Electrolyte for zinc batteries, and zinc batteries
The electrolyte for zinc batteries, comprising alkali metal hydroxide and surfactants, addresses low-temperature discharge issues by enhancing electrolyte diffusion and reducing DC resistance, thus improving battery performance and lifespan.
Patent Information
- Application Number
- JP2023544010
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-27
- Filing Date
- 2022-08-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-26
AI Technical Summary
Zinc batteries experience deterioration in low-temperature discharge performance and dendrite formation, leading to short circuits and reduced lifespan, particularly in environments below 0°C.
An electrolyte for zinc batteries containing an alkali metal hydroxide and a surfactant, with specific organic compounds like ether compounds and glyme, improves electrolyte diffusion and reduces DC resistance, thereby enhancing low-temperature discharge performance.
The electrolyte suppresses the decrease in low-temperature discharge performance and dendrite formation, improving the lifespan and efficiency of zinc batteries in cold conditions.
Smart Images

Figure 0007955276000001 
Figure 0007955276000002 
Figure 0007955276000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to an electrolyte solution for a zinc battery and a zinc battery. [Background Art]
[0002] Known examples of zinc batteries include nickel-zinc batteries, air-zinc batteries, and silver-zinc batteries. For example, a nickel-zinc battery is an aqueous battery that uses an aqueous electrolyte such as an aqueous potassium hydroxide solution, and thus has high safety. Additionally, it is known that the combination of a zinc electrode and a nickel electrode provides a high electromotive force for an aqueous battery. Furthermore, nickel-zinc batteries have excellent input / output performance and low cost, and thus their applicability to industrial applications (e.g., backup power supplies) and automotive applications (e.g., hybrid vehicles) is being studied.
[0003] The charge-discharge reaction of a nickel-zinc battery proceeds, for example, according to the following formula (discharge reaction: rightward, charge reaction: leftward). (Positive electrode) 2NiOOH+2H2O+2e - → 2Ni(OH)2+2OH - (Negative electrode) Zn+2OH - → Zn(OH)2+2e -
[0004] As shown in the above formula, in a zinc battery, zinc hydroxide (Zn(OH)2) is generated by a discharge reaction. Zinc hydroxide is soluble in the electrolyte, and when zinc hydroxide dissolves in the electrolyte, tetrahydroxozincate ions ([Zn(OH)4] 2-) diffuses into the electrolyte. As a result, the negative electrode undergoes a change in shape (deformation) and the distribution of the charging current becomes uneven, causing localized zinc deposition on the negative electrode and the formation of dendrites (dendritic crystals). In conventional zinc batteries, if dendrites grow due to repeated charging and discharging, the dendrites may penetrate the separator and cause a short circuit. Therefore, various attempts have been made to prevent such short circuits caused by dendrites and to improve lifespan performance. For example, Patent Document 1 below discloses a nickel-zinc battery characterized by having an electrolyte containing sugars. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2021-77594 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] Zinc batteries are sometimes used in low-temperature environments such as 0°C to -30°C, and it is necessary to improve their lifespan performance while suppressing the deterioration of low-temperature discharge performance.
[0007] One aspect of the present invention aims to provide an electrolyte for zinc batteries that can suppress the deterioration of the low-temperature discharge performance of zinc batteries. Another aspect of the present invention aims to provide a zinc battery equipped with said electrolyte for zinc batteries. [Means for solving the problem]
[0008] The specific means for achieving the aforementioned objectives are as follows: <1> An electrolyte for a zinc battery containing an alkali metal hydroxide and a surfactant, wherein the amount of the surfactant is 0.01% by mass or more relative to the total mass of the electrolyte for the zinc battery. <2> The alkali metal hydroxide includes potassium hydroxide. <1> The electrolyte for zinc batteries described above. <3> The surfactant includes at least one selected from the group consisting of cationic surfactants, nonionic surfactants, and anionic surfactants. <1> or <2> The electrolyte for zinc batteries described above. <4> The electrolyte for the zinc battery contains an organic compound containing an oxygen atom. <1> ~ <3> Electrolyte for zinc batteries as described in any one of the items. <5> The organic compound containing the oxygen atom has at least one selected from the group consisting of a carboxyl group, a carboxylic acid base, a hydroxyl group, an epoxy group, and an ether group. <4> The electrolyte for zinc batteries described above. <6> The organic compound containing the oxygen atom includes an ether compound having a heterocycle containing an ether group. <4> or <5> The electrolyte for zinc batteries described above. <7> The aforementioned organic compound containing an oxygen atom includes an ether compound represented by the following general formula (3): <4> ~ <6> Electrolyte for zinc batteries as described in any one of the items.
[0009] [ka]
[0010] [In equation (3), n represents an integer from 1 to 10, and R 1 and R 2 This indicates an organic group. <8> The organic group in the above general formula (3) is an alkyl group or an aryl group. <7> The electrolyte for zinc batteries described above. <9> The ether compound represented by the general formula (3) includes a glyme compound. <7> or <8> The electrolyte for zinc batteries described above. <10> The aforementioned glyme compound includes at least one selected from the group consisting of monoglyme, diglyme, triglyme, and tetraglyme. <9> The electrolyte for zinc batteries described above. <11> Positive electrode and negative electrode, <1> ~ <10> A zinc battery comprising an electrolyte for zinc batteries as described in any one of the items. [Effects of the Invention]
[0011] According to one aspect of the present invention, it is possible to provide an electrolyte for a zinc battery that can suppress the decrease in low-temperature discharge performance of the zinc battery. According to another aspect of the present invention, it is possible to provide a zinc battery equipped with the said electrolyte for a zinc battery. [Modes for carrying out the invention]
[0012] In this disclosure, numerical ranges indicated using "~" represent a range that includes the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of a numerical range in one stage can be arbitrarily combined with the upper or lower limit of a numerical range in another stage. In numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with the values shown in the experimental examples. "A or B" means that either A or B is included, or both are included. Unless otherwise specified, the materials exemplified in this disclosure can be used individually or in combination of two or more. In this disclosure, the amount of each component used in a composition means the total amount of multiple substances present in the composition if there are multiple substances corresponding to each component in the composition, unless otherwise specified. In this disclosure, the terms "film" or "layer" include not only structures that are formed over the entire surface when observed as a plan view, but also structures that are formed in part. In this disclosure, the term "process" includes not only independent processes but also any process that cannot be clearly distinguished from other processes, as long as its intended function is achieved.
[0013] The embodiments of the present invention will be described in detail below. However, the present invention is not limited to the embodiments described below, and can be implemented in various ways within the scope of its gist.
[0014] The electrolyte for a zinc battery according to this embodiment (hereinafter, sometimes simply referred to as "electrolyte") is used as the electrolyte for a zinc battery (e.g., a zinc secondary battery). The zinc battery according to this embodiment comprises a positive electrode, a negative electrode, and the electrolyte according to this embodiment. The zinc battery may be equipped with a zinc electrode as the negative electrode. Examples of zinc batteries include nickel-zinc batteries (e.g., nickel-zinc secondary batteries) in which the positive electrode is a nickel electrode; air-zinc batteries (e.g., air-zinc secondary batteries) in which the positive electrode is an air electrode; and silver-zinc batteries (e.g., silver-zinc secondary batteries) in which the positive electrode is a silver oxide electrode.
[0015] The electrolyte according to this embodiment is an electrolyte for a zinc battery containing an alkali metal hydroxide and a surfactant, wherein the total mass of the surfactant is 0.01% by mass or more of the total mass of the electrolyte for the zinc battery. According to the electrolyte according to this embodiment, it is possible to suppress the decrease in the low-temperature discharge performance of the zinc battery, and for example, it is possible to reduce the DC resistance (hereinafter sometimes referred to as DCR) when the zinc battery is discharged in an environment of -30°C.
[0016] Factors contributing to such effects include, but are not limited to, the following. Specifically, in conventional zinc batteries, the electrolyte does not diffuse uniformly onto the surface of the active material (zinc component) of the zinc electrode, and it is thought that the DC resistance during discharge increases because the active material that does not come into contact with the electrolyte becomes inactive. However, when using the electrolyte of this embodiment, it is presumed that the diffusion of the electrolyte onto the surface of the active material is improved by the surfactant mentioned above, thereby reducing the DC resistance during discharge.
[0017] Examples of alkali metal hydroxides include potassium hydroxide (KOH), sodium hydroxide (NaOH), and lithium hydroxide (LiOH). Alkali metal hydroxides may be ionized (dissociated) in aqueous solution and may exist as salts. From the viewpoint of suppressing the decrease in discharge capacity when zinc batteries are stored and from the viewpoint of easily obtaining excellent high-rate discharge performance, it is preferable that the alkali metal hydroxide contains at least one selected from the group consisting of potassium hydroxide and lithium hydroxide, and more preferably potassium hydroxide.
[0018] The alkali metal hydroxide content (total mass of alkali metal hydroxides) in the electrolyte is preferably within the following ranges based on the total mass of the electrolyte, from the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance. The alkali metal hydroxide content is preferably 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more. The alkali metal hydroxide content is preferably 50% by mass or less, 45% by mass or less, 40% by mass or less, or 35% by mass or less. From these viewpoints, the alkali metal hydroxide content is preferably 10 to 50% by mass.
[0019] From the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance, the potassium hydroxide content in the electrolyte is preferably within the following ranges based on the total mass of the electrolyte. The potassium hydroxide content is preferably 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more. The potassium hydroxide content is preferably 50% by mass or less, 45% by mass or less, 40% by mass or less, or 35% by mass or less. From these viewpoints, the potassium hydroxide content is preferably 10 to 50% by mass.
[0020] From the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance, the lithium hydroxide content in the electrolyte is preferably within the following ranges based on the total mass of the electrolyte. The lithium hydroxide content is preferably 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.8% by mass or more, or 1% by mass or more. The lithium hydroxide content is preferably 3% by mass or less, 2% by mass or less, 1.5% by mass or less, or 1.2% by mass or less. From these viewpoints, the lithium hydroxide content is preferably 0.1 to 3% by mass.
[0021] The electrolytic solution according to the present embodiment contains a surfactant. Examples of the surfactant include cationic surfactants, nonionic surfactants, anionic surfactants, amphoteric surfactants, and the like. From the viewpoint of easily suppressing a decrease in low-temperature discharge performance of a zinc battery, the surfactant preferably contains at least one selected from the group consisting of cationic surfactants, nonionic surfactants, and anionic surfactants. The surfactant is preferably in an aspect containing a cationic surfactant, preferably in an aspect containing a nonionic surfactant, and preferably in an aspect containing an anionic surfactant.
[0022] The cationic surfactant has a cationic hydrophilic group and a hydrophobic group. Examples of the cationic surfactant include quaternary ammonium salt-type cationic surfactants such as aliphatic amines or salts thereof, alkylamidoamine salts, monoalkyltrimethylammonium salts, dialkyldimethylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, and benzethonium chloride salts. From the viewpoint of easily suppressing a decrease in low-temperature discharge performance of a zinc battery, the cationic surfactant preferably contains at least one selected from the group consisting of monoalkyltrimethylammonium salts and dialkyldimethylammonium salts, and more preferably contains a monoalkyltrimethylammonium salt.
[0023] The monoalkyltrimethylammonium salt and the dialkyldimethylammonium salt have, for example, a structure represented by the following general formula (2). (R 2a ) n N + (R 2b ) 4-n X - ···(2) [In formula (2), n is 1 or 2, and R 2a and R 2b are each independently a hydrocarbon group having 1 to 20 carbon atoms, and X - is an anion. When n is 2, a plurality of R 2a may be the same as or different from each other. A plurality of R2b They may be the same or different from each other.
[0024] R 2a The hydrocarbon group may be linear, branched, saturated, or unsaturated, and may include a cyclic structure such as an alicyclic structure. 2a The hydrocarbon group is preferably an alkyl group. 2a The number of carbon atoms in the hydrocarbon group is preferably 12 to 18, and more preferably 14 to 16. 2b The hydrocarbon group may be linear or branched, and may be saturated or unsaturated. 2b The hydrocarbon group is preferably an alkyl group. 2b The number of carbon atoms in the hydrocarbon group is preferably 1 to 4, more preferably 1, 2, or 3. - any anion that can form a salt with the quaternary ammonium ion of formula (2), for example, F - Cl - , Br - , I - Halide ions such as CH3COO - These may be carboxylate ions, sulfate ions, phosphate ions, etc.
[0025] Specific examples of monoalkyltrimethylammonium salts include dodecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, tridecyltrimethylammonium bromide, tridecyltrimethylammonium chloride, tetradecyltrimethylammonium bromide, tetradecyltrimethylammonium chloride, pentadecyltrimethylammonium bromide, pentadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, heptadecyltrimethylammonium bromide, heptadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, and octadecyltrimethylammonium chloride.
[0026] Specific examples of dialkyldimethylammonium salts include didodecyldimethylammonium bromide, didodecyldimethylammonium chloride, ditridecyldimethylammonium bromide, ditridecyldimethylammonium chloride, ditetradecyldimethylammonium bromide, ditetradecyldimethylammonium chloride, dipentadecyldimethylammonium bromide, dipentadecyldimethylammonium chloride, dihexadecyldimethylammonium bromide, dihexadecyldimethylammonium chloride, diheptadecyldimethylammonium bromide, diheptadecyldimethylammonium chloride, dioctadecyldimethylammonium bromide, and dioctadecyldimethylammonium chloride.
[0027] Nonionic surfactants have both a nonionic hydrophilic group and a hydrophobic group. Examples of nonionic surfactants include polyoxyethylene-containing ester compounds such as polyoxyethylene fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene sorbitol fatty acid esters; and polyoxyethylene-containing ether compounds such as polyoxyethylene alkyl ethers and polyoxyethylene alkylphenyl ethers. From the viewpoint of easily suppressing the decrease in low-temperature discharge performance of zinc batteries, the nonionic surfactant preferably contains at least one selected from the group consisting of polyoxyethylene alkyl ethers and polyoxyethylene alkylphenyl ethers, and more preferably contains polyoxyethylene alkylphenyl ethers.
[0028] Polyoxyethylene alkyl ethers have a structure represented by the following general formula (1a), for example. R 1a O(CH2CH2O) m1 H ···(1a) [In equation (1a), m1 is an integer between 2 and 60, R 1a This refers to a hydrocarbon group having 1 to 30 carbon atoms.
[0029] Polyoxyethylene alkylphenyl ethers have a structure represented by the following general formula (1b), for example. R 1b C6H4O(CH2CH2O) m2 H ···(1b) [In equation (1b), m2 is an integer between 2 and 60, R 1b This refers to a hydrocarbon group having 1 to 30 carbon atoms.
[0030] R 1a and R 1b The hydrocarbon group may be linear or branched, and may be saturated or unsaturated. 1a and R 1b The hydrocarbon group is preferably an alkyl group. 1a The number of carbon atoms in the hydrocarbon group is preferably 10 to 18. 1b The number of carbon atoms in the hydrocarbon group is preferably 4 to 12, more preferably 6 to 10, and even more preferably 8. m1 and m2 are the average degrees of polymerization, preferably 5 to 12, and more preferably 7 to 10.
[0031] Specific examples of polyoxyethylene alkyl ethers include polyoxyethylene decyl ether, polyoxyethylene undecyl ether, polyoxyethylene dodecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene tetradecyl ether, polyoxyethylene pentadecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene heptadecyl ether, and polyoxyethylene octadecyl ether.
[0032] Specific examples of polyoxyethylene alkylphenyl ethers include polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether.
[0033] Anionic surfactants have an anionic hydrophilic group and a hydrophobic group. Examples of anionic surfactants include polyoxyalkylene alkyl ether phosphates (e.g., polyoxyethylene alkyl ether phosphates), polyoxyethylene alkyl ether sulfates, sodium dodecylbenzenesulfonate, alkali salts of styrene-acrylic acid copolymers, sodium alkylnaphthalene sulfonate, sodium alkyldiphenyl ether disulfonate, monoethanolamine lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, monoethanolamine stearate, sodium stearate, sodium lauryl sulfate, and monoethanolamine of styrene-acrylic acid copolymers. From the viewpoint of easily suppressing the decrease in low-temperature discharge performance of zinc batteries, anionic surfactants preferably contain polyoxyalkylene alkyl ether phosphates, and more preferably contain polyoxyethylene alkyl ether phosphates.
[0034] When the surfactant includes a cationic surfactant, a nonionic surfactant, or anionic surfactant, the content of the cationic surfactant, nonionic surfactant, or anionic surfactant in the surfactant is preferably 50% by mass or more, 70% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more, based on the total mass of the surfactant, from the viewpoint of easily suppressing a decrease in the charge acceptance of the zinc battery. The surfactant may also be substantially composed of a nonionic surfactant, anionic surfactant, or cationic surfactant (a configuration in which substantially 100% by mass of the surfactant is a nonionic surfactant, anionic surfactant, or cationic surfactant).
[0035] The surfactant content (total mass of surfactants) in the electrolyte is preferably 0.01% by mass or more, based on the total mass of the electrolyte. From the viewpoint of suppressing a decrease in the discharge performance of the zinc battery, the surfactant content is preferably 0.05% by mass or more, 0.06% by mass or more, 0.07% by mass or more, 0.08% by mass or more, or 0.1% by mass or more. From the viewpoint of suppressing a decrease in the discharge performance of the zinc battery, the surfactant content is preferably 5% by mass or less, 2.5% by mass or less, 1% by mass or less, 0.7% by mass or less, or 0.5% by mass or less. From these viewpoints, the surfactant content is preferably 0.01 to 5% by mass. Furthermore, from the viewpoint of suppressing a decrease in the discharge performance of the zinc battery, the surfactant content is particularly preferably 0.1 to 5% by mass.
[0036] When the surfactant includes a cationic surfactant, a nonionic surfactant, or an anionic surfactant, the content of the cationic surfactant, nonionic surfactant, or anionic surfactant in the electrolyte is preferably within the following ranges based on the total amount of the electrolyte, from the viewpoint of suppressing the deterioration of the discharge performance of the zinc battery. The content is preferably 0.01% by mass or more, 0.05% by mass or more, 0.06% by mass or more, 0.07% by mass or more, 0.08% by mass or more, or 0.1% by mass or more. The content is preferably 5% by mass or less, 2.5% by mass or less, 1% by mass or less, 0.7% by mass or less, or 0.5% by mass or less. From these viewpoints, a content of 0.1 to 5% by mass is particularly preferred.
[0037] The electrolyte according to this embodiment may contain an organic compound containing an oxygen atom (excluding alkali metal hydroxides or surfactants; hereinafter referred to as "oxygen-containing compound" as may be used). The oxygen-containing compound may have a functional group containing an oxygen atom. Examples of functional groups containing an oxygen atom include carboxyl groups, carboxylic acid bases, hydroxyl groups (excluding OH structures contained within carboxyl groups), epoxy groups, ether groups, alkoxide groups, ester groups, ketone groups, and aldehyde groups. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, it is preferable that the oxygen-containing compound has at least one selected from the group consisting of carboxyl groups, carboxylic acid bases, hydroxyl groups, epoxy groups, and ether groups.
[0038] When an oxygen-containing compound has an OH structure, the ratio of the number of OH structures to the number of carbon atoms in the oxygen-containing compound (number of OH structures / number of carbon atoms) is preferably within the following ranges from the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance. The ratio is preferably 0.01 or more, 0.03 or more, 0.05 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 5 / 6 or more. The ratio is preferably 2 or less, 1.5 or less, 1.2 or less, 1 or less, 0.9 or less, or 5 / 6 or less. From these viewpoints, the ratio (number of OH structures / number of carbon atoms) is preferably 0.01 to 2. The oxygen-containing compound does not need to have an OH structure.
[0039] From the viewpoint of easily suppressing the decrease in discharge capacity when zinc batteries are stored and from the viewpoint of easily obtaining excellent high-rate discharge performance, it is preferable that the oxygen-containing compound contains at least one selected from the group consisting of sugars, carboxylic acids (excluding compounds that fall under the category of sugars), carboxylates (excluding compounds that fall under the category of sugars), epoxy compounds (compounds having an epoxy group; excluding compounds that fall under the category of sugars, carboxylic acids, or carboxylates), and ether compounds (compounds having an ether group; excluding compounds that fall under the category of sugars, carboxylic acids, carboxylates, or epoxy compounds).
[0040] The carbohydrates used may include monosaccharides, disaccharides, trisaccharides, and polysaccharides (excluding sugars that fall under disaccharides or trisaccharides). Examples of monosaccharides include glucose, fructose, galactose, arabinose, ribose, mannose, xylose, sorbose, rhamnose, fucose, ribodextrose, and their hydrates. Examples of disaccharides include sucrose, maltose, trehalose, cellobiose, genthiobiose, lactose, melibiose, and their hydrates. Examples of trisaccharides include kestose, meletitose, gentianose, raffinose, and their hydrates. Examples of polysaccharides include cyclodextrin (e.g., γ-cyclodextrin) and stachyose. Furthermore, it is preferable that the carbohydrates include non-reducing sugars from the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance.
[0041] Non-reducing sugars are defined as sugars that do not have a free reducing group, as opposed to reducing sugars (sugars that have a free aldehyde group or ketone group, or a hemiacetal-bonded aldehyde group or ketone group) (Comprehensive Dictionary of Chemistry, 1st Edition, published by Tokyo Kagaku Dojin Co., Ltd.). In other words, non-reducing sugars are sugars that do not have a free aldehyde group or ketone group, nor a hemiacetal-bonded aldehyde group or ketone group. Non-reducing sugars may also be hydrates.
[0042] Examples of non-reducing sugars include disaccharides such as sucrose, trehalose, and their hydrates; trisaccharides such as kestose, meletitose, gentianose, and their hydrates; tetrasaccharides such as fungitetraose and its hydrate; and polysaccharides such as α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, and their hydrates. Non-reducing sugars may include disaccharides from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity, and may include at least one selected from the group consisting of sucrose, trehalose, and their hydrates.
[0043] If the non-reducing sugar contains disaccharides, the disaccharide content in the non-reducing sugar may be 50% or more by mass, 70% or more by mass, 90% or more by mass, 95% or more by mass, 97% or more by mass, or 99% or more by mass, based on the total mass of non-reducing sugars contained in the electrolyte, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity. The non-reducing sugar may also be substantially composed of disaccharides (a configuration in which substantially 100% by mass of the non-reducing sugar is disaccharides). If the non-reducing sugar contains sucrose, the sucrose content in the non-reducing sugar may be within the above range from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity. If the non-reducing sugar contains trehalose, the trehalose content in the non-reducing sugar may be within the above range from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity.
[0044] The number of methylol groups (-CH2OH) in a non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity: The number of methylol groups may be 8 or less, 6 or less, 4 or less, 3 or less, or 2 or less. The number of methylol groups may be 2 or more, or 3 or more. From these viewpoints, the number of methylol groups may be between 2 and 8.
[0045] The number of ether groups in a non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity: The number of ether groups may be 16 or less, 12 or less, 8 or less, 6 or less, or 4 or less. The number of ether groups may be 3 or more. From these viewpoints, the number of ether groups may be between 3 and 16.
[0046] The number of hydroxyl groups (excluding OH structures contained within methylol groups) in a non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity: The number of hydroxyl groups may be 16 or less, 12 or less, 8 or less, or 6 or less. The number of hydroxyl groups may be 5 or more, or 6 or more. From these viewpoints, the number of hydroxyl groups may be between 5 and 16.
[0047] The number of carbon atoms in the non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing the decrease in discharge capacity: The number of carbon atoms may be 48 or less, 42 or less, 36 or less, 30 or less, 24 or less, or 18 or less. The number of carbon atoms may be 12 or more. From these viewpoints, the number of carbon atoms may be between 12 and 48.
[0048] The number of five-membered ring structures in a non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity: The number of five-membered ring structures may be 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or 0. The number of five-membered ring structures may be 0 or 1 or more. From these viewpoints, the number of five-membered ring structures may be between 0 and 5.
[0049] The number of six-membered ring structures in a non-reducing sugar may be within the following ranges, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity: The number of six-membered ring structures may be 8 or less, 4 or less, 3 or less, 2 or less, or 1. The number of six-membered ring structures may be 1 or more, or 2 or more. From these viewpoints, the number of six-membered ring structures may be between 1 and 8.
[0050] The content of non-reducing sugars in the electrolyte (total mass of non-reducing sugars contained in the electrolyte) may be within the following ranges based on the total mass of the electrolyte, from the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing a decrease in discharge capacity. The content of non-reducing sugars may be 0.01% by mass or more, 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 1.5% by mass or more, 2% by mass or more, 3% by mass or more, or 4% by mass or more. The content of non-reducing sugars may be 20% by mass or less, 10% by mass or less, 8% by mass or less, 5% by mass or less, 4% by mass or less, 3% by mass or less, 2% by mass or less, or 1% by mass or less. From these viewpoints, the content of non-reducing sugars may be 0.01 to 20% by mass, 0.1 to 10% by mass, 1 to 8% by mass, 1 to 5% by mass, or 1 to 4% by mass.
[0051] From the viewpoint of easily obtaining excellent cycle characteristics and easily suppressing the decrease in discharge capacity, the content of non-reducing sugars may be in the following ranges per 100 parts by mass of alkali metal hydroxide: The content of non-reducing sugars may be 1 part by mass or more, 2 parts by mass or more, 3 parts by mass or more, 6 parts by mass or more, 9 parts by mass or more, or 13 parts by mass or more. The content of non-reducing sugars may be 30 parts by mass or less, 20 parts by mass or less, 16 parts by mass or less, 14 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, or 7 parts by mass or less. From these viewpoints, the content of non-reducing sugars may be 1 to 30 parts by mass.
[0052] Examples of carboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, benzoic acid, salicylic acid, 3,4,5-trihydroxybenzoic acid, benzenehexacarboxylic acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, aconitic acid, pyruvate, oxaloacetate, glycidyl formate, glycidyl acetate, and glycidyl benzoate. Examples of carboxylate salts include salts of these carboxylic acids. Examples of carboxylate salts include alkali metal salts such as sodium salts (e.g., disodium terephthalate) and potassium salts. From the viewpoint of suppressing the decrease in discharge capacity when zinc batteries are stored and from the viewpoint of easily obtaining excellent high-rate discharge performance, it is preferable for carboxylate salts to contain alkali metal salts, and more preferably sodium salts. The oxygen-containing compound preferably contains at least one selected from the group consisting of aromatic ring-containing carboxylic acids and aromatic ring-containing carboxylate salts, from the viewpoint of easily suppressing the decrease in discharge capacity when zinc batteries are stored and easily obtaining excellent high-rate discharge performance, more preferably contains at least one selected from the group consisting of terephthalic acid and terephthalate salts, and even more preferably contains at least one selected from the group consisting of terephthalic acid and sodium salts of terephthalic acid.
[0053] The number of carboxyl groups in a carboxylic acid, or the number of carboxylic acid bases in a carboxylate salt, is preferably one or more. From the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance, the following ranges are preferred: The number of carboxyl groups or carboxylic acid bases is preferably two or more. The number of carboxyl groups or carboxylic acid bases is preferably four or less, three or less, or two or less. The number of carboxyl groups or carboxylic acid bases is preferably one to four.
[0054] Examples of epoxy compounds include monofunctional epoxy compounds and polyfunctional epoxy compounds. Examples of monofunctional epoxy compounds include 1,2-epoxyethane, 1,2-epoxypropane, 1,2-epoxybutane, 1,2-epoxy-2-methylpropane, 1-phenyl-1,2-epoxyethane, epichlorohydrin, epibromohydrin, glycidyl methyl ether, allyl glycidyl ether, polyethylene oxide glycidyl ether, glycidylamide, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, stearyl glycidyl ether, lauryl glycidyl ether, butoxy polyethylene glycol glycidyl ether, phenol polyethylene glycol glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, p-methylphenyl glycidyl ether, p-ethylphenyl glycidyl ether, p-sec-butylphenyl glycidyl ether, p-tert-butylphenyl glycidyl ether, glycidyl acrylate, and glycidyl methacrylate. Examples of polyfunctional epoxy compounds include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, polyphenol type epoxy compounds, cyclic aliphatic epoxy compounds, aliphatic glycidyl ether epoxy compounds, glycidyl ester epoxy compounds, glycidyl diamine epoxy compounds, and heterocyclic epoxy compounds. The oxygen-containing compound is preferably a monofunctional epoxy compound, and more preferably 1,2-epoxy-2-methylpropane, from the viewpoint of suppressing the decrease in discharge capacity when zinc batteries are stored and from the viewpoint of easily obtaining excellent high-rate discharge performance.
[0055] Examples of ether compounds include crown ether compounds such as 18-crown-6, 15-crown-5, 12-crown-4, dibenzo-18-crown-6, dicyclohexano-18-crown-6, and dibenzo-24-crown-8; polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; and glycerin. Polyether compounds can be used as the ether compound. The oxygen-containing compound is preferably an ether compound having a heterocyclic ring containing an ether group, and more preferably 18-crown-6, from the viewpoint of easily suppressing the decrease in discharge capacity when zinc batteries are stored and easily obtaining excellent high-rate discharge performance.
[0056] The number of ether groups in the ether compound is preferably one or more, from the viewpoint of suppressing the decrease in discharge capacity when storing zinc batteries and from the viewpoint of easily obtaining excellent high-rate discharge performance, the following ranges are preferred: The number of ether groups is preferably two or more, three or more, four or more, five or more, or six or more. The number of ether groups is preferably 10 or less, nine or less, eight or less, seven or less, or six or less. The number of ether groups is preferably 1 to 10.
[0057] The oxygen-containing compound may also include an ether compound represented by the following general formula (3).
[0058] [ka]
[0059] In equation (3), n represents an integer from 1 to 10, and R 1 and R 2 This indicates an organic group.
[0060] In general formula (3), n may be within the following ranges from the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance: n may be 8 or less, 6 or less, 4 or less, 3 or less, or 2 or less. n may be 2 or more, 3 or more, or 4 or more. From these viewpoints, n may be 1 to 8, 1 to 6, or 1 to 4.
[0061] The number of ether groups in an ether compound represented by general formula (3) may be within the following ranges, from the viewpoint of easily obtaining excellent lifetime performance and excellent high-rate discharge performance: The number of ether groups may be 9 or less, 7 or less, 5 or less, 4 or less, or 3 or less. The number of ether groups may be 1 or more, 2 or more, 3 or more, 4 or more, or 5 or more. From these viewpoints, the number of ether groups may be 1 to 9, 2 to 7, or 2 to 5.
[0062] R in general formula (3) 1 and R 2 From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, both may be organic groups. Examples of organic groups include alkyl groups, aryl groups, ester groups, carboxyl groups, and carboxylic acid bases (sodium salts, potassium salts, etc.). From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, the organic group may be an alkyl group or an aryl group, or it may be an alkyl group.
[0063] The organic group may have substituents. Examples of substituents include halogen atoms, carboxyl groups, carboxylic acid bases, ether groups, alkoxide groups, ester groups, ketone groups, and aldehyde groups. From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, the organic group may be an unsubstituted organic group, an unsubstituted alkyl group, or an unsubstituted aryl group, or an unsubstituted alkyl group.
[0064] The number of carbon atoms in the organic group (including the carbon atoms of substituents on the organic group) may be 8 or less, 6 or less, 4 or less, 3 or less, 2 or less, or 1, from the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance. The number of carbon atoms in the organic group may be 1 or more. From these viewpoints, the number of carbon atoms in the organic group may be 1 to 8.
[0065] The alkyl group may be linear or branched. From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, the alkyl group may be a linear alkyl group, and may be a methyl group, an ethyl group, an n-propyl group, or an n-butyl group, or it may be a methyl group.
[0066] R 1 and R 2 From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, these may be the same organic group, the same alkyl group, or a methyl group.
[0067] Examples of ether compounds represented by general formula (3) include polyoxyethylene dialkyl ethers (hereinafter sometimes referred to as glyme compounds) and polyoxyethylene alkyl ether compounds such as polyoxyethylene alkylphenyl ethers. From the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance, the ether compound represented by general formula (3) may contain polyoxyethylene alkyl ether compounds and may contain glyme compounds.
[0068] Examples of glyme compounds include polyoxyethylene dimethyl ether, polyoxyethylene diethyl ether, polyoxyethylene dipropyl ether, polyoxyethylene dibutyl ether, polyoxyethylene dipentyl ether, polyoxyethylene dihexyl ether, polyoxyethylene diheptyl ether, polyoxyethylene dioctyl ether, and polyoxyethylene methyl ethyl ether.
[0069] The glyme compound may be a monoglyme compound such as monoglyme (ethylene glycol dimethyl ether), ethylene glycol diethyl ether, ethylene glycol dipropyl ether, or ethylene glycol dibutyl ether; a diglyme compound such as diglyme (diethylene glycol dimethyl ether), diethylene glycol diethyl ether, diethylene glycol dipropyl ether, or diethylene glycol dibutyl ether; a triglyme compound such as triglyme (triethylene glycol dimethyl ether), triethylene glycol diethyl ether, triethylene glycol dipropyl ether, or triethylene glycol dibutyl ether; or a tetraglyme compound such as tetraglyme (tetraethylene glycol dimethyl ether), tetraethylene glycol diethyl ether, tetraethylene glycol dipropyl ether, or tetraethylene glycol dibutyl ether. The ether compound represented by general formula (3) may contain at least one selected from the group consisting of monoglime compounds, diglime compounds, triglime compounds, and tetraglime compounds, from the viewpoint of easily obtaining excellent lifetime performance and excellent high-rate discharge performance, it may contain at least one selected from the group consisting of monoglime, diglime, triglime, and tetraglime, it may contain at least one selected from the group consisting of diglime and triglime, and it may contain diglime.
[0070] Examples of polyoxyethylene alkylphenyl ethers include polyoxyethylene methylphenyl ether, polyoxyethylene ethylphenyl ether, polyoxyethylene propylphenyl ether, polyoxyethylene butylphenyl ether, polyoxyethylene pentylphenyl ether, polyoxyethylene hexylphenyl ether, polyoxyethylene heptylphenyl ether, and polyoxyethylene nonylphenyl ether.
[0071] When the ether compound represented by general formula (3) contains a glyme compound, the amount of the glyme compound in the ether compound represented by general formula (3) may be 50% by mass or more, 70% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more, based on the amount of the ether compound represented by general formula (3) (total amount of the ether compound represented by general formula (3)), from the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance. The ether compound represented by general formula (3) may also be substantially composed of a glyme compound (substantially 100% by mass of the ether compound represented by general formula (3) is a glyme compound).
[0072] The content of the ether compound represented by general formula (3) may be within the following ranges per 100 parts by mass of alkali metal hydroxide, from the viewpoint of easily obtaining excellent lifespan performance and excellent high-rate discharge performance. The content of the ether compound represented by general formula (3) may be 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 5.5 parts by mass or more, or 6 parts by mass or more. The content of the ether compound represented by general formula (3) may be 30 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, or 6.5 parts by mass or less. From these viewpoints, the content of the ether compound represented by general formula (3) may be 1 to 30 parts by mass.
[0073] From the viewpoint of easily suppressing the decrease in discharge capacity when zinc batteries are stored and easily obtaining excellent high-rate discharge performance, the molecular weight of the oxygen-containing compound is preferably 50 or more, 70 or more, 80 or more, 100 or more, 120 or more, 150 or more, 160 or more, 170 or more, or 180 or more. From the viewpoint of easily suppressing the decrease in discharge capacity when zinc batteries are stored and easily obtaining excellent high-rate discharge performance, the molecular weight of the oxygen-containing compound is preferably 2000 or less, 1500 or less, 1300 or less, 1200 or less, 1000 or less, 800 or less, or 600 or less. From these viewpoints, the molecular weight of the oxygen-containing compound is preferably 50 to 2000. The molecular weight of the oxygen-containing compound may be 190 or more, 200 or more, 210 or more, 220 or more, 240 or more, 260 or more, 300 or more, 340 or more, 350 or more, 400 or more, 450 or more, or 500 or more. The molecular weight of the oxygen-containing compound may be 500 or less, 400 or less, 350 or less, 340 or less, 320 or less, 300 or less, 280 or less, 270 or less, 260 or less, 250 or less, 230 or less, 220 or less, 210 or less, 200 or less, 190 or less, or 185 or less. The molecular weight is measured by the GPC (Gel Permeation Chromatography) method. If the oxygen-containing compound is a pure substance such as a monosaccharide, disaccharide, or glyme compound, the molecular weight of the oxygen-containing compound refers to the chemical formula weight of that compound.
[0074] As the oxygen-containing compound, it is preferable to use a compound that has high solubility in the electrolyte. Even compounds with low solubility can be used after removing residue by filtration, etc. The electrolyte according to this embodiment does not need to contain alcohol.
[0075] The oxygen-containing compound content in the electrolyte is preferably within the following ranges based on the total mass of the electrolyte. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the oxygen-containing compound content is preferably 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.8% by mass or more, or 1% by mass or more. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the oxygen-containing compound content is preferably 5% by mass or less, 4.5% by mass or less, 4% by mass or less, 3.5% by mass or less, or 3% by mass or less. From these viewpoints, the oxygen-containing compound content is preferably 0.1 to 5% by mass. From the viewpoint of further easily suppressing the decrease in discharge capacity when storing zinc batteries, the oxygen-containing compound content is preferably 1.2% by mass or more, 1.5% by mass or more, 1.8% by mass or more, 2% by mass or more, 2.2% by mass or more, 2.5% by mass or more, 2.7% by mass or more, or 3% by mass or more. The oxygen-containing compound content may be 3.5% by mass or more, 4% by mass or more, 4.5% by mass or more, or 5% by mass or more. From the viewpoint of obtaining even better high-rate discharge performance, the oxygen-containing compound content is preferably 2.7% by mass or less, 2.5% by mass or less, 2.2% by mass or less, 2% by mass or less, 1.7% by mass or less, 1.5% by mass or less, 1.2% by mass or less, or 1% by mass or less. The oxygen-containing compound content may be less than 0.5 mol / L based on the total amount of electrolyte.
[0076] The content of the oxygen-containing compound is preferably within the following ranges per 1 part by mass of surfactant. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the content of the oxygen-containing compound is preferably 2 parts by mass or more, 3 parts by mass or more, 5 parts by mass or more, 10 parts by mass or more, 30 parts by mass or more, 50 parts by mass or more, 80 parts by mass or more, or 100 parts by mass or more. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the content of the oxygen-containing compound is preferably 1000 parts by mass or less, 800 parts by mass or less, 600 parts by mass or less, 500 parts by mass or less, 450 parts by mass or less, 400 parts by mass or less, 350 parts by mass or less, or 300 parts by mass or less. From these viewpoints, the content of the oxygen-containing compound may be 2 to 1000 parts by mass, and is preferably 10 to 1000 parts by mass. From the viewpoint of further suppressing the decrease in discharge capacity when zinc batteries are stored, the oxygen-containing compound content is preferably 150 parts by mass or more, 200 parts by mass or more, 250 parts by mass or more, or 300 parts by mass or more. The oxygen-containing compound content may be 350 parts by mass or more, 400 parts by mass or more, 450 parts by mass or more, or 500 parts by mass or more. The oxygen-containing compound content is preferably 250 parts by mass or less, 200 parts by mass or less, 150 parts by mass or less, or 100 parts by mass or less.
[0077] The oxygen-containing compound content is preferably within the following ranges per 100 parts by mass of alkali metal hydroxide. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the oxygen-containing compound content is preferably 1 part by mass or more, 1.5 parts by mass or more, 2 parts by mass or more, 2.5 parts by mass or more, or 3 parts by mass or more. From the viewpoint of easily suppressing the decrease in discharge capacity when storing zinc batteries and easily obtaining excellent high-rate discharge performance, the oxygen-containing compound content is preferably 30 parts by mass or less, 25 parts by mass or less, 20 parts by mass or less, 16 parts by mass or less, 15 parts by mass or less, 13 parts by mass or less, 12 parts by mass or less, or 10 parts by mass or less. From these viewpoints, the oxygen-containing compound content is preferably 1 to 30 parts by mass. From the viewpoint of further easily suppressing the decrease in discharge capacity when storing zinc batteries, the oxygen-containing compound content is preferably 4 parts by mass or more, 5 parts by mass or more, 6 parts by mass or more, 7 parts by mass or more, 8 parts by mass or more, or 9 parts by mass or more. The oxygen-containing compound content may be 10 parts by mass or more, 12 parts by mass or more, 13 parts by mass or more, 15 parts by mass or more, or 16 parts by mass or more. From the viewpoint of obtaining even better high-rate discharge performance, the oxygen-containing compound content is preferably 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, 6 parts by mass or less, 5 parts by mass or less, or 4 parts by mass or less.
[0078] The electrolyte according to this embodiment may contain a liquid medium such as water (e.g., deionized water).
[0079] Below, a nickel-zinc battery will be described as an example of a zinc battery using the electrolyte according to the above embodiment.
[0080] The zinc battery according to this embodiment comprises, for example, a battery case, an electrode group (e.g., an electrode plate group) and an electrolyte housed in the battery case. The zinc battery according to this embodiment may be either post-chemically converted or pre-chemically converted.
[0081] The electrode group comprises, for example, a positive electrode (e.g., a positive electrode plate), a negative electrode (e.g., a negative electrode plate), and a separator. The positive electrode and the negative electrode are adjacent to each other, separated by one or more separators. That is, one or more separators are provided between adjacent positive and negative electrodes. The electrode group may comprise multiple positive electrodes, negative electrodes, and separators. When the electrode group comprises multiple positive electrodes and / or multiple negative electrodes, the positive and negative electrodes may be stacked alternately via separators. Multiple positive electrodes and multiple negative electrodes may be connected to each other, for example, by straps.
[0082] In the zinc battery according to this embodiment, the negative electrode comprises a negative electrode current collector and a negative electrode material (electrode material) supported by the current collector. The negative electrode may be either pre-chemical or post-chemical.
[0083] The negative electrode current collector constitutes the conductive path for the current from the negative electrode material. The negative electrode current collector has a shape such as a flat plate or a sheet. The negative electrode current collector may also be a current collector with a three-dimensional mesh structure composed of foamed metal, expanded metal, perforated metal, felt-like material of metal fibers, etc. The negative electrode current collector is made of a material that has conductivity and alkali resistance. As such a material, for example, a material that is stable even at the reaction potential of the negative electrode (a material having an oxidation-reduction potential nobler than the reaction potential of the negative electrode, a material that forms a protective film such as an oxide film on the substrate surface in an alkaline aqueous solution to stabilize it, etc.) can be used. In addition, at the negative electrode, a decomposition reaction of the electrolyte proceeds as a side reaction and hydrogen gas is generated, but a material with a high hydrogen overpotential is preferable in that it can suppress the progress of such a side reaction. Specific examples of materials that constitute the negative electrode current collector include metal materials with metal plating such as zinc, lead, tin, etc. (copper, brass, steel, nickel, etc.).
[0084] The negative electrode material may, for example, be layered. That is, the negative electrode may have a negative electrode material layer. The negative electrode material layer may be formed on the negative electrode current collector. If the portion of the negative electrode current collector that supports the negative electrode material has a three-dimensional mesh structure, the negative electrode material may be filled between the mesh of the current collector to form the negative electrode material layer.
[0085] The negative electrode material contains a negative electrode active material (electrode active material) containing zinc. Examples of negative electrode active materials include metallic zinc, zinc oxide, and zinc hydroxide. The negative electrode active material may contain one of these components alone or multiple components. For example, the negative electrode material contains metallic zinc in the fully charged state and zinc oxide and zinc hydroxide in the discharged state. The discharged state refers to the state after discharge to a termination voltage of 1.1V. The negative electrode active material is, for example, particulate. That is, the negative electrode material may contain at least one selected from the group consisting of metallic zinc particles, zinc oxide particles, and zinc hydroxide particles. The content of the negative electrode active material may be, for example, 50 to 95% by mass based on the total mass of the negative electrode material.
[0086] The negative electrode material may contain additives. Examples of additives include binders. Examples of binders include polytetrafluoroethylene, hydroxyethylcellulose, polyethylene oxide, polyethylene, and polypropylene. The amount of binder may be, for example, 0.5 to 10 parts by mass per 100 parts by mass of the negative electrode active material.
[0087] The positive electrode comprises, for example, a positive electrode current collector and a positive electrode material supported by the positive electrode current collector. The positive electrode may be either pre-chemical or post-chemical.
[0088] The positive electrode current collector constitutes the conductive path for the current from the positive electrode material. The positive electrode current collector has a shape such as a flat plate or a sheet. The positive electrode current collector may also be a current collector with a three-dimensional mesh structure composed of foamed metal, expanded metal, perforated metal, felt-like material of metal fibers, etc. The positive electrode current collector is made of a material that has conductivity and alkali resistance. As such a material, for example, a material that is stable even at the reaction potential of the positive electrode (a material having an oxidation-reduction potential nobler than the reaction potential of the positive electrode, a material that forms a protective film such as an oxide film on the surface of the substrate in an alkaline aqueous solution to stabilize it, etc.) can be used. In addition, at the positive electrode, a decomposition reaction of the electrolyte proceeds as a side reaction and oxygen gas is generated, but a material with a high oxygen overpotential is preferable in that it can suppress the progress of such a side reaction. Specific examples of materials that constitute the positive electrode current collector include platinum; nickel (foamed nickel, etc.); and metal materials with metal plating such as nickel (copper, brass, steel, etc.). Among these, a positive electrode current collector made of foamed nickel is preferably used. From the viewpoint of further improving high-rate discharge performance, it is preferable that at least the portion of the positive electrode current collector that supports the positive electrode material (positive electrode material support portion) is made of foamed nickel.
[0089] The positive electrode material may, for example, be layered. That is, the positive electrode may have a positive electrode material layer. The positive electrode material layer may be formed on the positive electrode current collector. If the positive electrode material support portion of the positive electrode current collector has a three-dimensional mesh structure, the positive electrode material may be filled between the mesh of the current collector to form the positive electrode material layer.
[0090] The positive electrode material contains a positive electrode active material (electrode active material) containing nickel. Examples of positive electrode active materials include nickel oxyhydroxide (NiOOH) and nickel hydroxide. For example, the positive electrode material contains nickel oxyhydroxide in the fully charged state and nickel hydroxide in the discharged state. The content of the positive electrode active material may be, for example, 50 to 95% by mass based on the total mass of the positive electrode material.
[0091] The positive electrode material may further contain other components besides the positive electrode active material as additives. Examples of additives include binders, conductive agents, and swelling inhibitors.
[0092] Examples of binders include hydrophilic or hydrophobic polymers. Specifically, for example, carboxymethylcellulose (CMC), hydroxyethylcellulose (HEC), hydroxypropylmethylcellulose (HPMC), sodium polyacrylate (SPA), and fluorine-based polymers (such as polytetrafluoroethylene (PTFE)) can be used as binders. The binder content may be, for example, 0.01 to 5 parts by mass per 100 parts by mass of positive electrode active material.
[0093] Examples of conductive agents include cobalt compounds (metallic cobalt, cobalt oxide, cobalt hydroxide, etc.). The content of the conductive agent may be, for example, 1 to 20 parts by mass per 100 parts by mass of positive electrode active material.
[0094] Examples of expansion inhibitors include zinc oxide. The amount of expansion inhibitor may be, for example, 0.01 to 5 parts by mass per 100 parts by mass of positive electrode active material.
[0095] The separator may have a shape such as a flat plate or a sheet. Examples of separators include polyolefin-based microporous membranes, nylon-based microporous membranes, oxidation-resistant ion exchange resin membranes, cellophane-based recycled resin membranes, microporous membranes containing inorganic particles, and polyolefin-based nonwoven fabrics. The separator may be processed into a bag shape so as to be able to accommodate the positive electrode and / or negative electrode. In this case, the positive electrode and / or negative electrode may be housed in the separator. One type of separator may be used alone, or two or more types may be used in combination.
[0096] The nickel-zinc battery manufacturing method described above comprises, for example, a component manufacturing step for obtaining components of a zinc battery, and an assembly step for assembling the components to obtain a zinc battery. In the component manufacturing step, at least electrodes (positive electrode and negative electrode) are obtained.
[0097] Electrodes can be obtained, for example, by adding a solvent (e.g., water) to the raw materials of the electrode material (positive electrode material and negative electrode material) and kneading them to obtain an electrode material paste (paste-like electrode material), and then forming an electrode material layer using the electrode material paste.
[0098] Examples of raw materials for the positive electrode material include raw materials for the positive electrode active material (e.g., nickel hydroxide) and additives (e.g., the above-mentioned binders). Examples of raw materials for the negative electrode material include raw materials for the negative electrode active material (e.g., metallic zinc, zinc oxide, and zinc hydroxide) and additives (e.g., binders).
[0099] One method for forming the electrode material layer is to apply or fill an electrode material paste onto a current collector and then dry it to obtain the electrode material layer. The density of the electrode material layer may be increased as needed by pressing with rollers or the like.
[0100] In the assembly process, for example, the positive and negative electrodes obtained in the component manufacturing process are stacked alternately with separators in between, and then the positive electrodes and negative electrodes are connected with straps to create an electrode group. Next, this electrode group is placed in the battery case, and then a lid is glued to the top surface of the battery case to obtain an unformed zinc battery (nickel-zinc battery).
[0101] Next, the electrolyte according to this embodiment is injected into the battery case of an unformed zinc battery and left for a certain period of time. Then, charging is performed under predetermined conditions to form a zinc battery (nickel-zinc battery). The formation conditions can be adjusted according to the properties of the electrode active materials (positive electrode active material and negative electrode active material). For example, a nickel-zinc battery after formation can be produced by charging under conditions of 32 mA for 12 hours.
[0102] The above describes an example of a nickel-zinc battery (e.g., a nickel-zinc secondary battery) in which the positive electrode is a nickel electrode. However, a zinc battery may also be an air-zinc battery (e.g., an air-zinc secondary battery) in which the positive electrode is an air electrode, or a silver-zinc battery (e.g., a silver-zinc secondary battery) in which the positive electrode is a silver oxide electrode. The above zinc battery, from the perspective of suppressing the decrease in discharge performance at low temperatures, ideally has a DC resistance (DCR) per unit area of total electrode area at -30°C of 0 Ω·cm. 2 This is the most preferable option, but it is difficult in practice, and at least 20 Ω·cm is required. 2 Below, 15Ω cm 2 Below, 10Ω cm 2 Below, 5Ω cm 2 The following, or 1Ω·cm 2 The following are preferable.
[0103] As the air electrode of a zinc-air battery, a known air electrode used in zinc-air batteries can be used. The air electrode includes, for example, an air electrode catalyst, an electronically conductive material, etc. As the air electrode catalyst, an air electrode catalyst that also functions as an electronically conductive material can be used.
[0104] As the air electrode catalyst, it is possible to use one that functions as the positive electrode in a zinc-air cell, and various air electrode catalysts that can utilize oxygen as the positive electrode active material can be used. Examples of air electrode catalysts include carbon-based materials (such as graphite) with redox catalytic function, metal materials (such as platinum and nickel) with redox catalytic function, and inorganic oxide materials (such as perovskite oxides, manganese dioxide, nickel oxide, cobalt oxide, and spinel oxide) with redox catalytic function. The shape of the air electrode catalyst is not particularly limited, but may be particulate, for example. The amount of air electrode catalyst used in the air electrode may be 5 to 70% by volume, 5 to 60% by volume, or 5 to 50% by volume, relative to the total volume of the air electrode.
[0105] As the electronically conductive material, any material that is conductive and enables electron conduction between the air electrode catalyst and the separator can be used. Examples of electronically conductive materials include carbon blacks such as Ketjenblack, acetylene black, channel black, furnace black, lamp black, and thermal black; graphites such as natural graphite, artificial graphite, and expanded graphite; conductive fibers such as carbon fibers and metal fibers; metal powders such as copper, silver, nickel, and aluminum; organic electronically conductive materials such as polyphenylene derivatives; and any mixture thereof. The shape of the electronically conductive material may be particulate or other shapes. Preferably, the electronically conductive material is used in a form that provides a continuous phase in the thickness direction at the air electrode. For example, the electronically conductive material may be a porous material. Furthermore, the electronically conductive material may be in the form of a mixture or composite with the air electrode catalyst, or, as mentioned above, the air electrode catalyst may also function as an electronically conductive material. The amount of electronically conductive material used in the air electrode may be 10 to 80% by volume, 15 to 80% by volume, or 20 to 80% by volume, relative to the total volume of the air electrode.
[0106] For the silver oxide electrode of a silver-zinc battery, a known silver oxide electrode used in silver-zinc batteries can be used. The silver oxide electrode contains, for example, silver(I) oxide. [Examples]
[0107] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples.
[0108] <Preparation of Electrolyte> (Examples 1-20 and Comparative Examples 1-2) An electrolyte solution (containing 30% potassium hydroxide, 1% lithium hydroxide, and the additives shown in Table 1, relative to the total mass of the electrolyte solution) was prepared by mixing deionized water, potassium hydroxide (KOH), lithium hydroxide (LiOH), and the additives shown in Table 1 below.
[0109] As the cationic surfactant, tetradecyltrimethylammonium bromide (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used.
[0110] <Fabrication of the positive electrode> A lattice made of foamed nickel with a porosity of 95% was prepared, and a positive electrode current collector was obtained by pressure molding the lattice. Next, a positive electrode material paste was prepared by weighing and mixing predetermined amounts of cobalt-coated nickel hydroxide powder (manufactured by Gold Shine Energy Material Co., Ltd., Y6 (trade name)), metallic cobalt (manufactured by Nikko Co., Ltd., EXTRA FINE (trade name)), cobalt hydroxide (manufactured by Ise Chemical Industry Co., Ltd.), yttrium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent grade), carboxymethylcellulose (CMC, manufactured by Wei Yi Chemical (Suzhou) Co., Ltd., BH90-3 (trade name)), polytetrafluoroethylene (PTFE, manufactured by Daikin Industries, Ltd., D210-C (trade name)), and deionized water, and stirring the mixture. At this time, the mass ratio of solids was adjusted to "nickel hydroxide: metallic cobalt: yttrium oxide: cobalt hydroxide: CMC: PTFE = 88.0:10.3:1.0:0.3:0.3:0.1". The moisture content of the positive electrode paste was adjusted to 27.5% by mass based on the total mass of the positive electrode paste. Next, the positive electrode paste was applied to the positive electrode support part of the positive electrode current collector and dried at 80°C for 30 minutes. After that, it was pressure-molded using a roll press to obtain an unformed positive electrode having a positive electrode layer.
[0111] <Fabrication of the negative electrode> A tin-plated steel plate perforated metal with a 50% porosity was prepared as the negative electrode current collector. Next, predetermined amounts of zinc oxide (manufactured by Mitsui Mining & Smelting Co., Ltd., general product), metallic zinc (manufactured by Mitsui Mining & Smelting Co., Ltd., MA-ZB (product name)), bismuth oxide (manufactured by Corefront Co., Ltd., 4115CB (product name)), hydroxyethylcellulose (HEC, manufactured by Sumitomo Seika Co., Ltd., AV-15F (product name)), and deionized water were weighed and mixed, and the resulting mixture was stirred to prepare a negative electrode material paste. At this time, the mass ratio of solids was adjusted to "zinc oxide:metallic zinc:bismuth oxide:HEC = 73.0:20.5:5.0:1.5". The moisture content of the negative electrode material paste was adjusted to 22.5% by mass based on the total mass of the negative electrode material paste. Next, the negative electrode material paste was applied to the negative electrode current collector and dried at 80°C for 30 minutes. Subsequently, the material was pressure-molded using a roll press to obtain an unformed negative electrode having a negative electrode material (negative electrode material layer).
[0112] <Preparing the separator> For the separator, UP3355 (manufactured by Ube Industries, Ltd., trade name, air permeability: 440 sec / 100 mL) was used as the microporous membrane, and nonwoven fabric (manufactured by Nippon Kodo Paper Industry Co., Ltd., trade name: VL-100, air permeability: 0.3 sec / 100 mL) was used as the nonwoven fabric. The microporous membrane was hydrophilized with the surfactant Triton-X100 (manufactured by Sigma-Aldrich Japan LLC) before battery assembly. The hydrophilization treatment was performed by immersing the microporous membrane in an aqueous solution containing 1% by mass of Triton-X100 for 24 hours, followed by drying at room temperature for 1 hour. The air permeability of the microporous membrane is shown as the value after the hydrophilization treatment. Furthermore, the microporous membrane was cut to a predetermined size, folded in half, and processed into a bag shape by heat-sealing the sides with the folded part as the bottom. The nonwoven fabric was cut to a predetermined size. The air permeability referred to here is a value measured according to the method specified in JIS P 8117:2009.
[0113] <Manufacturing of nickel-zinc batteries> One positive electrode (unformed positive electrode) and one negative electrode (unformed negative electrode) were housed in a microporous membrane processed into a bag shape. The positive electrode housed in the microporous membrane, the negative electrode housed in the microporous membrane, and a nonwoven fabric were laminated together, and then electrode plates of the same polarity were connected with straps to create an electrode group (electrode plate group). The electrode group consisted of two positive electrodes and three negative electrodes, with one nonwoven fabric placed between each positive and negative electrode (between the microporous membrane on the positive electrode side and the microporous membrane on the negative electrode side). After placing this electrode group in a battery case, a lid was attached to the top surface of the battery case, and the electrolyte was injected into the battery case to obtain an unformed nickel-zinc battery. Subsequently, charging was performed under conditions of an ambient temperature of 25°C, 32mA, and 12 hours to produce a nickel-zinc battery with a nominal capacity of 320mAh.
[0114] <Evaluation of DC resistance> Using the nickel-zinc batteries of the above-described examples and comparative examples, constant voltage charging was performed at 1.9V (charging terminated when the current decreased to 16mA (0.05C)) in an environment of 25°C. Then, constant current discharge was performed for 1 second at current values of 160mA (0.5C), 320mA (1C), 640mA (2C), and 960mA (3C) in an environment of -30°C, and the DC resistance per total electrode area (DCR) was calculated using the following formula. After constant current discharge, each battery was charged at a constant current of 1C (current value 320mA) in an environment of -30°C until the discharge capacity equaled the charge capacity. The unit "C" represents the relative magnitude of the current when discharging from a fully charged state to the rated capacity at a constant current. The unit "C" means "discharge current value (A) / battery capacity (Ah)". For example, we define "1C" as the current that can completely discharge the rated capacity in one hour, and "0.5C" as the current that can discharge it in two hours. DCR={(ΔV 0.5C -V)(I 0.5C -I)+(ΔV 1.0C -V)(I 1.0C -I)+(ΔV 2.0C -V)(I 2.0C ―I)+(ΔV 3.0C -V)(I 3.0C ―I)} / {(I 0.5C -I) 2 +( I 1.0C -I)2 +( I 2.0C -I) 2 +( I 3.0C -I) 2}·A E Here, I = ( 0.5C +I 1.0C +I 2.0C +I 3.0C ) / 4, V=ΔV 0.5C +ΔV 1.0C +ΔV 2.0C +ΔV 3.0C ) / 4, and I 0.5C , I 1.0C , I 2.0C and I 3.0C These represent the discharge current values corresponding to the discharge rates of 0.5C, 1.0C, 2.0C, and 3.0C, respectively, and ΔV 0.5C , ΔV 1.0C , ΔV 2.0C and ΔV 3.0C This shows the voltage change after 1 second for each discharge current value. E This indicates the total electrode area.
[0115] <Evaluation of cycle life performance> At 70°C, a nickel-zinc battery was charged at a constant voltage of 1.88V with a current of 105.7mA (0.33C) until the current decreased to 16mA (0.05C). This was followed by discharging the battery at a constant current of 105.7mA (0.33C) until the battery voltage reached 1.1V. One cycle was defined as this process. The number of cycles required to achieve a 70% retention rate of the discharge capacity relative to the discharge capacity of the first cycle was defined as the cycle life performance.
[0116] [Table 1]
[0117] In Table 1, the compound names A to G are as follows: A: Tetradecyltrimethylammonium bromide ba: sucrose C: Jig Lime D: Glucose E: Monoglim F: Triglyme G: Tetraglyme
[0118] The DCR of the zinc batteries in Examples 1 and 2, which do not contain oxygen-containing compounds, is lower than that of the zinc batteries in Comparative Examples 1 and 2. The cycle life performance of the zinc batteries in Examples 4-20 and Comparative Examples 1-2 was equivalent, but the DCR of the zinc batteries in Examples 4-20 was significantly reduced compared to the DCR of the zinc batteries in Comparative Examples 1-2. This is thought to be due to improved diffusion of the electrolyte onto the active material surface.
[0119] The disclosure of Japanese Patent Application No. 2021-138859, filed on 27 August 2021, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted as being incorporated by reference.
Claims
1. An electrolyte for a zinc battery containing an alkali metal hydroxide and a surfactant, wherein the amount of the surfactant is 0.01% by mass or more relative to the total mass of the zinc battery electrolyte. The electrolyte for the zinc battery contains an organic compound containing an oxygen atom, An electrolyte for a zinc battery, wherein the organic compound containing the oxygen atom contains an ether compound having a heterocycle containing an ether group.
2. An electrolyte for a zinc battery containing an alkali metal hydroxide and a surfactant, wherein the amount of the surfactant is 0.01% by mass or more relative to the total mass of the zinc battery electrolyte. The electrolyte for the zinc battery contains an organic compound containing an oxygen atom, The aforementioned organic compound containing an oxygen atom includes an ether compound represented by the following general formula (3): An electrolyte for a zinc battery, wherein the ether compound represented by the general formula (3) contains a glyme compound. 【Chemistry 1】 [In equation (3), n represents an integer from 1 to 10, and R 1 and R 2 This indicates an organic group.
3. The electrolyte for a zinc battery according to claim 2, wherein the glyme compound comprises at least one selected from the group consisting of monoglyme, diglyme, triglyme, and tetraglyme.
4. An electrolyte for a zinc battery containing an alkali metal hydroxide and a surfactant, wherein the amount of the surfactant is 0.01% by mass or more relative to the total mass of the zinc battery electrolyte. The electrolyte for the zinc battery contains an organic compound containing an oxygen atom, An electrolyte for a zinc battery, wherein the aforementioned organic compound containing an oxygen atom comprises at least one selected from the group consisting of oxalic acid and oxalates.
5. The electrolyte for a zinc battery according to claim 1, 2, or 4, wherein the alkali metal hydroxide contains potassium hydroxide.
6. The electrolyte for a zinc battery according to claim 1, 2, or 4, wherein the surfactant comprises at least one selected from the group consisting of cationic surfactants, nonionic surfactants, and anionic surfactants.
7. A zinc battery comprising a positive electrode, a negative electrode, and the electrolyte for a zinc battery according to claim 1, 2, or 4.
Citation Information
Patent Citations
Alkali storage battery
JP2019160669A
Zinc battery electrolyte and zinc battery
JP2020155266A
Electrolyte for zinc battery and zinc battery
JP2021077594A