Low-hydrogen coated arc welding rods
A low-hydrogen coated arc welding rod with a tailored composition addresses arc stability and burn-back issues, ensuring stable arcs and high-quality welds with improved mechanical properties.
Patent Information
- Application Number
- JP2023045696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Low-hydrogen coated arc welding electrodes suffer from poor arc stability, slow melting rate, convex bead shape, and burn-back phenomena during high-current welding, leading to welding defects and reduced efficiency.
A low-hydrogen coated arc welding rod with a specific composition of calcium carbonate, barium carbonate, fluorite, titanium oxide, silicon oxide, sodium and potassium compounds, magnesium oxide, manganese, iron, and nickel, applied at a controlled coverage rate, to enhance arc stability and resistance to burn-back.
The rod provides stable arcs, improved bead shape, and reduced burn-back, resulting in high-quality welded joints with enhanced mechanical performance and reduced welding defects.
Smart Images

Figure 0007955203000001 
Figure 0007955203000002 
Figure 0007955203000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a low-hydrogen coated arc welding electrode, and more particularly to a low-hydrogen coated arc welding electrode with excellent burn-back resistance. [Background Art]
[0002] Low-hydrogen coated arc welding electrodes consist of a basic coating containing metal carbonates and metal fluorides as main components, and are widely used because they can produce weld metals with excellent mechanical properties. However, compared to ilmenite-type or lime-titania-type electrodes, these low-hydrogen electrodes have drawbacks such as poor arc stability, slow melting rate, poor bead elongation, and convex bead shape, resulting in poor welding workability. Furthermore, when welding under high-current conditions for high-efficiency welding, while the welding efficiency improves, the steel core wire generates heat in the latter half of the electrode, causing the coating to burn, that is, a burn-back phenomenon (hereinafter referred to as "burn-back"). Using an electrode that has undergone burn-back leads to unstable arcs during welding, not only deteriorating welding workability but also causing welding defects such as blowholes and incomplete penetration.
[0003] Various proposals have been made to improve arc stability in response to these issues. For example, Patent Document 1 discloses a technique for improving arc stability in low-current ranges to reduce welding heat input. According to this technique, the arc in low-current ranges is stabilized by controlling the particle size distribution of calcium carbonate and the content of mica. However, the arc concentration and arc stability in the appropriate current range are poor, which is likely to cause welding defects such as incomplete fusion.
[0004] Furthermore, the coated arc welding electrode described in Patent Document 2 can improve the arc stability and mechanical performance of weld metals, which have been considered problems with conventional low-hydrogen coated arc welding electrodes, but it has been difficult to improve burn-back resistance. [Prior Art Documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-276081 [Patent Document 2] Japanese Patent Application Publication No. 57-72790 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] This invention was devised in view of the above-mentioned problems, and aims to provide a low-hydrogen coated arc welding rod that is less prone to burning even when welding under high-current welding conditions. [Means for solving the problem]
[0007] The gist of this invention is, (1) In a low-hydrogen coated arc welding rod in which a coating agent is applied to a steel core wire, the coating agent consists of, in mass % of the total mass of the coating agent, calcium carbonate: 25-55%, barium carbonate: 2-6%, fluorite: 10-25%, and fluorite particles with a particle size of 75 μm or larger in weight % of fluorite: 70% or more, total Ti oxide equivalent value: 2.0-5.0%, total Si oxide equivalent value: 4-10%, and Na equivalent value of Na compounds. The coating agent is characterized by containing the following components: a total of 1.6-2.5% of one or more K compounds in terms of K equivalent value, a total of 0.12-0.40% of Mg oxides in terms of MgO equivalent value, 2-6% of Si, 2.0-5.5% of Mn, and 5-15% of Fe, with Mg being 1.0% or less and Ti being 1.0% or less, and the remainder consisting of coating agents and impurities, which is applied to a steel core wire at a coating rate of 25-40% by mass relative to the total mass of the low-hydrogen coated arc welding rod.
[0008] (2) The low hydrogen coated arc welding rod according to (1), characterized in that it further contains, by mass % of the total mass of the coating, Ni: 0.5 to 10.0%, and the sum of the B equivalent values of one or more metals B, B alloys and B oxides: 0.05 to 0.50%.
[0009] (3) The low hydrogen coated arc welding rod according to (1) or (2), characterized in that it further contains Mo: 0.5 to 2.0% by mass relative to the total mass of the coating agent. [Effects of the Invention]
[0010] The present invention provides a low-hydrogen coated arc welding rod that is less prone to burning even when welding under high current welding conditions, and that offers good welding workability and mechanical performance, resulting in a high-quality welded joint. [Modes for carrying out the invention]
[0011] To solve the above-mentioned problems, the inventors of the present invention conducted a detailed study on the composition of the coating agent for a low-hydrogen coated arc welding rod that is less prone to burning even when welding under high-current welding conditions, and also has good weldability and mechanical performance.
[0012] As a result, we found that by adjusting the amounts of calcium carbonate, barium carbonate, fluorite, the particle size of fluorite, the sum of the TiO2 equivalent values of Ti oxide, the sum of the SiO2 equivalent values of Si oxide, the sum of one or more Na equivalent values of Na compounds and K equivalent values of K compounds, the sum of the MgO equivalent values of Mg oxide, Si, Mn, Fe, Mg, and Ti, and setting the coverage rate to 25-40%, welding rod burning is less likely to occur even under high current welding conditions, and welding workability and mechanical performance can be improved. Further investigations led to the completion of the present invention.
[0013] The following will explain in detail the reasons for limiting the composition of each component in the coating for the low-hydrogen coated arc welding rod in the present invention. The content of each component in the composition of the low-hydrogen coated arc welding rod will be expressed as a mass % relative to the total mass of the coating, and when expressing the mass %, it will simply be written as %.
[0014] [Calcium carbonate: 25-55%] Calcium carbonate decomposes in the heat of the arc, generating CO2 gas, which protects the weld metal from the atmosphere. If the calcium carbonate content is less than 25%, the shielding effect is insufficient, and blowholes are more likely to occur. Also, if the calcium carbonate content is less than 25%, nitrogen from the atmosphere is mixed into the weld metal, reducing its toughness. On the other hand, if the calcium carbonate content exceeds 55%, the arc becomes unstable, the bead shape becomes convex, and the slag detachability also deteriorates. Therefore, the calcium carbonate content should be between 25% and 55%.
[0015] [Fluorite: 10~25%] [More than 70% of particles have a particle size of 75 μm or larger] Fluorite has the effect of improving the appearance of the weld bead by adjusting the fluidity of the molten slag. If the fluorite content is less than 10%, the fluidity of the molten slag deteriorates, the slag coating becomes unstable, and the appearance of the bead deteriorates. On the other hand, if the fluorite content exceeds 25%, the shape of the coating tube becomes incomplete, resulting in a one-sided melting state and an unstable arc. Therefore, the fluorite content should be between 10% and 25%. Furthermore, if the fluorite contains less than 70% particles with a particle size of 75 μm or larger, the resistance to rod burning deteriorates, the shielding effect becomes insufficient in the latter half of welding, and blowholes are more likely to occur. Therefore, the fluorite content should contain 70% or more particles with a particle size of 75 μm or larger.
[0016] [Total Ti oxide content in TiO2 equivalent: 2.0-5.0%] Titanium oxides are added from sources such as rutile, titanium oxide, titanium slag, and calcium titanate to adjust the viscosity of the molten slag and improve the bead shape. If the TiO2 equivalent value of the Ti oxide is less than 2.0%, the viscosity of the slag decreases, resulting in a poor bead shape. On the other hand, if the TiO2 equivalent value of the Ti oxide exceeds 5.0%, the viscosity of the molten slag increases, reducing its fluidity, and resulting in a convex bead shape. Therefore, the TiO2 equivalent value of the Ti oxide should be between 2.0% and 5.0%.
[0017] [Total SiO2 equivalent value of Si oxide: 4-10%] Si oxide is added from silica sand, feldspar, water glass, etc., and has the effect of increasing the viscosity of the molten slag, ensuring slag with an appropriate viscosity, and improving the bead shape. If the total SiO2 equivalent value of Si oxide is less than 4%, the viscosity of the molten slag will be low, resulting in a poor bead shape. On the other hand, if the total SiO2 equivalent value of Si oxide exceeds 10%, the slag will become glassy, and the slag peelability will be poor. Therefore, the total SiO2 equivalent value of Si oxide is set to 4 to 10%.
[0018] [Barium carbonate: 2 to 6%] Barium carbonate has the effect of lowering the arc voltage and improving arc stability. If the barium carbonate content is less than 2%, the arc will become unstable and the bead appearance will be poor. On the other hand, if the barium carbonate content exceeds 6%, the arc will become too weak and unstable. Therefore, the barium carbonate content is set to 2 to 6%.
[0019] [Total of one or more of the Na equivalent value of the Na compound and the K equivalent value of the K compound: 1.6 to 2.5%] Na compounds and K compounds are mainly added from water glass such as sodium silicate and potassium silicate, and have the effect of improving the coating property during welding rod manufacturing and the arc stability during welding. They are also added from potassium feldspar, sodium fluoride, and sodium borate, and are necessary for ensuring welding workability. If the total of one or more of the Na equivalent value of the Na compound and the K equivalent value of the K compound is less than 1.6%, the arc will become unstable. In addition, cracks are likely to occur on the surface of the coating agent during welding rod manufacturing, and the peeling resistance is reduced. On the other hand, if the total of one or more of the Na equivalent value of the Na compound and the K equivalent value of the K compound exceeds 2.5%, the arc spray will be strong and unstable. Therefore, the total of one or more of the Na equivalent value of the Na compound and the K equivalent value of the K compound is set to 1.6 to 2.5%.
[0020] [Total MgO equivalent value of Mg oxide: 0.12 to 0.40%] Mg oxide is added from magnesium oxide, magnesia clinker, or the like, and has good reaction curability with potassium silicate and sodium silicate, excellent heat resistance, and improves the adhesion of the coating agent to enhance the coating agent's spalling resistance and rod burn resistance. If the total MgO equivalent of Mg oxide is less than 0.12%, curability and heat resistance are insufficient, resulting in poor spalling resistance and rod burn resistance. On the other hand, if the total MgO equivalent of Mg oxide exceeds 0.40%, the viscosity of the molten slag increases, causing the bead shape to become convex. Therefore, the total MgO equivalent of Mg oxide is set to 0.12 to 0.40%.
[0021] [Mg: 1.0% or less] Mg is added from metallic Mg, Al-Mg, or the like, and has higher reactivity than other alloying components, thus improving the meltability of the coating. It also has the effect of lowering the potential gradient of the arc to stabilize the voltage, resulting in good arc continuity and enabling arc stabilization. On the other hand, if Mg exceeds 1.0%, the coating becomes excessively molten, the arc spread deteriorates and becomes unstable, and the bead shape becomes poor. Therefore, Mg is set to 1.0% or less.
[0022] [Si: 2 to 6%] Si is added from metallic Si, Fe-Si, Fe-Si-Mn, or the like, and is used for deoxidizing the weld metal, as well as being necessary from the viewpoint of welding workability. If Si is less than 2%, deoxidation is insufficient, and blowholes are likely to occur in the weld metal. On the other hand, if Si exceeds 6%, low-melting-point oxides precipitate at the grain boundaries of the weld metal, reducing the toughness of the weld metal. Therefore, Si is set to 2 to 6%.
[0023] [Mn: 2.0 to 5.5%] Mn is added from metallic Mn, Fe-Mn, Fe-Si-Mn, or the like, and is important as a deoxidizer similarly to Si, and has the effect of refining the weld metal structure to enhance the toughness and strength of the weld metal. If Mn is less than 2.0%, the strength of the weld metal is low, deoxidation is insufficient, and blowholes are likely to occur in the weld metal. On the other hand, if Mn exceeds 5.5%, hardenability acts strongly, the strength of the weld metal becomes excessively high, and toughness decreases. Therefore, Mn is set to 2.0 to 5.5%.
[0024] [Fe: 5~15%] Fe is added from iron powder, iron alloy powders such as Fe-Mn and Fe-Mo, or iron oxides. It has the effect of lowering the arc potential gradient, shortening the arc length, and preventing uneven melting of the coating. If the Fe content is less than 5%, the arc length becomes long, the arc is prone to disappearing during welding, and the arc becomes unstable. On the other hand, if the Fe content exceeds 15%, the amount of slag material decreases, resulting in uneven slag coverage and poor bead shape. Therefore, the Fe content should be between 5% and 15%.
[0025] [Ti: 1.0% or less] Ti, added from sources such as metallic Ti and Fe-Ti, is effective as a deoxidizing agent and also refines the microstructure of the weld metal, improving its toughness. On the other hand, if the Ti content exceeds 1.0%, the precipitation of Ti oxides in the weld metal increases, reducing the toughness of the weld metal. Therefore, the Ti content should be kept below 1.0%.
[0026] [Coverage: 25-40% by mass of coating agent relative to the total mass of the low-hydrogen coated arc welding electrode] The coverage rate of the coating on the outer circumference of the steel core wire greatly affects the shielding resistance during welding. If the coverage rate is less than 25% of the total mass of the coating relative to the total mass of the low-hydrogen coated arc welding electrode (hereinafter simply referred to as %), there will be insufficient coating material, resulting in inadequate shielding, an increase in the nitrogen content in the weld metal, and a decrease in the toughness of the weld metal. On the other hand, if the coverage rate exceeds 40%, the amount of slag will be excessive, making the arc unstable. Therefore, the coverage rate should be between 25% and 40%.
[0027] [Ni: 0.5~10.0%] Ni is an element added from metallic nickel to improve the toughness of the weld metal. Below 0.5% Ni, no improvement in toughness is observed. Conversely, if Ni exceeds 10.0%, the strength of the weld metal becomes excessively high, and its toughness decreases. Therefore, Ni should be between 0.5% and 10.0%.
[0028] [Total equivalent value of one or more B components from metal B, B alloys, and B oxides: 0.05~0.50%] B is an element added from metal B, Fe-B, Fe-Mn-B, borax, colemanite, etc., and is effective in improving hardenability and suppressing the formation of grain boundary ferrites in trace amounts, thus improving the toughness of the weld metal. If the sum of the B equivalent values of one or more types of metal B, B alloys, and B oxides is less than 0.05%, the effect of improving toughness will not be obtained. On the other hand, if the sum of the B equivalent values of one or more types of metal B, B alloys, and B oxides exceeds 0.50%, the strength of the weld metal will become excessively high and the toughness will decrease. Therefore, the sum of the B equivalent values of one or more types of metal B, B alloys, and B oxides should be between 0.05% and 0.50%.
[0029] [Total Mo: 0.5-2.0%] Mo (Mo), added from sources such as metallic Mo or Fe-Mo, has the effect of further improving the strength of the weld metal. Below 0.5% Mo, no strength improvement is observed. On the other hand, if Mo exceeds 2.0%, the strength of the weld metal becomes excessively high, and its toughness decreases. Therefore, the total Mo content should be between 0.5% and 2.0%.
[0030] Furthermore, the remainder of the coating agent in the low-hydrogen coated arc welding rod of the present invention consists of the paint agent and impurities contained in the alloy powder. The paint agent may be hectorite, mica, or the like, preferably one or more of these in total amount of 5% or less. [Examples]
[0031] The effects of the present invention will be specifically explained below with reference to examples.
[0032] In this embodiment, using a welding rod coating machine, various low-hydrogen coated arc welding rods were prototyped by coating a 4 mm diameter, 400 mm long steel core wire with the composition components shown in Table 1 with the coating components shown in Tables 2 and 3 at the coverage rate shown in Table 2, and then drying them.
[0033] In addition, the "-" notation in Tables 1, 2, and 3 indicates that the ingredient has been intentionally omitted.
[0034] [Table 1]
[0035] [Table 2]
[0036] [Table 3]
[0037] We investigated the burn resistance, coating shedding rate, welding workability, mechanical performance, and welding defects of the manufactured welding rods.
[0038] [Rubber burn resistance] Resistance to rod burning was assessed by performing downward welding at 200A until the remaining welding rod length was 50-60mm. A good test was defined as one where the coating was sound, a clear protective tube was formed at the tip of the welding rod, and there was no rod burning.
[0039] [Shedding rate of the covering] The resistance to shedding was evaluated by measuring the shedding rate of the coating. Approximately 1.5 kg of welding rod was placed in a 55 mm x 300 mm x 500 mm steel box made of 6 mm thick plate. The box was rotated for 5 minutes at a speed of 40 revolutions per minute around its longitudinal axis, and the weight percentage of the coating that detached was measured. A shedding rate of less than 2.0% was considered good.
[0040] [Welding workability] The weldability was evaluated using steel plates conforming to JIS G 3106 SM490A, with a thickness of 16 mm, a width of 100 mm, and a length of 450 mm. AC welding was performed using downward, horizontal fillet, and vertical upward welding, and an overall subjective evaluation was conducted.
[0041] (Arc state) A stable welding process was defined as one in which the arc did not disappear during welding, a constant arc length was obtained, and the arc's straightness was undisturbed.
[0042] (Bead shape) A good result was achieved when both ends were aligned, and the excess bead height, bead width, wave pattern, and surface condition were consistent.
[0043] (Slag fluidity) A good welding result was defined as one in which a sound molten pool was obtained during welding, molten slag did not enter the molten pool, and molten slag did not come into contact with the tip of the welding rod.
[0044] (Slag detachability) After welding, when the solidified slag was struck with a chipping hammer, it was considered good if the slag cracked and could then be easily removed.
[0045] [Evaluation of machine performance] Using 20mm thick steel plates conforming to JIS G 3106 SM490A, weld metal test specimens were prepared according to JIS Z 3211, with alternating current (AC), a welding current of 150-170A, and preheating / interpass temperatures of 90-110°C.
[0046] Mechanical performance was evaluated by the tensile strength of the weld metal and the average absorbed energy of three Charpy impact tests at -30°C. Products with a tensile strength of 490 MPa or higher and an absorbed energy of 80 J or higher were considered good.
[0047] [Welding defects] Welding defects (such as blowholes) were assessed in the weld metal according to JIS Z 3104 "Radiographic Testing Method for Steel Welded Joints" before taking mechanical test specimens. From the radiographs, it was determined which of the four types of defects (Type 1 to 4) it belonged to, according to "Appendix 4, Table 1: Types of Defects," and the defects were classified into four categories (Types 1 to 4) in "6. Classification of Defects." Of these, Type 1 was classified as A, Type 2 as B, and Type 3 and Type 4 as C, with A and B being good and C being poor.
[0048] These analysis results and survey findings are summarized in Table 4.
[0049] [Table 4]
[0050] Welding rods No. 1 to 15 in Tables 2 and 3 are examples of the present invention, and welding rods No. 16 to 31 are comparative examples. Welding rods No. 1 to 15, which are examples of the present invention, consist of appropriate amounts of calcium carbonate, barium carbonate, fluorite, fluorite particle size, sum of Ti oxide equivalent values (TiO2), sum of Si oxide equivalent values (SiO2), sum of one or more Na equivalent values of Na compounds and K equivalent values of K compounds, sum of Mg oxide equivalent values (MgO), and appropriate amounts of Si, Mn, Fe, Mg, and Ti, in mass % of the total mass of the coating. The coating was applied to the steel core wire in an appropriate amount in mass % of the total mass of the welding rod. As a result, in these examples of the present invention, the arc was stable, the bead shape was good, the slag flowability was good, the slag peelability was good, the rod burn resistance was good, the coating peeling rate was low, and there were no welding defects. Furthermore, in these examples of the present invention, the mechanical properties of the tensile strength and absorbed energy of the weld metal were good. Furthermore, welding rods No. 2, 3, 5, 7, 10, 12, and 14 had an appropriate amount of Ni, and welding rods No. 1, 6, 7, 8, 11, 13, and 14 had an appropriate sum of B equivalent values for one or more types of metal B, B alloys, and B oxides, resulting in better absorbed energy. On the other hand, welding rods No. 1, 2, 3, 8, 9, 10, 11, 13, and 14 had an appropriate amount of Mo, resulting in better tensile strength.
[0051] In comparative examples, welding rods No. 16 to 31 failed one or more evaluation items because the components, in terms of mass % of the total mass of the coating agent, were outside the range specified in this disclosure.
[0052] Welding rod No. 16 had a low calcium carbonate content, which resulted in blowholes in the weld metal and low absorbed energy. Also, the Na compound... Na equivalent value and K compound K equivalent value Because the sum of one or more of the above types was low, the arc was unstable and the rate of coating shedding was high. Furthermore, because the sum of the B equivalent values was low, no further improvement in absorbed energy was achieved.
[0053] Welding rod No. 17 had a low absorption energy due to its high Si content. Furthermore, its low Fe content resulted in an unstable arc. Additionally, its low Ni content prevented any further improvement in absorption energy.
[0054] Welding rod No. 18 had a low manganese content, resulting in low weld metal strength and the occurrence of blowholes. Furthermore, its low molybdenum content did not provide any further improvement in strength.
[0055] Welding rod No. 19 had a high calcium carbonate content, which resulted in an unstable arc, a convex bead shape, and poor slag detachability. Furthermore, its low silicon content caused blowholes to form in the weld metal.
[0056] Welding rod No. 20 had a low barium content, resulting in an unstable arc and poor bead appearance. Furthermore, its high total SiO2 equivalent value led to poor slag release properties.
[0057] Welding rod No. 21 had a high barium carbonate content, which resulted in an unstable arc. Additionally, the high total TiO2 equivalent value worsened the slag's fluidity, leading to a convex weld bead shape.
[0058] Welding rod No. 22 had a low fluorite content, resulting in poor slag fluidity and a poor bead shape. Furthermore, its low total MgO equivalent value led to poor resistance to burning and a high rate of coating shedding.
[0059] Welding rod No. 23, due to its high fluorite content, resulted in uneven melting and an unstable arc. Furthermore, its high B equivalent value resulted in high strength and low absorbed energy.
[0060] Welding rod No. 24 had a low total TiO2 equivalent value, resulting in a poor bead shape.
[0061] Furthermore, the high manganese content resulted in high intensity and low absorbed energy.
[0062] Welding rod No. 25 had a low total SiO2 equivalent value, resulting in low slag fluidity and poor bead shape. Additionally, its high Ti content resulted in low absorbed energy.
[0063] Welding rod No. 26 is a sodium compound Na equivalent value and K compound K equivalent value The presence of one or more of these elements in total resulted in an unstable arc. Additionally, the high Mo content led to high intensity and low absorbed energy.
[0064] Welding rod No. 27 had a high total MgO equivalent value, resulting in poor slag fluidity and a convex bead shape. Additionally, its high Ni content resulted in high strength and low absorbed energy.
[0065] Welding rod No. 28 had poor resistance to burning due to a low number of fluorite particles with a particle size of 75 μm or larger, resulting in blowholes in the weld metal. Furthermore, the high Fe content resulted in poor bead shape.
[0066] Welding rod No. 29 had a low absorption energy due to a low coating density. Furthermore, the high Mg content resulted in an unstable arc and poor bead shape.
[0067] The welding rod No. 30 had a high coating rate, resulting in an unstable arc. Furthermore, the low total TiO2 equivalent value led to a poor bead shape.
[0068] Welding rod No. 31 had a low total SiO2 equivalent value, resulting in low slag fluidity and poor bead shape. Also, the Na compound... Na equivalent value and K compound K equivalent value The arc was unstable because there was a high proportion of one or more of these elements combined.
Claims
1. In a low-hydrogen coated arc welding rod in which a coating agent is applied to the steel core wire, The coating agent is, in mass % of the total mass of the coating agent, Calcium carbonate: 25-55%, Barium carbonate: 2-6%, Fluorite: 10-25%, and fluorite particles with a grain size of 75 μm or larger by weight: 70% or more. Ti oxide TiO 2 Total converted value: 2.0-5.0% SiO 2 Total conversion value: 4-10% The sum of one or more of the sodium equivalent values of sodium compounds and the potassium equivalent values of potassium compounds: 1.6–2.5% Total Mg oxide equivalent value: 0.12–0.40% Si: 2-6%, Mn: 2.0 to 5.5%, Fe: Contains 5-15%, Mg: 1.0% or less, Ti: 1.0% or less, A low-hydrogen coated arc welding rod characterized by coating the steel core wire with a coating agent consisting of the remainder being a paint agent and impurities, at a coating rate of 25 to 40% by mass relative to the total mass of the low-hydrogen coated arc welding rod.
2. In mass % of the total mass of the coating agent, Ni: 0.5-10.0%, The low-hydrogen coated arc welding electrode according to claim 1, further characterized by containing one or more of the following B equivalent values: 0.05 to 0.50% of one or more of metal B, B alloys, and B oxides.
3. In mass % of the total mass of the coating agent, A low-hydrogen coated arc welding rod according to claim 1 or 2, further characterized by containing Mo: 0.5 to 2.0%.
Citation Information
Patent Citations
Low hydrogen type coated electrode for vertical down welding
JP1982072790A
Manufacture of low-hydrogen type coated electrode
JP1982160597A
Low hydrogen type coated electrode
JP1995276081A
Lime-based covered electrode, welding method and welded joint
JP2005279767A
Coated electrode and coated arc welding method
JP2020040094A