Films and laminates
By optimizing the carbon and oxygen element ratios in the resin substrate and applying oxygen-induced coupled plasma treatment, the film achieves improved adhesion with inorganic layers, addressing the adhesion issues in existing laminated films.
Patent Information
- Application Number
- JP2023113718
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-07-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-07-11
AI Technical Summary
Existing laminated films with organic and inorganic layers suffer from insufficient adhesion between the hard coat film and the anti-reflective layer.
The film comprises a resin substrate with specific carbon and oxygen element ratios measured at different angles using X-ray photoelectron spectroscopy, and undergoes oxygen-induced coupled plasma treatment to enhance adhesion, particularly with an inorganic layer.
The enhanced adhesion improves the bonding between the film and inorganic layers, ensuring better durability and performance.
Smart Images

Figure 0007955231000002 
Figure 0007955231000003 
Figure 0007955231000004
Abstract
Description
[Technical Field]
[0001] The present invention relates to films and laminates, and more particularly to films and laminates comprising such films. [Background technology]
[0002] In electronic products, composite materials, which combine organic and inorganic materials, are being developed from the viewpoint of weight reduction and high functionality. As an example of a composite material, a laminated film comprising an organic material base film and an inorganic layer on the base film is known.
[0003] As an example of such a laminated film, an anti-reflective film has been proposed that comprises, in order, a hard coat film having a film substrate and a hard coat layer, an inorganic oxide primer layer, and an anti-reflective layer (see, for example, Patent Document 1).
[0004] In Patent Document 1, the hard coat layer is subjected to plasma treatment before the primer layer is formed on the hard coat layer. This treatment can remove dirt and moisture from the surface of the hard coat film (hard coat layer), and can improve the adhesion between the hard coat film and the anti-reflective layer. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2022-65437 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] However, the base film (hard coat film) described in Patent Document 1 has the drawback of insufficient adhesion. Therefore, even better adhesion is required for the base film (hard coat film).
[0007] The present invention provides a film having excellent adhesion, and a laminate including the film. (Means for Solving the Problems)
[0008] The present invention [1] is a film comprising a resin base material, wherein a carbon element ratio C measured by the following first test 90 , an oxygen element ratio O 90 , a carbon element ratio C 15 and an oxygen element ratio O 15 satisfy the following formula (1). O 15 / C 15 >O 90 / C 90 (1) First test: (1) Using X-ray photoelectron spectroscopy, a carbon element ratio C is measured with respect to one surface in the thickness direction of the resin base material by adjusting a photoelectron take-off angle to 90°. 90 and an oxygen element ratio O 90 is measured. (2) Using X-ray photoelectron spectroscopy, a carbon element ratio C is measured with respect to one surface in the thickness direction of the resin base material by adjusting a photoelectron take-off angle to 15°. 15 and an oxygen element ratio O 15 is measured.
[0009] The present invention [2] includes the film according to [1] above, wherein the resin base material is composed of a base material layer, and in the first test, the carbon element ratio C 90 and the oxygen element ratio O 90 is measured with respect to one surface in the thickness direction of the base material layer by adjusting a photoelectron take-off angle to 90°, and the carbon element ratio C 15 and the oxygen element ratio O 15 is measured with respect to one surface in the thickness direction of the base material layer by adjusting a photoelectron take-off angle to 15°.
[0010] The present invention [3] includes the film according to any one of [1] and [2] above, wherein the resin base material includes a base material layer and a cured resin layer in order toward one side in the thickness direction, and in the first test, the carbon element ratio C 90 and the oxygen element ratio O90 The carbon element ratio C is measured by adjusting the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the cured resin layer. 15 and the oxygen element ratio O 15 The film described in [1] above is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer.
[0011] The present invention [4] comprises the film described in [3] above, wherein the cured resin layer includes an acrylic urethane resin.
[0012] The present invention [5] is a film made of a resin substrate, wherein the carbon element ratio C is measured by the second test described below. 15 and oxygen element ratio O 15 However, it is a film that satisfies the following equation (2). O 15 / C 15 >0.3 (2) Second test: Using X-ray photoelectron spectroscopy, the photoelectron extraction angle was adjusted to 15° for one side in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.
[0013] The present invention [6] is that the resin substrate consists of a substrate layer, and in the second test, the carbon element ratio C 15 and the oxygen element ratio O 15 The film described in [5] above is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the substrate layer.
[0014] The present invention [7] provides that the resin substrate comprises a substrate layer and a cured resin layer in order toward one side in the thickness direction, and in the second test, the carbon element ratio C 15 and the oxygen element ratio O 15 The film described in [5] above is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer.
[0015] The present invention [8] comprises the film described in [7] above, wherein the cured resin layer includes an acrylic urethane resin.
[0016] The present invention [9] includes a laminate comprising a film according to any one of the above [1] to [8] and an inorganic layer, arranged sequentially toward one side in the thickness direction.
[0017] The present invention
[10] includes the laminate described in [9] above, wherein the inorganic layer is an anti-reflective layer, and the anti-reflective layer comprises a plurality of layers having different refractive indices along the thickness direction.
[0018] The present invention
[11] includes the laminate described in [9] above, wherein the inorganic layer is a conductive layer. [Effects of the Invention]
[0019] The film of the present invention has a carbon element ratio C measured by a predetermined first test. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C satisfies the following formula (1), or is measured by the prescribed second test. 15 and oxygen element ratio O 15 However, it satisfies equation (2) below. Therefore, adhesion can be improved. O 15 / C 15 >O 90 / C 90 (1) O 15 / C 15 >0.3 (2)
[0020] The laminate of the present invention comprises the film of the present invention and an inorganic layer in sequence toward one side in the thickness direction. Therefore, excellent adhesion is achieved between the film and the inorganic layer. [Brief explanation of the drawing]
[0021] [Figure 1]Figure 1 shows a first embodiment of the film of the present invention. [Figure 2] Figure 2 shows a perspective view illustrating the positional relationship between the low-inductance antenna and the resin substrate. [Figure 3] Figure 3 is a cross-sectional view showing the positional relationship between the low-inductance antenna and the resin substrate. [Figure 4] Figure 4 shows a second embodiment of the film of the present invention. [Figure 5] Figure 5 shows one embodiment of the laminate of the present invention. [Figure 6] Figure 6 shows one embodiment of a laminate in which the inorganic layer is an anti-reflective layer. [Modes for carrying out the invention]
[0022] The film of the present invention is made of a resin substrate.
[0023] The following description details a first embodiment in which the resin substrate consists of a base layer, and a second embodiment in which the resin substrate has a base layer and a cured resin layer arranged sequentially on one side in the thickness direction.
[0024] Furthermore, the film of the present invention has a carbon element ratio C measured by the first test described below. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C satisfies the following formula (1), or is measured by the second test below. 15 and oxygen element ratio O 15 However, it satisfies equation (2) below. O 15 / C 15 >O 90 / C 90 (1) O 15 / C 15 >0.3 (2)
[0025] Furthermore, the first test involves (1) using X-ray photoelectron spectroscopy to adjust the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the resin substrate, and determining the carbon element ratio C 90 and oxygen element ratio O 90 (2) X-ray photoelectron spectroscopy is used to measure the carbon element ratio C by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the resin substrate. 15 and oxygen element ratio O 15 This is a test to measure [something].
[0026] Furthermore, the second test involves using X-ray photoelectron spectroscopy to adjust the photoelectron extraction angle to 15° relative to one side in the thickness direction of the resin substrate, and determining the carbon element ratio C 15 and oxygen element ratio O 15 This is a test to measure [something].
[0027] As will be explained in more detail later, in the first embodiment, in the first test described above, the carbon element ratio C 90 and oxygen element ratio O 90 This was measured by adjusting the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the substrate layer, and the carbon element ratio C 15 and oxygen element ratio O 15 This is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the substrate layer (this first test is referred to as Test 1A).
[0028] Furthermore, as will be described in more detail later, in the first embodiment, in the second test described above, the carbon element ratio C 15 and oxygen element ratio O 15 This is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the substrate layer (this type of second test is referred to as the 2A test).
[0029] Furthermore, as will be described in more detail later, in the second embodiment, in the first test described above, the carbon element ratio C 90 and oxygen element ratio O 90 This was measured by adjusting the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the cured resin layer, and the carbon element ratio C 15 and oxygen element ratio O 15This is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer (this first test is referred to as the 1B test).
[0030] Furthermore, as will be described in more detail later, in the second embodiment, in the second test described above, the carbon element ratio C 15 and oxygen element ratio O 15 This is measured by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer (this type of second test is referred to as the 2B test).
[0031] 1. First Embodiment A first embodiment of the film of the present invention will be described with reference to Figure 1.
[0032] In Figure 1, the vertical direction of the paper is the vertical direction (thickness direction). The upper side of the paper is the upper side (one side in the thickness direction). The lower side of the paper is the lower side (the other side in the thickness direction). The horizontal direction and depth direction of the paper are plane directions perpendicular to the vertical direction. Specifically, these correspond to the directional arrows in each figure.
[0033] The film 1 has a film shape (including a sheet shape) with a predetermined thickness. The film 1 extends in a planar direction perpendicular to the thickness direction. The film 1 has a flat top surface and a flat bottom surface. Preferably, the film 1 is flexible.
[0034] Film 1 is preferably transparent. Specifically, the total light transmittance of film 1 (JIS K 7375-2008) is, for example, 80% or more, preferably 85% or more.
[0035] The thickness of film 1 is, for example, 10 μm or more, preferably 20 μm or more, more preferably 35 μm or more. Furthermore, from the viewpoint of handling in the roll-to-roll method described later, it is, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 60 μm or less. In addition, a carrier film may be laminated to the back surface of film 1 to ensure the transportability and handling of film 1 in the roll-to-roll process.
[0036] The thickness of film 1 can be measured using a dial gauge (PEACOCK, "DG-205").
[0037] Film 1 consists of a resin substrate 2.
[0038] <Resin substrate> The resin substrate 2 consists of a substrate layer 3.
[0039] The base layer 3 has a film shape. Preferably, the base layer 3 is flexible.
[0040] Examples of the base material layer 3 include polymer films.
[0041] Examples of polymer film materials include polyester resin, (meth)acrylic resin, olefin resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of (meth)acrylic resins include polymethyl methacrylate. Examples of olefin resins include polyethylene, polypropylene, and cycloolefin polymers. Examples of cellulose resins include triacetylcellulose.
[0042] Preferably, cellulose resin is used as the material for the polymer film. More preferably, triacetylcellulose is used as the material for the polymer film.
[0043] The thickness of the base layer 3 is, for example, 10 μm or more, preferably 20 μm or more, and more preferably 30 μm or more, from the viewpoint of ensuring mechanical strength. Furthermore, from the viewpoint of ease of handling in the roll-to-roll method described later, it is, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.
[0044] The thickness of the base layer 3 can be measured using a dial gauge (PEACOCK, "DG-205").
[0045] The substrate layer 3 is preferably transparent. Specifically, the total light transmittance (JIS K 7375-2008) of the substrate layer 3 is, for example, 80% or more, preferably 85% or more.
[0046] <Carbon element ratio C 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 > Film 1 has a carbon element ratio C measured by the following 1A test. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C is satisfied by the following formula (1A) or by the following 2A test. 15 and oxygen element ratio O 15 However, it satisfies equation (2A) below. O 15 / C 15 >O 90 / C 90 (1A) O 15 / C 15 >0.3 (2A)
[0047] Furthermore, the 1A test refers to (1) adjusting the photoelectron take-off angle to 90° relative to one surface in the thickness direction of the base material layer 3 using X-ray photoelectron spectroscopy, and measuring the carbon element ratio C 90 and oxygen element ratio O 90 , and then (2) adjusting the photoelectron take-off angle to 15° relative to one surface in the thickness direction of the base material layer 3 using X-ray photoelectron spectroscopy, and measuring the carbon element ratio C 15 and oxygen element ratio O 15 .
[0048] Furthermore, the 2A test refers to adjusting the photoelectron take-off angle to 15° relative to one surface in the thickness direction of the base material layer 3 using X-ray photoelectron spectroscopy, and measuring the carbon element ratio C 15 and oxygen element ratio O 15 .
[0049] If the carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 measured by the above 1A test satisfy the above formula (1A), or if the carbon element ratio C 15 and oxygen element ratio O 15 measured by the above 2A test satisfy the above formula (2A), adhesion can be improved.
[0050] On the other hand, if the carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 measured by the above 1A test do not satisfy the above formula (1A), and the carbon element ratio C 15 and oxygen element ratio O 15 measured by the above 2A test do not satisfy the above formula (2A), adhesion decreases.
[0051] Preferably, the carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O15 However, the carbon element ratio C that satisfies the above formula (1A) and is measured by the above 2A test is 15 and oxygen element ratio O 15 However, it satisfies the above equation (2A). This further improves adhesion.
[0052] To satisfy equation (1A) and / or equation (2A) above, the surface of the resin substrate 2 is subjected to oxygen-LAICP treatment (described later). In this oxygen-LAICP treatment, for example, the transport speed of the resin substrate 2 (described later), the type of LA21 (described later), the oxygen concentration in the vacuum chamber during the oxygen-LAICP treatment (described later), the pressure in the vacuum chamber during the oxygen-LAICP treatment (described later), the frequency and magnitude of the high-frequency power applied to LA21 during the oxygen-LAICP treatment (described later), and the plasma current density during the oxygen-LAICP treatment (described later) are adjusted.
[0053] Carbon element ratio C 90 For example, this could be 50% or more, or 80% or less.
[0054] Oxygen element ratio O 90 For example, this could be 10 atomic% or more, or 50 atomic% or less.
[0055] Carbon element ratio C 15 For example, this could be 50% or more, or 80% or less.
[0056] Oxygen element ratio O 15 For example, this could be 10 atomic% or more, or 50 atomic% or less.
[0057] <How to process the film> The film processing method comprises a first step of preparing a resin substrate 2 and a second step of applying plasma treatment to one side of the resin substrate 2 in the thickness direction. This method is preferably carried out using a roll-to-roll method. In such cases, the conveying speed is, for example, 0.1 m / min or more, and for example, 20.0 m / min or less.
[0058] [1st step] In the first step, the resin substrate 2 is prepared. Specifically, the substrate layer 3 is prepared.
[0059] [Second process] In the second step, plasma treatment is applied to one side of the resin substrate 2 (substrate layer 3) in the thickness direction.
[0060] Plasma treatment specifically refers to treatment using inductively coupled plasma (oxygen-LAICP treatment) of an oxygen-containing gas generated by applying high-frequency power to a low-inductance antenna.
[0061] A low-inductance antenna is an antenna that has a low inductance of 7.5 μH or less and can generate inductively coupled plasma by applying high-frequency power.
[0062] The low-inductance antenna 21 (LA21) is supported by a mounting bracket 22 and covered by a cover block 23 (omitted in Figure 3), as shown in Figures 2 and 3 (the case where there are 4 LA21s is illustrated as an example). The multiple LA21s are arranged in alignment so as to be aligned in the direction of travel of the resin substrate 2 and in a direction perpendicular to the direction of travel (the width direction of the resin substrate 2).
[0063] LA21 is formed of a conductor. Examples of conductors include copper and silver, with copper being preferred. LA21 may be covered with an insulator. Examples of insulators include glass and quartz.
[0064] The LA21 is electrically connected to the high-frequency power supply (RF power supply) via an impedance matching circuit.
[0065] LA21 has an open-loop shape. Having an open-loop shape in LA21 allows for a lower inductance. Therefore, with an open-loop LA21, the increase in voltage due to an increase in the power applied to LA21 can be suppressed. This suppresses abnormal discharge during plasma processing. By suppressing abnormal discharge, damage to the resin substrate 2 being plasma-treated can be suppressed.
[0066] Specifically, LA21 has a U-shape with two free ends. Each LA21 is fixed to the mounting fixture 22 such that the two free ends are aligned in the width direction of the resin substrate 2. More specifically, LA21 is fixed to the mounting fixture 22 via a field-through 24, as shown in Figure 3.
[0067] Furthermore, LA21 has extensions 21a on the side opposite to the two free ends. The extensions 21a extend in the width direction of the resin substrate 2. Each extension 21a may extend in the running direction of the resin substrate 2 (two LA21 may be arranged in this manner).
[0068] LA21 extends from the mounting fixture 22 toward the resin substrate 2. LA21 extends perpendicularly to the mounting fixture 22. The extension length d1 of LA21 from the mounting fixture 22 is, for example, 30 mm or more, and for example, 150 mm or less.
[0069] The maximum length d2 of LA21 in the planar direction of the resin substrate 2 is, for example, 50 mm or more, and for example, 150 mm or less.
[0070] The separation distance d3 between LA21 and the resin substrate 2 is, for example, 50 mm or more, and for example, 200 mm or less.
[0071] Preferably, the extension length d1 and the separation distance d3 are the same.
[0072] The ratio of the separation distance d3 to the extension length d1 (d3 / d1) is, for example, 0.5 or more, and for example, 3.5 or less.
[0073] In the direction of travel of the resin substrate 2, the distance d4 between the centers of adjacent LA21 is, for example, 100 mm or more, and for example, 500 mm or less. The number of LA21 arranged spaced apart in the direction of travel of the resin substrate 2 (number of rows) may be 1, 2 or 3, or 4 or more if necessary, depending on the travel speed of the resin substrate 2 (i.e., plasma processing time).
[0074] In the width direction of the resin substrate 2, the distance d5 between the centers of adjacent LA21 is, for example, 200 mm or less, or for example, 500 mm or less. By adjusting the distance d5 between centers, the uniformity of the plasma density in the width direction of the resin substrate 2 can be controlled.
[0075] Preferably, the center-to-center distance d4 and the center-to-center distance d5 are the same.
[0076] The center points of the extensions 21a of the four LA21 preferably form a square with vertices. With such a set of LA21, a plasma with high in-plane uniformity and high density can be generated. As the LA21, for example, a high-frequency antenna for plasma generation described in Japanese Patent Application Publication No. 2013-258153 can be used.
[0077] Furthermore, LA21 may have a coil shape instead of an open-loop shape.
[0078] The cover block 23 comprises a block body 23A and a plurality of partition plates 23B. The block body 23A has a plurality of storage spaces 23a. One LA 21 is housed in each storage space 23a. The partition plates 23B are arranged to close the storage spaces 23a. The inside of the storage spaces 23a is a sealed space. In the cover block 23, the block body 23A is made of, for example, aluminum. For example, aluminum A5052 can be used as the aluminum. The partition plates 23B are made of an insulating material. For example, quartz and glass can be used as the insulating material. The separation distance d' (shown in Figure 3) between the moving resin substrate 2 and the cover block 23 is, for example, 50 mm or more, and for example, 200 mm or less. Such a cover block 23 helps to avoid damage and contamination of LA21 due to plasma treatment without excessively reducing the plasma conversion efficiency due to the power applied to LA21, and also helps to suppress damage to the resin substrate 2 being plasma treated.
[0079] In the oxygen-LAICP treatment, LA21 is placed inside the vacuum chamber, and the resin substrate 2 is transported to supply oxygen to the vacuum chamber.
[0080] From the viewpoint of improving adhesion, the oxygen concentration in the vacuum chamber is, for example, 30% by volume or more, more preferably 50% by volume or more, and even more preferably 80% by volume or more. Also from the viewpoint of improving adhesion, it is, for example, 100% by volume or less, preferably 95% by volume or less, and more preferably 90% by volume or less.
[0081] Furthermore, an inert gas or an active gas other than oxygen may be introduced into the vacuum chamber. Examples of inert gases include noble gases (argon, krypton, and xenon). Examples of active gases include nitrogen and water vapor.
[0082] Furthermore, the pressure inside the vacuum chamber during oxygen-LAICP treatment is, for example, 0.1 Pa or higher, preferably 0.2 Pa or higher, more preferably 0.3 Pa or higher, and also, for example, 7.0 Pa or lower, preferably 5.0 Pa or lower, more preferably 3.0 Pa or lower, and even more preferably 1.0 Pa or lower. The above pressure can be adjusted by the amount of oxygen supplied to the vacuum chamber.
[0083] Furthermore, the frequency of the high-frequency power applied to LA21 during oxygen-LAICP treatment is, for example, 1 MHz or higher, preferably 3 MHz or higher, more preferably 5 MHz or higher, even more preferably 10 MHz or higher, and also, for example, 100 MHz or lower, preferably 80 MHz or lower, and more preferably 60 MHz or lower.
[0084] Furthermore, the high-frequency power is, for example, 1.0 kW or more, preferably 1.5 kW or more, more preferably 1.8 kW or more, and also, for example, 10 kW or less, preferably 8 kW or less, more preferably 6 kW or less.
[0085] Furthermore, in the oxygen-LAICP treatment, the plasma current density at the intermediate position between LA21 and the resin substrate 2 is, for example, 1.0 mA / cm². 3 Preferably, 2.0 mA / cm² 3 More preferably, 3.0 mA / cm² 3 More preferably, 4.0 mA / cm² 3 In addition, for example, 10mA / cm 3 Preferably, 8 mA / cm 3 More preferably, 5 mA / cm 3 The following applies:
[0086] The plasma current density can be adjusted by the amount of oxygen introduced, the frequency of the high-frequency power, and the high-frequency power itself.
[0087] This allows plasma treatment to be applied to one side in the thickness direction of the resin substrate 2 (substrate layer 3).
[0088] 2. Second Embodiment A second embodiment of the film of the present invention will be described with reference to Figure 4.
[0089] In the second embodiment, the same reference numerals are used for components and processes as in the first embodiment, and their detailed descriptions are omitted. Furthermore, the second embodiment can achieve the same effects and advantages as the first embodiment, unless otherwise specified.
[0090] Film 1 consists of a resin substrate 2.
[0091] <Resin substrate> The resin substrate 2 comprises a base layer 3 and a cured resin layer 4 arranged sequentially on one side in the thickness direction. Specifically, the resin substrate 2 comprises a base layer 3 and a cured resin layer 4 directly disposed on the upper surface (one side in the thickness direction) of the base layer 3. Preferably, the resin substrate 2 consists of a base layer 3 and a cured resin layer 4.
[0092] [Base material layer] The base layer 3 is a base material that ensures the mechanical strength of the film 1.
[0093] The base layer 3 is positioned to cover the entire lower surface of the cured resin layer 4 so as to be in contact with its lower surface. The base layer 3 is the bottommost layer in the film 1.
[0094] [Cured resin layer] The cured resin layer 4 has a film shape. The cured resin layer 4 is arranged to cover the entire upper surface of the base material layer 3, in contact with the upper surface of the base material layer 3. The cured resin layer 4 is the uppermost layer of the film 1.
[0095] Examples of the cured resin layer 4 include a hard coat layer, an easy-adhesion layer, and an anti-blocking (AB) layer. Preferably, the cured resin layer 4 is a hard coat layer. The hard coat layer is a scratch-protective layer that makes it difficult for scratches to occur on the film 1.
[0096] The hard coat layer is a cured product of a hard coat composition containing a curable resin.
[0097] Examples of curable resins include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. Preferably, acrylic urethane resin is used as the curable resin. In other words, the hard coat layer preferably contains acrylic urethane resin. If the hard coat layer contains acrylic urethane resin, the carbon element ratio C, as described later, will be... 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, it can be adjusted to fully satisfy equations (1B) and (2B) described later.
[0098] Curable resins can be used alone or in combination of two or more types.
[0099] Examples of curable resins include UV-curable resins and thermosetting resins. Preferably, the curable resin is a UV-curable resin. If the curable resin is a UV-curable resin, it can be cured without heating, thus improving the manufacturing efficiency of the film 1.
[0100] In the hard coat composition, the content of the curable resin is, for example, 80% by mass or more, preferably 90% by mass or more, and for example, 99% by mass or less, preferably 95% by mass or less.
[0101] The hard coat composition may optionally include particles, initiators (thermal polymerization initiators, photopolymerization initiators), and leveling agents.
[0102] Examples of particles include inorganic particles and organic particles. Examples of inorganic particles include inorganic oxide particles. Examples of materials for inorganic oxide particles include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of materials for organic particles include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate.
[0103] A lower inorganic particle content is preferable. The lower the inorganic particle content, the more effectively light scattering caused by the inorganic particles can be suppressed, and the lower the manufacturing cost. In a hard coat composition, from the viewpoint of visibility (described later), the inorganic particle content is, for example, 20% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, particularly preferably 0.5% by mass or less, most preferably 0.2% by mass or less, even more preferably 0.1% by mass or less, and even more preferably 0.0% by mass.
[0104] The hard coat composition may be diluted with a solvent as needed. Examples of solvents include butyl acetate, ethyl acetate, toluene, and cyclopentanone.
[0105] When diluting a hard coat composition with a solvent, the solid content concentration is, for example, 10% by mass or more, preferably 30% by mass or more, and for example, 70% by mass or less, preferably 60% by mass or less.
[0106] As will be explained in more detail later, the hard coat layer is formed by applying the hard coat composition to one side of the substrate layer 3 in the thickness direction, drying it as necessary, and curing it.
[0107] The hard coat layer is preferably transparent. Specifically, the total light transmittance of the hard coat layer (JIS K 7375-2008) is, for example, 80% or more, preferably 85% or more.
[0108] The thickness of the cured resin layer 4 is, for example, 0.5 μm or more, preferably 2 μm or more, more preferably 3 μm or more, and also, for example, 30 μm or less, preferably 25 μm or less, more preferably 20 μm or less.
[0109] <Carbon element ratio C 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 > Film 1 has a carbon element ratio C measured by the following 1B test. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C satisfies the following formula (1B) or is measured by the following 2B test. 15 and oxygen element ratio O 15 However, it satisfies equation (2B) below. O 15 / C 15 >O 90 / C 90 (1B) O 15 / C 15 >0.3 (2B)
[0110] Furthermore, the 1B test involves (1) using X-ray photoelectron spectroscopy to adjust the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the cured resin layer 4, and determining the carbon element ratio C 90 and oxygen element ratio O 90 (2) X-ray photoelectron spectroscopy is used to measure the carbon element ratio C, and then the photoelectron extraction angle is adjusted to 15° with respect to one side in the thickness direction of the cured resin layer 4. 15 and oxygen element ratio O 15 This is a test to measure [something].
[0111] Furthermore, the 2B test involves using X-ray photoelectron spectroscopy to adjust the photoelectron extraction angle to 15° relative to one side in the thickness direction of the cured resin layer 4, thereby determining the carbon element ratio C 15 and oxygen element ratio O 15 This is a test to measure [something].
[0112] The carbon element ratio C measured by the above 1B test 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C satisfies the above formula (1B) or is measured by the above 2B test. 15 and oxygen element ratio O 15 However, if the above equation (2B) is satisfied, the adhesion can be improved.
[0113] On the other hand, the carbon element ratio C measured by the above 1B test 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, if the above formula (1B) is not satisfied, and the carbon element ratio C measured by the above 2B test is not satisfied, 15 and oxygen element ratio O 15 However, if the above equation (2B) is not satisfied, the adhesion will decrease.
[0114] Preferably, the carbon element ratio C measured by the above 1B test. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C that satisfies the above formula (1B) and is measured by the above 2B test is 15 and oxygen element ratio O 15 However, it satisfies equation (2B) above. This further improves adhesion.
[0115] To satisfy equation (1B) and / or equation (2B) above, the surface of the resin substrate 2 is subjected to oxygen-LAICP treatment. In this oxygen-LAICP treatment, for example, the transport speed of the resin substrate 2, the type of LA21, the oxygen concentration in the vacuum chamber during the oxygen-LAICP treatment, the pressure in the vacuum chamber during the oxygen-LAICP treatment, the frequency and magnitude of the high-frequency power applied to LA21 during the oxygen-LAICP treatment, and the plasma current density during the oxygen-LAICP treatment are adjusted.
[0116] <Film manufacturing method> The method for manufacturing the film comprises a first step of preparing a resin substrate 2 and a second step of applying plasma treatment to one side of the resin substrate 2 in the thickness direction. This method is preferably carried out using a roll-to-roll method. In such cases, the transport speed is, for example, 0.1 m / min or more, and for example, 20.0 m / min or less. The following description will detail the case where the cured resin layer 4 is a hard coat layer.
[0117] [1st step] In the first step, the resin substrate 2 is prepared.
[0118] Specifically, first, prepare the base layer 3.
[0119] Next, a hard coat layer (cured resin layer 4) is placed on one side of the base layer 3 in the thickness direction. To place the hard coat layer on one side of the base layer 3 in the thickness direction, a hard coat composition is applied to that side of the base layer 3 in the thickness direction, dried if necessary, and cured.
[0120] The drying conditions include a drying temperature of, for example, 50°C or higher, and for example, 120°C or lower. The drying time is, for example, 10 seconds or more, and for example, 10 minutes or less.
[0121] If the hard coat composition contains an ultraviolet-curable resin, the curable resin is cured by ultraviolet irradiation. Examples of ultraviolet irradiation light sources include high-pressure mercury lamps and LED lights. The cumulative amount of ultraviolet irradiation is, for example, 100 mJ / cm². 2 In addition, for example, 500 mJ / cm 2 The following applies:
[0122] If the hard coat composition contains a thermosetting resin, the curable resin is cured by heating. The heating temperature is, for example, 100°C or higher, or, for example, 150°C or lower. The heating time is, for example, 10 seconds or more, or, for example, 10 minutes or less.
[0123] This prepares the resin substrate 2 by placing a hard coat layer (cured resin layer 4) on one side in the thickness direction of the substrate layer 3.
[0124] [Second process] In the second step, plasma treatment is performed on one side of the resin substrate 2 (cured resin layer 4) in the thickness direction using the same procedure as in the first embodiment. This is used to manufacture the film 1.
[0125] <Laminate> As shown in Figure 5, the laminate 10 comprises a film 1 (specifically, the film 1 of the first embodiment or the film 1 of the second embodiment) and an inorganic layer 11 arranged sequentially toward one side in the thickness direction (Note that Figure 5 shows the case where film 1 is the film 1 of the second embodiment). Specifically, the laminate 10 comprises a film 1 and an inorganic layer 11 directly disposed on the upper surface (one side in the thickness direction) of the film 1. Preferably, the laminate 10 consists of a film 1 and an inorganic layer 11.
[0126] [film] Film 1 is positioned over the entire lower surface of the inorganic layer 11 so as to be in contact with the lower surface of the inorganic layer 11. Film 1 is the bottom layer in the laminate 10.
[0127] [Inorganic layer] The inorganic layer 11 has a film shape. The inorganic layer 11 is arranged to cover the entire upper surface of the film 1, in contact with the upper surface of the film 1. The inorganic layer 11 is the uppermost layer in the laminate 10.
[0128] Examples of inorganic layers 11 include anti-reflective layers and conductive layers. The cases in which the inorganic layer 11 is an anti-reflective layer or a conductive layer will be described in detail below.
[0129] (When the inorganic layer is an anti-reflective layer) Referring to Figure 6, we will now describe in detail the case where the inorganic layer 11 is an anti-reflective layer.
[0130] If the inorganic layer 11 is an anti-reflective layer, then the laminate 10 is an anti-reflective film.
[0131] The anti-reflective layer comprises multiple layers having different refractive indices along the thickness direction. Specifically, the anti-reflective layer alternates between high refractive index layers with relatively high refractive indices and low refractive index layers with relatively low refractive indices along the thickness direction. In the anti-reflective layer, the net reflected light intensity is attenuated by the interference effect between reflected light at multiple interfaces in the multiple thin layers (high refractive index layers, low refractive index layers) contained therein. Furthermore, in the anti-reflective layer, the interference effect that attenuates the reflected light intensity can be made to occur by adjusting the optical film thickness (product of refractive index and thickness) of each thin layer. Such an anti-reflective layer comprises high refractive index layers 12 and low refractive index layers 13 alternately in sequence along one side of the thickness direction.
[0132] The anti-reflective layer (specifically, the high refractive index layer 12 and the low refractive index layer 13) preferably includes one selected from the group consisting of metals, alloys, metal oxides, metal nitrides, and metal fluorides, and more preferably includes one selected from the group consisting of metals, metal oxides, and metal nitrides. This allows the anti-reflective layer to suppress the reflection intensity of ambient light.
[0133] Examples of metals include silicon, nickel, chromium, aluminum, tin, gold, silver, platinum, zinc, titanium, tungsten, zirconium, niobium, and palladium. Examples of alloys include alloys of the above metals. Examples of metal oxides include metal oxides of the above metals. Examples of metal nitrides include metal nitrides of the above metals. Examples of metal fluorides include metal nitrides of metal fluorides of the above metals.
[0134] In particular, the material used for the anti-reflective layer is selected according to the desired refractive index.
[0135] Specifically, examples of high refractive index materials constituting the high refractive index layer 12 include niobium oxide (Nb2O5), titanium oxide, zirconium oxide, indium tin oxide (ITO), and antimond-doped tin oxide (ATO). Indium tin oxide (ITO) is preferred as the high refractive index material.
[0136] Furthermore, examples of low refractive index materials constituting the low refractive index layer 13 include silicon dioxide (SiO2) and magnesium fluoride. Silicon dioxide (SiO2) is preferred as the low refractive index material.
[0137] Furthermore, in the anti-reflective layer, the thickness of the high refractive index layer 12 is, for example, 1 nm or more, preferably 3 nm or more, and for example, 15 nm or less, preferably 10 nm or less.
[0138] Furthermore, the thickness of the low refractive index layer 13 is greater than the thickness of the high refractive index layer 12, for example, exceeding 15 nm, and for example, being 50 nm or less, preferably 30 nm or less.
[0139] The ratio of the thickness of the low refractive index layer 13 to the thickness of the high refractive index layer 12 (thickness of the low refractive index layer 13 / thickness of the high refractive index layer 12) is, for example, greater than 1, preferably 2 or more, more preferably 3 or more, and also, for example, 10 or less, preferably 5 or less.
[0140] The thickness of the anti-reflective layer is, for example, 20 nm or more, and for example, 300 nm or less, preferably 250 nm or less, and more preferably 200 nm or less.
[0141] Furthermore, if the inorganic layer 11 is an anti-reflective layer, the laminate 10 can be manufactured by arranging the anti-reflective layer on one side of the film 1 in the thickness direction using a known sputtering method.
[0142] Furthermore, the number of high-refractive-index layers and low-refractive-index layers in the above-mentioned anti-reflective layer is not particularly limited.
[0143] (When the inorganic layer is a conductive layer) If the inorganic layer 11 is a conductive layer, the laminate 10 is a transparent conductive film.
[0144] Examples of materials for the conductive layer include metals and metal oxides. Examples of metals include copper, silver, gold, nickel, chromium, and alloys thereof. Examples of metal oxides include indium-containing conductive oxides and antimony-containing conductive oxides. Examples of indium-containing conductive oxides include indium-tin composite oxide (ITO), indium-zinc composite oxide (IZO), indium-gallium composite oxide (IGO), and indium-gallium-zinc composite oxide (IGZO). An example of an antimony-containing conductive oxide is antimony-tin composite oxide (ATO).
[0145] The thickness of the conductive layer is, for example, 1 nm or more, preferably 5 nm or more, and also, for example, 100 nm or less.
[0146] Furthermore, if the inorganic layer 11 is a conductive layer, the laminate 10 can be manufactured by arranging the conductive layer on one side of the film 1 in the thickness direction using a known sputtering method.
[0147] <Effects and Effects> In the first embodiment, the film 1 has a carbon element ratio C measured by the first A test described above. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C that satisfies the above formula (1A) or is measured by the above 2A test 15 and oxygen element ratio O 15 However, it satisfies the above equation (2A). Therefore, adhesion can be improved.
[0148] Furthermore, in the second embodiment, the film 1 has a carbon element ratio C measured by the first B test described above. 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the carbon element ratio C satisfies the above formula (1B) or is measured by the above 2B test. 15 and oxygen element ratio O 15 However, it satisfies equation (2B) above. Therefore, adhesion can be improved.
[0149] More specifically, in X-ray photoelectron spectroscopy, the smaller the photoelectron extraction angle, the shallower the detection depth on the surface of film 1 (specifically, the substrate layer 3 or the cured resin layer 4). Conversely, the larger the photoelectron extraction angle, the deeper the detection depth on the surface of film 1 (substrate layer 3 or cured resin layer 4).
[0150] In other words, the ratio of carbon elements C 15 This is the carbon element ratio based on a relatively shallow detection depth, and also the carbon element ratio C 90 This represents the carbon element ratio based on a relatively deep detection depth.
[0151] In other words, the ratio of carbon elements C 15 This is the carbon element ratio derived from the vicinity of the surface of film 1 (substrate layer 3 or cured resin layer 4), and the carbon element ratio C 90 This is the carbon element ratio derived from within the film 1 (substrate layer 3 or cured resin layer 4).
[0152] Similarly, the oxygen element ratio O 15 This is the oxygen element ratio derived from the vicinity of the surface of film 1 (substrate layer 3 or cured resin layer 4), and the oxygen element ratio O 90 This is the ratio of oxygen elements originating from within the film 1 (substrate layer 3 or cured resin layer 4).
[0153] Furthermore, satisfying either formula (1A) or formula (1B) above means that the oxygen element ratio is higher near the surface of film 1 (substrate layer 3 or cured resin layer 4) than inside film 1 (substrate layer 3 or cured resin layer 4).
[0154] From this, it can be inferred that oxygen modification is applied to the surface of film 1 (substrate layer 3 or cured resin layer 4). As a result, film 1 (substrate layer 3 or cured resin layer 4) and the inorganic layer 11 are chemically bonded via oxygen, improving adhesion.
[0155] The laminate 10 is composed of a film 1 and an inorganic layer 11 arranged sequentially in one direction in the thickness direction. Therefore, excellent adhesion is achieved between the film 1 and the inorganic layer 11. [Examples]
[0156] The present invention will be further described below with reference to examples and comparative examples. However, the present invention is not limited in any way to the examples and comparative examples. Furthermore, specific numerical values such as blending ratios (content ratios), physical properties, and parameters used in the following description can be replaced with the corresponding upper limits (numerical values defined as "less than or equal to" or "less than") or lower limits (numerical values defined as "greater than or equal to" or "greater than or equal to") of the blending ratios (content ratios), physical properties, and parameters described in the "Modes for Carrying Out the Invention" above.
[0157] Example 1 <Film Manufacturing> [1st step] In the first step, the resin substrate was prepared. Specifically, a long TAC film (triacetylcellulose film, 100m in length, 340mm in width, and 40μm in thickness) was prepared as the substrate layer.
[0158] Next, a hard coat layer (cured resin layer) was placed on one side in the thickness direction of the substrate layer. Specifically, first, 100 parts by mass (solid content equivalent) of a butyl acetate solution of UV-curable acrylic urethane resin (product name "Luxidia 17-806", solid content concentration 80% by mass, manufactured by DIC Corporation), 5 parts by mass of a photopolymerization initiator (product name "Omnirad 907", manufactured by IGM Resins), 0.03 parts by mass of a leveling agent (product name "GRANDIC PC4100", manufactured by DIC Corporation), and butyl acetate as a solvent were mixed to adjust the solid content concentration to 75% by mass. Then, cyclopentanone was added as a solvent to prepare a hard coat composition (solid content concentration 50% by mass).
[0159] Next, a hard coat composition was applied to one side of the substrate layer in the thickness direction to form a coating film. Then, this coating film was dried by heating and cured by ultraviolet irradiation. As a result, a hard coat layer (5 μm thick) was placed on one side of the substrate layer in the thickness direction.
[0160] The heating temperature was set to 100°C and the heating time to 60 seconds. For ultraviolet irradiation, a high-pressure mercury lamp was used as the light source, and ultraviolet light with a wavelength of 365 nm was irradiated onto the coating film, with an integrated irradiation dose of 300 mJ / cm². 2 That's what I decided.
[0161] Based on the above, the resin substrate was prepared.
[0162] [Second process] In the second step, plasma treatment was applied to one side of the resin substrate (hard coat layer) in the thickness direction.
[0163] Specifically, under vacuum conditions, the resin substrate was transported into the vacuum chamber using a roll-to-roll method at a transport speed of 1.0 m / min, and plasma treatment was performed on the resin substrate (hard coat layer).
[0164] For the plasma treatment, oxygen-LAICP treatment was performed. A low-inductance antenna, as shown in Figures 2 and 3, was used.
[0165] In the low-inductance antenna, the extension length d1 is 88 mm, the maximum length d2 is 100 mm, the separation distance d3 is 112 mm, the center-to-center distance d4 is 290 mm, the center-to-center distance d5 is 280 mm, and the separation distance d' is 100 mm. Each low-inductance antenna is electrically connected to a high-frequency power supply (RF power supply, frequency 13.56 MHz) via an impedance matching circuit.
[0166] The ultimate vacuum level of the vacuum chamber is 1.0 × 10⁻⁶ -4 After evacuating the apparatus to a vacuum of 0.5 Pa, oxygen gas (100% oxygen concentration) was introduced into the vacuum chamber, and the atmospheric pressure inside the vacuum chamber was set to 0.5 Pa. By applying a high-frequency power of 5.0 kW to four low-inductance antennas using a high-frequency power supply, an inductively coupled plasma of oxygen-containing gas was formed around these antennas (this plasma was used to treat the resin substrate (hard coat layer)). The plasma current density at the intermediate position between the low-inductance antennas and the resin substrate was 4.2 mA / cm². 3 That's what I decided.
[0167] This allowed them to manufacture the film.
[0168] <Manufacturing of laminates> An anti-reflective layer was applied to one side of the film in the thickness direction using the sputtering method.
[0169] Specifically, after evacuating the vacuum chamber, 1.0 × 10 -4The pressure was reduced to Pa, argon gas was introduced as the sputtering gas, and a high refractive index layer (ITO film, 5 nm thick) was placed on an ITO target (SnO ratio 10 mass%, length 600 mm x width 150 mm x thickness 5 mm, single cathode method) (input power 1.0 kW, deposition chamber pressure: 0.3 Pa, DC discharge). Next, a low refractive index layer (SiO2 film, 20 nm thick) was placed on a pure Si target (length 600 mm x width 50 mm x thickness 5 mm, dual cathode method) (input power: 3.0 kW, deposition pressure 0.3 Pa, O2 / Ar=0.3, MFAC power supply 60 kHz).
[0170] This allowed us to manufacture the laminate.
[0171] Comparative Example 1 <Film Manufacturing> A resin substrate was prepared based on the same procedure as in the first step of Example 1.
[0172] In the second step, bombardment treatment with argon ions was performed on one side in the thickness direction of the resin substrate (hard coat layer).
[0173] Specifically, under vacuum conditions, the resin substrate was transported into the vacuum chamber using a roll-to-roll method at a transport speed of 1.0 m / min.
[0174] The vacuum chamber is equipped with a pair of planar electrodes for plasma generation: a cathode electrode and an anode electrode (both rectangular electrodes made of SUS304 stainless steel). The pair of planar electrodes are spaced 50 mm apart and positioned parallel to the resin substrate passing through the vacuum chamber. The anode electrode is positioned 35 mm away from the resin substrate and is grounded outside the vacuum chamber. The cathode electrode is positioned facing the hard coat layer surface of the resin substrate and is electrically connected to a high-frequency power supply (RF power supply, 13.56 MHz) via an impedance matching circuit. Each electrode has a length of 110 mm in the film travel direction and a length of 430 mm in the width direction.
[0175] The ultimate vacuum level of the vacuum chamber is 1.0 × 10⁻⁶ -4 After evacuating the apparatus to a vacuum of 0.5 Pa, argon gas was introduced as an inert gas into the vacuum chamber, and the pressure inside the vacuum chamber was set to 0.5 Pa. By applying 550 W of power from a high-frequency power supply between the planar electrodes, a capacitively coupled plasma (CCP) was generated. Under this plasma environment, bombardment treatment with argon ions was performed on the surface of the resin substrate (hard coat layer).
[0176] <Manufacturing of laminates> The laminate was prepared following the same procedure as in Example 1.
[0177] <Rating> [Carbon element ratio C 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 [Measurement] Tests 1B and 2B were performed on the films of each example and each comparative example.
[0178] Furthermore, the central portion of the film in the width direction (340 mm width) was cut out and used as a sample approximately 1 cm square.
[0179] Specifically, in the 1B test, (1) X-ray photoelectron spectroscopy was used to adjust the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the hard coat layer, and the carbon element ratio C 90 and oxygen element ratio O 90 (2) X-ray photoelectron spectroscopy was used to measure the carbon element ratio C by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the hard coat layer. 15 and oxygen element ratio O 15 We measured it.
[0180] Furthermore, in the 2B test, using X-ray photoelectron spectroscopy, the photoelectron extraction angle was adjusted to 15° with respect to one side in the thickness direction of the hard coat layer, and the carbon element ratio C 15 and oxygen element ratio O 15We measured it.
[0181] The conditions for X-ray photoelectron spectroscopy are as follows: {conditions} Equipment: "KRATOS ULTRA2" (manufactured by Shimadzu Corporation) X-ray source: Monochrome Al Kα X-ray setting:700×300μm [5mA, 75W] Neutralization of static charge: Yes
[0182] The results are shown in Table 1. Also, "O 15 / C 15 " and "O 90 / C 90 This indicates ".
[0183] [Adhesion] The laminates of each example and each comparative example were cut into 50mm x 50mm pieces to be used as samples. Next, cuts were made at 1mm intervals on the treated surface of the samples to create a grid of 100 squares, and then the samples were placed in a weather resistance tester under the following conditions. {conditions} SUV irradiation conditions Temperature and humidity conditions: 85℃45%Rh Light source used: Metal halide lamp Irradiation conditions: 150mW / cm 2 (290-450nm) Input time: 32.5 hours
[0184] Next, to prevent the surface of the anti-reflective layer from drying, 2 mL of isopropyl alcohol was continuously dripped onto the grid, and a polyester wiper (Sanplatec's "Anticon Gold") fixed to a 20 mm square SUS jig was slid across the grid (load: 1.5 kg, 1000 reciprocations). Grid areas where the anti-reflective layer peeled off over more than 1 / 4 of the grid area were counted as "peeling". Adhesion was evaluated based on the following criteria. The results are shown in Table 1. {standard} ○: The number of "peeling" squares was 5 or less. ×: The number of "peeling" squares exceeds 5.
[0185] [Table 1] [Explanation of Symbols]
[0186] 1 film 2 Resin base material 3 Base material layer 4 Cured resin layer 10 Laminate 11 Inorganic layer
Claims
1. A film made of a resin substrate, The carbon element ratio C measured by the first test described below 90 , Oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, the film satisfies the following equation (1). O 15 / C 15 >O 90 / C 90 (1) Test 1: (1) Using X-ray photoelectron spectroscopy, the carbon element ratio C is measured on one surface of the resin substrate in the thickness direction by adjusting the photoelectron take-off angle to 90° 90 and the oxygen element ratio O 90 . (2) Using X-ray photoelectron spectroscopy, the photoelectron extraction angle is adjusted to 15° with respect to one side in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.
2. The aforementioned resin substrate consists of a substrate layer, In the first test described above, The carbon element ratio C 90 and the oxygen element ratio O 90 This is measured by adjusting the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the substrate layer. The carbon element ratio C 15 and the oxygen element ratio O 15 The film according to claim 1, wherein the measurement is performed by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the substrate layer.
3. The resin substrate comprises a base layer and a cured resin layer in order toward one side in the thickness direction, In the first test described above, The carbon element ratio C 90 and the oxygen element ratio O 90 This is measured by adjusting the photoelectron extraction angle to 90° with respect to one side in the thickness direction of the cured resin layer. The carbon element ratio C 15 and the oxygen element ratio O 15 The film according to claim 1, wherein the measurement is performed by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer.
4. The film according to claim 3, wherein the cured resin layer comprises an acrylic urethane resin.
5. A film made of a resin substrate, The carbon element ratio C measured by the second test described below 15 and oxygen element ratio O 15 However, the film satisfies the following equation (2). O 15 / C 15 >0.3 (2) Second test: Using X-ray photoelectron spectroscopy, the photoelectron extraction angle was adjusted to 15° relative to one side in the thickness direction of the resin substrate, and the carbon element ratio C was determined. 15 and oxygen element ratio O 15 Measure.
6. The aforementioned resin substrate consists of a substrate layer, In the second test described above, The carbon element ratio C 15 and the oxygen element ratio O 15 The film according to claim 5, wherein the measurement is performed by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the substrate layer.
7. The resin substrate comprises a base layer and a cured resin layer in order toward one side in the thickness direction, In the second test described above, The carbon element ratio C 15 and the oxygen element ratio O 15 The film according to claim 5, wherein the measurement is performed by adjusting the photoelectron extraction angle to 15° with respect to one side in the thickness direction of the cured resin layer.
8. The film according to claim 7, wherein the cured resin layer comprises an acrylic urethane resin.
9. A laminate comprising, in order toward one side in the thickness direction, a film according to any one of claims 1 to 8 and an inorganic layer.
10. The inorganic layer is an anti-reflective layer, The laminate according to claim 9, wherein the anti-reflective layer comprises a plurality of layers having different refractive indices along the thickness direction.
11. The laminate according to claim 9, wherein the inorganic layer is a conductive layer.
Citation Information
Patent Citations
Hydrophilization of hydrophobic polymers
JP1997512294A
Manufacture of metal element-containing thin film laminate
JP2000185362A
Method for surface treatment of polymeric materials using hydrogen ion assisted reaction
JP2003509558A
Improved method for modifying polymer surfaces
JP2005511876A
Hard coat film
JP2011043606A