Diamond-coated cutting tools

A diamond-coated cutting tool with a silicon nitride or sialon sintered body and controlled residual stress addresses purity and adhesion issues, enhancing peel resistance and cutting efficiency.

JP7955193B2Active Publication Date: 2026-11-24NTK CUTTING TOOLS CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023037396
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2026-11-24
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Existing diamond-coated cutting tools face issues with reduced diamond purity due to doping, insufficient adhesion caused by excessive residual compressive stress, and limited application range.

Method used

A diamond-coated cutting tool with a silicon nitride or sialon sintered body substrate having a specific thermal expansion coefficient range and a diamond layer with controlled compressive residual stress, combined with specific phase compositions to enhance adhesion and peel resistance.

Benefits of technology

The solution provides high adhesion of the diamond layer to the substrate, improving peel resistance and extending tool lifespan under demanding conditions, with enhanced cutting efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955193000002
    Figure 0007955193000002
  • Figure 0007955193000003
    Figure 0007955193000003
  • Figure 0007955193000001
    Figure 0007955193000001
Patent Text Reader

Abstract

To provide a diamond-coated cutting tool in which adhesiveness of a diamond layer relative to a substrate is high.SOLUTION: A diamond-coated cutting tool 1 comprises: a substrate 3 constituted of a silicon nitride sintered body or a sialon sintered body; and a diamond layer 7 coated on a surface of the substrate 3. The substrate 3 has an average thermal expansion coefficient x at 25°C-600°C that satisfies 2.6×10-6 / K≤x≤4.0×10-6 / K. The diamond layer 7 has a compressive residual stress of 50 MPa to 1800 MPa.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to diamond-coated cutting tools. [Background technology]

[0002] Patent Document 1 discloses a diamond-coated cemented carbide tool in which a thin diamond film is coated on the surface of a base material by a vapor phase synthesis method. In this diamond-coated cemented carbide tool, nitrogen is doped into the film during vapor phase synthesis of the diamond coating to relieve stress in the diamond film, thereby adjusting the residual stress during film formation and applying tensile stress to the film to improve the adhesion at the film-substrate interface.

[0003] Patent Document 2 discloses a cutting tool made of cemented carbide coated with artificial diamond. This cutting tool made of cemented carbide coated with artificial diamond is described as having high compressive residual stress due to the repeated formation of a diamond coating by a vapor phase synthesis method.

[0004] Patent Document 3 discloses a diamond-coated cutting tool comprising a substrate and a diamond layer covering the surface of the substrate. The diamond layer has multiple voids extending in the crystal growth direction from the portion in contact with the substrate. This diamond-coated cutting tool improves the adhesion of the diamond layer to the substrate and improves peel resistance by setting the average distance between the centers of adjacent voids to a specific range. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-076775 [Patent Document 2] Japanese Patent Application Publication No. 9-234604 [Patent Document 3] Japanese Patent Publication No. 2021-142575 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] However, as described in Patent Document 1, doping a diamond coating with other elements can reduce the purity of the diamond, potentially affecting the various physical properties of the diamond coating. Furthermore, as described in Patent Document 2, applying excessive residual compressive stress to the diamond film raises concerns about insufficient adhesion. Additionally, there is a need for a novel technology with a broader range of application than that described in Patent Document 3. This disclosure is made in view of the above circumstances and aims to provide a diamond-coated cutting tool with high adhesion of the diamond layer to the substrate. This disclosure can be realized in the following forms. [Means for solving the problem]

[0007] [1] A diamond-coated cutting tool comprising a substrate made of a silicon nitride sintered body or a sialon sintered body, and a diamond layer covering the surface of the substrate, The above-mentioned substrate has an average thermal expansion coefficient x from 25°C to 600°C, 2.6 × 10 -6 / K≦x≦4.0×10 -6 / K Satisfying the conditions, and The diamond layer of the diamond-coated cutting tool has a compressive residual stress of 50 MPa to 1800 MPa.

[0008] [2] The silicon nitride sintered body or sialon sintered body of the substrate is Phase 1 containing β-silicon nitride or β-sialon, A diamond-coated cutting tool according to [1], comprising a second phase containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, Ti carbide, 12H-sialon, 15R-sialon, 21R-sialon, and α-sialon.

[0009] [3] The silicon nitride sintered body or sialon sintered body of the substrate is A silicon nitride sintered body containing 2% to 35% by mass of Al in terms of oxide, or The diamond-coated cutting tool according to [1] or [2], which is a sialon sintered body containing Al in an amount of 2 mass% or more and 35 mass% or less in terms of oxide.

[0010] [4] The silicon nitride sintered body or sialon sintered body of the base material is A silicon nitride sintered body containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, and Ti carbide in a total amount of 5 mass% or more and 20 mass% or less, or The diamond-coated cutting tool according to any one of [1] to [3], which is a sialon sintered body containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, and Ti carbide in a total amount of 5 mass% or more and 20 mass% or less. [Advantageous Effects of Invention]

[0011] The diamond-coated cutting tool of the present disclosure has high adhesion of the diamond layer to the base material. [Brief Description of Drawings]

[0012] [Figure 1] It is a perspective view of an example of a diamond-coated cutting tool. [Figure 2] It is a cross-sectional view of an example of a diamond-coated cutting tool. [Description of Embodiments]

[0013] 1. Diamond-coated cutting tool 1 (1) Configuration of diamond-coated cutting tool 1 Diamond-coated cutting tool 1 includes a base material 3 made of a silicon nitride sintered body or a sialon sintered body, and a diamond layer 7 covering the surface of base material 3. The average coefficient of thermal expansion x of base material 3 from 25°C to 600°C satisfies the following relational expression 1. 2.6×10 -6 / K≦x≦4.0×10 -6 / K ···Relational expression 1 Furthermore, the diamond layer 7 has a compressive residual stress of 50 MPa or more and 1800 MPa or less.

[0014] (2) Base material 3 (2.1) Average thermal expansion coefficient of the base material 3 x As described above, the average thermal expansion coefficient x of the substrate 3 from 25°C to 600°C preferably satisfies relational equation 1, more preferably satisfies relational equation 2, and even more preferably satisfies relational equation 3, from the viewpoint of improving the adhesion of the diamond layer 7 to the substrate 3. The average thermal expansion coefficient x can be measured using TMA (Thermo Mechanical Analysis). 2.8 × 10 -6 / K≦x≦3.7×10 -6 / K ···Relational formula 2 3.0×10 -6 / K≦x≦3.5×10 -6 / K ···Relational formula 3

[0015] The average thermal expansion coefficient x of the base material 3 can be controlled by adjusting the type of components in the base material 3 and the content of each component. In the following explanation, Ti nitrides, Ti carbonitrides, and Ti carbides are also referred to as Ti compounds. Furthermore, 12H-Sialon, 15R-Sialon, and 21R-Sialon are also referred to as polytype Sialon. β-silicon nitride and β-sialon have relatively low coefficients of thermal expansion, while Ti compounds, polytype sialon, and α-sialon tend to have relatively high coefficients of thermal expansion. Therefore, for example, by decreasing the total content of β-silicon nitride and β-sialon in the base material 3 and increasing the total content of Ti compounds, polytype sialon, and α-sialon, the average coefficient of thermal expansion x can be increased. Also, for example, by increasing the total content of β-silicon nitride, β-sialon, and α-sialon in the base material 3 and decreasing the total content of Ti compounds and polytype sialon, the average coefficient of thermal expansion x can be decreased.

[0016] (2.2) Preferred configuration of base material 3 The base material 3 preferably comprises a first phase containing β-silicon nitride or β-sialon, and a second phase containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, Ti carbide, 12H-sialon, 15R-sialon, 21R-sialon, and α-sialon.

[0017] The area ratios of the first phase and the second phase are not particularly limited as long as they satisfy the above relational expression 1. From the viewpoint of increasing toughness, the area ratio of the first phase is preferably 50% or more when the total area of ​​the substrate 3 is taken as 100%. The upper limit of the area ratio of the first phase is not particularly limited and may be, for example, 95% or less. The area ratio of the second phase is preferably 40% or less when the total area of ​​the substrate 3 is taken as 100%. The lower limit of the area ratio of the second phase is not particularly limited and may be greater than 0%, for example, 5% or more. The area ratio of the first and second phases can be calculated by scanning the cross-section of the substrate 3 with a scanning electron microscope at a magnification of 2000x and performing image analysis.

[0018] The total content of β-silicon nitride and β-sialon in the first phase is not particularly limited. The content in the first phase is preferably 60% by mass or more. The upper limit of the content in the first phase is not particularly limited and may be 100% by mass or less. The total content of the Ti compound, polytype sialon, and α-sialon in the second phase is not particularly limited. The content in the second phase is preferably 60% by mass or more. The upper limit of the content in the second phase is not particularly limited and may be 100% by mass or less.

[0019] The substrate 3 containing the second phase can be manufactured, for example, using the following raw materials by the method for manufacturing the diamond-coated cutting tool 1 described later. If the second phase contains a Ti compound, then a Ti compound can be used as a starting material. In this way, the blended Ti compound can directly constitute the second phase. If the second phase contains polytype sialon or α-sialon, then an Al compound and a specific rare earth element compound may be used as raw materials. For example, using a La (lanthanum) compound as the specific rare earth element compound tends to easily produce polytype sialon. Also, using only at least one compound selected from the group consisting of Y (yttrium), Dy (dysprosium), and Er (erbium) as the specific rare earth element compound tends to easily produce α-sialon. In this way, the second phase can be composed of the produced polytype sialon or α-sialon.

[0020] The silicon nitride sintered body constituting the base material 3 is, for example, a sintered body in which the total amount of β-silicon nitride and α-silicon nitride relative to the entire silicon nitride sintered body is 50% by mass or more. The sialon sintered body constituting the base material 3 is, for example, a sintered body in which the total amount of β-sialon, α-sialon, and polytype relative to the entire sialon sintered body is 50% by mass or more.

[0021] In silicon nitride sintered bodies, silicon nitride (Si3N4) is a ceramic crystalline grain composed of Si (silicon) and N (nitrogen), and is sintered by adding sintering aids to the raw material silicon nitride. Silicon nitride exists in two phases: an α phase with equiaxed particle shape and a β phase with needle-shaped particle shape, and the toughness and hardness properties can be controlled by the ratio of these phases. β-silicon nitride has a structure in which needle-shaped structures are intertwined, resulting in high toughness, while α-silicon nitride, with its equiaxed particle shape, has lower toughness compared to β-silicon nitride but high hardness. In silicon nitride contained in silicon nitride sintered bodies, the types of these crystalline phases and their ratios are not particularly limited.

[0022] The silicon nitride sintered body may contain at least one element selected from the group consisting of Group 4 elements, rare earth elements, and Mg (magnesium) in the periodic table (hereinafter sometimes referred to as "specific elements"). The content ratio is not particularly limited; for example, it may be contained in an amount of 0.5 mol% or more and less than 2.6 mol% in terms of oxide relative to the silicon nitride sintered body. The periodic table referred to here is as defined in Table I-3.2 "Designation of Groups in the Periodic Table" on page 43 of "Inorganic Chemical Nomenclature - IUPAC 1990 Recommendation -" edited by G.J. Leich, translated and authored by Kazuo Yamazaki, published March 26, 1993, by Tokyo Kagaku Dojin Co., Ltd.

[0023] As one of the aforementioned specific elements, Group 4 elements of the periodic table can be cited as preferred examples, such as titanium (Ti), zirconium (Zr), and hafnium (Hf). As rare earth elements, scandium (Sc), yttrium (Y), lanthanides, and actinides can be cited. As lanthanides, cerium group elements and yttrium group elements can be cited. As cerium group elements, lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), and samarium (Sm) can be cited, and as yttrium group elements, europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu) can be cited. Examples of the aforementioned actinides include actinium (Ac) and thorium (Th). Note that "oxide conversion" refers to converting an element to an oxide formed by oxidizing it or combining it with oxygen.

[0024] The aforementioned specific elements may be present in the silicon nitride sintered body as a single element, or multiple types of the aforementioned specific elements may be present in the silicon nitride sintered body.

[0025] From the following viewpoints, the silicon nitride sintered body preferably contains at least one selected from the group consisting of a Ti (titanium) nitride, a Ti carbonitride, and a Ti carbide in a total amount of 5% by mass or more and 20% by mass or less, more preferably in a total amount of 5% by mass or more and 15% by mass or less, and even more preferably in a total amount of 10% by mass or more and 15% by mass or less. When the silicon nitride sintered body contains the above Ti compound within the above range, further peeling resistance can be expected. That is, by combining silicon nitride (α-silicon nitride, β-silicon nitride) as a matrix having a smaller coefficient of thermal expansion than the diamond layer 7, and the above Ti (titanium) compound having a larger thermal expansion than the diamond layer 7, tensile stress and compressive stress are randomly applied to offset the stress, while the thermal expansion of the entire sintered body falls within the range of the above relational expression 1, so that further peeling resistance can be expected. Preferable examples of the Ti (titanium) nitride, the Ti carbonitride, and the Ti carbide include TiC x N (1-x) (0≦X≦1).

[0026] Sialon (SiAlON) in the sialon sintered body is a ceramic crystal particle made of Si (silicon), Al (aluminum), O (oxygen), and N (nitrogen). Sialon is formed by adding a sintering aid or the like to a raw material powder containing constituent elements such as Si, Al, O, and N, such as silicon nitride, alumina, aluminum nitride, and silica, which are raw materials, and sintering the mixture. The sialon particles have a composition formula of Si 6-Z Al Z O Z N 8-Z β-sialon represented by (0<Z≦4.2), and a composition formula Mx(Si,Al) 12 (O,N) 16 (0<X≦2, M represents an element such as Mg, Ca, Sc, Y, Dy, Er, Yb, and Lu, which becomes an interstitial solid solution) and the like. Since β-sialon has a structure in which acicular structures are entangled with each other like silicon nitride, it has high toughness. Since α-sialon has an equiaxed particle shape, it has lower toughness than β-sialon, but has high hardness. In the sialon, the ratio of α-sialon to β-sialon is not particularly limited.

[0027] The Sialon sintered body may contain, in terms of oxide, 1% to 10% by mass of at least one element selected from the group consisting of Sc, Y, Dy, Yb, Er, Sm, Ce, and Lu, which is used as a sintering aid.

[0028] From the viewpoint of further improving the peel resistance of the diamond layer 7, the Sialon sintered body preferably contains 2% to 35% by mass of Al (aluminum) in terms of oxide, more preferably 5% to 30% by mass, and even more preferably 15% to 25% by mass.

[0029] From the following viewpoints, the Sialon sintered body preferably contains at least one selected from titanium nitride, titanium carbonitride, and titanium carbide in a total amount of 5% to 20% by mass, more preferably 5% to 15% by mass, and even more preferably 5% to 10% by mass. By containing the above titanium compound in the Sialon sintered body within the above range, further peel resistance can be expected. That is, by combining a Sialon sintered body with a matrix having a smaller coefficient of thermal expansion than the diamond layer 7 and the above titanium compound having a larger coefficient of thermal expansion than the diamond layer 7, tensile and compressive stresses are applied randomly, and the stresses cancel each other out, so that the thermal expansion of the entire sintered body falls within the range of the above relational expression 1, and further peel resistance can be expected. Suitable examples of titanium nitrides, titanium carbonitrides, and titanium carbides include TiC x N (1-x) (0 ≤ X ≤ 1) is one example.

[0030] From the viewpoint of further improving peel resistance, the sialon sintered body preferably contains a polytype crystalline phase. The polytype is preferably at least one selected from the group consisting of 12H, 15R, and 21R. That is, the sialon sintered body preferably contains at least one polytype sialon selected from the group consisting of 12H-sialon (general formula: SiAl5O2N5), 15R-sialon (general formula: SiAl4O2N4), and 21R-sialon (general formula: SiAl6O2N6). The inclusion of a polytype crystalline phase in the sialon sintered body can be expected to provide even greater peel resistance. Specifically, by combining β-sialon, which has a relatively small coefficient of thermal expansion, with sialon (polytype sialon, α-sialon), which has a relatively large coefficient of thermal expansion, tensile and compressive stresses are applied randomly, canceling each other out, and the thermal expansion of the entire sintered body falls within the range of the above relational equation 1, thus providing even greater peel resistance. The polytype crystalline phase contained in the Sialon sintered body can be identified by X-ray diffraction analysis of the sintered body.

[0031] (3) Diamond layer 7 The diamond layer 7 has a compressive residual stress of 50 MPa to 1800 MPa. Preferably, the diamond layer 7 has a compressive residual stress of 150 MPa to 1600 MPa, and more preferably, a compressive residual stress of 300 MPa to 1400 MPa.

[0032] The residual stress in diamond layer 7 is sin 2 The measurement is performed using the Ψ method. The measurement location is on the rake face 7A of the diamond-coated cutting tool 1, at a position up to 1500 μm from the cutting edge of the diamond-coated cutting tool 1. The residual stress is measured using an X-ray diffractometer that uses Cu-Kα rays. However, in diamond-coated cutting tools with cemented carbide as the base material, the Co (cobalt) contained in the base material overlaps with the diamond crystal plane, making it difficult to measure the compressive stress using the above measurement method. It is desirable that the diamond-coated cutting tool 1 of this disclosure does not contain Co in order to accurately evaluate the residual stress.

[0033] The compressive residual stress of the diamond layer 7 can be controlled, for example, by adjusting the thermal expansion coefficient of the base material 3. Increasing the thermal expansion coefficient of the base material 3 will increase the compressive residual stress of the diamond layer 7. Conversely, decreasing the thermal expansion coefficient of the base material 3 will decrease the compressive residual stress of the diamond layer 7. Furthermore, the residual stress in the diamond layer 7 can be controlled, for example, by post-coating treatment described later. Increasing the irradiation pressure during blasting tends to increase the compressive residual stress, while decreasing it tends to decrease it. Similarly, increasing the irradiation time during blasting tends to increase the compressive residual stress, while decreasing the irradiation time tends to decrease it.

[0034] The diamond layer 7 preferably has a multilayer structure in order to reduce the surface roughness of the film and provide high film toughness. The diamond layer 7 is preferably made of polycrystalline diamond. Here, polycrystalline diamond is a material in which diamond nanoparticles are tightly bonded together. The diamond layer 7 may contain heterogeneous atoms such as boron, nitrogen, and silicon, as well as unavoidable impurities other than these elements.

[0035] The method for forming the diamond layer 7 is not particularly limited. The preferred method for forming the diamond layer 7 is CVD (chemical vapor deposition). Examples of CVD methods include microwave plasma CVD, hot filament CVD, and high-frequency plasma CVD. Among these CVD methods, microwave plasma CVD, which easily produces films with fine grain size and low surface roughness, is preferred.

[0036] The thickness of the diamond layer 7 is not particularly limited. Preferably, the thickness of the diamond layer 7 is 8 μm or more and 20 μm or less. A thickness of 8 μm or more improves adhesion, and a thickness of 20 μm or less makes it easier to sharpen the cutting edge, thus improving cutting performance.

[0037] (4) The reason why the configuration of this disclosure is presumed to improve the adhesion of the diamond layer 7 to the substrate 3 and thus improve peel resistance The coefficient of thermal expansion of the diamond layer 7 (diamond coating) according to this embodiment is 3.1 × 10⁻⁶. -6 The coefficient of thermal expansion of the diamond layer 7 is / K. In order to improve the adhesion of the diamond layer 7 to the base material 3 by applying an appropriate compressive residual stress to the diamond layer 7, it is necessary to adjust the thermal expansion coefficient of the base material 3 relative to the diamond layer 7. That is, if the thermal expansion coefficient of the base material 3 is too small compared to the diamond layer 7, tensile stress will be applied to the diamond layer 7, and the adhesion of the diamond layer 7 to the base material 3 will decrease. Also, if the thermal expansion coefficient of the base material 3 is too large compared to the diamond layer 7, excessive compressive stress will be applied to the diamond layer 7, and the adhesion of the diamond layer 7 to the base material 3 will decrease. Therefore, it is presumed that the adhesion of the diamond layer 7 to the base material 3 will improve by setting the average thermal expansion coefficient x of the base material 3 to the specific range shown in relational equation 1 above, and setting the compressive residual stress applied to the diamond layer 7 to 50 MPa or more and 1800 MPa or less. Furthermore, the improved adhesion of the diamond layer 7 to the substrate 3 reduces the likelihood of peeling not only during the initial stages of cutting but also during prolonged cutting, thus extending the tool's lifespan. In addition, the diamond-coated cutting tool 1 of this disclosure can be used under more demanding conditions, thereby increasing cutting efficiency.

[0038] 2. Manufacturing method of diamond-coated cutting tool 1 The method for manufacturing the diamond-coated cutting tool 1 is not particularly limited. An example of a method for manufacturing the diamond-coated cutting tool 1 is shown below.

[0039] (1) Raw materials For example, the following raw material powders are used as raw materials. ·Main ingredient α-Si3N4 powder • Sintering aids can be selected from Y2O3 (yttrium oxide), Yb2O3 (ytterbium oxide), La2O3 (lanthanum oxide), CeO2 (cerium(IV) oxide), Sm2O3 (samarium oxide), Er2O3 (erbium oxide), Dy2O3 (dysprosium oxide), MgO (magnesium oxide), MgCO3 (magnesium carbonate), Al2O3 (aluminum oxide), AlN (aluminum nitride), ZrO2 (zirconium oxide), TiN (titanium nitride), and TiC (titanium carbide).

[0040] (2) Preparation of base material 3 A slurry is obtained by wet mixing the raw material powder, an organic binder dissolved in a solvent, and the solvent using a ball. The slurry is dried and press-molded into the desired shape (tool) to obtain a molded body. The molded body is degreased in a heating device under a predetermined atmosphere, for example, at 400°C to 800°C for 60 to 120 minutes. Furthermore, the degreased molded body is placed in a container and heated under a predetermined atmosphere, for example, at 1700°C to 1900°C for 120 to 360 minutes to obtain a sintered body. If the theoretical density of the sintered body is less than 99%, further HIP (Hot Isostatic Pressing) is performed under a predetermined atmosphere, for example, 1000 atmospheres, for example, at 1500°C to 1700°C for 120 to 240 minutes to obtain a dense body with a theoretical density of 99% or more. The sintered body or dense body thus produced corresponds to the base material 3.

[0041] (3) Pre-coating treatment A pre-coating treatment may be performed before coating the diamond layer 7. The pre-coating treatment is performed to improve the adhesion of the diamond layer 7 to the substrate 3. Specifically, examples include surface roughening treatment of the substrate 3. For surface roughening treatment, chemical corrosion such as electrolytic polishing or sandblasting with abrasive grains such as SiC may be used.

[0042] (4) Coating of the diamond layer 7 (formation of the diamond layer 7) For coating the diamond layer 7, for example, a microwave plasma CVD method can be used. For example, methane (CH4), hydrogen (H2), carbon monoxide (CO), etc., are supplied as raw material gases and the coating is performed. The coating process is carried out by repeatedly performing the following two steps, for example. The nucleation step and crystal growth step described below are repeated until the desired film thickness is reached, thereby coating the surface of the substrate 3 with a multilayer diamond layer 7. (4.1) Nucleation process The flow rates of methane and hydrogen are adjusted so that the methane concentration is within a set range of 10% to 30%. At this time, the surface temperature of the substrate 3 is within a set range of 700°C to 900°C, and the gas pressure inside the reactor is 2.5 × 10⁻⁶. 2 Pa to 3.0 × 10 3 The system maintains a set pressure within the specified range of Pa for 0.1 to 2 hours. (4.2) Crystal growth process The flow rates of methane and hydrogen are adjusted so that the methane concentration is within a set range of 1% to 4%. At this time, the surface temperature of the substrate 3 is within a set range of 800°C to 900°C, and the gas pressure inside the reactor is 1.0 × 10⁻⁶. 3 Pa to 7.0 × 10 3 Crystal growth is carried out at a set pressure defined within the range of Pa.

[0043] (5) Post-coating treatment The residual stress of the coated diamond layer 7 is adjusted by blast treatment using abrasive grains such as SiC. In this process, the surface of the diamond layer 7 is blast-treated at a predetermined pressure (0.1 MPa to 0.6 MPa) and a predetermined irradiation time (1 s to 40 s) so that the compressive residual stress of the diamond layer 7 is between 50 MPa and 1800 MPa. [Examples]

[0044] The following will provide a more detailed explanation using examples.

[0045] 1. Fabrication of diamond-coated cutting tools (examples and comparative examples) (1) Preparation of the base material α-Si3N4 powder with an average particle size of 1.0 μm or less, and the sintering aids Y2O3 (yttrium oxide), Yb2O3 (ytterbium oxide), La2O3 (lanthanum oxide), CeO2 (cerium(IV) oxide), Sm2O3 (samarium oxide), Er2O3 (erbium oxide), Dy2O3 (dysprosium oxide), MgO (magnesium oxide), MgCO3 (magnesium carbonate), Al2O3 (aluminum oxide), AlN (aluminum nitride), ZrO2 (zirconium oxide), TiN (titanium nitride), and TiC (titanium carbide) were weighed to obtain the raw material powders according to the formulations shown in Table 1. In Table 1, the "Sintering Aid A" and "Sintering Aid B" columns show the compound name in the upper row and the amount (mass%) in the lower row. A slurry was obtained by wet mixing the raw material powder, a microwax-based organic binder dissolved in ethanol, and ethanol using a ball mill with a Si3N4 ball. The slurry was dried and press-molded into the shape of SPGN422 according to ISO standards to obtain a molded body. The molded body was degreased in a heating device under a nitrogen atmosphere of 1 atmosphere at 400°C to 800°C for 60 to 120 minutes. Furthermore, the degreased molded body was placed in a Si3N4 container and heated under a nitrogen atmosphere at 1700°C to 1900°C for 120 to 360 minutes to obtain a sintered body. If the theoretical density of the sintered body was less than 99%, a further HIP treatment was performed under a nitrogen atmosphere of 1000 atmospheres at 1500°C to 1700°C for 120 to 240 minutes to obtain a dense body with a theoretical density of 99% or more. The sintered body or dense body thus produced was used as the substrate.

[0046] [Table 1]

[0047] (2) Coating Microwave plasma CVD was used to coat the diamond layer. Methane (CH4), hydrogen (H2), carbon monoxide (CO), etc. were used as raw material gases. The coating process involved repeatedly performing the nucleation process described in section (4.1) and the crystal growth process described in section (4.2) until the target film thickness (12 μm) was reached, thereby coating the surface of the substrate with a multilayer diamond layer.

[0048] (3) Post-coating treatment The coated diamond layer was subjected to blast treatment using SiC abrasive grains with a grit size of #600. The irradiation pressure (MPa) and irradiation time (s, seconds) during the blast treatment were as specified in Table 1.

[0049] 2. Measurement methods for diamond-coated cutting tools, etc. (1) Method for calculating the content of Al in terms of oxides and the content of Ti compounds The content of Al (in terms of oxides) and the content of Ti compounds were calculated by measuring X-ray fluorescence spectrometry on the substrate. Here, "Ti compound" refers to at least one selected from Ti nitrides, Ti carbonitrides, and Ti carbides. The "Al content" and "Ti compound (TiN) content" columns in Table 1 represent the calculated Al content in terms of oxides and the Ti compound content, respectively. "-" means that the Al compound or Ti compound was below the detection limit.

[0050] (2) Crystal phase identification method The second phase in the sintered body was identified by X-ray diffraction analysis of the substrate. Here, the second phase is identified as a phase containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, Ti carbide, 12H-sialon, 15R-sialon, 21R-sialon, and α-sialon. In addition, each example in Table 1 where the "Contains Phase 2" column is "Yes" comprises a first phase containing β-silicon nitride or β-sialon, and the above-mentioned second phase.

[0051] (3) Method for measuring the coefficient of thermal expansion Measurements were performed on each substrate using Thermo Mechanical Analysis (TMA). The measurement conditions were RT (25°C) to 1000°C, under an Ar atmosphere, at a rate of 10°C / min.

[0052] (4) Method for measuring residual stress The residual stress in the diamond layer is sin 2 The measurement was performed using the Ψ method. The measurement point was 1500 μm from the cutting edge of the diamond-coated cutting tool on the rake face. Residual stress was measured using the parallel-angle method with an X-ray diffractometer using Cu-Kα rays. <Measurement conditions> Peak used: C(331) Young's modulus: 1050 GPa Poisson's ratio (v): 0.2 Collimator diameter: 0.3mm Measurement: When Ψ is in the range of -43.1069° to 0°, sin 2 Fifteen measurements were taken so that Ψ was equally spaced.

[0053] 3. Cutting Test of Diamond-Coated Cutting Tools (1) Test method Cutting tests were conducted using each diamond-coated cutting tool. The test conditions were as follows. In the cutting tests, the number of passes until the diamond layer peeled off from the diamond-coated cutting tool was measured. A higher number of passes resulted in a higher evaluation. The evaluation was as follows. <Test Conditions> • Workpiece material: Aluminum (AC4A-T6) ·Cutting speed: 300m / min • Cutting depth: 1.0 mm Feed rate: 0.25mm / rev. • Length per pass: 200mm • Cutting environment: Cooling water available <Rating> "A"...1400+ passes "B" ... 1000 passes or more, less than 1400 passes "C" ... 900 passes or more but less than 1000 passes "D"... Less than 900 passes

[0054] (2) Test results The test results are shown in Table 1. The average coefficient of thermal expansion x is 2.6 × 10 -6 / K≦x≦4.0×10 -6 Examples 1 to 8, which satisfy the / K requirement and have a diamond layer with a compressive residual stress of 50 MPa to 1800 MPa, all received a good evaluation of "A" or "B". In contrast, when the average thermal expansion coefficient x was 2.6 × 10⁻⁶ -6 / K≦x≦4.0×10 -6 Comparative Examples 1 to 3, which were not / K or whose diamond layer did not have a compressive residual stress of 50 MPa to 1800 MPa, all received a poor evaluation of "D". More specifically, while Examples 1 to 8 had at least 1000 passes until peeling, Comparative Examples 1 to 3 had a maximum of 600 passes until peeling, resulting in a significant difference in peel resistance.

[0055] Comparing Examples 2 and 3, Example 3, which included both Phase 1 and Phase 2, received a higher evaluation than Example 2, which did not include Phase 2. Comparing Examples 2, 3, and 4, Examples 3 and 4, which contained 2% to 35% by mass of Al in terms of oxide, were evaluated higher than Example 2, which was outside this range. Comparing Examples 2, 5, and 6, Examples 5 and 6, which contained 5% to 20% by mass of Ti nitride (TiN), required more passes to delamination than Example 2, which was outside this range.

[0056] This disclosure is not limited to the embodiments detailed above, and various modifications or changes are possible within the scope of the claims of this disclosure. [Explanation of Symbols]

[0057] 1. Diamond-coated cutting tools 3...Base material 7. Diamond layer 7A…Surface

Claims

1. A diamond-coated cutting tool comprising a substrate made of a silicon nitride sintered body or a sialon sintered body, and a diamond layer covering the surface of the substrate, The above-mentioned substrate has an average thermal expansion coefficient x from 25°C to 600°C, 2.6×10 -6 / K≦x≦4.0×10 -6 / K Satisfying the conditions, and The diamond layer has a compressive residual stress of 50 MPa to 1800 MPa. The silicon nitride sintered body or sialon sintered body of the aforementioned substrate is Phase 1 containing β-silicon nitride or β-sialon, A diamond-coated cutting tool comprising a second phase containing at least one selected from the group consisting of Ti nitride, Ti carbonitride, Ti carbide, 12H-sialon, 15R-sialon, 21R-sialon, and α-sialon.

2. The silicon nitride sintered body or sialon sintered body of the substrate is A silicon nitride sintered body containing at least one selected from Ti nitride, Ti carbonitride, and Ti carbide in a total amount of 5% by mass or more and 20% by mass or less, or The diamond-coated cutting tool according to claim 1, which is a SiAlON sintered body containing a total of 5% by mass or more and 20% by mass or less of at least one selected from Ti nitride, Ti carbonitride, and Ti carbide.

3. A diamond-coated cutting tool comprising a base material made of a sialon sintered body and a diamond layer covering the surface of the base material, The above-mentioned substrate has an average thermal expansion coefficient x from 25°C to 600°C, 2.6×10 -6 / K≦x≦4.0×10 -6 / K Satisfying the conditions, and The diamond layer has a compressive residual stress of 50 MPa to 1800 MPa. The aforementioned substrate sialon sintered body is A diamond-coated cutting tool made of a SiAlon sintered body containing 2% to 35% by mass of Al in terms of oxide.

4. The aforementioned substrate sialon sintered body is The diamond-coated cutting tool according to claim 3, which is a Sialon sintered body containing a total of 5% by mass or more and 20% by mass or less of at least one selected from Ti nitride, Ti carbonitride, and Ti carbide.

Citation Information

Patent Citations

  • Ceramic material and cutting tools made thereof for toughness demanding operations

    CN101209924A

  • Tool of surface-coated silicon-nitride sintered body

    JP1992331006A

  • Diamond-coated cemented carbide tool

    JP1995076775A

  • Artificial diamond coated sintered hard alloy cutting tool having excellent wear resistance

    JP1997234604A

  • Surface-coated cemented carbide-cutting tool having excellent chipping resistance in thich-film artificial diamond coating layer

    JP1999050254A