Lithium nitride passivation as a cathode prelithium reagent
A passivation coating on Li3N particles addresses the reactivity issues, stabilizing Li3N and improving the electrochemical performance and processing flexibility of lithium-ion batteries.
Patent Information
- Application Number
- JP2023547096
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-03
- Filing Date
- 2022-02-01
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-02-01
AI Technical Summary
Lithium nitride (Li3N) is not practical for commercialization in lithium-ion batteries due to its high reactivity with moisture, air, and common electrode slurry solvents, leading to undesirable reactions and processing complications, which affect the electrochemical performance and stability of the battery.
A passivation coating is applied to Li3N particles to protect them from environmental reactions, ensuring a reproducible, thin, and uniform coating that maintains the electrochemical performance and stability of lithium-ion batteries.
The passivation coating stabilizes Li3N, enhancing its electrochemical performance by minimizing degradation and improving the energy density and processing flexibility of lithium-ion batteries.
Smart Images

Figure 0007955277000001 
Figure 0007955277000002 
Figure 0007955277000003
Abstract
Description
[Technical Field]
[0001] Cross-reference of related applications This application claims priority to U.S. Provisional Application No. 63 / 145,390, “PASSIVATED LITHIUM NITRIDE AS CATHODE PRE-LITHIATION REAGENT,” filed on 3 February 2021. The entire contents of the above application are incorporated herein by reference for all purposes.
[0002] This specification relates to a system and method for passivating lithium nitride (Li3N), particularly for use as a cathode pre-lithiumation reagent. [Background technology]
[0003] Lithium-ion batteries are widely used in a wide range of applications, including consumer electronics, uninterruptible power supplies, transportation, and fixed applications. A lithium-ion battery consists of a cathode containing a positive electrode or positive electrode active material (e.g., lithium insertion / deinsertion material) and a lithium-based negative electrode or anode. + Ions are passed through during battery charging, and then Li during battery discharge. + It functions by returning ions from the anode to the cathode. As a result of the charge-discharge process, a solid electrolyte interface (SEI) layer is formed on the anode during the initial charge cycle. The formation process of the SEI layer is particularly pronounced in silicon-based anodes. + Because it causes consumption, it can be detrimental to electrochemical performance. Thus, SEI formation can reduce the first-cycle Coulomb efficiency (FCE), potentially leading to reduced capacity and lower initial energy density in lithium-ion batteries.
[0004] To counteract the low FCE caused by anode SEI formation and the resulting capacity and initial energy density losses, a pre-lithiation approach is employed to add excess Li to the anode before or during the first charge / discharge. +ions can be supplied. Prelithiation can be achieved in many ways, such as by chemical treatment of the anode or incorporation of a sacrificial prelithiation reagent at the cathode. To expand on the latter case, an increased amount of Li during initial charging of a lithium-ion battery + one or more sacrificial lithium sources can be added to the cathode such that ions flow to the anode.
[0005] For example, lithium nitride (Li3N) can be included in the cathode as a sacrificial prelithiation reagent to improve the energy density of a lithium-ion battery. Li3N is desirable as a sacrificial prelithiation reagent over other options because of many different processing and electrochemical advantages. As a first example, Li3N has a particularly high theoretical capacity compared to other common sacrificial prelithiation reagents. Specifically, the following reaction corresponds to 2309 mAh g -1 theoretical capacity. 2Li3N→6Li + +3N2+6e - (1) Thus, compared to other common sacrificial prelithiation reagents, less Li3N can be used to provide Li during initial battery charging + equivalent release of ions can be obtained, thereby minimizing potential complications resulting from including a sacrificial prelithiation reagent in the electrode slurry (discussed in more detail below) used in forming a given electrode. can be suppressed.
[0006] As a second example, the use of a cathode catalyst can be eliminated due to decomposition of Li3N at practical cathode potentials. In the case of other common sacrificial prelithiation reagents, reaction kinetics and surface impurity layers can result in large overpotentials for uncatalyzed decomposition (the use of such options is not practical unless a cathode catalyst is included). On the other hand, Li3N is Li / Li + It has a low theoretical decomposition potential of ~0.44V relative to the cathode, and decomposition can proceed during battery charging without a cathode catalyst.
[0007] As a third example, the decomposition of Li3N produces an inert nitrogen gas (N2) byproduct (see reaction (1)), which can be readily removed during the formation of lithium-ion batteries. In contrast, some compounds may produce an oxygen gas (O2) byproduct, which may be involved in parasitic reactions with the electrode active material and / or electrolyte species. Therefore, compounds that produce such O2 may be undesirable as primary sacrificial prelithiation reagents due to electrochemical and safety drawbacks.
[0008] Despite these promising properties, pure (untreated) Li3N may not be practical for commercialization due to its high reactivity in moisture, air, and common electrode slurry solvents and components such as N-2-methylpyrrolidone (NMP) and polyvinylidene fluoride (PVDF). Incompatibility with air and PVDF, in particular, may be at least partially due to the trace amounts of moisture present. For example, Li3N readily reacts with water to form a basal environment within lithium-ion batteries. In the presence of PVDF, this basal environment can induce dehydrogenation and fluorination of the PVDF, leading to undesirable binder crosslinking and gelation (and thus a substantially unprocessable electrode slurry).
[0009] Therefore, to improve reactivity and protect and stabilize Li3N for use in lithium-ion battery environments, a passivation coating can be applied to untreated Li3N particles. However, the inventors hereby consider, for several reasons, that the passivation of Li3N is not obvious. For example, the design of the passivation coating process is carefully calibrated so as not to hinder the decomposition of Li3N before it is incorporated into a lithium-ion battery, thereby enabling maximum pre-lithiation during battery charging. In particular, uncontrolled environmental conditions can complicate reproducible passivation. For example, the passivation coating may preferably be thin and uniform. However, some passivation coating processes, such as surface transformation of Li3N particles in a moisture- or oxygen-covered atmosphere, can generate gases that hinder the formation of a controllable thin and uniform passivation coating (furthermore, high temperatures can promote such surface transformation, leading to undesirable excessive Li3N transformation).
[0010] The inventors identified the above problems and determined solutions to at least partially solve them. In one example, Li3N particles are passivated by precise control of chemical / physical interactions with one or more passivation precursors, resulting in the formation of a reproducible, thin, and uniform passivation coating on the surface of the Li3N particles. In several examples, the passivation coating can substantially completely cover the Li3N particles so that minimal Li3N is exposed to the surrounding processing environment. In this way, the Li3N particles are protected during battery manufacturing to provide maximum pre-lithiation of lithium-ion batteries containing the passivated Li3N particles, thereby improving the overall electrochemical performance of the lithium-ion batteries. Furthermore, the Li3N particles may be protected from reactions with other compounds present during electrode slurry formation (NMP, PVDF, etc.), potentially improving processing flexibility.
[0011] In some examples, the passivation coating may serve additional functions in lithium-ion batteries. For example, the passivation coating may include secondary sacrificial pre-lithiation reagents such as Li2O or Li2CO3, which may also decompose during initial battery charging. In this way, a cathode catalyst may optionally be provided to facilitate decomposition of the secondary sacrificial pre-lithiation reagent (however, as noted above, Li3N particles functioning as primary sacrificial pre-lithiation reagent may decompose without catalysis). As another example, a carbonaceous coating may enhance electronic conductivity during operation of the lithium-ion battery. As yet another example, certain passivation coating compositions, such as those based on polymeric ionic liquids (PILs) or ionomers, may improve Li + ionic conductivity by promoting transport. When included, PILs and ionomers may be further selected with hydrophobicity in mind to further protect Li3N from undesirable reactions with moisture. As yet another example, a metal or metal oxide may be included in the passivation coating to stabilize the cathode active material of the cathode and improve cycling performance of the lithium-ion battery.
[0012] In additional or alternative examples, the passivation coating may readily decompose during battery charging, enabling faster decomposition of Li3N, thereby enabling faster Li + ion release. Readily decomposition of the passivation coating may be provided, for example, by decomposition of the secondary sacrificial pre-lithiation reagent noted above. Where Li3N particles are coated with a miscible organic material, the passivation coating may dissolve upon immersion in the electrolytic environment. In this way, the passivation precursor may be selected to further enhance overall battery performance by protecting the Li3N particles during processing, providing additional electrochemical benefits, and / or promoting decomposition of Li3N to increase pre-lithiation rate during initial cycles of the lithium-ion battery.
[0013] In one example, the cathode prelithiation reagent can include core particles comprising Li₃N and a passivation coating uniformly disposed on at least a portion of a surface of the core particles. In this way, following processing and manufacturing of the lithium-ion battery, the uniformly passivated Li₃N core particles contained therein can decompose to provide maximum prelithiation and associated capacity increase during initial cycles of the lithium-ion battery.
[0014] It should be understood that the above summary is provided to introduce a selection of concepts in a simplified form that is further described below in the Detailed Description. It is not intended to identify key or essential features of the claimed subject matter, the scope of which is defined solely by the claims that follow the Detailed Description. Furthermore, the claimed subject matter is not limited to implementations that solve any disadvantages noted above or in any part of this disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] [Figure 1A] A schematic illustration of an example passivated lithium nitride (Li₃N) particle is shown. [Figure 1B] A schematic illustration of an example passivated lithium nitride (Li₃N) particle is shown. [Figure 1C] A schematic illustration of an example passivated lithium nitride (Li₃N) particle is shown. [Figure 1D] A schematic illustration of an example passivated lithium nitride (Li₃N) particle is shown. [Figure 2] A schematic illustration of an example decomposition process of a passivated Li₃N particle is shown. [Figure 3A] A schematic illustration of an example coated cathode structure is shown. [Figure 3B] A schematic illustration of an example coated cathode structure is shown. [Figure 4A] A schematic illustration of an example positive electrode active material particle coated with passivated Li₃N particles is shown. [Figure 4B]A schematic diagram of exemplary cathode active material particles coated with passivated Li3N particles is shown. [Figure 4C] A schematic diagram of exemplary cathode active material particles coated with passivated Li3N particles is shown. [Figure 5] A flowchart illustrating a method for forming a cathode containing passivated Li3N particles is shown. [Figure 6] A flowchart of a first exemplary method for passivating Li3N particles, including passivation of Li3N particles by reaction with a passivation atmosphere, is shown. [Figure 7] A flowchart of a second exemplary method for passivating Li3N particles, including passivation of Li3N particles by mechanical mixing, is shown. [Figure 8] A flowchart of a third exemplary method for passivating Li3N particles, including passivation of Li3N particles by wet coating and firing, is shown. [Figure 9] A flowchart of a fourth exemplary method for passivating Li3N particles, including passivation of Li3N particles by reactive sputtering, is shown. [Figure 10] A flowchart of a fifth exemplary method for passivating Li3N particles, including passivation of Li3N particles by wet coating and purification, is shown. [Figure 11] A flowchart of a sixth exemplary method for passivating Li3N particles is shown, including passivation of Li3N particles by wet coating and purification. [Figure 12] Figures 3A and 3B show an example of a lithium-ion battery pack formed from multiple lithium-ion battery cells in which the coated cathode structure can be implemented. [Modes for carrying out the invention]
[0016] The following description relates to a system and method for passivating lithium nitride (Li3N) for use as a cathode prelithiation reagent in lithium-ion batteries, for example, an example of which is shown in Figure 12. Specifically, as described herein with reference to Figures 1A to 1D, Li3N may be provided in the form of a powder, fine particles, or particles on which a uniform passivation coating is disposed. The uniform passivation coating can cover at least a portion (e.g., the majority or substantially all) of the surface of the Li3N particles. In this way, undesirable side reactions can be mitigated during the processing and manufacture of lithium-ion batteries containing passivation-coated Li3N particles, and degradation of Li3N can be prevented before the initial charge-discharge cycle of the lithium-ion battery.
[0017] As used herein, “uniform” when referring to a coating on a given surface of particles or other structures can be used to describe substantially similar densities of coatings within or on any threshold portion of a given surface (e.g., total surface area or less than total surface area). Furthermore, “substantially” can be used herein as a modifier meaning “effectively” or “practically.” Thus, as used herein, “substantially complete” or “substantially all” when referring to surface coverage can, for practical considerations, refer to overall and complete surface coverage. For example, given Li3N particles can be considered substantially completely covered by a uniform passivation coating, even if relatively small gaps remain in the uniform passivation coating, if such relatively small gaps negligibly reduce the electrochemical performance.
[0018] As shown in Figure 2, during the initial charge and discharge of a lithium-ion battery, Li3N particles are Li +It can be decomposed into ions and nitrogen gas (N2). Since N2 is inert, it can be easily removed from lithium-ion batteries by degassing (e.g., by compression rolling of the pouch cell). In some examples, a uniform passivation coating can be added to the lithium-ion battery. + It can be decomposed into ions and additional gases and / or inert residues. In other examples, a uniform passivation coating can be dissolved in the electrolyte of a lithium-ion battery with little or no effect on the electrochemical performance after dissolution. In other examples, a uniform passivation coating can be retained in the cathode of a lithium-ion battery, where it can provide secondary electrochemical advantages.
[0019] In some examples, a cathode pre-lithification reagent (e.g., Li3N particles with a uniform passivation coating on top) can be incorporated into the cathode slurry along with cathode active material particles. The cathode slurry can be cast, dried, and calendered onto a cathode structure (e.g., a current collector with an optionally placed coating layer on top) to form a layered cathode structure. In other examples, the cathode active material and cathode pre-lithification reagent can be incorporated into the cathode as a discontinuous slurry base layer. Exemplary layered cathode structures are shown in Figures 3A and 3B.
[0020] In some examples, as also shown in Figures 4A and 4B, the cathode active material particles may be coated with uniformly passivated Li3N particles, in some cases in addition to or containing carbonaceous conductive and / or binder additives. In other examples, as also shown in Figure 4C, the cathode active material particles may be coated with pure (unpassivated) Li3N particles. The Li3N-coated cathode active material particles may then be coated with a uniform passivation coating. In this way, a uniform distribution of the cathode pre-lithification reagent (e.g., Li3N particles) in the cathode active material particle coating is promoted, thereby minimizing the effects of the addition and decomposition of the cathode pre-lithification reagent on the mechanical and electrochemical integrity of the cathode active material particle coating.
[0021] The method shown in Figure 5 details the preparation of a uniform passivation coating on Li3N particles or Li3N-coated cathode active material particles, followed by the formation of a cathode containing such uniformly passivated particles. Passivation can be achieved by specific passivation coating processes, such as one of the exemplary methods shown in Figures 6–11, the steps of which can be selected and adjusted according to the desired passivation coating composition.
[0022] Referring next to Figure 1A, a schematic cross-sectional view is shown illustrating pre-lithiumization reagent particles 100, such as the cathode of a lithium-ion battery. The pre-lithiumization reagent particles 100 can be passivated, including core particles 102 surrounded by a passivation coating 104. As shown, the core particles 102 may consist substantially entirely of Li3N. For example, the pre-lithiumization reagent particles 100 may be prepared by passivating pure chemical-grade Li3N particles such that the core particles 102 consist of Li3N and trace impurities, or are substantially impurity-free.
[0023] Prelithiation reagents, such as prelithiation reagent particles 100, decompose at least partially during the initial charge-discharge cycles of lithium-ion batteries, adding Li + By supplying (sacrificing) ions, the energy density of lithium-ion batteries can be improved. In this respect, it has desirable advantages (low theoretical resolution, high theoretical capacity, etc.), but Li3N is not practical for large-scale implementations due to its high reactivity.
[0024] To improve the stability and practicality of Li3N as a pre-lithiumization reagent, a passivation coating, such as passivation coating 104, can be placed on the surface of Li3N core particles, such as core particle 102, as a blocking interface to improve the stability of Li3N and reduce the degradation rate of Li3N before charge-discharge cycles. In addition to protecting and passivating the Li3N core particles, the passivation coating improves one or more of the following: electronic conductivity, ionic conductivity, cycle performance, and the stability of the electrode active material, and / or additional Li + It can also perform other functions in lithium-ion batteries, such as supplying ions.
[0025] As an example, the passivation coating 104 may contain one or more of the following: lithium peroxide (Li2O2), lithium oxide or lithia (Li2O), lithium carbonate (Li2CO3), lithium sulfide (Li2S), and lithium fluoride (LiF). When included in the passivation coating 104, Li2O2, Li2O, Li2CO3, Li2S, and / or LiF may provide additional Li during the initial charging cycle of a lithium-ion battery containing pre-lithification reagent particles 100. + It can function as a secondary pre-lithiation reagent that provides ions (Li3N is the primary pre-lithiation reagent).
[0026] In some cases, such as when the secondary prelithiation reagent (Li2O2, Li2O, Li2CO3, Li2S, and / or LiF) is included in the passivation coating 104, a cathode catalyst may be further included in the passivation coating 104. The cathode catalyst may include any material that catalyzes the decomposition of the secondary prelithiation reagent during the prelithiation of the lithium-ion battery. However, it will be understood that the primary prelithiation reagent Li3N can be decomposed without catalytic action by the cathode catalyst due to its low theoretical decomposition capacity. Therefore, in some cases (such as when the secondary prelithiation reagent is not included in the passivation coating 104), the cathode catalyst may be absent or added, for example, before the initial cycle. In other cases (such as when the passivation coating 104 has a relatively thin thickness 106), the secondary prelithiation reagent may be included in the passivation coating 104 and may decompose without a cathode catalyst.
[0027] The cathode catalyst may include a material that is not consumed during the initial charging cycle and does not completely decompose during the life of the lithium-ion battery (at least some residual cathode catalyst remains in the lithium-ion battery). In some examples, the cathode catalyst may include a lithium-based active cathode catalyst, which may be any lithium compound that reversibly releases and accepts lithium ions during the charging cycle and catalyzes the decomposition of the secondary prelithiation reagent. For example, the cathode catalyst may include one or more metallic lithium phosphates, such as lithium iron phosphate (LFP) and / or manganese iron lithium phosphate (LMFP). In some examples, the cathode catalyst may include a transition metal-based compound having partially arranged d and / or f orbitals, which can induce electronic transitions and lower the activation energy for the decomposition of the secondary prelithiation reagent. For example, the cathode catalyst may be a transition metal oxide such as cobalt tetroxide (Co3O4).
[0028] As another example, the passivation coating 104 may contain carbonaceous conductive additives. For example, the passivation coating 104 may contain one or more of carbon black, graphene, graphene oxide, and carbon nanotubes (CNTs). In addition to passivation and protection, carbonaceous conductive additives can also increase electronic conductivity and reduce the total amount of carbon used in preparing the electrode slurry for forming the electrodes of lithium-ion batteries.
[0029] As another example, the passivation coating 104 may include one or more organic materials, such as one or more waxes, one or more long-chain conductive polymers, and / or one or more small organic molecules. For example, the one or more organic materials may include one or more of natural waxes, paraffin waxes, polyethylene (PE), polypropylene (PP), polystyrene (PS), oleic acid, stearic acid, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), poly(ethylene) oxide (PEO), poly(methyl methacrylate) (PMMA), poly(methyl acrylate) (PMA), etc. The one or more organic materials may be selected based on their solubility in the electrolytic environment of the lithium-ion battery. Specifically, when the passivation coating 104 containing one or more organic materials is exposed to the electrolyte, each of the one or more organic materials dissolves in the electrolyte and is exposed in such a way that the core particles 102 decompose more rapidly and efficiently. For example, the one or more organic materials that dissolve in the electrolyte may include one or more of PEO, PMMA, PMA, etc. Furthermore, since one or more organic materials can be selected to be substantially electrochemically inert, the electrochemical properties of one or more organic materials are not substantially impaired after they are dissolved in the electrolyte.
[0030] As another example, the passivation coating 104 may contain one or more polymer ionic liquids (PILs) and / or one or more polymer salts such as ionomers. Options for PILs that may be included in the passivation coating 104 include, for example, hexafluorophosphate (PF6). -) or tetrafluoroboric acid (BF4 - ) combined with Imadazolium (C3H5N2 + ) may include. Furthermore, ammonium (NH4 + ), phosphonium (e.g., H4P + ), pyridinium (HC5H5N + ) and sulfonium (e.g., H3S + )One or more cations, such as cations, can be reacted with an alkyl brominated chain to generate oligomeric cations that can undergo additional polymerization reactions (provided that one of the parts extending from the primary ionic molecular center of the given oligomeric cation contains a terminal alkene group). The additional anion pair is a chloride (Cl - ), bromide (Br - ), iodide (I - ), nitrates (NO3 - ), methyl sulfate (CH3O4S - ), bis(trifluoromethanesulfonyl)imide (C2F6NO4S2 - ), trifluoromethanesulfonate (CF3O3S - ), dicyanamide (C2N3 - ), dimethyl phosphate (C2H6O4P - ), acetate (C2H3O2 - ), tosylate (H3CC6H4SO3 - ), including one or more alkylsulfates, the choice of which depends on the voltage range of the resulting PIL stability.
[0031] PILs are a subclass of ionic liquids, anion / cation pairs that exist in a liquid state at room temperature and possess relatively high ionic conductivity. Therefore, ionic liquids can facilitate lithium transport in lithium-ion batteries, thereby improving their electrochemical performance. Furthermore, ionic liquids may have relatively low toxicity, solubilize other compounds, and exhibit high thermal and electrochemical stability.
[0032] Either the anion or cation of a given PIL anion / cation pair can undergo polymerization by chemical, photochemical, or thermal initiation, resulting in the growth of a polymer backbone where each monomer unit holds an ionic charge together with its associated counterion. Thus, PIL can be applied in liquid form to the surface of Li3N particles (such as core particle 102), and in-situ polymerization can produce a robust and highly ionically conductive polymer matrix.
[0033] The virtually infinite combinations of anion and cation identity when selecting the PIL composition allow for the adjustment of one or more of the following processing and electrochemical performance parameters. • Electrochemical stability of the anode and / or cathode. • Viscosity and temperature response of PIL in its liquid state. • Compatibility of ion species within lithium-ion batteries. • Selection of solvent-based or solvent-free applications. • Formation of composites with polymer matrices and other materials. • Selection of parts that fulfill the desired purpose and provide the desired characteristics. • Hydrophobic / hydrophilic (due to ion exchange). • pH control during electrode slurry formation. • Selection of polymerization before and after coating, either on the substrate surface (such as the surface of core particles 102) or within the electrode formed as a binder. • Formation of porous or non-porous networks.
[0034] To prepare the PIL for slurry processing, water removal and purification can be performed by batch hydrolysis or liquid-liquid extraction. A given PIL for inclusion in the passivation coating 104 can be further selected for its high hydrophobicity (which can mitigate aqueous degradation of core particles 102 by inducing resistance to water uptake) and ease of application as a uniform, continuous coating. As used herein, "continuous," when referring to a layer or coating on a substrate (such as particles), can mean that a given coated surface area of the substrate is completely or substantially completely coated with a continuous film. Furthermore, by selecting the PIL to respond to changes in the pH of the electrode slurry, gelation of the electrode slurry can be reduced in some examples. Additionally, by controlling the viscosity of the PIL, water uptake can be prevented even during slurry processing.
[0035] Ionomers are ionically charged polymers that may possess at least some properties similar to PILs, such as good ionic conductivity (depending on the degree of protonation). For example, solvents can be used for desolvation and solution treatment to apply ionomers to the surface of a substrate (e.g., the surface of core particles 102). One example of an ionomer that may be included in lithium-ion batteries is Nafion®. However, cost considerations may limit the large-scale implementation of currently available ionomers.
[0036] As another example, the passivation coating 104 may contain one or more non-lithium metals or metal oxides. For example, the passivation coating 104 may contain one or more of Al, Fe, Cu, W, V, Ti, Ni, Zn, Cd, Ag, Co and their oxides. The non-lithium metals or metal oxides can stabilize the electrode active material in the electrode slurry (such as lithium nickel manganese cobalt oxide or NMC, as described in detail with reference to Figures 4A to 4C) and improve the cycling performance of the electrode formed from the electrode slurry.
[0037] The passivation coating 104 is not limited to the compositions described above. Specifically, other options or types of compounds can be included in the passivation coating 104, either independently or in combination with the compositions described above.
[0038] The size of the pre-lithiumation reagent particles 100 and the thickness 106 of the passivation coating 104 may be selected to provide improved electrochemical performance through maximum pre-lithiumation while maintaining protection of the core particles 102 during slurry processing. In some examples, the relationship between multiple pre-lithiumation reagent particles 100 may be formed such that each pre-lithiumation reagent particle 100 has a similar size to one another. For example, multiple pre-lithiumation reagent particles 100 for inclusion in an electrode slurry may be ground to produce a pre-selected particle size distribution (PSD) with a peak below 150 nm. In some examples, the PSD may be a single or bimodal PSD.
[0039] In some examples, the average size (e.g., D50 size) of multiple pre-lithiumated reagent particles 100 may be 150 nm or less. In additional or alternative examples, any given pre-lithiumated reagent particle 100 may have a maximum cross-sectional dimension of 500 nm or less.
[0040] In some examples, the thickness 106 of the passivation coating 104 can be controlled during the passivation of the core particles 102 such that the passivation coating 104 is not so thick as to significantly inhibit the rate of pre-lithiation, nor so thin as to passivate the core particles 102 during slurry processing. Therefore, the thickness 106 of the passivation coating 104 may be, for example, 20 nm or less. In additional or alternative examples, the thickness 106 of the passivation coating 104 may be 10 nm or more. In one example, the thickness 106 of the passivation coating 104 may be in the range of 1 nm to 50 nm.
[0041] In one example, as shown in Figure 1A, the passivation coating 104 can uniformly, continuously, and completely cover the surface of the core particle 102. Specifically, the passivation coating 104 may be uniformly distributed over nearly 100% of the surface of the core particle 102, forming a continuous layer thereon. However, in other examples, the passivation coating 104 may be distributed over only a portion of the surface of the core particle 102 (e.g., less than 100%).
[0042] An example of such a partial passivation coating is shown in Figure 1B. Referring to Figure 1B, a schematic cross-sectional view is shown showing pre-lithification reagent particles 125 for use in the cathode of a lithium-ion battery, etc. Similar to the pre-lithification reagent particles 100 in Figure 1A, the pre-lithification reagent particles 125 may include core particles 102 on which a passivation coating 126 is placed, and the core particles 102 may be substantially composed entirely of Li3N. Further configurations and embodiments of the core particles 102 can be as described above with reference to Figure 1A. Furthermore, as described above with reference to Figure 1A, it will be understood that the composition of the passivation coating 126 may be similar to or the same as the composition of the passivation coating 104, etc.
[0043] As shown in Figure 1B, the passivation coating 126 may include one or more gaps 128. One or more gaps 128 may expose at least a portion of the surface of the core particles 102 to the surrounding environment. However, it will be understood that the passivation coating 126 may still be able to cover a large portion (at least 50%) of the surface of the core particles 102. Furthermore, it will be understood that one or more gaps 128 may not collectively expose enough of the surface of the core particles 102 to cause significant degradation of the core particles 102, for example, sufficient degradation that adversely affects their electrochemical performance, before they are incorporated into a lithium-ion battery.
[0044] As further shown in Figure 1B, the passivation coating 126 may include one or more low-coating regions 130 having a thickness less than the (maximum) thickness 132 of the passivation coating 126. In some examples, the thickness 132 of the passivation coating 126 may be 20 nm or less. In additional or alternative examples, the thickness 132 of the passivation coating 126 may be 10 nm or more. In one example, the thickness 132 of the passivation coating 126 may be in the range of 1 nm to 50 nm. It will be understood that the one or more low-coating regions 130 may be limited to relatively small portions of the surface of the core particles 102, and that the passivation coating 126 may uniformly coat most of the surface of the core particles 102 (at least 50%) with a thickness of 132, as the thickness 132 of the passivation coating 126 can be controlled during passivation so that it does not become so thin that the core particles 102 are not adequately passivated during slurry processing. Furthermore, it will be understood that one or more low-coating regions 130 on the core particles, where the coating area is relatively small, do not result in significantly large degradation of the core particles 102 before they are incorporated into the lithium-ion battery.
[0045] The coating area of a continuous passivation coating on the core particles 102 is shown in Figures 1A and 1B, but in other examples, the passivation coating may be a discontinuous coating. As used herein, “discontinuous” when referring to a coating or layer on a substrate (such as particles) may mean that a given coated surface area of a substrate having a discontinuous layer of particles is completely or substantially completely coated (e.g., more than 50%).
[0046] An example of such a discontinuous passivation coating is shown in Figure 1C. Referring to Figure 1C, a schematic cross-sectional view is shown illustrating pre-lithification reagent particles 150 for applications such as the cathode of a lithium-ion battery. Similar to the pre-lithification reagent particles 100 and 125 in Figures 1A and 1B, respectively, the pre-lithification reagent particles 150 include core particles 102 with a uniformly distributed passivation coating 152, the core particles 102 may be substantially composed entirely of Li3N. Further configurations and configurations of the core particles 102 can be as described above with reference to Figure 1A. Furthermore, as described above with reference to Figure 1A, it will be understood that the composition of multiple passivation particles 154 may be similar to or the same as the composition of the passivation coating 104. For example, multiple passivation particles 154 may consist of one or more of a secondary pre-lithification reagent, a carbonaceous conductive additive, a non-lithium metal, or a metal oxide.
[0047] As shown in Figure 1C, the passivation coating 152 may be a discontinuous coating composed of multiple passivation particles 154. In some examples, the multiple passivation particles 154 may coat the core particle 102 at such a high density that the passivation coating 152 is considered to completely and uniformly cover the surface of the core particle 102. Further configurations of the core particle 102 are described in detail above with reference to Figure 1A.
[0048] The passivation coating 152 may have a maximum range 156. Therefore, each of the multiple passivation particles 154 may be positioned between the surface of the core particle 102 and the maximum range 156 of the passivation coating 152. The maximum range 156 may also be defined by the thickness 158 of the passivation coating 152, which may correspond to the maximum particle size of the multiple passivation particles 154. In some examples, the multiple passivation particles 154 may have a narrow, conventional PSD such that each of the multiple passivation particles 154 is approximately the same size. In one example, the maximum particle size of the multiple passivation particles 154 and the thickness 158 of the passivation coating 152 may each be 50 nm or less.
[0049] In some examples, the surface of the core particle 102 may include one or more surface structures 160. For example, one or more surface structures 160 may be openings or cracks within the surface of the core particle 102, and their size and / or depth may vary. Specifically, in some examples, one or more surface structures 160 may be irregular (e.g., having different shapes and sizes). One or more surface structures 160 can, of course, increase the surface area of the core particle 102.
[0050] Multiple passivation particles 154 can be retained in place by van der Waals molecular, mechanical, and / or other physical attractive forces, in direct contact with each other and with both the core particle 102. Specifically, in some examples, at least some of the multiple passivation particles 154 can adhere to and / or into one or more surface structures 160 by van der Waals molecular, mechanical, and / or other physical attractive forces. Thus, the size of the multiple passivation particles 154 may be complementary to the size of the mutual surface structures 160 so that the multiple passivation particles 154 can be at least partially fixed therein. In some examples, the multiple passivation particles 154 may be ground to a pre-selected average size (e.g., corresponding to a narrow, ordinary PSD). The pre-selected average size of the multiple passivation particles 154 allows for their retention on and in part on surface structures 160 of complementary sizes on the surface of the core particle 102.
[0051] Figures 1A to 1C show single-layer passivation coating configurations, but in other examples, multi-layer passivation coating configurations can be applied to the surface of the core particles 102. Therefore, the total number and thickness of the passivation coating layers depend on the balance between protecting the core particles 102 and effectively pre-lithifying the lithium-ion battery (as described above), as well as other practical considerations such as interlayer adhesion, total cost, and relative processing difficulty.
[0052] An example of such a multilayer passivation coating configuration is shown in Figure 1D. Referring to Figure 1D, a schematic cross-sectional view is shown showing pre-lithiumization reagent particles 175 for applications such as the cathode of a lithium-ion battery. Similar to the pre-lithiumization reagent particles 100, 125, and 150 in Figures 1A to 1C, the pre-lithiumization reagent particles 175 may include core particles 102 in which at least one passivation coating is uniformly arranged, and the core particles 102 may be substantially composed entirely of Li3N. Further configurations and embodiments of the core particles 102 may be as described above with reference to Figure 1A. Furthermore, the composition of each passivation coating of the at least one passivation coating may be similar to or the same as the composition and structure of the (continuous) passivation coating 104, as described above with reference to Figure 1A. Alternatively, the composition of each passivation coating of the at least one passivation coating may be similar to or the same as the composition and structure of the (discontinuous) passivation coating 152, as described above with reference to Figure 1C.
[0053] As shown in Figure 1D, the pre-lithiumized reagent particles 175 may include core particles 102 surrounded by a first passivation coating 176. In one example, the first passivation coating 176 can uniformly, continuously, and completely cover the surface of the core particles 102. Specifically, the first passivation coating 176 can be uniformly distributed over substantially 100% of the surface of the core particles 102, and as a result, the first passivation coating 176 can be formed as a continuous layer thereon. However, in other examples, the first passivation coating 176 can be distributed over less than 100% of the surface of the core particles 102. Furthermore, during the passivation of the core particles 102, the thickness 180 of the first passivation coating 176 can be controlled to, for example, 20 nm or less.
[0054] In some examples, the first passivation coating 176 may be a discontinuous coating consisting of multiple passivation particles (not shown in Figure 1D). In such examples, the multiple passivation particles can coat the core particle 102 at such a high density that the first passivation coating 176 is considered to completely and uniformly cover the surface of the core particle 102.
[0055] As further shown in Figure 1D, the first passivation coating 176 can be surrounded by a second passivation coating 178. In one example, the second passivation coating 178 can uniformly, continuously, and completely cover the first passivation coating 176. Specifically, the second passivation coating 178 can be uniformly placed on substantially 100% of the first passivation coating 176 so that the second passivation coating 178 forms a continuous layer thereon. However, in other examples, the second passivation coating 178 can be placed on less than 100% of the first passivation coating 176. Furthermore, the thickness 182 of the second passivation coating 178 can be controlled, for example, to less than 20 nm during the coating of the first passivation coating 176.
[0056] In some examples, the second passivation coating 178 may be a discontinuous coating consisting of multiple passivation particles (not shown in Figure 1D). In such examples, the multiple passivation particles can coat the first passivation coating 176 at such a high density that the second passivation coating 178 is considered to completely and uniformly cover the first passivation coating 176.
[0057] In some examples, a second passivation coating 178 may be provided to ensure that 100% of the surface of the core particles 102 is uniformly coated to a desired thickness. For example, the thickness 180 of one or more areas of the first passivation coating 176 may be less than desired, or there may be one or more gaps in the first passivation coating 176. Thus, the second passivation coating 178 may be coated on core particles 102 previously coated with the first passivation coating 176 to provide a uniform, complete, and continuous coating of the core particles 102.
[0058] In some examples, the second passivation coating 178 may have a different composition from the first passivation coating 176. For example, the composition of the second passivation coating 178 may be selected to dissolve / decompose in the electrolyte during the initial cycle of the lithium-ion battery, while the first passivation coating 176 may be selected to be retained on the cathode.
[0059] In some examples, the first passivation coating 176 may be a discontinuous coating consisting of multiple passivation particles, and the second passivation coating 178 may be a uniform continuous layer completely surrounding the (discontinuous) first passivation coating 176. In other examples, the first passivation coating 176 may be a uniform continuous layer completely surrounding the core particle 102, and the second passivation coating 178 may be a discontinuous coating consisting of multiple passivation particles. In other examples, each of the first and second passivation coatings 176, 178 may be a discontinuous coating consisting of multiple passivation particles. In other examples, the first passivation coating 176 may be a uniform continuous layer completely surrounding the core particle 102, and the second passivation coating 178 may be a uniform continuous layer completely surrounding the first passivation coating 176.
[0060] Referring next to Figure 2, a schematic diagram illustrating an exemplary prelithiation process 200 in a lithium-ion battery is shown. The prelithiation reagent particles 100 in Figure 1A are shown as a sacrificial lithium source for the prelithiation process 200, but in another embodiment, any of the prelithiation reagent particles 125, 150, and 175 in Figures 1B to 1D can be substituted, respectively. As described above with reference to Figure 1A, the prelithiation reagent particles 100 may include core particles 102 surrounded by a passivation coating 104, core particles 102 composed of a primary prelithiation reagent (Li3N) and a passivation coating 104 composed of a secondary prelithiation reagent, a cathode catalyst (which in some examples catalyzes the decomposition of the secondary prelithiation reagent), carbonaceous conductive additives, organic materials, polymer salts, non-lithium metals (or metal oxides), or combinations thereof.
[0061] The core particles 102 and optionally the passivation coating 104 can be decomposed by decomposition 225, generating at least two decomposition products. These at least two decomposition products may originate from the core particles 102 alone or from both the core particles 102 and the passivation coating 104. Therefore, the at least two decomposition products may include (sacrificial) Li + It can contain ion 256.
[0062] More specifically, after decomposition 225, pre-lithiumated reagent particles 250 may remain. In one example, the pre-lithiumated reagent particles contain at least Li + It may include at least partially depleted core particles 252 surrounded by a passivation coating 254 (which may or may not be at least partially depleted as a result of decomposition 225) that emits ions 256 and N2 gas 258. +Ions 256 and N2 gas 258 may be decomposition products of the core particle 102. Since the core particle 102 can be designed to decompose substantially completely (depending on the battery environment, the thickness of the passivation coating, etc.), the decomposition 225 can be considered partial decomposition (e.g., midway through the initial cycle of a lithium-ion battery), and the pre-lithiumized reagent particles 250 may be products of partial decomposition.
[0063] Li + Ion 256 and N2 gas 258 may be decomposition products of core particle 102. However, in some cases, such as when the passivation coating 104 contains a secondary pre-lithification reagent, Li + At least some of the ions 256 may originate from the decomposition of the passivation coating 104. In such cases, the decomposition of the passivation coating 104 further produces additional gaseous residue 260. For example, if the passivation coating 104 contains Li2O2 as a secondary pre-lithification reagent, the decomposition of the passivation coating 104 will result in Li + This process generates at least some of the ions 256 and additional gaseous residue 260, the additional gaseous residue 260 being O2 gas. Both the N2 gas 258 and the additional gaseous residue 260 can be removed from the lithium-ion battery by a degassing step (for example, if the lithium-ion battery is formed in a pouch cell configuration, degassing can be achieved by compression rolling).
[0064] In additional or alternative examples, such as when the passivation coating 104 contains a cathode catalyst or organic material, a non-gaseous residue 262 can be generated. In such examples, the non-gaseous residue 262 can be dissolved in the electrolyte of the lithium-ion battery without substantially affecting the electrochemical performance.
[0065] In additional or alternative examples, such as when the passivation coating 104 contains carbonaceous conductive additives, polymer salts, or non-lithium metals, at least a portion of the passivation coating 104 may remain even after complete decomposition. In such examples, the composition of the passivation coating 104 can be selected to improve or substantially avoid affecting the electrochemical performance. In examples where the passivation coating 104 contains only non-residue-forming components, substantially all of the passivation coating 104 may remain after decomposition 225 (e.g., as passivation coating 254).
[0066] After the complete decomposition of the pre-lithiumation reagent particles 100, voids may remain in the electrode containing the pre-lithiumation reagent particles 100 (e.g., the coated cathode structure 300 in Figures 3A-3B) (i.e., where the pre-lithiumation reagent particles 100 were located before decomposition). In cases where the passivation coating 104 was not completely decomposed during the pre-lithiumation process 200, the voids may be surrounded by at least a portion of the passivation coating 104 (e.g., passivation coating 254). Thus, the passivation coating 104 is semipermeable, and Li + This allows ions 256 and N2 gas 258 to pass through the core particles 102 in a well-dispersed state during decomposition.
[0067] In some examples, the pre-lithiumization reagent particles 100 are included in the cathode of a lithium-ion battery, for example, in the slurry coating layer of the cathode (for example, a layered configuration which will be described in detail below with reference to Figures 3A and 3B). Thus, during the pre-lithiumization process 200, Li + Ions pass through the passivation coating 104, allowing the anode of the lithium-ion battery to be pre-lithified from the cathode.
[0068] Referring next to Figure 3A, a schematic cross-sectional view is shown illustrating an exemplary coated cathode structure 300 for use in a lithium-ion battery. During formation, the coated cathode structure 300 can be placed within a lithium-ion battery so that it can supply power to the lithium-ion battery. In some examples, the lithium-ion battery is one of several lithium-ion battery cells in a lithium-ion battery pack, and each of the several lithium-ion battery cells may have substantially similar configurations to one another.
[0069] The coated cathode structure 300 includes a current collector 302 having a first side 310 and a second side 312, the sides 310 and 312 facing each other. The current collector 302 may have a coating layer 304 disposed on one or both of the sides 310 and 312, the coating layer 304 in surface-sharing contact with the current collector 302. Thus, sequentially along an axis 308 parallel to the minimum dimension of the current collector 302, the coated cathode structure 300 may include a coating layer 304, a current collector 302, and a coating layer 304 (i.e., the current collector 302 may be interposed between two coating layers 304 of a similar configuration).
[0070] The current collector 302 may be a metal sheet or foil such as Cu foil, Ni foil, or Al foil, or any other configuration that conducts electricity and allows current to flow. In one example, the thickness of the current collector 302 may be approximately 10 μm. However, it will be understood that the thickness of the current collector 302 may vary significantly, for example, up to 500 μm. In this specification, "approximately" when referring to numerical values may include deviations of 5% or less.
[0071] In some examples, the coating layer 304 may be a slurry-based layer comprising a binder, a cathode active material, a passivation prelithiation reagent, and optionally a conductive additive. In some examples, the passivation prelithiation reagent may include Li3N particles (as the primary prelithiation reagent) coated with a passivation coating comprising a secondary prelithiation reagent, a carbonaceous material, an organic material, a polymer salt, a non-lithium metal (or metal oxide), or a combination thereof.
[0072] In some examples, the binder may contain one or more polymers. For example, the binder may contain one or more conductive polymers such as polyvinylidene fluoride (PVDF), polyvinylpyrrolidone (PVP), PEO or cross-linked PEO, polytetrafluoroethylene (PTFE), PMMA, poly(acrylic acid) (PAA), PVDF-HFP, poly(3,4-ethylenedioxythiophene) (PEDOT), PEDOT polystyrene sulfonate (PEDOT:PSS), cellulose derivatives, and linear, semi-aromatic, or aromatic polyimides (PI). In examples where the binder contains PVDF, Li3N may be used in the passivation pre-lithiating reagent since it can be passivated by a passivation coating (although Li3N may be substantially incompatible with PVDF).
[0073] In some examples, the conductive additive may be carbonaceous. For example, the conductive additive may include carbon black, graphene, graphene oxide, and / or CNTs. In examples where the passivation coating also includes carbonaceous material, the conductive additive may have the same or a different composition as the carbonaceous material in the passivation coating. Furthermore, in such examples, the amount of conductive additive in the coating layer 304 may be reduced or removed due to the presence of carbonaceous material in the passivation coating (similar purposes can be achieved in lithium-ion batteries).
[0074] In some examples, the cathode active material may include lithium-inserted materials. For example, the lithium-inserted material may include one or more of lithium nickel-cobalt-manganese oxide (NCM or NMC), lithium iron phosphate (LFP), lithium iron manganese phosphate (LMFP), lithium nickel-cobalt-aluminum oxide (NCA), lithium cobalt oxide (NCO), lithium manganese-nickel oxide (LMN), lithium manganese oxide (LMO), lithium cobalt-lithium phosphate (LCP), lithium nickel-phosphate (LNP), and lithium manganese phosphate (LMP), and / or any number of other lithium-inserted materials known to those skilled in the art. In one example, the cathode active material may be a layered structure material of a lithium mixed metal oxide. In some examples, as will be described in detail below with reference to Figures 4A and 4B, the cathode active material is particulate and coated with passivated Li3N particles, so that discontinuous pre-lithification reagents are not used. In other examples, as will be described in detail below with reference to Figure 4C, the cathode active material is particulate and coated with pure (unpassivated) Li3N particles, and a passivation coating may be further applied on top of the Li3N-coated cathode active material.
[0075] After the coating layer 304 is coated and calendered, its thickness along the axis 308 can be determined. In some examples, the thickness of the coating layer 304 may be 50 μm or more and 500 μm or less.
[0076] In some cases, to minimize the effect of adding the prelithiation reagent on the mechanical and electrochemical integrity of the coated cathode structure, the prelithiation reagent can be included in a separate coating layer from the cathode active material. For example, the cathode active material can be included in a layer close to the current collector, and the prelithiation reagent in a layer farther away from the current collector. In another example, the prelithiation reagent can be included in a layer close to the current collector, and the cathode active material in a layer farther away from the current collector.
[0077] An example of such a multilayer cathode structure is shown in Figure 3B. Referring to Figure 3B, a schematic cross-sectional view is shown of an exemplary coated cathode structure 350 for use in a lithium-ion battery. During formation, the coated cathode structure 350 can be placed inside a lithium-ion battery so that it can supply power to the lithium-ion battery. In some examples, the lithium-ion battery is one of several lithium-ion battery cells in a lithium-ion battery pack, and each of the several lithium-ion battery cells may have substantially similar configurations to one another.
[0078] The coated cathode structure 350 includes a current collector 302 (as described in detail above with reference to Figure 3A) having a first side 310 and a second side 312, the sides 310 and 312 facing each other. The current collector 302 has a first coating layer 352 disposed on one or both of the sides 310 and 312, the first coating layer 352 in surface-sharing contact with the current collector 302. Furthermore, a second coating layer 354 is disposed on one or both of the sides 310 and 312, on the first coating layer 352, the second coating layer 354 in surface-sharing contact with the first coating layer 352, and the first coating layer 352 is interposed between the current collector 302 and the second coating layer 354. Therefore, the coated cathode structure 350 sequentially along an axis 358 parallel to the minimum dimension of the current collector 302 may include a second coating layer 354, a first coating layer 352, the current collector 302, the first coating layer 352, and the second coating layer 354.
[0079] In the first embodiment, the first coating layer 352 may be a slurry layer comprising a binder, a cathode active material, and optionally a conductive additive, and the second coating layer 354 may be a slurry layer comprising a binder, a passivation pre-lithiation reagent, and optionally a conductive additive. In the second embodiment, the first coating layer 352 may be a slurry base layer comprising a binder, a passivation pre-lithiation reagent, and optionally a conductive additive, and the second coating layer 354 may be a slurry base layer comprising a binder, a cathode active material, and optionally a conductive additive. In the first and second embodiments, the cathode active material and the passivation pre-lithiation reagent do not have to be included in the same coating layer 352 or 354. Therefore, one of the coating layers 352, 354 may provide lithium insertion / de-insertion functionality, and the other of the coating layers 352, 354 may provide pre-lithiation functionality.
[0080] In the third example, the first coating layer 352 may be a slurry base layer comprising a binder, a cathode active material, a passivated pre-lithiumization reagent, and optionally a conductive additive, and the second coating layer 354 may be a slurry base layer comprising a binder, a cathode active material, and optionally a conductive additive. Thus, the passivated pre-lithiumization reagent and the cathode active material are mounted on the same coating layer.
[0081] In the fourth embodiment, the first coating layer 352 may be a slurry base layer comprising a binder, a cathode active material, and optionally a conductive additive, and the second coating layer 354 may be a slurry base layer comprising a binder, a cathode active material, a passivated pre-lithification reagent, and optionally a conductive additive. Thus, both coating layers contain a cathode active material, but only one of the coating layers contains a pre-lithification reagent.
[0082] In the fifth example, both the first coating layer 352 and the second coating layer 354 may be slurry-based layers comprising a binder, a cathode active material, a passivated prelithiation reagent, and optionally a conductive additive. Each coating layer contains the same material, but the relative amounts of the binder, cathode active material, passivated prelithiation reagent, and optionally a conductive additive may vary between the first coating layer 352 and the second coating layer 354. For example, the first coating layer 352 may have a weight percentage of cathode active material higher than the weight percentage of passivated prelithiation reagent, and the second coating layer 354 may have a weight percentage of cathode active material higher than the weight percentage of passivated prelithiation reagent.
[0083] The compositions of the binder, cathode active material, conductive additive, and passivated prelithiation reagent can be as described above with reference to Figure 3A. For example, as described above with reference to Figure 3A, the amount of conductive additive can be reduced or removed if the passivation coating of the passivated prelithiation reagent contains a carbonaceous material that performs a similar function.
[0084] After the coating layers 352 and 354 are coated and calendered, their thickness along the axis 358 can be determined. In some examples, the thickness of each of the coating layers 352 and 354 may be between 50 μm and 500 μm. In some examples, the thickness of the coating layers 352 and / or 354 may be between 1 μm and 10 μm. In some examples, the thickness of the coating layers 352 and / or 354 may be between 10 μm and 50 μm.
[0085] Referring to Figure 4A, a schematic cross-sectional view is shown of coated cathode active material particles 400, such as the cathode of a lithium-ion battery. The coated cathode active material particles 400 may include core particles 402 surrounded by a pre-lithiumization coating 404. As shown, the pre-lithiumization coating 404 may be a discontinuous coating composed of a plurality of pre-lithiumization reagent particles 100 (e.g., passivated Li3N core particles). The composition and constituent surfaces of the pre-lithiumization reagent particles 100 are described in detail above with reference to Figure 1A.
[0086] The core particles 402 may consist substantially entirely of a cathode active material, such as a lithium-doped material. The lithium-doped material may include, but is not limited to, these types of electrochemically active materials, lithium metal oxides, lithium phosphate compounds, or combinations thereof. As non-limiting examples of lithiated compounds, the core particles 402 may include one or more of NMC, LFP, LMFP, NCA, NCO, LMN, LMO, LCP, LNP, and LMP. In one example, the core particles 402 may consist substantially entirely of a layered structural material of a lithium-mixed metal oxide.
[0087] In some examples, the average size of the core particles 402 (e.g., D50 size) may be between 5 μm and 15 μm. In some examples, the relationship between multiple core particles 402 may be formed such that each core particle 402 has a similar size. In some examples, the core particles 402 may be larger secondary particles composed of smaller primary particles. Specifically, each secondary particle may contain multiple primary particles.
[0088] The pre-lithiumated coating 404 may have a maximum range 406. Therefore, each of the multiple pre-lithiumated reagent particles 100 may be positioned between the surface of the core particle 402 and the maximum range 406 of the pre-lithiumated coating 404. The maximum range 406 may be defined by the thickness 408 of the pre-lithiumated coating 404, which can correspond to the maximum particle size of the multiple pre-lithiumated reagent particles 100. The maximum particle size of the multiple pre-lithiumated reagent particles 100 can be based on the maximum cross-sectional dimensions of the core particle 102 and the maximum thickness of the passivation coating 104, as described above with reference to Figure 1A. For example, the thickness 408 of the pre-lithiumated coating 404 may be 500 nm or less.
[0089] In some examples, the surface of the core particle 402 may include one or more surface structures 410. For example, one or more surface structures 410 may be openings or cracks within the surface of the core particle 402, and their size and / or depth may vary. Specifically, in some examples, one or more surface structures 410 may be irregular (e.g., having different shapes and sizes). One or more surface structures 410 can, of course, increase the surface area of the core particle 402.
[0090] Multiple pre-lithiated reagent particles 100 can be retained in place by van der Waals molecular, mechanical, and / or other physical attractive forces, in direct contact with each other and with both the core particle 402. Specifically, in some examples, at least some of the multiple pre-lithiated reagent particles 100 can adhere to and / or into one or more surface structures 410 by van der Waals molecular, mechanical, and / or other physical attractive forces. Thus, the size of the multiple pre-lithiated reagent particles 100 can be complementary to the size of the mutual surface structures 410 so that the multiple pre-lithiated reagent particles 100 can be at least partially fixed therein. In some examples, the multiple pre-lithiated reagent particles 100 can be ground to a pre-selected average size (e.g., corresponding to a given PSD) before or during the passivation step. The pre-selected average size of the multiple pre-lithiated reagent particles 100 can enable retention on and partially into surface structures 410 of complementary sizes on the surface of the core particle 402.
[0091] Although shown mechanically bonded in Figure 4A, in some examples the prelithiated reagent particles may instead be chemically bonded to the surface of the cathode active material particles or attached to the surface of the cathode active material particles using a binder. One exemplary coating configuration is shown in Figure 4B. Referring to Figure 4B, a schematic cross-sectional view is shown showing coated cathode active material particles 425, such as the cathode of a lithium-ion battery. Similar to the coated cathode active material particles 400 in Figure 4A, the coated cathode active material particles 425 may include core particles 402 surrounded by a prelithiated coating 428, the core particles 402 may be substantially composed entirely of cathode active material (e.g., lithium-insulated material). Further configurations and embodiments of the core particles 402 are described in detail above with reference to Figure 4A.
[0092] The pre-lithium coating 428 may include a binder 426 that adheres, binds, or anneals a plurality of pre-lithium reagent particles 100 (e.g., passivated Li3N core particles) to each other and to the surface of the core particles 402. The composition and configurations of the pre-lithium reagent particles 100 are described in detail above with reference to Figure 1A.
[0093] In some examples, the binder 426 may include one or more of PVDF, PVP, PEO or crosslinked PEO, PTFE, PMMA, PAA, PVDF-HFP, one or more conductive polymers (e.g., PEDOT, PEDOT:PSS, etc.), cellulose derivatives, and linear, semi-aromatic, or aromatic PI. In one example, the binder 426 may include aromatic PI that can be crosslinked by heat treatment at approximately 350°C, so that the binder 426 can give lithium-ion batteries increased partial electrical conductivity. In the example where the binder 426 includes PVDF, Li3N can still be used in multiple pre-lithiated reagent particles 100, as it can be passivated by a passivation coating (as described in detail above with reference to Figure 1A) (although Li3N may be substantially incompatible with PVDF). Furthermore, the PVDF can further enhance the pre-lithiated coating 428 by gelling and promoting the formation of a three-dimensional structural network by fixing the multiple pre-lithiated reagent particles 100 in place. Since gelation may be undesirable during the production of the cathode slurry, it will be understood that the beneficial effects attributed to PVDF in the pre-lithiumized coating 428 are in contrast to the inclusion of PVDF as a discontinuous binder between multiple coated cathode active material particles 425 in the ultimately formed cathode slurry.
[0094] The pre-lithiumized coating 428 may have a maximum range 430. Thus, each of the multiple pre-lithiumized reagent particles 100 may be positioned between the surface of the core particle 402 and the maximum range 430 of the pre-lithiumized coating 428. The maximum range 430 may be defined by the thickness 432 of the pre-lithiumized coating 428, which in one example may be 500 nm or less.
[0095] Although the pre-lithiumization coatings 404 and 428 in Figures 4A and 4B were described above as containing the pre-lithiumization reagent particles 100 in Figure 1A, it should be understood that the pre-lithiumization reagent particles 125, 150, and 175 in Figures 1B and 1D can be substituted independently or in any desired combination. In other examples, pure (unpassivated) Li3N particles may instead be coated onto the cathode active material particles, and the passivation coating may be applied to the Li3N-coated core particles.
[0096] One exemplary coating configuration is shown in Figure 4C. Referring to Figure 4C, a schematic cross-sectional view is shown showing coated cathode active material particles 450, such as the cathode of a lithium-ion battery. Similar to the coated cathode active material particles 400 and 425 in Figures 4A and 4B, respectively, the coated cathode active material particle 450 may include a core particle 402 surrounded by a pre-lithiumized coating 456, the core particle may be substantially composed entirely of cathode active material (e.g., lithium-filled material). Further configurations and embodiments of the core particle 402 are described in detail above with reference to Figure 4A.
[0097] The pre-lithiumized coating 456 may contain a binder 452 that adheres, binds, or anneals a plurality of Li3N particles 102 (which may function as core particles, for example, in the pre-lithiumized reagent particles 100, 125, 150, and 175 in Figures 1A to 1D) to each other and to the surface of the core particles 402. The plurality of Li3N particles 102 contained within the pre-lithiumized coating 456, as illustrated, may not be substantially pure and passivated. The composition and configurations of the Li3N particles 102 are described in detail above with reference to Figure 1A. Furthermore, it will be understood that the composition of the binder 452 may be similar to or the same as the composition of the binder 426, as described in detail above with reference to Figure 4B.
[0098] The pre-lithiumization coating 456 may further include a passivation coating 454 surrounding the core particles 402 coated with a binder 452 and a plurality of Li3N particles 102. As shown in Figure 4C, the passivation coating 454 may be in direct contact with the binder 452 or in contact with the surface of the plurality of Li3N particles 102 that remain exposed while being bound to the core particles 402 by the binder 452. Thus, the plurality of Li3N particles 102 may be protected from degradation during slurry processing and thus substantially preserved for pre-lithiumization of lithium-ion batteries.
[0099] In some examples, the thickness 458 of the passivation coating 454 can be controlled such that, during the passivation of the core particles 402 and multiple Li3N particles 102 coated with the binder 452, the passivation coating 454 is not so thick as to significantly hinder the rate of pre-lithiation, nor is it so thin as to result in insufficient passivation during slurry processing. Therefore, the thickness 458 of the passivation coating 454 may be, for example, 50 nm or less.
[0100] It will be understood that the thickness 460 of the pre-lithiumized coating 456 may be greater than the thickness 458 of the passivation coating 454. However, there may still be a practical upper limit to the thickness 460 of the pre-lithiumized coating 456. For example, the thickness 460 of the pre-lithiumized coating 456 may be 500 nm or less.
[0101] The pre-lithiated coatings 404, 428 in Figures 4A, 4B, and 4C, respectively, and 456 in Figure 4C, respectively, are described above as being formed from multiple microparticles mechanically or chemically bonded, i.e., multiple (pure) Li3N particles 102 or multiple pre-lithiated reagent particles 100, 125, 150, or 175. However, it will be understood that the multiple microparticles may include additional microparticle species such as cathode catalyst particles, conductive carbon particles, binder particles, pre-lithiated reagent particles including non-Li3N core particles, or combinations thereof. The specific compositions of the cathode catalyst, conductive carbon, binder, and secondary pre-lithiated reagent are not particularly limited and may include any of the compositions of the cathode catalyst, conductive carbon, binder, and pre-lithiated reagent described herein.
[0102] For example, as shown in Figure 4C, at least some of the particles forming the pre-lithiumized coating 456 may be a plurality of additive particles 462. In some examples, the plurality of additive particles 462 may consist of a cathode catalyst, conductive carbon, a binder (e.g., having a different or the same composition as the binder 452), a secondary (e.g., non-Li3N) pre-lithiumizing reagent, or a combination thereof. However, in other examples, the plurality of Li3N particles 102 may be the only particles included in the pre-lithiumized coating 456.
[0103] Similarly, in further examples, the multiple particles forming the pre-lithiumated coating may include multiple pre-lithiumated reagent particles (e.g., passivated Li3N particles) and multiple additive particles. For example, the pre-lithiumated coatings 404 and 428 in Figures 4A and 4B may include multiple additive particles in addition to the pre-lithiumated reagent particles 100. Thus, it should be understood that in some examples, the pre-lithiumated coating may include (passivated) pre-lithiumated reagent particles 100, (unpassivated) Li3N particles 102, additive particles, or a combination thereof. Alternatively, as shown in Figures 4A and 4B, the pre-lithiumated reagent particles 100 may be the only particles included in the pre-lithiumated coatings 404 and 428.
[0104] Referring next to Figure 5, a flowchart of method 500 for producing a cathode slurry for forming a layered cathode is shown, and the cathode slurry may contain passivated Li3N particles. As will be discussed later in 506, the passivation of Li3N particles can be achieved by various passivation coating processes, depending on the desired composition of the passivation coating that is ultimately formed. The specific steps, step sequence, and parameters of the passivation coating process can be calibrated to obtain a well-balanced, thin, and uniform passivation coating with reproducibility.
[0105] It will be understood that Method 500 can be described with respect to the components described in detail above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be the pre-lithiumated reagent particles 100, 125, 150, or 175 of Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as the coated cathode active material particles 400, 425, or 450 of Figures 4A to 4C.
[0106] Furthermore, while the passivation coating processes described herein are intended for the use of passivated Li3N particles as pre-lithification reagents, it will be understood that at least some of the passivation coating processes can be adapted to the passivation of particles with a partial Li3N composition or particles that are substantially Li3N-free. For example, at least some of the passivation coating processes described below in detail with reference to Figures 6 to 11 can be adapted to particles other than pure Li3N particles.
[0107] Furthermore, while the embodiments described herein concern the formation of cathodes containing pre-lithiumization reagents, it will be understood that at least some of the embodiments described herein can be adapted for anode formation. For example, Figure 5 can be adapted for the preparation of an anode slurry for forming a layered anode, and the anode slurry may contain passivated Li3N particles. Thus, Figures 6 to 11 can illustrate certain passivation coating processes that are at least partially interchangeable within such anode formation.
[0108] In 502, method 500 includes selecting a passivation precursor for forming a uniform passivation coating by a passivation coating process. In some examples, the passivation precursor may include one or more precursor compounds having a different chemical or structural configuration from that contained in the final formed passivation coating (i.e., after the chemical / physical manipulation by the passivation coating process). In other examples, the passivation precursor may include a substance that may not be chemically altered during the passivation coating process and may become a passivating agent that is not yet coated on the surface of the Li3N particles.
[0109] In 504, method 500 optionally includes coating the cathode active material with Li3N particles. The Li3N particles are bonded to the surface of the cathode active material physically (e.g., by van der Waals forces, mechanical forces, etc.) or chemically (e.g., by chemical bonding), or attached to the surface of the cathode active material by a binder. In such examples, the Li3N-coated cathode active material may instead undergo a passivation coating process. Thus, the exposed surface of the Li3N particles coated on the cathode active material may be passivated by the passivation coating process.
[0110] In 506, method 500 includes passivating Li3N particles having a uniform passivation coating based on a selected passivation precursor. As described above, a particular passivation coating process may depend on the selection of the passivation precursor. In particular, the chemical and physical properties of the passivation precursor may be well suited to a particular passivation coating process. Exemplary embodiments of passivation coating processes are described below in detail with reference to Figures 6 to 11. In non-limiting examples, passivation may be achieved by reaction with a passivation atmosphere, mechanical mixing, heat treatment, reactive sputtering, wet coating, polymerization, or surface reaction processes, or a combination thereof.
[0111] It will be understood that Li3N particles may be ground to a desired average size before passivation in 506 (or coating on the cathode active material in 504). For example, Li3N precursor particles may be dispersed in one or more solvents in a wet grinding process. One or more solvents may be anhydrous to mitigate the chemical decomposition of Li3N particles during grinding. In some examples, an additional grinding step may be performed after passivation to expose an additional Li3N surface for further passivation.
[0112] In 508, method 500 optionally includes coating the cathode active material with passivated Li3N particles. The passivated Li3N particles may be mechanically bonded or attached to the surface of the cathode active material by a binder. In such an example, the coated Li3N particles (and optionally the binder) are thought to form a pre-lithiumated coating on the cathode active material.
[0113] In 510, method 500 comprises forming a cathode slurry containing passivated Li3N particles (or coated cathode active material) dispersed in a solvent. In some examples, depending on the composition of the passivated Li3N particles, the cathode slurry may further contain one or more of a binder, a conductive additive, and a cathode active material. The relative amounts of the passivated Li3N particles, binder, conductive additive, and cathode active material can be selected to control the viscosity of the cathode slurry and the resulting solid content. In one example, ball mill mixing can be used to spatially uniformly disperse the passivated Li3N particles among other slurry components and within the ultimately formed cathode.
[0114] In 512, Method 500 includes casting a cathode slurry onto a cathode structure to form a slurry-coated cathode structure. In some examples, the cathode structure may include only a current collector, such as aluminum foil. In other examples, the cathode structure may further include a cathode layer formed on the current collector. For example, the cathode layer may include a cathode active material such that passivated Li3N particles are contained in another layer within the ultimately formed cathode. Numerous slurry-based coating processes, including but not limited to slot die coating, roll-to-roll coating (e.g., gravure coating, screen printing, flexographic printing), doctor blade casting, tape casting, spray (aerosol) coating, reverse comma coating, etc., can be utilized without departing from the scope of this disclosure.
[0115] In 514, method 500 includes drying the slurry-coated cathode structure. Drying the slurry-coated cathode structure may include evaporating the solvent at a relatively low temperature (e.g., below 200°C).
[0116] In 516, method 500 includes calendering a cathode structure coated with a dry slurry. Thus, the cathode may be formed comprising Li3N particles having a thin, uniform, and reproducible passivation coating placed thereon.
[0117] Next, referring to Figure 6, a flowchart of method 600 for passivating Li3N particles by reaction with a controlled passivation atmosphere is shown. Thus, as described above, the steps of method 600 can replace step 506 of method 500, as described above with reference to Figure 5. Furthermore, it will be understood that method 600 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0118] In 602, method 600 comprises encapsulating Li3N particles in a vessel having a passivation precursor in the form of a controlled passivation atmosphere. In some examples, the controlled passivation atmosphere may contain one or more of O2, carbon dioxide (CO2), hydrogen sulfide (H2S), and hydrogen fluoride (HF) as secondary pre-lithification reagents (i.e., as primary pre-lithification reagents in addition to Li3N), to form one or more of Li2O, Li2CO3, Li2S, or LiF, respectively. In additional or alternative examples, the controlled passivation atmosphere may contain one or more of acetylene and toluene vapor to form carbonaceous conductive additives (such as carbon black).
[0119] In some examples, the Li3N particles may include cathode catalyst particles that have been attached to them by mechanical mixing before the Li3N particles are sealed in the container. In other examples, the cathode catalyst particles can be attached to the Li3N particles after passivation by mechanical mixing of the cathode catalyst particles and the (passivated) Li3N particles (e.g., 604). Alternatively, the cathode catalyst can be added by flowing a cathode catalyst precursor into the container before or after the passivation of the Li3N particles.
[0120] In some cases, a controlled passivation atmosphere can be supplied through the container. Therefore, it will be understood that "encapsulation" as used in 602 means arranging the Li3N particles so that they are exposed only to a controlled passivation atmosphere, and does not necessarily mean that the Li3N particles are enclosed within the container so that they are isolated from the gas supply.
[0121] In 604, Method 600 includes passivating Li3N particles by reaction of the surface of the Li3N particles with a controlled passivation atmosphere. Specifically, one or more components of the controlled passivation atmosphere can be directed (e.g., as a flow gas) to the surface of the Li3N particles and react with the surface of the Li3N particles. In some examples, the Li3N particles may be exposed to a controlled passivation atmosphere for a long period of time (e.g., 0.5 hours to 7 days) at a relatively high temperature (e.g., from 20°C to 500°C). The composition of the passivation coating on the Li3N particles can be controlled accordingly by supplying the controlled passivation atmosphere by a container while monitoring and adjusting the composition of the controlled passivation atmosphere. For example, with a pure and dry O2 supply, the composition of the passivation coating after the surface of the Li3N particles reacts with the controlled passivation atmosphere may mainly consist of Li2O.
[0122] In 606, method 600 optionally includes activating the passivation coating on the passivated Li3N particles. For example, in a specific example in which a carbonaceous conductive additive is included in the passivation coating, activation may be achieved by applying additional pressure (e.g., by mechanical pressing) or by applying ultrasonic treatment.
[0123] In 608, method 600 optionally includes chemically treating passivated Li3N particles with an additional passivation precursor. Specifically, the additional passivation precursor can further react with the passivation coating on the Li3N particles. For example, in a particular example in which Li2O is included in the passivation coating, the additional passivation precursor may be hydrogen peroxide (H2O2) such that at least some Li2O can be converted to Li2O2 (and may also be used as a secondary pre-lithification reagent).
[0124] Next, referring to Figure 7, a flowchart of method 700 for passivating Li3N particles by a mechanical mixing process is shown. Thus, as described above, the steps of method 700 can replace step 506 of method 500, as described above with reference to Figure 5. Furthermore, it will be understood that method 700 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0125] In 702, method 700 comprises optionally combining a cathode catalyst with a passivation precursor in a container. In some examples, the passivation precursor may include one or more secondary prelithiation reagents such as Li2O, Li2CO3, Li2S, or LiF. Thus, in such examples, the cathode catalyst may be utilized as needed to promote the decomposition of the secondary prelithiation reagent during prelithiation in the final lithium-ion battery. In some examples, the cathode catalyst may include one or more of Co3O4, LFP, and LMFP.
[0126] In 704, method 700 includes adding Li3N particles to a container having a passivation precursor. In some examples, Li3N particles may be added to the container under an inert atmosphere to mitigate the degradation of Li3N. 702 is optional, and the cathode catalyst may or may not be present when the Li3N particles are added to the container.
[0127] In 706, method 700 comprises mechanically mixing Li3N particles with a passivation precursor to passivate the Li3N particles with a high-density or continuous passivation coating. Mechanical mixing can be achieved by wet or dry grinding, smearing, or mechanofusion processes, among other mechanical mixing processes. In some examples, the passivation precursor may include a secondary pre-lithification reagent, as described above in 702, which can be coated onto the surface of the Li3N particles by grinding or mechanofusion processes. In additional or alternative examples, the passivation precursor may include one or more carbonaceous conductive additives, such as carbon black, graphene, and graphene oxide, which can be coated onto the surface of the Li3N particles by mechanofusion processes. In additional or alternative examples, the passivation precursor may include one or more PILs (or their monomeric units), which can be coated onto the surface of the Li3N particles by grinding or smearing processes.
[0128] To adequately passivate Li3N particles, a continuous and uniform coating can be applied to the majority of the surface of the Li3N particles. However, some mechanical mixing processes can instead form a discontinuous coating of densely and uniformly packed particles, which serves a similar function to the continuous coating achieved by other mechanical mixing processes.
[0129] In 708, method 700 optionally includes activating the passivation coating on the passivated Li3N particles. For example, in a specific example in which a carbonaceous conductive additive is included in the passivation coating, activation may be achieved by applying additional pressure (e.g., by mechanical pressing) or by ultrasonic irradiation.
[0130] In method 700, method 700 optionally includes drying the passivated Li3N particles. For example, in certain cases in which one or more PILs are included in the passivated coating, drying may be achieved by spray drying.
[0131] Referring to Figure 8, a flowchart of Method 800 for passivating Li3N particles by a wet coating and calcination process is shown. Thus, as described above, the steps of Method 800 can replace step 506 of Method 500, as described above with reference to Figure 5. Furthermore, it will be understood that Method 800 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0132] In 802, method 800 comprises adding Li3N particles to a passivation precursor solution to obtain Li3N particles coated with a precursor. In some examples, to mitigate the degradation of Li3N, the Li3N particles may be added to the passivation precursor solution under inert atmosphere conditions. In some examples, the passivation precursor solution may contain a carbonaceous polymer binder (as a passivation precursor) dispersed in a suitable solvent. In such examples, the solvent in the passivation precursor solution may be gradually dried or evaporated with stirring at room temperature (~20°C) or high temperature (<300°C) to promote the formation of a uniform precursor coating on the surface of the Li3N particles. Inert atmosphere conditions may be maintained to protect the Li3N particles during the evaporation of the solvent. In some examples, the passivation precursor solution may contain pitch black as the passivation precursor.
[0133] In 804, method 800 includes obtaining passivated Li3N particles by calcining Li3N particles coated with a precursor. Specifically, Li3N particles can be immersed in a passivation precursor solution and then coated with the passivation precursor. Next, the Li3N particles coated with the precursor can be calcined in an inert atmosphere at a relatively high temperature (e.g., 700°C to 1200°C) to form a passivation coating on the Li3N particles, where the passivation coating may include, for example, a carbonaceous conductive additive. For example, in an example where the passivation precursor solution contains pitch black as the passivation precursor, a carbon passivation coating can be realized on the surface of the Li3N particles by calcining the precursor-coated Li3N particles at 700-1200°C.
[0134] In 806, method 800 optionally includes activating the passivation coating on the passivated Li3N particles. For example, in a specific example in which a carbonaceous conductive additive is included in the passivation coating, activation may be achieved by applying additional pressure (e.g., by mechanical pressing) or by applying ultrasonic treatment.
[0135] Next, with reference to Figure 9, a flowchart of Method 900 for passivating Li3N particles by a reactive sputtering process is shown. Thus, as described above, the steps of Method 900 can replace step 506 of Method 500, as described above with reference to Figure 5. Furthermore, it will be understood that Method 900 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0136] In 902, method 900 includes adding Li3N particles to a container having a passivation precursor in the form of a metal precursor target. In some examples, the Li3N particles may be added to the container under an inert atmosphere to mitigate the degradation of Li3N. In some examples, the metal precursor target (e.g., a plate) may include a metal oxide containing at least one non-lithium metal, such as one or more of Al, Fe, Cu, W, V, Ti, Ni, Zn, Cd, Ag, and Co.
[0137] In 904, method 900 includes passivating Li3N particles by reactive sputtering of a metal precursor target. Specifically, reactive sputtering may occur while the Li3N particles are continuously mixed in a container so that a passivation coating containing a non-lithium metal can be formed on the surface of the Li3N particles.
[0138] In 906, method 900 optionally includes activating the passivation coating on the passivated Li3N particles. For example, in certain cases where the passivation coating contains a non-lithium metal, activation may be achieved by applying additional pressure (e.g., by mechanical pressing) or by applying ultrasonic treatment.
[0139] Next, referring to Figure 10, a flowchart of Method 1000 for passivating Li3N particles by a first wet coating and purification process is shown. Thus, as described above, the steps of Method 1000 can replace step 506 of Method 500, as described above with reference to Figure 5. Furthermore, it will be understood that Method 1000 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0140] In 1002, method 1000 comprises adding Li3N particles to a passivation precursor solution. In some examples, Li3N particles can be added to the passivation precursor solution under inert atmosphere conditions to mitigate the degradation of Li3N. In some examples, the passivation precursor solution may contain organic materials dispersed in a suitable solvent. The organic materials may include one or more waxes, one or more long-chain conductive polymers, and / or one or more small organic molecules, such as natural waxes, paraffin waxes, PE, PP, PS, oleic acid, stearic acid, PVDF-HFP, PEO, PMMA, and / or PMA. Furthermore or alternatively, the solvent may include inert organic solvents such as hendecane (undecane), dodecane, mineral oil mixtures, linear polysiloxanes, or combinations thereof.
[0141] In 1004, method 1000 includes reacting Li3N particles in a passivation precursor to obtain Li3N particles coated with the precursor. Specifically, the surface of the Li3N particles can react with one or more passivation precursors, such as H2O, H2O2, and H2S, to form a passivation layer thereon. In cases where a relatively thin passivation layer is desired, the thickness of the passivation layer can be adjusted by selecting the concentration of the passivation precursor in the passivation precursor solution and the reaction temperature. In additional or alternative examples, particles or molecules of the passivation precursor can be attached to the surface of the Li3N particles by surface grafting. In such examples, heat, light (e.g., ultraviolet light) and / or stirring can be supplied to achieve efficient and uniform grafting and thereby obtain Li3N particles coated with the precursor.
[0142] In 1006, method 1000 includes purifying precursor-coated Li3N particles to obtain passivated Li3N particles. Purification may include removing excess solvent and by-products from the surface of the passivated Li3N particles. Specifically, in 1008, method 1000 may include filtering the precursor-coated Li3N particles before washing in 1010. In 1010, method 1000 may include washing the precursor-coated Li3N particles. In one example, washing may involve using an additional inert organic solvent such as hexane to dissolve and remove by-products from the surface of the passivated Li3N particles. In 1012, method 1000 may include filtering the precursor-coated Li3N particles after washing in 1010. In 1014, method 1000 may include drying the precursor-coated Li3N particles. The precursor-coated Li3N particles can be vacuum-dried, for example.
[0143] Next, referring to Figure 11, a flowchart of Method 1100 for passivating Li3N particles by a second wet coating and purification process is shown. Thus, as described above, the steps of Method 1100 can replace step 506 of Method 500, as described above with reference to Figure 5. Furthermore, it will be understood that Method 1100 can be described with reference to the components described above with reference to Figures 1A to 4C. For example, the passivated Li3N particles may be pre-lithiated reagent particles 100, 125, 150 or 175 in Figures 1A to 1D, or the Li3N particles may be contained in coated cathode active material particles such as coated cathode active material particles 400, 425 or 450 in Figures 4A to 4C.
[0144] In 1102, method 1100 comprises optionally combining a first co-solvent with a passivation precursor in a container. In some examples, the passivation precursor may include one or more PILs. To control the desired viscosity and concentration of the PIL (therefore, the uniformity and thickness of the final passivated coating), the first co-solvent may be added to the container in appropriate amounts as needed. In examples where the first co-solvent is added to the container, a wide range of compositions of the first co-solvent are conceivable for the versatility of the PIL. For example, the first co-solvent may include one or more anhydrous alcohols (e.g., methanol, ethanol, isopropanol, etc.), carbonates (e.g., one or more ethylene carbonate, propylene carbonate, etc.), glycols, chloroform, ethyl acetate, dichloromethane, pyridine, acetone, acetonitrile, etc. However, the selection of the first co-solvent may be limited in some examples based on toxicity or other properties harmful to human health.
[0145] In further examples, the first cosolvent may include water. Thus, one or more PILs may be selected to be compatible with water (e.g., Cl - and I - PILs containing hydrophilic anions (such as PF6). However, dispersing hydrophilic PILs in water can disrupt the association (e.g., increase dissociation) between anion and cation pairs in the solution, potentially affecting the overall coating quality of the passivation layer that ultimately forms. In particular, depending on the concentration and anion selection, if one or more PILs dissolve in water (e.g., to overcome their Hildebrand solubility parameter), the dissociation between anion and cation pairs in the solution can increase. Thus, one or more PILs may be selected to be incompatible with water (e.g., PF6). - PIL containing hydrophobic anions such as [example of PIL]. In other examples, the first cosolvent may be non-aqueous.
[0146] In 1104, method 1100 includes adding Li3N particles to a container having a passivation precursor. In some examples, Li3N particles may be added to the container under an inert atmosphere to mitigate the degradation of Li3N. 1102 is optional, and the first cosolvent may or may not be present when adding the Li3N particles to the container.
[0147] In 1106, method 1100 comprises coating Li3N particles with a passivation precursor to obtain precursor-coated Li3N particles. In some examples, coating can be achieved by immersing Li3N particles (as passivation precursor) in pure (undiluted) PIL and stirring the container. In one example, the passivation precursor may be one or more PILs or one or more ionomers, which may be locally melted by shear due to physical mixing. In such examples, the passivation precursor may form a passivation coating on Li3N particles alone or on larger structures such as Li3N-coated cathode active material particles (which may contain exposed Li3N).
[0148] In certain examples where the passivation precursor includes one or more PILs, the coating of Li3N particles may be configured to crosslink and / or polymerize one or more PILs thereon. For example, in 1108, method 1100 may optionally include initiating polymerization of the passivation precursor. For example, the passivation precursor may include one or more PILs that can be (further) polymerized by the addition of a free radical initiator and heating, or by ultraviolet-based (UV) treatment. However, in other examples, polymerization initiation may not be employed because one or more PILs can be polymerized before being added to the container. In another example, in 1110, method 1100 may optionally include adding a surfactant or a second cosolvent to the container to induce a coating of the passivation precursor on the surface of the Li3N particles, the second cosolvent having opposite polarity to the first cosolvent. Therefore, in examples where the passivation precursor contains one or more PILs, a surfactant or a second cosolvent can cause one or more PILs to coagulate on the surface of the Li3N particles (for example, driven by the difference in miscibility between the surfactant and the first cosolvent or between the first and second cosolvents).
[0149] In 1112, method 1100 includes purifying the precursor-coated Li3N particles to obtain passivated Li3N particles. Specifically, in 1114, method 1100 may optionally include evaporating a first and / or second cosolvent (if present). In 1116, method 1100 may include filtering the precursor-coated Li3N particles. In 1118, method 1100 may include drying the precursor-coated Li3N particles.
[0150] Once passivated, Li3N particles can be incorporated into a cathode structure such as cathode structure 300 or 350 in Figures 3A-B. The cathode structure can be further combined with other components to form a Li-ion battery cell, as detailed in Figure 12 below. Furthermore, multiple Li-ion battery cells can be combined to form a Li-ion battery pack. A schematic diagram 1200 showing a battery pack 1202 is shown in Figure 12. In some examples, the battery pack 1202 may comprise a battery pack assembly in which multiple lithium-ion battery cells 1204 are detachably mounted on a housing base 1212. Thus, it will be understood that each lithium-ion battery cell 1204 can represent a basic unit that can constitute a battery pack having any size, any power, and any number of lithium-ion battery cells 1204. Furthermore, it will be understood that other embodiments not shown in Figure 12 may include battery packs having only one lithium-ion battery cell.
[0151] Furthermore, each of the multiple lithium-ion battery cells 1204 can be configured to expose a positive electrode tab 1206 and a negative electrode tab 1208, and to be coupled to the positive and negative electrodes, respectively. The positive electrode may be a cathode incorporating Li3N passivation particles, such as the cathode structure 300 or 350 shown in Figures 3A-B.
[0152] Multiple lithium-ion battery cells 1204 may be held in a stacked configuration by bands 1210. As shown, one or more bands 1210 can encapsulate multiple lithium-ion battery cells 1204 so as to prevent the individual lithium-ion battery cells 1204 from displacing each other.
[0153] In this way, passivated Li3N particles are provided as sacrificial pre-lithification reagents to improve the initial cycle performance in lithium-ion batteries. In some examples, the passivation coating process for Li3N particles is carried out under precise environmental conditions such that a thin, uniform, and reproducible passivation coating is formed. For example, the passivation coating can be thin enough not to hinder the pre-lithification of the Li3N drive in the lithium-ion battery, while still adequately covering the surface of the Li3N particles to prevent undesirable side reactions. Therefore, important experiments can be employed to carefully adjust the parameters of the passivation coating process so that maximum pre-lithification is consistently supplied to the lithium-ion battery during initial charging, thereby improving the overall electrochemical performance.
[0154] Furthermore, electronic conductivity, ionic conductivity, cycle performance, electrode active material stability, and / or additional sacrificial Li + The composition of the passivation coating can be selected to provide ions. In addition, or alternatively, the composition of the passivation coating can be selected to rapidly decompose / dissolve in the battery environment, thereby increasing the rate of pre-lithiation on the exposed Li3N surface. Correspondingly, the passivation coating process can be further adjusted to considerations specific to the selected composition so that sufficient protection of the Li3N particles can be maintained while further improving the overall electrochemical performance of the lithium-ion battery.
[0155] In one example, the cathode pre-lithiation reagent comprises a core particle containing Li3N and a passivation coating uniformly distributed on at least a portion of the surface of the core particle. The first example of the cathode pre-lithiation reagent further comprises the passivation coating having a thickness of 20 nm or less. The second example of the cathode pre-lithiation reagent optionally comprises the first example of the cathode pre-lithiation reagent and further comprises the passivation coating uniformly distributed substantially 100% of the surface of the core particle. The third example of the cathode pre-lithiation reagent optionally comprises one or more of the first and second examples of the cathode pre-lithiation reagent and further comprises the passivation coating being formed as a continuous layer on the surface of the core particle. The fourth example of the cathode pre-lithiation reagent optionally comprises one or more of the first to third examples of the cathode pre-lithiation reagent and further comprises the passivation coating being formed as a discontinuous coating of passivation particles physically or chemically bonded to the surface of the core particle. A fifth example of a cathode pre-lithiumation reagent optionally includes one or more of the first to fourth examples of cathode pre-lithiumation reagents, and further includes a passivation coating containing one or more of Li2O2, Li2O, Li2CO3, Li2S, and LiF. A sixth example of a cathode pre-lithiumation reagent optionally includes one or more of the first to fifth examples of cathode pre-lithiumation reagents, and further includes a passivation coating containing one or more of carbon black, graphene, graphene oxide, and carbon nanotubes. A seventh example of a cathode pre-lithiumation reagent optionally includes one or more of the first to sixth examples of cathode pre-lithiumation reagents, and further includes a passivation coating containing one or more organic materials. An eighth example of the cathode prelithiation reagent optionally includes one or more of the first to seventh examples of the cathode prelithiation reagent, and further includes a passivation coating that includes one or more ionomers and / or polymerized ionic liquids. A ninth example of the cathode prelithiation reagent optionally includes one or more of the first to eighth examples of the cathode prelithiation reagent, and further includes a passivation coating that includes one or more non-lithium metals or metal oxides, including oxides of Al, Fe, Cu, W, V, Ti, Ni, Zn, Cd, Ag, and / or Co.
[0156] In another example, a lithium-ion battery comprises a cathode, a lithium-ion anode, and an electrolyte, each comprising a lithiated cathode active material, a primary sacrificial prelithiation reagent consisting of pure Li3N particles, and a passivation coating uniformly distributed on the surface of the primary sacrificial prelithiation reagent, wherein the cathode and lithium-ion anode are immersed in the electrolyte, and the passivation coating separates the primary sacrificial prelithiation reagent from the electrolyte. The first example of a lithium-ion battery further comprises the primary sacrificial prelithiation reagent decomposing to provide lithium ions during the prelithiation of the lithium-ion battery, and the absence of a cathode catalyst in the lithium-ion battery prior to the initial cycle of the lithium-ion battery. The second example of a lithium-ion battery optionally comprises the first example of a lithium-ion battery and further comprises the passivation coating comprising a secondary sacrificial prelithiation reagent, the secondary sacrificial prelithiation reagent comprising one or more lithium-containing compounds, and each of the primary and secondary sacrificial prelithiation reagents decomposing to provide lithium ions during the prelithiation of the lithium-ion battery. A third example of a lithium-ion battery optionally includes one or more of the first and second examples of lithium-ion batteries, further comprising a passivation coating that includes a cathode catalyst, the cathode catalyst catalyzing the decomposition of a secondary sacrificial prelithiation reagent during the prelithiation of the lithium-ion battery. A fourth example of a lithium-ion battery optionally includes one or more of the first to third examples of lithium-ion batteries, further comprising a passivation coating that includes a carbonaceous conductive additive. A fifth example of a lithium-ion battery optionally includes one or more of the first to fourth examples of lithium-ion batteries, further comprising a passivation coating that includes one or more organic materials, each of which is dissolved in the electrolyte. A sixth example of a lithium-ion battery optionally includes one or more of the first to fifth examples of lithium-ion batteries, further comprising a passivation coating that includes one or more polymer salts.A seventh example of a lithium-ion battery optionally includes one or more of the first to sixth examples of lithium-ion batteries, and further includes a passivation coating that includes one or more non-lithium metals or metal oxides. An eighth example of a lithium-ion battery optionally includes one or more of the first to seventh examples of lithium-ion batteries, and further includes a passivation coating that has a thickness of 20 nm or less. A ninth example of a lithium-ion battery optionally includes one or more of the first to eighth examples of lithium-ion batteries, and further includes a lithium-ionized cathode active material being particulate and the lithium-ionized cathode active material being coated with a primary sacrificial prelithiation reagent.
[0157] In yet another example, the method includes passivating Li3N particles to form a uniform passivation coating thereon, and forming a cathode slurry containing the passivated Li3N particles. The first example of the method further includes the Li3N particles having a normal particle size distribution with peaks of 150 nm or less. The second example of the method optionally includes the first example of the method and further includes the Li3N particles having a D50 size of 150 nm or less. The third example of the method optionally includes one or more of the first and second examples of the method and further includes the uniform passivation coating having a thickness in the range of 1 nm to 50 nm. The fourth example of the method optionally includes one or more of the first to third examples of the method and further includes coating the cathode active material with Li3N particles before or after passivation. A fifth example of the method optionally includes one or more of the first to fourth examples of the method, comprising passivating Li3N particles, encapsulating the Li3N particles in a vessel having a controlled passivation atmosphere, and coating the Li3N particles by reaction with the controlled passivation atmosphere. A sixth example of the method optionally includes one or more of the first to fifth examples of the method, further comprising passivating Li3N particles and chemically treating the coated Li3N particles. A seventh example of the method optionally includes one or more of the first to sixth examples of the method, further comprising passivating Li3N particles and coating the Li3N particles with a passivation precursor by mechanical mixing. An eighth example of the method optionally includes one or more of the first to seventh examples of the method, further comprising homogeneously mixing a cathode catalyst with the passivation precursor before mechanically mixing the Li3N particles with the passivation precursor. A ninth embodiment of the present method optionally includes one or more of the first to eighth embodiments of the present method, and comprises passivating Li3N particles, coating Li3N particles with a passivation precursor, and calcining the coated Li3N particles.A tenth example of the Method optionally includes one or more of the first to ninth examples of the Method, comprising passivation of Li3N particles and coating of Li3N particles by reactive sputtering of a metal precursor target. An eleventh example of the Method optionally includes one or more of the first to tenth examples of the Method, further comprising passivation of Li3N particles and activation of the coated Li3N particles. A twelfth example of the Method optionally includes one or more of the first to eleventh examples of the Method, comprising passivation of Li3N particles, coating of Li3N particles with a passivation precursor and purification of the coated Li3N particles. A thirteenth example of the Method optionally includes one or more of the first to twelfth examples of the Method, further comprising passivation of Li3N particles and addition of a first cosolvent before coating of Li3N particles with a passivation precursor. A 14th example of this method optionally includes one or more of the 1st to 13th examples of this method, further comprising coating Li3N particles with a passivation precursor and adding a surfactant or a second co-solvent to induce coating of the passivation precursor on the surface of the Li3N particles, wherein the second co-solvent has opposite polarity to the first co-solvent. A 15th example of this method optionally includes one or more of the 1st to 14th examples of this method, further comprising coating Li3N particles with a passivation precursor and initiating polymerization of the passivation precursor. A 16th example of this method optionally includes one or more of the 1st to 15th examples of this method, further comprising forming a layered cathode including a cathode structure coated with a cathode slurry.
[0158] In yet another example, a layered cathode comprising a current collector and one or more slurry coating layers positioned on the opposite side of the current collector, wherein at least one of the slurry coating layers comprises uniformly and completely passivated lithium nitride particles. The first example of the layered cathode comprises: a plurality of lithium nitride particles having an average size of 150 nm or less; and a passivation coating uniformly and completely covering each of the plurality of lithium nitride particles. The second example of the layered cathode optionally includes the first example of the layered cathode, further comprising the passivation coating having a thickness of 20 nm or less.
[0159] The following claims specifically point to certain combinations and partial combinations that are considered novel and non-obvious. These claims may refer to “a certain” element, “a first” element, or any of the same, etc. Such claims should be understood to include the incorporation of one or more such elements, and not to require or exclude two or more such elements. Other combinations and partial combinations of the disclosed features, functions, elements and / or properties may be claimed through amendments to these claims or through the presentation of new claims in this application or a related application. Such claims, whether broader, narrower, similar, or different from the original claims, shall be deemed to be included in the subject matter of this disclosure.
Claims
1. Li 3 A core particle containing N, The material includes a passivation coating uniformly distributed on at least a portion of the surface of the core particles, The passivation coating comprises one or more metal oxides, including oxides of Al, Fe, Cu, W, V, Ti, Ni, Zn, Cd, Ag and / or Co. The passivation coating has a thickness of 50 nm or less. Cathode prelithiation reagent.
2. The passivation coating has a thickness of 20 nm or less and is formed as a continuous layer on the surface of the core particles. The cathode prelithiation reagent according to claim 1.
3. The passivation coating is formed as a discontinuous coating of passivation particles physically or chemically bonded to the surface of the core particles. The cathode prelithiation reagent according to claim 1.
4. The passivation coating is Li 2 O 2 Li 2 O, Li 2 CO 3 Li 2 S and Includes one or more of the LiF The cathode prelithiation reagent according to claim 1.
5. The passivation coating comprises one or more of carbon black, graphene, graphene oxide, and carbon nanotubes, and comprises one or more organic materials. The cathode prelithiation reagent according to claim 1.
6. The passivation coating comprises one or more ionomers and / or polymerized ionic liquids. The cathode prelithiation reagent according to claim 1.
7. The passivation coating separates the core particles from the electrolyte. The cathode prelithiation reagent according to claim 1.
8. The aforementioned core particles decompose during the pre-lithification of lithium-ion batteries to supply lithium ions. Before the initial cycle of the lithium-ion battery, the lithium-ion battery does not have a cathode catalyst. The cathode prelithiation reagent according to claim 1.
9. The passivation coating comprises a secondary sacrificial prelithiation reagent, The aforementioned secondary sacrificial prelithiation reagent comprises one or more lithium-containing compounds. Each of the core particles and the secondary sacrificial prelithiation reagent decomposes during the prelithiation of the lithium-ion battery to supply lithium ions. The cathode prelithiation reagent according to claim 1.
10. Li 3 Passivating N particles and forming a uniform passivation coating on them, and Li having a uniform passivation coating 3 to form a cathode slurry containing N particles This includes, The passivation coating comprises one or more metal oxides, including oxides of Al, Fe, Cu, W, V, Ti, Ni, Zn, Cd, Ag and / or Co. The passivation coating has a thickness of 50 nm or less. method.
11. The Li 3 N particles have a D50 size of 150 nm or less. The method according to claim 10.
12. The Li 3 Passivating N particles is performed by placing them in a container with a controlled passivation atmosphere. The Li 3 By encapsulating N particles and reacting with the controlled passivation atmosphere, The Li 3 Including coating N particles, The method according to claim 10.
13. The Li 3 Passivating N particles is a process that involves mechanical mixing or the reaction of a metal precursor target. Responsive sputtering is used to passivate the Li 3 Coating N particles include, The method according to claim 10.
14. The Li 3 Passivation of N particles is performed using the passivation precursor Li 3 Coating N particles To coat, and the Li coated with the passivation precursor 3 Burning N particles Including forming or purifying, The method according to claim 10.
Citation Information
Patent Citations
Lithium nitride composite material and preparation and application
CN111224077A
Lithium supplementing agent and application thereof
CN112054181A
Cathode additive for rechargeable lithium batteries
JP2018522371A