weight of the crushed material 20. In the resin composition of the flexible polyvinyl chloride after production, 30 parts by weight of the first powder material 30, 24 parts by weight of the second powder material 40, and 60 parts by weight of the plasticizer 50 were added to 100 parts by weight of the crushed material 20. In this example, the resin composition of the flexible polyvinyl chloride was produced by recycling the resin profile 10.

[0049] As described above, this embodiment discloses a method for producing the resin composition described in (1) to (7) below.

[0050] (1) A method for producing a resin composition of flexible polyvinyl chloride using a resin profile mainly composed of rigid polyvinyl chloride as a raw material, A grinding step of crushing the aforementioned resin profile to form a crushed material, A kneading process in which a first powder material mainly composed of rigid polyvinyl chloride, a second powder material mainly composed of calcium carbonate, and a plasticizer are kneaded while heating to obtain a kneaded product, A mixing step of kneading the kneaded mixture and the pulverized material while heating them to produce the resin composition in which the kneaded mixture and the pulverized material are mixed, A method for producing a resin composition having [the specified characteristic]. In the method for producing the resin composition described in (1), a resin composition of flexible polyvinyl chloride can be easily produced by recycling a resin profile mainly composed of rigid polyvinyl chloride.

[0051] (2) In the method for producing the resin composition described in (1), The process includes a step of processing the aforementioned kneaded material to form pellets of the kneaded material, A method for producing a resin composition, wherein the mixing step involves kneading the pellets of the kneaded material and the pulverized material while heating them. In the method for producing the resin composition described in (2), the compound pellets and the pulverized material are dispersed, and the compound and the pulverized material can be smoothly mixed.

[0052] (3) In the method for producing the resin composition described in (1) or (2), A method for producing a resin composition in which the particle size of the first powder material is 500 μm or less in the kneading step. In the method for producing the resin composition described in (3), the plasticizer is more easily absorbed by the first powder material, and the plasticizer can be efficiently absorbed by the first powder material.

[0053] (4) In a method for producing a resin composition as described in any of (1) to (3), A method for producing a resin composition, wherein in the kneading step, 50 to 150 parts by weight of the second powder material and 100 to 250 parts by weight of the plasticizer are added to 100 parts by weight of the first powder material. In the method for producing the resin composition described in (4), the plasticizer is more easily mixed into the compound, the effect of calcium carbonate on the hardness of the resin composition can be reduced, and the amount of pulverized material that can be mixed with the compound can also be secured.

[0054] (5) In a method for producing a resin composition as described in any of (1) to (4), A method for producing a resin composition, wherein in the mixing step, 80 parts by weight or more of the kneaded material are added to 100 parts by weight of the pulverized material. (5) The method for producing the resin composition described above makes it possible to sufficiently lower the hardness of the resin composition.

[0055] (6) In a method for producing a resin composition as described in any of (1) to (5), A method for producing a resin composition in which the maximum size of the pulverized material is 15 mm or less in the mixing step. In the method for producing the resin composition described in (6), the pulverized material can be dispersed and smoothly mixed with the compound.

[0056] (7) In a method for producing a resin composition as described in any of (1) to (6), A method for producing a resin composition, comprising grinding a resin profile having a main body made of rigid polyvinyl chloride and an attached part made of flexible polyvinyl chloride, in the grinding step. (7) In the method for producing the resin composition described above, the resin profile can be easily recycled without separating the main body from the attached parts of the resin profile. [Explanation of Symbols]

[0057] 10... Resin profiles, 11... Main body, 12... Accessories, 20... Crushed material, 30... First powder material, 40... Second powder material, 50... Plasticizer, 60... Mixture, 61... Pellets, 62... Calcium carbonate, R... Maximum dimensions.

Claims

1. A method for producing a resin composition of flexible polyvinyl chloride using a resin profile mainly composed of rigid polyvinyl chloride as a raw material, A grinding step of grinding the aforementioned resin profile to form a pulverized material, A kneading process in which a first powder material mainly composed of rigid polyvinyl chloride, a second powder material mainly composed of calcium carbonate, and a plasticizer are kneaded while heating to obtain a kneaded product, A mixing step of kneading the kneaded mixture and the pulverized material while heating them to produce the resin composition in which the kneaded mixture and the pulverized material are mixed, A method for producing a resin composition having [the specified characteristic].

2. In the method for producing the resin composition described in claim 1, The process includes a step of processing the aforementioned kneaded material to form pellets of the kneaded material, A method for producing a resin composition, wherein the mixing step involves kneading the pellets of the kneaded material and the pulverized material while heating them.

3. In a method for producing a resin composition according to claim 1 or 2, A method for producing a resin composition in which the particle size of the first powder material is 500 μm or less in the kneading step.

4. In a method for producing a resin composition according to claim 1 or 2, A method for producing a resin composition, wherein in the kneading step, 50 to 150 parts by weight of the second powder material and 100 to 250 parts by weight of the plasticizer are added to 100 parts by weight of the first powder material.

5. In a method for producing a resin composition according to claim 1 or 2, A method for producing a resin composition, wherein in the mixing step, 80 parts by weight or more of the kneaded material are added to 100 parts by weight of the pulverized material.

6. In a method for producing a resin composition according to claim 1 or 2, A method for producing a resin composition in which the maximum size of the pulverized material is 15 mm or less in the mixing step.

7. In a method for producing a resin composition according to claim 1 or 2, A method for producing a resin composition, comprising grinding a resin profile having a main body made of rigid polyvinyl chloride and an attached part made of flexible polyvinyl chloride, in the grinding step.

Citation Information

Patent Citations

  • JP1960-011682B

  • Application of irregular type refractories

    JP1979046105A

  • Production of regenerated polyvinyl chloride resin sheet

    JP1994008248A

  • Vinyl chloride resin composition and method for producing molded product

    JP2009215439A

  • Method for producing non-rigid vinyl chloride-based resin composition and molded article

    JP2009215446A