Thermistor elements and electromagnetic wave sensors
The thermistor element with a spinel-type crystal structure and controlled oxygen concentration addresses the issue of reduced measurement accuracy in conventional CPP structured sensors by minimizing in-plane current flow, enhancing sensor performance.
Patent Information
- Application Number
- JP2023037506
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-03-10
AI Technical Summary
Conventional electromagnetic wave sensors using thermistor elements with a CPP structure suffer from reduced measurement accuracy due to current components flowing in the in-plane direction within the thermistor film.
A thermistor element with a spinel-type crystal structure is designed, where the oxygen concentration in a specific region between the electrodes is higher than in regions overlapping with the electrodes, reducing in-plane current flow and enhancing measurement accuracy.
The thermistor element with a spinel-type crystal structure and controlled oxygen concentration improves measurement accuracy by minimizing in-plane current components, resulting in better sensor performance.
Smart Images

Figure 0007955194000002 
Figure 0007955194000003 
Figure 0007955194000004
Abstract
Description
[Technical Field]
[0001] The present invention relates to a thermistor element and an electromagnetic wave sensor. [Background Art]
[0002] Conventionally, there has been an electromagnetic wave sensor including an electromagnetic wave detection unit such as a thermistor element. As a thermistor element provided in such an electromagnetic wave sensor, there is a thermistor element in which infrared rays incident on the thermistor element are absorbed by the thermistor film or a material around the thermistor film, thereby changing the temperature of the thermistor film, and accordingly, the electrical resistance of the thermistor film changes.
[0003] As an electromagnetic wave sensor using a thermistor element, for example, there is one described in Patent Document 1. Patent Document 1 describes an electromagnetic wave sensor including thermistor elements arranged in an array. Patent Document 1 describes a thermistor element including a thermistor film, a pair of first electrodes provided in contact with one surface of the thermistor film, and a second electrode provided in contact with the other surface of the thermistor film. Patent Document 1 describes a thermistor element having a CPP (Current-Perpendicular-to-Plane) structure in which a current flows in a direction perpendicular to a surface of the thermistor film. [Prior Art Documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Unexamined Patent Application Publication No. 2022-126582 [Summary of Invention] [Problems to be Solved by the Invention]
[0005] However, in a conventional electromagnetic wave sensor using a thermistor element having a CPP structure in which a current flows in a direction perpendicular to a surface of a thermistor film, further improvement in measurement accuracy is required. The present invention has been made in view of the above problems, and aims to provide a thermistor element that can provide an electromagnetic wave sensor with good measurement accuracy, and an electromagnetic wave sensor equipped with the same. [Means for solving the problem]
[0006] To solve the above problems, the following means are provided. A thermistor element according to one aspect of the present invention comprises a thermistor film made of an oxide having a spinel-type crystal structure, a first-surface electrode provided in contact with a first surface of the thermistor film, and a second-surface electrode provided in contact with a second surface of the thermistor film, wherein the first-surface electrode consists of a first electrode and a second electrode spaced apart from the first electrode in a plan view, and at least a portion of the first electrode and at least a portion of the second electrode are arranged to overlap with the second-surface electrode in a plan view, and the thermistor film is characterized in that the oxygen concentration in the second region located between the first electrode and the second electrode in a plan view is higher than the oxygen concentration in the second region located between the first electrode and the second electrode in a plan view than in the first region consisting of a region overlapping with the first electrode and the second-surface electrode in a plan view and a region overlapping with the second electrode and the second-surface electrode in a plan view. [Effects of the Invention]
[0007] The thermistor element of the present invention comprises a thermistor film made of an oxide having a spinel-type crystal structure, in which the oxygen concentration in the second region located between the first and second electrodes in a plan view is higher than that in the first region, which consists of a region overlapping with the first and second surface electrodes in a plan view and a region overlapping with the second electrode and the second surface electrode in a plan view. Therefore, in the thermistor element of the present invention, current is less likely to flow in the in-plane direction within the second region of the thermistor film. As a result, electromagnetic wave sensors equipped with the thermistor element of the present invention are less susceptible to a decrease in measurement accuracy due to current components flowing in the in-plane direction within the thermistor film of the thermistor element, and thus exhibit good measurement accuracy. [Brief explanation of the drawing]
[0008] [Figure 1] This is a plan view showing the configuration of an electromagnetic wave sensor according to one embodiment of the present invention. [Figure 2] Figure 1 is an exploded perspective view showing the configuration of the electromagnetic wave sensor. [Figure 3] Figure 1 is a plan view showing a magnified portion of the electromagnetic wave sensor, specifically a plan view of the layer where the first surface electrode of the thermistor element is located. [Figure 4] This is a cross-sectional view showing an enlarged portion of the electromagnetic wave sensor shown in Figure 1, and is a cross-sectional view of line segment AA shown in Figure 3. [Figure 5] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 6] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 7] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 8] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 9] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 10] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 11] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 12] This is a cross-sectional view illustrating the manufacturing process of the thermistor element in the electromagnetic wave sensor shown in Figure 1. [Figure 13] This graph shows the relationship between the position in the thickness direction of the cross-section including the first region 5a of the thermistor element 4 in Example 1 and the concentration of each element. [Figure 14] This graph shows the relationship between the position in the thickness direction of the cross-section including the second region 5b of the thermistor element 4 in Example 1 and the concentration of each element. [Modes for carrying out the invention]
[0009] The present inventors have conducted intensive studies to solve the above problems, and to improve the measurement accuracy of an electromagnetic wave sensor including a thermistor element including a first electrode and a second electrode that are provided in contact with a first surface of the thermistor film and are spaced apart from each other, and a second surface-side electrode that is provided in contact with a second surface of the thermistor film.
[0010] As a result, it has been found that a current component flowing through the thermistor film in an in-plane direction between the first electrode and the second electrode is one of the causes of a decrease in measurement accuracy of an electromagnetic wave sensor including the thermistor element.
[0011] Therefore, the present inventors have focused on the electrical resistance and the material of the thermistor film and have conducted repeated studies. As a result, as the thermistor film of the thermistor element, it has been found that the oxygen concentration in a second region, which is made of an oxide having a spinel-type crystal structure and is located between the first electrode and the second electrode in a plan view, may be higher than that in a first region including a region overlapping with the first electrode and the second surface-side electrode in a plan view and a region overlapping with the second electrode and the second surface-side electrode in a plan view, and the present invention has been conceived.
[0012] In such a thermistor element, it is estimated that the electrical resistivity of the thermistor film is higher in the second region than in the first region, and current is less likely to flow between the first electrode and the second electrode in the in-plane direction of the thermistor film. As a result, it is estimated that an electromagnetic wave sensor including this thermistor element is less likely to have a decrease in measurement accuracy due to a current component flowing in the in-plane direction of the thermistor film between the first electrode and the second electrode, and has good measurement accuracy.
[0013] The present invention includes the following aspects. [1] A thermistor film made of an oxide having a spinel-type crystal structure, and a first surface-side electrode provided in contact with a first surface of the thermistor film, and a second surface-side electrode provided in contact with a second surface of the thermistor film. The first surface-side electrode is composed of a first electrode and a second electrode arranged spaced apart from the first electrode in plan view, and at least a part of the first electrode and at least a part of the second electrode are arranged so as to overlap with the second surface-side electrode in plan view. The thermistor element is characterized in that, in the thermistor film, the oxygen concentration in a second region located between the first electrode and the second electrode in plan view is higher than that in a first region composed of a region overlapping with the first electrode and the second surface-side electrode in plan view and a region overlapping with the second electrode and the second surface-side electrode in plan view.
[0014] [2] An electromagnetic wave sensor comprising the thermistor element according to [1]. [3] The electromagnetic wave sensor according to [2], comprising a plurality of the thermistor elements, wherein the plurality of thermistor elements are arranged in an array.
[0015] Hereinafter, the thermistor element and the electromagnetic wave sensor of the present embodiment will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged manner for convenience in order to make the features of the present invention easy to understand. Therefore, the dimensional ratios and the like of each component may differ from the actual ones. The materials, dimensions, and the like exemplified in the following description are merely examples, and the present invention is not limited thereto, and can be appropriately modified and implemented without departing from the scope of the present invention.
[0016] [Electromagnetic Wave Sensor] The electromagnetic wave sensor of this embodiment detects electromagnetic waves emitted from a measurement target. Examples of electromagnetic waves detected by the electromagnetic wave sensor of this embodiment include infrared rays and terahertz waves. Specifically, the electromagnetic wave sensor of this embodiment may detect infrared rays (hereinafter sometimes referred to as "infrared IR") with a wavelength of 0.75 μm or more and 1000 μm or less. Infrared IR may be far-infrared rays, mid-infrared rays, or near-infrared rays. Infrared IR may also be long-wavelength infrared rays with a wavelength of 8 to 14 μm. Furthermore, the electromagnetic wave sensor of this embodiment may detect terahertz waves with a wavelength of 30 μm or more and 3 mm or less.
[0017] The following description will use an electromagnetic wave sensor that detects infrared (IR) emitted from a measurement target as an example of the electromagnetic wave sensor of this embodiment. The electromagnetic wave sensor of this embodiment may also be an infrared image sensor that detects infrared (IR) emitted from a measurement target and detects (images) the temperature distribution of the measurement target in two dimensions. The infrared image sensor can be preferably used as an infrared camera for indoor and / or outdoor night vision, etc. The infrared image sensor can also be preferably used as a non-contact temperature sensor for measuring the temperature of people and objects, etc.
[0018] Figure 1 is a plan view showing the configuration of an electromagnetic wave sensor according to one embodiment of the present invention. Figure 2 is an exploded perspective view showing the configuration of the electromagnetic wave sensor shown in Figure 1. Figure 3 is an enlarged plan view of a part of the electromagnetic wave sensor shown in Figure 1, and is a plan view of the layer in which the first surface electrode of the thermistor element is arranged. Figure 4 is an enlarged cross-sectional view of a part of the electromagnetic wave sensor shown in Figure 1, and is a cross-sectional view of line segment AA shown in Figure 3. Figures 5 to 12 are cross-sectional views illustrating the manufacturing process of the thermistor element provided in the electromagnetic wave sensor shown in Figure 1.
[0019] Figures 1 to 12 show the establishment of an XYZ Cartesian coordinate system. In Figures 1 to 12, the X-axis direction is shown as the first direction X within a specific plane of the electromagnetic wave sensor, the Y-axis direction is shown as the second direction Y which is perpendicular to the first direction X within a specific plane of the electromagnetic wave sensor, and the Z-axis direction is shown as the third direction Z which is perpendicular to the specific plane of the electromagnetic wave sensor.
[0020] As shown in Figure 2, the electromagnetic wave sensor 1 of this embodiment comprises a first substrate 2 and a second substrate 3 arranged facing each other, and a plurality of thermistor elements 4 arranged between the first substrate 2 and the second substrate 3. One thermistor element 4 is provided for each region E. As shown in Figures 1 and 2, region E is a region demarcated in a plan view by a plurality of first lead wires 9a and a plurality of second lead wires 9b.
[0021] As shown in Figure 2, the first substrate 2 and the second substrate 3 are sealed around the perimeter of their opposing surfaces with a sealing material (not shown), thereby forming a sealed internal space K between them. The internal space K is reduced to a high vacuum. As a result, in the electromagnetic wave sensor 1 of this embodiment, the influence of heat due to convection in the internal space K is suppressed, and the influence of heat other than infrared (IR) emitted from the object being measured on the thermistor element 4 is eliminated.
[0022] The electromagnetic wave sensor 1 of this embodiment is not limited to the configuration having a sealed, depressurized internal space K as described above. The electromagnetic wave sensor 1 of this embodiment may have a configuration having a sealed internal space K at atmospheric pressure, or it may have a configuration having an open internal space K.
[0023] The first substrate 2 and the second substrate 3 are made of substrates that are transparent to electromagnetic waves of a specific wavelength. If the electromagnetic waves of a specific wavelength are, for example, infrared (IR), then the first substrate 2 and the second substrate 3 can be, for example, silicon substrates, or germanium substrates.
[0024] The multiple thermistor elements 4 provided in the electromagnetic wave sensor 1 are formed to be the same size as each other. As shown in Figures 1 and 2, the multiple thermistor elements 4 are arranged in an array in a plane parallel to the first substrate 2 and the second substrate 3 (hereinafter referred to as "a specific plane").
[0025] Multiple thermistor elements 4 are arranged in a matrix in a first direction X and a second direction Y that intersect (orthogonal in this embodiment) within a specific plane, with each being provided in a region E as shown in Figures 1 and 2. Each thermistor element 4 is arranged at regular intervals in the first direction X, with the first direction X being the row direction and the second direction Y being the column direction, and is also arranged at regular intervals in the second direction Y. The number of matrices in the thermistor element 4 (in other words, the number of matrices in region E) may be, for example, 640 rows × 480 columns or 1024 rows × 768 columns. The number of matrices in the thermistor element 4 is not necessarily limited to these numbers and can be changed as appropriate.
[0026] [Thermistor element] As shown in Figure 4, the thermistor element 4 comprises a thermistor film 5 as a temperature sensing element, a first-surface side electrode 6 provided in contact with one surface (first surface) of the thermistor film 5, and a second-surface side electrode 6c provided in contact with the other surface (second surface) of the thermistor film 5.
[0027] The first surface electrode 6 is a pair of electrodes consisting of a first electrode 6a and a second electrode 6b. As shown in Figures 3 and 4, the first electrode 6a and the second electrode 6b are spaced apart in a plan view. At least a portion (all in this embodiment) of the first electrode 6a and at least a portion (all in this embodiment) of the second electrode 6b are arranged to overlap with the second surface electrode 6c and the thermistor film 5 in a plan view, as shown in Figures 3 and 4. The first electrode 6a and the second electrode 6b in this embodiment are substantially the same shape.
[0028] Furthermore, the second surface electrode 6c in this embodiment can be the same shape as the thermistor film 5 in a plan view, for example, as shown in Figures 3 and 4.
[0029] The thermistor element 4 provided in the electromagnetic wave sensor 1 of this embodiment, as shown in Figure 4, has a CPP (Current-Perpendicular-to-Plane) structure in which a current flows in the direction perpendicular to the plane of the thermistor film 5, with a first surface electrode 6 (first electrode 6a and second electrode 6b) and a second surface electrode 6c provided so as to sandwich the thermistor film 5. Specifically, the thermistor element 4 is capable of flowing a current perpendicular to the plane of the thermistor film 5 from the first electrode 6a of the first surface electrode 6 to the second surface electrode 6c, and also from the second surface electrode 6c to the second electrode 6b.
[0030] As shown in Figure 4, the wiring layers 21a and 21b are in contact with the thermistor film 5 on the sides of the first electrode 6a and second electrode 6b, which constitute the first surface electrode 6. In this embodiment, the portions of the first electrode 6a and second electrode 6b that are not in contact with the thermistor film 5 and the wiring layers 21a and 21b are covered by a second insulating film 7b (insulating film). As shown in Figures 3 and 4, the second insulating film 7b is also positioned between the first electrode 6a and the second electrode 6b of the first surface electrode 6 in a plan view. As a result, the second insulating film 7b is in contact with the portion of one surface (first surface) of the thermistor film 5 that is not in contact with the first surface electrode 6 (first electrode 6a and second electrode 6b).
[0031] As shown in Figures 3 and 4, the second insulating film 7b provided in this embodiment has circular openings 20a and 20b that penetrate the second insulating film 7b, respectively, at positions that overlap with the approximate center of the first electrode 6a and the approximate center of the second electrode 6b in a plan view. Furthermore, as shown in Figures 3 and 4, the first electrode 6a and the second electrode 6b provided in this embodiment are formed continuously in a portion located within the region overlapping with the openings 20a and 20b in a plan view, and in a portion located outside the region overlapping with the openings 20a and 20b in a plan view. As a result, the first electrode 6a and the second electrode 6b each have a shape with an uneven surface, where the thermistor film 5 side is concave and the wiring layer 21a and 21b side is convex. Consequently, the first electrode 6a and the second electrode 6b have a larger contact area with the thermistor film 5 compared to the case where there is no uneven surface.
[0032] In this embodiment, as shown in Figures 3 and 4, the entire surfaces of the thermistor film 5-facing sides of the first electrode 6a and the second electrode 6b are in contact with one surface of the thermistor film 5, and the entire surface of the thermistor film 5-facing side of the second electrode 6c is in contact with the other surface of the thermistor film 5. Therefore, as shown in Figure 4, the thermistor film 5 and the second electrode 6c have two protrusions that conform to the shape of the protrusions within the protrusions of the first electrode 6a and the second electrode 6b.
[0033] As shown in Figure 4, on the side of the wiring layers 21a, 21b and the second insulating film 7b opposite to the thermistor film 5, an insulating layer 7a is arranged so as to cover the wiring layers 21a, 21b and the second insulating film 7b.
[0034] Furthermore, a third insulating film 7c is provided on the side of the second surface electrode 6c opposite to the thermistor film 5, in contact with the second surface electrode 6c. In this embodiment, as shown in Figure 4, the third insulating film 7c covers the sides of the second surface electrode 6c and the thermistor film 5, and is in contact with the surface of the second insulating film 7b that faces the thermistor film 5.
[0035] The thermistor film 5 is made of an oxide having a spinel-type crystal structure, and the oxygen concentration in the second region 5b, located between the first electrode 6a and the second electrode 6b in a plan view, is higher than that in the first region 5a, which consists of a region overlapping with the first electrode 6a and the second surface electrode 6c in a plan view, and a region overlapping with the second electrode 6b and the second surface electrode 6c in a plan view.
[0036] The oxygen concentration in the second region 5b should be more than 1 times the oxygen concentration in the first region 5a, preferably 1.2 times or more, and more preferably 1.5 times or more. The larger the oxygen concentration ratio between the second region 5b and the first region 5a of the thermistor film 5, the larger the difference in electrical resistivity between the first region 5a and the second region 5b. This makes it easier for current to flow perpendicular to the plane within the first region 5a and more difficult for current to flow in the in-plane direction within the second region 5b. As a result, the reduction in measurement accuracy due to the current component flowing in the in-plane direction within the thermistor film 5 is less likely to occur, resulting in good measurement accuracy. Furthermore, the oxygen concentration in the second region 5b is preferably twice or less the oxygen concentration in the first region 5a, and more preferably 1.8 times or less, since it can be efficiently produced using the manufacturing method described later.
[0037] It is preferable that the oxygen concentration in the first region 5a is substantially uniform in the thickness direction. In this embodiment, when the thermistor film 5 is divided into three equal regions in the thickness direction—a region close to one surface (first surface), a region close to the other surface (second surface), and a region including the center in the thickness direction—the oxygen concentration in the second region 5b is higher than the oxygen concentration in the first region 5a in all three regions. This is because current flows more easily in the direction perpendicular to the surface in the first region 5a, and current flows less easily in the direction in the in-plane direction within the second region 6c.
[0038] The thermistor film 5 is made of an oxide having a spinel-type crystal structure. When a film made of an oxide having a spinel-type crystal structure is placed in contact with an insulating film made of an oxide, and then heat-treated at a temperature of 250°C or higher in an atmospheric environment, for example, oxygen diffuses from the insulating film, increasing the oxygen concentration in the oxide having a spinel-type crystal structure.
[0039] Preferably, the oxide having a spinel-type crystal structure has, for example, a base metal element consisting of cobalt (Co) and manganese (Mn), or a base metal element consisting of nickel (Ni) and manganese (Mn), located in at least a portion of either one or both of the A site and the B site of the spinel-type crystal structure. These base metal elements can be located in either the A site or the B site of the spinel-type crystal structure represented by the general formula AB2O4.
[0040] Furthermore, oxides having a spinel-type crystal structure may also contain, in addition to these base metal elements, transition metal elements such as cobalt (Co), nickel (Ni), copper (Cu), iron (Fe), zirconium (Zr), titanium (Ti), vanadium (V), chromium (Cr), scandium (Sc), yttrium (Y), niobium (Nb), and molybdenum (Mo), as well as at least one additive element selected from aluminum (Al) and zinc (Zn). Preferably, the additive element contains at least one selected from aluminum (Al), cobalt (Co), nickel (Ni), copper (Cu), iron (Fe), and zirconium (Zr). The additive element may be located at either the A site or the B site of the spinel-type crystal structure represented by the general formula AB2O4. These additive elements may be substituted and dissolved in at least a portion of either one or both of the A and B sites of the spinel-type crystal structure, or they may not be substituted and dissolved in the A and B sites, but may be located at a different location from the A and B sites.
[0041] In this embodiment, the thickness of the thermistor film 5 is preferably in the range of 80 nm to 300 nm, and more preferably in the range of 100 nm to 200 nm.
[0042] The first electrode 6a, the second electrode 6b, and the second electrode 6c, which constitute the first surface electrode 6, are all made of conductive films. The first electrode 6a and the second electrode 6b also function as oxygen diffusion suppression layers to suppress the diffusion of oxygen from the second insulating film 7b to the thermistor film 5 when the thermistor element 4 is manufactured using the manufacturing method described later. The second electrode 6c also functions as an oxygen diffusion suppression layer to suppress the diffusion of oxygen from the atmosphere during heat treatment (e.g., air atmosphere) to the thermistor film 5 when the thermistor element 4 is manufactured using the manufacturing method described later. The conductive films forming the first electrode 6a, the second electrode 6b, and the second surface electrode 6c may be different from each other, or they may be partially or entirely the same.
[0043] In this embodiment, the conductive films forming the first electrode 6a and second electrode 6b, and the second electrode 6c, which constitute the first front electrode 6, can be made from at least one selected from platinum (Pt), gold (Au), palladium (Pd), silver (Ag), ruthenium (Ru), iridium (Ir), rhodium (Rh), osmium (Os), titanium (Ti), rhenium (Re), copper (Cu), nickel (Ni), tantalum (Ta), chromium (Cr), and nickel-chromium (NiCr) alloys. Each of the first electrode 6a, second electrode 6b, and second front electrode 6c may be a laminated film in which multiple conductive films are stacked. For example, each of the first electrode 6a and second electrode 6b can be a laminated film in which two conductive films, a nickel-chromium (NiCr) alloy film and a platinum (Pt) film, are stacked.
[0044] In this embodiment, it is preferable that the first electrode 6a, the second electrode 6b, and the second surface electrode 6c are all conductive films made of precious metals selected from platinum (Pt), gold (Au), palladium (Pd), silver (Ag), ruthenium (Ru), iridium (Ir), rhodium (Rh), osmium (Os), and rhenium (Re) (single precious metals or alloys made of these precious metal elements). This is because they are less likely to deteriorate during the heat treatment in the manufacturing method of the thermistor element 4 described later, and are less likely to form a deteriorated layer between them and the thermistor film 5. Furthermore, it is preferable that the first electrode 6a, the second electrode 6, and the second surface electrode 6c are all conductive films made of precious metals, as this results in excellent conductivity. When each of the first electrode 6a, the second electrode 6b, and the second surface electrode 6c is a laminated film in which multiple conductive films are stacked, it is preferable that the conductive film in contact with the thermistor film 5 is made of a precious metal.
[0045] In this embodiment, the thicknesses of the first electrode 6a, the second electrode 6b, and the second surface electrode 6c are all, for example, in the range of 7 nm to 100 nm. The thicknesses of the first electrode 6a and the second electrode 6b are preferably such that they function as oxygen diffusion suppression layers that suppress the diffusion of oxygen from the second insulating film 7b to the thermistor film 5 during heat treatment. The thicknesses of the first electrode 6a and the second electrode 6b are appropriately determined according to the materials of the first electrode 6a and the second electrode 6b and the material of the second insulating film 7b. The thickness of the second surface electrode 6c is preferably such that it functions as an oxygen diffusion suppression layer that suppresses the diffusion of oxygen from the heat treatment atmosphere (e.g., air atmosphere) to the thermistor film 5 during heat treatment. The thickness of the second surface electrode 6c is appropriately determined according to the material of the second surface electrode 6c.
[0046] The materials of the first insulating film 7a, the second insulating film 7b, and the third insulating film 7c may be different from each other, or they may be partially or entirely the same. For example, the first insulating film 7a, the second insulating film 7b, and the third insulating film 7c can be made from aluminum nitride, silicon nitride, aluminum oxide, silicon oxide, magnesium oxide, tantalum oxide, niobium oxide, hafnium oxide, zirconium oxide, germanium oxide, yttrium oxide, tungsten oxide, bismuth oxide, calcium oxide, aluminum oxynitride, silicon oxynitride, magnesium aluminum oxide, silicon boride, boron nitride, or SiAlON (oxynitride of silicon and aluminum).
[0047] In this embodiment, for the reasons described below, it is preferable that at least the second insulating film 7b among the first insulating film 7a, the second insulating film 7b, and the third insulating film 7c is made of an oxide. A portion of the second insulating film 7b is located between the first electrode 6a and the second electrode 6b of the first surface electrode 6, as shown in Figures 3 and 4, and is in contact with the portion of one surface (first surface) of the thermistor film 5 that is located between the first electrode 6a and the second electrode 6b in a plan view. Therefore, if the second insulating film 7b is made of an oxide, oxygen can be diffused from the second insulating film 7b to the thermistor film 5 by manufacturing the thermistor element 4 using the manufacturing method described later. Thus, a thermistor element 4 having a thermistor film 5 with a higher oxygen concentration in the second region 5b than in the first region 5a can be easily manufactured.
[0048] [Element peripheral structure] As shown in Figure 2, one side of the first substrate 2 in the electromagnetic wave sensor 1 of this embodiment (the side facing the second substrate 3) is provided with a first insulating layer 8, a wiring section 9 electrically connected to a circuit section 15 (described later), and a first connection section 10 that electrically connects each thermistor element 4 to the wiring section 9.
[0049] The first insulating layer 8 is an insulating film laminated on one side of the first substrate 2 (the side facing the second substrate 3). As the first insulating layer 8, one or more insulating films can be used, such as aluminum nitride, silicon nitride, aluminum oxide, silicon oxide, magnesium oxide, tantalum oxide, niobium oxide, hafnium oxide, zirconium oxide, germanium oxide, yttrium oxide, tungsten oxide, bismuth oxide, calcium oxide, aluminum oxynitride, silicon oxynitride, magnesium aluminum oxide, silicon boride, boron nitride, and SiAlON (oxynitride of silicon and aluminum).
[0050] As shown in Figures 1 and 2, the wiring section 9 has a plurality of first lead wires 9a and a plurality of second lead wires 9b. The plurality of first lead wires 9a extend in a first direction X and are arranged at regular intervals in a second direction Y. On the other hand, the plurality of second lead wires 9b extend in a second direction Y and are arranged at regular intervals in the first direction X. As shown in Figure 4, the plurality of first lead wires 9a and the plurality of second lead wires 9b are arranged at different positions in the thickness direction (third direction Z) of the first insulator layer 8 and are arranged to intersect three-dimensionally as shown in Figure 2. The first lead wiring 9a and the second lead wiring 9b are made of a conductive film such as copper or gold.
[0051] The first connecting portion 10 has a pair of first connecting members 11a and 11b. As shown in Figures 3 and 4, the pair of first connecting members 11a and 11b have a pair of arm portions 12a and 12b and a pair of leg portions 13a and 13b. The leg portions 13a and 13b of the pair of first connecting members 11a and 11b are respectively positioned at the diagonal ends of each of the substantially rectangular region E in plan view (see Figures 1 to 4).
[0052] As shown in Figure 4, each arm portion 12a and 12b consists of a part of the wiring layers 21a and 21b (the conductor pattern portion described later), a first insulating film 7a covering one side of the wiring layers 21a and 21b, a second insulating film 7b covering the other side of the wiring layers 21a and 21b, and a third insulating film 7c covering the side of the second insulating film 7b opposite to the wiring layers 21a and 21b.
[0053] As shown in Figures 3 and 4, the wiring layers 21a and 21b are formed by a folded linear conductor pattern portion formed along the periphery of the thermistor film 5 in a plan view, and a conductor portion formed at a position overlapping with the thermistor film 5 in a plan view and connected to the first electrode 6a or the second electrode 6b. The first insulating film 7a, second insulating film 7b, and third insulating film 7c that cover the wiring layers 21a and 21b forming the conductor pattern are all substantially the same shape as the wiring layers 21a and 21b forming the conductor pattern when viewed from above.
[0054] Each of the wiring layers 21a and 21b consists of at least one material selected from, for example, aluminum, tungsten, titanium, tantalum, titanium nitride, tantalum nitride, chromium nitride, and zirconium nitride.
[0055] The leg portion 13a functions as a contact plug that electrically connects the first lead wiring 9a to the wiring layer 21a of the arm portion 12a. The leg portion 13b also functions as a contact plug that electrically connects the second lead wiring 9b to the wiring layer 21b of the arm portion 12b. Each leg portion 13a, 13b is formed by a conductor pillar with a circular cross-section that extends in the third direction Z, as shown in Figures 3 and 4. Each leg portion 13a, 13b is made of, for example, copper, gold, FeCoNi alloy, or NiFe alloy (permalloy).
[0056] As shown in Figures 3 and 4, the first connecting member 11a has a wiring layer 21a that is electrically connected to the first electrode 6a of the first surface electrode 6, and a leg portion 13a that electrically connects the wiring layer 21a and the first lead wiring 9a, thereby electrically connecting the first electrode 6a and the first lead wiring 9a. The first connecting member 11b has a wiring layer 21b that is electrically connected to the second electrode 6b, and a leg portion 13b that electrically connects the wiring layer 21b and the second lead wiring 9b, thereby electrically connecting the second electrode 6b and the second lead wiring 9b.
[0057] As shown in Figure 2, one side of the second substrate 3 in the electromagnetic wave sensor 1 of this embodiment (the side facing the first substrate 2) is provided with a second insulating layer 14, a circuit section 15, a second connection section 16, and connection terminals 17a and 17b.
[0058] The second insulating layer 14 is an insulating film laminated on one side of the second substrate 3 (the side facing the first substrate 2). The second insulating layer 14 can be the same insulating film that can be used for the first insulating layer 8. The insulating film forming the second insulating layer 14 may be the same as the insulating film forming the first insulating layer 8, or they may be different.
[0059] The circuit section 15 detects the change in voltage output from the thermistor element 4 and converts it into brightness temperature. The circuit section 15 is located within the second insulating layer 14. The circuit section 15 consists of a read-out integrated circuit (ROIC), a regulator, an analog-to-digital converter, a multiplexer, and the like.
[0060] As shown in Figure 2, the circuit section 15 is electrically connected to a plurality of first lead wires 9a via a second connecting member 18a and a connecting terminal 17a. The circuit section 15 is also electrically connected to a plurality of second lead wires 9b via a second connecting member 18b and a connecting terminal 17b.
[0061] As shown in Figure 2, the second connection portion 16 has a plurality of second connecting members 18a, 18b. The plurality of second connecting members 18a, 18b consist of conductive pillars with a circular cross-section that are formed extending in the third direction Z. The plurality of second connecting members 18a, 18b are provided corresponding to each of the plurality of first lead wires 9a and the plurality of second lead wires 9b. The second connecting member 18a electrically connects one end of the first lead wire 9a to the connection terminal 17a. The second connecting member 18b electrically connects one end of the second lead wire 9b to the connection terminal 17b. The multiple second connecting members 18a, 18b are made of a conductive material such as copper and / or gold.
[0062] As shown in Figure 2, the connection terminals 17a and 17b are provided on the surface of the second insulating layer 14. Each of the connection terminals 17a and 17b corresponds to one of the plurality of first lead wires 9a and one of the plurality of second lead wires 9b. The connection terminals 17a are located in a region on one side of the first direction X surrounding the circuit section 15 and are arranged at regular intervals in the second direction Y. The connection terminals 17b are located in a region on one side of the second direction Y surrounding the circuit section 15 and are arranged at regular intervals in the first direction X. The connection terminals 17a and 17b are made of a conductive film such as copper and / or gold.
[0063] As shown in Figures 1 and 2, each thermistor element 4 in the electromagnetic wave sensor 1 of this embodiment is provided in a region demarcated by a plurality of first lead wires 9a and a plurality of second lead wires 9b in a plan view. As shown in Figures 2 and 4, the multiple thermistor elements 4 are supported by a pair of first connecting members 11a and 11b, suspended in a third direction Z. As a result, as shown in Figure 4, a space G is provided between the thermistor elements 4 and the first insulating layer 8. Also, as shown in Figure 4, in the region of the thermistor film 5 of each thermistor element 4 that faces the first substrate 2 in the thickness direction (the region that overlaps in a plan view), there is a window W that transmits infrared IR between the first substrate 2 and the thermistor film 5.
[0064] In the electromagnetic wave sensor 1 of this embodiment, infrared radiation (IR) emitted from the object to be measured enters the thermistor element 4 from the first substrate 2 side through the window W. The infrared radiation (IR) that enters the thermistor element 4 is absorbed by the first insulating film 7a, the second insulating film 7b, the third insulating film 7c, and the thermistor film 5, which are formed in the vicinity of the thermistor film 5. As a result, the temperature of the thermistor film 5 changes, which changes its electrical resistance, and the output voltage between the first electrode 6a and the second electrode 6b, which are the first surface electrodes 6, changes. Therefore, in the electromagnetic wave sensor 1 of this embodiment, the thermistor element 4 functions as a bolometer element.
[0065] The electromagnetic wave sensor 1 of this embodiment detects infrared (IR) emitted from the object to be measured in a planar manner using multiple thermistor elements 4. Furthermore, the electromagnetic wave sensor 1 of this embodiment can detect (image) the temperature distribution (temperature image) of the object to be measured in two dimensions by converting the electrical signal (voltage signal) output from each thermistor element 4 into brightness temperature. When a constant voltage is applied to the thermistor film 5 in the thermistor element 4, it is also possible to detect the change in current flowing through the thermistor film 5 in response to the temperature change of the thermistor film 5 and convert it into brightness temperature.
[0066] [Method for manufacturing electromagnetic wave sensors] Next, the manufacturing method of the electromagnetic wave sensor 1 of this embodiment will be described. The electromagnetic wave sensor 1 of this embodiment can be manufactured, for example, by the manufacturing method shown below. First, the above-mentioned components, such as the first insulating layer 8, wiring portion 9, and leg portions 13a and 13b, are formed on the first substrate 2 by known methods. Then, the thermistor element 4 is formed on the surface of the first substrate 2 facing the first insulating layer 8 by the method described below.
[0067] Figures 5 to 12 are cross-sectional views illustrating the manufacturing process of the thermistor element provided in the electromagnetic wave sensor shown in Figure 1. In this embodiment, for example, the case in which each component forming the thermistor element 4 is formed sequentially from the component located on the first insulating film 7a side to the third insulating film 7c will be used as an example for explanation.
[0068] First, a known organic material layer 30, such as a resist, is formed on the surface of the first substrate 2 on which the above-mentioned components are formed, on the side facing the first insulating layer 8. Next, as shown in Figure 5, a first insulating film 7a, for example, made of aluminum oxide (Al2O3), is deposited over the entire surface on the organic material layer 30.
[0069] Next, a conductive film made of, for example, titanium (Ti) is deposited over the entire surface of the first insulating film 7a shown in Figure 5. Then, the conductive film is patterned using photolithography. This forms wiring layers 21a and 21b having a predetermined pattern shape, as shown in Figure 6.
[0070] Next, as shown in Figure 7, a second insulating film 7b, made of, for example, aluminum oxide (Al2O3), is deposited over the entire surface on the wiring layers 21a and 21b. Next, the second insulating film 7b is patterned using photolithography. This creates openings 20a and 20b on the wiring layers 21a and 21b, respectively, that penetrate the second insulating film 7b.
[0071] Next, a conductive film 53 made of, for example, platinum (Pt) is deposited over the entire surface of the second insulating film 7b having openings 20a and 20b, and the conductive film 53 is embedded in the openings 20a and 20b. After that, the conductive film 53 is patterned using photolithography. This forms the first surface electrode 6, consisting of a first electrode 6a and a second electrode 6b, as shown in Figure 9.
[0072] In this embodiment, when forming the first surface electrode 6 made of platinum (Pt), the film thickness of the first surface electrode 6 is preferably 20 nm or more and 60 nm or less. When the film thickness of the first surface electrode 6 made of platinum (Pt) is 20 nm or more, the first surface electrode 6 effectively functions as an oxygen diffusion suppression layer that suppresses the diffusion of oxygen from the second insulating film 7b to the thermistor film 5. Furthermore, when the film thickness of the first surface electrode 6 made of platinum (Pt) is 60 nm or less, the process of patterning the conductive film 53 to form the first surface electrode 6 is easier, which is preferable.
[0073] Next, as shown in Figure 10, a thermistor material film 54 made of an oxide having a spinel-type crystal structure and a conductive film 55 made of, for example, platinum (Pt) are deposited on the second insulating film 7b on which the first surface electrode 6 is provided, in this order over the entire surface. Next, by patterning the thermistor material film 54 and the conductive film 55 using photolithography technology, a second surface electrode 6c and thermistor film 5 are formed, which are patterned to the same shape as each other, as shown in Figure 11.
[0074] In this embodiment, when forming the second side electrode 6c made of platinum (Pt), the film thickness of the second side electrode 6c is preferably 20 nm or more and 60 nm or less. When the film thickness of the second side electrode 6c made of platinum (Pt) is 20 nm or more, the second side electrode 6c effectively functions as an oxygen diffusion suppression layer that suppresses the diffusion of oxygen from the heat treatment atmosphere (e.g., air atmosphere) to the thermistor film 5 during heat treatment. Furthermore, when the film thickness of the second side electrode 6c made of platinum (Pt) is 60 nm or less, the process of patterning the conductive film 55 to form the second side electrode 6c is easier, which is preferable.
[0075] Next, in this embodiment, the thermistor element in the process of being manufactured, with each layer up to the second surface electrode 6c, is subjected to heat treatment (annealing) at a temperature of 250°C or higher in an atmospheric environment. This causes oxygen to diffuse from the second insulating film 7b to the thermistor film 5 which is in contact with the second insulating film 7b. At this time, the diffusion of oxygen from the second insulating film 7b to the thermistor film 5 which is in contact with the first surface electrode 6 (first electrode 6a, second electrode 6b) is suppressed by the first electrode 6a and the second electrode 6b. In addition, the diffusion of oxygen from the atmospheric environment to the thermistor film 5 which is in contact with the second surface electrode 6c is suppressed by the second surface electrode 6c. As a result, the thermistor film 5 has a higher oxygen concentration in the second region 5b than in the first region 5a.
[0076] The heat treatment temperature in the above heat treatment is, for example, 250°C or higher, and preferably 250°C to 325°C, when the material of the second insulating film 7b is aluminum oxide (Al2O3). Since the heat treatment temperature is 250°C or higher, oxygen can be diffused from the second insulating film 7b to the thermistor film 5 which is in contact with the second insulating film 7b. When the heat treatment temperature is 325°C or lower, delamination due to film thinning of the organic material layer 30 is less likely to occur, which is preferable.
[0077] The heat treatment time in the above heat treatment can be, for example, 0.5 hours to 5 hours, and preferably 1 hour to 3 hours. The heat treatment time in the above heat treatment can be appropriately determined depending on the material of each component that forms the thermistor element 4, the material of the second insulating film 7b, the material and thickness of the thermistor film 5, etc.
[0078] In this embodiment, since the atmosphere during the heat treatment is an atmospheric atmosphere, the second surface electrode 6c can suppress the diffusion of oxygen from the atmospheric atmosphere into the thermistor film 5. In contrast, if the heat treatment is performed in an oxygen atmosphere, for example, the effect of preventing the diffusion of oxygen from the oxygen atmosphere into the thermistor film 5 by the second surface electrode 6c may not be sufficient, and the overall oxygen concentration of the thermistor film 5 may increase.
[0079] Next, as shown in Figure 12, an insulating film made of, for example, silicon dioxide (SiO2) is deposited over the entire surface of the second surface electrode 6c to form a third insulating film 7c that covers the second surface electrode 6c and the sides of the second surface electrode 6c and the thermistor film 5. Subsequently, the thermistor element 4 and the arm portions 12a and 12b are formed into predetermined shapes as shown in Figure 4 by patterning. Subsequently, the organic material layer 30 is removed by ashing to form space G. The above thermistor element 4 is obtained by going through the above process.
[0080] Furthermore, a second substrate 3 having the above-mentioned components is manufactured by a known method. Then, the second substrate 3 is placed on one side (the side with the thermistor element 4) of the first substrate 2 having the thermistor element 4. Subsequently, the first substrate 2 and the second substrate 3 are electrically connected using the above-mentioned components by known methods, and the periphery of the opposing surfaces of the first substrate 2 and the second substrate 3 is sealed with a sealing material (not shown) to form a sealed internal space K (see Figure 2) between them. By following the above steps, the electromagnetic wave sensor 1 of this embodiment can be obtained.
[0081] The thermistor element 4 of this embodiment is made of an oxide having a spinel-type crystal structure and comprises a thermistor film 5 in which the oxygen concentration in the second region 5b, located between the first electrode 6a and the second electrode 6b in a plan view, is higher than that in the first region 5a, which consists of a region overlapping with the first electrode 6a and the second surface electrode 6c in a plan view and a region overlapping with the second electrode 6b and the second surface electrode 6c in a plan view. Therefore, in the thermistor element 4 of this embodiment, current is less likely to flow in the in-plane direction within the second region 6c of the thermistor film 5.
[0082] Therefore, the electromagnetic wave sensor 1 equipped with the thermistor element 4 of this embodiment is less susceptible to a decrease in measurement accuracy due to the current component flowing in the in-plane direction within the thermistor film 5 of the thermistor element 4, resulting in good measurement accuracy.
[0083] Although embodiments of the present invention have been described in detail above with reference to the drawings, the configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications to the configurations are possible without departing from the spirit of the present invention.
[0084] For example, the thermistor element of the present invention is not necessarily limited to being applied to an infrared image sensor in which the above-described plurality of thermistor elements 4 are arranged in an array. The thermistor element of the present invention may be applied to an electromagnetic wave sensor using a single thermistor element 4, or it can be applied to an electromagnetic wave sensor in which a plurality of thermistor elements 4 are arranged in a linear fashion. Furthermore, the thermistor element of the present invention can also be used as a temperature sensor for measuring temperature.
[0085] Furthermore, in the above-described embodiment, the case was explained using as an example a case in which the oxygen concentration in the second region 5b of the thermistor film 5 made of an oxide having a spinel-type crystal structure is higher than that in the first region 5a by heat treatment (annealing) at a temperature of 250°C or higher in an atmospheric atmosphere on a thermistor element in the process of manufacturing, in which each layer up to the second surface electrode 6c has been provided. However, the method for manufacturing the thermistor element of the present invention is not limited to the above method, as long as it is possible to form a thermistor film 5 made of an oxide having a spinel-type crystal structure in which the oxygen concentration in the second region 5b is higher than that in the first region 5a.
[0086] Furthermore, the planar shapes of the thermistor film 5, the first electrode 6a, the second surface electrode 6c, and the second electrode 6b of the thermistor element 4 can be changed as appropriate. Furthermore, in the thermistor element 4 of the above-described embodiment, the shape, arrangement, and number of openings 20a and 20b are not necessarily limited to the configuration described above and can be changed as appropriate. [Examples]
[0087] (Example 1) [Method for manufacturing electromagnetic wave sensors] The thermistor element 4 shown in Figure 12 was manufactured using the manufacturing method described below. On a first substrate 2 made of a silicon substrate, the components shown in Figure 4, such as the first insulating layer 8, wiring portion 9, and leg portions 13a and 13b, were formed, and an organic material layer 30 made of resist was provided on the side facing the first insulating layer 8. Next, as shown in Figure 5, a first insulating film 7a made of aluminum oxide (Al2O3) with a thickness of 200 nm was deposited over the entire surface of the organic material layer 30 by sputtering.
[0088] Next, a 60 nm thick conductive film made of titanium (Ti) was deposited over the entire surface of the first insulating film 7a shown in Figure 5 by sputtering. Subsequently, the conductive film was patterned using photolithography. This formed wiring layers 21a and 21b having a predetermined pattern shape, as shown in Figure 6.
[0089] Next, as shown in Figure 7, a second insulating film 7b made of aluminum oxide (Al2O3) with a thickness of 70 nm was deposited over the entire surface of the wiring layers 21a and 21b by sputtering. Next, the second insulating film 7b was patterned using photolithography. As a result, as shown in Figure 8, circular openings 20a and 20b with a diameter of 1.2 μm were formed on the wiring layers 21a and 21b, respectively, penetrating the second insulating film 7b.
[0090] Next, a 30 nm thick conductive film 53 made of platinum (Pt) was deposited over the entire surface of the second insulating film 7b having openings 20a and 20b by sputtering, and the conductive film 53 was embedded in the openings 20a and 20b. Subsequently, the conductive film 53 was patterned using photolithography. As a result, a first surface electrode 6 consisting of a first electrode 6a and a second electrode 6b was formed, as shown in Figure 9.
[0091] Next, as shown in Figure 10, a thermistor material film 54 with a thickness of 100 nm made of an oxide having a spinel-type crystal structure and a conductive film 55 with a thickness of 20 nm made of platinum (Pt) were deposited on the second insulating film 7b on which the first surface electrode 6 is provided, in that order, over the entire surface by sputtering. As the thermistor material film 54, an oxide having a spinel-type crystal structure with base metal elements of Co and Mn and Ni as an additive element was used (Co:Mn:Ni = 43.7 atoms:42.3 atoms:14.0 atoms).
[0092] Next, by patterning the thermistor material film 54 and the conductive film 55 using photolithography technology, a second surface electrode 6c and thermistor film 5, which were patterned to the same shape as each other, were formed, as shown in Figure 11.
[0093] Next, the thermistor element in the manufacturing process, with each layer up to the second surface electrode 6c already formed, was subjected to heat treatment (annealing) in an atmospheric environment at a temperature of 250°C for 1 hour. Next, as shown in Figure 12, a third insulating film 7c made of aluminum oxide (Al2O3) was deposited over the entire surface of the second surface electrode 6c by sputtering. This formed the third insulating film 7c covering the second surface electrode 6c and the sides of the second surface electrode 6c and the thermistor film 5. Subsequently, the organic material layer 30 was removed by ashing. By following the above steps, the thermistor element 4 of Example 1 was obtained.
[0094] The oxygen concentration in the thickness direction of the thermistor film 5 of the thermistor element 4 obtained in this manner was measured using the method described below. ≪Measurement of Oxygen Concentration≫ A thermistor element 4 was fabricated as a thin film using a Dual Beam FIB (Focus Ion Beam) processing and observation system (product name: Helios450F1; manufactured by Thermo Fisher), and a test specimen was prepared. The test specimen was designed to allow observation of the cross-section of the first region 5a of the thermistor film 5, which consists of the region overlapping with the first electrode 6a and the second surface electrode 6c in a plan view, and the region overlapping with the second electrode 6b and the second surface electrode 6c in a plan view, as well as the cross-section of the second region 5b, which is located between the first electrode 6a and the second electrode 6b in a plan view.
[0095] Energy-dispersive X-ray spectroscopy (EDS) (product name: NSS (NORAN System Seven); Thermo Fisher Corporation) was performed on the specimens obtained in this manner, while scanning the specimens from the first electrode 6 side to the second electrode 6c side using a scanning transmission electron microscope (STEM) (product name: ARM200F; manufactured by JEOL Ltd.). This allowed for the measurement of the elemental concentrations of oxygen (O), titanium (Ti), manganese (Mn), nickel (Ni), aluminum (Al), cobalt (Co), and platinum (Pt) in the thickness direction of the cross-sections of the first region 5a and the second region 5b. The results are shown in Figures 13 and 14.
[0096] Figure 13 is a graph showing the relationship between the position in the thickness direction of the cross-section containing the first region 5a of the thermistor element 4 of Example 1 and the concentration of each element. Figure 14 is a graph showing the relationship between the position in the thickness direction of the cross-section containing the second region 5b of the thermistor element 4 of Example 1 and the concentration of each element. In Figures 13 and 14, the horizontal axis represents the position in the thickness direction between the first insulating film 7a and the third insulating film 7c, showing the position (nm) when any position in the first insulating film 7a is set to 0. The vertical axis in Figures 13 and 14 represents the elemental concentration (atomic %).
[0097] In Figures 13 and 14, the platinum (Pt) peaks indicate the positions of the first-side electrode 6 and the second-side electrode 6c in the thickness direction of the test specimen. The titanium (Ti) peaks indicate the positions of the wiring layers 21a and 21b in the thickness direction of the test specimen. The manganese (Mn), nickel (Ni), and cobalt (Co) peaks indicate the positions of the thermistor film 5 in the thickness direction of the test specimen. The aluminum (Al) peaks indicate the positions of the first insulating film 7a, the second insulating film 7b, and the third insulating film 7c in the thickness direction of the test specimen.
[0098] The oxygen (O) peaks in the regions where manganese (Mn), nickel (Ni), and cobalt (Co) are detected, as shown in Figure 13, indicate the oxygen concentration in the thermistor film 5 in region 1 5a. Furthermore, the oxygen (O) peaks in the regions where manganese (Mn), nickel (Ni), and cobalt (Co) are detected, as shown in Figure 14, indicate the oxygen concentration in the thermistor film 5 in region 2 5b.
[0099] As shown in Figure 13, the oxygen concentration in the first region 5a of the thermistor film 5 was in the range of 30 atomic% to 40 atomic%. Also, as shown in Figure 14, the oxygen concentration in the second region 5b of the thermistor film 5 was approximately 50 atomic% and was substantially constant in the thickness direction. From this, it was confirmed that the thermistor film 5 of the thermistor element 4 of Example 1 had a higher oxygen concentration in the second region 5b than in the first region 5a. Furthermore, as shown in Figures 13 and 14, when the thermistor film 5 was divided into three equal regions in the thickness direction—a region close to the second surface electrode 6c, a region far from the second surface electrode 6c, and a region including the center in the thickness direction—it was confirmed that in all three regions, the oxygen concentration in the second region 5b was higher than the oxygen concentration in the first region 5a.
[0100] (Experimental Example 1) A 200 nm thick insulating film made of aluminum oxide (Al2O3) was deposited over the entire surface of a silicon substrate, and then a 100 nm thick thermistor material film made of an oxide having a spinel-type crystal structure was deposited over the entire surface to obtain the laminate of Experimental Example 1. As the thermistor material film, an oxide having a spinel-type crystal structure with Co and Mn as the base metal elements and Ni as the additive element was used (Co:Mn:Ni = 43.7 atoms:42.3 atoms:14.0 atoms).
[0101] (Experimental Example 2) The laminate of Experimental Example 2 was obtained in the same manner as in Experimental Example 1, except that the thermistor material film used was an oxide having a spinel-type crystal structure in which the base metal elements were Mn and Ni, and Fe, Cu, and Zr were added as additive elements (Mn:Ni:Fe:Cu:Zr = 35.1 atoms:32.8 atoms:24.1 atoms:4.9 atoms:3.1 atoms).
[0102] The thermistor material films of the laminates obtained in Experimental Example 1 and Experimental Example 2 were subjected to current in the in-plane direction, and their resistivity was measured using a four-probe sheet resistance meter (product name: Prometrix RS75; manufactured by KLA-Tencor). The results are shown in Table 1.
[0103] Furthermore, the laminates from Experimental Example 1 and Experimental Example 2 were processed into thin films using a Dual Beam FIB (Focus Ion Beam) processing and observation system (product name: Helios450F1; manufactured by Thermo Fisher), and test specimens were prepared.
[0104] Energy-dispersive X-ray diffraction (EDS) (product name: NSS (NORAN System Seven); Thermo Fisher Corporation) was performed on the obtained test specimens using a scanning transmission electron microscope (STEM) (product name: ARM200F; manufactured by JEOL Ltd.), scanning the specimens from the insulating film side to the surface side of the thermistor material film. This allowed for the measurement of the oxygen (O) concentration in the thickness direction in the cross-section of the thermistor material film of the laminates in Experimental Example 1 and Experimental Example 2.
[0105] Subsequently, the thermistor film 5 was divided into three equal regions in the thickness direction: a region close to the insulating film, a region far from the insulating film (a region close to the surface), and a region including the central part in the thickness direction. The arithmetic mean was calculated using the oxygen (O) concentration measurement results from multiple measurement points in the region including the central part, and this was used as the average oxygen concentration of the thermistor material film. The spacing of the measurement points in the thickness direction was set to 2.4 nm. The results are shown in Table 1.
[0106] Furthermore, the laminates of Experimental Example 1 and Experimental Example 2 were subjected to heat treatment (annealing) at 250°C for 1 hour in an air atmosphere. Subsequently, in the same manner as before the heat treatment, an electric current was passed through the thermistor material film of the laminates of Experimental Example 1 and Experimental Example 2 in the in-plane direction, and the resistivity was measured. The results are shown in Table 1.
[0107] Furthermore, test specimens were taken from the laminates of Experimental Example 1 and Experimental Example 2 after heat treatment (annealing) using the same method as before heat treatment. The oxygen concentration in the thickness direction was measured in the same manner as before heat treatment, and the average oxygen concentration of the thermistor material film was calculated. The results are shown in Table 1.
[0108] [Table 1]
[0109] As shown in Table 1, in both Experimental Example 1 and Experimental Example 2, the thermistor material film after heat treatment had a higher oxygen concentration compared to the thermistor material film before heat treatment. Furthermore, in both Experimental Example 1 and Experimental Example 2, the thermistor material film with a relatively high oxygen concentration after heat treatment exhibited higher resistivity compared to the thermistor material film with a relatively low oxygen concentration before heat treatment. [Explanation of Symbols]
[0110] 1...Electromagnetic wave sensor 2...First substrate 3...Second substrate 4...Thermistor element 5...Thermistor film 5a...First region 5b...Second region 6...First side electrode 6a...First electrode 6b...Second electrode 6c...Second side electrode 7a...First insulating film 7b...Second insulating film 7c...Third insulating film 8...First insulator layer 9...Wiring section 9a...First lead wiring 9b...Second lead wiring 10...First connection section 11a, 11b...First connecting member 12a, 12b...Arm section 13a, 13b...Leg section 14...Second insulator layer 15...Circuit section 16...Second connection section 17a, 17b...Connection terminal 18a, 18b...Second connecting member 20a, 20b...Opening, 21a, 21b...Wiring layer, 30...Organic material layer; 53, 55...Conductive film; 54...Thermistor material film; E...Region; G...Space; IR...Infrared; K...Internal space; W...Window area.
Claims
1. A thermistor film made of an oxide having a spinel-type crystal structure, A first surface side electrode provided in contact with the first surface of the thermistor film, The device comprises a second surface side electrode provided in contact with the second surface of the thermistor film, The first surface electrode comprises a first electrode and a second electrode positioned spaced apart from the first electrode in a plan view, wherein at least a portion of the first electrode and at least a portion of the second electrode are positioned to overlap with the second surface electrode in a plan view. The thermistor element is characterized in that the oxygen concentration in the second region located between the first electrode and the second electrode in a plan view is higher than that in the first region, which consists of a region overlapping with the first electrode and the second side electrode in a plan view and a region overlapping with the second electrode and the second side electrode in a plan view.
2. An electromagnetic wave sensor characterized by comprising the thermistor element described in claim 1.
3. The electromagnetic wave sensor according to claim 2, characterized in that it comprises a plurality of thermistor elements, wherein the plurality of thermistor elements are arranged in an array.
Citation Information
Patent Citations
Infrared detector
JP1990196929A
Variable-resistance element and its manufacturing method and its driving method
JP2008235427A
Method for manufacturing segmented contacts for radiation detectors using direct photolithography
JP2009527922A
Thin film thermistor element