Curable resin compositions, cured products, and adhesives
A curable resin composition with an amine-based latent curing agent improves conductivity and curability in cyanate ester and epoxy resin systems, addressing the limitations of existing adhesives.
Patent Information
- Application Number
- JP2023554529
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-18
- Filing Date
- 2022-10-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-11
AI Technical Summary
Existing conductive adhesives using cyanate ester and epoxy resins with imidazole-modified core-shell curing agents do not provide satisfactory conductivity and curability.
A curable resin composition containing a cyanate ester resin, an epoxy resin, and a conductive filler, using an amine-based latent curing agent with active hydrogen to enhance conductivity and curability.
The composition yields a cured product with excellent conductivity and curability, suitable for electronic applications.
Smart Images

Figure 0007955283000008 
Figure 0007955283000009 
Figure 0007955283000010
Abstract
Description
[Technical Field]
[0001] The present invention relates to a curable resin composition containing a cyanate ester resin, an epoxy resin, a latent curing agent, and a conductive filler. [Background technology]
[0002] Traditionally, solder has been used as a conductive bonding agent for electronic components, and in most cases, Sn-Pb alloy has been used. However, because it contains lead, there are concerns about adverse effects on human health and the environment, and it also has the problem of low heat resistance. Therefore, conductive adhesives, which are obtained by compounding conductive fillers into polymer materials, have come into use as an alternative to solder. Conductive adhesives have advantages such as low environmental impact, the ability to be mounted at low temperatures, and the ability to maintain adhesive strength even at high temperatures.
[0003] Many techniques have been proposed for incorporating conductive fillers into polymers. For example, Patent Document 1 proposes incorporating conductive particles, such as metal particles, into an adhesive composition obtained by containing a cyanate ester resin, an epoxy resin, and a latent curing agent. In the examples, a core-shell type curing agent with an imidazole modified material as the core is described as suitable, but it did not provide satisfactory conductivity or curability. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-279121 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] The problem that this invention aims to solve is to provide a curable resin composition that yields a cured product with excellent conductivity and curability. [Means for solving the problem]
[0006] The present inventors have discovered that by using an amine-based latent curing agent having active hydrogen as the latent curing agent in a curable resin composition containing a cyanate ester resin, an epoxy resin, a latent curing agent, and a conductive filler, a curable resin composition with excellent conductivity can be obtained, thus completing the present invention.
[0007] The present invention relates to a curable resin composition containing (A) a cyanate ester resin, (B) an epoxy resin, (C) a latent curing agent containing an amine-based latent curing agent having active hydrogen obtained by reacting an amine compound with an epoxy compound, and (D) a conductive filler. [Effects of the Invention]
[0008] According to the present invention, it is possible to provide a curable resin composition that yields a cured product with excellent conductivity and curability. [Brief explanation of the drawing]
[0009] [Figure 1] Figure 1 is an SEM image of the cured product of Example 1. [Figure 2] Figure 2 shows an SEM image of the cured product of Comparative Example 3. [Figure 3] Figure 3 is an SEM image of the cured product from Example 2. [Figure 4] Figure 4 shows an SEM image of the cured product of Comparative Example 1. [Figure 5] Figure 5 is an SEM image of the cured product of Example 3. [Modes for carrying out the invention]
[0010] The curable resin composition of the present invention will be described below. The cyanate ester resin, which is component (A) used in this invention, can be any compound having two or more cyanate groups, and can be used without any particular restrictions on molecular structure, molecular weight, etc.
[0011] Examples of the cyanate ester resin include a compound represented by the following formula (1), a compound represented by the following formula (2), and polymers thereof.
[0012] [Chemical Formula] (In the formula, Y 1 represents a divalent hydrocarbon group which is unsubstituted or substituted with a fluorine atom or a cyanate group, or represents -O-, -S-, or a single bond; A 1 and A 2 each independently represent a phenylene group which is unsubstituted or substituted with 1 to 4 alkyl groups.)
[0013] [Chemical Formula] (In the formula, m is an integer of 1 or more; Y 2 and Y 3 each independently represent -S-, or represent a divalent hydrocarbon group which is unsubstituted or substituted with a fluorine atom or a cyanate group; R 1 , R 2 and R 3 each independently represent an alkyl group having 1 to 4 carbon atoms; and each n is independently an integer of 0 to 2.)
[0014] Examples of Y 1 in the formula (1), and Y 2 and Y 3 in the formula (2) include groups represented by the following formulas (Y-1) to (Y-9).
[0015] [Chemical Formula] (In the formula, n is an integer of 4 to 12; R 7 and R 8 each independently represent a hydrogen atom or a methyl group which is unsubstituted or substituted with a fluorine atom. In addition, * represents a bond.)
[0016] Commercially available cyanate ester resins include, but are not limited to, Lonza's Cyanate LECy, PT-15, PT30, PT-60, etc., Huntsman's L-10, XU366, XU371, XU378, etc., and Mitsubishi Gas Chemical's CA200, etc. These cyanate ester resins may be used individually or in combination of two or more types.
[0017] Among the cyanate ester resins mentioned above, bisphenol-type, biphenyl-type, and novolacphenol-type cyanate ester resins are preferred, and in particular, bisphenol-type cyanate ester resins such as bisphenol A-type, bisphenol E-type, and bisphenol F-type are preferred.
[0018] The epoxy resin (component B) used in this invention only needs to have two or more epoxy groups in its molecule, and there are no particular restrictions on its molecular structure, molecular weight, etc.
[0019] The epoxy resins include polyglycidyl ether compounds of mononuclear polyhydric phenol compounds such as hydroquinone, resorcinol, pyrocatechol, and phloroglucinol; dihydroxynaphthalene, biphenol, methylenebisphenol (bisphenol F), methylenebis(orthocresol), ethylidenebisphenol, isopropylidenebisphenol (bisphenol A), isopropylidenebis(orthocresol), tetrabromobisphenol A, 1,3-bis(4-hydroxycumylbenzene), 1,4-bis(4-hydroxycumylbenzene), 1,1,3-tris(4-hydroxyphenyl)butane, 1,1,2,2-tetra(4-hydroxyphenyl)ethane, thiobisphenol, sulfobisphenol, oxybisphenol, phenol novolac, orthocresol novolac, ethylphenol novolac, butylphenol novolac, octylphenol novolac, resorcinol novolac, terpene phenol, and other polynuclear poly Polyglycidyl ether compounds of valent phenol compounds; polyglycidyl ether compounds of polyhydric alcohol compounds such as ethylene glycol, propylene glycol, butylene glycol, hexanediol, polyethylene glycol, polypropylene glycol, thioglycol, dicyclopentadiene dimethanol, 2,2-bis(4-hydroxycyclohexyl)propane (hydrogenated bisphenol A), glycerin, trimethylolpropane, pentaerythritol, sorbitol, and bisphenol A alkylene oxide adducts; homopolymers or copolymers of glycidyl ester compounds and glycidyl methacrylates of aliphatic, aromatic, or alicyclic polybasic acids such as maleic acid, fumaric acid, itaconic acid, succinic acid, glutaric acid, suberic acid, adipic acid, azelaic acid, sebacic acid, dimer acid, trimer acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, trimesic acid, pyromellitic acid, tetrahydrophthalic acid, and endomethylenetetrahydrophthalic acid;Epoxy compounds having a glycidylamino group, such as N,N-diglycidylaniline, bis(4-(N-methyl-N-glycidylamino)phenyl)methane, diglycidyl orthotoluidine, N,N-bis(2,3-epoxypropyl)-4-(2,3-epoxypropoxy)-2-methylaniline, N,N-bis(2,3-epoxypropyl)-4-(2,3-epoxypropoxy)aniline, and N,N,N',N'-tetra(2,3-epoxypropyl)-4,4-diaminodiphenylmethane; vinylcyclohexene diepoxides Examples include epoxidized cyclic olefin compounds such as cyclopentanediene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-6-methylcyclohexanecarboxylate, and bis(3,4-epoxy-6-methylcyclohexylmethyl) adipate; epoxidized conjugated diene polymers such as epoxidized polybutadiene and epoxidized styrene-butadiene copolymers; and heterocyclic compounds such as triglycidyl isocyanurates. Furthermore, these epoxy resins may be internally crosslinked with terminal isocyanate prepolymers, or have high molecular weights due to polyvalent active hydrogen compounds (polyvalent phenols, polyamines, carbonyl group-containing compounds, polyphosphate esters, etc.). These epoxy resins may be used individually or in combination of two or more types.
[0020] Among the epoxy resins mentioned above, polyglycidyl ether compounds of polynuclear polyvalent phenol compounds are preferred.
[0021] The content of epoxy resin, which is component (B), is preferably 20 to 200 parts by mass, and more preferably 30 to 150 parts by mass, per 100 parts by mass of cyanate ester resin, which is component (A), in order to obtain a cured product with excellent physical properties.
[0022] The latent curing agent, which is component (C) used in the present invention, contains an amine-based latent curing agent having active hydrogen obtained by reacting an amine compound with an epoxy compound.
[0023] The amine compound is an amine compound having one or more active hydrogen atoms, and examples include alkylenediamines such as ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,3-diaminobutane, 1,4-diaminobutane, and hexamethylenediamine; polyalkyl polyamines such as diethylenetriamine, triethylenetriamine, and tetraethylenepentamine; polyoxyalkylene polyamines such as polyoxypropylenediamine and polyoxypropylenetriamine; 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, 1,3-diaminomethylcyclohexane, 1,2-diaminocyclohexane, 1,4-diamino-3,6-diethylcyclohexane, 4,4'-diaminodicyclohexylmethane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 4,4'-diaminodicyclohexylpropane, bis(4-aminocyclohexyl)sulfone, and 4,4'-diamino Alicyclic polyamines such as nodicyclohexyl ether, 2,2'-dimethyl-4,4'-diaminodicyclohexylmethane, isophoronediamine, norbornenediamine; m-xylylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diethyltoluenediamine, 1-methyl-3,5-diethyl-2,4-diaminebenzene, 1-methyl-3,5-diethyl-2,6-diaminobenzene, 1,3,5-triethyl-2,6-diaminobenzene, 3, Aromatic polyamines such as 3'-diethyl-4,4'-diaminodiphenylmethane and 3,5,3',5'-tetramethyl-4,4'-diaminodiphenylmethane; guanamines such as benzoguanamine and acetoguanamine; dihydrazides such as oxalate dihydrazide, malonate dihydrazide, succinate dihydrazide, glutarate dihydrazide, adipic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacate dihydrazide, and phthalate dihydrazide;N,N-dimethylaminoethylamine, N,N-diethylaminoethylamine, N,N-diisopropylaminoethylamine, N,N-diallylaminoethylamine, N,N-benzylmethylaminoethylamine, N,N-dibenzylaminoethylamine, N,N-cyclohexylmethylaminoethylamine, N,N-dicyclohexylaminoethylamine, N-(2-aminoethyl)pyrrolidine, N-(2-aminoethyl)piperidine, N-(2-aminoethyl)morpholine, N-(2-aminoethyl)piperazine, N-(2-aminoethyl)-N'-methylpiperazine, N,N-dimethylaminopropylamine, N,N-diethylaminopropylamine, N,N-diisopropylaminopropylamine, N,N-diallylaminopropylamine, N,N-benzylmethylaminopropylamine, N,N-dibenzylaminopropylamine, N,N-cyclohexylmethylaminopropylamine, N,N-dicyclohexylaminopropylamine, N-(3-aminopropyl)pyrrolidine, N-(3-aminopropyl)piperidine, N-(3-aminopropyl)morpholine, N-(3-aminopropyl)piperazine, N-(3-aminopropyl)-N'-methylpiperidine, 4-(N,N-dimethylamino)benzylamine, 4-(N,N-diethylamino)benzylamine, 4-(N,N-diisopropylamino)benzylamine, N,N,-dimethylisophoronediamine, N,N-dimethylbisaminocyclohexane, N,N,N'-trimethylethylenediamine, N'-ethyl-N,N-dimethylethylenediamine, N,N,N'-trimethylethylenediamine, N'-ethyl-N,N-dimethylpropanediamine, N'-ethyl-N,N-dibenzyaminopropylamine;Examples include N,N-(bisaminopropyl)-N-methylamine, N,N-bisaminopropylethylamine, N,N-bisaminopropylpropylamine, N,N-bisaminopropylbutylamine, N,N-bisaminopropylpentylamine, N,N-bisaminopropylhexylamine, N,N-bisaminopropyl-2-ethylhexylamine, N,N-bisaminopropylcyclohexylamine, N,N-bisaminopropylbenzylamine, N,N-bisaminopropylallylamine, bis[3-(N,N-dimethylaminopropyl)]amine, bis[3-(N,N-diethylaminopropyl)]amine, bis[3-(N,N-diisopropylaminopropyl)]amine, bis[3-(N,N-dibutylaminopropyl)]amine, etc.
[0024] The active hydrogen equivalent of the amine compound is preferably between 10 and 300, and more preferably between 15 and 150, from the viewpoint of balancing curability and storage stability.
[0025] Among the aforementioned amine compounds, it is preferable to use one or more selected from aliphatic amines and alicyclic amines, in order to obtain excellent curing properties. Specifically, alkylenediamines such as ethylenediamine and 1,2-propylenediamine; polyalkylene polyamines such as diethylenetriamine and triethylenetetramine; polyoxyalkylene polyamines such as dioxypropylenediamine, polyoxypropylene polyamine and polyoxyethylene polyamine; and alicyclic amines such as isophoronediamine, 1,3-diaminomethylcyclohexane, and N-(2-aminoethyl)piperazine are particularly preferred. 1,2-propylenediamine, dioxypropylenediamine, and N-(2-aminoethyl)piperazine are especially preferred.
[0026] Examples of the epoxy compounds include polyglycidyl ether compounds of mononuclear polyvalent phenol compounds such as hydroquinone, resorcinol, pyrocatechol, and phloroglucinol; dihydroxynaphthalene, biphenol, methylenebisphenol (bisphenol F), methylenebis(orthocresol), ethylidenebisphenol, isopropylidenebisphenol (bisphenol A), isopropylidenebis(orthocresol), tetrabromobisphenol A, 1,3-bis(4-hydroxycumylbenzene), 1,4-bis(4-hydroxycumylbenzene), 1,1,3-tris(4-hydroxyphenyl)butane, 1,1,2,2-tetra(4-hydroxyphenyl)ethane, thiobisphenol, sulfonylbisphenol, oxybisphenol, phenol novolac, orthocresol novolac, ethylphenol novolac, butylphenol novolac, octylphenol novolac, resorcinol novolac, terpene phenol, and other polynuclear polyvalent phenols. Polyglycidyl ether compounds of polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, hexanediol, polyglycol, thiodiglycol, glycerin, trimethylolpropane, pentaerythritol, sorbitol, bisphenol A alkylene oxide adducts, etc.; maleic acid, fumaric acid, itaconic acid, succinic acid, glutaric acid, suberic acid, adipic acid, azelaic acid, sebacic acid, dimer acid, trimer acid, Glycidyl esters of aliphatic, aromatic, or alicyclic polybasic acids such as phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, trimesic acid, pyromellitic acid, tetrahydrophthalic acid, hexahydrophthalic acid, and endomethylenetetrahydrophthalic acid, and homopolymers or copolymers of glycidyl methacrylates; epoxy compounds having a glycidylamino group such as N,N-diglycidylaniline, bis(4-(N-methyl-N-glycidylamino)phenyl)methane, and diglycidyl orthotoluidine;Examples include epoxides of cyclic olefin compounds such as vinylcyclohexene diepoxide, dicyclopentanediene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-6-methylcyclohexanecarboxylate, and bis(3,4-epoxy-6-methylcyclohexylmethyl) adipate; epoxidized conjugated diene polymers such as epoxidized polybutadiene and epoxidized styrene-butadiene copolymers; and heterocyclic compounds such as triglycidyl isocyanurates.
[0027] The epoxy compound may be either a glycidyl-type epoxy compound or a cycloalkene oxide-type epoxy compound, such as an epoxidized cyclic olefin compound. Furthermore, if it is a glycidyl-type epoxy compound, it may be either an aromatic epoxy compound having an aromatic ring or an aliphatic epoxy compound without an aromatic ring. From the viewpoint of reactivity, a glycidyl-type epoxy compound is preferred, and from the viewpoint of heat resistance, a glycidyl-type aromatic epoxy compound is more preferred.
[0028] The aforementioned amine-based latent curing agent is obtained by reacting an amine compound with an epoxy compound, and it is preferable that the amount of epoxy compound reacted is such that the amount of epoxy groups in the epoxy compound is 0.1 to 0.9 equivalents, particularly 0.2 to 0.8 equivalents, for every 1 equivalent of active hydrogen in the amine compound. It is preferable to set the amount of epoxy compound relative to the amine compound to be above the lower limit, as this improves the storage stability of the curable resin composition, and it is preferable to set it to be below the upper limit, as this ensures that curability is obtained.
[0029] The method for producing the amine-based latent curing agent is not particularly limited, but one possible method is to use a solvent as needed and react the agent under heating at room temperature to 140°C for 1 to 10 hours. If a solvent is used, the solvent can be removed after the reaction is complete by heating under atmospheric pressure or reduced pressure.
[0030] Solvents used in the production of the amine-based latent curing agent include ketones such as methyl ethyl ketone, methyl amyl ketone, diethyl ketone, acetone, methyl isopropyl ketone, propylene glycol monomethyl ether acetate, and cyclohexane; ethers such as tetrahydrofuran, 1,2-dimethoxyethane, 1,2-diethoxyethane, and propylene glycol monomethyl ether; esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated aliphatic hydrocarbons such as carbon tetrachloride, chloroform, trichloroethylene, and methylene chloride; and halogenated aromatic hydrocarbons such as chlorobenzene.
[0031] The latent curing agent, which is component (C) used in this invention, is preferably further enriched with a phenolic resin, as this can improve its stability.
[0032] Examples of the phenol resins include polyhydric phenol compounds such as phenol novolac resins, cresol novolac resins, aromatic hydrocarbon formaldehyde resin-modified phenol resins, dicyclopentadienephenol addition resins, phenol aralkyl resins (Zyloc resins), naphthol aralkyl resins, trisphenylol methane resins, tetraphenylolethane resins, naphthol novolac resins, naphthol-phenol cocondensed novolac resins, naphthol-cresol cocondensed novolac resins, biphenyl-modified phenol resins (polyhydric phenol compounds in which the phenol core is linked by a bismethylene group), biphenyl-modified naphthol resins (polyhydric naphthol compounds in which the phenol core is linked by a bismethylene group), aminotriazine-modified phenol resins (compounds having a phenol skeleton, a triazine ring, and a primary amino group in their molecular structure), and alkoxy-group-containing aromatic ring-modified novolac resins (polyhydric phenol compounds in which the phenol core and alkoxy-group-containing aromatic ring are linked by formaldehyde).
[0033] In the present invention, from the viewpoint of obtaining a curable resin composition with an excellent balance between storage stability and curability, it is preferable to use a phenolic resin with a softening point of 50 to 200°C.
[0034] The amount of phenol resin used is preferably 10 to 100 parts by mass, and particularly preferably 20 to 60 parts by mass, per 100 parts by mass of the amine-based latent curing agent. Using 10 parts by mass or more provides sufficient curability, while using 100 parts by mass or less is preferable because it more reliably avoids a decrease in the physical properties of the cured product.
[0035] If the latent curing agent, which is component (C) used in this invention, is a solid, it may be used after being pulverized using a pulverizer such as a jet mill.
[0036] The latent curing agent may contain other latent curing agents besides the amine-based latent curing agent and phenolic resin. Examples of other latent curing agents include dibasic acid dihydrazides such as oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacate acid dihydrazide, and phthalic acid dihydrazide; guanidine compounds such as dicyandiamide, benzoguanamine, and acetoguanamine; melamine; and modified amines such as dehydration condensates of amines and carboxylic acids, adducts of amines and isocyanates, Michael adducts of amines, Mannich reaction products of amines, condensates of amines and urea, and condensates of amines and ketones. However, when using these, it is desirable that their content in the latent curing agent does not exceed 50% by mass, as this may reduce conductivity.
[0037] The content of the latent curing agent, which is component (C), is not particularly limited, but for reasons of reactivity and one-component stability, it is preferably 1 to 70 parts by mass, and more preferably 3 to 60 parts by mass, per 100 parts by mass of the total amount of the cyanate ester resin (component (A)) and the epoxy resin (component (B)).
[0038] The conductive filler, which is component (D) used in the present invention, can be any material that is conductive, such as metal particles such as gold, silver, nickel, copper, and solder; metal oxides such as tin oxide, indium oxide, and zinc oxide; and carbon-based materials such as carbon black, graphite, carbon nanotubes, and carbon fibers. Furthermore, materials such as nonmetallic glass, ceramics, and plastics coated with the conductive layer can also be used. From the viewpoint of having excellent ease of penetration into gaps and meltability, and sufficient conductivity imparting effect, the average particle size of these materials is preferably 0.1 to 50 μm, and particularly preferably 0.5 to 30 μm. The average particle size is measured using a particle size distribution analyzer that measures by laser diffraction. Furthermore, the particle shape can be spherical, flattened, plate-like, flake-like, flaky, rod-like, dendritic, fibrous, needle-like, scaly, angular, or polyhedral, but is not particularly limited.
[0039] (D) The content of the conductive filler, which is component D, is preferably 30 to 90% by mass in the curable resin composition, and particularly preferably 50 to 80% by mass, from the viewpoint of providing sufficient conductivity.
[0040] Furthermore, in a system in which epoxy resin and cyanate ester resin are combined with a latent curing agent containing active hydrogen obtained by reacting an amine compound and an epoxy compound, and a conductive filler, localization of the conductive filler occurs in the cured product (see SEM images in Figures 1 to 4), and it is thought that conductivity is improved by the formation and increase of conductive paths. Localization is not observed when cyanate ester resin is not used or when an amine-based latent curing agent without active hydrogen is used.
[0041] In the present invention, known curing accelerators may be used in combination as needed. Specific examples of these curing accelerators include phosphines such as triphenylphosphine; phosphonium salts such as tetraphenylphosphonium bromide; imidazoles such as 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, and 1-cyanoethyl-2-methylimidazole; imidazole salts which are salts of the aforementioned imidazoles with trimellitic acid, isocyanuric acid, boron, etc.; benzyldimethylamine, 2,4,6-tris Examples of curing accelerators include amines such as (dimethylaminomethyl)phenol; quaternary ammonium salts such as trimethylammonium chloride; ureas such as 3-(p-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-phenyl-1,1-dimethylurea, isophorone diisocyanate-dimethylurea, and tolylene diisocyanate-dimethylurea; and complex compounds of boron trifluoride with amines or ether compounds. These curing accelerators may be used alone or in combination of two or more. There are no particular restrictions on the content of the curing accelerators, and they can be set appropriately depending on the application.
[0042] The curable resin composition of the present invention may contain various additives as needed. Additives include: phenolic compounds such as biphenol; reactive diluents such as p-tert-butylglycidyl ether, n-butylglycidyl ether, and C12-13 mixed alcohol glycidyl ether; non-reactive diluents (plasticizers) such as dioctyl phthalate, dibutyl phthalate, benzyl alcohol, and coal tar; silica such as fused silica and crystalline silica; powders such as aluminum oxide (alumina), magnesium oxide, zinc oxide, magnesium hydroxide, aluminum hydroxide, aluminum nitride, silicon nitride, boron nitride, zinc molybdate, calcium carbonate, silicon carbonate, calcium silicate, potassium titanate, beryllia, zirconia, zircon, fossilite, steatite, spinel, mullite, titania, etc., or beads formed from these; and fillers such as glass fibers, pulp fibers, synthetic fibers, and ceramic fibers; reinforcing materials such as glass cloth, aramid cloth, and carbon fiber; pigments; and γ-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyl Ropiltriethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltriethoxysilane, γ-anilinopropyltriethoxysilane, γ-glycidoxypropyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, vinyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-chloropropyl Common additives include silane coupling agents such as dimethoxysilane and γ-mercaptopropyltrimethoxysilane; lubricants such as candelilla wax, carnauba wax, wood wax, privet wax, beeswax, lanolin, whale wax, montan wax, petroleum wax, aliphatic wax, aliphatic ester, aliphatic ether, aromatic ester, and aromatic ether; thickeners; thixotropic agents; antioxidants; light stabilizers; ultraviolet absorbers; defoamers; rust inhibitors; and colloidal silica and colloidal alumina. Furthermore, adhesive resins such as xylene resin and petroleum resin can also be used in combination.
[0043] When curing the curable resin composition of the present invention, heating at, for example, 80 to 200°C is preferable in order to exhibit the physical properties of the cured product.
[0044] The curable resin composition of the present invention can be used as an adhesive in a wide range of applications. In particular, because the cured product has excellent conductivity, it can be suitably used in electronic applications such as semiconductor encapsulation and adhesives for electronic components. [Examples]
[0045] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited in any way by these examples.
[0046] [Manufacturing Example 1] (Synthesis of latent curing agent EH-1) 201 g of 1,2-diaminopropane was placed in a flask and heated to 60°C. Then, 580 g of Adekarezin EP-4100E (a product name of ADEKA Corporation; a bisphenol A type epoxy resin with an epoxy equivalent of 190) [epoxy equivalent of Adekarezin EP-4100E per mole of 1,2-diaminopropane: 1.12] was added little by little while maintaining the system temperature at 100-110°C. After all of the Adekarezin EP-4100E had been added, the reaction system was heated to 140°C and reacted for 1.5 hours to obtain an amine-based latent curing agent containing active hydrogen. Next, 30 g of MP-800K (manufactured by Asahi Organic Chemicals Co., Ltd.; phenolic resin, softening point 100°C) was added to 100 g of the obtained amine-based latent curing agent containing active hydrogen. Unreacted materials and solvent were removed by degassing under reduced pressure for 1 hour at 180-190°C and 30-40 Tor, and the mixture was pulverized using a jet mill to obtain the latent curing agent (EH-1).
[0047] [Manufacturing Example 2] (Synthesis of latent curing agent EH-2) 352 g of isophorone diamine was placed in a flask and heated to 60°C. Then, 580 g of Adekarezin EP-4100E (a product name of ADEKA Corporation; a bisphenol A type epoxy resin with an epoxy equivalent of 190) [epoxy equivalent of Adekarezin EP-4100E per mole of isophorone diamine: 1.47] was added little by little while maintaining the system temperature at 100-110°C. After all of the Adekarezin EP-4100E had been added, the reaction system was heated to 140°C and reacted for 1.5 hours to obtain an amine-based latent curing agent containing active hydrogen. Next, 30 g of MP-800K (manufactured by Asahi Organic Chemicals Co., Ltd.; phenolic resin, softening point 100°C) was added to 100 g of the obtained amine-based latent curing agent containing active hydrogen. Unreacted materials and solvent were removed by degassing under reduced pressure for 1 hour at 180-190°C and 30-40 Tor, and the mixture was pulverized using a jet mill to obtain the latent curing agent (EH-2).
[0048] [Manufacturing Example 3] (Synthesis of latent curing agent EH-3) 190 g of 2-ethyl-4-methylimidazole was placed in a flask and heated to 60°C. Then, 409 g of Adekarezin EP-4100E (a product name of ADEKA Corporation; a bisphenol A type epoxy resin with an epoxy equivalent of 190) [active hydrogen equivalent of 2-ethyl-4-methylimidazole: epoxy equivalent of the aforementioned Adekarezin EP-4100E; 1:1.24] was added little by little while maintaining the system temperature at 100-110°C. After all of the Adekarezin EP-4100E had been added, the reaction system was heated to 140°C and reacted for 1.5 hours to obtain a modified imidazole that did not contain active hydrogen. Next, 30 g of MP-800K (manufactured by Asahi Organic Chemicals Co., Ltd.; phenolic resin, softening point 100°C) was added to 100 g of the obtained modified imidazole, and unreacted material and solvent were removed by vacuum degassing under conditions of 180-190°C and 30-40 Tor for 1 hour. The mixture was then pulverized using a jet mill to obtain a latent curing agent (EH-3).
[0049] [Examples 1-4 and Comparative Examples 1-3] Resin compositions were prepared by mixing each component according to the formulations listed in Table 1 below, and the following tests were conducted. The evaluation results are shown in Table 1 below. Note that the values for the formulations listed in Table 1 represent parts by mass.
[0050] [Table 1]
[0051] EP-1: EP-4901E (Bisphenol F type epoxy resin) manufactured by ADEKA Corporation EP-2: ED-509S (4-tert-butylphenylglycidyl ether) manufactured by ADEKA Corporation CY-1: LECy (Bisphenol-type cyanate ester resin) manufactured by Lonza Corporation EH-1: Latent curing agent (EH-1) manufactured in manufacturing example 1 EH-2: Latent curing agent (EH-2) manufactured in manufacturing example 2 EH-3: Latent curing agent (EH-3) manufactured in manufacturing example 3 EH-4: Dicyandiamide KBM-403: KBM-403 (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd. Ag-1: Flattened silver particles with an average particle size of 4.8 μm. Ag-2: Spherical silver particles with an average particle size of 0.9 μm. Ag-3: Dendritic electrolytic silver powder with average particle size of 1.0μm Ag / Cu-1: Flattened silver-plated copper powder with an average particle size of 6.0 μm.
[0052] <Conductive> The curable resin compositions of the examples and comparative examples were applied to a glass plate using a barcode method to a thickness of 100 to 300 μm. The films were heated in a circulating constant temperature bath maintained at 150°C for 30 minutes to cure. The thickness of the resulting cured film was measured, and the volume resistivity was measured to evaluate its conductivity. The volume resistivity (Ω·cm) was calculated using a 4-terminal 4-probe resistivity meter (Loresta GPMPC-T610, manufactured by Mitsubishi Chemical Analytec Co., Ltd.). The resistance value is 1.0 × 10 -2Those with a resistivity of Ω·cm or less were designated as A, and those with a resistivity of 1.0×10 -2 Ω·cm were designated as B.
[0053] <Gel Time> The temperature of a hot plate was set to 150±2°C, approximately 1 g of the curable compositions of the Examples and Comparative Examples were placed on the hot plate, and the time until stirring became impossible while stirring (gel time) was measured. Those with a gel time of less than 10 seconds were designated as A, and those with a gel time of 10 seconds or more were designated as B.
[0054] <SEM Image> For the cured products obtained from the curable resin compositions of the Examples and Comparative Examples, the cured coating film on a glass plate was observed using SEM. Figure 1 is an image of the cured product of Example 1 magnified 4000 times, Figure 2 is an image of the cured product of Comparative Example 3 magnified 4000 times, Figure 3 is an image of the cured product of Example 2 magnified 2000 times, and Figure 4 is an image of the cured product of Comparative Example 1 magnified 2000 times. By comparing Figure 1 and Figure 2, and Figure 3 and Figure 4, respectively, it is considered that in Examples 1 and 2, localization of silver was observed, conductive paths were formed, and conductivity was improved. Figure 5 is an image of the cured product of Example 3 magnified 2000 times, and localization of silver was observed as in Examples 1 and 2.
[0055] As shown by the Examples, the curable resin composition of the present invention is a curable resin composition from which a cured product having excellent conductivity and curability can be obtained. [Industrial Applicability]
[0056] According to the present invention, since it is possible to provide a curable resin composition from which a cured product having particularly excellent conductivity can be obtained, it can be suitably used for conductive materials such as, for example, solder replacement materials.
Claims
1. A curable resin composition containing (A) a cyanate ester resin, (B) an epoxy resin, (C) an amine-based latent curing agent having active hydrogen obtained by reacting an amine compound with an epoxy compound, and a latent curing agent containing a guanidine compound, and (D) a conductive filler.
2. The curable resin composition according to claim 1, wherein the cyanate ester resin, which is component (A), is one or more selected from polymers of compounds represented by the following formula (1) and compounds represented by the following formula (2), and at least one compound selected from these. 【Chemistry 1】 (In the formula, Y 1 This indicates an unsubstituted or divalent hydrocarbon group substituted with a fluorine atom or a cyanate group, or -O-, -S-, or a single bond, A 1 and A 2 Each of these independently represents an unsubstituted or phenylene group substituted with 1 to 4 alkyl groups. 【Chemistry 2】 (In the formula, m is an integer greater than or equal to 1, and Y 2 and Y 3 Each independently represents either -S- or an unsubstituted or divalent hydrocarbon group substituted with a fluorine atom or a cyanate group, R 1 , R 2 and R 3 Each of these independently represents an alkyl group having 1 to 4 carbon atoms, and each of these independently represents an integer from 0 to 2.
3. Y in the formula (1) 1 , and Y in the formula (2) 2 and Y 3 are each independently one or more selected from the following formulas (Y-1) to (Y-9), the curable resin composition according to claim 2. 【Transformation 3】 (In the formula, n is an integer from 4 to 12, R 7 and R 8 Each of these independently represents a hydrogen atom or a methyl group that is unsubstituted or substituted with a fluorine atom. * represents a bond.
4. The curable resin composition according to claim 1, wherein the amine compound in component (C) is one or more selected from aliphatic amines and alicyclic amines.
5. The curable resin composition according to claim 1, wherein the latent curing agent, which is component (C), further contains a phenolic resin.
6. The curable resin composition according to claim 1, wherein the conductive filler component (D) is one or more selected from silver particles and copper particles.
7. The curable resin composition according to claim 1, wherein the particle size of the conductive filler, which is component (D), is 0.1 to 50 μm.
8. The curable resin composition according to claim 1, wherein the content of the conductive filler, which is component (D), is 30 to 90% by mass in the curable resin composition.
9. A cured product obtained by curing a curable resin composition according to any one of claims 1 to 8.
10. An adhesive comprising a curable resin composition as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Curable epoxy resin composition
JP1987265323A
Adhesive composition and connection member consisting of the composition
JP1997279121A
Conductive resin paste
JP1999134940A
Anisotropic electroconductive adhesive
JP2004352785A
Thermosetting resin composition containing modified polyimide resin
JP2006037083A