Memory device

The semiconductor device design addresses miniaturization and integration challenges by employing a layered structure with oxide semiconductors and capacitive elements, achieving improved performance and efficiency in oxide semiconductor devices.

JP7955300B2Active Publication Date: 2026-11-24SEMICON ENERGY LAB CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023579876
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-10
Filing Date
2023-01-30
Publication Date
2026-11-24
Estimated Expiration
2043-01-30

AI Technical Summary

Technical Problem

Existing semiconductor devices face challenges in miniaturization, integration, operating speed, electrical variability, reliability, on-current, power consumption, and manufacturing complexity, particularly in the context of oxide semiconductor-based transistors and memory devices.

Method used

A semiconductor device design incorporating a memory cell with a transistor and capacitive element, featuring multiple insulator and conductor layers, including oxide semiconductors, to create a compact and efficient structure with overlapping conductors and openings, allowing for high integration and reduced manufacturing steps.

Benefits of technology

The design enables miniaturization, high integration, improved operating speed, reduced electrical variability, enhanced reliability, increased on-current, lower power consumption, and simplified manufacturing processes, while maintaining good electrical characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955300000001
    Figure 0007955300000001
  • Figure 0007955300000002
    Figure 0007955300000002
  • Figure 0007955300000003
    Figure 0007955300000003
Patent Text Reader

Abstract

Provided is a storage device that enables miniaturization or high integration. Provided is a storage device comprising a memory cell which includes a transistor and a capacitive element, a first insulator, a second insulator on the first insulator, and a third insulator on the second insulator, the transistor includes an oxide on the first insulator, a first conductor and a second conductor on the oxide, a fourth insulator on the oxide, and a third conductor on the fourth insulator, the second insulator has a first opening, the fourth insulator and the third conductor are arranged in the first opening, the second insulator and the third insulator have a second opening, the capacitive element includes, in the second opening, a fourth conductor in contact with the upper surface of the second conductor, a fifth insulator on the fourth conductor, and a fifth conductor on the fifth insulator, the second insulator has a third opening, the first insulator has a fourth opening, the third insulator has a fifth opening, the third opening overlaps at least a part of the fourth opening and at least a part of the fifth opening in a plan view, a sixth conductor and a part of the first conductor are arranged in the third opening, and the sixth conductor has a region in contact with a part of the upper surface and a part of a side surface of the first conductor.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] One aspect of the present invention relates to transistors, semiconductor devices, memory devices, and electronic devices. Alternatively, one aspect of the present invention relates to a method for manufacturing semiconductor devices. Alternatively, one aspect of the present invention relates to semiconductor wafers and modules.

[0002] In this specification, the term "semiconductor device" refers to any device that can function by utilizing semiconductor properties. Semiconductor elements such as transistors, as well as semiconductor circuits, computing devices, and memory devices, are all forms of semiconductor devices. Display devices (such as liquid crystal displays and light-emitting displays), projection devices, lighting devices, electro-optical devices, energy storage devices, memory devices, semiconductor circuits, imaging devices, and electronic devices may also be considered to have semiconductor devices.

[0003] Furthermore, one aspect of the present invention is not limited to the above-mentioned technical field. One aspect of the invention disclosed herein relates to a product, a method, or a method of manufacture. Another aspect of the present invention relates to a process, a machine, a manufacture, or a composition of matter. [Background technology]

[0004] In recent years, the development of semiconductor devices has progressed, with LSIs, CPUs, and memory being the main components used in semiconductor devices. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memory) formed on chips by processing semiconductor wafers, and electrodes that serve as connection terminals are formed on them.

[0005] Semiconductor circuits (IC chips) such as LSIs, CPUs, and memory are mounted on circuit boards, such as printed circuit boards, and used as components in various electronic devices.

[0006] Furthermore, the technology of constructing transistors using semiconductor thin films formed on substrates with insulating surfaces is attracting attention. These transistors are widely applied in electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors are attracting attention as other materials.

[0007] Furthermore, transistors using oxide semiconductors are known to have extremely low leakage current in the non-conductive state. For example, Patent Document 1 discloses a low-power CPU that utilizes the low leakage current characteristic of transistors using oxide semiconductors. Also, for example, Patent Document 2 discloses a memory device that can retain its contents for a long period of time by utilizing the low leakage current characteristic of transistors using oxide semiconductors.

[0008] Furthermore, in recent years, with the miniaturization and weight reduction of electronic devices, there has been a growing demand for even higher density integrated circuits. There is also a need to improve the productivity of semiconductor devices, including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technology for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide multiple superimposed memory cells. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 2012-257187 [Patent Document 2] Japanese Patent Publication No. 2011-151383 [Patent Document 3] International Publication No. 2021 / 053473 [Non-patent literature]

[0010] [Non-Patent Document 1] M.Oota et.al, “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech.Dig., 2019, pp.50-53 [Overview of the Initiative] [Problems that the invention aims to solve]

[0011] One aspect of the present invention aims to provide a semiconductor device that can be miniaturized or highly integrated. Alternatively, it aims to provide a semiconductor device with a high operating speed. Alternatively, it aims to provide a semiconductor device with good electrical characteristics. Alternatively, it aims to provide a semiconductor device with little variation in the electrical characteristics of transistors. Alternatively, it aims to provide a semiconductor device with good reliability. Alternatively, it aims to provide a semiconductor device with a large on-current. Alternatively, it aims to provide a semiconductor device with low power consumption. Alternatively, it aims to provide a novel semiconductor device. Alternatively, it aims to provide a method for manufacturing a semiconductor device with a reduced number of manufacturing steps. Alternatively, it aims to provide a memory device having a novel semiconductor device.

[0012] Furthermore, the description of these problems does not preclude the existence of other problems. Moreover, one aspect of the present invention does not need to solve all of these problems. Other problems will naturally become apparent from the description in the specification, drawings, and claims, and it is possible to extract other problems from the description in the specification, drawings, and claims. [Means for solving the problem]

[0013] One aspect of the present invention includes a memory cell having a transistor and a capacitive element, a first insulator, a second insulator on the first insulator, and a third insulator on the second insulator, wherein the transistor has an oxide on the first insulator, a first conductor and a second conductor on the oxide, a fourth insulator on the oxide, and a third conductor on the fourth insulator, wherein the second insulator is arranged on the first conductor and the second conductor, the third insulator is arranged on the third conductor and the second insulator, the second insulator has a first opening having a region overlapping with the oxide, the fourth insulator and the third conductor are arranged within the first opening, and the second insulator and the third insulator have a second conductor A memory device having a second opening that overlaps with the electric body, the capacitive element having a fourth conductor in contact with the upper surface of the second conductor, a fifth insulator on the fourth conductor, and a fifth conductor on the fifth insulator, the fourth conductor, the fifth insulator, and the fifth conductor arranged within the second opening, the second insulator having a third opening, the first insulator having a fourth opening, the third insulator having a fifth opening, the third opening overlapping with at least a part of the fourth opening and at least a part of the fifth opening in a plan view, a sixth conductor and a part of the first conductor arranged within the third opening, the sixth conductor having a region in contact with a part of the upper surface and a part of the side surface of the first conductor.

[0014] Another aspect of the present invention relates to a memory cell having a transistor and a capacitive element, comprising a plurality of layers including a first insulator, a second insulator on the first insulator, and a third insulator on the second insulator, wherein the plurality of layers are stacked, and the transistor comprises an oxide on the first insulator, a first conductor and a second conductor on the oxide, a fourth insulator on the oxide, and a third conductor on the fourth insulator, wherein the second insulator is arranged on the first conductor and the second conductor, the third insulator is arranged on the third conductor and the second insulator, the second insulator has a first opening having a region overlapping with the oxide, the fourth insulator and the third conductor are arranged within the first opening, and the second insulator and the third The insulator has a second opening that overlaps with the second conductor, and the capacitive element has a fourth conductor in contact with the upper surface of the second conductor, a fifth insulator on the fourth conductor, and a fifth conductor on the fifth insulator, and the fourth conductor, the fifth insulator, and the fifth conductor are arranged within the second opening, the second insulator has a third opening, the first insulator has a fourth opening, the third insulator has a fifth opening, the third opening overlaps with at least a part of the fourth opening and at least a part of the fifth opening in a plan view, and a sixth conductor and a part of the first conductor are arranged within the third opening, the sixth conductor has a region that is in contact with a part of the upper surface and a part of the side surface of the first conductor, thus forming a memory device.

[0015] In the above-mentioned memory device, it is preferable that a drive circuit is provided, and that the multiple layers are stacked on top of the drive circuit. Furthermore, in the above-mentioned memory device, it is preferable that a functional layer having a functional circuit and wiring are provided, the functional layer is provided between the substrate on which the drive circuit is provided and the multiple layers, the wiring has the function of electrically connecting the drive circuit and the functional circuit, and the functional circuit has a gate that has a second transistor electrically connected to a sixth conductor electrically connected to a memory cell, and has the function of transmitting a signal to the wiring according to the potential of the sixth conductor.

[0016] Furthermore, in the above-mentioned storage device, it is preferable that a sixth insulator is placed below the first insulator, the sixth insulator has a sixth opening, and the third opening overlaps with at least a portion of the sixth opening in a plan view.

[0017] Furthermore, in the above-mentioned storage device, it is preferable that the third opening is located inside the fourth opening, inside the fifth opening, and inside the sixth opening in a plan view.

[0018] Furthermore, in the above-mentioned storage device, the fourth, fifth, and sixth openings may be configured to be located inside the third opening in a plan view.

[0019] Furthermore, in the above-mentioned storage device, it is preferable that the first insulator has hafnium oxide. Furthermore, in the above-mentioned storage device, it is preferable that the third insulator and the sixth insulator have aluminum oxide.

[0020] Furthermore, in the above-mentioned storage device, it is preferable that the fourth insulator has regions that are in contact with the upper surface and side surface of the oxide, and with the side wall of the first opening of the second insulator.

[0021] Furthermore, in the above-mentioned storage device, it is preferable that the first conductor and the second conductor are in contact with the upper surface and side surface of the oxide, respectively.

[0022] Furthermore, in the above-mentioned storage device, it is preferable that a portion of the fourth conductor, a portion of the fifth insulator, and a portion of the fifth conductor are located above the upper surface of the third conductor.

[0023] Furthermore, in the above-mentioned storage device, it is preferable that the fourth conductor has a region that is in contact with the side wall of the second opening of the second insulator.

[0024] Furthermore, in the above-mentioned storage device, it is preferable that, at the third opening, the side surface of the first conductor protrudes from the side surface of the second insulator.

[0025] Furthermore, in the above-mentioned storage device, it is preferable that the third insulator is positioned in contact with the upper surface of the second insulator and the upper surface of the third conductor, and that a part of the fourth conductor and a part of the fifth insulator are in contact with the upper surface of the third insulator. [Effects of the Invention]

[0026] One aspect of the present invention can provide a semiconductor device that can be miniaturized or highly integrated. Alternatively, it can provide a semiconductor device with a high operating speed. Alternatively, it can provide a semiconductor device with good reliability. Alternatively, it can provide a semiconductor device with little variation in the electrical characteristics of transistors. Alternatively, it can provide a semiconductor device with good electrical characteristics. Alternatively, it can provide a semiconductor device with a large on-current. Alternatively, it can provide a semiconductor device with low power consumption. Alternatively, it can provide a novel semiconductor device. Alternatively, it can provide a method for manufacturing a semiconductor device with a reduced number of manufacturing steps. Alternatively, it can provide a memory device having a novel semiconductor device.

[0027] Furthermore, the description of these effects does not preclude the existence of other effects. Moreover, one embodiment of the present invention does not need to possess all of these effects. Other effects will naturally become apparent from the description in the specification, drawings, and claims, and it is possible to extract other effects from the description in the specification, drawings, and claims. [Brief explanation of the drawing]

[0028] Figure 1A is a top view of a semiconductor device according to one embodiment of the present invention. Figures 1B to 1D are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figure 2 is a circuit diagram illustrating the configuration of a storage device according to one aspect of the present invention. Figures 3A to 3C are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figures 4A and 4B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figures 5A and 5B are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figures 6A to 6C are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figure 7A is a cross-sectional view of a semiconductor device according to one aspect of the present invention. Figure 7B is a top view of a semiconductor device according to one aspect of the present invention. Figure 8A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 8B to 8D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 9A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 9B to 9D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 10A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 10B to 10D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 11A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 11B to 11D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 12A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 12B to 12D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 13A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 13B to 13D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 14A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 14B to 14D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 15A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 15B to 15D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 16A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 16B to 16D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 17A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 17B to 17D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 18A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 18B to 18D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 19A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 19B to 19D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 20A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 20B to 20D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 21A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 21B to 21D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 22A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 22B to 22D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 23A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 23B to 23D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 24A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 24B to 24D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 25A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 25B to 25D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 26A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 26B to 26D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 27A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 27B to 27D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 28A is a top view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figures 28B to 28D are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention. Figure 29 is a top view illustrating a microwave processing apparatus according to one aspect of the present invention. Figure 30 is a cross-sectional view illustrating a microwave apparatus according to one aspect of the present invention. Figure 31 is a cross-sectional view illustrating a microwave processing apparatus according to one aspect of the present invention. Figure 32 is a cross-sectional view illustrating a microwave processing apparatus according to one aspect of the present invention. Figure 33A is a top view of a semiconductor device according to one embodiment of the present invention. Figures 33B to 33D are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figure 34A is a top view of a semiconductor device according to one embodiment of the present invention. Figures 34B to 34D are cross-sectional views of a semiconductor device according to one embodiment of the present invention. Figure 35A is a cross-sectional view of a semiconductor device according to one aspect of the present invention. Figure 35B is a top view of a semiconductor device according to one aspect of the present invention. Figures 36A and 36B are cross-sectional views of a semiconductor device according to one aspect of the present invention. Figure 37 is a cross-sectional view of a semiconductor device according to one aspect of the present invention. Figure 38 is a cross-sectional view of a semiconductor device according to one aspect of the present invention. Figure 39 is a block diagram illustrating an example of a storage device configuration. Figures 40A and 40B are schematic diagrams and circuit diagrams illustrating example configurations of storage devices. Figures 41A and 41B are schematic diagrams illustrating an example of a storage device configuration. Figure 42 is a circuit diagram illustrating an example of a memory device configuration. Figure 43 is a timing chart illustrating an example of a storage device configuration. Figures 44A and 44B are circuit diagrams illustrating an example of a memory device configuration. Figures 45A and 45B are circuit diagrams illustrating an example of a memory device configuration. Figures 46A and 46B are layout diagrams illustrating the configuration of a storage device according to one aspect of the present invention. Figure 47 is a cross-sectional view showing the configuration of a storage device according to one aspect of the present invention. Figure 48 is a cross-sectional view showing the configuration of a storage device according to one aspect of the present invention. Figure 49 is a layout diagram illustrating the configuration of a storage device according to one aspect of the present invention. Figures 50A and 50B are schematic diagrams of a semiconductor device according to one embodiment of the present invention. Figures 51A and 51B illustrate an example of an electronic component. Figures 52A to 52E are schematic diagrams of a storage device according to one embodiment of the present invention. Figures 53A to 53H show an electronic device according to one embodiment of the present invention. Figure 54 shows an example of space equipment. [Modes for carrying out the invention]

[0029] The embodiments will be described below with reference to the drawings. However, it will be readily apparent to those skilled in the art that the embodiments can be implemented in many different ways, and their form and details can be modified in various ways without departing from the spirit and scope. Therefore, the present invention is not to be construed as being limited to the following embodiments.

[0030] Furthermore, in drawings, size, layer thickness, or area may be exaggerated for clarity. Therefore, they are not necessarily limited to that scale. Also, the drawings are schematic representations of ideal examples and are not limited to the shapes or values ​​shown in the drawings. For example, in the actual manufacturing process, layers or resist masks may be unintentionally reduced due to processes such as etching, but this may not be reflected in the drawings for ease of understanding. In addition, in drawings, the same reference numerals may be used in common across different drawings for the same part or parts with similar functions, and repeated explanations may be omitted. Also, when referring to similar functions, the hatch patterns may be the same, and no specific reference numeral may be assigned.

[0031] Furthermore, in particular, in top views (also called "plan views") or perspective views, descriptions of some components may be omitted to facilitate understanding of the invention. Also, descriptions of some hidden lines may be omitted.

[0032] Furthermore, the ordinal numbers used in this specification, such as "first," "second," etc., are for convenience only and do not indicate the order of processes or stacking. Therefore, for example, "first" can be replaced with "second" or "third," etc., as appropriate in the explanation. Also, the ordinal numbers described in this specification may not be the same as the ordinal numbers used to specify an aspect of the present invention.

[0033] Furthermore, in this specification, terms indicating placement, such as "above" and "below," are used for convenience to explain the positional relationships between components with reference to the drawings. The positional relationships between components change as appropriate depending on the direction in which each component is depicted. Therefore, the terms used are not limited to those described in the specification and can be appropriately rephrased depending on the situation.

[0034] For example, in this specification, "X and Y are connected" means that X and Y are electrically connected. Here, "X and Y are electrically connected" means a connection in which electrical signals can be transmitted between X and Y when an object (such as a switch, transistor, or diode, or a circuit including such an object and wiring) is present between X and Y. Note that "X and Y are electrically connected" includes cases where X and Y are directly connected. Here, "X and Y are directly connected" means a connection in which electrical signals can be transmitted between X and Y via wiring (or electrodes) without the need for the aforementioned object. In other words, a direct connection means a connection that can be considered as the same circuit diagram when represented by an equivalent circuit.

[0035] Furthermore, in this specification, a transistor is defined as an element having at least three terminals, including a gate, a drain, and a source. It also has a region where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode) (hereinafter also referred to as the channel-forming region), and current can flow between the source and the drain through the channel-forming region. In this specification, the channel-forming region refers to the region through which current primarily flows.

[0036] Furthermore, the functions of the source or drain may be reversed when transistors of different polarities are used, or when the direction of current changes during circuit operation. For this reason, the terms source and drain may be used interchangeably in this specification.

[0037] The channel length refers to the distance between the source (source region or source electrode) and the drain (drain region or drain electrode) in the region where the semiconductor (or the part of the semiconductor through which current flows when the transistor is ON) and the gate electrode overlap, or in the channel formation region, as seen in a top view of a transistor. It should be noted that the channel length is not necessarily the same in all regions of a single transistor. That is, the channel length of a single transistor may not be a single fixed value. Therefore, in this specification, the channel length is defined as any one value, maximum value, minimum value, or average value in the channel formation region.

[0038] Channel width refers to the length of the channel formation region perpendicular to the channel length direction, for example, in a top view of a transistor, where the semiconductor (or the part of the semiconductor through which current flows when the transistor is ON) and the gate electrode overlap, or within the channel formation region. Note that the channel width is not necessarily the same across all regions in a single transistor. That is, the channel width of a single transistor may not be a single fixed value. Therefore, in this specification, the channel width is defined as any one value, maximum value, minimum value, or average value within the channel formation region.

[0039] In this specification, depending on the transistor structure, the channel width in the region where the channel is actually formed (hereinafter also referred to as the "effective channel width") may differ from the channel width shown in the top view of the transistor (hereinafter also referred to as the "apparent channel width"). For example, when the gate electrode covers the side surface of the semiconductor, the effective channel width may become larger than the apparent channel width, and this effect may not be negligible. For example, in a miniature transistor where the gate electrode covers the side surface of the semiconductor, the proportion of the channel formation region formed on the side surface of the semiconductor may be large. In that case, the effective channel width will be larger than the apparent channel width.

[0040] In such cases, it can be difficult to estimate the effective channel width through actual measurements. For example, estimating the effective channel width from design values ​​requires the assumption that the semiconductor shape is known. Therefore, if the semiconductor shape is not precisely known, it is difficult to accurately measure the effective channel width.

[0041] In this specification, when simply referred to as "channel width," it may refer to the apparent channel width. Alternatively, when simply referred to as "channel width," it may refer to the effective channel width. Note that channel length, channel width, effective channel width, or apparent channel width can be determined, for example, by analyzing cross-sectional TEM images.

[0042] Impurities in semiconductors refer to elements other than the main components that make up the semiconductor. For example, elements with a concentration of less than 0.1 atomic percent can be considered impurities. The presence of impurities can cause, for example, an increase in the defect level density of the semiconductor or a decrease in crystallinity. In the case of oxide semiconductors, impurities that alter the properties of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of oxide semiconductors, such as hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Water can also function as an impurity. Furthermore, for example, the inclusion of impurities can cause oxygen vacancies (V) in oxide semiconductors. O (Also known as an oxygen vacancy) may form.

[0043] In this specification, silicon oxide nitride refers to a material whose composition contains more oxygen than nitrogen. Similarly, silicon oxide nitride refers to a material whose composition contains more nitrogen than oxygen. Similarly, aluminum oxide nitride refers to a material whose composition contains more oxygen than nitrogen. Similarly, aluminum oxide nitride refers to a material whose composition contains more nitrogen than oxygen. Similarly, hafnium oxide nitride refers to a material whose composition contains more oxygen than nitrogen. Similarly, hafnium oxide nitride refers to a material whose composition contains more nitrogen than oxygen.

[0044] Furthermore, in this specification, the term "insulator" may be replaced with "insulating film" or "insulating layer." Similarly, the term "conductor" may be replaced with "conductive film" or "conductive layer." Finally, the term "semiconductor" may be replaced with "semiconductor film" or "semiconductor layer."

[0045] Furthermore, in this specification, "parallel" means a state in which two lines are positioned at an angle of -10 degrees or more and 10 degrees or less. Therefore, the case of -5 degrees or more and 5 degrees or less is also included. Also, "approximately parallel" means a state in which two lines are positioned at an angle of -30 degrees or more and 30 degrees or less. Also, "perpendicular" means a state in which two lines are positioned at an angle of 80 degrees or more and 100 degrees or less. Therefore, the case of 85 degrees or more and 95 degrees or less is also included. Also, "approximately perpendicular" means a state in which two lines are positioned at an angle of 60 degrees or more and 120 degrees or less.

[0046] In this specification, "metal oxide" refers to an oxide of a metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors), oxide semiconductors (also called oxide semiconductors or simply OS), etc. For example, when a metal oxide is used in the semiconductor layer of a transistor, that metal oxide may be referred to as an oxide semiconductor. In other words, when an OS transistor is described, it can be rephrased as a transistor having a metal oxide or oxide semiconductor.

[0047] Furthermore, in this specification, normally off means that when no potential is applied to the gate, or when the gate is given a ground potential, the drain current flowing through the transistor per 1 μm of channel width is 1 × 10⁻¹⁶ at room temperature. -20 A or less, 1 × 10 at 85℃ -18 A or less, or 1 × 10 at 125°C -16 This means being less than or equal to A.

[0048] Furthermore, in this specification, "voltage" and "potential" may be used interchangeably as appropriate. "Voltage" is the potential difference from a reference potential. For example, if the reference potential is the ground potential (earth potential), then "voltage" can be replaced with "potential." Note that the ground potential does not necessarily mean 0V. Also, potential is relative, and as the reference potential changes, the potential applied to the wiring, the potential applied to the circuit, and the potential output from the circuit also change.

[0049] In this specification, when the same symbol is used for multiple elements, and especially when it is necessary to distinguish them, an identifying symbol such as "_1", "[n]", or "[m,n]" may be added to the symbol.

[0050] In this specification, "heights match or approximately match" refers to a configuration in which the heights from a reference surface (e.g., a flat surface such as the substrate surface) are equal in a cross-sectional view. For example, in the manufacturing process of semiconductor devices, planarization (typically CMP) may expose the surfaces of one or more layers. In this case, the surfaces subjected to CMP will have a configuration in which the heights from the reference surface are equal. However, the heights of the multiple layers may differ depending on the processing apparatus, processing method, or material of the surface subjected to CMP. In this specification, this case will also be treated as "heights match or approximately match." For example, if there are two layers with different heights (here referred to as a first layer and a second layer) with respect to a reference surface, if the difference between the height of the top surface of the first layer and the height of the top surface of the second layer is 20 nm or less, it is also said that the heights match or approximately match.

[0051] In this specification, "ends coincide or roughly coincide" means that, in a plan view, at least a portion of the contours of the stacked layers overlap. This includes, for example, cases where the upper and lower layers are processed with the same mask pattern, or partially with the same mask pattern. However, strictly speaking, the contours may not overlap, and the contour of the upper layer may be located inside the contour of the lower layer, or the contour of the upper layer may be located outside the contour of the lower layer; in this case, it is also referred to as "ends coincide or roughly coincide."

[0052] (Embodiment 1) In this embodiment, an example of a semiconductor device according to one aspect of the present invention and a method for manufacturing the same will be described with reference to Figures 1A to 38. The semiconductor device according to one aspect of the present invention has a transistor and a capacitive element.

[0053] <Example of semiconductor device configuration> The configuration of a semiconductor device having transistors and capacitive elements will be explained using Figure 1. Figures 1A to 1D are top views and cross-sectional views of a semiconductor device having transistors 200a, 200b, 100a, and 100b. Figure 1A is a top view of the semiconductor device. Figures 1B to 1D are cross-sectional views of the same semiconductor device. Here, Figure 1B is a cross-sectional view of the area indicated by the dashed line A1-A2 in Figure 1A, and is also a cross-sectional view of transistors 200a, 200b, 100a, and 100b in the channel length direction. Figure 1C is a cross-sectional view of the area indicated by the dashed line A3-A4 in Figure 1A, and is also a cross-sectional view of transistor 200a in the channel width direction. Figure 1D is a cross-sectional view of the area indicated by the dashed line A5-A6 in Figure 1A. Note that some elements have been omitted from the top view of Figure 1A for clarity.

[0054] Furthermore, the X direction shown in Figure 1A is parallel to the channel length direction of transistor 200a and the channel length direction of transistor 200b, the Y direction is perpendicular to the X direction, and the Z direction is perpendicular to both the X and Y directions. The X, Y, and Z directions shown in Figure 1A are also illustrated in Figures 1B to 1D.

[0055] A semiconductor device according to one aspect of the present invention includes an insulator 214 on a substrate (not shown), transistors 200a, 200b, capacitive elements 100a, and 100b on the insulator 214, an insulator 280 on an insulator 275 provided on transistors 200a and 200b, an insulator 282 on the insulator 280, an insulator 285 on the capacitive elements 100a, on the capacitive elements 100b, and on the insulator 282, and a conductor 240 (conductor 240a and conductor 240b). The insulators 214, 280, 282, and 285 function as interlayer films. As shown in Figure 1B, each of the transistors 200a, 200b, 100a, and 100b is arranged with at least a portion embedded in the insulator 280.

[0056] Here, transistors 200a and 200b each have an oxide 230 that functions as a semiconductor layer, a conductor 260 that functions as a first gate (also called a top gate) electrode, a conductor 205 that functions as a second gate (also called a back gate) electrode, a conductor 242a that functions as either a source electrode or a drain electrode, and a conductor 242b that functions as the other of the source electrode or a drain electrode. They also have insulators 253 and 254 that function as first gate insulators, and insulators 222 and 224 that function as second gate insulators. Note that gate insulators are sometimes called gate insulating layers or gate insulating films.

[0057] Since transistors 200a and 200b have the same configuration, in the following explanations, when describing matters common to both transistors 200a and 200b, the symbol attached to the reference numeral may be omitted, and they may be referred to simply as transistor 200.

[0058] The first gate electrode and the first gate insulating film are placed within the opening 258 formed in the insulators 280 and 275. That is, the conductor 260, insulator 254, and insulator 253 are placed within the opening 258.

[0059] Each capacitive element 100a and each capacitive element 100b has a conductor 156 that functions as a lower electrode, an insulator 153 that functions as a dielectric, and a conductor 160 that functions as an upper electrode. In other words, each capacitive element 100a and each capacitive element 100b constitutes a MIM (Metal-Insulator-Metal) capacitance.

[0060] Since capacitive elements 100a and 100b have the same configuration, in the following explanations, when describing matters common to both capacitive elements 100a and 100b, the symbols attached to the reference numerals may be omitted, and they may be simply referred to as capacitive element 100.

[0061] The upper electrode, dielectric, and a portion of the lower electrode of the capacitive element 100 are placed within the opening 158 formed in the insulators 282, 280, and 275. That is, the conductor 160, insulator 153, and conductor 156 are placed within the opening 158.

[0062] Furthermore, a semiconductor device according to one aspect of the present invention includes a conductor 240 (conductor 240a and conductor 240b) that is electrically connected to a transistor 200 and functions as a plug (which can also be called a connecting electrode). The conductor 240 is placed in an opening 206 formed in an insulator 280 or the like. The conductor 240 has a region that is in contact with a part of the upper surface and a part of the side surface of the conductor 242a.

[0063] Furthermore, a semiconductor device according to one aspect of the present invention has an insulator 210 and a conductor 209 between a substrate (not shown) and an insulator 214. The conductor 209 is arranged so as to be embedded in the insulator 210. The conductor 209 has a region that is in contact with the conductor 240.

[0064] Furthermore, a semiconductor device according to one aspect of the present invention may have an insulator 212 between the insulator 210 and the conductor 209 and the insulator 214.

[0065] The semiconductor device having a transistor 200 and a capacitive element 100 as shown in this embodiment can be used as a memory cell of a memory device. In this case, the conductor 240 may be electrically connected to a sense amplifier, and the conductor 240 functions as a bit line. Here, as shown in Figure 1A, the capacitive element 100 is provided such that at least a part of it overlaps with the conductor 242b of the transistor 200. Therefore, in a plan view, the capacitive element 100 can be provided without significantly increasing the occupied area, and thus the semiconductor device according to this embodiment can be miniaturized or highly integrated.

[0066] Furthermore, the semiconductor device shown in this embodiment has a line-symmetric configuration with respect to the dashed line A7-A8 shown in Figure 1A as the axis of symmetry. In other words, transistor 200b is positioned symmetrically with respect to transistor 200a, with respect to the conductor 240 as the axis of symmetry. Similarly, capacitive element 100b is positioned symmetrically with respect to capacitive element 100a, with respect to the conductor 240 as the axis of symmetry. Here, the conductor 242a serves as both the source electrode or drain electrode of transistor 200a and the source electrode or drain electrode of transistor 200b. In addition, the conductor 240 functions as a plug in both transistor 200a and transistor 200b. By connecting the two transistors, two capacitive elements, and plug in the above configuration, a semiconductor device that can be miniaturized or highly integrated can be provided.

[0067] Figure 2 shows a circuit diagram when the semiconductor device shown in this embodiment is used as a memory device. A semiconductor device having transistor 200a and capacitive element 100a can be used as a memory cell of the memory device. Alternatively, a semiconductor device having transistor 200b and capacitive element 100b can be used as a memory cell of the memory device.

[0068] As shown in Figure 2, the semiconductor device shown in Figures 1A to 1D can be described as a memory device composed of two memory cells. One memory cell has a transistor Tra and a capacitive element Ca. The other memory cell has a transistor Trb and a capacitive element Cb.

[0069] Here, transistors Tra, Trb, Ca, and Cb correspond to transistors 200a, 200b, 100a, and 100b, respectively.

[0070] In one memory cell, either the source or drain of transistor Tra is connected to wiring BL. The other source or drain of transistor Tra is connected to one electrode of capacitive element Ca. The gate of transistor Tra is connected to wiring WL. The other electrode of capacitive element Ca is connected to wiring PL.

[0071] In the other memory cell, either the source or drain of transistor Trb is connected to wiring BL. The other source or drain of transistor Trb is connected to one electrode of capacitive element Cb. The gate of transistor Trb is connected to wiring WL. The other electrode of capacitive element Cb is connected to wiring PL.

[0072] The memory cells will be described in detail in a later embodiment.

[0073] [Transistor 200] As shown in Figures 1A to 1D, the transistor 200 comprises an insulator 216 on an insulator 214, a conductor 205 (conductor 205a and conductor 205b) arranged to be embedded in the insulator 216, an insulator 222 on the insulator 216 and the conductor 205, an insulator 224 on the insulator 222, an oxide 230a on the insulator 224, an oxide 230b on the oxide 230a, and a conductor 242a (conductor 242a1 and conductor 242a1 and conductor 242a1) on the oxide 230b. The device comprises a body 242a2) and a conductor 242b (conductors 242b1 and 242b2), an insulator 253 on oxide 230b, an insulator 254 on insulator 253, a conductor 260 (conductors 260a and 260b) located on insulator 254 and overlapping with a portion of oxide 230b, and an insulator 275 arranged on insulator 222, insulator 224, oxide 230a, oxide 230b, conductor 242a, and conductor 242b.

[0074] In this specification, oxides 230a and 230b may be collectively referred to as oxide 230. Similarly, conductors 242a and 242b may be collectively referred to as conductor 242.

[0075] Insulators 280 and 275 are provided with an opening 258 that reaches the oxide 230b. In other words, the opening 258 has a region that overlaps with the oxide 230b. Insulator 275 also has an opening that overlaps with the opening of insulator 280. In other words, the opening 258 includes the opening of insulator 280 and the opening of insulator 275. Insulators 253, 254, and conductor 260 are arranged within the opening 258. In other words, conductor 260 has a region that overlaps with the oxide 230b via insulators 253 and 254. In addition, in the channel length direction of transistor 200, conductor 260, insulator 253, and insulator 254 are provided between conductor 242a and conductor 242b. The insulator 254 has a region in contact with the side surface of the conductor 260 and a region in contact with the bottom surface of the conductor 260. As shown in Figure 1C, the opening 258 reaches the insulator 222 in the region that does not overlap with the oxide 230.

[0076] Preferably, the oxide 230 has an oxide 230a disposed on top of the insulator 224 and an oxide 230b disposed on top of the oxide 230a. By having oxide 230a below oxide 230b, the diffusion of impurities from structures formed below oxide 230a to oxide 230b can be suppressed.

[0077] In the transistor 200, the oxide 230 is shown as having a configuration in which two layers of oxide 230a and oxide 230b are stacked, but the present invention is not limited to this. For example, it may be a single layer of oxide 230b, or a configuration with a stacked structure of three or more layers, or oxide 230a and oxide 230b may each have a stacked structure.

[0078] Conductor 260 functions as a first gate electrode, and conductor 205 functions as a second gate electrode. Insulators 253 and 254 function as first gate insulators, and insulators 222 and 224 function as second gate insulators. Conductor 242a functions as either a source electrode or a drain electrode, and conductor 242b functions as either a source electrode or a drain electrode. At least a portion of the region of oxide 230 that overlaps with conductor 260 functions as a channel-forming region.

[0079] Here, an enlarged view of the vicinity of the channel formation region in Figure 1B is shown in Figure 3A. The opening 258 can also be considered as having a shape in which a part of the structure made of insulator 224 and oxide 230 protrudes into an opening with insulator 222 as the bottom surface and insulators 280 and 275 as the sides.

[0080] As shown in Figures 3A and 1C, an insulator 253 is provided in contact with the bottom surface and inner wall (also called the side wall) of the opening 258. Thus, the insulator 253 is in contact with at least a portion of the top surface of the insulator 222, the side surface of the insulator 224, the side surface of the oxide 230a, the top and side surfaces of the oxide 230b, the side surfaces of the conductors 242a and 242b, the side surface of the insulator 275, the side surface of the insulator 280, and the bottom surface of the insulator 254.

[0081] As shown in Figure 3A, the width of the aperture 258 in the channel length direction roughly coincides with the distance between the conductors 242a and 242b. Therefore, a channel formation region is formed in the region of the oxide 230b that overlaps with the width of the aperture 258 in the channel length direction. Here, the distance between the conductors 242a and 242b is preferably, for example, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and preferably 1 nm or more, or 5 nm or more. By making the channel formation region of the transistor 200 a very fine structure in this way, the on-current of the transistor 200 can be increased, and the frequency characteristics can be improved. In addition, when providing multiple transistors 200, it becomes possible to reduce the area and increase the density. However, it is not limited to the above, and the distance between the conductors 242a and 242b can also be 60 nm or more.

[0082] Furthermore, miniaturizing transistor 200 can improve its high-frequency characteristics. Specifically, the cutoff frequency can be improved. When the gate length is within the above range, the cutoff frequency of the transistor can be set to 50 GHz or higher, or 100 GHz or higher, for example, under room temperature conditions.

[0083] Figure 3A shows a configuration in which the side wall of the opening 258 is approximately perpendicular to the upper surface of the insulator 222, but the present invention is not limited to this. As shown in Figure 3B, the side wall of the opening 258 may be tapered. By making the side wall of the opening 258 tapered, the covering of the insulator 253 and the like can be improved in subsequent processes, and defects such as porosity can be reduced.

[0084] In this specification, a tapered shape refers to a shape in which at least a portion of the side surface of the structure is inclined with respect to the substrate surface. For example, it is preferable to have a region in which the angle between the inclined side surface and the substrate surface (hereinafter sometimes referred to as the taper angle) is less than 90°. The side surface of the structure and the substrate surface do not necessarily have to be perfectly flat, and may be substantially planar with a fine curvature, or substantially planar with fine irregularities.

[0085] Furthermore, as shown in Figure 3C, in a cross-sectional view of the transistor 200 in the channel length direction, the distance L2 between conductor 242a and conductor 242b may be configured to be smaller than the width of the opening 258. Here, the width of the opening 258 corresponds to the distance L1 between the interface of insulator 280 and insulator 253 on the conductor 242a side and the interface of insulator 280 and insulator 253 on the conductor 242b side, as shown in Figure 3C. With such a configuration, the distance L2 between conductor 242a and conductor 242b can be made into a very fine structure (for example, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 1 nm or more, or 5 nm or more). Also, since conductor 260 has a region with a distance L1 that is larger than distance L2, the increase in resistance of conductor 260 located in the region of distance L1 is suppressed, and conductor 260 can function as wiring.

[0086] Furthermore, as shown in Figure 3C, in a cross-sectional view of the transistor 200 in the channel length direction, the width of the opening of the insulator 280 in the opening 258 is equal to the distance L1, and the width of the opening of the insulator 275 in the opening 258 is equal to the distance L2.

[0087] The opening 258 can also be considered as having a shape in which a part of the structure consisting of insulator 224, oxide 230, conductor 242, and insulator 275 protrudes into an opening with insulator 222 as the bottom surface and insulator 280 as the side surface. Furthermore, in the structure consisting of insulator 224, oxide 230, conductor 242, and insulator 275, the region of oxide 230 sandwiched between conductor 242a and conductor 242b can be considered as being exposed.

[0088] As shown in Figures 3C and 1C, an insulator 253 is provided in contact with the bottom surface and inner wall (also called the side wall) of the opening 258. Therefore, the insulator 253 is in contact with at least a portion of the top surface of the insulator 222, the side surface of the insulator 224, the side surface of the oxide 230a, the top and side surfaces of the oxide 230b, the side surfaces of the conductors 242a and 242b, the side surface of the insulator 275, the side surface of the insulator 280, and the bottom surface of the insulator 254. In addition, the insulator 254 and the conductor 260 are laminated on the insulator 253. For this reason, the insulator 253, insulator 254, and conductor 260 are provided to cover the conductors 242 and insulator 275 that partially protrude into the opening 258.

[0089] A channel formation region is formed in the oxide 230b at a distance L2. Therefore, the channel formation region of transistor 200 has a very fine structure. This increases the on-current of transistor 200, improving its frequency characteristics.

[0090] As shown in Figure 3A, the oxide 230b has a region 230bc that functions as a channel formation region of the transistor 200, and regions 230ba and 230bb that are provided so as to sandwich region 230bc and function as a source region or drain region. Region 230bc is superimposed on the conductor 260 in at least a portion thereof. In other words, region 230bc is provided in the region between the conductors 242a and 242b. Region 230ba is provided superimposed on the conductor 242a, and region 230bb is provided superimposed on the conductor 242b.

[0091] Region 230bc, which functions as a channel-forming region, is a high-resistance region with a lower carrier concentration due to fewer oxygen vacancies or lower impurity concentrations compared to regions 230ba and 230bb. Therefore, region 230bc can be said to be type i (intrinsic) or substantially type i.

[0092] Furthermore, regions 230ba and 230bb, which function as source or drain regions, are regions with high oxygen deficiencies or high concentrations of impurities such as hydrogen, nitrogen, and metallic elements, resulting in increased carrier concentration and low resistance. In other words, regions 230ba and 230bb are n-type regions with higher carrier concentration and lower resistance compared to region 230bc.

[0093] Here, as shown in Figure 3A, it is preferable that the opposing sides of conductor 242a and conductor 242b are approximately perpendicular to the upper surface of oxide 230b. This configuration prevents the side edge of region 230ba formed beneath conductor 242a on the region 230bc side from receding excessively from the side edge of conductor 242a on the region 230bc side. Similarly, it prevents the side edge of region 230bb formed beneath conductor 242b on the region 230bc side from receding excessively from the side edge of conductor 242b on the region 230bc side. This reduces the formation of so-called Loff regions between region 230ba and region 230bc, and between region 230bb and region 230bc. Here, when we say that the side edge of region 230ba on the region 230bc side is receding, it means that the side edge of region 230ba is located closer to conductor 240 than the side of conductor 242a on the region 230bc side. Furthermore, when we say that the side edge of region 230bb on the region 230bc side is recessed, it means that the side edge of region 230bb is located closer to the conductor 160 than the side surface of the conductor 242b on the region 230bc side.

[0094] As a result, the frequency characteristics of the transistor 200 can be improved, and the operating speed of the semiconductor device according to one aspect of the present invention can be improved. For example, when the semiconductor device according to one aspect of the present invention is used as a memory cell in a storage device, the writing speed and reading speed can be improved.

[0095] Furthermore, the carrier concentration in region 230bc, which functions as a channel-forming region, is 1 × 10⁻⁶. 18 cm -3 The following is preferable: 1 × 10 17 cm -3More preferably, it is less than 1×10 16 cm -3 Even more preferably, it is less than 1×10 13 cm -3 Even more preferably, it is less than 1×10 12 cm -3 Even more preferably, it is less than. Further, the lower limit of the carrier concentration in the region 230bc functioning as a channel formation region is not particularly limited, but for example, it can be 1×10 -9 cm -3 .

[0096] Further, a region may be formed between the region 230bc and the region 230ba or the region 230bb, where the carrier concentration is equal to or lower than the carrier concentration of the region 230ba and the region 230bb, and equal to or higher than the carrier concentration of the region 230bc. That is, the region functions as a junction region between the region 230bc and the region 230ba or the region 230bb. The junction region may have a hydrogen concentration equal to or lower than the hydrogen concentration of the region 230ba and the region 230bb, and equal to or higher than the hydrogen concentration of the region 230bc. Further, the junction region may have oxygen vacancies equal to or fewer than the oxygen vacancies in the region 230ba and the region 230bb, and equal to or more than the oxygen vacancies in the region 230bc.

[0097] Note that, although FIG. 3A illustrates an example in which the region 230ba, the region 230bb, and the region 230bc are formed in the oxide 230b, the present invention is not limited thereto. For example, each of the above regions may be formed not only in the oxide 230b but also in the oxide 230a.

[0098] Furthermore, in oxide 230, it can be difficult to clearly detect the boundaries between each region. The concentrations of metal elements, as well as impurity elements such as hydrogen and nitrogen, detected within each region may not be limited to stepwise changes between regions, but may also change continuously within each region. In other words, the closer a region is to the channel-forming region, the lower the concentrations of metal elements, as well as impurity elements such as hydrogen and nitrogen should be.

[0099] In transistor 200, it is preferable to use a metal oxide (hereinafter also referred to as an oxide semiconductor) that functions as a semiconductor for the oxide 230 (oxide 230a and oxide 230b) which includes the channel formation region.

[0100] Furthermore, the band gap of the metal oxide that functions as a semiconductor is preferably 2 eV or more, and more preferably 2.5 eV or more. By using a metal oxide with a large band gap, the off-current of the transistor can be reduced.

[0101] As oxide 230, it is preferable to use a metal oxide such as indium oxide, gallium oxide, and zinc oxide. Alternatively, as oxide 230, it is preferable to use a metal oxide having two or three elements selected from indium, element M, and zinc. Element M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium. In particular, it is preferable that element M is one or more selected from aluminum, gallium, yttrium, and tin. A metal oxide having indium, element M, and zinc may be referred to as In-M-Zn oxide.

[0102] The oxide 230 preferably has a laminated structure of multiple oxide layers with different chemical compositions. For example, in the metal oxide used for oxide 230a, it is preferable that the atomic ratio of element M to the main metal element is greater than the atomic ratio of element M to the main metal element in the metal oxide used for oxide 230b. Furthermore, in the metal oxide used for oxide 230a, it is preferable that the atomic ratio of element M to In is greater than the atomic ratio of element M to In in the metal oxide used for oxide 230b. This configuration suppresses the diffusion of impurities and oxygen from structures formed below oxide 230a to oxide 230b.

[0103] Furthermore, it is preferable that the atomic ratio of In to element M in the metal oxide used for oxide 230b is greater than the atomic ratio of In to element M in the metal oxide used for oxide 230a. With this configuration, transistor 200 can obtain a large on-current and high frequency characteristics.

[0104] Furthermore, because oxides 230a and 230b share a common element other than oxygen as their main component, the defect level density at the interface between oxides 230a and 230b can be reduced. As a result, the influence of interfacial scattering on carrier conduction is reduced, and transistor 200 can obtain a large on-current and high frequency characteristics.

[0105] Specifically, for oxide 230a, a metal oxide with a composition of In:M:Zn=1:3:4 [atomic ratio] or nearby, In:M:Zn=1:3:2 [atomic ratio] or nearby, or In:M:Zn=1:1:0.5 [atomic ratio] or nearby may be used. For oxide 230b, a metal oxide with a composition of In:M:Zn=1:1:1 [atomic ratio] or nearby, In:M:Zn=1:1:1.2 [atomic ratio] or nearby, In:M:Zn=1:1:2 [atomic ratio] or nearby, or In:M:Zn=4:2:3 [atomic ratio] or nearby may be used. Note that nearby compositions include a range of ±30% of the desired atomic ratio. Furthermore, it is preferable to use gallium as element M. Furthermore, when a single layer of oxide 230b is provided as oxide 230, a metal oxide that can be used for oxide 230a may be applied as oxide 230b.

[0106] Furthermore, when depositing metal oxide films by sputtering, the above atomic ratio is not limited to the atomic ratio of the deposited metal oxide film, but may also be the atomic ratio of the sputtering target used for depositing the metal oxide film.

[0107] It is preferable that oxide 230b is crystalline. In particular, it is preferable to use CAAC-OS (c-axis aligned crystalline oxide semiconductor) as oxide 230b.

[0108] CAAC-OS is a metal oxide with a highly crystalline, dense structure and few impurities and defects (e.g., oxygen vacancies). In particular, by heat-treating the metal oxide after its formation at a temperature that does not cause polycrystallization (e.g., between 400°C and 600°C), the CAAC-OS can be made to have an even more crystalline and dense structure. By increasing the density of CAAC-OS in this way, the diffusion of impurities or oxygen within the CAAC-OS can be further reduced.

[0109] Furthermore, because it is difficult to identify clear grain boundaries in CAAC-OS, a decrease in electron mobility due to grain boundary issues is less likely to occur. Therefore, metal oxides containing CAAC-OS have stable physical properties. Consequently, metal oxides containing CAAC-OS are highly heat-resistant and reliable.

[0110] Furthermore, by using a crystalline oxide such as CAAC-OS as oxide 230b, the extraction of oxygen from oxide 230b by the source electrode or drain electrode can be suppressed. As a result, even when heat treatment is performed, the extraction of oxygen from oxide 230b is reduced, making transistor 200 stable against high temperatures (so-called thermal budget) in the manufacturing process.

[0111] In transistors using oxide semiconductors, the electrical properties tend to fluctuate and reliability may be poor if impurities and oxygen vacancies are present in the region where the channel is formed in the oxide semiconductor. Furthermore, hydrogen near the oxygen vacancy can fill the oxygen vacancy, creating a defect (hereinafter referred to as V). O Oxygen vacancies (sometimes called H) can form and generate electron carriers. Therefore, if the region where channels are formed in an oxide semiconductor contains oxygen vacancies, the transistor is likely to exhibit normally-on characteristics (a characteristic in which channels exist and current flows through the transistor even without applying voltage to the gate electrode). Consequently, in the region where channels are formed in an oxide semiconductor, impurities, oxygen vacancies, and V are likely to be present. O It is preferable that H is reduced as much as possible. In other words, it is preferable that the region in the oxide semiconductor where the channel is formed has a reduced carrier concentration and is type i (intrinsed) or substantially type i.

[0112] In contrast, by placing an insulator containing oxygen that is released by heating (hereinafter sometimes referred to as excess oxygen) near the oxide semiconductor and performing heat treatment, oxygen is supplied from the insulator to the oxide semiconductor, eliminating oxygen deficiencies and V OH can be reduced. However, if an excessive amount of oxygen is supplied to the source or drain region, it may cause a decrease in the on-current of transistor 200 or a decrease in field-effect mobility. Furthermore, variations in the amount of oxygen supplied to the source or drain region within the substrate surface will result in variations in the characteristics of the semiconductor device containing the transistor. In addition, if the oxygen supplied from the insulator to the oxide semiconductor diffuses into conductors such as the gate electrode, source electrode, and drain electrode, these conductors may oxidize, impairing their conductivity and potentially adversely affecting the electrical characteristics and reliability of the transistor.

[0113] Therefore, in an oxide semiconductor, the region 230bc, which functions as a channel-forming region, preferably has a reduced carrier concentration and is i-type or substantially i-type, while the regions 230ba and 230bb, which function as a source region or drain region, preferably have a high carrier concentration and are n-type. In other words, oxygen vacancies in region 230bc of the oxide semiconductor, and V O It is preferable to reduce H. Also, ensure that an excessive amount of oxygen is not supplied to regions 230ba and 230bb, and that the V in regions 230ba and 230bb is reduced. O It is preferable to prevent an excessive reduction in the amount of H. Furthermore, it is preferable to have a configuration that suppresses a decrease in the conductivity of conductors 260, 242a, and 242b. For example, it is preferable to have a configuration that suppresses oxidation of conductors 260, 242a, and 242b. Note that hydrogen in oxide semiconductors is V. O Since H can be formed, V O To reduce the amount of H, it is necessary to reduce the hydrogen concentration.

[0114] Therefore, in this embodiment, the semiconductor device is configured to reduce the hydrogen concentration in region 230bc, suppress oxidation of conductors 242a, 242b, and 260, and suppress the reduction of hydrogen concentration in regions 230ba and 230bb.

[0115] To reduce the hydrogen concentration in region 230bc, it is preferable that the insulator 253 has the function of capturing and fixing hydrogen. As shown in Figure 3(A), the insulator 253 has a region that is in contact with the oxide 230b region 230bc. With this configuration, the hydrogen concentration in the oxide 230b region 230bc can be reduced. Therefore, the hydrogen in region 230bc O By reducing H, region 230bc can be made i-type or substantially i-type.

[0116] Examples of insulators that have the function of capturing and fixing hydrogen include metal oxides having an amorphous structure. For example, it is preferable to use metal oxides such as magnesium oxide, or oxides containing one or both of aluminum and hafnium. In such amorphous metal oxides, oxygen atoms have dangling bonds, and these dangling bonds may have the property of capturing or fixing hydrogen. In other words, amorphous metal oxides can be said to have a high ability to capture or fix hydrogen.

[0117] In particular, it is preferable to use an oxide containing one or both of aluminum and hafnium as the insulator 253, and it is more preferable to use an oxide containing one or both of aluminum and hafnium having an amorphous structure, and it is even more preferable to use hafnium oxide having an amorphous structure. In this embodiment, hafnium oxide is used as the insulator 253. In this case, the insulator 253 is an insulator having at least oxygen and hafnium. Furthermore, the hafnium oxide has an amorphous structure. In this case, the insulator 253 has an amorphous structure.

[0118] However, the insulator that can be used for insulator 253 is not limited to the hydrogen barrier insulator described above. It is also possible to use an insulator with a thermally stable structure, such as silicon oxide or silicon oxynitride. For example, as insulator 253, a multilayer film having an aluminum oxide film and a silicon oxide film or silicon oxynitride film on the aluminum oxide film may be used. Alternatively, as insulator 253, a multilayer film having an aluminum oxide film, a silicon oxide film or silicon oxynitride film on the aluminum oxide film and a hafnium oxide film on the silicon oxide film or silicon oxynitride film may be used.

[0119] To suppress oxidation of conductors 242a, 242b, and 260, it is preferable to provide oxygen barrier insulators near each of conductors 242a, 242b, and 260. In the semiconductor device described in this embodiment, the insulators are, for example, insulator 253, insulator 254, and insulator 275.

[0120] In this specification, a barrier insulator refers to an insulator that possesses barrier properties. In this specification, barrier properties refer to the function of suppressing the diffusion of the corresponding substance (also known as low permeability), or the function of capturing and fixing the corresponding substance (also known as gettering).

[0121] Examples of oxygen barrier insulators include oxides containing one or both aluminum and hafnium, magnesium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate). For example, insulators 253, 254, and 275 can each be made up of the above oxygen barrier insulators in a single layer or a multi-layer structure.

[0122] The insulator 253 preferably has barrier properties against oxygen. The insulator 253 only needs to be less permeable to oxygen than the insulator 280. The insulator 253 has regions that are in contact with the side surfaces of the conductor 242a and the conductor 242b. The oxygen barrier properties of the insulator 253 suppress oxidation of the side surfaces of the conductors 242a and 242b, preventing the formation of an oxide film on these surfaces. This suppresses a decrease in the on-current of the transistor 200 or a decrease in the field-effect mobility.

[0123] Furthermore, the insulator 253 is provided in contact with the upper and side surfaces of oxide 230b, the side surfaces of oxide 230a, the side surfaces of insulator 224, and the upper surface of insulator 222. Because the insulator 253 has an oxygen barrier property, it can suppress the detachment of oxygen from the oxide 230b region 230bc when heat treatment or the like is performed. Therefore, the formation of oxygen vacancies in oxide 230a and oxide 230b can be reduced.

[0124] Furthermore, even if the insulator 280 contains an excess amount of oxygen, it is possible to suppress the excessive supply of that oxygen to oxides 230a and 230b. Therefore, it is possible to suppress excessive oxidation of regions 230ba and 230bb, which would otherwise cause a decrease in the on-current of transistor 200 or a decrease in field-effect mobility.

[0125] Oxides containing either or both aluminum and hafnium have barrier properties against oxygen and can therefore be suitably used as insulator 253.

[0126] The insulator 254 preferably has barrier properties against oxygen. The insulator 254 is provided between the oxide 230b region 230bc and the conductor 260, and between the insulator 280 and the conductor 260. This configuration suppresses the diffusion of oxygen contained in the oxide 230b region 230bc into the conductor 260, preventing the formation of oxygen vacancies in the oxide 230b region 230bc. Furthermore, it suppresses the diffusion of oxygen contained in the oxide 230b and oxygen contained in the insulator 280 into the conductor 260, preventing the oxidation of the conductor 260. The insulator 254 only needs to be less permeable to oxygen than the insulator 280. For example, it is preferable to use silicon nitride as the insulator 254. In this case, the insulator 254 will be an insulator containing at least nitrogen and silicon.

[0127] The insulator 275 preferably has barrier properties against oxygen. The insulator 275 is provided between the insulator 280 and the conductors 242a and 242b. This configuration suppresses the diffusion of oxygen contained in the insulator 280 to the conductors 242a and 242b. Therefore, it is possible to suppress the oxidation of the conductors 242a and 242b by the oxygen contained in the insulator 280, which increases their resistivity and reduces the on-current of the transistor 200. The insulator 275 only needs to be less permeable to oxygen than the insulator 280. For example, it is preferable to use silicon nitride as the insulator 275. In this case, the insulator 275 will be an insulator containing at least nitrogen and silicon.

[0128] To suppress the reduction of hydrogen concentration in regions 230ba and 230bb, it is preferable to provide hydrogen barrier insulators near regions 230ba and 230bb, respectively. In the semiconductor device described in this embodiment, the hydrogen barrier insulator is, for example, insulator 275.

[0129] Examples of hydrogen barrier insulators include oxides such as aluminum oxide, hafnium oxide, and tantalum oxide, and nitrides such as silicon nitride. For example, the insulator 275 may be made of the above hydrogen barrier insulator in a single layer or a multi-layer structure.

[0130] The insulator 275 is preferably one that has barrier properties against hydrogen. The insulator 275 is arranged in contact with the side surface of region 230ba of oxide 230b and the side surface of region 230bb of oxide 230b. By providing such an insulator 275, the diffusion of hydrogen from regions 230ba and 230bb to the outside can be reduced, and thus the decrease in hydrogen concentration in regions 230ba and 230bb can be suppressed. Therefore, regions 230ba and 230bb can be n-type.

[0131] By adopting the above configuration, the region 230bc, which functions as a channel-forming region, can be made i-type or substantially i-type, and the regions 230ba and 230bb, which function as source regions or drain regions, can be made n-type, thereby providing a semiconductor device with good electrical characteristics. Furthermore, by adopting the above configuration, the semiconductor device can maintain good electrical characteristics even when miniaturized or highly integrated.

[0132] The insulator 253 functions as part of the gate insulator. As shown in Figure 1B, the insulator 253 is provided in contact with the side surface of the insulator 275 and the side surface of the insulator 280.

[0133] The insulator 253, along with the insulator 254 and the conductor 260, must be provided in an opening formed in the insulator 280 or the like. When miniaturizing the transistor 200, it is preferable that the thickness of the insulator 253 be thin. The thickness of the insulator 253 is 0.1 nm or more and 5.0 nm or less, preferably 0.5 nm or more and 5.0 nm or less, more preferably 1.0 nm or more and less than 5.0 nm, and even more preferably 1.0 nm or more and 3.0 nm or less. In this case, it is sufficient that the insulator 253 has at least a portion of the above-mentioned thickness region.

[0134] To achieve the thin film thickness of insulator 253 as described above, it is preferable to deposit the film using atomic layer deposition (ALD). ALD methods include thermal ALD, which uses only thermal energy for the reaction between the precursor and reactant, and plasma-enhanced ALD (PEALD), which uses plasma-excited reactants. PEALD is preferable in some cases because the use of plasma allows for film deposition at lower temperatures.

[0135] The ALD method allows for the deposition of atoms layer by layer, resulting in several advantages: the ability to deposit extremely thin films, films on structures with high aspect ratios, films with fewer defects such as pinholes, films with excellent coverage, and films at low temperatures. Therefore, the insulator 253 can be deposited with good coverage and a thin film thickness as described above on the sides of openings formed in the insulator 280 and on the side edges of the conductor 242.

[0136] Note that precursors used in the ALD method may contain carbon and other impurities. Therefore, films formed by the ALD method may contain more carbon and other impurities compared to films formed by other film deposition methods. The quantity of impurities can be quantified using secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), or Auger electron spectroscopy (AES).

[0137] However, the film thickness of the insulator 253 is not limited to the above. For example, if the insulator 253 is made up of a laminated structure of an aluminum oxide film, a silicon oxide film on the aluminum oxide film, and a hafnium oxide film on the silicon oxide film, the film thickness of the insulator 253 can be appropriately set within a range of approximately 0.1 nm to 30 nm.

[0138] The insulator 254 functions as part of the gate insulator. Preferably, the insulator 254 has barrier properties against hydrogen. This prevents impurities such as hydrogen contained in the conductor 260 from diffusing into the oxide 230b.

[0139] Furthermore, the insulator 254, along with the insulator 253 and the conductor 260, must be provided in an opening formed in the insulator 280 or the like. In order to miniaturize the transistor 200, it is preferable that the film thickness of the insulator 254 be thin. The film thickness of the insulator 254 should be 0.1 nm or more and 5.0 nm or less, preferably 0.5 nm or more and 3.0 nm or less, and more preferably 1.0 nm or more and 3.0 nm or less. In this case, it is sufficient that the insulator 254 has a region with the above-mentioned film thickness in at least a part of it.

[0140] For example, silicon nitride deposited by the PEALD method can be used as the insulator 254.

[0141] Furthermore, by using an insulator 253 that has the function of suppressing the permeation of impurities such as hydrogen and oxygen, such as hafnium oxide, the insulator 253 can also perform the function of the insulator 254. In such a case, by omitting the insulator 254, the manufacturing process of the semiconductor device can be simplified and productivity can be improved.

[0142] The insulator 275 is provided so as to cover the insulator 222, the insulator 224, the oxide 230a, the oxide 230b, and the conductor 242. The insulator 275 can be configured to have regions that are in contact with the upper surface of the insulator 222, the side surface of the insulator 224, the side surface of the oxide 230a, the side surface of the oxide 230b, the upper and side surfaces of the conductor 242a, and the upper and side surfaces of the conductor 242b.

[0143] It is preferable to use conductive materials that are resistant to oxidation or conductive materials that have a function to suppress the diffusion of oxygen as conductors 242a, conductor 242b, and conductor 260. Examples of such conductive materials include conductive materials containing nitrogen and conductive materials containing oxygen. This makes it possible to suppress a decrease in the conductivity of conductors 242a, conductor 242b, and conductor 260. When conductive materials containing metal and nitrogen are used as conductors 242a, conductor 242b, and conductor 260, conductors 242a, conductor 242b, and conductor 260 become conductors having at least a metal and nitrogen.

[0144] One or both of the conductors 242 and 260 may have a laminated structure. For example, as shown in Figure 1B, each of the conductors 242a and 242b may have a two-layer laminated structure. In this case, the layers in contact with the oxide 230b (conductors 242a1 and 242b1) should be made of a conductive material that is resistant to oxidation or a conductive material that has a function to suppress oxygen diffusion. Also, for example, as shown in Figure 1B, when the conductor 260 has a laminated structure of conductors 260a and 260b, the conductor 260a should be made of a conductive material that is resistant to oxidation or a conductive material that has a function to suppress oxygen diffusion.

[0145] Furthermore, in order to suppress the decrease in conductivity of conductor 242, it is preferable to use a crystalline oxide such as CAAC-OS as oxide 230b. It is preferable to use a metal oxide applicable to oxide 230 as described above. In particular, it is preferable to use a metal oxide having indium, zinc, and one or more selected from gallium, aluminum, and tin. CAAC-OS is a crystalline oxide, and the c-axis of the crystal is approximately perpendicular to the surface of the oxide or the surface on which it is formed. This suppresses the extraction of oxygen from oxide 230b by conductor 242a or conductor 242b. It also suppresses the decrease in conductivity of conductors 242a and 242b.

[0146] Furthermore, in this embodiment, with the conductors 242a and 242b placed on the oxide 230b, microwave treatment is performed in an oxygen-containing atmosphere to eliminate oxygen deficiencies in region 230bc, and V O The aim is to reduce H. Here, microwave processing refers to processing using a device that has a power supply that generates high-density plasma using microwaves, for example.

[0147] By performing microwave treatment in an oxygen-containing atmosphere, the oxygen gas can be converted into plasma using microwaves or high-frequency waves such as RF, and this oxygen plasma can be applied. At this time, microwaves or high-frequency waves such as RF can also be irradiated into region 230bc. Due to the action of plasma, microwaves, etc., the V of region 230bc O H can be separated into an oxygen deficiency and hydrogen, the hydrogen can be removed from region 230bc, and the oxygen deficiency can be compensated for with oxygen. Therefore, the hydrogen concentration, oxygen deficiency, and V in region 230bc can be determined. O This can reduce H and lower the carrier concentration.

[0148] Furthermore, when performing microwave processing in an oxygen-containing atmosphere, the effects of microwaves, high frequencies such as RF, and oxygen plasma are shielded by conductors 242a and 242b and do not reach regions 230ba and 230bb. In addition, the effect of oxygen plasma can be reduced by insulators 275 and 280, which are provided covering oxide 230b and conductor 242. As a result, during microwave processing, in regions 230ba and 230bb, V O This reduces H and prevents excessive oxygen supply, thus preventing a decrease in carrier concentration.

[0149] Furthermore, it is preferable to perform microwave treatment in an oxygen-containing atmosphere after forming the insulating film that will become the insulator 253. Also, if the insulator 253 is in a laminated structure, the microwave treatment may be performed after a portion of the insulator 253 has been formed. For example, if the insulator 253 includes a silicon oxide film or a silicon oxynitride film, the microwave treatment may be performed at the stage when the silicon oxide film or silicon oxynitride film has been formed.

[0150] By performing microwave processing in an oxygen-containing atmosphere via the insulator 253 in this manner, oxygen can be efficiently injected into region 230bc. Furthermore, by positioning the insulator 253 in contact with the side surface of the conductor 242 and the surface of region 230bc, the injection of more oxygen than necessary into region 230bc can be suppressed, thereby preventing oxidation of the side surface of the conductor 242.

[0151] Furthermore, the oxygen injected into region 230bc can take various forms, including oxygen atoms, oxygen molecules, oxygen ions, and oxygen radicals (also called O radicals, which are atoms, molecules, or ions with unpaired electrons). Note that the oxygen injected into region 230bc may be one or more of the above forms, and oxygen radicals are particularly preferred. Additionally, the film quality of the insulator 253 can be improved, thereby increasing the reliability of the transistor 200.

[0152] In this way, oxygen vacancies are selectively created in the oxide semiconductor region 230bc, and V O By removing H, region 230bc can be made i-type or substantially i-type. Furthermore, it is possible to suppress the supply of excess oxygen to regions 230ba and 230bb, which function as source or drain regions, and maintain the state of the n-type region before microwave processing. This suppresses variations in the electrical properties of transistor 200 and prevents variations in the electrical properties of transistor 200 within the substrate plane.

[0153] By adopting the above configuration, it is possible to provide a semiconductor device with minimal variation in transistor characteristics, good frequency characteristics, high operating speed, high reliability, good electrical characteristics, and the ability to miniaturize or highly integrate the device.

[0154] As shown in Figure 1C, in a cross-sectional view of the transistor 200 in the channel width direction, there may be a curved surface between the side surface and the top surface of the oxide 230b. That is, the ends of the side surface and the ends of the top surface may be curved (hereinafter also referred to as rounded).

[0155] The radius of curvature of the curved surface is preferably greater than 0 nm and less than the film thickness of the oxide 230b in the region overlapping with the conductor 242, or less than half the length of the region without the curved surface. Specifically, the radius of curvature of the curved surface is greater than 0 nm and 20 nm or less, preferably 1 nm to 15 nm, and more preferably 2 nm to 10 nm. By adopting such a shape, the coverage of the oxide 230b by the insulator 253, insulator 254, and conductor 260 can be improved.

[0156] Furthermore, during the manufacturing process of the transistor 200, it is preferable to perform a heat treatment with the surface of the oxide 230 exposed. This heat treatment may be performed, for example, at a temperature of 100°C to 600°C, more preferably 350°C to 550°C. The heat treatment should be performed in an atmosphere of nitrogen gas or an inert gas, or in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, it is preferable to perform the heat treatment in an oxygen atmosphere. This allows oxygen to be supplied to the oxide 230, thereby reducing oxygen deficiency. The heat treatment may also be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere of nitrogen gas or an inert gas, and then in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas to replenish the desorbed oxygen. Alternatively, the heat treatment may be performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas, and then continuously in an atmosphere of nitrogen gas or an inert gas.

[0157] Furthermore, by performing an oxygenation treatment on oxide 230, oxygen deficiencies in oxide 230 can be repaired by the supplied oxygen. In addition, the supplied oxygen reacts with the hydrogen remaining in oxide 230, removing the hydrogen as H2O (dehydration). As a result, the hydrogen remaining in oxide 230 recombines with the oxygen deficiencies and V O This can suppress the formation of H.

[0158] Furthermore, as shown in Figure 1C and other figures, by providing an insulator 253 in contact with the top and side surfaces of the oxide 230, the indium contained in the oxide 230 may be unevenly distributed at and near the interface between the oxide 230 and the insulator 253. As a result, the atomic ratio near the surface of the oxide 230 becomes similar to that of indium oxide, or similar to that of In-Zn oxide. By increasing the atomic ratio of indium near the surface of the oxide 230, particularly oxide 230b, the field-effect mobility of the transistor 200 can be improved.

[0159] Furthermore, in this embodiment, it is preferable to configure the semiconductor device to suppress the ingress of hydrogen into the transistor 200, in addition to the above configuration. For example, it is preferable to provide an insulator having the function of suppressing hydrogen diffusion so as to cover the transistor 200. In the semiconductor device described in this embodiment, the insulator is, for example, an insulator 212.

[0160] It is preferable to use an insulator 212 that has the function of suppressing hydrogen diffusion. This suppresses the diffusion of hydrogen from below the insulator 212 to the transistor 200. Note that any insulator that can be used for the insulator 275 described above may be used for the insulator 212.

[0161] It is preferable that at least one of insulators 212, 214, and 282 functions as a barrier insulating film that suppresses the diffusion of impurities such as water and hydrogen from the substrate side or from above the transistor 200 into the transistor 200. Therefore, it is preferable that at least one of insulators 212, 214, and 282 is an insulating material that has the function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms (i.e., the above impurities do not easily permeate through it). Alternatively, it is preferable to use an insulating material that has the function of suppressing the diffusion of oxygen (e.g., at least one such as oxygen atoms and oxygen molecules) (i.e., the above oxygen does not easily permeate through it).

[0162] It is preferable to use insulators 212, 214, and 282 that have the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen. For example, aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, or silicon nitride oxide can be used. For example, it is preferable to use silicon nitride, which has higher hydrogen barrier properties, as insulator 212. Also, for example, it is preferable to use aluminum oxide or magnesium oxide, which have high hydrogen capture and hydrogen fixation functions, as insulators 214 and 282. This makes it possible to suppress the diffusion of impurities such as water and hydrogen from the substrate side to the transistor 200 side via insulators 212 and 214. Alternatively, it is possible to suppress the diffusion of impurities such as water and hydrogen from the interlayer insulating film located outside of insulator 282 to the transistor 200 side. Alternatively, it is possible to suppress the diffusion of oxygen contained in insulator 224, etc., to the substrate side via insulators 212 and 214. Alternatively, the diffusion of oxygen contained in the insulator 280, etc., upward from the transistor 200 via the insulator 282, etc., can be suppressed. Thus, it is preferable to have a structure in which the transistor 200 is surrounded by insulators 212, 214, and 282, which have the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen.

[0163] Here, it is preferable to use oxides having an amorphous structure as insulators 212, 214, and 282. For example, AlO x (x is any number greater than 0), or MgO yIt is preferable to use a metal oxide such as (y is any number greater than 0). In such amorphous metal oxides, oxygen atoms have dangling bonds, and these dangling bonds may have the property of capturing or fixing hydrogen. By using such an amorphous metal oxide as a component of the transistor 200, or by providing it around the transistor 200, hydrogen contained in the transistor 200, or hydrogen present around the transistor 200, can be captured or fixed. It is particularly preferable to capture or fix hydrogen contained in the channel formation region of the transistor 200. By using an amorphous metal oxide as a component of the transistor 200, or by providing it around the transistor 200, a transistor 200 and semiconductor device with good characteristics and high reliability can be manufactured.

[0164] Furthermore, while insulators 212, 214, and 282 are preferably amorphous, they may also have regions of polycrystalline structure. In addition, insulators 212, 214, and 282 may have a multilayer structure in which an amorphous layer and a polycrystalline layer are stacked. For example, a stacked structure in which a polycrystalline layer is formed on top of an amorphous layer is also possible.

[0165] The insulators 212, 214, and 282 can be deposited, for example, by sputtering. Since sputtering does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration of insulators 212, 214, and 282 can be reduced. The deposition method is not limited to sputtering; chemical vapor deposition (CVD), molecular beam epitaxy (MBE), pulsed laser deposition (PLD), ALD, etc., may be used as appropriate.

[0166] Furthermore, it may be preferable to lower the resistivity of the insulator 212. For example, the resistivity of the insulator 212 is approximately 1 × 10⁻⁶. 13 By setting the resistivity to Ωcm, the insulator 212 may be able to mitigate charge-up of conductors 205, 242, 260, or 240 in processes using plasma in semiconductor device manufacturing. The resistivity of the insulator 212 is preferably 1 × 10⁻⁶. 10 Ωcm or more, 1 × 10 15 The density should be less than or equal to Ωcm.

[0167] Furthermore, it is preferable that insulators 216, 280, and 285 have a lower dielectric constant than insulator 214. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance between wirings can be reduced. For example, silicon oxide, silicon oxynitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, and porous silicon oxide may be used as insulators 216, 280, and 285 as appropriate.

[0168] The conductor 205 is arranged to overlap with the oxide 230 and the conductor 260. Here, it is preferable that the conductor 205 is embedded in an opening formed in the insulator 216. In some cases, a portion of the conductor 205 may be embedded in the insulator 214.

[0169] The conductor 205 comprises a conductor 205a and a conductor 205b. The conductor 205a is provided in contact with the bottom surface and side wall of the opening. The conductor 205b is provided so as to be embedded in a recess formed in the conductor 205a. Here, the height of the upper surface of the conductor 205b is equal to or approximately equal to the height of the upper surface of the conductor 205a and the height of the upper surface of the insulator 216.

[0170] Here, it is preferable to use a conductive material for the conductor 205a that has the function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms. Alternatively, it is preferable to use a conductive material that has the function of suppressing the diffusion of oxygen (for example, at least one such as oxygen atoms and oxygen molecules).

[0171] By using a conductive material that has the function of reducing hydrogen diffusion for the conductor 205a, it is possible to prevent impurities such as hydrogen contained in the conductor 205b from diffusing into the oxide 230 via the insulators 216 and 224. Furthermore, by using a conductive material that has the function of suppressing oxygen diffusion for the conductor 205a, it is possible to suppress the oxidation of the conductor 205b and the resulting decrease in conductivity. As a conductive material that has the function of suppressing oxygen diffusion, it is preferable to use, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, or ruthenium oxide. Therefore, the conductor 205a can be made of the above conductive material in a single layer or a laminate. For example, titanium nitride can be used for the conductor 205a.

[0172] Furthermore, it is preferable to use a conductive material whose main component is tungsten, copper, or aluminum for the conductor 205b. For example, tungsten may be used for the conductor 205b.

[0173] Conductor 205 may function as a second gate electrode. In this case, the threshold voltage (Vth) of transistor 200 can be controlled by changing the potential applied to conductor 205 independently of the potential applied to conductor 260, without linking it to the potential applied to conductor 260. In particular, by applying a negative potential to conductor 205, it is possible to increase the Vth of transistor 200 and reduce the off-current. Therefore, applying a negative potential to conductor 205 reduces the drain current when the potential applied to conductor 260 is 0V compared to not applying a negative potential.

[0174] Furthermore, the electrical resistivity of the conductor 205 is designed considering the potential applied to the conductor 205, and the film thickness of the conductor 205 is set to match this electrical resistivity. Also, the film thickness of the insulator 216 is approximately the same as the film thickness of the conductor 205. Here, it is preferable to make the film thicknesses of the conductor 205 and the insulator 216 as thin as possible within the limits permitted by the design of the conductor 205. By making the film thickness of the insulator 216 thin, the absolute amount of impurities such as hydrogen contained in the insulator 216 can be reduced, thereby reducing the diffusion of these impurities into the oxide 230.

[0175] Furthermore, as shown in Figure 1A, the conductor 205 should be larger than the area of ​​the oxide 230 that does not overlap with the conductors 242a and 242b. In particular, as shown in Figure 1C, it is preferable that the conductor 205 extends to the area outside the ends of the oxide 230a and oxide 230b in the channel width direction. That is, it is preferable that the conductor 205 and the conductor 260 are superimposed on the outside of the side surface of the oxide 230 in the channel width direction, with an insulator in between. With this configuration, the channel-forming region of the oxide 230 can be electrically surrounded by the electric field of the conductor 260, which functions as the first gate electrode, and the electric field of the conductor 205, which functions as the second gate electrode.

[0176] In this specification, a transistor structure in which the channel formation region is electrically surrounded by the electric field of at least the first gate electrode is called a surrounded channel (S-channel) structure. Furthermore, the S-channel structure disclosed in this specification has a structure different from that of the Fin-type structure and the planar-type structure. On the other hand, the S-channel structure disclosed in this specification can also be considered as a type of Fin-type structure. In this specification, the Fin-type structure refers to a structure in which the gate electrode is arranged to surround at least two or more sides of the channel (specifically, two, three, or four sides, etc.). By adopting the Fin-type structure and the S-channel structure, it is possible to increase resistance to short-channel effects, or in other words, to create a transistor in which short-channel effects are less likely to occur.

[0177] By making transistor 200 an S-channel structure as described above, the channel formation region can be electrically surrounded. Since the S-channel structure electrically surrounds the channel formation region, it can be said to be essentially equivalent to a GAA (Gate All Around) structure or an LGAA (Lateral Gate All Around) structure. By making transistor 200 an S-channel, GAA, or LGAA structure, the channel formation region formed at or near the interface between the oxide 230 and the gate insulator can be made from the entire bulk of the oxide 230. Therefore, it becomes possible to improve the current density flowing through the transistor, which can be expected to improve the transistor's on-current or increase its field-effect mobility.

[0178] Although the transistor 200 shown in Figure 1B is an example of an S-channel structure, the semiconductor device of one aspect of the present invention is not limited to this. For example, the transistor structure that can be used in one aspect of the present invention may be one or more selected from the planar structure, fin structure, and GAA structure.

[0179] Furthermore, as shown in Figure 1C, the conductor 205 extends and functions as wiring. However, the configuration is not limited to this, and a conductor that functions as wiring may be provided beneath the conductor 205. Also, it is not necessary to provide one conductor 205 for each transistor. For example, the conductor 205 may be shared by multiple transistors.

[0180] In the transistor 200, the conductor 205 is shown as a stacked structure of conductors 205a and 205b, but the present invention is not limited to this. For example, the conductor 205 may be provided as a single layer or as a stacked structure of three or more layers.

[0181] Insulators 222 and 224 function as second gate insulators.

[0182] Preferably, the insulator 222 has the function of suppressing the diffusion of hydrogen (for example, at least one such as hydrogen atoms and hydrogen molecules). Furthermore, preferably, the insulator 222 has the function of suppressing the diffusion of oxygen (for example, at least one such as oxygen atoms and oxygen molecules). For example, it is preferable that the insulator 222 has the function of suppressing the diffusion of one or both hydrogen and oxygen more effectively than the insulator 224.

[0183] The insulator 222 may be an insulator containing an oxide of one or both of the insulating materials aluminum and hafnium. Preferably, the insulator is an oxide containing aluminum oxide, hafnium oxide, or an oxide containing aluminum and hafnium (hafnium aluminate). Alternatively, an oxide containing hafnium and zirconium, such as hafnium-zirconium oxide, is preferred. When the insulator 222 is formed using such a material, the insulator 222 functions as a layer that suppresses the release of oxygen from the oxide 230 to the substrate side and the diffusion of impurities such as hydrogen from the periphery of the transistor 200 to the oxide 230. Therefore, by providing the insulator 222, the diffusion of impurities such as hydrogen into the inside of the transistor 200 can be suppressed, and the generation of oxygen vacancies in the oxide 230 can be suppressed. In addition, the reaction of the conductor 205 with the oxygen contained in the insulator 224 and the oxide 230 can be suppressed.

[0184] Alternatively, aluminum oxide, bismuth oxide, germanium oxide, niobium oxide, silicon oxide, titanium oxide, tungsten oxide, yttrium oxide, or zirconium oxide may be added to the above insulator. Alternatively, these insulators may be subjected to nitriding treatment. Furthermore, insulator 222 may be used by laminating silicon oxide, silicon oxide nitride, or silicon nitride onto the above insulator.

[0185] Furthermore, the insulator 222 may be a single-layer or multi-layer insulator containing so-called high-k materials, such as aluminum oxide, hafnium oxide, tantalum oxide, zirconium oxide, or hafnium-zirconium oxide. As transistors become smaller and more integrated, thinning of the gate insulator can lead to problems such as leakage current. By using a high-k material as the insulator that functions as the gate insulator, it is possible to reduce the gate potential during transistor operation while maintaining the physical film thickness. In addition, materials with high dielectric constants, such as lead zirconate titanate (PZT), strontium titanate (SrTiO3), and (Ba,Sr)TiO3 (BST), may also be used as the insulator 222.

[0186] The insulator 224 in contact with the oxide 230 can be, for example, silicon oxide, silicon oxide nitride, or the like, as appropriate.

[0187] Furthermore, the insulators 222 and 224 may have a laminated structure of two or more layers. In this case, the laminated structure is not limited to being made of the same material, but may be made of different materials. Also, as shown in Figure 1B, the insulator 224 may be formed in an island shape by being superimposed with the oxide 230a. In this case, the insulator 275 will be in contact with the side surface of the insulator 224 and the upper surface of the insulator 222. In this specification, "island shape" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated.

[0188] Conductors 242a and 242b are provided in contact with the top and side surfaces of oxide 230b, the side surfaces of oxide 230a, and the side surfaces of insulator 224. Here, conductors 242a and 242b can also be configured to be in contact with the side surfaces of insulator 224, oxide 230a, and oxide 230b in the channel length direction, but not in contact with the side surfaces of insulator 224, oxide 230a, and oxide 230b in the channel width direction. In addition, a portion of conductor 242a and a portion of conductor 242b are provided in contact with the top surface of insulator 222. Furthermore, a portion of conductor 242a is provided in contact with the side surfaces of insulator 222 and a portion of insulator 216. Conductors 242a and 242b function as the source electrode or drain electrode of transistor 200, respectively.

[0189] As the conductor 242 (conductor 242a and conductor 242b), it is preferable to use, for example, a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, or a nitride containing titanium and aluminum. In one embodiment of the present invention, a nitride containing tantalum is particularly preferred. Alternatively, for example, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel may be used. These materials are preferred because they are conductive materials that are resistant to oxidation or maintain conductivity even when absorbing oxygen.

[0190] Furthermore, hydrogen contained in oxide 230b, etc., may diffuse into conductor 242a or conductor 242b. In particular, by using tantalum-containing nitrides for conductor 242a and conductor 242b, hydrogen contained in oxide 230b, etc., is more likely to diffuse into conductor 242a or conductor 242b, and the diffused hydrogen may combine with nitrogen present in conductor 242a or conductor 242b. In other words, hydrogen contained in oxide 230b, etc., may be absorbed by conductor 242a or conductor 242b.

[0191] Furthermore, it is preferable that no curved surface is formed between the side surface of the conductor 242 and the top surface of the conductor 242. By using a conductor 242 without such a curved surface, the cross-sectional area of ​​the conductor 242 in the channel width direction can be increased, as shown in Figure 1D and other figures. By increasing the cross-sectional area of ​​the conductor 242, the resistance of the conductor 242 can be reduced, and the on-current of the transistor 200 can be increased.

[0192] Furthermore, as shown in Figure 1A, the conductor 242a has an opening in the region between transistors 200a and 200b. Conductor 240 is positioned so as to overlap with this opening. In a plan view of transistor 200, it is preferable that the size of the opening is smaller than the size of conductor 240. This configuration allows for a region where conductor 242a and conductor 240 are in contact. As a result, conductor 242a and conductor 240 are electrically connected.

[0193] Although Figure 1A shows a memory cell in which the conductors 242a of transistors 200a and 200b are integrated, the present invention is not limited to this configuration. For example, the conductor 242a of transistor 200a and the conductor 242a of transistor 200b may be separated. By using such a configuration, the width of the conductor 242 in the Y direction can be set to the minimum line width, thereby enabling high integration of the semiconductor device. In the above case, a part of the upper surface and a part of the side surface of the conductor 242a of transistor 200a are in contact with the conductor 240, and a part of the upper surface and a part of the side surface of the conductor 242a of transistor 200b are in contact with the conductor 240. With this structure, the conductor 240, which functions as a plug, is electrically connected to transistors 200a and 200b.

[0194] Furthermore, when heat treatment is performed with the conductor 242a (conductor 242b) and the oxide 230b in contact, the sheet resistance of the oxide 230b in the region overlapping with the conductor 242a (conductor 242b) may decrease. Also, the carrier concentration may increase. Therefore, the oxide 230b in the region overlapping with the conductor 242a (conductor 242b) can be made to have a self-aligned low resistance.

[0195] It is preferable that the conductors 242a and 242b are formed using a conductive film having compressive stress. This makes it possible to form a strain that expands in the tensile direction (hereinafter sometimes referred to as tensile strain) in regions 230ba and 230bb. The tensile strain causes V O By stably forming H, regions 230ba and 230bb can be made into stable n-type regions. The compressive stress in conductor 242a is the stress that attempts to relax the compressive shape of conductor 242a, and is a stress with a vector direction from the center to the ends of conductor 242a. The same applies to the compressive stress in conductor 242b.

[0196] The magnitude of the compressive stress of the conductor 242a is preferably 500 MPa or more, more preferably 1000 MPa or more, more preferably 1500 MPa or more, and even more preferably 2000 MPa or more. The magnitude of the stress of the conductor 242a may also be determined by preparing a sample in which the conductive film used for the conductor 242a is deposited on a substrate, and measuring the stress of the sample. The same applies to the magnitude of the compressive stress of the conductor 242b. Examples of conductors having the above-mentioned magnitude of compressive stress include nitrides containing tantalum.

[0197] The compressive stresses of conductors 242a and 242b cause strain to form in regions 230ba and 230bb, respectively. This strain is a strain (tensile strain) that has been expanded in the tensile direction due to the compressive stresses of conductors 242a and 242b. If regions 230ba and 230bb have a CAAC structure, this strain corresponds to elongation in the direction perpendicular to the c-axis of the CAAC structure. Because the CAAC structure is elongated in the direction perpendicular to the c-axis of the CAAC structure, oxygen vacancies are easily formed in this strain. In addition, hydrogen is easily incorporated into this strain, V O H is easily formed. Therefore, under this strain, oxygen deficiency and V O H atoms are easily formed, and these readily adopt stable structures. As a result, regions 230ba and 230bb become stable n-type regions with high carrier concentrations.

[0198] While the strain formed in oxide 230b has been described above, the present invention is not limited thereto. Similar strain may be formed in oxide 230a.

[0199] In the semiconductor device shown in Figures 1A to 1D, the conductor 242 has a two-layer stacked structure. Specifically, the conductor 242a has a conductor 242a1 and a conductor 242a2 on the conductor 242a1. Similarly, the conductor 242b has a conductor 242b1 and a conductor 242b2 on the conductor 242b1. In this case, the conductors 242a1 and 242b1 are arranged on the side that is in contact with the oxide 230b.

[0200] As will be described in detail later, conductors 242a1 and 242a2 can be formed from the same material and using the same process as conductors 242b1 and 242b2, respectively. Therefore, it is preferable that conductor 242a1 has the same conductive material as conductor 242b1. It is also preferable that conductor 242a2 has the same conductive material as conductor 242b2.

[0201] In the following, conductors 242a1 and 242b1 may be collectively referred to as the lower layer of conductor 242. Also, conductors 242a2 and 242b2 may be collectively referred to as the upper layer of conductor 242.

[0202] The lower layers of the conductor 242 (conductors 242a1 and 242b1) are preferably composed of a conductive material that is resistant to oxidation. This suppresses oxidation of the lower layers of the conductor 242 and prevents a decrease in the conductivity of the conductor 242. The lower layers of the conductor 242 may also have properties that easily absorb (extract) hydrogen. This allows hydrogen from the oxide 230 to diffuse into the lower layers of the conductor 242, reducing the hydrogen concentration of the oxide 230. Thus, stable electrical characteristics can be imparted to the transistor 200. Furthermore, the lower layers of the conductor 242 preferably have high compressive stress, and preferably have greater compressive stress than the upper layers of the conductor 242. This allows regions 230ba and 230bb, which are in contact with the lower layers of the conductor 242, to be stable n-type regions with high carrier concentration.

[0203] Furthermore, it is preferable that the upper layers of the conductor 242 (conductors 242a2 and 242b2) have higher conductivity than the lower layers of the conductor 242 (conductors 242a1 and 242b1). For example, the film thickness of the upper layer of the conductor 242 can be made greater than the film thickness of the lower layer of the conductor 242. The upper layer of the conductor 242 may have regions that are more conductive than the lower layer of the conductor 242, at least in part. Alternatively, it is preferable that the upper layer of the conductor 242 is composed of a conductive material with lower resistivity than the lower layer of the conductor 242. This makes it possible to manufacture a semiconductor device with suppressed wiring delay.

[0204] Furthermore, the upper layer of the conductor 242 may have properties that make it easy to absorb hydrogen. This allows hydrogen absorbed into the lower layer of the conductor 242 to diffuse into the upper layer of the conductor 242, further reducing the hydrogen concentration in the oxide 230. Thus, stable electrical characteristics can be imparted to the transistor 200.

[0205] When the conductor 242 has a two-layer laminated structure, one or more of the constituent elements, chemical composition, and film formation conditions of the lower layer and the upper layer of the conductor 242 may be different.

[0206] For example, tantalum nitride or titanium nitride can be used as the lower layer of conductor 242 (conductors 242a1 and 242b1), and tungsten can be used as the upper layer of conductor 242 (conductors 242a2 and 242b2). In this case, conductors 242a1 and 242b1 will be conductors having tantalum or titanium and nitrogen. This configuration suppresses oxidation of the lower layer of conductor 242 and a decrease in the conductivity of conductor 242. Furthermore, with this configuration, conductor 242a2 can be surrounded by an insulator 275 having barrier properties against oxygen and conductor 242a1 having oxidation resistance, and conductor 242b2 can be surrounded by an insulator 275 having barrier properties against oxygen and conductor 242b1 having oxidation resistance. Therefore, it is possible to fabricate a semiconductor device that suppresses the oxidation of conductors 242a2 and 242b2, thereby suppressing wiring delay. Furthermore, by using tungsten as the upper layer of conductor 242, conductor 242 can function as wiring.

[0207] Alternatively, for example, a nitride containing tantalum (e.g., tantalum nitride) may be used as the lower layer of the conductor 242, and a nitride containing titanium (e.g., titanium nitride) may be used as the upper layer of the conductor 242. Since titanium nitride can have higher conductivity than tantalum nitride, the conductivity of the upper layer of the conductor 242 can be made higher than that of the lower layer of the conductor 242. Therefore, the contact resistance with the conductor 240 provided in contact with the upper surface of the conductor 242 can be reduced, making it possible to manufacture a semiconductor device with suppressed wiring delay.

[0208] While examples have been shown in which the lower layer and the upper layer of the conductor 242 are made of different conductive materials, the present invention is not limited thereto.

[0209] The lower layer and the upper layer of the conductor 242 may be made of conductive materials that have the same constituent elements but different chemical compositions. In this case, the lower layer and the upper layer of the conductor 242 can be continuously deposited without exposure to the atmospheric environment. By depositing the film without exposure to the atmosphere, it is possible to prevent impurities or moisture from the atmospheric environment from adhering to the surface of the lower layer of the conductor 242, and to keep the vicinity of the interface between the lower layer and the upper layer of the conductor 242 clean.

[0210] Furthermore, it is preferable to use a tantalum-containing nitride with a high atomic ratio of nitrogen to tantalum in the lower layer of the conductor 242, and a tantalum-containing nitride with a low atomic ratio of nitrogen to tantalum in the upper layer of the conductor 242. For example, as the lower layer of the conductor 242, a tantalum-containing nitride with an atomic ratio of nitrogen to tantalum of 1.0 or more and 2.0 or less, preferably 1.1 or more and 1.8 or less, and more preferably 1.2 or more and 1.5 or less, is used. Alternatively, as the upper layer of the conductor 242, a tantalum-containing nitride with an atomic ratio of nitrogen to tantalum of 0.3 or more and 1.5 or less, preferably 0.5 or more and 1.3 or less, and more preferably 0.6 or more and 1.0 or less, is used.

[0211] In tantalum-containing nitrides, increasing the atomic ratio of nitrogen to tantalum can suppress oxidation of the tantalum-containing nitride. Furthermore, it can improve the oxidation resistance of the tantalum-containing nitride. Additionally, it can suppress the diffusion of oxygen into the tantalum-containing nitride. Therefore, it is preferable to use a tantalum-containing nitride with a high atomic ratio of nitrogen to tantalum as the layer beneath the conductor 242. This prevents the formation of an oxide layer between the layer beneath the conductor 242 and the oxide 230, or reduces the thickness of the oxide layer.

[0212] Furthermore, in tantalum-containing nitrides, the resistivity of the nitride can be reduced by lowering the atomic ratio of nitrogen to tantalum. Therefore, it is preferable to use a tantalum-containing nitride with a low atomic ratio of nitrogen to tantalum as the upper layer of the conductor 242. This makes it possible to manufacture a semiconductor device with suppressed wiring delay.

[0213] Furthermore, in the conductor 242, it may be difficult to clearly detect the boundary between the upper and lower layers. When a nitride containing tantalum is used for the conductor 242, the tantalum and nitrogen concentrations detected within each layer may not be limited to stepwise changes within each layer, but may also change continuously (also called a gradient) in the region between the upper and lower layers. In other words, the closer the region of the conductor 242 is to the oxide 230, the higher the atomic ratio of nitrogen to tantalum should be. Therefore, it is preferable that the atomic ratio of nitrogen to tantalum in the region located below the conductor 242 is higher than the atomic ratio of nitrogen to tantalum in the region located above the conductor 242.

[0214] Although the transistor 200 shows a configuration in which the conductor 242 is a two-layer stacked structure, the present invention is not limited to this. For example, the conductor 242 may be provided as a single layer or as a stacked structure of three or more layers. When a structure has a stacked structure, an ordinal number may be assigned to distinguish it according to the order of formation.

[0215] The conductor 260 is positioned such that its upper surface is at the same or approximately the same height as the top of the insulator 254, the top of the insulator 253, and the upper surface of the insulator 280.

[0216] The conductor 260 functions as the first gate electrode of the transistor 200. Preferably, the conductor 260 has a conductor 260a and a conductor 260b disposed on top of the conductor 260a. For example, it is preferable that the conductor 260a is arranged to enclose the bottom and sides of the conductor 260b. In Figures 1B and 1C, the conductor 260 is shown as a two-layer structure of conductor 260a and conductor 260b, but it may also be a single-layer structure or a stacked structure of three or more layers.

[0217] It is preferable to use a conductive material for the conductor 260a that has the function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, and copper atoms. Alternatively, it is preferable to use a conductive material that has the function of suppressing the diffusion of oxygen (for example, at least one such as oxygen atoms and oxygen molecules).

[0218] Furthermore, because the conductor 260a has the function of suppressing oxygen diffusion, it is possible to suppress the oxidation of the conductor 260b and the resulting decrease in conductivity due to oxygen contained in the insulator 280, etc. As a conductive material that has the function of suppressing oxygen diffusion, it is preferable to use, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, ruthenium oxide, etc.

[0219] Furthermore, the conductor 260 is formed to fill the opening 258 which extends in the channel width direction, and the conductor 260 also extends in the channel width direction. This allows the conductor 260 to function as wiring when multiple transistors 200 are provided. In this case, the insulators 253 and 254 are also provided extending along with the conductor 260.

[0220] Furthermore, since the conductor 260 also functions as wiring, it is preferable to use a conductor with high conductivity. For example, the conductor 260b can be a conductive material mainly composed of tungsten, copper, or aluminum. The conductor 260b may also be in a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above conductive material.

[0221] Furthermore, in transistor 200, the conductor 260 is formed in a self-aligning manner so as to fill the opening 258 formed in the insulator 280 or the like. By forming the conductor 260 in this way, the conductor 260 can be reliably positioned in the region between the conductors 242a and 242b without the need for alignment.

[0222] Furthermore, as shown in Figure 1C, in the channel width direction of transistor 200, with reference to the bottom surface of insulator 222, the height of the bottom surface of the conductor 260 in the region where conductor 260 and oxide 230b do not overlap is preferably lower than the height of the bottom surface of oxide 230b. By configuring conductor 260, which functions as a gate electrode, to cover the side and top surfaces of the channel formation region of oxide 230b via insulator 253 or the like, the electric field of conductor 260 can be more easily applied to the entire channel formation region of oxide 230b. Therefore, the on-current of transistor 200 can be increased and the frequency characteristics can be improved. With reference to the bottom surface of insulator 222, the difference between the height of the bottom surface of conductor 260 in the region where oxide 230a and oxide 230b and conductor 260 do not overlap and the height of the bottom surface of oxide 230b is 0 nm or more and 100 nm or less, preferably 3 nm or more and 50 nm or less, and more preferably 5 nm or more and 20 nm or less.

[0223] The insulator 280 is provided on the insulator 275, and an opening 258 is formed in the region where the insulators 253, 254, and conductor 260 are provided. The upper surface of the insulator 280 may also be flattened.

[0224] The insulator 280, which functions as an interlayer film, preferably has a low dielectric constant. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance occurring between the wiring can be reduced. The insulator 280 is preferably made of the same material as the insulator 216, for example. Silicon oxide and silicon oxynitride are particularly preferred because they are thermally stable. Materials such as silicon oxide, silicon oxynitride, and silicon oxide with vacancies are particularly preferred because they can easily form regions containing oxygen that is desorbed by heating.

[0225] It is preferable that the concentration of impurities such as water and hydrogen in the insulator 280 is reduced. For example, the insulator 280 may be made of silicon oxide such as silicon oxide or silicon oxynitride.

[0226] The insulator 282 is positioned so as to be in contact with at least a portion of the upper surfaces of the conductor 260, insulator 253, insulator 254, and insulator 280.

[0227] The insulator 282 preferably functions as a barrier insulating film that suppresses the diffusion of impurities such as water and hydrogen into the insulator 280 from above, and preferably has the function of capturing impurities such as hydrogen. Furthermore, the insulator 282 preferably functions as a barrier insulating film that suppresses the permeation of oxygen. As the insulator 282, an amorphous metal oxide, such as aluminum oxide, may be used. In this case, the insulator 282 will be an insulator having at least oxygen and aluminum. By providing an insulator 282 that has the function of capturing impurities such as hydrogen in contact with the insulator 280, impurities such as hydrogen contained in the insulator 280 can be captured. In particular, using amorphous aluminum oxide as the insulator 282 is preferable because it may be possible to capture or fix hydrogen more effectively. This makes it possible to manufacture a transistor 200 and a semiconductor device that have good characteristics and are highly reliable.

[0228] As the insulator 282, aluminum oxide is preferably deposited by a sputtering method, and aluminum oxide is more preferably deposited by a pulsed DC sputtering method using an aluminum target in an atmosphere containing an oxygen gas. By using the pulsed DC sputtering method, the thickness distribution can be made more uniform, and the sputtering rate and film quality can be improved. Here, RF (Radio Frequency) power may be applied to the substrate. The amount of oxygen implanted into a layer below the insulator 282 can be controlled by the magnitude of the RF power applied to the substrate. For example, as the RF power is lower, the amount of oxygen implanted into the layer below the insulator 282 is reduced, and even when the insulator 282 is thin, the amount of oxygen is likely to be saturated. Further, as the RF power is higher, the amount of oxygen implanted into the layer below the insulator 282 is increased.

[0229] As the RF power, for example, it is greater than or equal to 0 W / cm 2 and less than or equal to 1.86 W / cm 2 . In other words, by the RF power at the time of formation of the insulator 282, oxygen can be implanted while the amount of oxygen suitable for transistor characteristics is changed. Thus, the amount of oxygen suitable for improving the reliability of the transistor can be implanted. Note that the RF power of 0 W / cm 2 is synonymous with no RF power being applied to the substrate.

[0230] The frequency of the RF power is preferably 10 MHz or higher. Typical example is 13.56 MHz. As the frequency of the RF power is higher, damage to the substrate can be reduced.

[0231] FIGS. 1A to 1D and the like illustrate the structure in which the insulator 282 is a single layer layer; however, the present invention is not limited thereto, and a stacked-layer structure of two or more layers may be employed. For example, the insulator 282 may have a two-layer stacked structure.

[0232] The upper and lower layers of the insulator 282 may be formed from the same material using different methods. For example, when aluminum oxide is deposited as the insulator 282 using pulsed DC sputtering with an aluminum target in an oxygen-containing atmosphere, it is preferable that the RF power applied to the substrate when depositing the lower layer of the insulator 282 is different from the RF power applied to the substrate when depositing the upper layer of the insulator 282, and more preferably that the RF power applied to the substrate when depositing the lower layer of the insulator 282 is lower than the RF power applied to the substrate when depositing the upper layer of the insulator 282. Specifically, the RF power applied to the substrate for depositing the lower layer of the insulator 282 should be 0 W / cm². 2 More than 0.62W / cm 2 The film is formed as follows, and the RF power applied to the substrate above the insulator 282 is 1.86 W / cm². 2 The film is deposited as follows. More specifically, the RF power applied to the substrate is set to 0 W / cm² to deposit the layer below the insulator 282. 2 The film is formed as such, and the RF power applied to the substrate is 0.31 W / cm² to the upper layer of the insulator 282. 2 The film is formed in this manner. By adopting this configuration, the insulator 282 can be made amorphous, and the amount of oxygen supplied to the insulator 280 can be adjusted.

[0233] Furthermore, the RF power applied to the substrate when depositing the lower layer of the insulator 282 may be higher than the RF power applied to the substrate when depositing the upper layer of the insulator 282. Specifically, the RF power applied to the substrate when depositing the lower layer of the insulator 282 may be 1.86 W / cm². 2 The film is formed as follows, and the RF power applied to the substrate is 0 W / cm² on top of the insulator 282. 2 More than 0.62W / cm 2 The film is deposited as follows. More specifically, the RF power applied to the substrate below the insulator 282 is 1.86 W / cm². 2 The film is formed as such, and the RF power applied to the substrate is 0.62 W / cm². 2 The film is formed in this manner. By using this configuration, the amount of oxygen supplied to the insulator 280 can be increased.

[0234] Further, the thickness of the lower layer of the insulator 282 is 1 nm or more and 20 nm or less, preferably 1.5 nm or more and 15 nm or less, more preferably 2 nm or more and 10 nm or less, still more preferably 3 nm or more and 8 nm or less. With this configuration, the lower layer of the insulator 282 can have an amorphous structure regardless of the RF power. Moreover, since the lower layer of the insulator 282 has an amorphous structure, the upper layer of the insulator 282 easily has an amorphous structure, and the insulator 282 can have an amorphous structure.

[0235] Although the lower layer of the insulator 282 and the upper layer of the insulator 282 have a stacked structure made of the same material, the present invention is not limited to this. The lower layer of the insulator 282 and the upper layer of the insulator 282 may have a stacked structure made of different materials.

[0236] The above is the description of the transistor 200.

[0237] [Capacitor 100] FIG. 4A is an enlarged view of the capacitor 100 in FIG. 1B and the vicinity thereof, and FIG. 4B is an enlarged view of the capacitor 100 in FIG. 1D and the vicinity thereof.

[0238] The capacitor 100 includes a conductor 156, an insulator 153, and a conductor 160 (a conductor 160a and a conductor 160b). The conductor 156 functions as one of a pair of electrodes of the capacitor 100 (also referred to as a lower electrode), the conductor 160 functions as the other of the pair of electrodes of the capacitor 100 (also referred to as an upper electrode), and the insulator 153 functions as a dielectric of the capacitor 100.

[0239] At least part of the conductor 156, the insulator 153, the conductor 160a, and the conductor 160b is placed in an opening 158 provided in the insulator 275, the insulator 280, and the insulator 282. The conductor 156 is placed over the conductor 242b, the insulator 153 is placed over the conductor 156, the conductor 160a is placed over the insulator 153, and the conductor 160b is placed over the conductor 160a.

[0240] The conductor 156 is arranged along the openings 158 formed in the insulators 275, 280, and 282. Preferably, the height of a portion of the upper surface of the conductor 156 is higher than the height of the upper surface of the insulator 282. The upper surface of the conductor 242b is in contact with the lower surface of the conductor 156. The conductor 156 is preferably deposited using a film deposition method with good coverage, such as the ALD method or the CVD method, and any conductor that can be used for the conductor 205, conductor 260, or conductor 242 may be used. For example, by using the same conductive material as the conductor 242b for the conductor 156, the contact resistance between the conductor 156 and the conductor 242b can be reduced. For example, titanium nitride or tantalum nitride deposited using the ALD method can be used for the conductor 156.

[0241] The insulator 153 is positioned to cover the conductor 156 and a portion of the insulator 282. It is preferable to use a high-dielectric constant (high-k) material (a material with a high relative permittivity) for the insulator 153. It is preferable to deposit the insulator 153 using a film deposition method that provides good coverage, such as the ALD method or the CVD method.

[0242] Furthermore, as the insulator of the high-dielectric constant (high-k) material, oxides, oxidized nitrides, nitride oxides, or nitrides containing one or more metal elements selected from aluminum, hafnium, zirconium, and gallium can be used. Silicon may also be included in the above oxides, oxidized nitrides, nitride oxides, or nitrides. Additionally, insulating layers made of the above materials can be laminated and used.

[0243] For example, as an insulator made of high-dielectric constant (high-k) material, aluminum oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxides containing aluminum and hafnium, oxides containing silicon and hafnium, oxides containing silicon and hafnium, oxides containing silicon and zirconium, oxides containing silicon and zirconium, oxides containing hafnium and zirconium, oxides containing hafnium and zirconium, etc. can be used. By using such high-k material, the insulator 153 can be made thick enough to suppress leakage current, and the capacitance of the capacitive element 100 can be sufficiently secured.

[0244] Furthermore, it is preferable to use an insulating layer made of the above materials in a laminated manner, and it is preferable to use a laminated structure of a high dielectric constant (high-k) material and a material with a greater dielectric strength than the high dielectric constant (high-k) material. For example, as the insulator 153, an insulating film laminated in the order of zirconium oxide, aluminum oxide, and zirconium oxide can be used. Alternatively, for example, an insulating film laminated in the order of zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide can be used. Alternatively, for example, an insulating film laminated in the order of hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide can be used. By using an insulating material with a relatively high dielectric strength, such as aluminum oxide, in a laminated manner, the dielectric strength can be improved, and electrostatic discharge breakdown of the capacitive element 100 can be suppressed.

[0245] The conductor 160 is positioned to fill the openings 158 formed in the insulators 275, 280, and 282. The conductor 160 is preferably deposited using the ALD method or the CVD method, and any conductor that can be used for the conductor 205 or conductor 260 may be used. For example, titanium nitride deposited using the ALD method can be used as the conductor 160a, and tungsten deposited using the CVD method can be used as the conductor 160b. If the adhesion of tungsten to the insulator 153 is sufficiently high, a single layer of tungsten deposited using the CVD method may be used as the conductor 160.

[0246] The opening 158 is provided so as to reach the conductor 242b. In other words, the opening 158 has a region that overlaps with the conductor 242b. The conductor 242b is the other of the source electrode and drain electrode of the transistor 200, and by contacting the lower surface of the conductor 156 provided in the opening 158, the transistor 200 and the capacitive element 100 can be electrically connected.

[0247] In a plan view, it is preferable that the distance between the aperture 158 and the oxide 230 is small. By adopting such a structure, the occupied area of ​​the memory cell having the capacitive element 100 and the transistor 200 can be reduced. In a plan view, the shape of the aperture 158 may be a rectangle, a polygon other than a rectangle, a polygon with curved corners, or a circle including an ellipse.

[0248] As shown in Figures 4A and 4B, a conductor 156 is provided in contact with the bottom surface and inner wall of the opening 158. Thus, the conductor 156 is in contact with the sides of the insulators 275, 280, and 282, the sides of the conductor 242b1, the sides and top surface of the conductor 242b2, and the top surface of the insulator 222. In addition, an insulator 153 is provided in contact with the top surface of the conductor 156, a conductor 160a is provided in contact with the top surface of the insulator 153, and a conductor 160b is provided in contact with the top surface of the conductor 160a.

[0249] By having the capacitive element 100 adopt the structure described above, a capacitive element 100 can be formed in which the conductor 156 and the conductor 160 are arranged opposite each other on the bottom and side surfaces of the opening 158 via the insulator 153, as shown in Figures 4A and 4B. Therefore, by increasing the depth of the opening 158 (which can also be called the thickness of the insulator 280), the capacitance of the capacitive element 100 can be increased. In this way, by increasing the capacitance per unit area of ​​the capacitive element 100, the read operation of the memory device can be made more stable.

[0250] Furthermore, as shown in Figure 4A, a portion of the conductor 156, a portion of the insulator 153, and a portion of the conductor 160 are provided exposed through the opening 158. In other words, a portion of the conductor 156, a portion of the insulator 153, and a portion of the conductor 160 are formed above the upper surface of the conductor 260 or above the upper surface of the insulator 282.

[0251] A portion of the conductor 156 and a portion of the insulator 153 are in contact with the upper surface of the insulator 282. In other words, the side edge of the conductor 156 is covered by the insulator 153. Furthermore, it is preferable that the conductor 160 has a region that overlaps with the insulator 282 via the insulator 153. Here, as shown in Figure 4A, the side edge of the conductor 160 and the side edge of the insulator 153 roughly coincide. With this configuration, the conductor 160 and the conductor 156 can be separated by the insulator 153, thereby suppressing short circuits between the conductor 160 and the conductor 156.

[0252] Furthermore, the portion of the conductor 160 above the insulator 282 may be routed and formed into a wiring-like structure. For example, as shown in Figure 1D, the conductor 160 can be provided extending in the channel width direction of the transistor 200. This allows the conductor 160 to function as wiring when multiple transistors 200 and capacitive elements 100 are provided. In this case, the insulator 153 can also be provided extending together with the conductor 160.

[0253] In addition, the capacitor 100 may have a structure as illustrated in FIGS. 5A and 5B. Here, FIG. 5A is an enlarged view corresponding to the capacitor 100 in FIG. 1B, and FIG. 5B is an enlarged view corresponding to the capacitor 100 in FIG. 1D.

[0254] As illustrated in FIGS. 5A and 5B, the capacitor 100 may have a configuration in which the topmost portion of the conductor 156 substantially coincides with the upper surface of the insulator 282.

[0255] Furthermore, as illustrated in FIGS. 5A and 5B, the capacitor 100 may have a configuration in which part of the insulator 153 is exposed from the conductor 160.

[0256] In addition, as illustrated in FIG. 5B, the capacitor 100 may have a configuration in which part of the conductor 242b is exposed from the conductor 156 in a cross-sectional view in the channel width direction.

[0257] Furthermore, the capacitor 100 may have a structure as illustrated in FIGS. 6A and 6B. Here, FIG. 6A is an enlarged view corresponding to the capacitor 100 in FIG. 1B, and FIG. 6B is an enlarged view corresponding to the capacitor 100 in FIG. 1D.

[0258] As illustrated in FIG. 6A, in the capacitor 100, the insulator 224, the oxide 230a, and the oxide 230b may be formed below the conductor 242b in the opening 158. In this case, as illustrated in FIG. 6B, it is preferable that the conductor 156 be provided in contact with a side surface of the insulator 224, a side surface of the oxide 230a, a side surface of the oxide 230b, and a side surface of the conductor 242. Accordingly, the capacitor 100 is formed along the side surface of the insulator 224, the side surface of the oxide 230a, the side surface of the oxide 230b, and the side surface of the conductor 242, so that the capacitance of the capacitor 100 can be increased.

[0259] Alternatively, the capacitive element 100 may have a shape, for example, as shown in Figure 6C. Specifically, a portion of the opening 158 overlaps only with the conductor 242b, similar to the structure shown in Figure 5A, while another portion of the opening 158 overlaps with the conductor 242b, oxide 230b, oxide 230a, and insulator 224, similar to the structure shown in Figure 6A.

[0260] Figures 4A to 6C show a configuration in which the side wall of the opening 158 is approximately perpendicular to the upper surface of the insulator 222, but the present invention is not limited to this. The side wall of the opening 158 may be tapered. By making the side wall of the opening 158 tapered, the covering of the insulator 153 and the like can be improved in subsequent processes, and defects such as porosity can be reduced.

[0261] The above is a description of the capacitive element 100.

[0262] The conductor 240 is provided in contact with the inner wall of the opening 206 formed in the insulators 285, 280, 275, conductor 242a, 216, and 212. The conductor 240 also has a region in contact with the upper surface of the conductor 209. It can also be considered that a portion of the conductor 242a is positioned protruding into the opening 206.

[0263] The conductor 240 functions as a plug or wire for electrically connecting the transistor 200 to circuit elements such as switches, transistors, capacitive elements, inductors, resistive elements, and diodes, as well as wiring, electrodes, or terminals.

[0264] The conductor 240 is preferably a laminated structure of conductor 240a and conductor 240b. For example, as shown in Figure 1B, the conductor 240 can be structured such that conductor 240a is provided in contact with the inner wall of the opening, and conductor 240b is provided further inside. In other words, conductor 240a is arranged in the vicinity of insulators 285, 280, 275, conductor 242a, 216, and 212.

[0265] Here, it is preferable that the conductor 240a is deposited using a film deposition method that provides good coverage, such as the ALD method. With this deposition method, the general shape of the conductor 240a generally matches the shape formed by the inner wall of the opening 206. In Figure 1B and other figures, the conductor 240a is shown with a uniform thickness, but in areas that are in the shadow of the conductor 242a, there may be areas with a thinner thickness or areas where no film is deposited.

[0266] As the conductor 240a, it is preferable to use a conductive material that has the function of suppressing the permeation of impurities such as water and hydrogen. For example, it is preferable to use tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, ruthenium oxide, etc. Furthermore, the conductive material that has the function of suppressing the permeation of impurities such as water and hydrogen may be used in a single layer or a laminate. In addition, it is possible to suppress the mixing of impurities such as water and hydrogen contained in the layer above the insulator 282 into the oxide 230 through the conductor 240.

[0267] Furthermore, since the conductor 240 also functions as wiring, it is preferable to use a conductor with high conductivity. For example, the conductor 240b can be a conductive material mainly composed of tungsten, copper, or aluminum.

[0268] For example, it is preferable to use titanium nitride as conductor 240a and tungsten as conductor 240b. In this case, conductor 240a will be a conductor containing titanium and nitrogen, and conductor 240b will be a conductor containing tungsten.

[0269] Although the transistor 200 shows a configuration in which the conductor 240 is made up of stacked conductors 240a and 240b, the present invention is not limited to this. For example, the conductor 240 may be provided as a single layer or as a stacked structure of three or more layers. When the structure has a stacked structure, an ordinal number may be assigned to distinguish it according to the order of formation. Also, although not shown in Figure 1B, the height of the upper surface of the conductor 240 may be higher than the height of the upper surface of the insulator 285.

[0270] Figure 7A shows an enlarged view of the region in contact with the conductor 240 and its vicinity. As shown in Figure 7A, the conductor 240 is arranged within the openings 206 formed in the insulators 285, 280, 275, conductor 242a, 216, and 212. Insulator 214, located between insulators 212 and 216, has an opening 206a. Insulator 222, located between insulators 216 and 275, has an opening 206b. Insulator 282, located between insulators 280 and 285, has an opening 206c. In the cross-sectional view shown in Figure 7A, the width of opening 206 is defined as width W1, the width of opening 206a as width W3a, the width of opening 206b as width W3b, and the width of opening 206c as width W3c.

[0271] Here, Figure 7B shows a plan view corresponding to Figure 7A. As shown in Figure 7B, it is preferable that the opening 206 overlaps with at least a portion of the opening 206a, at least a portion of the opening 206b, and at least a portion of the opening 206c in a plan view. Furthermore, as shown in Figure 7B, it is preferable that the opening 206 is located inside the opening 206a, inside the opening 206b, and inside the opening 206c in a plan view. In this case, as shown in Figure 7A, the width W1 becomes smaller than the widths W3a, W3b, and W3c. Therefore, the sides of insulators 212, 216, 275, 280, and 285 protrude toward the conductor 240 side than the sides of insulators 214, 222, and 282.

[0272] By making the opening 206 structured as described above, the opening 206 can be formed without etching the insulators 214, 222, and 282. As mentioned above, the insulators 214, 222, and 282 are insulating layers made of so-called difficult-to-etch materials, such as aluminum oxide or hafnium oxide. If such insulating layers made of difficult-to-etch materials are sandwiched in the region where the opening 206 is formed, the etching rate of the insulating layers made of difficult-to-etch materials will differ greatly from that of the other insulating layers, which may lead to the formation of abnormal shapes in the opening 206.

[0273] In this embodiment, an opening 206a is formed in the insulator 214, an opening 206b in the insulator 222, and an opening 206c in the insulator 282, superimposed on the region where the opening 206 is formed. This eliminates the need to etch the insulating layer made of a difficult-to-etch material when forming the opening 206, thus enabling the production of the opening 206 with a high yield and improving the productivity of the memory device. Preferably, the side walls of the opening 206 can be provided approximately perpendicular to the substrate surface or the upper surface of the conductor 209. This reduces the area occupied by the opening 206 and the area occupied per memory cell, thereby increasing the storage capacity per unit area of ​​the memory device.

[0274] Furthermore, as shown in Figure 7A, a recess may be formed on the upper surface of the insulator 280, superimposed on the opening 206c of the insulator 282. In addition, an insulator 285 may be formed to fill the opening 206c and the recess. In this case, the insulator 285 will be formed between the insulator 282 and the conductor 240.

[0275] Similarly, a recess may be formed on the upper surface of the insulator 216, superimposed on the opening 206b of the insulator 222. Furthermore, conductors 242a1 and 242a2 may be formed to fill the opening 206b and the recess. In this case, conductors 242a1 and 242a2 will be formed between the insulator 222 and the conductor 240.

[0276] Similarly, a recess may be formed on the upper surface of the insulator 212, superimposed on the opening 206a of the insulator 214. Furthermore, an insulator 216 may be formed to fill the opening 206a and the recess. In this case, the insulator 216 will be formed between the insulator 214 and the conductor 240. Note that if the thickness of the insulator 212 is thin, an opening may be formed in the insulator 212 that superimposes the opening 206a. In this case, a part of the insulator 216 will be in contact with a part of the conductor 209.

[0277] In Figure 7B, the shapes of the openings 206, 206a, 206b, and 206c are shown as quadrilaterals in plan view, but the invention is not limited to this. For example, the openings 206, 206a, 206b, and 206c may be circular, elliptical or other approximately circular shapes, quadrilaterals or other polygonal shapes, or quadrilaterals or other polygonal shapes with rounded corners in plan view. Also, in Figure 7B, the ends of openings 206a, 206b, and 206c are shown to be roughly coincidental in plan view, but the present invention is not limited to this. The sizes of openings 206a, 206b, and 206c may be different, and their respective ends may not roughly coincide in plan view. Furthermore, in Figure 7A, the side wall of opening 206 is shown to be roughly perpendicular to the upper surface of the conductor 209, but the present invention is not limited to this, and the side wall of opening 206 may be tapered.

[0278] Furthermore, as shown in Figure 7A, in the A1-A2 direction, the conductor 240 has a region having a width W1 and a region having a width W2. Width W1 corresponds to the width of the conductor 240 in contact with the side wall of the opening 206. Width W2 corresponds to the width of the opening in the conductor 242a. Note that, as described above, if the conductor 242a is provided separately on the transistor 200a side and the transistor 200b side, width W2 corresponds to the distance between the conductor 242a on the transistor 200a side and the conductor 242a on the transistor 200b side.

[0279] As shown in Figure 7A, it is preferable that the width W1 is greater than the width W2. In this configuration, the conductor 240 is in contact with at least a portion of the upper surface and a portion of the side surface of the conductor 242a. Therefore, the area of ​​the region in contact between the conductor 240 and the conductor 242a can be increased. Here, as shown in Figure 7A, in the opening 206, the side surface of the conductor 242a protrudes from the side surfaces of the insulators 280 and 275. In this specification, the contact between the conductor 240 and the conductor 242a is sometimes referred to as a top-side contact.

[0280] Furthermore, as shown in Figure 7A, the conductor 240 may be in contact with a portion of the lower surface of the conductor 242a. This configuration allows for an even larger area of ​​contact between the conductor 240 and the conductor 242a. Here, as shown in Figure 7A, in the opening 206, the side surface of the conductor 242a protrudes from the side surface of the insulator 216.

[0281] As described above, by increasing the contact area between the conductor 240 and the conductor 242a, contact resistance can be reduced. This makes it possible to improve the operating speed and reduce the power consumption of the memory device according to the present invention.

[0282] Furthermore, as described above, if a recess is formed on the upper surface of the insulator 216 that overlaps with the opening 206b, the conductors 242a1 and 242a2 are formed to fill the recess. At this time, the conductor 242a1 is in contact with the upper and side surfaces of the oxide 230b, the side surfaces of the oxide 230a, the side surfaces of the insulator 224, the side surfaces of the insulator 222, and the upper and side surfaces of the recess of the insulator 216.

[0283] The conductor 209 functions as part of a circuit element such as a switch, transistor, capacitive element, inductor, resistor, and diode, as well as as wiring, an electrode, or a terminal.

[0284] Furthermore, the insulator 210 functions as an interlayer film. The insulator 210 can be any insulator that can be used for the aforementioned insulators 214 and 216.

[0285] <Component materials for semiconductor devices> The following describes the constituent materials that can be used in semiconductor devices.

[0286] <<Substrate>> As the substrate for forming transistor 200, for example, an insulating substrate, a semiconductor substrate, or a conductive substrate may be used. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (such as yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon and germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Furthermore, there are semiconductor substrates having insulating regions within the aforementioned semiconductor substrates, such as SOI (Silicon On Insulator) substrates. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Alternatively, there are substrates having metal nitrides or metal oxides. Furthermore, there are substrates on which a conductor or semiconductor is provided on an insulating substrate, substrates on which a conductor or insulator is provided on a semiconductor substrate, and substrates on which a semiconductor or insulator is provided on a conductive substrate. Alternatively, substrates with elements mounted on them may be used. Examples of elements mounted on the substrate include capacitive elements, resistive elements, switch elements, light-emitting elements, and memory elements.

[0287] <<Insulator>> Insulators include insulating oxides, nitrides, oxidized nitrides, nitride oxides, metal oxides, metal oxidized nitrides, and metal nitride oxides.

[0288] For example, as transistors become smaller and more integrated, thinning of the gate insulator can lead to problems such as leakage current. By using a high-k material for the insulator that functions as the gate insulator, it is possible to lower the voltage during transistor operation while maintaining the physical film thickness. On the other hand, by using a material with a low dielectric constant for the insulator that functions as the interlayer film, parasitic capacitance between wiring can be reduced. Therefore, it is best to select the material according to the function of the insulator.

[0289] Furthermore, examples of insulators with high dielectric constants include gallium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxidized nitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxidized nitrides containing silicon and hafnium, or nitrides containing silicon and hafnium.

[0290] Insulators with low dielectric constants include silicon oxide, silicon oxide nitride, silicon oxide nitride, silicon nitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, silicon oxide with vacancies, or resins.

[0291] Furthermore, the electrical properties of transistors using metal oxides can be stabilized by surrounding them with an insulator that has the function of suppressing the permeation of impurities such as hydrogen and oxygen. As an insulator that has the function of suppressing the permeation of impurities such as hydrogen and oxygen, for example, an insulator containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, or tantalum can be used in a single layer or in a multilayer structure. Specifically, as an insulator that has the function of suppressing the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon oxide nitride, and silicon nitride can be used.

[0292] Furthermore, the insulator that functions as a gate insulator is preferably an insulator that has a region containing oxygen that is desorbed by heating. For example, by having a silicon oxide or silicon oxynitride having a region containing oxygen that is desorbed by heating in contact with the oxide 230, the oxygen deficiency of the oxide 230 can be compensated for.

[0293] <<Conductive material>> As the conductor, it is preferable to use a metallic element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above metallic elements, or an alloy combining the above metallic elements. For example, it is preferable to use tantalum nitride, titanium nitride, tungsten, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, oxides containing lanthanum and nickel, etc. Furthermore, tantalum nitride, titanium nitride, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel are preferred because they are conductive materials that are resistant to oxidation or maintain conductivity even when absorbing oxygen. Alternatively, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements like phosphorus, or silicides such as nickel silicide may be used.

[0294] Furthermore, multiple conductive layers formed from the above materials may be used in a laminated structure. For example, a laminated structure may be formed by combining the aforementioned metal element material with an oxygen-containing conductive material. Alternatively, a laminated structure may be formed by combining the aforementioned metal element material with a nitrogen-containing conductive material. Alternatively, a laminated structure may be formed by combining the aforementioned metal element material with an oxygen-containing conductive material and a nitrogen-containing conductive material.

[0295] Furthermore, when using an oxide in the channel formation region of a transistor, it is preferable to use a laminated structure for the conductor functioning as the gate electrode, which combines a material containing the aforementioned metal element with a conductive material containing oxygen. In this case, it is preferable to provide the conductive material containing oxygen on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen detached from the conductive material is more easily supplied to the channel formation region.

[0296] In particular, it is preferable to use a conductive material containing metal elements and oxygen contained in the metal oxide in which the channel is formed as the conductor that functions as the gate electrode. Alternatively, conductive materials containing the aforementioned metal elements and nitrogen may be used. For example, conductive materials containing nitrogen such as titanium nitride and tantalum nitride may be used. In addition, indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and silicon-doped indium tin oxide may be used. In addition, indium gallium zinc oxide containing nitrogen may be used. By using such materials, it may be possible to capture hydrogen contained in the metal oxide in which the channel is formed. Alternatively, it may be possible to capture hydrogen that is mixed in from an external insulator or the like.

[0297] <<Metal Oxides>> It is preferable to use a metal oxide (oxide semiconductor) that functions as a semiconductor as oxide 230. Below, metal oxides applicable to oxide 230 according to the present invention will be described.

[0298] The metal oxide preferably contains at least indium or zinc. In particular, it is preferable that it contains indium and zinc. In addition, it is preferable that it contains aluminum, gallium, yttrium, tin, etc. It may also contain one or more selected from boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, cobalt, etc.

[0299] Here, we consider the case where the metal oxide is an In-M-Zn oxide containing indium, element M, and zinc. Element M is aluminum, gallium, yttrium, or tin. Other elements that can be used for element M include boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, magnesium, and cobalt. However, it is also possible to use a combination of multiple of the aforementioned elements for element M. In particular, it is preferable that element M is one or more elements selected from gallium, aluminum, yttrium, and tin.

[0300] In particular, it is preferable to use an oxide containing indium (In), gallium (Ga), and zinc (Zn) (also written as IGZO) as the semiconductor layer of the transistor. Alternatively, an oxide containing indium (In), aluminum (Al), and zinc (Zn) (also written as IAZO) may be used as the semiconductor layer of the transistor. Alternatively, an oxide containing indium (In), aluminum (Al), gallium (Ga), and zinc (Zn) (IAGZO or IGAZO) may be used as the semiconductor layer.

[0301] In this specification, metal oxides containing nitrogen may also be collectively referred to as metal oxides. Furthermore, metal oxides containing nitrogen may also be called metal oxynitrides.

[0302] In the following sections, we will describe oxides containing indium (In), gallium (Ga), and zinc (Zn) as examples of metal oxides. Note that oxides containing indium (In), gallium (Ga), and zinc (Zn) are sometimes called In-Ga-Zn oxides.

[0303] <Classification of crystal structures> Examples of crystalline structures for oxide semiconductors include amorphous (including completely amorphous), CAAC (c-axis-aligned crystalline), nc (nanocrystalline), CAC (cloud-aligned composite), single crystal, and polycrystal.

[0304] The crystal structure of a film or substrate can be evaluated using X-ray diffraction (XRD) spectroscopy. For example, it can be evaluated using the XRD spectrum obtained from a GIXD (Grazing-Incidence XRD) measurement. The GIXD method is also known as the thin-film method or the Seemann-Bohlin method. In the following text, the XRD spectrum obtained from a GIXD measurement may simply be referred to as the XRD spectrum.

[0305] For example, in a quartz glass substrate, the peak shape of the XRD spectrum is nearly symmetrical. On the other hand, in an In-Ga-Zn oxide film with a crystalline structure, the peak shape of the XRD spectrum is asymmetrical. The asymmetrical shape of the XRD spectrum peaks clearly indicates the presence of crystals in the film or substrate. In other words, if the peak shape of the XRD spectrum is not symmetrical, the film or substrate cannot be said to be in an amorphous state.

[0306] Furthermore, the crystalline structure of a film or substrate can be evaluated by the diffraction pattern (also called the nano-beam electron diffraction pattern) observed using nano-beam electron diffraction (NBED). For example, a halo is observed in the diffraction pattern of a quartz glass substrate, confirming that the quartz glass is in an amorphous state. On the other hand, a spot-like pattern is observed in the diffraction pattern of an In-Ga-Zn oxide film deposited at room temperature, rather than a halo. Therefore, it is presumed that the In-Ga-Zn oxide deposited at room temperature is in an intermediate state, neither single-crystal nor polycrystalline, nor amorphous, and cannot be concluded to be in an amorphous state.

[0307] <<Oxide semiconductor structure>> It should be noted that oxide semiconductors may be classified differently from those described above when considering their structure. For example, oxide semiconductors can be divided into single-crystal oxide semiconductors and other non-single-crystal oxide semiconductors. Examples of non-single-crystal oxide semiconductors include the aforementioned CAAC-OS and nc-OS. Non-single-crystal oxide semiconductors also include polycrystalline oxide semiconductors, pseudo-amorphous oxide semiconductors (a-like OS), and amorphous oxide semiconductors.

[0308] Here, we will explain the details of the CAAC-OS, nc-OS, and a-like OS mentioned above.

[0309] [CAAC-OS] CAAC-OS is an oxide semiconductor having multiple crystalline regions, the c-axis of which is oriented in a specific direction. This specific direction is the thickness direction of the CAAC-OS film, the normal direction to the surface on which the CAAC-OS film is formed, or the normal direction to the surface of the CAAC-OS film. A crystalline region is a region with periodic atomic arrangement. If we consider the atomic arrangement as a lattice arrangement, then a crystalline region is also a region with a aligned lattice arrangement. Furthermore, CAAC-OS has regions where multiple crystalline regions are connected in the ab-plane direction, and these regions may exhibit distortion. Distortion refers to a point in the connected region where the orientation of the lattice arrangement changes between a region with a aligned lattice arrangement and another region with a aligned lattice arrangement. In short, CAAC-OS is an oxide semiconductor that is c-axis oriented and does not exhibit clear orientation in the ab-plane direction.

[0310] Each of the above-mentioned crystalline regions is composed of one or more minute crystals (crystals with a maximum diameter of less than 10 nm). When a crystalline region is composed of one minute crystal, the maximum diameter of that crystalline region will be less than 10 nm. When a crystalline region is composed of many minute crystals, the maximum diameter of that crystalline region may be around several tens of nm.

[0311] Furthermore, in In-Ga-Zn oxides, CAAC-OS tends to have a layered crystalline structure (also called a layered structure) consisting of layers containing indium (In) and oxygen (hereinafter referred to as the In layer) and layers containing gallium (Ga), zinc (Zn), and oxygen (hereinafter referred to as the (Ga,Zn) layer). Note that indium and gallium are mutually substitutable. Therefore, the (Ga,Zn) layer may contain indium. Also, the In layer may contain gallium. Also, the In layer may contain zinc. This layered structure can be observed, for example, as a lattice image in high-resolution TEM (Transmission Electron Microscope) images.

[0312] When structural analysis of a CAAC-OS film is performed using an XRD instrument, for example, out-of-plane XRD measurements using θ / 2θ scanning show a peak indicating c-axis orientation at 2θ = 31° or nearby. Note that the position of the c-axis orientation peak (value of 2θ) may vary depending on the type and composition of the metal elements constituting the CAAC-OS.

[0313] Furthermore, for example, multiple bright spots are observed in the electron diffraction pattern of a CAAC-OS film. These spots are observed at point-symmetric positions with respect to the incident electron beam spot (also called the direct spot) that passed through the sample.

[0314] When the crystal region is observed from the specific direction described above, the lattice arrangement within that crystal region is based on a hexagonal lattice, but the unit cell is not necessarily a regular hexagon and may be non-regular hexagonal. Furthermore, the strain may have lattice arrangements such as pentagons or heptagons. Moreover, in CAAC-OS, clear grain boundaries cannot be observed even near the strain. In other words, it can be seen that the formation of grain boundaries is suppressed by the strain in the lattice arrangement. This is thought to be because CAAC-OS can tolerate strain due to the fact that the arrangement of oxygen atoms is not dense in the ab-plane direction, and the bond distance between atoms changes due to the substitution of metal atoms.

[0315] Furthermore, a crystal structure in which clear grain boundaries can be observed is called a polycrystalline material. Grain boundaries act as recombination centers, trapping carriers and potentially causing a decrease in transistor on-current and field-effect mobility. Therefore, CAAC-OS, in which clear grain boundaries cannot be observed, is one of the crystalline oxides with a suitable crystal structure for the semiconductor layer of a transistor. In addition, a structure containing Zn is preferred for the composition of CAAC-OS. For example, In-Zn oxide and In-Ga-Zn oxide are preferred because they can suppress the generation of grain boundaries more effectively than In oxide.

[0316] CAAC-OS is an oxide semiconductor with high crystallinity and no clearly defined grain boundaries. Therefore, CAAC-OS is less susceptible to the decrease in electron mobility caused by grain boundaries. Furthermore, since the crystallinity of oxide semiconductors can decrease due to the inclusion of impurities and the generation of defects, CAAC-OS can be said to be an oxide semiconductor with few impurities and defects (such as oxygen vacancies). Consequently, oxide semiconductors containing CAAC-OS have stable physical properties. Therefore, oxide semiconductors containing CAAC-OS are heat-resistant and highly reliable. In addition, CAAC-OS is stable even at high temperatures (so-called thermal budget) during the manufacturing process. Therefore, using CAAC-OS in transistors with metal oxide in the channel formation region (sometimes called OS transistors) allows for greater flexibility in the manufacturing process.

[0317] [nc-OS] nc-OS exhibits periodicity in atomic arrangement in minute regions (e.g., regions between 1 nm and 10 nm, particularly between 1 nm and 3 nm). In other words, nc-OS contains minute crystals. These minute crystals are also called nanocrystals because their size is, for example, between 1 nm and 10 nm, particularly between 1 nm and 3 nm. Furthermore, nc-OS shows no regularity in crystal orientation between different nanocrystals. Therefore, no orientation is observed throughout the film. Consequently, depending on the analytical method, nc-OS may be indistinguishable from a-like OS or amorphous oxide semiconductors. For example, when structural analysis of an nc-OS film is performed using an XRD instrument, no peaks indicating crystallinity are detected in out-of-plane XRD measurements using θ / 2θ scanning. Also, when electron diffraction (also called limited-field electron diffraction) is performed on an nc-OS film using an electron beam with a probe diameter larger than that of the nanocrystals (e.g., 50 nm or larger), a diffraction pattern resembling a halo pattern is observed. On the other hand, when electron diffraction (also called nanobeam electron diffraction) is performed on an nc-OS film using an electron beam with a probe diameter close to or smaller than the size of the nanocrystal (for example, 1 nm to 30 nm), an electron diffraction pattern may be obtained in which multiple spots are observed within a ring-shaped region centered on the direct spot.

[0318] [a-like OS] a-like OS is an oxide semiconductor having a structure between nc-OS and amorphous oxide semiconductors. a-like OS has porous or low-density regions. That is, a-like OS has lower crystallinity compared to nc-OS and CAAC-OS. Also, a-like OS has a higher hydrogen concentration in the film compared to nc-OS and CAAC-OS.

[0319] <<Oxide Semiconductor Composition>> Next, we will explain the details of CAC-OS mentioned above. Note that CAC-OS refers to the material composition.

[0320] [CAC-OS] CAC-OS is a material composition in which, for example, the elements constituting the metal oxide are unevenly distributed in sizes of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or close to that size. In the following, a state in which one or more metal elements are unevenly distributed in a metal oxide, and the regions containing these metal elements are mixed in sizes of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or close to that size, is also referred to as a mosaic or patchy state.

[0321] Furthermore, CAC-OS is a composite metal oxide having a mosaic-like structure formed by the separation of the material into a first region and a second region, with the first region distributed within the film (hereinafter also referred to as a cloud-like structure). In other words, CAC-OS is a composite metal oxide having a structure in which the first region and the second region are mixed.

[0322] Here, the atomic ratios of In, Ga, and Zn to the metal elements constituting the CAC-OS in In-Ga-Zn oxide are denoted as [In], [Ga], and [Zn], respectively. For example, in the CAC-OS of In-Ga-Zn oxide, the first region is the region where [In] is greater than the [In] in the composition of the CAC-OS film. The second region is the region where [Ga] is greater than the [Ga] in the composition of the CAC-OS film. Alternatively, for example, the first region is the region where [In] is greater than the [In] in the second region, and [Ga] is smaller than the [Ga] in the second region. The second region is the region where [Ga] is greater than the [Ga] in the first region, and [In] is smaller than the [In] in the first region.

[0323] Specifically, the first region described above is a region whose main components are indium oxide, indium zinc oxide, etc. The second region described above is a region whose main components are gallium oxide, gallium zinc oxide, etc. In other words, the first region can be rephrased as a region whose main component is In. Similarly, the second region can be rephrased as a region whose main component is Ga.

[0324] Furthermore, a clear boundary may not be observed between the first region and the second region described above.

[0325] Furthermore, CAC-OS in In-Ga-Zn oxide refers to a material composition containing In, Ga, Zn, and O, in which regions with Ga as the main component and regions with In as the main component are arranged in a mosaic-like fashion, with these regions existing randomly. Therefore, it is presumed that CAC-OS has a structure in which the metallic elements are unevenly distributed.

[0326] CAC-OS can be formed, for example, by sputtering under conditions where the substrate is not heated. When forming CAC-OS by sputtering, one or more gases selected from inert gases (typically argon), oxygen gas, and nitrogen gas may be used as the deposition gas. Furthermore, a lower ratio of the oxygen gas flow rate to the total deposition gas flow rate during deposition is preferable. For example, the ratio of the oxygen gas flow rate to the total deposition gas flow rate during deposition should be 0% or more and less than 30%, preferably 0% or more and 10% or less.

[0327] Furthermore, for example, in the case of CAC-OS in In-Ga-Zn oxide, EDX mapping obtained using energy dispersive X-ray spectroscopy (EDX) confirms that it has a structure in which regions mainly composed of In (first region) and regions mainly composed of Ga (second region) are unevenly distributed and mixed.

[0328] Here, the first region is a region with higher conductivity compared to the second region. In other words, the conductivity of the metal oxide is exhibited when carriers flow through the first region. Therefore, a high field-effect mobility (μ) can be achieved when the first region is distributed in a cloud-like manner within the metal oxide.

[0329] On the other hand, the second region is a region with higher insulating properties compared to the first region. In other words, the distribution of the second region within the metal oxide can suppress leakage current.

[0330] Therefore, when CAC-OS is used in a transistor, the conductivity due to the first region and the insulation due to the second region work complementaryly to give CAC-OS a switching function (on / off function). In other words, CAC-OS has conductive function in part of the material, insulating function in part of the material, and semiconductor function as a whole. By separating the conductive function and the insulating function, both functions can be maximized. Therefore, by using CAC-OS in a transistor, a high on-current (I on This enables high field-effect mobility (μ) and good switching operation.

[0331] Furthermore, transistors using CAC-OS offer high reliability. Therefore, CAC-OS is ideal for various semiconductor devices, including display devices.

[0332] Oxide semiconductors can take on diverse structures, each possessing different properties. One embodiment of the present invention may include two or more of the following: amorphous oxide semiconductors, polycrystalline oxide semiconductors, a-like OS, CAC-OS, nc-OS, and CAAC-OS.

[0333] <Transistors containing oxide semiconductors> Next, we will explain the case where the above oxide semiconductor is used in a transistor.

[0334] By using the above-mentioned oxide semiconductor in transistors, it is possible to realize transistors with high field-effect mobility. Furthermore, it is possible to realize highly reliable transistors.

[0335] It is preferable to use an oxide semiconductor with a low carrier concentration for the transistor. For example, the carrier concentration of an oxide semiconductor is 1 × 10⁻⁶. 17 cm -3 The following is preferably 1 × 10 15 cm -3 More preferably 1 × 10 13 cm -3 More preferably 1 × 10 11 cm -3 More preferably 1 × 10 10 cm -3 It is less than 1 × 10 -9 cm -3 This concludes the explanation. Furthermore, when lowering the carrier concentration of an oxide semiconductor film, the impurity concentration in the oxide semiconductor film should be lowered to reduce the defect level density. In this specification, a low impurity concentration and low defect level density are referred to as high-purity intrinsic or substantially high-purity intrinsic. Note that oxide semiconductors with low carrier concentrations are sometimes referred to as high-purity intrinsic or substantially high-purity intrinsic oxide semiconductors.

[0336] Furthermore, oxide semiconductor films that are highly pure or substantially highly pure have a low defect level density, which may result in a low trap level density.

[0337] Furthermore, charges trapped in the trap levels of oxide semiconductors can take a long time to disappear, sometimes behaving like fixed charges. Therefore, transistors in which channel formation regions are formed in oxide semiconductors with a high trap level density may exhibit unstable electrical properties.

[0338] Therefore, reducing the impurity concentration in the oxide semiconductor is effective in stabilizing the electrical characteristics of a transistor. Furthermore, in order to reduce the impurity concentration in the oxide semiconductor, it is preferable to also reduce the impurity concentration in adjacent films. Examples of impurities include hydrogen, nitrogen, alkali metals, alkaline earth metals, iron, nickel, and silicon. Note that impurities in an oxide semiconductor refer to elements other than the main components that make up the oxide semiconductor. For example, elements with a concentration of less than 0.1 atomic percent can be considered impurities.

[0339] <Impurities> Here, we will explain the effects of various impurities in oxide semiconductors.

[0340] In oxide semiconductors, the presence of silicon or carbon, which are both Group 14 elements, leads to the formation of defect levels in the oxide semiconductor. Therefore, the concentration of silicon or carbon in the oxide semiconductor (the concentration obtained by secondary ion mass spectrometry (SIMS)) is 2 × 10⁻¹⁰. 18 atoms / cm 3 The following is preferably 2 × 10 17 atoms / cm 3 The following applies:

[0341] Furthermore, if an oxide semiconductor contains alkali metals or alkaline earth metals, it may form defect levels and generate carriers. Therefore, transistors using oxide semiconductors containing alkali metals or alkaline earth metals tend to exhibit normally-on characteristics. For this reason, the concentration of alkali metals or alkaline earth metals in the oxide semiconductor obtained by SIMS should be set to 1 × 10⁻⁶. 18 atoms / cm 3 The following is preferably 2 × 10 16 atoms / cm 3 Do the following:

[0342] Furthermore, in oxide semiconductors, the presence of nitrogen generates electrons, which act as carriers, increasing the carrier concentration and making it easier for the semiconductor to become n-type. As a result, transistors using oxide semiconductors containing nitrogen tend to exhibit normally-on characteristics. Alternatively, the presence of nitrogen in oxide semiconductors can lead to the formation of trap levels. As a result, the electrical properties of the transistor may become unstable. For this reason, the nitrogen concentration in oxide semiconductors obtained by SIMS should be set to 5 × 10⁻⁶. 19 atoms / cm 3 Less than 5 × 10 18 atoms / cm 3 More preferably 1 × 10 18atoms / cm 3 More preferably 5 × 10 17 atoms / cm 3 Do the following:

[0343] Furthermore, hydrogen contained in oxide semiconductors can react with oxygen bonded to metal atoms to form water, potentially creating oxygen vacancies. Hydrogen can then fill these vacancies, generating electrons as carriers. Additionally, some of the hydrogen can combine with oxygen bonded to metal atoms to generate electrons. Therefore, transistors using oxide semiconductors containing hydrogen tend to exhibit normally-on characteristics. For this reason, it is preferable to reduce the hydrogen content in oxide semiconductors as much as possible. Specifically, the hydrogen concentration in the oxide semiconductor obtained by SIMS should be 1 × 10⁻⁶. 20 atoms / cm 3 Less than 1 × 10 19 atoms / cm 3 Less than 5x10 18 atoms / cm 3 Less than 1 × 10 18 atoms / cm 3 Make it less than.

[0344] By using an oxide semiconductor with sufficiently reduced impurities in the channel formation region of a transistor, stable electrical characteristics can be provided.

[0345] <<Other Semiconductor Materials>> The semiconductor material that can be used for oxide 230 is not limited to the metal oxides described above. A semiconductor material having a band gap (a semiconductor material that is not a zero-gap semiconductor) may be used as oxide 230. For example, it is preferable to use semiconductors of elemental elements such as silicon, compound semiconductors such as gallium arsenide, or layered materials that function as semiconductors (also called atomic layer materials, two-dimensional materials, etc.) as semiconductor materials. In particular, it is preferable to use layered materials that function as semiconductors as semiconductor materials.

[0346] In this specification, the term "layered material" refers to a group of materials having a layered crystalline structure. A layered crystalline structure is a structure in which layers formed by covalent or ionic bonds are stacked via weaker bonds than covalent or ionic bonds, such as van der Waals forces. Layered materials have high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, it is possible to provide a transistor with a large on-current.

[0347] Layered materials include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogens. Chalcogens are a general term for elements belonging to Group 16, and include oxygen, sulfur, selenium, tellurium, polonium, and livermorium. Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides.

[0348] As oxide 230, it is preferable to use, for example, a transition metal chalcogenide that functions as a semiconductor. Specific examples of transition metal chalcogenides applicable as oxide 230 include molybdenum sulfide (typically MoS2), molybdenum selenide (typically MoSe2), molybdenum tellurium (typically MoTe2), tungsten sulfide (typically WS2), tungsten selenide (typically WSe2), tungsten tellurium (typically WTe2), hafnium sulfide (typically HfS2), hafnium selenide (typically HfSe2), zirconium sulfide (typically ZrS2), and zirconium selenide (typically ZrSe2). By applying the above-mentioned transition metal chalcogenides to oxide 230, a semiconductor device with a high on-current can be provided.

[0349] <Examples of semiconductor device fabrication methods> Next, a method for manufacturing a semiconductor device, which is one embodiment of the present invention as shown in Figures 1A to 1D, will be explained using Figures 8A to 28D.

[0350] In each figure, A shows a top view. In each figure, B is a cross-sectional view corresponding to the area indicated by the dashed line A1-A2 in A, and is also a cross-sectional view of transistor 200 in the channel length direction. In each figure, C is a cross-sectional view corresponding to the area indicated by the dashed line A3-A4 in A, and is also a cross-sectional view of transistor 200 in the channel width direction. In each figure, D is a cross-sectional view of the area indicated by the dashed line A5-A6 in A. Note that in the top view A of each figure, some elements have been omitted for clarity.

[0351] In the following, insulating materials for forming insulators, conductive materials for forming conductors, or semiconductor materials for forming semiconductors can be deposited using methods such as sputtering, CVD, MBE, PLD, and ALD as appropriate.

[0352] Sputtering methods include RF sputtering, which uses a high-frequency power supply; DC sputtering, which uses a direct current power supply; and pulsed DC sputtering, which changes the voltage applied to the electrodes in pulses. RF sputtering is mainly used for depositing insulating films, while DC sputtering is mainly used for depositing conductive metal films. Pulsed DC sputtering is mainly used when depositing compounds such as oxides, nitrides, and carbides using reactive sputtering.

[0353] Furthermore, CVD methods can be classified into plasma CVD (PECVD), which utilizes plasma; thermal CVD (TCVD), which utilizes heat; and photo CVD (Photo CVD), which utilizes light. They can also be further divided into metal CVD (MCVD) and metal-organic CVD (MOCVD) depending on the source gas used.

[0354] Plasma CVD allows for the production of high-quality films at relatively low temperatures. Thermal CVD, on the other hand, does not use plasma, thus minimizing plasma damage to the workpiece. For example, wiring, electrodes, and elements (transistors, capacitive elements, etc.) contained in semiconductor devices can be charged up by receiving charge from the plasma. In this case, the accumulated charge can destroy the wiring, electrodes, and elements contained in the semiconductor device. In contrast, thermal CVD, which does not use plasma, does not cause such plasma damage, thus increasing the yield of semiconductor devices. Furthermore, because thermal CVD does not cause plasma damage during film formation, films with fewer defects can be obtained.

[0355] Furthermore, ALD methods such as thermal ALD, which carries out the reaction of the precursor and reactant using only thermal energy, and PEALD, which uses plasma-excited reactants, can be used.

[0356] CVD and ALD methods differ from sputtering, where particles emitted from a target or other source are deposited. Therefore, they are less affected by the shape of the workpiece and provide good step-level coating. In particular, the ALD method is suitable for coating the surface of openings with high aspect ratios due to its excellent step-level coating and uniform thickness. However, because the ALD method has a relatively slow deposition rate, it is sometimes preferable to use it in combination with other deposition methods that have a faster deposition rate, such as the CVD method.

[0357] Furthermore, the CVD method allows for the deposition of films with any desired composition by changing the flow rate ratio of the raw material gases. For example, in the CVD method, films with continuously changing compositions can be deposited by changing the flow rate ratio of the raw material gases while the film is being deposited. When depositing films while changing the flow rate ratio of the raw material gases, the time required for film deposition can be shortened compared to depositing films using multiple deposition chambers, because time spent on transport or pressure adjustment is eliminated. Therefore, it may be possible to increase the productivity of semiconductor devices.

[0358] Furthermore, the ALD method allows for the deposition of films with any desired composition by simultaneously introducing multiple different types of precursors. Alternatively, when introducing multiple different types of precursors, films with any desired composition can be deposited by controlling the number of cycles for each precursor.

[0359] First, a substrate (not shown) is prepared, and an insulator 210 and a conductor 209 are formed on the substrate (see Figures 8A to 8D).

[0360] Next, an insulator 212 is deposited on the insulator 210 and the conductor 209 (see Figures 8A to 8D). The deposition of the insulator 212 is preferably carried out using a sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulator 212 can be reduced. However, the deposition of the insulator 212 is not limited to the sputtering method; CVD, MBE, PLD, ALD, etc., may be used as appropriate.

[0361] In this embodiment, silicon nitride is deposited as the insulator 212 using a silicon target in a nitrogen gas atmosphere by pulsed DC sputtering. By using pulsed DC sputtering, the generation of particles due to arcing on the target surface can be suppressed, resulting in a more uniform film thickness distribution. Furthermore, by using a pulsed voltage, the rise and fall of the discharge can be made steeper than with a high-frequency voltage. This allows for more efficient power supply to the electrode, improving the sputtering rate and film quality.

[0362] By using an insulator that is impermeable to impurities such as water and hydrogen, such as silicon nitride, the diffusion of impurities such as water and hydrogen contained in the layer below the insulator 212 can be suppressed. Furthermore, by using an insulator that is impermeable to copper, such as silicon nitride, as the insulator 212, even if a diffusive metal such as copper is used in the conductor (not shown) below the insulator 212, the diffusion of that metal upward through the insulator 212 can be suppressed.

[0363] Next, an insulator 214 is formed over the insulator 212 (see FIGS. 8A to 8D). The insulator 214 is preferably formed by a sputtering method. The use of a sputtering method, which does not require the use of hydrogen-containing molecules as a deposition gas, can reduce the hydrogen concentration in the insulator 214. However, the formation of the insulator 214 is not limited to the sputtering method, and a CVD method, an MBE method, a PLD method, an ALD method, or the like may be used as appropriate.

[0364] In this embodiment, as the insulator 214, aluminum oxide is formed by a pulsed DC sputtering method using an aluminum target in an atmosphere containing an oxygen gas. By using the pulsed DC sputtering method, the film thickness distribution can be made more uniform, and the sputtering rate and film quality can be improved. Here, RF power may be applied to the substrate. The amount of oxygen implanted into layers below the insulator 214 can be controlled by adjusting the magnitude of the RF power applied to the substrate. The RF power is set to 0 W / cm 2 or more and 1.86 W / cm 2 or less. That is, the amount of oxygen suitable for transistor characteristics can be changed and implanted depending on the RF power used for forming the insulator 214. Accordingly, an oxygen amount suitable for improving transistor reliability can be implanted. The RF frequency is preferably 10 MHz or higher, typically 13.56 MHz. Higher RF frequencies can reduce damage to the substrate.

[0365] As the insulator 214, a metal oxide with an amorphous structure that has a high ability to capture and fix hydrogen, such as aluminum oxide, is preferably used. This can capture or fix hydrogen contained in the insulator 216 or the like and prevent the hydrogen from diffusing into the oxide 230. In particular, using aluminum oxide with an amorphous structure as the insulator 214 is preferable because hydrogen can sometimes be captured or fixed more effectively. As a result, the transistor 200 and a semiconductor device with favorable characteristics and high reliability can be manufactured.

[0366] Next, an opening 206a is formed in the insulator 214 (see Figures 8A to 8D). The opening 206a can be formed using lithography. The opening 206a is formed superimposed on at least a portion of the area where the opening 206 will be formed in a later step. Preferably, the opening 206a is formed so as to encompass the area where the opening 206 will be formed in a later step. By forming the opening 206a in this way, it becomes unnecessary to etch the insulating layer made of a difficult-to-etch material when forming the opening 206, so that the opening 206 can be manufactured with a good yield.

[0367] The opening 206a can be formed using either a dry etching method or a wet etching method. Dry etching is preferable because it is suitable for microfabrication. As the etching gas, an etching gas containing halogens, including one or more of fluorine, chlorine, and bromine, can be used. For example, C4F6 gas, C5F6 gas, C4F8 gas, CF4 gas, SF6 gas, CHF3 gas, Cl2 gas, BCl3 gas, SiCl4 gas, or BBr3 gas can be used individually or in mixtures of two or more gases as the etching gas. In addition, oxygen gas, carbon dioxide gas, nitrogen gas, helium gas, argon gas, hydrogen gas, or hydrocarbon gas can be added to the above etching gas as appropriate. For example, when aluminum oxide is used for the insulator 214, a mixture of CHF3 and Ar can be used as the etching gas. The dry etching apparatus can be the dry etching apparatus described above. The etching conditions can be set as appropriate according to the object to be etched.

[0368] Furthermore, along with the formation of the opening 206a, a recess may be formed on the upper surface of the insulator 212 in the region overlapping with the opening 206a, as shown in Figure 8B. Also, if the thickness of the insulator 212 is thin, an opening may be formed in the insulator 212 that overlaps with the opening 206a.

[0369] In Figure 8A, the shape of the opening 206a is shown as a rectangle in plan view, but it is not limited to this. For example, the opening 206a may be circular, an ellipse or other approximate circular shape, a rectangle or other polygon, or a rectangle or other polygon with rounded corners in plan view.

[0370] Next, an insulator 216 is deposited on the insulator 214 (see Figures 9A to 9D). At this time, a portion of the insulator 216 is deposited so as to fill the opening 206a and the recess formed on the upper surface of the insulator 212. It is preferable to deposit the insulator 216 using a sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulator 216 can be reduced. However, the deposition of the insulator 216 is not limited to the sputtering method, and CVD, MBE, PLD, ALD, etc. may be used as appropriate.

[0371] In this embodiment, silicon oxide is deposited as the insulator 216 using a silicon target in an atmosphere containing oxygen gas by pulsed DC sputtering. By using pulsed DC sputtering, the film thickness distribution can be made more uniform, and the sputtering rate and film quality can be improved.

[0372] It is preferable to deposit insulators 212, 214, and 216 continuously without exposure to the atmosphere. For example, a multi-chamber type deposition apparatus can be used. This allows for the deposition of insulators 212, 214, and 216 with reduced hydrogen content in the films, and further reduces the incorporation of hydrogen into the films between each deposition process.

[0373] Next, an opening is formed in the insulator 216 that reaches the insulator 214. The opening includes, for example, grooves and slits. In some cases, the term "opening" refers to the region in which the opening is formed. The opening may be formed using wet etching, but dry etching is preferable for microfabrication. Furthermore, it is preferable to select an insulator 214 that functions as an etching stopper film when etching the insulator 216 to form grooves. For example, if silicon oxide or silicon oxynitride is used for the insulator 216 in which grooves are formed, silicon nitride, aluminum oxide, or hafnium oxide may be used for the insulator 214.

[0374] As a dry etching apparatus, a capacitively coupled plasma (CCP) etching apparatus having parallel plate electrodes can be used. The capacitively coupled plasma etching apparatus having parallel plate electrodes may be configured to apply a high-frequency voltage to one electrode of the parallel plate electrodes. Alternatively, it may be configured to apply multiple different high-frequency voltages to one electrode of the parallel plate electrodes. Alternatively, it may be configured to apply a high-frequency voltage of the same frequency to each of the parallel plate electrodes. Alternatively, it may be configured to apply high-frequency voltages of different frequencies to each of the parallel plate electrodes. Alternatively, a dry etching apparatus having a high-density plasma source can be used. A dry etching apparatus having a high-density plasma source may be, for example, an inductively coupled plasma (ICP) etching apparatus.

[0375] After the opening is formed, a conductive film that will become the conductor 205a is deposited. It is desirable that the conductive film that will become the conductor 205a contains a conductor that has the function of suppressing oxygen permeation. For example, tantalum nitride, tungsten nitride, titanium nitride, etc., can be used. Alternatively, a laminated film can be formed of a conductor that has the function of suppressing oxygen permeation and a tantalum, tungsten, titanium, molybdenum, aluminum, copper, or molybdenum-tungsten alloy. The conductive film that will become the conductor 205a can be deposited using sputtering, CVD, MBE, PLD, ALD, etc.

[0376] In this embodiment, titanium nitride is deposited as a conductive film that forms the conductor 205a. By using such a metal nitride as a layer beneath the conductor 205b, oxidation of the conductor 205b by the insulator 216 and the like can be suppressed. Furthermore, even if a highly diffusive metal such as copper is used as the conductor 205b, it is possible to prevent the metal from diffusing out of the conductor 205a.

[0377] Next, a conductive film to become the conductor 205b is deposited. As the conductive film to become the conductor 205b, tantalum, tungsten, titanium, molybdenum, aluminum, copper, molybdenum-tungsten alloy, etc., can be used. The conductive film can be deposited using methods such as plating, sputtering, CVD, MBE, PLD, ALD, etc. In this embodiment, tungsten is deposited as the conductive film to become the conductor 205b.

[0378] Next, by performing CMP treatment, a portion of the conductive film that will become conductor 205a and the conductive film that will become conductor 205b is removed, exposing the insulator 216 (see Figures 9A to 9D). As a result, conductor 205a and conductor 205b remain only in the opening. Note that a portion of the insulator 216 may be removed by this CMP treatment.

[0379] Next, an insulator 222 is deposited on the insulator 216 and the conductor 205 (see Figures 9A to 9D). It is preferable to deposit an insulator 222 containing an oxide of either or both aluminum and hafnium. Preferably, the insulator containing an oxide of either or both aluminum and hafnium is an aluminum oxide, hafnium oxide, or an oxide containing aluminum and hafnium (hafnium aluminate). Alternatively, hafnium zirconium oxide is preferred. An insulator containing an oxide of either or both aluminum and hafnium has barrier properties against oxygen, hydrogen, and water. Because the insulator 222 has barrier properties against hydrogen and water, the diffusion of hydrogen and water contained in the structure surrounding the transistor 200 into the transistor 200 through the insulator 222 is suppressed, thereby suppressing the generation of oxygen vacancies in the oxide 230.

[0380] The insulator 222 can be deposited using sputtering, CVD, MBE, PLD, ALD, or the like. In this embodiment, hafnium oxide is deposited as the insulator 222 using the ALD method. In particular, it is preferable to use a method for forming hafnium oxide with reduced hydrogen concentration, which is one aspect of the present invention.

[0381] Next, it is preferable to perform a heat treatment. The heat treatment should be performed at a temperature of 250°C to 650°C, preferably 300°C to 500°C, and more preferably 320°C to 450°C. The heat treatment should be performed in an atmosphere of nitrogen gas or an inert gas, or in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, when performing the heat treatment in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas should be about 20%. The heat treatment may also be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere of nitrogen gas or an inert gas, and then further in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas to replenish the desorbed oxygen.

[0382] Furthermore, it is preferable that the gas used in the above heat treatment is highly purified. For example, the amount of water contained in the gas used in the above heat treatment should be 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent as much as possible from moisture or other substances being incorporated into the insulator 222 and the like.

[0383] In this embodiment, as a heat treatment, after the insulator 222 is formed, the insulator is treated at a temperature of 400°C for 1 hour with a flow rate ratio of nitrogen gas to oxygen gas of 4:1. This heat treatment can remove impurities such as water and hydrogen contained in the insulator 222. Furthermore, when an oxide containing hafnium is used as the insulator 222, a portion of the insulator 222 may crystallize as a result of this heat treatment. The heat treatment can also be performed at a later time, such as after the formation of the insulator 224.

[0384] Next, an insulating film 224Af is deposited on the insulator 222 (see Figures 9A to 9D). The insulating film 224Af can be deposited using sputtering, CVD, MBE, PLD, ALD, etc. In this embodiment, silicon oxide is deposited as the insulating film 224Af using the sputtering method. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating film 224Af can be reduced. Since the insulating film 224Af will come into contact with the oxide 230a in a later step, it is preferable that the hydrogen concentration is reduced in this way.

[0385] Next, oxide films 230Af and 230Bf are sequentially deposited on the insulating film 224Af (see Figures 9A to 9D). It is preferable to deposit oxide films 230Af and 230Bf continuously without exposing them to the atmosphere. By depositing the films without exposure to the atmosphere, it is possible to prevent impurities or moisture from the atmosphere from adhering to oxide films 230Af and 230Bf, and to keep the vicinity of the interface between oxide films 230Af and 230Bf clean.

[0386] The oxide films 230Af and 230Bf can be deposited using sputtering, CVD, MBE, PLD, ALD, or other methods. In this embodiment, the oxide films 230Af and 230Bf are deposited using sputtering.

[0387] For example, when depositing oxide films 230Af and 230Bf by sputtering, oxygen or a mixture of oxygen and a noble gas is used as the sputtering gas. By increasing the proportion of oxygen in the sputtering gas, the excess oxygen in the deposited oxide film can be increased. Furthermore, when depositing the above oxide films by sputtering, the above-mentioned In-M-Zn oxide target can be used.

[0388] In particular, during the deposition of the oxide film 230Af, some of the oxygen contained in the sputtering gas may be supplied to the insulator 224. Therefore, the proportion of oxygen contained in the sputtering gas should be 70% or more, preferably 80% or more, and more preferably 100%.

[0389] Furthermore, when the oxide film 230Bf is formed by sputtering, if the proportion of oxygen in the sputtering gas is set to be more than 30% but 100% or less, preferably 70% or more but 100%, an oxygen-rich oxide semiconductor is formed. Transistors using an oxygen-rich oxide semiconductor in the channel formation region can achieve relatively high reliability. However, the present invention is not limited to this. When the oxide film 230Bf is formed by sputtering, if the proportion of oxygen in the sputtering gas is set to be 1% or more but 30% or less, preferably 5% or more but 20%, an oxygen-deficient oxide semiconductor is formed. Transistors using an oxygen-deficient oxide semiconductor in the channel formation region can achieve relatively high field-effect mobility. In addition, the crystallinity of the oxide film can be improved by performing film formation while heating the substrate.

[0390] In this embodiment, oxide film 230Af is deposited by sputtering using an oxide target with an In:Ga:Zn ratio of 1:3:4. Oxide film 230Bf is deposited by sputtering using an oxide target with an In:Ga:Zn ratio of 4:2:4.1, an In:Ga:Zn ratio of 1:1:1, an In:Ga:Zn ratio of 1:1:1.2, or an In:Ga:Zn ratio of 1:1:2. The deposition conditions and atomic ratios of each oxide film can be appropriately selected to match the desired properties of oxide 230a and oxide 230b.

[0391] Furthermore, it is preferable to deposit the insulating film 224Af, the oxide film 230Af, and the oxide film 230Bf by sputtering without exposure to the atmosphere. For example, a multi-chamber type deposition apparatus can be used. This reduces the incorporation of hydrogen into the films between each deposition process for the insulating film 224Af, the oxide film 230Af, and the oxide film 230Bf.

[0392] Furthermore, ALD (Advanced Laser Development) may be used to deposit oxide films 230Af and 230Bf. By using ALD to deposit oxide films 230Af and 230Bf, films of uniform thickness can be formed even in grooves or openings with large aspect ratios. In addition, by using PEALD (Pollution-Assisted Laser Development), oxide films 230Af and 230Bf can be formed at lower temperatures compared to thermal ALD.

[0393] Next, it is preferable to perform a heat treatment. The heat treatment should be performed within a temperature range in which the oxide films 230Af and 230Bf do not polycrystallize, and should be performed between 250°C and 650°C, preferably between 400°C and 600°C. The heat treatment should be performed in an atmosphere of nitrogen gas or an inert gas, or in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, when performing the heat treatment in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas should be about 20%. The heat treatment may also be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere of nitrogen gas or an inert gas, and then in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas to replenish the desorbed oxygen.

[0394] Furthermore, it is preferable that the gas used in the above heat treatment is highly purified. For example, the amount of water contained in the gas used in the above heat treatment should be 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent as much as possible from the incorporation of water and other substances into the oxide film 230Af and oxide film 230Bf.

[0395] In this embodiment, the heat treatment involves a nitrogen gas to oxygen gas flow rate ratio of 4:1 and a treatment at a temperature of 400°C for 1 hour. This heat treatment containing oxygen gas can reduce impurities such as carbon, water, and hydrogen in the oxide films 230Af and 230Bf. By reducing impurities in the films in this way, the crystallinity of the oxide film 230Bf can be improved, resulting in a denser, more compact structure. This increases the crystalline region in the oxide films 230Af and 230Bf, and reduces in-plane variation of the crystalline region in the oxide films 230Af and 230Bf. Therefore, in-plane variation in the electrical characteristics of the transistor 200 can be reduced.

[0396] Furthermore, by performing the heat treatment, hydrogen in the insulator 216, insulating film 224Af, oxide film 230Af, and oxide film 230Bf moves to the insulator 222 and is absorbed into the insulator 222. In other words, hydrogen in the insulator 216, insulating film 224Af, oxide film 230Af, and oxide film 230Bf diffuses into the insulator 222. Therefore, the hydrogen concentration in the insulator 222 increases, but the hydrogen concentrations in the insulator 216, insulating film 224Af, oxide film 230Af, and oxide film 230Bf decrease.

[0397] In particular, the insulating film 224Af functions as a second gate insulator of the transistor 200, and the oxide films 230Af and 230Bf function as channel formation regions of the transistor 200. Therefore, a transistor 200 having insulating films 224Af, 230Af, and 230Bf with reduced hydrogen concentrations is preferred because it has good reliability.

[0398] Next, the insulating film 224Af, oxide film 230Af, and oxide film 230Bf are processed into strips using lithography to form the insulating layer 224A, oxide layer 230A, and oxide layer 230B (see Figures 10A to 10D). Here, the insulating layer 224A, oxide layer 230A, and oxide layer 230B are formed to extend in a direction parallel to the dashed line A3-A4 (the channel width direction of the transistor 200, or the Y direction shown in Figure 1A). In addition, the insulating layer 224A, oxide layer 230A, and oxide layer 230B are formed so that at least a portion of them overlaps with the conductor 205. The above processing can be performed using either dry etching or wet etching. Dry etching is suitable for microfabrication. Furthermore, the processing of the insulating film 224Af, oxide film 230Af, and oxide film 230Bf may be carried out under different conditions.

[0399] In lithography, the resist is first exposed through a mask. Next, the exposed area is removed or left intact using a developer to form a resist mask. Then, the conductor, semiconductor, or insulator can be processed into a desired shape by etching through the resist mask. For example, the resist mask can be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, or EUV (Extreme Ultraviolet) light. Alternatively, immersion technology can be used, where a liquid (e.g., water) is filled between the substrate and the projection lens for exposure. In addition, an electron beam or ion beam may be used instead of the aforementioned light. When using an electron beam or ion beam, a mask is not required. The resist mask can be removed by dry etching such as ashing, wet etching, dry etching followed by wet etching, or wet etching followed by dry etching.

[0400] Furthermore, a hard mask made of an insulator or conductor may be used beneath the resist mask. When using a hard mask, an insulating film or conductive film that serves as the hard mask material is formed on the oxide film 230Bf, a resist mask is formed on top of it, and a hard mask of the desired shape can be formed by etching the hard mask material. Etching of the oxide film 230Bf may be performed after removing the resist mask, or it may be performed while the resist mask remains. In the latter case, the resist mask may disappear during etching. The hard mask may also be removed by etching after etching of the oxide film 230Bf. On the other hand, if the hard mask material does not affect subsequent processes or can be used in subsequent processes, it is not always necessary to remove the hard mask.

[0401] Next, an opening 206b is formed in the insulator 222 (see Figures 11A to 11D). The opening 206b can be formed using lithography. The opening 206b is formed superimposed on at least a portion of the area where the opening 206 will be formed in a later step. Preferably, the opening 206b is formed so as to encompass the area where the opening 206 will be formed in a later step. By forming the opening 206b in this way, it becomes unnecessary to etch the insulating layer made of a difficult-to-etch material when forming the opening 206, so that the opening 206 can be manufactured with a good yield.

[0402] The opening 206b can be formed using either a dry etching method or a wet etching method. Dry etching is preferable because it is suitable for microfabrication. As the etching gas, an etching gas containing halogens, including one or more of fluorine, chlorine, and bromine, can be used. For example, C4F6 gas, C5F6 gas, C4F8 gas, CF4 gas, SF6 gas, CHF3 gas, Cl2 gas, BCl3 gas, SiCl4 gas, or BBr3 gas can be used individually or in mixtures of two or more gases as the etching gas. In addition, oxygen gas, carbon dioxide gas, nitrogen gas, helium gas, argon gas, hydrogen gas, or hydrocarbon gas can be added to the above etching gas as appropriate. For example, when using hafnium oxide for the insulator 222, a mixed gas of C4F8, H2, and Ar can be used as the etching gas. The dry etching apparatus can be the dry etching apparatus described above. The etching conditions can be set as appropriate according to the object to be etched.

[0403] Furthermore, along with the formation of the opening 206b, a recess may be formed on the upper surface of the insulator 216 in the region overlapping with the opening 206b, as shown in Figure 11B.

[0404] In Figure 11A, the shape of the opening 206b is shown as a rectangle in plan view, but it is not limited to this. For example, the opening 206b may be circular, an ellipse or other approximate circular shape, a rectangle or other polygon, or a rectangle or other polygon with rounded corners in plan view.

[0405] Next, conductive films 242Af and 242Bf are deposited sequentially on the insulator 222 and the oxide layer 230B (see Figures 12A to 12D). At this time, a portion of the conductive films 242Af and 242Bf are deposited so as to fill the opening 206b and the recess formed on the upper surface of the insulator 216. The conductive films 242Af and 242Bf can be deposited using sputtering, CVD, MBE, PLD, ALD, etc. For example, tantalum nitride can be deposited as conductive film 242Af using sputtering, and tungsten can be deposited as conductive film 242Bf. Note that a heat treatment may be performed before depositing the conductive film 242Af. This heat treatment may be performed under reduced pressure, and the conductive films 242Af may be deposited continuously without exposure to the atmosphere. By performing this treatment, moisture and hydrogen adsorbed on the surface of the oxide layer 230B can be removed, and the moisture and hydrogen concentrations in the oxide layer 230A and oxide layer 230B can be further reduced. The heat treatment temperature is preferably between 100°C and 400°C. In this embodiment, the heat treatment temperature is set to 200°C.

[0406] Next, the insulating layer 224A, oxide layer 230A, oxide layer 230B, conductive film 242Af, and conductive film 242Bf are processed using lithography to form island-shaped insulators 224, oxides 230a and 230b, and island-shaped conductive layers 242A and 242B having openings (see Figures 13A to 13D). For example, after processing the insulating layer 224A, oxide layer 230A, oxide layer 230B, conductive film 242Af, and conductive film 242Bf to form island-shaped insulators 224, oxide 230a, and oxide 230b, and conductive layers 242A and 242B extending in a direction parallel to the dashed line A1-A2 (the channel length direction of transistor 200, or the X direction shown in Figure 1A), the conductive layers 242A and 242B are processed to form island-shaped conductive layers 242A and 242B having openings. Alternatively, for example, the insulating layer 224A, oxide layer 230A, oxide layer 230B, conductive film 242Af, and conductive film 242Bf may be processed into island shapes to form the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B, and then openings may be formed in the conductive layer 242A and conductive layer 242B.

[0407] Here, the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B are formed so that at least a portion of them overlaps with the conductor 205. In addition, the openings provided in conductive layer 242A and conductive layer 242B are formed in positions that do not overlap with oxide 230b. The above processing can be carried out by dry etching or wet etching. Dry etching is suitable for microfabrication. Furthermore, the processing of the insulating layer 224A, oxide layer 230A, oxide layer 230B, conductive film 242Af, and conductive film 242Bf may be carried out under different conditions.

[0408] Furthermore, as shown in Figures 13B to 13D, the sides of the insulator 224, oxide 230a, and oxide 230b may be tapered. For example, the tapered angle of the insulator 224, oxide 230a, and oxide 230b should be 60° or more and less than 90°. By making the sides tapered in this way, the coverage of the insulator 275 and other materials can be improved in subsequent processes, and defects such as porosity can be reduced.

[0409] However, the above is not limited to the above, and the sides of the insulator 224, oxide 230a, and oxide 230b may be configured to be approximately perpendicular to the upper surface of the insulator 222. Such a configuration makes it possible to reduce the area and increase the density when providing multiple transistors 200.

[0410] Furthermore, by-products generated during the etching process may form in layers on the sides of the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B. In this case, the layered by-products will be formed between the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B and the insulator 275. Therefore, it is preferable to remove the layered by-products formed in contact with the upper surface of the insulator 222.

[0411] Furthermore, although the etching process described above involves providing an opening in the center of the conductive layer 242A and the conductive layer 242B, the present invention is not limited to this. For example, the conductive layer 242A and the conductive layer 242B may be provided separately on the transistor 200a side and the transistor 200b side.

[0412] Next, an insulator 275 is formed by covering the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B (see Figures 14A to 14D). Here, it is preferable that the insulator 275 is in contact with the upper surface of the insulator 222 and the side surface of the insulator 224. The insulator 275 can be formed using sputtering, CVD, MBE, PLD, ALD, etc. It is preferable that the insulator 275 is an insulating film that has the function of suppressing oxygen permeation. For example, silicon nitride can be formed as the insulator 275 using the ALD method. Alternatively, aluminum oxide can be formed as the insulator 275 using the sputtering method, and then silicon nitride can be formed on top of it using the PEALD method. By making the insulator 275 such a layered structure, the function of suppressing the diffusion of impurities such as water and hydrogen, and oxygen may be improved.

[0413] In this way, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B can be covered with an insulator 275 that has the function of suppressing oxygen diffusion. This reduces the direct diffusion of oxygen from the insulator 280, etc., to the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B in subsequent processes.

[0414] Next, an insulating film, which will become an insulating film 280, is deposited on the insulator 275. The insulating film can be deposited using sputtering, CVD, MBE, PLD, ALD, or the like. For example, a silicon oxide film can be deposited as the insulating film using sputtering. By depositing the insulating film using sputtering in an oxygen-containing atmosphere, an insulating film 280 containing excess oxygen can be formed. Furthermore, by using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulating film 280 can be reduced. Note that a heat treatment may be performed before depositing the insulating film. The heat treatment may be performed under reduced pressure, and the insulating film may be deposited continuously without exposure to the atmosphere. By performing such a treatment, moisture and hydrogen adsorbed on the surface of the insulating film 275 can be removed, and the moisture and hydrogen concentrations in the oxide 230a, oxide 230b, and insulating film 224 can be further reduced. The heat treatment conditions described above can be used for this heat treatment.

[0415] Next, the insulating film that will become the insulator 280 is subjected to CMP treatment to form an insulator 280 with a flat top surface (see Figures 14A to 14D). Alternatively, silicon nitride may be deposited on the insulator 280 by, for example, a sputtering method, and the silicon nitride may be subjected to CMP treatment until it reaches the insulator 280.

[0416] Next, a portion of the insulator 280, a portion of the insulator 275, a portion of the conductive layer 242A, and a portion of the conductive layer 242B are processed to form an opening 258 that reaches the oxide 230b. By forming the opening 258, conductors 242a1 and 242b1 can be formed from the conductive layer 242A, and conductors 242a2 and 242b2 can be formed from the conductive layer 242B (see Figures 15A to 15D).

[0417] Furthermore, the processing of a portion of the insulator 280, a portion of the insulator 275, a portion of the conductive layer 242A, and a portion of the conductive layer 242B can be carried out using either a dry etching method or a wet etching method. Dry etching is suitable for microfabrication. Moreover, these processing methods may be carried out under different conditions. For example, a portion of the insulator 280 may be processed by dry etching, a portion of the insulator 275 may be processed by wet etching, and a portion of the conductive layer 242A and a portion of the conductive layer 242B may be processed by dry etching.

[0418] It is preferable that the opening 258 is formed to extend in a direction parallel to the dashed line A3-A4 (the channel width direction of the transistor, or the Y direction shown in Figure 1A), as shown in Figure 15A. By forming the opening 258 in this way, the conductor 260, which is formed later, can be provided extending in the above direction and function as wiring. It is also preferable that the opening 258 be formed to overlap with the conductor 205.

[0419] The width of the aperture 258 in the X direction is reflected in the channel length of the transistor 200, so it is preferable that it be fine. For example, it is preferable that the width of the aperture 258 in the X direction is 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 1 nm or more, or 5 nm or more. In this way, it is preferable to use a lithography method using short-wavelength light such as EUV light or an electron beam to finely process the aperture 258.

[0420] When processing the opening 258 finely, it is preferable to process a portion of the insulator 280, a portion of the insulator 275, a portion of the conductive layer 242B, and a portion of the conductive layer 242A using anisotropic etching. In particular, processing by dry etching is preferred because it is suitable for micro-processing. Furthermore, each of these processes may be carried out under different conditions.

[0421] By processing the insulator 280, insulator 275, conductive layer 242B, and conductive layer 242A using anisotropic etching, the opposing sides of the conductor 242a and conductor 242b can be formed so that they are approximately perpendicular to the upper surface of the oxide 230b. This configuration reduces the formation of so-called Loff regions between region 230ba and region 230bc, and between region 230bb and region 230bc. Therefore, the frequency characteristics of the transistor 200 can be improved, and the operating speed of the semiconductor device according to one embodiment of the present invention can be improved.

[0422] However, the above is not limited to the above, and as shown in Figure 3B, the sides of the insulator 280, insulator 275, and conductor 242 may be tapered. Also, the taper angle of the insulator 280 may be larger than the taper angle of the conductor 242. Furthermore, when forming the opening 258, the upper part of the oxide 230b may be removed.

[0423] The above etching process may result in the adhesion of impurities to the sides of oxide 230a, the top and sides of oxide 230b, the sides of conductor 242, the sides of insulator 280, etc., or the diffusion of such impurities into these surfaces. A step to remove such impurities may be performed. In addition, the above dry etching may form damaged areas on the surface of oxide 230b. Such damaged areas may be removed. Examples of such impurities include those resulting from components contained in insulator 280, insulator 275, conductive layer 242B, and conductive layer 242A, components contained in materials used in the apparatus used to form the above-mentioned openings, and components contained in the gas or liquid used for etching. Examples of such impurities include hafnium, aluminum, silicon, tantalum, fluorine, and chlorine.

[0424] In particular, impurities such as aluminum and silicon may reduce the crystallinity of oxide 230b. Therefore, it is preferable to remove impurities such as aluminum and silicon from the surface of oxide 230b and its vicinity. Furthermore, it is preferable to reduce the concentration of such impurities. For example, the concentration of aluminum atoms on the surface of oxide 230b and its vicinity should be 5.0 atomic% or less, preferably 2.0 atomic% or less, more preferably 1.5 atomic% or less, even more preferably 1.0 atomic% or less, and even more preferably less than 0.3 atomic%.

[0425] Furthermore, due to impurities such as aluminum and silicon, the crystallinity of oxide 230b is low in certain regions, and therefore the density of the crystal structure is reduced. O A large amount of H is formed, making it easier for the transistor to become normally-on. Therefore, it is preferable that regions with low crystallinity of oxide 230b are reduced or removed.

[0426] In contrast, it is preferable that the oxide 230b has a layered CAAC structure. In particular, it is preferable that the CAAC structure extends to the lower end of the drain of the oxide 230b. Here, in the transistor 200, the conductor 242a or conductor 242b, and its vicinity, function as a drain. That is, it is preferable that the oxide 230b near the lower end of the conductor 242a (conductor 242b) has a CAAC structure. In this way, even at the drain end, which significantly affects the drain breakdown voltage, the region of low crystallinity of the oxide 230b is removed and a CAAC structure is present, which further suppresses fluctuations in the electrical characteristics of the transistor 200. Furthermore, the reliability of the transistor 200 can be improved.

[0427] In order to remove impurities and other contaminants adhering to the oxide 230b surface during the etching process described above, a cleaning treatment is performed. Cleaning methods include wet cleaning using a cleaning solution (which can also be called wet etching), plasma treatment using plasma, and cleaning by heat treatment. These cleaning methods may be combined as appropriate. Note that this cleaning treatment may deepen the grooves.

[0428] Wet cleaning may be performed using aqueous solutions of ammonia water, oxalic acid, phosphoric acid, hydrofluoric acid, etc., diluted with carbonated water or distilled water, distilled water, carbonated water, etc. Alternatively, ultrasonic cleaning may be performed using these aqueous solutions, distilled water, or carbonated water. Alternatively, these cleaning methods may be combined as appropriate.

[0429] In this specification, an aqueous solution obtained by diluting hydrofluoric acid with pure water is sometimes referred to as diluted hydrofluoric acid, and an aqueous solution obtained by diluting ammonia water with pure water is sometimes referred to as diluted ammonia water. The concentration and temperature of the aqueous solution may be adjusted as appropriate depending on the impurities to be removed and the configuration of the semiconductor device to be cleaned. The ammonia concentration of the diluted ammonia water should be 0.01% to 5%, preferably 0.1% to 0.5%. The hydrogen fluoride concentration of the diluted hydrofluoric acid should be 0.01 ppm to 100 ppm, preferably 0.1 ppm to 10 ppm.

[0430] Furthermore, it is preferable to use a frequency of 200 kHz or higher for ultrasonic cleaning, and more preferably a frequency of 900 kHz or higher. Using these frequencies can reduce damage to oxides such as 230b.

[0431] Furthermore, the above cleaning process may be performed multiple times, and the cleaning solution may be changed each time. For example, the first cleaning process may be performed using diluted hydrofluoric acid or diluted ammonia water, and the second cleaning process may be performed using pure water or carbonated water.

[0432] In this embodiment, the cleaning process described above involves wet cleaning using diluted ammonia water. This cleaning process removes impurities that have adhered to the surface or diffused into the interior, such as oxide 230a and oxide 230b. Furthermore, it can improve the crystallinity of oxide 230b.

[0433] Heat treatment may be performed after the etching or cleaning described above. The heat treatment should be performed at a temperature of 100°C to 450°C, preferably 350°C to 400°C. The heat treatment should be performed in an atmosphere of nitrogen gas or an inert gas, or in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. For example, it is preferable to perform the heat treatment in an oxygen atmosphere. This allows oxygen to be supplied to oxides 230a and 230b, thereby reducing oxygen deficiency. Furthermore, such heat treatment can improve the crystallinity of oxide 230b. The heat treatment may also be performed under reduced pressure. Alternatively, after heat treatment in an oxygen atmosphere, continuous heat treatment in a nitrogen atmosphere may be performed without exposure to the atmosphere.

[0434] Next, the insulating film 253A is deposited (see Figures 16A to 16D). The insulating film 253A is the insulating film that will become the insulator 253 in a later step. The insulating film 253A can be deposited using sputtering, CVD, MBE, PLD, ALD, etc. It is preferable to deposit the insulating film 253A using the ALD method. As mentioned above, it is preferable to deposit the insulating film 253A with a thin film thickness, and it is necessary to minimize variations in film thickness. In contrast, the ALD method is a film deposition method that alternately introduces a precursor and a reactant (e.g., an oxidizing agent), and the film thickness can be adjusted by the number of times this cycle is repeated, thus enabling precise film thickness adjustment. Also, as shown in Figures 16B and 16C, the insulating film 253A needs to be deposited with good coverage on the bottom and side surfaces of the opening 258. It is preferable that the insulating film be deposited with good coverage on the top and side surfaces of the oxide 230 in the opening 258. By using the ALD method, atomic layers can be deposited one by one on the bottom and sides of the opening 258, allowing the insulating film 253A to be formed with good coverage over the opening.

[0435] Furthermore, when the insulating film 253A is deposited by the ALD method, ozone (O3), oxygen (O2), water (H2O), etc., can be used as oxidizing agents. By using hydrogen-free oxidizing agents such as ozone (O3) and oxygen (O2), the amount of hydrogen diffused into the oxide 230b can be reduced.

[0436] In this embodiment, hafnium oxide is deposited as the insulating film 253A by thermal ALD method.

[0437] Next, it is preferable to perform microwave processing in an oxygen-containing atmosphere (see Figures 16A to 16D). Here, microwave processing refers to processing using a device that has a power supply that generates high-density plasma using microwaves, for example. In this specification, microwaves refer to electromagnetic waves having a frequency of 300 MHz or more and 300 GHz or less. When the insulating film 253A has a laminated structure, microwave processing may be performed at the stage when a part of the insulating film 253A has been deposited. For example, when the insulating film 253A includes a silicon oxide film or a silicon oxynitride film, microwave processing may be performed at the stage when the silicon oxide film or silicon oxynitride film has been deposited.

[0438] The dotted arrows shown in Figures 16B to 16D represent microwaves, high frequencies such as RF, oxygen plasma, or oxygen radicals. For microwave processing, it is preferable to use a microwave processing apparatus that has a power supply for generating high-density plasma using microwaves. Here, the frequency of the microwave processing apparatus should be 300 MHz or more and 300 GHz or less, preferably 2.4 GHz or more and 2.5 GHz or less, for example, 2.45 GHz. By using high-density plasma, high-density oxygen radicals can be generated. The power of the power supply for applying microwaves to the microwave processing apparatus should be 1000 W or more and 10000 W or less, preferably 2000 W or more and 5000 W or less. The microwave processing apparatus may also have a power supply for applying RF to the substrate side. Furthermore, by applying RF to the substrate side, oxygen ions generated by the high-density plasma can be efficiently guided into the oxide 230b.

[0439] Furthermore, the above microwave treatment is preferably carried out under reduced pressure, with a pressure of 10 Pa to 1000 Pa, preferably 300 Pa to 700 Pa. The treatment temperature should be 750°C or lower, preferably 500°C or lower, for example, around 250°C. Alternatively, after oxygen plasma treatment, heat treatment may be carried out continuously without exposure to the outside air. For example, the temperature should be 100°C to 750°C, preferably 300°C to 500°C.

[0440] Furthermore, for example, the above microwave treatment may be carried out using oxygen gas and argon gas. Here, the oxygen flow rate ratio (O2 / (O2+Ar)) should be greater than 0% and 100% or less. Preferably, the oxygen flow rate ratio (O2 / (O2+Ar)) should be greater than 0% and 50% or less. More preferably, the oxygen flow rate ratio (O2 / (O2+Ar)) should be 10% or more and 40% or less. Even more preferably, the oxygen flow rate ratio (O2 / (O2+Ar)) should be 10% or more and 30% or less. In this way, by performing microwave treatment in an oxygen-containing atmosphere, the carrier concentration in region 230bc can be reduced. In addition, by preventing an excessive amount of oxygen from being introduced into the chamber during microwave treatment, it is possible to prevent an excessive decrease in carrier concentration in regions 230ba and 230bb.

[0441] As shown in Figures 16B to 16D, by performing microwave treatment in an oxygen-containing atmosphere, the oxygen gas can be plasma-generated using microwaves or high-frequency waves such as RF, and this oxygen plasma can be applied to the region between the conductors 242a and 242b of the oxide 230b. At this time, microwaves or high-frequency waves such as RF can also be irradiated onto region 230bc. In other words, microwaves or high-frequency waves such as RF, oxygen plasma, etc., can be applied to region 230bc shown in Figure 3A. Due to the action of plasma, microwaves, etc., the V of region 230bc O By cleaving H, hydrogen can be removed from region 230bc. In other words, V contained in region 230bc OH can be reduced. Therefore, oxygen deficiency in region 230bc, and V O By reducing H, the carrier concentration can be lowered. Furthermore, by supplying oxygen radicals generated by the oxygen plasma to the oxygen vacancy formed in region 230bc, the oxygen vacancy in region 230bc can be further reduced, and the carrier concentration can be lowered.

[0442] Meanwhile, conductors 242a and 242b are provided on regions 230ba and 230bb shown in Figure 3A. Here, it is preferable that the conductor 242 functions as a shielding film against the effects of microwaves, high frequencies such as RF, and oxygen plasma when microwave processing is performed in an oxygen-containing atmosphere. For this reason, it is preferable that the conductor 242 has the function of shielding electromagnetic waves between 300 MHz and 300 GHz, for example, between 2.4 GHz and 2.5 GHz.

[0443] As shown in Figures 16B to 16D, conductors 242a and 242b shield against microwaves, high-frequency waves such as RF, and oxygen plasma, so these effects do not extend to regions 230ba and 230bb. As a result, microwave processing does not affect regions 230ba and 230bb. O This reduces H and prevents excessive oxygen supply, thus preventing a decrease in carrier concentration.

[0444] Furthermore, an insulating film 253A, which has barrier properties against oxygen, is provided in contact with the sides of the conductors 242a and 242b. This suppresses the formation of oxide films on the sides of the conductors 242a and 242b by microwave processing.

[0445] Furthermore, since the film quality of the insulating film 253A can be improved, the reliability of the transistor 200 is enhanced.

[0446] As described above, oxygen vacancies are selectively created in the oxide semiconductor region 230bc, and V OBy removing H, region 230bc can be made i-type or substantially i-type. Furthermore, it is possible to suppress the supply of excess oxygen to regions 230ba and 230bb, which function as source or drain regions, while maintaining conductivity. This suppresses variations in the electrical properties of transistor 200 and prevents variations in the electrical properties of transistor 200 within the substrate plane.

[0447] In microwave processing, electromagnetic interaction between microwaves and molecules in oxide 230b can directly transfer thermal energy to oxide 230b. This thermal energy can cause oxide 230b to heat up. This type of heat treatment is sometimes called microwave annealing. Performing microwave processing in an oxygen-containing atmosphere can sometimes achieve effects equivalent to oxygen annealing. Furthermore, if oxide 230b contains hydrogen, this thermal energy may be transferred to the hydrogen in oxide 230b, causing activated hydrogen to be released from oxide 230b.

[0448] Alternatively, the microwave treatment performed before the deposition of the insulating film 253A may be omitted, instead of performing the microwave treatment after the deposition of the insulating film 253A.

[0449] Alternatively, after microwave treatment following the deposition of the insulating film 253A, a heat treatment may be performed while maintaining a reduced pressure state. By performing such a treatment, hydrogen in the insulating film 253A, oxide 230b, and oxide 230a can be efficiently removed. In addition, some of the hydrogen may be gettered by the conductor 242 (conductor 242a and conductor 242b). Alternatively, the step of performing a heat treatment while maintaining a reduced pressure state after microwave treatment may be repeated multiple times. By repeating the heat treatment, hydrogen in the insulating film 253A, oxide 230b, and oxide 230a can be removed even more efficiently. The heat treatment temperature is preferably 300°C to 500°C. Furthermore, the above microwave treatment, i.e., microwave annealing, may also serve as the heat treatment. If the oxide 230b, etc., is sufficiently heated by microwave annealing, the heat treatment may not be necessary.

[0450] Furthermore, by modifying the film quality of the insulating film 253A through microwave treatment, the diffusion of hydrogen, water, impurities, etc. can be suppressed. Therefore, in subsequent processes such as deposition of a conductive film that becomes the conductor 260, or post-treatment such as heat treatment, the diffusion of hydrogen, water, impurities, etc., into oxides 230b, oxides 230a, etc., through the insulator 253 can be suppressed.

[0451] Next, an insulating film to become the insulator 254 is deposited. This insulating film can be deposited using sputtering, CVD, MBE, PLD, ALD, or other methods. It is preferable to deposit this insulating film using the ALD method, similar to insulating film 253A. Using the ALD method allows for the deposition of a thin insulating film with good coverage. In this embodiment, silicon nitride is deposited as the insulating film using the PEALD method.

[0452] Next, a conductive film to become conductor 260a and a conductive film to become conductor 260b are deposited in sequence. The conductive films to become conductor 260a and conductor 260b can be deposited using sputtering, CVD, MBE, PLD, ALD, etc. In this embodiment, titanium nitride is deposited as the conductive film to become conductor 260a using the ALD method, and tungsten is deposited as the conductive film to become conductor 260b using the CVD method.

[0453] Next, the insulating film 253A, the insulating film that will become the insulator 254, the conductive film that will become the conductor 260a, and the conductive film that will become the conductor 260b are polished by CMP until the insulator 280 is exposed. In other words, the portions of the insulating film 253A, the insulating film that will become the insulator 254, the conductive film that will become the conductor 260a, and the conductive film that will become the conductor 260b that are exposed from the opening 258 are removed. This forms the insulator 253, the insulator 254, and the conductor 260 (conductor 260a and conductor 260b) within the opening 258 (see Figures 17A to 17D).

[0454] Thus, the insulator 253 is provided in contact with the inner wall and the side surface of the opening 258 overlapping with the oxide 230b. Further, the conductor 260 is arranged to fill the opening 258 with the insulator 253 and the insulator 254 therebetween. In this manner, the transistor 200 is formed.

[0455] Next, heat treatment may be performed under the same conditions as the above heat treatment. In this embodiment, treatment is performed at 400° C. for 1 hour in a nitrogen atmosphere. By the heat treatment, the water concentration and the hydrogen concentration in the insulator 280 can be reduced. Note that after the heat treatment, the insulator 282 may be continuously formed without exposure to the air.

[0456] Next, the insulator 282 is formed over the insulator 253, the insulator 254, the conductor 260, and the insulator 280 (see FIGS. 18A to 18D). The insulator 282 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like. The insulator 282 is preferably formed by a sputtering method. By a sputtering method in which a molecule containing hydrogen is not used as a deposition gas, the hydrogen concentration in the insulator 282 can be reduced.

[0457] In this embodiment, as the insulator 282, aluminum oxide is formed by a pulsed DC sputtering method using an aluminum target in an atmosphere containing oxygen gas. By the pulsed DC sputtering method, the film thickness distribution can be more uniform, and the sputtering rate and the film quality can be improved. Further, RF power applied to the substrate is set to be 1.86 W / cm 2 or less. Preferably, the RF power is 0 W / cm 2 or more and 0.62 W / cm 2 or less. By reducing the RF power, the amount of oxygen injected into the insulator 280 can be suppressed. Alternatively, the insulator 282 may be formed to have a two-layer stacked structure. In that case, a lower layer of the insulator 282 is formed with RF power applied to the substrate of 0 W / cm 2 , and an upper layer of the insulator 282 is formed with RF power applied to the substrate of 0.62 W / cm 2 .

[0458] Furthermore, by using the sputtering method to deposit the insulator 282 in an oxygen-containing atmosphere, oxygen can be added to the insulator 280 during film formation. This allows the insulator 280 to contain excess oxygen. In this case, it is preferable to deposit the insulator 282 while heating the substrate.

[0459] Next, a portion of the insulator 282, a portion of the insulator 280, and a portion of the insulator 275 are processed to form an opening 158 that reaches the conductor 242b (see Figures 19A to 19D). The opening 158 can be formed using lithography. In Figure 19A, the shape of the opening 158 is shown as a rectangle in plan view, but it is not limited to this. For example, the opening may be circular, an ellipse or other approximate circular shape, a rectangle or other polygonal shape, or a rectangle or other polygonal shape with rounded corners in plan view.

[0460] The width of the aperture 158 in the X direction is preferably fine. For example, the width of the aperture 158 in the X direction is preferably 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 1 nm or more, or 5 nm or more. In this way, it is preferable to use a lithography method using short-wavelength light such as EUV light or an electron beam to finely process the aperture 158.

[0461] Since the aperture 158 has a large aspect ratio, it is preferable to process a portion of the insulator 282, a portion of the insulator 280, and a portion of the insulator 275 using anisotropic etching. In particular, processing by dry etching is preferred because it is suitable for micro-processing. Furthermore, each of these processes may be carried out under different conditions.

[0462] Next, a conductive film 156A is formed to cover the opening 158 and the insulator 282 (see Figures 20A to 20D). The conductive film 156A is the conductive film that will become the conductor 156 in a later step. It is preferable that the conductive film 156A is formed in contact with the side and bottom surfaces of the opening 158, which have a large aspect ratio. For this reason, it is preferable to form the conductive film 156A using a film formation method that provides good coverage, such as the ALD method or the CVD method. For example, titanium nitride or tantalum nitride can be formed using the ALD method.

[0463] Next, the conductive film 156A is processed using lithography to form the conductor 156 (see Figures 21A to 21D). As a result, a portion of the conductor 156 is formed on the opening 158 and comes into contact with a portion of the upper surface of the insulator 282.

[0464] Alternatively, the conductive film 156A may be processed using the CMP method. In this case, the opening 158 is filled with a filler, and the CMP treatment is performed on the filler and the conductive film 156A until the insulator 282 is exposed. This makes it possible to form the uppermost part of the conductor 156 to roughly coincide with the upper surface of the insulator 282, similar to Figures 5A and 5B. The filler can be removed after the conductor 156 has been formed.

[0465] Next, an insulating film 153A is deposited on the conductor 156 (see Figures 22A to 22D). The insulating film 153A is the insulating film that will become the insulator 153 in a later step. Preferably, the insulating film 153A is formed in contact with the conductor 156 which is provided inside the opening 158 with a large aspect ratio. For this reason, it is preferable to deposit the insulating film 153A using a film deposition method with good coverage, such as the ALD method or the CVD method. The insulating film 153A can be made from the high-k material described above.

[0466] Next, conductive film 160A, which will become conductor 160a, and conductive film 160B, which will become conductor 160b, are deposited in sequence (see Figures 22A to 22D). Conductive film 160A is a conductive film that will become conductor 160a in a later step, and conductive film 160B is a conductive film that will become conductor 160b in a later step. It is preferable that conductive film 160A is formed in contact with insulating film 153A provided inside the opening 158 with a large aspect ratio, and it is preferable that conductive film 160B is formed so as to fill the opening 158. For this reason, it is preferable to deposit conductive film 160A and conductive film 160B using a film deposition method that has good coverage, such as the ALD method or the CVD method. For example, titanium nitride can be deposited as conductive film 160A using the ALD method, and tungsten can be deposited as conductive film 160B using the CVD method.

[0467] When the conductive film 160B is deposited using the CVD method, the average surface roughness of the upper surface of the conductive film 160B may increase, as shown in Figures 22B to 22D. In this case, it is preferable to flatten the conductive film 160B using the CMP method (see Figures 23A to 23D). In this case, before performing the CMP treatment, a silicon oxide film or silicon oxidizide film may be deposited on the conductive film 160B, and the CMP treatment may be performed until the silicon oxide film or silicon oxidizide film is removed.

[0468] Next, the insulating film 153A, the conductive film 160A, and the conductive film 160B are processed using lithography to form the insulator 153, the conductor 160a, and the conductor 160b (see Figures 24A to 24D). At this time, it is preferable that the insulator 153, the conductor 160a, and the conductor 160b are formed to cover the side edges of the conductor 156. With this configuration, the conductor 160 and the conductor 156 can be separated by the insulator 153, thereby suppressing short circuits between the conductor 160 and the conductor 156.

[0469] Furthermore, as shown in Figures 24A and 24D, it is preferable to provide the conductor 160 extending in the A5-A6 direction. In this case, the insulator 153 can also be provided extending together with the conductor 160.

[0470] Although the above example shows the insulating film 153A also being processed into the insulator 153, the present invention is not limited to this. Alternatively, only the conductive film 160A and the conductive film 160B may be processed, leaving the insulating film 153A intact. In this case, as shown in Figures 5A and 5B, a portion of the insulator 153 is exposed from the conductor 160. This eliminates the need to process the insulator 153, thereby reducing the manufacturing process of the memory device and improving productivity.

[0471] In this way, a capacitive element 100 can be formed in which at least a portion of the conductor 156, the insulator 153, and the conductor 160 is formed within the opening 158.

[0472] Next, an opening 206c is formed in the insulator 282 (see Figures 25A to 25D). The opening 206c can be formed using lithography. The opening 206c is formed superimposed on at least a portion of the area where the opening 206 will be formed in a later step. Preferably, the opening 206c is formed so as to encompass the area where the opening 206 will be formed in a later step. By forming the opening 206c in this way, it becomes unnecessary to etch the insulating layer made of a difficult-to-etch material when forming the opening 206, so that the opening 206 can be manufactured with a good yield.

[0473] The opening 206c can be formed using either a dry etching method or a wet etching method. Dry etching is preferable because it is suitable for microfabrication. As the etching gas, an etching gas containing halogens, including one or more of fluorine, chlorine, and bromine, can be used. For example, C4F6 gas, C5F6 gas, C4F8 gas, CF4 gas, SF6 gas, CHF3 gas, Cl2 gas, BCl3 gas, SiCl4 gas, or BBr3 gas can be used as the etching gas, either alone or in a mixture of two or more gases. In addition, oxygen gas, carbon dioxide gas, nitrogen gas, helium gas, argon gas, hydrogen gas, or hydrocarbon gas can be added to the above etching gas as appropriate. For example, when aluminum oxide is used for the insulator 282, a mixture of CHF3 and Ar can be used as the etching gas. The dry etching apparatus can be the dry etching apparatus described above. The etching conditions can be set as appropriate according to the object to be etched.

[0474] Furthermore, along with the formation of the opening 206c, a recess may be formed on the upper surface of the insulator 280 in the region overlapping with the opening 206c, as shown in Figure 25B.

[0475] In Figure 25A, the shape of the opening 206c is shown as a rectangle in plan view, but it is not limited to this. For example, the opening 206c may be circular, an ellipse or other approximate circular shape, a rectangle or other polygon, or a rectangle or other polygon with rounded corners in plan view.

[0476] Next, an insulator 285 is formed on the insulator 282 and the conductor 160 (see Figures 26A to 26D). At this time, a portion of the insulator 285 is deposited so as to fill the opening 206c and the recess formed on the upper surface of the insulator 280. The insulator 285 can be deposited using sputtering, CVD, MBE, PLD, or ALD. It is preferable to deposit the insulator 285 using sputtering. By using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the insulator 285 can be reduced.

[0477] In this embodiment, silicon oxide is deposited as the insulator 285 by sputtering.

[0478] Next, openings 206 reaching the conductor 209 are formed in the insulators 212, 216, 275, 280, and 285 (see Figures 26A and 26B). Here, the openings 206 are formed such that a portion of the conductor 242a protrudes into the openings 206. Therefore, in the openings 206, the side surface of the conductor 242a protrudes from the side surfaces of the insulators 280, 216, etc. The openings 206 can be formed using lithography. Note that in Figure 26A, the shape of the openings 206 is shown as a rectangle in plan view, but it is not limited to this. For example, the openings may be circular, elliptical or other approximate circular shapes, quadrilaterals or other polygonal shapes, or quadrilaterals or other polygonal shapes with rounded corners in plan view.

[0479] The opening 206 can be formed, for example, by exposing the upper surface of the conductor 209 by anisotropic etching, and then performing isotropic etching to set back the sides of the insulators 212, 216, 275, 280, and 285 from the sides of the conductor 242a. Here, conditions are used in the isotropic etching to make it difficult to etch the conductor 242.

[0480] It is preferable to perform anisotropic etching and isotropic etching continuously without exposure to the atmosphere by changing the conditions in the same etching apparatus. For example, when using the dry etching method for both anisotropic and isotropic etching, it is possible to switch from anisotropic etching to isotropic etching by changing one or more conditions such as power supply power, bias power, etching gas flow rate, etching gas type, or pressure.

[0481] Alternatively, different etching methods may be used for anisotropic etching and isotropic etching. For example, a dry etching method can be used for anisotropic etching, and a wet etching method can be used for isotropic etching.

[0482] Here, the opening 206 is formed so as to overlap with at least a portion of the opening 206a, at least a portion of the opening 206b, and at least a portion of the opening 206c in a plan view. Preferably, the opening 206 is formed so as to be located inside the opening 206a, inside the opening 206b, and inside the opening 206c in a plan view. As a result, the sides of the insulators 212, 216, 275, 280, and 285 protrude more toward the center of the opening 206 than the sides of the insulators 214, 222, and 282.

[0483] As described above, by forming the opening 206, it becomes unnecessary to etch the insulating layer made of a difficult-to-etch material when forming the opening 206, thus enabling the production of the opening 206 with a high yield and improving the productivity of the memory device. Furthermore, since it is not necessary to etch the insulating layer made of a difficult-to-etch material, the etching rate will not drop significantly during the formation of the opening 206, preventing the formation of abnormal shapes in the opening 206. Therefore, the side walls of the opening 206 can be provided approximately perpendicular to the substrate surface or the upper surface of the conductor 209. This reduces the area occupied by the opening 206 and the area occupied per memory cell, thereby increasing the storage capacity per unit area of ​​the memory device.

[0484] Next, a conductive film to become conductor 240a and a conductive film to become conductor 240b are deposited in sequence. These conductive films can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. Since conductor 240a is provided in contact with the bottom surface and side walls of the opening 206, it is provided in contact with a part of conductor 242a that is formed protruding into the opening 206.

[0485] The conductive film that forms the conductor 240a preferably has the function of suppressing the permeation of impurities such as water and hydrogen. For the deposition of the conductive film that forms the conductor 240a, it is preferable to use a deposition method that provides good coverage, such as the ALD method. Examples of conductive films that form the conductor 240a include tantalum nitride and titanium nitride.

[0486] Furthermore, it is preferable to use a film deposition method that provides good embedding properties, such as the CVD method, for the deposition of the conductive film that will become the conductor 240b. For example, tungsten, molybdenum, copper, etc., can be used as the conductive film that will become the conductor 240b.

[0487] Next, by performing CMP treatment, a portion of the conductive film that will become conductor 240a and a portion of the conductive film that will become conductor 240b are removed, exposing the upper surface of the insulator 285. As a result, these conductive films remain only in the opening 206, making it possible to form a conductor 240 (conductor 240a and conductor 240b) with a flat upper surface (see Figures 1A to 1D). Note that this CMP treatment may remove a portion of the upper surface of the insulator 285.

[0488] As described above, a semiconductor device having the transistor 200 and the capacitive element 100 shown in Figures 1A to 1D can be fabricated. As shown in Figures 8A to 26D, by using the semiconductor device fabrication method shown in this embodiment, the fabrication process for a semiconductor device having the capacitive element 100 and the transistor 200 can be reduced.

[0489] The methods for forming the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B are not limited to those described above. Other methods for forming the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B are described below.

[0490] The process for depositing the insulating film 224Af, the oxide film 230Af, and the oxide film 230Bf is the same as described above.

[0491] Next, the insulating film 224Af, oxide film 230Af, and oxide film 230Bf are processed into island-like structures using lithography to form the insulator 224, oxide 230a, and oxide 230b (see Figures 27A to 27D). Here, the insulator 224, oxide 230a, and oxide 230b are formed so that at least a portion of them overlaps with the conductor 205. The above processing can be performed using either dry etching or wet etching. Dry etching is suitable for microfabrication. Furthermore, the processing of the insulating film 224Af, oxide film 230Af, and oxide film 230Bf may be carried out under different conditions.

[0492] Next, an opening 206b is formed in the insulator 222 in the same manner as the process shown in Figures 11A to 11D.

[0493] Next, conductive films 242Af and 242Bf are deposited sequentially on the insulator 222 and oxide 230b (see Figures 28A to 28D). For details on the deposition methods of conductive films 242Af and 242Bf, please refer to the descriptions in Figures 12A to 12D.

[0494] Next, the conductive films 242Af and 242Bf are processed using lithography to form island-like conductive layers 242A and 242B (see Figures 13A to 13D). Openings may also be formed when processing the conductive films 242Af and 242Bf into island shapes.

[0495] By using the above method, the processing of the insulator 224, oxide 230a, and oxide 230b, and the processing of the conductive layer 242A and conductive layer 242B can be carried out independently.

[0496] The above describes another method for forming the insulator 224, oxide 230a, oxide 230b, conductive layer 242A, and conductive layer 242B.

[0497] <Microwave Processing Equipment> The following describes a microwave processing apparatus that can be used in the manufacturing method of the semiconductor device described above.

[0498] First, we will explain the configuration of a manufacturing equipment that minimizes the inclusion of impurities during the manufacturing of semiconductor devices and other equipment, using Figures 29 to 32.

[0499] Figure 29 schematically shows a top view of a single-wafer multi-chamber manufacturing apparatus 2700. The manufacturing apparatus 2700 includes an atmospheric substrate supply chamber 2701 equipped with a cassette port 2761 for housing substrates and an alignment port 2762 for aligning substrates; an atmospheric substrate transport chamber 2702 for transporting substrates from the atmospheric substrate supply chamber 2701; a load lock chamber 2703a for loading substrates and switching the pressure inside the chamber from atmospheric pressure to reduced pressure or from reduced pressure to atmospheric pressure; an unload lock chamber 2703b for unloading substrates and switching the pressure inside the chamber from reduced pressure to atmospheric pressure or from atmospheric pressure to reduced pressure; a transport chamber 2704 for transporting substrates in a vacuum; and chambers 2706a, 2706b, 2706c, and 2706d.

[0500] Furthermore, the atmospheric substrate transport chamber 2702 is connected to the load lock chamber 2703a and the unload lock chamber 2703b, the load lock chamber 2703a and the unload lock chamber 2703b are connected to the transport chamber 2704, and the transport chamber 2704 is connected to chambers 2706a, 2706b, 2706c, and 2706d.

[0501] Furthermore, gate valves GV are provided at the connection points of each chamber, and each chamber can be independently maintained in a vacuum state, except for the atmospheric substrate supply chamber 2701 and the atmospheric substrate transport chamber 2702. In addition, a transport robot 2763a is provided in the atmospheric substrate transport chamber 2702, and a transport robot 2763b is provided in the transport chamber 2704. Transport robots 2763a and 2763b can transport substrates within the manufacturing apparatus 2700.

[0502] The back pressure (total pressure) in the transport chamber 2704 and each chamber is, for example, 1 × 10⁻⁶. -4 Pa or less, preferably 3 × 10 -5 Pa or less, more preferably 1 × 10⁻⁶ -5 The pressure shall be less than or equal to Pa. Furthermore, the partial pressure of gas molecules (atoms) with a mass-to-charge ratio (m / z) of 18 in the transport chamber 2704 and each chamber shall be, for example, 3 × 10⁻⁶. -5 Pa or less, preferably 1 × 10⁻⁶ -5 Pa or less, more preferably 3 × 10 -6 The pressure shall be less than or equal to Pa. Furthermore, the partial pressure of gas molecules (atoms) with an m / z of 28 in the transport chamber 2704 and each chamber shall be, for example, 3 × 10⁻⁶. -5 Pa or less, preferably 1 × 10⁻⁶ -5 Pa or less, more preferably 3 × 10 -6 The pressure shall be less than or equal to Pa. Furthermore, the partial pressure of gas molecules (atoms) with an m / z of 44 in the transport chamber 2704 and each chamber shall be, for example, 3 × 10⁻⁶. -5 Pa or less, preferably 1 × 10⁻⁶ -5 Pa or less, more preferably 3 × 10 -6 It should be Pa or less.

[0503] The total pressure and partial pressure in the transport chamber 2704 and each chamber can be measured using an ionization vacuum gauge, mass spectrometer, etc.

[0504] Furthermore, it is desirable that the transport chamber 2704 and each chamber be configured to minimize external or internal leaks. For example, the leak rate of the transport chamber 2704 should be 1 × 10⁻⁶. 0 Pa / min or less, preferably 5 × 10 -1The pressure should be less than or equal to Pa / min. Furthermore, the leak rate of each chamber should be 1 × 10⁻⁶. -1 Pa / min or less, preferably 5 × 10 -2 The rate should be less than or equal to Pa / min.

[0505] The leak rate can be derived from the total pressure and partial pressure measured using an ionization vacuum gauge, mass spectrometer, etc. For example, it can be derived from the total pressure 10 minutes after starting vacuuming with a vacuum pump such as a turbomolecular pump, and the total pressure 10 minutes after closing the valve. The total pressure 10 minutes after starting vacuuming should be the average value obtained by measuring the total pressure multiple times.

[0506] The leak rate depends on both external and internal leaks. External leaks occur when gas enters from outside the vacuum system due to tiny holes, faulty seals, etc. Internal leaks are caused by leaks from valves or other partitions within the vacuum system, or by the release of gas from internal components. To keep the leak rate below the aforementioned values, countermeasures must be taken from both external and internal leaks.

[0507] For example, the opening and closing parts of the conveying chamber 2704 and each chamber may be sealed with metal gaskets. Preferably, the metal gaskets are made of metal coated with iron fluoride, aluminum oxide, or chromium oxide. Metal gaskets offer better adhesion than O-rings, reducing external leakage. Furthermore, using a passivated metal coated with iron fluoride, aluminum oxide, or chromium oxide suppresses the release of impurity-containing gases from the metal gasket, thereby reducing internal leakage.

[0508] Furthermore, aluminum, chromium, titanium, zirconium, nickel, or vanadium, which emit less impurity-containing gas, are used as components of the manufacturing apparatus 2700. Alternatively, the aforementioned metals that emit less impurity-containing gas may be used as a coating on an alloy containing iron, chromium, and nickel. Alloys containing iron, chromium, and nickel are rigid, heat-resistant, and suitable for processing. Here, reducing the surface area by reducing surface irregularities of the components through polishing or other means can reduce the emission of gas.

[0509] Alternatively, the components of the aforementioned manufacturing apparatus 2700 may be coated with iron fluoride, aluminum oxide, chromium oxide, or the like.

[0510] The components of the manufacturing apparatus 2700 are preferably made of metal as much as possible. For example, when installing viewing windows made of quartz or the like, it is advisable to thinly coat the surface with iron fluoride, aluminum oxide, chromium oxide, etc., to suppress the release of gases.

[0511] The adsorbed substances present in the transport chamber 2704 and each chamber do not affect the pressure in the transport chamber 2704 and each chamber because they are adsorbed onto the inner walls, but they cause gas release when the transport chamber 2704 and each chamber are evacuated. Therefore, although there is no correlation between the leak rate and the exhaust rate, it is important to use a pump with high exhaust capacity to desorb as much of the adsorbed substances present in the transport chamber 2704 and each chamber as possible and evacuate them in advance. In addition, the transport chamber 2704 and each chamber may be baked to promote the desorption of adsorbed substances. Baking can increase the desorption rate of adsorbed substances by about 10 times. Baking should be performed at a temperature between 100°C and 450°C. At this time, if the adsorbed substances are removed while introducing an inert gas into the transport chamber 2704 and each chamber, the desorption rate of water and other substances that are difficult to desorb by exhaust alone can be further increased. In addition, the desorption rate of adsorbed substances can be further increased by heating the introduced inert gas to the same temperature as the baking temperature. It is preferable to use a noble gas as the inert gas here.

[0512] Alternatively, it is preferable to increase the pressure in the transport chamber 2704 and each chamber by introducing an inert gas such as a heated noble gas or oxygen, and then exhaust the transport chamber 2704 and each chamber again after a certain period of time. By introducing a heated gas, adsorbed substances can be removed from the transport chamber 2704 and each chamber, and impurities present in the transport chamber 2704 and each chamber can be reduced. This process is most effective when repeated 2 to 30 times, preferably 5 to 15 times. Specifically, the pressure in the transport chamber 2704 and each chamber can be set to 0.1 Pa to 10 kPa, preferably 1 Pa to 1 kPa, and more preferably 5 Pa to 100 Pa by introducing an inert gas or oxygen with a temperature of 40°C to 400°C, preferably 50°C to 200°C, and the period for maintaining the pressure should be 1 minute to 300 minutes, preferably 5 minutes to 120 minutes. Subsequently, the transport chamber 2704 and each chamber are evacuated for a period of 5 minutes to 300 minutes, preferably 10 minutes to 120 minutes.

[0513] Next, chambers 2706b and 2706c will be described using the schematic cross-sectional diagrams shown in Figure 30.

[0514] Chambers 2706b and 2706c are chambers capable of performing microwave processing on an object to be processed. The only difference between chambers 2706b and 2706c is the atmosphere used during microwave processing. Other configurations are common to both chambers, and will therefore be described together below.

[0515] Chambers 2706b and 2706c each have a slot antenna plate 2808, a dielectric plate 2809, a substrate holder 2812, and an exhaust port 2819. Outside of chambers 2706b and 2706c, a gas supply source 2801, a valve 2802, a high-frequency generator 2803, a waveguide 2804, a mode converter 2805, a gas pipe 2806, a waveguide 2807, a matching box 2815, a high-frequency power supply 2816, a vacuum pump 2817, and a valve 2818.

[0516] The high-frequency generator 2803 is connected to the mode converter 2805 via a waveguide 2804. The mode converter 2805 is connected to the slot antenna plate 2808 via a waveguide 2807. The slot antenna plate 2808 is positioned in contact with the dielectric plate 2809. The gas supply source 2801 is connected to the mode converter 2805 via a valve 2802. Gas is then supplied to chambers 2706b and 2706c through a gas pipe 2806 that passes through the mode converter 2805, waveguide 2807, and dielectric plate 2809. The vacuum pump 2817 has the function of exhausting gas and other substances from chambers 2706b and 2706c via a valve 2818 and an exhaust port 2819. The high-frequency power supply 2816 is connected to the substrate holder 2812 via a matching box 2815.

[0517] The substrate holder 2812 has the function of holding the substrate 2811. For example, it has the function of electrostatically or mechanically chucking the substrate 2811. It also functions as an electrode to which power is supplied from the high-frequency power supply 2816. It also has an internal heating mechanism 2813 and has the function of heating the substrate 2811.

[0518] As the vacuum pump 2817, for example, a dry pump, mechanical booster pump, ion pump, titanium sublimation pump, cryopump, or turbomolecular pump can be used. In addition to the vacuum pump 2817, a cryotrap may also be used. Using a cryopump and cryotrap is particularly preferable because it allows for efficient water removal.

[0519] Furthermore, the heating mechanism 2813 may be, for example, a heating mechanism that uses a resistance heating element. Alternatively, it may be a heating mechanism that heats by heat conduction or thermal radiation from a heated medium such as a gas. For example, RTA (Rapid Thermal Annealing) such as GRTA (Gas Rapid Thermal Annealing) or LRTA (Lamp Rapid Thermal Annealing) can be used. GRTA performs heat treatment using a high-temperature gas. An inert gas is used as the gas.

[0520] Furthermore, the gas supply source 2801 may be connected to the purifier via a mass flow controller. It is preferable to use a gas with a dew point of -80°C or lower, preferably -100°C or lower. For example, oxygen gas, nitrogen gas, and noble gases (such as argon gas) may be used.

[0521] For example, silicon oxide (quartz), aluminum oxide (alumina), or yttrium oxide (yttria) may be used as the dielectric plate 2809. Furthermore, another protective layer may be formed on the surface of the dielectric plate 2809. The protective layer may be made of magnesium oxide, titanium oxide, chromium oxide, zirconium oxide, hafnium oxide, tantalum oxide, silicon oxide, aluminum oxide, or yttrium oxide. Since the dielectric plate 2809 will be exposed to particularly high-density regions of the high-density plasma 2810 described later, providing a protective layer can mitigate damage. As a result, an increase in particles during processing can be suppressed.

[0522] The high-frequency generator 2803 has the function of generating microwaves in frequencies such as 0.3 GHz to 3.0 GHz, 0.7 GHz to 1.1 GHz, or 2.2 GHz to 2.8 GHz. The microwaves generated by the high-frequency generator 2803 are transmitted to the mode converter 2805 via the waveguide 2804. In the mode converter 2805, the microwaves transmitted as TE mode are converted to TEM mode. The microwaves are then transmitted to the slot antenna plate 2808 via the waveguide 2807. The slot antenna plate 2808 is provided with multiple slot holes, and the microwaves pass through these slot holes and the dielectric plate 2809. This generates an electric field below the dielectric plate 2809, thereby generating a high-density plasma 2810. The high-density plasma 2810 contains ions and radicals depending on the type of gas supplied from the gas supply source 2801. For example, oxygen radicals are present.

[0523] At this time, the ions and radicals generated in the high-density plasma 2810 can modify the film on the substrate 2811. It is preferable to apply a bias to the substrate 2811 using the high-frequency power supply 2816. For example, the high-frequency power supply 2816 can be an RF (Radio Frequency) power supply with frequencies such as 13.56 MHz or 27.12 MHz. By applying a bias to the substrate, the ions in the high-density plasma 2810 can efficiently reach deep into the openings of the film on the substrate 2811.

[0524] For example, oxygen radical treatment using high-density plasma 2810 can be performed by introducing oxygen from gas supply source 2801 in chamber 2706b or chamber 2706c.

[0525] Next, chambers 2706a and 2706d will be described using the schematic cross-sectional diagrams shown in Figure 31.

[0526] Chambers 2706a and 2706d are chambers capable of irradiating the workpiece with electromagnetic waves, for example. The only difference between chambers 2706a and 2706d is the type of electromagnetic wave they emit. Since many other components are common to both, they will be described together below.

[0527] Chambers 2706a and 2706d each have one or more lamps 2820, a substrate holder 2825, a gas inlet 2823, and an exhaust port 2830. Outside of chambers 2706a and 2706d, a gas supply source 2821, a valve 2822, a vacuum pump 2828, and a valve 2829 are provided.

[0528] The gas supply source 2821 is connected to the gas inlet 2823 via valve 2822. The vacuum pump 2828 is connected to the exhaust port 2830 via valve 2829. The lamp 2820 is positioned opposite the substrate holder 2825. The substrate holder 2825 has the function of holding the substrate 2824. The substrate holder 2825 also has an internal heating mechanism 2826 that has the function of heating the substrate 2824.

[0529] For lamp 2820, for example, a light source having the function of emitting electromagnetic waves such as visible light or ultraviolet light may be used. For example, a light source having the function of emitting electromagnetic waves with peaks in wavelengths of 10 nm to 2500 nm, 500 nm to 2000 nm, or 40 nm to 340 nm may be used.

[0530] For example, lamp 2820 can be a light source such as a halogen lamp, metal halide lamp, xenon arc lamp, carbon arc lamp, high-pressure sodium lamp, or high-pressure mercury lamp.

[0531] For example, electromagnetic waves emitted from the lamp 2820 can be partially or entirely absorbed by the substrate 2824, thereby modifying the film on the substrate 2824. For example, defects can be created or reduced, or impurities can be removed. Furthermore, if the substrate 2824 is heated during the process, the creation or reduction of defects or the removal of impurities can be performed more efficiently.

[0532] Alternatively, for example, the substrate holder 2825 may be heated by electromagnetic waves emitted from the lamp 2820, thereby heating the substrate 2824. In this case, the substrate holder 2825 does not need to have a heating mechanism 2826 inside.

[0533] For vacuum pump 2828, refer to the description for vacuum pump 2817. For heating mechanism 2826, refer to the description for heating mechanism 2813. For gas supply source 2821, refer to the description for gas supply source 2801.

[0534] The microwave processing apparatus that can be used in this embodiment is not limited to the one described above. The microwave processing apparatus 2900 shown in Figure 32 can be used. The microwave processing apparatus 2900 has a quartz tube 2901, an exhaust port 2819, a gas supply source 2801, a valve 2802, a high-frequency generator 2803, a waveguide 2804, a gas pipe 2806, a vacuum pump 2817, and a valve 2818. The microwave processing apparatus 2900 also has a substrate holder 2902 inside the quartz tube 2901 that holds a plurality of substrates 2811 (2811_1 to 2811_n, where n is an integer of 2 or more). The microwave processing apparatus 2900 may also have a heating means 2903 on the outside of the quartz tube 2901.

[0535] Microwaves generated by the high-frequency generator 2803 are irradiated onto a substrate placed inside the quartz tube 2901 via the waveguide 2804. The vacuum pump 2817 is connected to the exhaust port 2819 via the valve 2818, and can adjust the pressure inside the quartz tube 2901. The gas supply source 2801 is connected to the gas pipe 2806 via the valve 2802, and can introduce a desired gas into the quartz tube 2901. The heating means 2903 can heat the substrate 2811 inside the quartz tube 2901 to a desired temperature. Alternatively, the heating means 2903 may heat the gas supplied from the gas supply source 2801. The microwave processing device 2900 can perform heating and microwave processing on the substrate 2811 simultaneously. Alternatively, the substrate 2811 can be heated first, followed by microwave processing, or the substrate 2811 can be microwaved first, followed by heating.

[0536] Substrates 2811_1 to 2811_n may all be processing substrates forming semiconductor devices or memory devices, or some of the substrates may be dummy substrates. For example, substrates 2811_1 and 2811_n may be dummy substrates, and substrates 2811_2 to 2811_n-1 may be processing substrates. Alternatively, substrates 2811_1, 2811_2, 2811_n-1, and 2811_n may be dummy substrates, and substrates 2811_3 to 2811_n-2 may be processing substrates. Using dummy substrates is preferable because it allows multiple processing substrates to be processed uniformly during microwave processing or heat processing, reducing variations between processing substrates. For example, it is preferable to place dummy substrates on the processing substrates closest to the high-frequency generator 2803 and waveguide 2804, as this suppresses direct exposure of the processing substrates to microwaves.

[0537] By using the above manufacturing equipment, it becomes possible to modify the film while suppressing the inclusion of impurities in the processed material.

[0538] <Modified examples of semiconductor devices> In the following section, an example of a semiconductor device, which is one embodiment of the present invention, will be described using Figures 33A to 35B.

[0539] In Figures 33 and 34, A in each figure shows a top view of the semiconductor device. B in each figure is a cross-sectional view corresponding to the area indicated by the dashed line A1-A2 in A of each figure. C in each figure is a cross-sectional view corresponding to the area indicated by the dashed line A3-A4 in A of each figure. D in each figure is a cross-sectional view corresponding to the area indicated by the dashed line A5-A6 in A of each figure. In the top view A of each figure, some elements have been omitted for clarity.

[0540] In the semiconductor devices shown in Figures 33A to 35B, structures having the same function as those constituting the semiconductor device shown in <Example of Semiconductor Device Configuration> are denoted by the same reference numerals. Furthermore, in this section as well, the materials used for the semiconductor device components are those described in detail in <Example of Semiconductor Device Configuration>.

[0541] The semiconductor devices shown in Figures 33A to 33D are modified versions of the semiconductor devices shown in Figures 1A to 1D. The semiconductor devices shown in Figures 33A to 33D differ from those shown in Figures 1A to 1D in that they have insulators 283 and 221.

[0542] The insulator 283 is provided between the insulator 282 and the insulator 285. In this case, a part of the conductor 156 and a part of the insulator 153 are in contact with the upper surface of the insulator 283. It is preferable to use an insulator 283 that has the function of suppressing hydrogen diffusion. This prevents hydrogen from diffusing from above the insulator 283 to the transistor 200. The insulator 283 can be any insulator that can be used for the insulator 275 described above. For example, silicon nitride deposited by sputtering can be used as the insulator 283. By depositing the insulator 283 by sputtering, a high-density silicon nitride film can be formed. Alternatively, as the insulator 283, silicon nitride deposited by PEALD or CVD may be laminated on top of the silicon nitride deposited by sputtering.

[0543] By providing an insulator 282 in the region sandwiched between insulators 212 and 283, in contact with insulator 280, and having the function of capturing impurities such as hydrogen, impurities such as hydrogen contained in insulator 280 can be captured, and the amount of hydrogen in that region can be kept constant. In particular, using aluminum oxide having an amorphous structure as insulator 282 is preferable because it can capture or fix hydrogen more effectively. As a result, a transistor 200 and semiconductor device with good characteristics and high reliability can be manufactured.

[0544] In this case, it is preferable that the insulator 283 is formed together with the insulator 282 to create the opening 206c. That is, it is preferable to form the insulator 283 on the insulator 282 first, and then to perform the step of forming the opening 206c shown in Figure 25.

[0545] The transistor 200 shown in Figures 33A to 33D is configured in which the insulator 283 is provided as a single layer, but the present invention is not limited to this. For example, the insulator 283 may be provided as a stacked structure of two or more layers.

[0546] For example, when forming a two-layer laminated structure of the insulator 283, silicon nitride may be deposited as the lower layer of the insulator 283 using the sputtering method, and silicon nitride may be deposited as the upper layer of the insulator 283 using the ALD method. By using the sputtering method, which does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration in the lower layer of the insulator 283 can be reduced. Furthermore, if pinholes or stepped defects are formed in the film deposited by the sputtering method, the portion overlapping with the pinholes or stepped defects can be sealed using the film deposited by the ALD method, which has good coverage.

[0547] Furthermore, when the insulator 283 is constructed in a two-layer laminated structure, a portion of the upper surface of the upper layer of the insulator 283 may be removed. Also, it may be difficult to clearly detect the boundary between the upper and lower layers of the insulator 283.

[0548] The insulator 221 is provided between the insulator 216 and the conductor 205 and the insulator 222. Preferably, the insulator 221 has the function of suppressing hydrogen diffusion. This prevents hydrogen from diffusing from below the insulator 221 to the transistor 200. The insulator 221 can also perform the function of the insulator 212. In such a case, by omitting the insulator 212, the manufacturing process of the semiconductor device can be simplified and productivity can be improved.

[0549] Furthermore, any insulator that can be used for the insulator 275 described above may be used as the insulator 221. For example, it is preferable to use silicon nitride deposited by the ALD method (especially the PEALD method) as the insulator 221. By using the ALD method to deposit the insulator 221, even if irregularities are formed between the insulator 216 and the conductor 205, the insulator 221 can be deposited with good coverage. Therefore, it is possible to suppress the formation of pinholes or stepped breaks in the insulator 222 deposited on the insulator 221.

[0550] In this case, an opening may be formed in the insulator 221, overlapping with the opening 206b formed in the insulator 222. Also, if the film thickness of the insulator 221 is thick, a recess may be formed in the insulator 222, overlapping with the opening 206b formed in the insulator 222.

[0551] Furthermore, an insulator having the function of suppressing hydrogen diffusion may be provided between insulator 222 and insulator 224. This suppresses the diffusion of hydrogen from below the insulator to transistor 200.

[0552] Furthermore, as shown in Figures 33B and 33C, the conductor 205 may be a three-layer laminated structure of conductor 205a, conductor 205b, and conductor 205c. Conductor 205c is provided in contact with the upper surface of conductor 205b. The side surface of conductor 205c may be in contact with conductor 205a. Alternatively, the upper surface of conductor 205c and the uppermost part of conductor 205a may coincide or approximately coincide.

[0553] It is preferable that the conductor 205c be made of a conductive material that has the function of reducing hydrogen diffusion, similar to the conductor 205a. This allows the conductor 205b to be enclosed by the conductors 205a and 205c, thereby preventing impurities such as hydrogen contained in the conductor 205b from diffusing into the oxide 230 via the insulators 216 and 224. Furthermore, by using conductive materials for the conductors 205a and 205c that have the function of suppressing oxygen diffusion, it is possible to suppress the oxidation of the conductor 205b and the resulting decrease in conductivity.

[0554] The semiconductor devices shown in Figures 34A to 34D are modified versions of the semiconductor devices shown in Figures 1A to 1D. Figure 35A shows an enlarged cross-sectional view of the vicinity of the conductor 240 shown in Figure 34B, and Figure 35B shows a plan view corresponding to Figure 35A. The semiconductor devices shown in Figures 34 and 35 differ from the semiconductor devices shown in Figures 1A to 1D in that the insulator 214 has an opening 206d, the insulator 222 has an opening 206e, and the insulator 282 has an opening 206f. In the cross-sectional view shown in Figure 35A, the width of the opening 206d is defined as width W3d, the width of the opening 206e is defined as width W3e, and the width of the opening 206f is defined as width W3f.

[0555] As shown in Figure 35B, it is preferable that openings 206d, 206e, and 206f are positioned inside opening 206 in a plan view. In this case, as shown in Figure 35A, widths W3d, W3e, and W3f become smaller than width W1. Therefore, the sides of insulators 214, 222, and 282 protrude towards the conductor 240 side more than the sides of insulators 212, 216, 275, 280, and 285.

[0556] In the structures shown in Figures 34 and 35, a portion of the insulator 214, a portion of the insulator 222, and a portion of the insulator 282 are arranged to protrude, superimposed on the region where the opening 206 is formed. In other words, protrusions made of a difficult-to-etch material are repeatedly provided superimposed on the region where the opening 206 is formed. By using such a structure, it is possible to prevent the width W1 of the opening 206 from becoming excessively large when the opening 206 is opened all at once in the process shown in Figure 26. This reduces the area occupied by the opening...

Claims

[Claim 1] A memory cell having a transistor and a capacitive element, a first insulator, a second insulator on the first insulator, and a third insulator on the second insulator, The aforementioned transistor is The oxide on the first insulator and, A first conductor and a second conductor on the oxide, A fourth insulator on the aforementioned oxide, The fourth insulator has a third conductor, The second insulator is placed on the first conductor and the second conductor. The third insulator is placed on the third conductor and the second insulator. The second insulator has a first opening that overlaps with the oxide, The fourth insulator and the third conductor are arranged within the first opening. The second insulator and the third insulator each have a second opening that overlaps with the second conductor, The capacitive element has a fourth conductor in contact with the upper surface of the second conductor, a fifth insulator on the fourth conductor, and a fifth conductor on the fifth insulator. The fourth conductor, the fifth insulator, and the fifth conductor are arranged within the second opening. The second insulator has a third opening, The first insulator has a fourth opening, The third insulator has a fifth opening, The third opening, in a plan view, overlaps with at least a portion of the fourth opening and at least a portion of the fifth opening. A sixth conductor and a portion of the first conductor are arranged within the third opening. The sixth conductor is a storage device having a region that contacts a part of the upper surface and a part of the side surface of the first conductor, A sixth insulator is placed beneath the first insulator. The sixth insulator has a sixth opening, The third opening overlaps with at least a portion of the sixth opening in a plan view. The fourth, fifth, and sixth openings are located inside the third opening in a plan view, and are used as a storage device.

Citation Information

Patent Citations

  • Semiconductor device

    JP2011151383A

  • Semiconductor integrated circuit

    JP2012257187A

  • Semiconductor device

    JP2015181159A

  • Semiconductor device

    JP2015188070A

  • Semiconductor device and method of manufacturing semiconductor device

    WO2020008304A1