Submerged arc welding method for high-tensile steel

The submerged arc welding method optimizes bond flux and solid wire compositions to achieve stable weld metal strength, low-temperature toughness, and low diffusible hydrogen content, addressing the limitations of existing methods and ensuring high-quality welds.

JP7955209B2Active Publication Date: 2026-11-24NIPPON STEEL WELDING & ENGINEERING CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023051557
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2026-11-24
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing submerged arc welding methods for high-tensile steel fail to achieve stable weld metal strength, low-temperature toughness, low diffusible hydrogen content, and good welding workability, often resulting in welding defects and inadequate mechanical performance.

Method used

A submerged arc welding method using a bond flux composition of SiO2: 5-20%, CaO: 5-20%, MgO: 25-35%, Al2O3: 10-20%, CaF2: 23-35%, CO2 equivalent values of CaCO3 and MgCO3: 2-7%, Si: 0.3-2.0%, Na2O and K2O: 1-5%, with 0.1% TiO2, and a solid wire composition of C: 0.08-0.15%, Si: 0.1-0.3%, Mn: 1.5-2.5%, Ni: 2.0-3.0%, Mo: 0.5-1.5%, Ti: 0.02-0.08%, Al: 0.05% or less, P: 0.015% or less, S: 0.015% or less, with the remainder being Fe and unavoidable impurities, to optimize chemical components for improved slag properties and metal strength.

Benefits of technology

The method provides stable weld metal strength, low-temperature toughness, low diffusible hydrogen content, and good welding workability, ensuring high-efficiency and high-quality welds without defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955209000001
    Figure 0007955209000001
  • Figure 0007955209000002
    Figure 0007955209000002
  • Figure 0007955209000003
    Figure 0007955209000003
Patent Text Reader

Abstract

To provide a submerged arc welding method by which stable strength and low-temperature toughness of a weld metal can be obtained, the amount of diffusible hydrogen in the weld metal is low, there is no weld defect, and welding workability is excellent.SOLUTION: In a submerged arc welding method for high-tensile strength steel, welding is performed by combining: a bond flux which comprises CO2 conversion value: 2-7% of one or two of SiO2: 5-20%, CaO: 5-20%, MgO: 25-35%, Al2O3: 10-20%, CaF2: 23-35%, CaCO3 and MgCO3, the total: 1-5% of one or two of Si: 0.3-2.0%, Na2O and K2O, and TiO2: 0.1% or less; and a solid wire which comprises C: and 0.08-0.15%, Si: 0.1-0.3%, Mn: 1.5-2.5%, Ni: 2.0-3.0%, Mo: 0.5-1.5%, Ti: 0.02-0.08%, Al: 0.05% or less, P: 0.015% or less, and S: 0.015% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a submerged arc welding method for 780 MPa-class high-tensile strength steel, and more particularly to a submerged arc welding method that provides stable weld metal strength and low-temperature toughness, a low amount of diffusible hydrogen in the weld metal, no weld defects, and excellent weld workability.

Background Art

[0002] Submerged arc welding is applied in a wide range of fields, such as shipbuilding, steel frames, pipe manufacturing, bridges, and vehicles, because it provides weld metal with high efficiency, good welding workability, and excellent mechanical performance.

[0003] In recent years, with the development of the energy industry, studies have been conducted on increasing the strength and toughness of steel materials, and on increasing the plate thickness along with the increase in the size of structures. From the viewpoints of quality and productivity, the application ratio of submerged arc welding is increasing year by year. In such submerged arc welding of high-tensile strength steel, further quality improvement is required to improve productivity and ensure safety and durability during welding. Among these, there is a demand for higher welding efficiency and weld metal strength and toughness that match the steel material properties. Compared to covered arc welding and gas shielded arc welding, submerged arc welding has a higher welding heat input and a higher base metal dilution rate, so the weld workability and weld metal performance are almost determined by the component composition of the flux and wire. In submerged arc welding of high-tensile strength steel, bonded flux is used, which allows the chemical composition of the weld metal to be freely adjusted in order to ensure the strength and toughness of the weld metal that matches the steel material. However, in the welding of high-tensile strength steel, it is not possible to obtain high strength and high toughness of the weld metal simply by adding alloy components to the bonded flux. Therefore, in order to obtain appropriate strength and toughness of the weld metal, it is necessary to include alloy components such as Si and Mn in the solid wire to be combined, and to consider the chemical components of both the flux and the solid wire together to select the optimal combination.

[0004] Considering these points, various technological developments have been carried out to develop submerged arc welding methods for high-tensile steel that can obtain good weldability and weld metal mechanical performance.

[0005] For example, Patent Document 1 discloses a bond flux and wire for submerged arc welding that, by optimizing the composition of the bond flux and wire, can produce a weld metal with high strength and excellent low-temperature toughness down to -60°C. However, the bond flux described in Patent Document 1 contains only a small amount of CaF2, resulting in low basicity of the slag, and the Si and Ti in the solid wire are not appropriate, so -60°C below However, this presented a problem: it was not possible to obtain weld metal with stable low-temperature toughness.

[0006] Furthermore, Patent Document 2 discloses a weld metal that achieves high strength and excellent toughness down to -20°C by optimizing the composition of the weld metal obtained by combining a solid wire and bond flux. However, the CaF2 in the bond flux and the Si and Ti in the solid wire used to obtain the weld metal described in Patent Document 2 are not appropriate, so -60°C below There was a problem in that weld metal with good low-temperature toughness could not be obtained.

[0007] Furthermore, Patent Document 3 discloses a submerged arc welding method for high-tensile steel, in which excellent toughness down to -30°C can be obtained in both as-welded and PWHT by specifying the composition of the bond flux and the carbon equivalent of the solid wire. However, because the Ni and Ti of the solid wire described in Patent Document 3 are not appropriate, -60°C below There was a problem in that weld metal with good low-temperature toughness could not be obtained.

[0008] Furthermore, Patent Document 4 discloses a technique for submerged arc welding of high-tensile steel in which a weld metal with high strength and good low-temperature toughness can be obtained by optimizing the composition of the bond flux and lowering the Si content of the solid wire to bring the carbon equivalent into an appropriate range. However, the bond flux described in Patent Document 4 has a low CaF2 content and a low Si content in the wire, which results in a high oxygen content in the weld metal, and thus the problem is that even better and more stable low-temperature toughness cannot be obtained even at -60°C. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 2013-39604 [Patent Document 2] Japanese Patent Publication No. 2007-260696 [Patent Document 3] Japanese Patent Application Publication No. 8-257789 [Patent Document 4] Japanese Patent Application Publication No. 5-212583 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] The present invention was devised in view of the above-mentioned problems, and relates to a submerged arc welding method for 780 MPa class high-tensile steel, with the aim of providing a submerged arc welding method that can obtain stable weld metal strength and low-temperature toughness, has a low diffusible hydrogen content in the weld metal, is free from welding defects, and has good welding workability. [Means for solving the problem]

[0011] The gist of the present invention is a submerged arc welding method for high-tensile steel, wherein the bond flux composition, in mass %, is as follows: SiO2: 5-20%, CaO: 5-20%, MgO: 25-35%, Al2O3: 10-20%, CaF2: 23-35%, CO2 equivalent values ​​of one or two of CaCO3 and MgCO3: 2-7%, Si: 0.3-2.0%, and one or of Na2O and K2O. Total of 2 types The present invention relates to a submerged arc welding method for high-tensile steel, characterized by welding a bond flux consisting of 1-5% of iron alloy and 0.1% or less of TiO2, with the remainder being Fe from the iron alloy and unavoidable impurities, and a solid wire consisting of C: 0.08-0.15%, Si: 0.1-0.3%, Mn: 1.5-2.5%, Ni: 2.0-3.0%, Mo: 0.5-1.5%, Ti: 0.02-0.08%, Al: 0.05% or less, P: 0.015% or less, and S: 0.015% or less, with the remainder being Fe, Cu from the copper plating on the wire surface and unavoidable impurities, in mass % of the total mass of the solid wire. [Effects of the Invention]

[0012] The submerged arc welding method for high-tensile steel to which the present invention is applied provides stable weld metal strength and low-temperature toughness, low diffusible hydrogen content in the weld metal, no welding defects, and good welding workability, making it possible to provide high-efficiency, high-quality welds. [Modes for carrying out the invention]

[0013] The inventors of the present invention, in order to solve the above-mentioned problems in submerged arc welding of 780 MPa class high-tensile steel, fabricated and investigated various chemical compositions of bond flux for submerged arc welding (hereinafter referred to as "bond flux") and the chemical components of solid wire to be combined with it. As a result, they found that by including appropriate amounts of CaO, MgO, and CaF2 in the flux to increase the basicity of the slag, and by adding an appropriate amount of Si, a deoxidizing element, and by setting the C, Si, Mn, Ni, Mo, and Ti of the combined solid wire within appropriate ranges, the strength and oxygen content of the weld metal can be optimized, and stable low-temperature toughness can be obtained. They also found that the amount of diffusible hydrogen can be reduced by adjusting the amount of metal carbonate in the flux. Furthermore, they found that the welding workability can be improved by adjusting the amounts of Na2O, K2O, and Al2O3 for arc stability, and by including an appropriate amount of SiO2 for slag detachability.

[0014] First, the reasons for limiting the bond flux component composition used in the submerged arc welding method to which the present invention is applied will be explained below. In the following, the percentages for each component represent the mass percentage relative to the total mass of the bond flux.

[0015] [SiO2: 5~20%] SiO2 is an important component for adjusting the viscosity of slag and forming a good weld bead. Adding SiO2 gives the slag a glassy texture, resulting in a slag that is easily broken and has good release properties. If the SiO2 content is less than 5%, the slag release properties deteriorate, and undercuts become more likely. On the other hand, if the SiO2 content exceeds 20%, the oxygen content of the weld metal increases, degrading its low-temperature toughness. Therefore, the SiO2 content should be between 5% and 20%. SiO2 can be added from raw materials such as silica sand and water glass.

[0016] [CaO: 5-20%] CaO has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the amount of oxygen in the weld metal. If the CaO content is less than 5%, this effect cannot be obtained, and the low-temperature toughness of the weld metal decreases. On the other hand, if the CaO content exceeds 20%, the basicity of the slag increases, the arc becomes unstable, and the slag removability deteriorates. Therefore, the CaO content is set to 5 to 20%. CaO can be added from raw materials such as wollastonite and calcium oxide.

[0017] [MgO: 25 to 35%] MgO has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the amount of oxygen in the weld metal. If the MgO content is less than 25%, this effect cannot be obtained, and the low-temperature toughness of the weld metal deteriorates. On the other hand, if the MgO content exceeds 35%, the melting point of the slag increases, the slag removability and bead appearance deteriorate, and welding defects such as slag entrainment tend to occur. Therefore, the MgO content is set to 25 to 35%. MgO can be added from raw materials such as magnesia clinker.

[0018] [Al2O3: 10 to 20%] Al2O3 acts as a slag forming agent and also has the effect of improving arc stability. If the Al2O3 content is less than 10%, the arc becomes unstable, and the slag removability and bead appearance deteriorate. On the other hand, if the Al2O3 content exceeds 20%, the amount of oxygen in the weld metal increases, and the low-temperature toughness of the weld metal deteriorates. Therefore, the Al2O3 content is set to 10 to 20%. Al2O3 can be added from raw materials such as alumina.

[0019] [CaF2: 23 to 35%] CaF2 has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the amount of oxygen in the weld metal. If the CaF2 content is less than 23%, this effect cannot be obtained, and the low-temperature toughness of the weld metal decreases. On the other hand, if the CaF2 content exceeds 35%, the arc becomes unstable, and the slag removability and bead appearance deteriorate. Therefore, the CaF2 content is set to 23 to 35%. CaF2 can be added from raw materials such as fluorite.

[0020] [CO2 equivalent of one or two of CaCO3 and MgCO3: 2 to 7%] The CO2 equivalent of CaCO3 or MgCO3 has an effect of decomposing CaCO3 or MgCO3 during welding to generate CO or CO2 gas, which lowers the hydrogen partial pressure in the arc atmosphere and reduces the amount of diffusible hydrogen in the weld metal. If the CO2 equivalent of one or two of CaCO3 and MgCO3 is less than 2%, the effect of reducing the amount of diffusible hydrogen cannot be obtained. On the other hand, if the CO2 equivalent of one or two of CaCO3 and MgCO3 exceeds 7%, pock marks are likely to occur on the bead surface, the oxygen content of the weld metal increases, and the low-temperature toughness of the weld metal deteriorates. Therefore, the CO2 equivalent of one or two of CaCO3 and MgCO3 is set to 2 to 7%.

[0021] [Si: 0.3 to 2.0%] Si is a deoxidizing element and has the effect of improving the bead appearance by reducing the oxygen content of the weld metal. If Si is less than 0.3%, the deoxidation effect cannot be obtained, and pock marks are likely to occur on the bead surface. On the other hand, if Si exceeds 2.0%, the strength of the weld metal increases, and the low-temperature toughness deteriorates. Therefore, Si is set to 0.3 to 2.0%. Si can be added as a raw material from, for example, metallic Si, Fe-Si, Fe-Si-Mn, or the like.

[0022] [Total of one or two of Na2O and K2O: 1 to 5%] Na2O and K2O have the effect of improving arc stability. If the total of one or two of Na2O and K2O is less than 1%, this effect cannot be obtained, and the arc becomes unstable. If the total of one or two of Na2O and K2O exceeds 5%, pock marks are likely to occur, and the bead appearance deteriorates. Therefore, the total of one or two of Na2O and K2O is set to 1 to 5%. Na2O and K2O can be added as raw materials from, for example, sodium carbonate, potassium carbonate, or the like.

[0023] [TiO2: 0.1% or less] TiO2 degrades slag release properties, so it is desirable to minimize its content as much as possible. In particular, the degradation of slag release properties becomes significant when TiO2 exceeds 0.1%. Therefore, the TiO2 content should be 0.1% or less. Note that TiO2 is added from calcium titanate, ilmenite, etc.

[0024] The remainder of the bond flux, other than the above-mentioned components, consists of unavoidable impurities such as Fe from the iron alloy, MnO, P, and S. Since both P and S form low-melting-point compounds that reduce toughness, it is preferable to keep their levels as low as possible.

[0025] Next, we will describe the components of the solid wire to be combined with the bond flux. The percentages given for each component below represent the mass percentage relative to the total mass of the solid wire.

[0026] [C:0.08~0.15%] Carbon (C) is an important element that ensures the strength of the weld metal through solid solution strengthening. It also reacts with oxygen in the arc, reducing the oxygen content in the arc atmosphere and the weld metal, thereby improving low-temperature toughness. If C is below 0.08%, the deoxidation effect is not achieved, leading to increased pockmark formation and a decrease in the low-temperature toughness of the weld metal. On the other hand, if C exceeds 0.15%, the strength of the weld metal becomes excessively high, degrading its low-temperature toughness. Therefore, C should be between 0.08% and 0.15%.

[0027] [Si: 0.1~0.3%] Si has the effect of reducing the oxygen content of the weld metal, improving the bead appearance and low-temperature toughness. If the Si content is less than 0.1%, the deoxidation effect is not obtained, and the low-temperature toughness of the weld metal decreases. On the other hand, if the Si content exceeds 0.3%, the matrix of the weld metal is strengthened by solid solution, but the grains become coarser, so the low-temperature toughness decreases significantly. Therefore, the Si content should be between 0.1% and 0.3%.

[0028] [Mn: 1.5~2.5%] Mn has the effect of improving the strength of the weld metal. If the Mn content is less than 1.5%, this effect cannot be obtained and the strength of the weld metal decreases. On the other hand, if the Mn content exceeds 2.5%, the strength of the weld metal becomes excessively high, resulting in deteriorated low-temperature toughness. Therefore, the Mn content is set to 1.5 to 2.5%.

[0029] [Ni: 2.0 to 3.0%] Ni has the effect of stabilizing the low-temperature toughness of the weld metal. If the Ni content is less than 2.0%, this effect cannot be obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if the Ni content exceeds 3.0%, the austenite grain size of the weld metal is coarsened, leading to reduced low-temperature toughness. Therefore, the Ni content is set to 2.0 to 3.0%.

[0030] [Mo: 0.5 to 1.5%] Mo has the effect of improving the strength of the weld metal. If the Mo content is less than 0.5%, this effect cannot be obtained and the strength of the weld metal decreases. On the other hand, if the Mo content exceeds 1.5%, intermetallic compounds are formed in the weld metal, making the strength of the weld metal excessively high and reducing the low-temperature toughness. Therefore, the Mo content is set to 0.5 to 1.5%.

[0031] [Ti: 0.02 to 0.08%] Ti has the effect of improving low-temperature toughness by reacting with oxygen in the arc to reduce the oxygen content in the arc atmosphere and the weld metal. If the Ti content is less than 0.02%, this effect cannot be obtained and the low-temperature toughness of the weld metal decreases. On the other hand, if the Ti content exceeds 0.08%, the amount of solute Ti in the weld metal increases, leading to reduced low-temperature toughness. Therefore, the Ti content is set to 0.02 to 0.08%.

[0032] [Al: 0.05% or less, P: 0.015% or less, S: 0.015% or less] Since Al, P, and S all form low-melting-point compounds that reduce low-temperature toughness, it is desirable to minimize their contents as much as possible. Therefore, the Al content is set to 0.05% or less, the P content to 0.015% or less, and the S content to 0.015% or less.

[0033] Furthermore, the remaining components of the solid wire other than those mentioned above are Fe, Cu from the copper plating on the wire surface, and unavoidable impurities such as W, V, P, and S. Since both P and S form low-melting-point compounds that reduce toughness, it is preferable to keep their levels as low as possible. [Examples]

[0034] The effects of the present invention will be described in more detail below with reference to examples.

[0035] Various bond fluxes with the components shown in Table 1 and solid wires shown in Table 2 were prototyped. To evaluate the weldability and mechanical performance of these combinations, a 25mm thick, 780MPa class steel plate with the chemical components shown in Table 3 was processed to a groove shape with a groove angle of 30° and a root gap of 13mm, and a backing plate was applied. Multilayer welding tests were then performed under the welding conditions shown in Table 4.

[0036] The bond flux shown in Table 1 was prepared by blending and mixing various mineral raw materials, then granulating it with water glass as a binder, and finally firing it at 400-550°C for 2 hours to achieve a uniform particle size of 1.4 × 0.15 mm. The wire shown in Table 2 was prepared by reducing the diameter of the original wire, annealing it, and plating it, and then drawing these wires to a diameter of 4.0 mm.

[0037] [Table 1]

[0038] [Table 2]

[0039] [Table 3]

[0040] [Table 4]

[0041] Table 5 shows the various combinations of prototype bond fluxes and prototype solid wires. Each test was evaluated by investigating the arc stability, bead appearance, slag detachability, and presence or absence of welding defects by X-ray transmission testing during multi-layer welding, as well as the mechanical properties of the weld metal.

[0042] (arc stability) We defined a stable welding system as one where the welding voltage fluctuated minimally and remained constant during welding.

[0043] (Bead appearance) A good bead was defined as one with consistent bead width, bead height, wave pattern, and surface condition, and without undercuts or pock marks.

[0044] (Slag detachability) After welding, a good result was defined as when the slag, either naturally delaminating or solidified, was struck with a chipping hammer, causing cracks to form in the slag, which could then be easily removed.

[0045] (Welding defects) In the X-ray transmission test, the test was conducted based on the radiographic test of steel welded joints as specified in JIS Z 3104:1995, and the absence of slag inclusion or other defects was considered "none."

[0046] (Machine performance evaluation) The mechanical performance of the weld metal was evaluated by mechanical testing of tensile and impact test specimens taken in accordance with AWS A5.23. For tensile testing, a tensile strength of 780 MPa to 880 MPa was considered good. For impact testing, a Charpy impact test was performed at -74°C, and for each test, an average of 80 J or higher (excluding the minimum and maximum values ​​from a total of 5 cycles) was considered good. The diffusible hydrogen content of the weld metal was measured in accordance with JIS Z3118:2007. A diffusible hydrogen content of 5 ml / 100 g or less was considered good. These investigation results are summarized in Table 5.

[0047] [Table 5]

[0048] In Table 5, test symbols T1 to T16 represent examples of the present invention, and test symbols T17 to T38 represent comparative examples. In the examples of the present invention, test symbols T1 to T16 satisfy the constituent requirements of the present invention because the flux symbols F1 to F16 and the combined wire symbols W1 to W14 satisfy the constituent requirements of the present invention. As a result, the arc is stable, the weld workability such as bead appearance and slag detachability is good, there are no welding defects, the tensile strength and absorbed energy of the weld metal are good, and the diffusible hydrogen content of the weld metal is low, resulting in extremely satisfactory results.

[0049] In the comparative example, test symbol T17 exhibited poor slag detachability and undercutting due to the low SiO2 content of flux symbol F17. Furthermore, the high Mo content of the combined wire symbol W15 resulted in a high tensile strength of the weld metal and a low absorbed energy.

[0050] Test symbol T18 indicates a high concentration of SiO2, as shown in flux symbol F18, resulting in a low absorbed energy value for the weld metal.

[0051] Test symbol T19 indicates that the amount of CaO in the flux symbol F19 is low, resulting in a low absorbed energy value for the weld metal.

[0052] Test symbol T20 showed unstable arc and poor slag detachability due to the high CaO content of flux symbol F20. Furthermore, the low C content of wire symbol W16 resulted in pockmarks and low absorbed energy of the weld metal.

[0053] Test symbol T21 indicated a low absorption energy of the weld metal because the amount of MgO in the flux symbol F21 was low. Furthermore, a high total amount of one or two types of Na2O and K2O resulted in the formation of pockmarks.

[0054] Test symbol T22 resulted in an unstable arc due to a low amount of Al2O3 in the flux symbol F22, leading to poor slag detachability and bead appearance. Additionally, the low amount of Si in the wire symbol W17 resulted in a low absorbed energy value for the weld metal.

[0055] Test symbol T23 resulted in a low absorbed energy of the weld metal because the flux symbol F23 contained a large amount of Al2O3. Additionally, the wire symbol W18 contained a small amount of Mn, resulting in a low tensile strength of the weld metal.

[0056] Test symbol T24 indicates that the amount of CaF2 in the flux symbol F24 is low, resulting in a low absorbed energy of the weld metal. Additionally, the arc was unstable due to a low total amount of either one or two types of Na2O and K2O.

[0057] Test symbol T25 resulted in an unstable arc due to a high CaF2 content in flux symbol F25, leading to poor slag detachability and bead appearance. Additionally, the high Mn content in wire symbol W19 resulted in high tensile strength of the weld metal and low absorbed energy.

[0058] Test symbol T26 resulted in poor slag detachability and bead appearance due to a high MgO content in flux symbol F26, and slag inclusion occurred in the weld metal. Furthermore, the low CO2 equivalent values ​​of one or two types of CaCO3 and MgCO3 resulted in a high diffusible hydrogen content in the weld metal. Additionally, the low Mo content in wire symbol W20 resulted in low tensile strength of the weld metal.

[0059] Test symbol T27 resulted in pockmarks due to a high CO2 equivalent value of one or two types of CaCO3 and MgCO3, as in flux symbol F27, and also indicated a low absorbed energy of the weld metal.

[0060] Test symbol T28 resulted in pockmarks due to a low Si content in flux symbol F28. Additionally, the high C content in wire symbol W21 resulted in a high tensile strength in the weld metal and a low absorbed energy value.

[0061] Test symbol T29 indicates a high Si content in the wire (W22), resulting in a low absorbed energy value for the weld metal.

[0062] Test symbol T30 indicates that the weld metal absorbed energy was low because the wire symbol W23 had a low amount of Ni.

[0063] Test symbol T31 indicates a high concentration of Ni in the wire symbol W24, resulting in a low absorbed energy value for the weld metal.

[0064] Test symbol T32, with flux symbol F29, had a high Si content, resulting in a high tensile strength in the weld metal and a low absorbed energy.

[0065] Test symbol T33 indicates a high concentration of Ti in the wire (W25), resulting in a low absorbed energy value for the weld metal.

[0066] Test symbol T34 indicates that the weld metal absorbed energy was low because the wire symbol W26 had a low Ti content.

[0067] Test symbol T35 had poor slag detachability because it contained a large amount of TiO2, which corresponds to flux symbol F30.

[0068] Test symbol T36 indicated that the absorbed energy of the weld metal was low due to the high Al content of the wire symbol W27.

[0069] Test symbol T37 indicated that the absorbed energy of the weld metal was low because the wire symbol W28 had a high P content.

[0070] Test symbol T38 indicated that the absorbed energy of the weld metal was low because the wire symbol W29 had a high proportion of S.

Claims

[Claim 1] In a submerged arc welding method for high-tensile steel, the mass percentage of the total mass of the bond flux for submerged arc welding is as follows: Yes 2 :5~20%、 CaO: 5-20%, MgO: 25-35%, Al 2 O 3 : 10-200 CaF 2 :23~35%、 CaCO 3 and MgCO 3 One or two types of CO 2 Conversion value: 2-7%, Si: 0.3-2.0%, Na 2 O and K 2 The total content of one or two of the above oxides is 1 to 5%, TiO 2 : Less than 0.1% The remainder consists of Fe from the iron alloy and unavoidable impurities, forming a bond flux for submerged arc welding. In terms of mass % relative to the total mass of the solid wire, C: 0.08-0.15%, Si: 0.1 to 0.3%, Mn: 1.5-2.5%, Ni: 2.0 to 3.0%, Mo: 0.5-1.5%, It contains Ti: 0.02-0.08%, Al: 0.05% or less, P: 0.015% or less, S: 0.015% or less, A submerged arc welding method for high-tensile steel, characterized by welding a solid wire consisting of Fe, Cu from the copper plating on the wire surface, and unavoidable impurities for the remainder.

Citation Information

Patent Citations

  • Submerged arc welding method for high tension steel

    JP1993212583A

  • Submerged arc welding

    JP1996257789A

  • Electroslag welding method

    JP2005246398A

  • Submerged arc weld metal of high tensile strength steel

    JP2007260696A

  • SUBMERGED ARC WELD METAL FOR 1.25%Cr-0.5%Mo STEEL, COKE DRUM AND BONDED FLUX

    JP2010110819A