Exterior materials for energy storage devices
The exterior material for energy storage devices addresses slipperiness and moldability issues by using mixed particles with specified sizes and a lubricant, ensuring uniform protrusions and reduced friction for enhanced moldability and reliability.
Patent Information
- Application Number
- JP2023067332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Conventional exterior materials for energy storage devices face issues with inconsistent slipperiness and moldability due to variations in lubricant distribution and delamination, especially in areas with angled molding, leading to unstable moldability and potential delamination.
The exterior material incorporates a heat-sealable layer containing mixed particles with different volume-average particle sizes, specified weight content, and a lubricant, forming uniform protrusions that reduce contact area with molds, enhancing slipperiness and moldability.
The solution provides stable and good moldability by uniformly dispersing mixed particles with specified sizes and content, reducing friction and delamination, resulting in improved operational reliability of energy storage devices.
Smart Images

Figure 0007955217000004 
Figure 0007955217000005 
Figure 0007955217000006
Abstract
Description
Technical Field
[0001] The present invention relates to exterior materials for power storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablet terminals, as well as batteries and capacitors used for power storage in hybrid vehicles, electric vehicles, wind power generation, solar power generation, and nighttime electricity storage.
Background Art
[0002] In recent years, as mobile devices such as smartphones and tablet terminals have become thinner and lighter, exterior materials for power storage devices mounted on these devices, such as lithium-ion secondary batteries, lithium-polymer secondary batteries, lithium-ion capacitors, and electric double-layer capacitors, have increasingly adopted laminates consisting of a heat-resistant resin layer (base layer) / adhesive layer / metal foil layer (barrier layer) / adhesive layer / thermoplastic resin layer (heat-sealing layer), replacing conventional metal cans. In addition, power sources for electric vehicles and the like, large-scale power sources for power storage applications, capacitors, and the like are also increasingly being packaged with laminates (exterior materials) having the above-described configuration. When producing exterior materials for power storage devices, the laminate is subjected to cold forming such as stretch forming or deep drawing to form a three-dimensional shape such as a substantially rectangular parallelepiped shape. By forming into such a three-dimensional shape, a storage space for accommodating the main body of the power storage device can be secured. Therefore, to ensure a highly accurate storage space, it is preferable to improve formability.
[0003] For example, the exterior material for power storage devices disclosed in Patent Document 1 below ensures good formability by adding a lubricant to the exposed surface of the inner layer (heat-sealing layer) to improve slipperiness.
[0004] In addition, the exterior material for power storage devices disclosed in Patent Document 2 below appropriately adjusts the center line average roughness (Ra) to ensure good formability by causing phase separation on the exposed surface of the heat-sealing layer or adding fine particles to the exposed surface layer.
Prior Art Documents
Patent Documents
[0005] [Patent Document 1] Patent No. 3774163 [Patent Document 2] Patent No. 5380762 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] However, in the conventional exterior material for energy storage devices shown in Patent Document 1, the surface layer to which the lubricant is added is a surface layer that is easily transferred, so the amount of lubricant present changes during use, resulting in variations in slipperiness and making it difficult to obtain stable and good moldability. Furthermore, in areas where molding is performed at an angle close to a right angle, such as the inner corners of the molded part, delamination is likely to occur, and from this point of view as well, good moldability could not be obtained.
[0007] Furthermore, in the conventional exterior material for energy storage devices shown in Patent Document 2, while unevenness such as undulations is necessary over a wide area of the surface, simply adjusting the centerline mean roughness (Ra) improves the slipperiness in some areas, but it is not possible to obtain consistent slipperiness over the entire area, and thus a stable and good moldability cannot be obtained.
[0008] This invention has been made in view of the above-mentioned problems, and aims to provide an exterior material for energy storage devices that can obtain stable and good moldability. [Means for solving the problem]
[0009] To solve the above problems, the present invention comprises the following means.
[0010] [1] An exterior material for an energy storage device comprising a metal foil layer, a resin substrate layer provided on the outer surface side of the metal foil layer, and a thermoplastic resin heat-sealable layer provided on the inner surface side of the metal foil layer, The seal layer, which is positioned on the innermost side of the heat-sealed layer, contains at least two or more mixed particles with different volume-average particle sizes, which are D50, the particle size that represents 50% of the cumulative distribution in particle size distribution measurement by laser diffraction scattering method. In the cumulative distribution of the mixed particles, counting from the smallest particle size, D10, which represents the 10% particle size of the cumulative distribution, is 2 μm or less, and D90, which represents the 90% particle size of the cumulative distribution, is 6 μm or more. The particle size distribution of the mixed particles contains only one peak in the range of D10 to D90. An outer casing material for an energy storage device, characterized in that the peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.
[0011] [2] The mixed particles include small particles, medium particles and large particles, which are mismatched particles with three different volume-average particle diameters. The volume-average particle diameter of the aforementioned small particles is 0.05 μm to 5 μm. The volume-average particle diameter of the aforementioned medium particles is 3 μm to 8 μm. The exterior material for an energy storage device according to item 1 above, wherein the volume-average particle diameter of the large particles is 7 to 15 μm.
[0012] [3] The sealing layer is an exterior material for an energy storage device according to paragraph 1 or 2, wherein the weight content of the mixed particles is 3,000 ppm to 20,000 ppm.
[0013] [4] The sealing layer is an exterior material for an energy storage device according to any one of paragraphs 1 to 3 above, wherein the sealing layer has a thickness of 5 μm or more.
[0014] [5] The mixed particles are an exterior material for an energy storage device according to any one of paragraphs 1 to 4 above, wherein the aspect ratio is 0.2 to 1.
[0015] [6] An exterior material for an energy storage device according to any one of paragraphs 1 to 5 above, wherein the sealing layer contains a lubricant.
[0016] [7] An exterior material for an energy storage device described in any one of the preceding items 1 to 6 that satisfies the relationship (D90-D10) / D50=0.5 to 5.
[0017] [8] A film for use in a heat-sealing layer of an exterior material for power storage devices according to any one of items 1 to 7, A film for a heat-sealing layer of an exterior material for power storage devices, characterized in that a portion corresponding to the seal layer is constituted by a resin layer containing the mixed particles.
[0018] [9] A method for producing a film for use in a heat-sealing layer of an exterior material for power storage devices according to any one of items 1 to 7, A method for producing a film for a heat-sealing layer of an exterior material for power storage devices, characterized in that a portion corresponding to the seal layer is formed by a resin layer containing the mixed particles.
[0019]
[10] A power storage device main body, and an exterior material according to any one of items 1 to 7, A power storage device, characterized in that the power storage device main body is covered with the exterior material. [Effects of the Invention]
[0020] According to the exterior material for a power storage device of Invention [1], since mixed particles having different particle diameters are added to the inner seal layer of the heat-sealing layer, large and small protrusions can be formed. Furthermore, since the mixed particles can be measured as particles having one peak within a certain particle size distribution range according to the particle size distribution measurement results, aggregation of the mixed particles is unlikely to occur. Each particle is dispersed on the inner surface of the heat-sealing layer, allowing uniform protrusions to be formed. This reduces the contact area with molding tools such as molds during molding, improves slipperiness, and enables stable and favorable moldability to be obtained.
[0021] According to the exterior material for a power storage device of Invention [2], since the seal layer contains small particles, medium particles, and large particles with specified particle diameters, it becomes easy to blend mixed particles with a desired particle size distribution. The intended unevenness can be formed on the inner surface of the heat-sealing layer, further reducing the contact area with molding tools during molding and further improving moldability.
[0022] According to the exterior material for energy storage devices of the invention [3], since the content of the mixed particles in the sealing layer is specified, the mixed particles can be appropriately dispersed and well-balanced within the sealing layer, and desired irregularities can be formed on the inner surface of the heat-sealed layer, thereby further improving moldability.
[0023] According to the exterior material for energy storage devices of the invention [4], since the thickness of the sealing layer is specified, the mixed particles can be firmly fixed to the sealing layer in a stable state, preventing problems such as the mixed particles falling off, and thereby further improving moldability.
[0024] According to the exterior material for energy storage devices of the invention [5], since the aspect ratio of the mixed particles is specified, a sufficient convex portion can be formed regardless of the direction in which the mixed particles are tilted, and detachment is less likely to occur, further improving moldability.
[0025] According to the exterior material for energy storage devices of the invention [6], since the seal layer contains a lubricant, when the temperature exceeds a certain level, the lubricant precipitates and appears on the inner surface of the heat-sealed layer, further improving the slipperiness and further improving the moldability.
[0026] According to the exterior material for energy storage devices of the invention [7], the relationship (D90-D10) / D50=0.5~5 is satisfied, so the volume distribution of the mixed particles can be more reliably made broader, and the moldability during molding can be further improved.
[0027] According to the heat-sealable film for the exterior material of the energy storage device of the invention [8], the exterior material of the above invention can be reliably manufactured using the film.
[0028] According to the method for manufacturing a heat-sealable film for the exterior material of an energy storage device of the invention [9], the exterior material of the above invention can be reliably manufactured.
[0029] According to the invention
[10] , a high-quality energy storage device with high operational reliability can be provided because it is equipped with the above-mentioned exterior material which has excellent sliding properties against the molding jig. [Brief explanation of the drawing]
[0030] [Figure 1] Figure 1 is a cross-sectional view showing an exterior material for an energy storage device, which is an embodiment of this invention. [Figure 2] Figure 2 is a schematic cross-sectional view illustrating the heat-sealed layer of the exterior material for an energy storage device according to an embodiment. [Figure 3] Figure 3 is a graph showing the particle size distribution of each particle and the entire mixed particle in the embodiment. [Figure 4] Figure 4 is a graph showing the particle size distribution and cumulative distribution of the mixed particles in the embodiment. [Figure 5] Figure 5 is a graph illustrating the peak values in the particle size distribution of the mixed particles in the embodiment. [Figure 6] Figure 6 is a schematic cross-sectional view illustrating the seal layer in which lubricant has been deposited in the heat-sealed layer of the embodiment. [Figure 7] Figure 7 is a cross-sectional view showing an energy storage device manufactured using the exterior material of the embodiment. [Figure 8] Figure 8 is a perspective view showing an exploded view of the energy storage device of the embodiment. [Modes for carrying out the invention]
[0031] Figure 1 is a cross-sectional view showing an exterior material for an energy storage device that is an embodiment of the present invention. As shown in the figure, this exterior material 1 for an energy storage device comprises a metal foil layer 4 made of metal foil, a heat-resistant resin base layer 2 provided on the outer surface side of the metal foil layer 4 as an outer layer, an adhesive layer 5 provided on the inner surface side of the metal foil layer 4, and a heat-sealable resin heat-sealable layer (sealant layer) 3 provided on the inner surface side of the adhesive layer 5 as an inner layer.
[0032] In this specification, when describing the position of each layer constituting the battery packaging material in terms of direction (upward direction in Figure 1), the direction of the base material layer 2 is referred to as the outside, and the direction of the heat-sealed layer 3 (downward direction in Figure 1) is referred to as the inside.
[0033] The base layer 2 is preferably made of polyamide resin, polyester resin, polyolefin resin, polyimide resin, etc., and the layer can be formed by a coating film or film. The base layer 2 is particularly preferably made of a biaxially oriented film of the above resin, and among these, biaxially oriented polyamide film and biaxially oriented polyester film are preferred. Among these, the biaxially oriented polyamide film is not particularly limited, but biaxially oriented nylon 6 film, biaxially oriented nylon 6,6 film, biaxially oriented MXD nylon film, etc. can be suitably used, and the polyester film can suitably be biaxially oriented polybutylene terephthalate (PBT) film, biaxially oriented polyethylene terephthalate (PET) film, biaxially oriented polyethylene naphthalate (PEN) film, etc.
[0034] Furthermore, as the heat-resistant resin constituting the base layer 2, it is preferable to use a thermoplastic resin with a temperature of 10°C or higher, and more preferably a thermoplastic resin with a temperature of 20°C or higher, compared to the heat-fusible resin constituting the heat-fusible layer 3. The thickness of the base layer 2 is preferably set to 9 μm to 50 μm.
[0035] The metal foil layer 4 can preferably be made from a single metal foil consisting of aluminum (Al) foil, copper (Cu) foil, stainless steel (SUS) foil, titanium (Ti) foil, or nickel (Ni) foil, or from a clad material made by bonding two or more metals together. The thickness of the metal foil layer 4 should be set to 20 μm to 150 μm. In other words, if this thickness is too thin, durability may decrease due to the occurrence of pinholes, etc., and conversely, if it is too thick, moldability may decrease.
[0036] It is preferable to form a base layer on at least one of the inner and outer surfaces of the metal foil layer 4, particularly on the surface facing the heat-sealed layer 3 (inner surface).
[0037] The underlayer can be formed by applying a silane coupling agent or performing chemical treatments such as chromate treatment. The thickness of the underlayer should ideally be set to 0.01 μm to 1 μm.
[0038] By forming the base layer in this manner, the corrosion resistance of the metal foil layer 4 can be improved, as can the adhesive strength with the adhesive layer 5 provided on the inner surface, and peeling of the adhesive layer 5 can be effectively prevented.
[0039] When forming a base layer by a chemical conversion coating (chemical conversion coating), the chemical conversion coating may be selected in combination with the adhesive layer 5, but for example, a coating by chromic acid treatment, a coating by chromate phosphate treatment, a coating by zinc phosphate treatment, a coating by non-chromate treatment using zirconium or titanium as the metal component instead of Cr, and an oxide coating by boehmite treatment can be suitably used.
[0040] The base material layer 2 is attached to the outer surface of this metal foil layer 4 via an adhesive as needed, thereby laminating and integrating them together.
[0041] For bonding the base layer 2 and the metal foil layer 4, and for bonding between films when forming the base layer 2 with multiple films, an adhesive layer formed by a two-component curing adhesive can be suitably used. For example, a two-component curing adhesive can be used, which consists of a first liquid (main component) made of one or more polyols selected from the group consisting of polyurethane polyols, polyester polyols, polyether polyols, and polyester urethane polyols, and a second liquid (curing agent) made of isocyanate. The thickness of this adhesive is preferably set to 2 μm to 5 μm.
[0042] As the adhesive layer 5 provided on the inner surface of the metal foil layer 4, adhesives containing one or more of polyurethane resins, acrylic resins, epoxy resins, polyolefin resins, elastomer resins, fluororesins, or acid-modified polypropylene resins can be suitably used, and among these, it is particularly preferable to use an adhesive made of a polyurethane composite resin with acid-modified polyolefin as the main component. The thickness of the adhesive layer 5 is preferably set to 2 μm to 5 μm.
[0043] The adhesive layer 5 may also be formed by heat lamination using a modified polyolefin (e.g., acid-modified polypropylene). In this case, the preferred thickness is 10 μm to 30 μm.
[0044] Examples of thermoplastic resins constituting the heat-sealable layer 3 include polyethylene resins such as LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), HDPE (high-density polyethylene), and polyethylene copolymers; polypropylene resins such as rPP (random polypropylene), bPP (block polypropylene), hPP (homopolypropylene), and polypropylene copolymers; polybutene copolymers; and ionomers. Among these, polypropylene resins are preferred due to their electrolyte resistance, water resistance, and oxygen barrier resistance. Furthermore, from the viewpoint of handling, it is preferable that the layer be in film form, and in particular, it is preferable to use unoriented polypropylene films such as CPP (cast polypropylene) and IPP (inflated polypropylene).
[0045] Figure 2 is a cross-sectional view showing the heat-sealing layer 3 in the exterior material 1 of this embodiment. As shown in Figures 1 and 2, in this embodiment, the heat-sealing layer 3 is composed of a laminate of three layers: a seal layer 31 located on the innermost side, an outer layer 33 also called a metal foil side layer or laminate layer located on the outermost side, and an intermediate layer 32 located between the seal layer 31 and the outer layer 33.
[0046] In this invention, the heat-sealable layer 3 is not limited to three layers, but may be a single layer, two layers, or four or more layers. However, in this invention, when the heat-sealable layer 3 is a laminated structure, having multiple layers makes it easier to form the desired laminated structure.
[0047] Furthermore, in the present invention, it is not necessarily required to change the resin in each layer. For example, the resin of the innermost layer to which mixed particles are added and the resin of the adjacent layer to which mixed particles are not added may be the same type of resin to constitute the seal layer 31, the intermediate layer 32, and the outer layer 33.
[0048] As previously described, the film for the heat-sealable layer 3 may be single-layer or multi-layer, but considering heat sealability, delamination resistance, and insulation, it is preferable to form it with a multi-layer film such as a co-extruded product. For example, in this embodiment, a three-layer co-extruded CPP film in which rPP layers are arranged on both sides of an hPP layer or a bPP layer can be suitably used. In this three-layer co-extruded CPP film heat-sealable layer 3, the intermediate hPP layer or bPP layer is configured as an intermediate layer 32, one of the rPP layers (inner or outer surface) is configured as a sealing layer 31, and the other rPP layer is configured as an outer layer 33.
[0049] In this embodiment, the overall thickness of the heat-sealing layer 3 is preferably set to 20 μm to 120 μm. The thickness of the seal layer 31 is preferably set to 5 μm or more, more preferably to 10 μm or more, and even more preferably to 20 μm or more. In other words, by specifying the thickness of the seal layer 31 within this range, the mixed particles contained in the seal layer 31, as described later, can be reliably and stably held in the seal layer, and problems such as the mixed particles falling off can be reliably prevented.
[0050] In this embodiment, the seal layer 31 contains three types of particles M1 to M3 as mixed particles, which are incompatible particles, i.e., incompatible particles.
[0051] As the mixed particles M1 to M3, metal oxides, resin beads, etc., can be used. Specific examples of suitable materials include silica, alumina, calcium carbonate, barium carbonate, titanium oxide, aluminum silicate, talc, kaolin, acrylic resin beads, polyethylene resin beads, and polyethylene elastomer. It is preferable to create the mixed particles by combining two or more of the above-mentioned particles. Using two or more particles with different compositions makes aggregation of the mixed particles due to van der Waals forces less likely, allowing the mixed particles to be dispersed within the seal layer 31 and forming appropriate irregularities.
[0052] The content of the mixed particles M1 to M3 in the seal layer 31 is preferably set to 3,000 ppm to 20,000 ppm by weight, and more preferably to 7,000 ppm to 18,000 ppm. In other words, when the content of the mixed particles M1 to M3 is set within this range, the mixed particles M1 to M3 can be appropriately dispersed and well-balanced within the seal layer 31, and the desired irregularities can be formed on the inner surface of the heat-sealed layer 3.
[0053] In this embodiment, the mixed particles (incompatible particles) contained in the seal layer 31 consist of three types of particles with different volume-average particle diameters (median diameters), namely small particles M1, medium particles M2, and large particles M3, which are D50, the 50% particle size of the cumulative distribution.
[0054] The sealing layer 31, which contains small particles M1, medium particles M2, and large particles M3 of different sizes, is arranged so that a portion of each particle M1 to M3 protrudes inward (downward in the same figure) from the inner surface (lower surface in Figures 1 and 2) of the resin component such as rPP, and an uneven surface is formed on the inner surface of the sealing layer 31.
[0055] For the small particles M1, it is preferable to use particles with a volume-average particle size (D50) of 0.05 μm to 5 μm, and more preferably particles with a volume-average particle size (D50) of 0.5 μm to 3 μm.
[0056] For the medium-sized particles M2, it is preferable to use particles with a volume-average particle size (D50) of 3 μm to 8 μm, and more preferably particles with a volume-average particle size (D50) of 4 μm to 7 μm.
[0057] For the large particles M3, it is preferable to use particles with a volume-average particle size (D50) of 7 μm to 15 μm, and more preferably particles with a volume-average particle size (D50) of 8 μm to 13 μm.
[0058] In this embodiment, the seal layer 31 contains three types of particles M1 to M3 with different particle diameters D50. The small particles M1 and large particles M3 broaden the particle size distribution, and the medium particles M2 combine them into a single distribution. This allows for the overall dispersion of particles of each size, contributing to the formation of evenly spaced protrusions of various sizes. When molding the exterior material 1, the contact area with the mold, such as a molding jig, can be reduced, improving slipperiness and resulting in stable and good moldability.
[0059] Furthermore, if particles of the same size rather than different sizes are mixed and included, the size of the protrusions will become uniform, which may result in a monotonous surface shape, a decrease in slipperiness and moldability, and the possibility of the protrusions imprinting the exterior material 1.
[0060] Furthermore, in this embodiment, the small particles M1 can form fine irregularities on the surface (inner surface) of the heat-sealing layer 3, thereby suppressing adhesion to the mold when molding the exterior material 1.
[0061] Furthermore, the large particles M3 ensure the reliable formation of protrusions (projections) on the inner surface of the heat-sealed layer 3, thereby reducing the dynamic frictional force with the mold when molding the exterior material 1.
[0062] Furthermore, the medium-sized particles M2 form small protrusions on the inner surface of the heat-sealed layer 3, and the uneven distribution of these protrusions can be prevented, thereby further enhancing the effects of the small particles M1 and large particles M3.
[0063] Furthermore, in this embodiment, by specifying the particle size (D50) of each particle M1 to M3 within the above range, it becomes easier to blend mixed particles having a desired particle size distribution, and the desired irregularities can be formed on the inner surface of the heat-sealed layer 3. This further reduces the contact area with the mold during molding of the outer material 1, thereby improving moldability even more.
[0064] Furthermore, in this embodiment, when the content of the mixed particles is specified within the above range, or when the thickness of the seal layer 31 is specified within the above range, it is possible to prevent each particle from falling off the seal layer 31, the effect of the protrusions can be fully utilized, and good moldability can be obtained more reliably.
[0065] In this embodiment, the mixing ratio (weight ratio) of large particles M3: medium particles M2: small particles M1 is preferably adjusted to 0.5~1.5:1~3:0.5~1.5, and more preferably to 0.8~1.2:1.5~2.5:0.8~1.2. That is, by adjusting the mixing ratio within this range, the above effects due to the mixing of particles M1~M3 can be obtained more reliably.
[0066] Figure 3 is a graph showing the particle size distribution of small particles M1, medium particles M2, and large particles M3 individually in this embodiment, as well as the particle size distribution of mixed particles obtained by mixing small particles M1, medium particles M2, and large particles M3. As shown in the figure, since small particles M1 and medium particles M2 have smaller particle diameters than large particles M3, when the same amount (weight or volume) is mixed as with large particles M3, the amount of particles present in the particle size distribution (number of particles) becomes larger.
[0067] In this invention, the particle size distribution and cumulative distribution are measured based on laser diffraction (laser diffraction scattering method).
[0068] In this embodiment, the example given is the use of three types of particles M1 to M3 with different volume-average particle sizes (D50) as the mixed particles. However, the invention is not limited to this, and as long as the mixed particles satisfy the conditions in particle size distribution, the present invention may use at least two types of particles with different volume-average particle sizes (D50) as the mixed particles. For example, the mixed particles may be made of two types of particles, small particle M1 and medium particle M2, or small particle M1 and large particle M3. Furthermore, the mixed particles may be formed using four or more types of particles with different volume-average particle sizes (D50).
[0069] Figure 4 is a graph showing the particle size distribution and cumulative distribution of the mixed particles in this embodiment. As shown in the figure, in the particle size distribution of the mixed particles, counting from the smallest particle size, there is only one peak (peak) within the range of 10% particle size (D10) to 90% particle size (D90) in the cumulative distribution, and there are no two or more peaks within that range.
[0070] In this invention, the particle size distribution of the mixed particles contains only one peak within the range of D10 to D90, and any peaks outside this range are irrelevant to this invention. For example, in the particle size distribution in Figure 5, there is a peak at a position below D10, but this peak is not counted in this invention. In other words, the particle size distribution in the same figure contains only one peak within the range of D10 to D90 and is therefore subject to this invention.
[0071] In this embodiment, the cumulative distribution of the mixed particles has a particle size of 2 μm or larger for D10 and a particle size of 6 μm or larger for D90. Furthermore, in this embodiment, the mode diameter as a peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.
[0072] In this embodiment, since the particle sizes of D10 and D90 and the mode diameters are specified to the above values, the entire mixed particle can have a single broad distribution that is not sharp, and the protrusions formed by particles M1 to M3 can be uniformly dispersed without bias on the inner surface of the heat-sealable layer 3. As a result, stress concentration on the mold is less likely to occur when molding the exterior material 1, so the slipperiness is improved and the moldability is further enhanced.
[0073] In this embodiment, it is preferable to satisfy the relationship (D90-D10) / D50 = 0.5 to 5, and more preferably (D90-D10) / D50 = 1.5 to 3. That is, when this relationship is satisfied, the volume distribution of the mixed particles as a whole can be more reliably made broader, and various sizes of irregularities can be created, thereby further improving the moldability of the exterior material 1 during molding.
[0074] Furthermore, in this embodiment, it is preferable to use particles M1 to M3 that constitute the mixed particles, with an aspect ratio (short diameter / long diameter) of 0.2 to 1. In this case, since the particles form a certain clump shape, a sufficient convex portion can be formed regardless of the direction in which the particles M1 to M3 are tilted, and detachment becomes less likely, further improving the moldability when molding the exterior material 1.
[0075] In this embodiment, it is preferable to include a lubricant in the sealing layer 31 of the heat-sealing layer 3.
[0076] Examples of lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylolamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, aromatic bisamides, and the like.
[0077] More specifically, examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide.
[0078] Furthermore, examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide.
[0079] Examples of substituted amides include N-oleyl palmitate amide, N-stearyl stearate amide, N-stearyl oleate amide, N-oleyl stearate amide, and N-stearyl erucate amide.
[0080] Furthermore, examples of methylolamides include methylol stearate amide.
[0081] Furthermore, examples of saturated fatty acid bisamides include methylenebisstearamide, ethylenebiscaprate, ethylenebislaurate, ethylenebisstearamide, ethylenebishydroxystearamide, ethylenebisbehenamide, hexamethylenebisstearamide, hexamethylenebisbehenamide, hexamethylenehydroxystearamide, N,N'-distearyladipamide, N,N'-distearylsebacinamide, and the like.
[0082] Furthermore, examples of unsaturated fatty acid bisamides include ethylenebisoleamide, ethylenebiserucamide, hexamethylenebisoleamide, N,N'-dioleyladipamide, and N,N'-dioleylsebacinamide.
[0083] Furthermore, stearamidoethyl stearate can be given as an example of a fatty acid ester amide.
[0084] Examples of aromatic bisamides include m-xylylenebisstearate, m-xylylenebishydroxystearate, and N,N'-cystearyl isophthalamide.
[0085] The amount of lubricant precipitated on the inner surface of the heat-sealed layer 3 is 0.1 μg / cm². 2 ~1 μg / cm³2 (0.1 μg / cm³) 2 and 1 μg / cm³ 2 It is preferable to adjust the amount to include the following. If the amount of lubricant precipitated is too small, good lubricity may not be obtained, which is undesirable. Conversely, if the amount of lubricant precipitated is too large, the frequency of occurrence of white powder and equipment contamination due to the lubricant may increase, which is also undesirable.
[0086] As shown in Figure 6, the inner surface of the heat-sealed layer 3 is formed with an uneven structure by particles M1 to M3. This suppresses the excessive precipitation of lubricant on the inner surface of the heat-sealed layer 3, while an appropriate amount of lubricant precipitates when the temperature exceeds a predetermined level. This lubricant then forms a lubricant layer 6 that covers the inner surface of the heat-sealed layer 3, further improving its sliding properties against the molding jig.
[0087] Furthermore, when the exterior material 1 of this embodiment is wound into a roll, for example, the heat-sealed layer 3 comes into contact with the outermost layer, such as the base material layer 2. As a result, the positions of the protrusions caused by each particle M1 to M3 preferentially come into contact with other parts (such as the base material layer 2), thus suppressing the transfer of lubricant to other parts.
[0088] In addition, in the present invention, a substrate protective layer formed of a binder resin containing fine particles may be provided on the outside of the substrate layer 2 in order to further improve the slipperiness during molding. As these fine particles, non-miscompatible particles used as the mixed particles in this embodiment can be used, and as the binder resin, urethane resins, acrylic resins, acrylic urethane resins, fluororesins, etc., can be used.
[0089] The exterior material 1 for the energy storage device of this embodiment, configured as described above, is used as an exterior case for an energy storage device, either in sheet form or, if necessary, molded into a predetermined shape by thermoforming such as deep drawing or stretch molding.
[0090] For example, Figures 7 and 8 are a cross-sectional view and an exploded perspective view showing a power storage device 30 manufactured using the exterior material 1 of this embodiment. As shown in both figures, this power storage device 30 is a lithium-ion secondary battery. In this embodiment, the exterior case 15 is composed of a tray member 14 obtained by molding the exterior material 1 and a lid member 10 made of a flat (sheet-shaped) exterior material 1. A power storage device body (electrochemical element, etc.) 35 in a substantially rectangular parallelepiped shape is housed in a housing recess of the tray member 14 obtained by molding the exterior material 1 of the present invention. The lid member 10 (exterior material 1) of the present invention is placed on the power storage device body 35 with its heat-sealed layer 3 side facing inward (downward). The outer peripheral edge of the heat-sealed layer 3 of the lid member 10 and the heat-sealed layer 3 of the flange portion (sealing peripheral edge portion) 29 of the tray member 14 are sealed by heat sealing, thereby forming the power storage device 30. Furthermore, the inner surface of the receiving recess of the tray member 14 is a heat-sealed layer 3, and the outer surface of the receiving recess is on the base material layer 2 side.
[0091] In Figure 7, the symbol "39" represents the heat-sealed portion where the outer peripheral edge of the lid member 10 and the flange portion (sealing peripheral edge) 29 of the tray member 14 are joined (welded). In the energy storage device 30, the tip of the tab lead connected to the main body 35 of the energy storage device is led out to the outside of the outer case 15, but this is not shown in the illustration.
[0092] The energy storage device 30 manufactured using the exterior material 1 of this embodiment has an exterior material 1 that has excellent slipperiness against the molding die and high adhesive strength between the heat-sealed layer 3 and the adhesive layer 5, thus ensuring high operational reliability and providing a high-quality energy storage device product.
[0093] The main body 35 of the energy storage device is not particularly limited, but examples include a battery body, a capacitor body, a capacitor body, etc.
[0094] In the above embodiment, the outer case 15 is composed of a tray member 14 obtained by molding the outer material 1 and a flat lid member 10. However, the present invention is not limited to such a combination. For example, the outer case 15 may be composed of a pair of flat (sheet-shaped) outer materials 1, or it may be composed of a pair of tray members 14 stacked facing each other. [Examples]
[0095] [Table 1]
[0096] [Table 2]
[0097] 1. Preparation of film for heat-sealing layer <Example 1> As shown in Tables 1 and 2, a film for the heat-seal layer 3 of Example 1 in the exterior material 1 for the energy storage device was fabricated. Specifically, as the film for the heat-seal layer 3, a CPP film was prepared by laminating a 16 μm thick rPP for the sealing layer, a 48 μm thick bPP for the intermediate layer, and a 16 μm thick rPP for the outer layer using a T-die in a three-layer co-extrusion.
[0098] In the heat-sealable film of this Example 1, 3000 ppm of silica particles with an average particle size of 1.5 μm were added to the seal layer 31 as small particles M1, 6000 ppm of silica particles with an average particle size of 6 μm as medium particles M2, and 3000 ppm of HDPE (high-density polyethylene) particles with an average particle size of 12 μm as large particles M3.
[0099] As shown in Table 2, for the mixed particles M1 to M3 added to the seal layer 31, the 10% particle size (D10) is 0.8 μm, the 50% particle size (D50) is 3.8 μm, the 90% particle size is 8.2 μm, (D90-D10) / D50 is 1.9, the aspect ratio is 0.8, the number of peaks in the volume distribution within the range of D10 to D90 is 1, and the peak position is 4.1 μm.
[0100] The particle size distribution of the mixed particles was determined using laser diffraction. Specifically, a Microtrac MT3000II was used as the instrument, with a measurement range of 0.02 μm–2000 μm, a measurement time of 30 seconds, two measurements, methanol as the solvent (refractive index 1.33), and non-spherical particles (refractive index 1.54).
[0101] The aspect ratio of each particle was measured using the FPIA-3000 from Sysmex Corporation.
[0102] <Examples 2-17> The resins for the sealing layer, intermediate layer, and outer layer shown in Tables 1 and 2 were laminated in the same manner as in Example 1 to produce the heat-sealable layer films of Examples 2 to 17.
[0103] <Examples 18, 19> Using the sealing layer resins shown in Tables 1 and 4, single-layer unstretched films were prepared using a T-die to obtain the heat-sealable films of Examples 18 and 19.
[0104] <Comparative Examples 1-4> A heat-sealable layer film was prepared by laminating the resins for the sealing layer, intermediate layer, and outer layer shown in Tables 1 and 2 in the same manner as in Example 1. In Comparative Example 1, the mixed particles had two peaks in the volume distribution range D10 to D90, with peak positions at 1.9 μm and 9.3 μm.
[0105] 2. Fabrication of exterior materials for energy storage devices A 40 μm thick aluminum foil (A8021-O), serving as the metal foil layer 4, was coated on both sides with a chemical conversion treatment solution consisting of phosphoric acid, polyacrylic acid (acrylic resin), chromium(III) salt compound, water, and alcohol. The solution was then dried at 180°C to form a chemical conversion film. The amount of chromium deposited on this chemical conversion film was 10 mg / m² per side. 2 That was the case.
[0106] Next, a 15 μm thick biaxially oriented nylon 6 (ONy) film was dry-laminated (bonded) to one side (outer surface) of the chemically treated aluminum foil (metal foil layer 4) via a two-component curing urethane adhesive (3 μm) as a base layer 2.
[0107] Next, the outer surface of the outer layer of the CPP film for the heat-sealing layer prepared in the above examples and comparative examples was superimposed on the other surface (inner surface) of the dry-laminated aluminum foil (metal foil layer) via a two-component curing adhesive (2 μm) of maleic acid-modified polypropylene resin and isocyanate. This was then dry-laminated by sandwiching it between a rubber nip roll and a laminating roll heated to 100°C and pressing it. After that, it was aged at 40°C for 10 days to obtain the exterior materials (laminated bodies) of the examples and comparative examples that would serve as samples.
[0108] 3. Evaluation tests for each exterior material.
[0109] [Table 3]
[0110] <Moldability Test> For each exterior material of the examples and comparative examples, test pieces were cut to a predetermined size and subjected to deep drawing tests using a deep drawing die. The test was conducted on a 55 mm x 35 mm area, increasing the drawing height (drawing depth) in 0.5 mm increments. The gauge pressure at the wrinkle-holding pressure during this molding was 0.475 MPa, and the actual pressure (calculated value) was 0.7 MPa.
[0111] Following this molding process, we visually inspected the corners of the constricted recesses using transmitted light to confirm whether pinholes were occurring.
[0112] Then, samples were evaluated as follows: those with a molding depth of 7 mm or more and pinholes were observed were marked "◎", those with a molding depth of 6 mm or more but less than 7 mm were marked "○", those with a molding depth of 5 mm or more but less than 6 μm were marked "△", and those with a molding depth of less than 5 mm were marked "×". In this evaluation, "◎", "○", and "△" were considered passing grades. The results are shown in Table 3.
[0113] <Laminate Strength (Sealing Performance) Test> Each exterior material from the examples and comparative examples was cut into 15mm wide strips, and the peel strength between the metal foil layer and the heat-sealed layer was measured in accordance with JIS K6854-3 (1999). Peel strengths of 4.0 N / 15mm or higher were rated "◎", 3.0 N / 15mm or higher and less than 4.0 N / 15mm were rated "○", 2.0 N / 15mm or higher and less than 3.0 N / 15mm were rated "△", and less than 2.0 N / 15mm were rated "×". In this example, "◎", "○", and "△" were considered acceptable. The results are shown in Table 3.
[0114] <Slippage Test (Coefficient of Dynamic Friction)> Each exterior material from the examples and comparative examples was cut to a size of 80 mm x 200 mm, and the coefficient of dynamic friction was measured in accordance with JIS K 7125. The measurement conditions were a roll cell weight of 100 N and a weight of 200 g (including the weight of the sliding piece). The results of the coefficient of dynamic friction are shown in Table 3.
[0115] <Overall assessment> As shown in Table 3, although there was some variation in the results, all of the exterior materials in the examples received satisfactory evaluations and reached an acceptable standard.
[0116] In contrast, the exterior materials of Comparative Examples 1 to 4, which deviate from the gist of the present invention, were inferior in any of the following: moldability, sealing ability, and slipperiness. [Industrial applicability]
[0117] The exterior material for energy storage devices of this invention can be suitably used when manufacturing energy storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablets, and batteries and capacitors used in hybrid vehicles, electric vehicles, wind power generation, solar power generation, and for storing nighttime electricity. [Explanation of Symbols]
[0118] 1: Exterior materials 2: Base material layer 3: Heat-sealed layer 30: Energy storage devices 31: Sealing layer 35: Device body 4: Metal foil layer 6: Lubricant layer M1: Small particles M2: Medium particle M3: large particles
Claims
1. An exterior material for an energy storage device comprising a metal foil layer, a resin substrate layer provided on the outer surface side of the metal foil layer, and a thermoplastic resin heat-sealable layer provided on the inner surface side of the metal foil layer, The seal layer, which is positioned on the innermost side of the heat-sealed layer, contains at least two or more mixed particles with different volume-average particle sizes, which are D50, the particle size that represents 50% of the cumulative distribution in particle size distribution measurement by laser diffraction scattering method. In the cumulative distribution of the mixed particles, counting from the smallest particle size, D10, which represents the 10% particle size of the cumulative distribution, is 2 μm or less, and D90, which represents the 90% particle size of the cumulative distribution, is 6 μm or more. The particle size distribution of the mixed particles contains only one peak in the range of D10 to D90. An outer casing material for an energy storage device, characterized in that the peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.
2. The aforementioned mixed particles include small, medium, and large particles, which are mismatched particles with three different volume-average particle diameters. The volume-average particle diameter of the aforementioned small particles is 0.05 μm to 5 μm. The volume-average particle diameter of the aforementioned medium particles is 3 μm to 8 μm. The exterior material for an energy storage device according to claim 1, wherein the volume-average particle diameter of the large particles is 7 to 15 μm.
3. The sealing layer is an exterior material for an energy storage device according to claim 1 or 2, wherein the weight content of the mixed particles is 3,000 ppm to 20,000 ppm.
4. The exterior material for an energy storage device according to claim 1 or 2, wherein the sealing layer has a thickness of 5 μm or more.
5. The aforementioned mixed particles have an aspect ratio of 0.2 to 1, as described in claim 1 or 2, for exterior material for energy storage devices.
6. The exterior material for an energy storage device according to claim 1 or 2, wherein the sealing layer contains a lubricant.
7. An exterior material for an energy storage device according to claim 1 or 2, which satisfies the relationship (D90 - D10) / D50 = 0.5 to 5.
8. A film used in the heat-sealable layer of the exterior material for an energy storage device according to claim 1 or 2, A heat-sealable film for an exterior material of an energy storage device, characterized in that the portion corresponding to the sealing layer is composed of a resin layer containing the mixed particles.
9. A method for manufacturing a film used in the heat-sealed layer of an exterior material for an energy storage device according to claim 1 or 2, A method for manufacturing a heat-sealable film for an exterior material of an energy storage device, characterized in that the portion corresponding to the sealing layer is formed by a resin layer containing the mixed particles.
10. The main body of the energy storage device, The exterior material is as described in claim 1 or 2, and comprises An energy storage device characterized in that the main body of the energy storage device is enclosed with the exterior material.
Citation Information
Patent Citations
Method of treating waste water by activated sludge process
JP1978080762A
Battery pack
JP2014032966A
Sheath material for secondary battery
JP2017004765A
Exterior material for power storage device, outer casing for power storage device and power storage device
JP2019061938A
Sealant film for battery external material
JP2021103679A