Doped amorphous optical instrument films and deposition via dopant atom incorporation
By depositing optical device and dopant materials at varying rates in a chamber, the method addresses the challenges of high costs and non-uniformity in amorphous film formation, achieving uniform refractive index and low absorption loss in optical device films across a wider temperature range.
Patent Information
- Application Number
- JP2024150487
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-22
- Filing Date
- 2024-09-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Conventional physical vapor deposition processes for forming amorphous optical device films require specialized hardware and high manufacturing costs due to the need for low substrate temperatures to prevent crystallization, while higher temperatures result in non-uniform polycrystalline films, and temperatures above 200°C cause significant crystallization.
A method involving the deposition of a doped optical device film by arranging an optical device substrate in a chamber with both an optical device material and a dielectric target, using different power levels to deposit optical device and dopant materials at varying rates, allowing for the formation of an amorphous film with a uniform refractive index greater than 2.0 and low absorption loss, even at temperatures up to 300°C.
The method enables the production of doped optical device films with uniform refractive index and low absorption loss, expanding the temperature process window for amorphous film formation and reducing manufacturing complexity and costs.
Smart Images

Figure 0007955317000001 
Figure 0007955317000002 
Figure 0007955317000003
Abstract
Description
[Technical Field]
[0001] Embodiments of the present disclosure generally relate to the manufacture of optical devices. More specifically, the embodiments described herein provide doped optical device films, optical devices having doped structures, and methods of forming doped optical device films and structures. [Background Art]
[0002] Optical devices such as waveguides, planar optical devices, metasurfaces, color filters, and anti-reflection coatings are designed to exhibit high refractive index and low absorption loss properties. Conductive materials have a high refractive index and low absorption loss, which enables efficient and large-scale manufacturing of optical devices.
[0003] Optical devices with polycrystalline films may be non-uniform, have high surface roughness, and be birefringent, whereas amorphous films are uniform, smooth, and have a uniform refractive index. However, conventional physical vapor deposition (PVD) processes for forming amorphous films for optical devices are performed at substrate temperatures below 30°C to suppress crystal formation. Processing titanium dioxide at temperatures below 30°C requires specialized hardware, increasing manufacturing costs and complexity, while processing temperatures above approximately 30°C result in polycrystalline titanium dioxide films with significantly increased non-uniformity. Furthermore, processing temperatures above approximately 200°C cause significant crystallization in the films.
[0004] Accordingly, there is a need in the art for improved doped optical device films, optical devices having doped structures, and methods of forming doped optical device films and structures. [Summary of the Invention]
[0005] In one embodiment, a method is provided. The method includes arranging an optical device substrate on a substrate support. The substrate support is arranged in a chamber. The chamber includes an optical device material target arranged in the chamber and a dielectric target arranged in the chamber. The optical device material target includes an optical device material, and the dielectric target includes a dopant material. A doped optical device film is deposited on the optical device substrate. Depositing the doped optical device film includes depositing the optical device material to form an optical device layer on the surface of the optical device substrate and depositing the dopant material in the optical device layer to form a doped optical device film. Depositing the optical device material includes providing a first power level to the optical device material target to deposit the optical device layer at a first deposition rate. Depositing the dopant material in the optical device layer includes providing a second power level to the dielectric target to deposit the dielectric target at a second deposition rate. The first deposition rate and the second deposition rate are different.
[0006] In another embodiment, a method is provided. This method involves placing an optical device substrate in a chamber containing a target having a pre-doped optical device material. The pre-doped optical device material includes an optical device material of a first concentration and a dopant material of a second concentration. Power is supplied to the target to deposit a doped amorphous optical device layer on the optical device substrate.
[0007] In another embodiment, a method is provided. This method includes arranging an optical device substrate on a substrate support. The substrate support is placed in a chamber. The chamber includes an optical device material target and a dielectric target. The optical device material target includes a metallic material, and the dielectric target includes a dopant material. A doped optical device film is deposited on the optical device substrate. Depositing the doped optical device film includes depositing the optical device material to form an optical device layer on the surface of the optical device substrate, and depositing the dopant material in the optical device layer to form a doped optical device film. Depositing the optical device material includes providing a first power level to the optical device material target and providing an oxygen-containing gas to the chamber to deposit the optical device layer at a first deposition rate. Depositing the dopant material in the optical device layer includes providing a second power level to the dielectric target to deposit the dielectric target at a second deposition rate. The first and second deposition rates are different.
[0008] In yet another embodiment, an optical device is provided. The optical device includes an amorphous optical device layer disposed on the surface of an optical device substrate. The amorphous optical device layer includes an amorphous optical device material and a dopant material, the dopant material being incorporated into the amorphous optical device material.
[0009] To allow for a more detailed understanding of the above-mentioned features of this disclosure, a more specific description of this disclosure, which has been briefly summarized above, can be obtained by referring to embodiments, some of which are shown in the accompanying drawings. However, it should be noted that the accompanying drawings show only exemplary embodiments and should not be considered to limit the scope of this disclosure, as other equally valid embodiments may also be permitted. [Brief explanation of the drawing]
[0010] [Figure 1] This is a cross-sectional view of an optical device including a doped optical device film disposed on an optical device substrate according to an embodiment. [Figure 2A] This is a schematic cross-sectional view of a binary optical device structure arranged on an optical device substrate according to an embodiment. [Figure 2B] This is a schematic cross-sectional view of an angled optical device structure arranged on an optical device substrate according to an embodiment. [Figure 3] This is a schematic cross-sectional view of a physical vapor deposition (PVD) processing chamber according to an embodiment. [Figure 4] This is a schematic cross-sectional view of a chemical vapor deposition (CVD) processing chamber according to an embodiment. [Figure 5] This is a schematic top view of a cluster tool according to an embodiment. [Figure 6] This is a flowchart of a method for manufacturing a doped optical device film according to an embodiment. [Figure 7] This is a flowchart of a method for manufacturing a doped optical device film according to an embodiment. [Figure 8] This is a flowchart of a method for manufacturing a doped optical device film according to an embodiment. [Figure 9] This is a flowchart of a method for manufacturing a doped optical device film according to an embodiment. [Modes for carrying out the invention]
[0011] To facilitate understanding, the same reference numerals have been used to indicate identical elements common to multiple figures where possible. It is assumed that elements and features of one embodiment may be advantageously incorporated into other embodiments without further description.
[0012] The embodiments described herein relate to the manufacture of optical devices. Specifically, the embodiments described herein provide doped optical device films, optical devices having doped structures, and methods for forming doped optical device films and structures. The embodiments described herein provide doped optical device films and structures having an optical device layer having an optical device material concentration of an optical device material, and a dopant material having a dopant concentration throughout the entire thickness of the doped optical device film and structure.
[0013] The optical device materials described and referenced herein have an optical device material refractive index of about 2.0 or greater. The dopant materials described and referenced herein have a dopant refractive index of less than 2.0. The combination of the optical device material and the uniformly distributed dopant material constitutes a doped optical device film with an optical device refractive index of about 2.0 or greater. The optical device layer is formed when the optical device material is oxidized, nitrided, or oxynitrided and deposited or flowed onto an optical device substrate. In one embodiment, which can be combined with other embodiments described herein, the optical device material includes a uniformly distributed dopant material.
[0014] In one embodiment, which can be combined with other embodiments described herein, the optical device material is a metal-containing material. Examples of metal-containing materials include, but are not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides. In another embodiment, which can be combined with other embodiments described herein, the optical device material is a semiconductor material. Examples of semiconductor materials include, but are not limited to, silicon (Si), germanium (Ge), silicon-germanium (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor material is an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, or transparent conductive oxides. Examples of dopant materials include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides.
[0015] In one embodiment, the method includes placing an optical device substrate on a substrate support arranged in a chamber. An optical device material is deposited on the surface of the optical device substrate to form an optical device layer. Depositing the optical device material includes providing a first power level to an optical device material target to deposit the optical device material at a first deposition rate. A dopant material is uniformly deposited in the optical device layer to form a doped optical device film. Depositing the dopant material includes providing a second power level to a dielectric target to deposit the dopant material at a second deposition rate.
[0016] Figure 1 is a cross-sectional view of the optical device 100. The doped optical device film 101 is placed on the surface 103 of the optical device substrate 102 according to embodiments described herein. The doped optical device film 101 is formed by the methods described herein 600, 700, 800, and 900. The optical device substrate 102 is any suitable optical device substrate on which an optical device can be formed. In one embodiment, the optical device substrate 102 includes, but is not limited to, silicon (Si), silicon nitride (SiN), silicon dioxide (SiO2), fused silica, quartz, silicon carbide (SiC), germanium (Ge), silicon germanium (SiGe), indium phosphide (InP), gallium arsenide (GaAs), gallium oxide (GaO), diamond, lithium niobate (LiNbO3), gallium nitride (GaN), sapphire, tantalum oxide (Ta2O5), titanium dioxide (TiO2), or combinations thereof. The optical device substrate 102 may include an optically transparent perovskite material.
[0017] The doped optical device film 101 includes an optical device layer containing an optical device material. The doped optical device film 101 also includes a dopant material distributed within the optical device layer. The doped optical device film 101 is amorphous to achieve optical properties including a uniform refractive index greater than about 2.0 and low absorption loss. The optical device layer is formed when the optical device material is oxidized, nitrided, or oxynitrided and deposited or flowed onto the optical device substrate 102. Examples of the doped optical device film 101 that can be formed from the reaction of the optical device material and the dopant material include, but are not limited to, tantalum pentoxide (Ta₂O₅), zirconium dioxide (ZrO₂), indium oxide (In₂O₃), or hafnium oxide (HfO₂).
[0018] The doped optical device film 101 has a thickness 110. The thickness 110 is divided into a series of zones 115. In one embodiment that can be combined with other embodiments described herein, the thickness 110 has a uniform or substantially uniform distribution of the dopant material throughout the series of zones 115. In one embodiment, the doped optical device film 101 includes an optical device refractive index greater than about 2.0 that is uniform throughout the thickness 110. In another embodiment, the doped optical device film 101 includes an optical device refractive index of about 2.6 to about 2.7 that is uniform throughout the thickness 110.
[0019] The dopant materials described and referenced herein have a dopant refractive index less than 2.0. The combination of the optical device material forming the optical device layer and the dopant material distributed throughout forms the doped optical device film 101 with an optical device refractive index of about 2.0 or greater.
[0020] The doped optical device film 101 includes the optical device material at an optical device material concentration and the dopant material at a dopant material concentration. The optical device material includes one or both of a metal-containing material and a semiconductor material. Adjustment of the optical device material concentration, the optical device material refractive index, the dopant material concentration, and the dopant material refractive index will determine the optical properties of the optical device film 101, such as the optical device refractive index.
[0021] In one embodiment, which can be combined with other embodiments described herein, the doped optical device film 101 includes an optical device material concentration of about 85% to about 100% atomic percentage. In another embodiment, which can be combined with other embodiments described herein, the doped optical device film 101 includes a dopant material at a dopant concentration of about 0% to 15% atomic percentage. A dopant concentration of about 0 to about 50% affects the morphology of the doped optical device film 101 without significantly detrimentally increasing the refractive index of the optical device layer.
[0022] To achieve desirable optical properties, the dopant material is distributed in the optical device layer and may be maintained within a temperature process window. In some embodiments, the dopant material is uniformly distributed in the optical device layer. The temperature process window is a temperature range in which the optical device layer is formed amorphous to achieve optical properties including uniform high refractive index and low absorption loss. Without the dopant material, the optical device layer is formed amorphous within a certain temperature process window, and forms a crystalline structure when the optical device layer exceeds the temperature process window. The optical device layer without the dopant material is formed amorphous within a temperature process window of less than 30°C, and becomes crystalline at temperatures greater than 30°C. The dopant material uniformly incorporated in the optical device layer suppresses growth of crystalline structures, as described in methods 600, 700, 800, and 900, and expands the temperature process window of the formed doped optical device film 101. The optical device layer with the dopant material uniformly incorporated in the optical device layer at a dopant concentration (e.g., 5 atomic%) expands the temperature process window in which the doped optical device film 101 is formed amorphous to temperatures greater than about 30°C, such as a temperature process window of about 30°C to 300°C.
[0023] Figure 2A is a schematic cross-sectional view of a binary optical device structure 201a disposed on an optical device substrate 102. Figure 2B is a schematic cross-sectional view of an angled optical device structure 201b disposed on an optical device substrate 102. The optical devices 200a and 200b include optical device structures 201a and 201b disposed on the surface 103 of the optical device substrate 102. The optical device structures 201a and 201b can be formed, for example, by etching a doped optical device film 101 formed by the methods 600, 700, 800, and 900 described herein.
[0024] As shown in Figure 2A, the optical device structure 201a is a binary (i.e., vertical) structure. As shown in Figure 2A, the optical device structure 201a includes an upper surface 204 parallel to the surface 103 of the optical device substrate 102. The first side wall 205 and the second side wall 206 are parallel to the third side wall 207 and the fourth side wall 208. The side walls 205, 206, 207, and 208 are oriented toward the principal axis of the optical device substrate 102.
[0025] As shown in Figure 2B, the optical device structure 201b is an angled structure. As shown in Figure 2B, the optical device structure 201b includes a first side wall 205 and a second side wall 206 parallel to the third side wall 207 and the fourth side wall 208. The side walls 205, 206, 207, and 208 are inclined with respect to the surface 103 of the optical device substrate 102.
[0026] The optical device structures 201a and 201b formed from the optical device film 101 include an optical device material concentration and a dopant material concentration distributed throughout the entire thickness 110 of the optical device film 101. The distribution of the dopant material throughout the entire thickness 110 provides a uniform refractive index greater than approximately 2.0 and low absorption loss.
[0027] Figure 3 is a schematic cross-sectional view of the PVD chamber 300. It should be understood that the PVD chamber 300 described below is an illustrative PVD chamber, and other PVD chambers, including PVD chambers from other manufacturers, may be used or modified to achieve embodiments of this disclosure. The PVD chamber 300 can be used in the methods 600, 700, 800, and 900 described herein.
[0028] The PVD chamber 300 is used to form a doped optical device film 101. The PVD chamber 300 includes a plurality of cathodes, including at least one dielectric target cathode 302 and at least one optical device material target cathode 303, each having a plurality of corresponding targets, including at least one dielectric target 304 and at least one optical device material (e.g., metal or semiconductor) target 306, mounted on the chamber body 308. Figure 3 shows one dielectric target 304 and one optical device material target 306, but the PVD chamber 300 may include one or more dielectric targets 304 and / or one or more optical device material targets 306. For example, the PVD chamber 300 may contain 3 to 5 targets selected from at least one of the dielectric targets 304 or the optical device material targets 306. In embodiments having one or more dielectric targets 304 and one or more optical device material targets 306, each dielectric target 304 is operable to deposit different dopant materials and / or each optical device material target 306 is operable to deposit different optical device materials.
[0029] The PVD chamber 300 is configured to include a substrate support 310 having a support surface 312 for supporting the optical device substrate 102. The PVD chamber 300 includes an opening 334 (e.g., a slit valve) through which the optical device substrate can enter the processing space 305.
[0030] In the embodiment shown in Figure 3, the substrate support 310 includes an RF bias power supply 314 coupled to a bias electrode 316 disposed within the substrate support 310. The PVD chamber 300 includes a sputtering gas source 336 that provides a sputtering gas such as argon (Ar). The PVD chamber 300 also includes a reactive gas source 338 that provides a reactive gas such as an oxygen-containing gas or a nitrogen-containing gas.
[0031] The substrate support 310 includes a mechanism (not shown) for holding the optical device substrate 102 on the support surface 312 of the substrate support 310, such as an electrostatic chuck, a vacuum chuck, or a substrate holding clamp. The substrate support 310 is configured to include a cooling conduit 318 disposed within the substrate support 310, which cools the substrate support 310 and the optical device substrate 102 positioned thereon to a predetermined temperature, for example, between approximately 30°C and approximately 300°C. The cooling conduit 318 is coupled to a cooling fluid source 320 to provide the cooling fluid. The substrate support 310 is further configured to include a heater 322 embedded therein. The heater 322, such as a resistive element, disposed within the substrate support 310 is coupled to an optional heater power supply 324 to heat the substrate support 310 and the optical device substrate 102 positioned thereon to a predetermined temperature, for example, between approximately 30°C and 300°C. Each target (e.g., dielectric target 304 or optical device material target 306) has a DC power supply 326 or an RF power supply 328 and an associated magnetron. Multiple power supplies allow both DC power supply processing and RF power supply processing to occur within the same PVD chamber 300.
[0032] The PVD chamber 300 includes a processing gas supply unit 330 for supplying a predetermined processing gas to the processing space 305 of the PVD chamber 300. For example, the processing gas supply unit 330 supplies an oxygen-containing gas to the processing space 305, creating an oxidizing environment in the processing space 305. The PVD chamber 300 may also include a precursor gas source 332 for supplying a precursor gas, such as a gaseous dopant precursor, which is controlled by a precursor gas flow controller 331.
[0033] Figure 4 is a schematic cross-sectional view of the CVD chamber 400. It should be understood that the CVD chamber 400 described below is an exemplary CVD chamber, and other CVD chambers, including CVD chambers from other manufacturers, may be used or modified to achieve aspects of this disclosure.
[0034] The CVD chamber 400 has a chamber body 408 including a processing space 405, on which a substrate support 410 is positioned, supporting an optical device substrate 102. The substrate support 410 includes a heating / cooling conduit 414 and a mechanism for holding the optical device substrate 102 on the support surface 412 of the substrate support 410, such as an electrostatic chuck, a vacuum chuck, or a substrate holding clamp. The substrate support 410 is connected to the processing space 405 and is movable by a stem 406 connected to a lift system (not shown) that moves the substrate support 410 between a raised processing position and a lowered position to facilitate the transfer of the optical device substrate 102 to and from the CVD chamber 400 through an opening 420.
[0035] The CVD chamber 400 includes a first gas source 402, a second gas source 403, and flow controllers 418a, 418b, such as mass flow control (MFC) devices, positioned between the chamber body 408 to control the flow rate of the process gas from the first gas source 402 and the second gas source 403 to a showerhead 404 used to distribute the process gas across the processing space 405. The first gas source 402 is operable to contain optical device material. The second gas source 403 is operable to contain dopant material. Although Figure 4 shows two gas sources 402, 403, the CVD chamber 400 may include one or more first gas sources 402 and / or one or more second gas sources 403. For example, three to five gas sources selected from at least one of the first gas sources 402 or the second gas sources 402 may be included in the chamber 300. In embodiments having one or more first gas sources 402 and one or more second gas sources 403, each first gas source 402 is operable to deposit different optical device materials, and / or each second gas source 403 is operable to deposit different dopant materials.
[0036] The showerhead 404 is connected to an RF power supply 416 by an RF feed 422 for generating plasma from the processing gas into the processing space 405. The RF power supply 416 provides RF energy to the showerhead 404 to facilitate plasma generation between the showerhead 404 and the substrate support 410. The stem 406 is configured to move the substrate support 410 to an elevated processing position.
[0037] Figure 5 is a schematic diagram of a cluster tool 502 in a factory environment 501. It should be understood that the cluster tool 502 described herein is an exemplary cluster and may be used in conjunction with or modified with other cluster tools to implement aspects of this disclosure. The cluster tool 602 described herein may be used in the methods described herein 700, 800, 900, and 1000.
[0038] The cluster tool 502 includes a transfer chamber 506 surrounded by one or more processing chambers 504. The processing chambers 504 may include any suitable type of processing chamber for forming the doped optical device film 101 described herein. In one embodiment, which may be combined with other embodiments described herein, the processing chamber 504 may be a PVD chamber 300. In another embodiment, which may be combined with other embodiments described herein, the processing chamber 504 may be a CVD chamber 400. In yet another embodiment, which may be combined with other embodiments described herein, the processing chamber 504 may be a combination of the PVD chamber 300 and the CVD chamber 400.
[0039] Furthermore, the cluster tool 502 includes a substrate access chamber 508 coupled to the load lock chamber 510. In one embodiment, the substrate access chamber 508 may be used to connect a factory environment 501, which is atmospheric pressure, to a load lock chamber 510, which is under vacuum pressure. In one embodiment, which may be combined with other embodiments described herein, the cluster tool 502 may be used for single-chamber processing, such that the processing chamber 504 is a PVD chamber 300 having at least two targets (e.g., a dielectric target 304 or an optical device material target 306). In another embodiment, which may be combined with other embodiments described herein, the cluster tool 502 may be used for multi-chamber processing, such that the multiple processing chambers are PVD chambers 300, CVD chambers 400, or a combination of both, as in methods 600 to 900. The cluster tool 502 will transport the optical device substrate 102 between the multiple processing chambers 504 so that an optical device layer or dopant material can be deposited in each zone of a series of zones 115 in each processing chamber 504. The optical device substrate enters each chamber 504 by passing through the openings 334 and 420 of the PVD chamber 300 and the CVD chamber 400, respectively.
[0040] Figure 6 is a flowchart of method 600 for manufacturing a doped optical device film 101. For ease of explanation, Figure 6 will be described with reference to the PVD chamber 300 in Figure 3 and the cluster tool 502 in Figure 5. However, it should be noted that PVD chambers other than the PVD chamber 300 in Figure 3 may be used in conjunction with method 600. Also, it should be noted that cluster tools other than the cluster tool 502 in Figure 5 may be used in conjunction with method 600. The cluster tool 502 described above may be used when the processing chamber 504 is the PVD chamber 300. Method 600 deposits the optical device material onto the optical device substrate 102 to form an optical device. In one embodiment, which can be combined with other embodiments described herein, the dopant material may be deposited uniformly over the entire thickness 110 of the optical device layer.
[0041] In operation 601, the optical device substrate 102 intended for coating is placed on a substrate support within the PVD chamber 300. For example, the optical device substrate 102 is placed on a substrate support 310.
[0042] In operation 602, optical device material is deposited. The optical device material is deposited from one or more optical device material targets 306 to form an optical device layer on the optical device substrate 102. The optical device material is either a metal-containing material or a semiconductor material, or both. The optical device material is deposited via a PVD process. In one embodiment, which can be combined with other embodiments described herein, the PVD process is a sputtering process. In another embodiment, which can be combined with other embodiments described herein, the PVD process is an evaporation process.
[0043] In embodiments where the optical device material is a metal, an optical device layer is formed when the deposited metal of one or more optical device material targets 306 reacts with a reactive gas to form an optical device layer on the optical device substrate 102. A reactive gas source 338 provides a reactive gas, such as an oxygen-containing gas or a nitrogen-containing gas. For example, when a pure titanium optical device material is deposited, titanium dioxide (TiO2) is formed as the reactive gas, such as oxygen. In embodiments where the optical device material is a metal oxide, metal nitride, or metal oxynitride, an optical device layer is formed when the optical device material is deposited on the optical device substrate 102. An optical device material target cathode 303 coupled to one or more optical device material targets 306 is set to a first power level to deposit the optical device material at a first deposition rate. When the first power level is applied, the first power level may remain constant throughout operations 602 and 603. The PVD chamber 300 may include one or more optical device material targets 306. For example, the PVD chamber 300 may contain 3 to 5 targets selected from at least one of the optical device material targets 306. In embodiments having one or more optical device material targets 306, each optical device material target 306 is operable to deposit a different optical device material.
[0044] The first power level of the target cathode is in the range of about 0% to about 100%. For example, the first power level of the target cathode is about 80%, and the corresponding first deposition rate is about 0.35 nm / s. In one embodiment, the optical device layer contains an optical device material concentration of about 85% to about 100% atomic percentage. In one embodiment, the optical device material contains a first refractive index. The first refractive index is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8. In embodiments where the optical device material is a metal-containing material, the metal-containing material may be, but is not limited to, metals, metal oxides, metal nitrides, or metal oxynitrides such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). In embodiments where the optical device material is a semiconductor material, the semiconductor material may include, but is not limited to, silicon (Si), germanium (Ge), silicon-germanium (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor material may be an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, or transparent conductive oxides.
[0045] In operation 603, dopant material is deposited. The dopant material is deposited from the dielectric target 304 to form a doped optical device film 101 on the optical device substrate 102. In one embodiment, which can be combined with other embodiments described herein, the dopant material is deposited so as to be uniformly concentrated within the optical device layer to form one or more zones of the doped optical device film 101. The dielectric target cathode 302 coupled to the dielectric target 304 is set to a second power level to deposit the dopant material at a second deposition rate. The second power level of the dielectric target cathode 302 is in the range of about 0% to about 100%. For example, the second power level of the dielectric target cathode 302 is about 80%, and the corresponding second deposition rate is about 0.35 nm / s. In one embodiment, the doped optical device film 101 contains dopant material at dopant concentrations of atomic percentage from about 0% to 15%. Examples of dopant materials include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. The PVD chamber 300 may include one or more dielectric targets 304. For example, the PVD chamber 300 may contain 3 to 5 targets selected from at least one of the dielectric targets 304. In embodiments having one or more dielectric targets 304, each dielectric target 304 is operable to deposit a different dopant material.
[0046] In one embodiment, which may be combined with other embodiments described herein, operations 602 and 603 are repeated by intervals in which a first power level is continuously applied to the optical device material target cathode 303 and intervals in which a second power level is applied to the dielectric target cathode 302. In another embodiment, the deposition of the dopant material at the second power level is carried out by pulse-supplying the second power level at a set frequency while the optical device material is being deposited. In yet another embodiment, which may be combined with other embodiments described herein, the optical device material and the dopant material are deposited simultaneously by simultaneously applying the first and second power levels to a target (e.g., a dielectric target 304 or an optical device material target 306) to form a doped optical device film 101. In one embodiment, which may be combined with other embodiments described herein, a single performance of operations 602 and 603 forms all zones of a series of zones 115. In another embodiment, a single performance of operations 602 and 603 forms a portion of the doped optical device film 101, where the portion may correspond to one or more zones of the series of zones 115. Each zone of the series of zones 115 may be 20 nm to 25 nm apart in thickness 110. Operations 602 and 603 are repeated until a predetermined thickness 110 is reached. In one embodiment, which may be combined with other embodiments described herein, operations 602 and 603 can be performed in a PVD chamber 300 having at least two targets (e.g., a dielectric target 304 or an optical device material target 306). In another embodiment, which may be combined with other embodiments described herein, operations 602 and 603 can be performed in a multi-processing chamber 504 of a cluster tool 502. For example, the optical device substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a PVD chamber 300 containing an optical device material target 306, and at least one of the processing chambers 504 is a PVD chamber 300 containing a dielectric target 302.
[0047] Figure 7 is a flowchart of method 700 for manufacturing a doped optical device film 101. For ease of explanation, Figure 7 will be described with reference to the PVD chamber 300 in Figure 3 and the cluster tool 502 in Figure 5. However, it should be noted that a PVD chamber other than the PVD chamber 300 in Figure 3 may be used in conjunction with method 700. Also, it should be noted that a cluster tool other than the cluster tool 502 in Figure 5 may be used in conjunction with method 700. The cluster tool 502 described above can be used when the processing chamber 504 is the PVD chamber 300.
[0048] In operation 701, the optical device substrate 102 intended for coating is placed on a substrate support within the PVD chamber 300. For example, the optical device substrate 102 is placed on a substrate support 310.
[0049] In operation 702, a pre-doped optical device material is deposited. The pre-doped optical device material is deposited from one or more optical device material targets 306 to form one or more zones 115 of a doped optical device film 101 on the optical device substrate 102. The pre-doped optical device material comprises an optical device material and a dopant material. The pre-doped optical device material may contain either or both a metal-containing material and / or a semiconductor material. Examples of metal-containing materials include, but are not limited to, metals, metal oxides, metal nitrides or metal oxynitrides such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). Examples of semiconductor materials include, but are not limited to, silicon (Si), germanium (Ge), silicon-germanium (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor material is an oxide, oxynitride, nitride, or carbide of Si, Ge, SiGe, III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, or transparent conductive oxides.
[0050] In embodiments where the pre-doped optical device material is a metal, the deposited metal reacts with a reactive gas to form one or more zones 115 of the doped optical device film 101 on the optical device substrate 102. The pre-doped optical device material further includes, but is not limited to, dopant materials, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which can be combined with other embodiments described herein, the dopant material is uniformly pre-doped over the entire pre-doped optical device material. The PVD chamber 300 may include one or more optical device material targets 306. For example, the PVD chamber 300 may contain 3 to 5 targets selected from at least one of the optical device material targets 306. In embodiments having one or more optical device material targets 306, each optical device material target 306 is operable to deposit different pre-doped optical device materials. In one embodiment, the pre-doped optical device material has a first refractive index, which is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8.
[0051] The optical device material target cathode 303 coupled to the optical device material target 306 is set to a first power level in order to deposit the pre-doped optical device material at a first deposition rate. When the first power level is applied, the first power level remains constant throughout operation 702. The pre-doped optical device material provided from the optical device material target 306 has a predetermined concentration, the concentration of the pre-doped optical device material corresponds to the concentration of the doped optical device film 101. In one embodiment, which may be combined with other embodiments described herein, the pre-doped optical device material includes an optical device material concentration of about 85% to about 100% atomic percentage and a dopant material with a dopant material concentration of about 0% to about 15% atomic percentage. For example, the pre-doped optical device material is a titanium dioxide (TiO2) optical device material having a dopant material such as silicon dioxide (TiO2) in the material at an atomic percentage of 5%. In one embodiment, in order to prevent the formation of titanium dioxide (TiO2) crystal grains in the doped optical device film 101, the deposition temperature of the pre-doped optical device material is maintained at approximately 270°C or lower.
[0052] In another embodiment, which may be combined with other embodiments described herein, a single application of operation 702 forms all zones of the series of zones 115. In another embodiment, repetition of operation 702 forms a portion of the doped optical device film 101, where the portion may correspond to one or more zones of the series of zones 115.
[0053] In yet another embodiment, which can be combined with other embodiments described herein, one or more optical device material targets 306 are operable to deposit pre-doped metal-containing material and pre-doped semiconductor material. The pre-doped metal-containing material may be deposited simultaneously with the pre-doped semiconductor material to form a series of zones 115. The pre-doped metal-containing material and the pre-doped semiconductor material may be deposited separately from the same optical device material target 306 or from different optical device material targets 306.
[0054] In yet another embodiment, which can be combined with other embodiments described herein, one or more optical device material targets 306 are operable to deposit pre-doped metal-containing material from two or more optical device material targets 306 to form a series of zones 115. The pre-doped metal-containing material may be deposited individually from the same optical device material target 306 or from different optical device material targets 306.
[0055] Figure 8 is a flow chart of an exemplary method 800 for manufacturing a doped optical device film 101. For ease of explanation, Figure 8 will be described with reference to the PVD chamber 300 in Figure 3, the CVD chamber 400 in Figure 4, and the cluster tool 502 in Figure 5. However, it should be noted that PVD chambers other than the PVD chamber 300 in Figure 3 may be used in conjunction with method 800. It should also be noted that CVD chambers other than the CVD chamber 400 in Figure 4 may be used in conjunction with method 800. Furthermore, it should be noted that cluster tools other than the cluster tool 502 in Figure 5 may be used in conjunction with method 800. The cluster tool 502 described above may be used when the processing chamber 504 is the PVD chamber 300 or the PVD chamber 400. In one embodiment, the processing chamber is a modified PVD chamber, for example, a modified version of the PVD chamber 300 described in Figure 3, equipped to supply a dopant precursor (e.g., a dopant precursor supplied from a precursor gas source 332 controlled by a precursor gas flow controller 331).
[0056] In operation 801, the substrate intended for coating is placed on a substrate support within the PVD chamber 300. For example, the optical device substrate 102 is placed on the substrate support 310.
[0057] In operation 802, optical device material is deposited. The optical device material is deposited from one or more optical device material targets 306 to form an optical device layer on the optical device substrate 102. The optical device material may include one or both of the following: a metal-containing material or a semiconductor material. In one embodiment of operation 802, the processing chamber is a PVD chamber, such as the multi-cathode PVD chamber in Figure 4, and includes an optical device material target cathode 303. The optical device material target cathode 303 is operated at a first power level to deposit the optical device material at a first deposition rate. The optical device material is deposited on the surface of the optical device substrate 102 by setting the optical device material target cathode 303 to a first power level in order to deposit at a first deposition rate and form an optical device layer. For example, the first power level of the optical device material target cathode 303 is in the range of about 0% to about 100%. For example, the first power level of the optical device material target cathode 303 is approximately 80%, and the first deposition rate is approximately 0.35 nm / s. The PVD chamber 300 may include one or more optical device material targets 306. For example, the PVD chamber 300 may contain 3 to 5 targets selected from at least one of the optical device material targets 306. In embodiments having one or more optical device material targets 306, each optical device material target 306 is operable to deposit different optical device materials.
[0058] The optical device layer contains an optical device material at a specific concentration of the optical device material. For example, the concentration of the optical device material is an atomic percentage ranging from about 85% to 100%. In one embodiment, the optical device material contains a first refractive index, which is greater than 2.0. For example, the first refractive index is between about 2.0 and about 2.8.
[0059] In operation 803, a dopant precursor is introduced. The dopant precursor includes a dopant material introduced from a precursor gas source 332 corresponding to the PVD chamber 300 or a second gas source 403 corresponding to the CVD chamber 400. The dopant precursor is introduced to form a doped optical device film 101 on the optical device substrate 102. Examples of dopant precursors include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which can be combined with other embodiments described herein, the dopant precursor is introduced so as to be uniformly concentrated within the optical device layer to form one or more zones of the doped optical device film 101. The optical device material reacts with the dopant precursor to form a doped optical device film 101 on the surface of the optical device substrate 102.
[0060] To deposit the dopant precursor at a flow rate, the dopant precursor is introduced at a second power level. In one embodiment, which may be combined with other embodiments described herein, the precursor gas flow controller 331 coupled to the precursor gas source 332 is set to a second power level. In another embodiment, which may be combined with other embodiments described herein, the second flow controller 418b coupled to the second gas source 403 is set to a first power level. The PVD chamber 300 may include one or more precursor gas sources 332. For example, three to five precursor gas sources 332 may be included in the PVD chamber 300. In embodiments having one or more precursor gas sources 332, each optical device material target 306 is operable to deposit different optical device materials. The CVD chamber 400 may include one or more second gas sources 403. For example, three to five second gas sources 403 may be included in the CVD chamber 400. In embodiments having one or more second gas sources 403, each second gas source 403 is operable to deposit a different dopant precursor.
[0061] In one embodiment, which may be combined with other embodiments described herein, the deposition rate of the optical device material exceeds the flow rate of the dopant precursor, so that the doped optical device film 101 has a lower concentration of dopant material than the optical device material. When a second power level is applied, the second power level remains constant throughout operation 803. In one embodiment, which may be combined with other embodiments described herein, the first power level and the second power level may be different. The optical device material provided by the optical device material target 306 and the dopant precursor provided by the precursor gas source 332 or the second gas source 403 have predetermined concentrations, and the concentration of the combination of optical device material and dopant material corresponds to the concentration of the doped optical device film 101. In one embodiment, which may be combined with other embodiments described herein, the optical device material contains an optical device material concentration of about 85% to about 100% atomic percentage, and the dopant precursor contains a dopant material concentration of about 0% to about 15% atomic percentage.
[0062] In one embodiment, which may be combined with other embodiments described herein, operations 802 and 803 are repeated by intervals of applying a first power level to the optical device material target cathode 303 and intervals of applying a second power level to the precursor gas flow controller 331 or the second flow controller 418b. In another embodiment, dopant material deposition at the second power level is carried out by pulse supplying the second power level at a set frequency while depositing the metallic optical device material. In yet another embodiment, which may be combined with other embodiments described herein, the optical device material is deposited and the dopant precursor is simultaneously flowed by applying the first and second power levels simultaneously to form a doped optical device film 101.
[0063] In one embodiment, which may be combined with other embodiments described herein, a single performance of operations 802 and 803 forms all zones of a series of zones 115 of the doped optical device film 101. In another embodiment, a single performance of operations 802 and 803 forms a portion of the doped optical device film 101, which may correspond to one or more zones of the series of zones 115. Each zone of the series of zones 115 may be 20 nm to 25 nm apart in thickness 110. Operations 802 and 803 are repeated until a predetermined thickness 110 of the doped optical device film 101 is achieved.
[0064] In one embodiment, which may be combined with other embodiments described herein, operations 802 and 803 can be performed in a PVD chamber 300 having at least an optical device material target 306 and a precursor gas source 332. In another embodiment, which may be combined with other embodiments described herein, operations 801 and 802 can be performed in a multi-processing chamber 504 of a cluster tool 502. For example, an optical device substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a PVD chamber 300 including an optical device material target 306, and at least another of the processing chambers 504 is a PVD chamber 300 including a precursor gas source 332. In another embodiment, at least one of the processing chambers 504 is a PVD chamber 300 including an optical device material target 306, and at least another of the processing chambers 504 is a CVD chamber 400 including a second gas source 403.
[0065] Figure 900 is a flowchart of an exemplary method 900 for manufacturing a doped optical device film 101. For ease of explanation, Figure 9 will be described with reference to the CVD chamber 400 in Figure 4 and the cluster tool 502 in Figure 5. However, it should be noted that a CVD chamber other than the CVD chamber 400 in Figure 4 may be used in conjunction with method 900. Also, it should be noted that a cluster tool other than the cluster tool 502 in Figure 5 may be used in conjunction with method 700. The cluster tool 502 described above can be used when the processing chamber 504 is the CVD chamber 400.
[0066] In operation 901, the substrate intended for coating is placed on a substrate support within the CVD chamber 400. For example, the optical device substrate 102 is placed on the substrate support 410.
[0067] In operation 902, an optical device material precursor is flowed. The optical device material precursor includes optical device material flowing in from a first gas source 402 to form an optical device layer on an optical device substrate 102. The optical device material may include one or both of a metal-containing material and / or a semiconductor material. Examples of metal-containing precursors include, but are not limited to, metals, metal oxides, metal nitrides or metal oxynitrides such as titanium dioxide (TiO2), tantalum pentoxide (Ta2O5), zirconium dioxide (ZrO2), indium oxide (In2O3), or hafnium oxide (HfO2). Examples of semiconductor precursors include, but are not limited to, silicon (Si), germanium (Ge), silicon germanium (SiGe), III-V semiconductors, II-IV semiconductors, ternary semiconductors, quaternary semiconductors, transparent conductive oxides, or combinations thereof. In other embodiments, the semiconductor precursor is Si, Ge, SiGe, a III-V semiconductor, a II-IV semiconductor, a ternary semiconductor, a quaternary semiconductor, or an oxide, oxynitride, nitride, or carbide of a transparent conductive oxide.
[0068] In embodiments where the optical device material is a metal, the optical device layer is formed when the metal flowed from the first gas source 402 reacts with a reactive gas to form an optical device layer on the optical device substrate 102. In embodiments where the optical device material is a metal oxide, metal nitride, or metal oxynitride, the optical device layer is formed when the optical device material flows onto the optical device substrate 102. A first flow controller 418a coupled to the first gas source 402 is set to a first power level to allow the optical device material precursor to flow in at a flow rate. Once the first power level is applied, it remains constant throughout operations 902 and 903. The CVD chamber 400 may include one or more first gas sources 402. For example, three to five first gas sources 402 may be included in the chamber 300. Each first gas source 402 is operable to deposit different optical device materials. The CVD chamber 400 may include one or more first gas sources 403. For example, the CVD chamber 400 may contain three to five first gas sources 402. In embodiments having one or more first gas sources 402, each first gas source 402 is operable to deposit different dopant precursors.
[0069] In operation 903, a dopant precursor is introduced. The dopant precursor includes a dopant material introduced from a second gas source 403. The dopant precursor is introduced to form a doped optical device film 101 on the optical device substrate 102. Examples of dopant precursors include, but are not limited to, silicon (Si), aluminum (Al), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), or hafnium (Hf), and their oxides, nitrides, or oxynitrides. In one embodiment, which can be combined with other embodiments described herein, the dopant precursor is introduced so as to be uniformly concentrated within the optical device layer to form one or more zones of the doped optical device film 101. In embodiments where the optical device material precursor is a titanium precursor and the dopant precursor is oxygen (O2), the metal-containing precursor reacts with the precursor to form titanium dioxide (TiO2).
[0070] To deposit the dopant precursor at a flow rate, the dopant precursor is introduced at a second power level. In one embodiment, which may be combined with other embodiments described herein, a second flow controller 418b coupled to a second gas source 403 is set to a second power level. In one embodiment, which may be combined with other embodiments described herein, the flow rate of the optical device material precursor exceeds the flow rate of the dopant precursor, so that the dopant material has a lower concentration in the doped optical device film 101 than in the optical device material. When the second power level is applied, the second power level remains constant throughout operation 903. In one embodiment, which may be combined with other embodiments described herein, the first and second power levels may be different. The optical device material provided by the first gas source 402 and the dopant precursor provided by the second gas source 403 have predetermined concentrations, and the concentration of the combination of optical device material and dopant material corresponds to the concentration of the doped optical device film 101. In one embodiment, which may be combined with other embodiments described herein, the optical device material precursor comprises an optical device material concentration of about 85% to about 100% atomic percentage, and the dopant precursor comprises a dopant material concentration of about 0% to about 15% atomic percentage. The CVD chamber 400 may include one or more second gas sources 403. For example, three to five second gas sources 403 may be included in the chamber 300. Each second gas source 403 is operable to deposit a different dopant precursor.
[0071] In one embodiment, which may be combined with other embodiments described herein, operations 902 and 903 are repeated by intervals of applying a first power level to the first flow controller 418a and intervals of applying a second power level to the second flow controller 418b. In another embodiment, flowing the dopant precursor at the second power level is performed by pulse-supplying the second power level at a set frequency while flowing the optical device material precursor. In yet another embodiment, which may be combined with other embodiments described herein, the optical device material precursor and the dopant precursor are flowed simultaneously by applying the first and second power levels simultaneously to form a doped optical device film 101.
[0072] In one embodiment, which may be combined with other embodiments described herein, a single performance of operations 902 and 903 forms all zones of a series of zones 115 of the doped optical device film 101. In another embodiment, a single performance of operations 902 and 903 forms a portion of the doped optical device film 101, which may correspond to one or more zones of the series of zones 115. Operations 902 and 903 are repeated until a predetermined thickness 110 of the doped optical device film 101 is achieved. In one embodiment, which may be combined with other embodiments described herein, operations 902 and 903 can be performed in a CVD chamber 400 having at least first and second gas sources 402, 403. In another embodiment, which may be combined with other embodiments described herein, operations 902 and 903 can be performed in a multi-processing chamber 504 of a cluster tool 502. For example, the optical device substrate 102 is transferred between at least two processing chambers 504. At least one of the processing chambers 504 is a CVD chamber 400 containing an optical device material target, and at least one of the processing chambers 504 is a CVD chamber 400 containing a second gas source 403.
[0073] In one embodiment, the doped optical device film 101 of methods 600-900 is maintained at a temperature within a range that allows the doped optical device film 101 to remain amorphous. In embodiments that may be combined with other embodiments described herein, the doped optical device film 101 is maintained in this temperature range through methods 600-900. In one embodiment, the optical device substrate 102 is maintained at a temperature higher than approximately 30°C, such as between approximately 30°C and 300°C. In one embodiment, the temperature is maintained by cooling the substrate supports 310, 410 and the optical device substrate 102 using cooling conduits 318, 414. For example, a cooling fluid flows through a cooling conduit 318 located within the substrate support 310. In one embodiment, the temperature is maintained by heating the substrate supports 310, 410 and the optical device substrate 102 using a heater 322 or a heating conduit 414.
[0074] In methods 600-900, the optical device material is exposed to a processing temperature of approximately 30°C or higher. The dopant material incorporated into the optical device layer enables the doped optical device film 101 to form amorphously at temperatures higher than approximately 30°C, for example, at approximately 100°C and approximately 300°C. The optical device material having the dopant material forms amorphously when the dopant material is incorporated into the optical device layer, where the dopant material alters the composition of the optical device material and interrupts the formation of crystalline structures in the optical device layer that would otherwise form above a certain temperature specific to the optical device material. For example, titanium dioxide (TiO2) may form polycrystalline titanium dioxide (TiO2) at temperatures between 30°C and 200°C or in between, and prominent crystals may form at temperatures above 200°C.
[0075] In summary, improved methods and materials for forming a doped optical device film 101 having optical properties including uniform high refractive index and low absorption loss are described herein. To achieve the desired optical properties, the dopant material is distributed in the optical device layer at a specific dopant concentration, and the doped optical device film is maintained within a temperature process window in which the doped optical device film can form amorphously (i.e., without forming a crystalline structure). The dopant concentration of the dopant material expands the temperature process window of the doped optical device film. The dopant material modifies the composition of the optical device layer so that crystal formation is interrupted at a given temperature. For example, if the optical device layer has a dopant material uniformly distributed throughout, crystal formation is interrupted at temperatures between approximately 30°C and 300°C. A concentration of 0-50% of dopant atoms in the dopant material affects the morphology of the doped optical device film without a significant and harmful increase in the refractive index of the optical device layer.
[0076] While the above description applies to embodiments of the Disclosure, other and further embodiments of the Disclosure may be devised without departing from the basic scope of the Disclosure, and the scope of the Disclosure is determined by the following claims.
Claims
1. The method involves arranging an optical device substrate in a chamber, wherein the chamber includes one or more targets, each having a pre-doped optical device material, and the pre-doped optical device material is Optical device material of a first concentration, and Second concentration dopant material Including the placement of an optical device substrate, A method of depositing a doped amorphous optical device film on an optical device substrate, wherein the optical device substrate is maintained at a temperature exceeding 30°C during the deposition of the doped amorphous optical device film, and the doped amorphous optical device film has a series of zones extending vertically from the surface of the optical device substrate to the upper surface of the doped amorphous optical device film, Etching the doped amorphous optical device film to form an optical device having a plurality of doped optical device structures, wherein each doped optical device structure has the dopant material distributed in each of the series of zones to form an optical device. A method for forming a film, including the following.
2. The optical device material is Tantalum pentoxide (Ta 2 O 5 ), zirconium dioxide (ZrO 2 ), indium oxide (In 2 O 3 ), or hafnium oxide (HfO 2 ) including metal-containing materials, and Semiconductor materials including silicon (Si), germanium (Ge), silicon germanium (SiGe), Group III-V semiconductors, Group II-IV semiconductors, ternary semiconductors, quaternary semiconductors, and transparent conductive oxides. A method for forming the film according to claim 1, comprising one or both of the above.
3. The method involves arranging an optical device substrate in a chamber, wherein the chamber includes one or more targets, each having a pre-doped optical device material, and the pre-doped optical device material is Optical device material of a first concentration, and Second concentration dopant material, Including the placement of an optical device substrate, A method of depositing a doped amorphous optical device film on the optical device substrate, wherein the optical device substrate is maintained at a temperature exceeding 30°C during the deposition of the doped amorphous optical device film, Includes, A method for forming a film wherein the dopant material comprises silicon (Si), niobium (Nb), titanium (Ti), tantalum (Ta), zirconium (Zr), indium (In), hafnium (Hf), or oxides thereof, and the dopant material and the optical device material are different from each other.
4. The amorphous optical device film has a first refractive index, and A method for forming a film according to claim 1, wherein the dopant material has a second refractive index and the first refractive index is greater than the second refractive index.
5. A method for forming a film according to claim 1, further comprising oxidizing the surface of the optical device substrate.
6. A method for forming the film according to claim 3, wherein the amorphous optical device film contains the dopant material with a dopant concentration of 15% or less in atomic percentage.
7. A method for forming a film according to claim 1, wherein depositing the doped amorphous optical device film on the optical device substrate includes applying power to one or more targets.
8. A method for forming a film according to claim 1, wherein depositing the doped amorphous optical device film on the optical device substrate comprises applying power to a magnetron associated with one or more targets.
9. Placing the optical device substrate inside the chamber, The optical device material precursor is flowed into the chamber at a first flow rate to deposit an optical device layer on the surface of the optical device substrate, The dopant precursor is flowed into the chamber at a second flow rate to form a doped amorphous optical device film on the optical device substrate. A method for forming a film, comprising the following: the optical device substrate is maintained at a temperature above 30°C while the optical device layer is being deposited and while the dopant precursor is being flowed.
10. A method for forming a film according to claim 9, wherein flowing the optical device material precursor into the chamber includes introducing an oxygen-containing precursor into the chamber.
11. The method for forming a film according to claim 10, wherein the optical device material precursor is a titanium precursor.
12. The dopant precursor is silane (SiH 4 A method for forming the film described in claim 9, wherein the film is formed as described in claim 9.
13. A method for forming a film according to claim 9, wherein the dopant precursor is deposited on the doped amorphous optical device film at a concentration of 15% or less of atomic percentage.
Citation Information
Patent Citations
Optical article with coating film and its production
JP1997211201A
Manufacture method for optical thin film
JP2002194529A
Titanium oxide transparent coating containing at least one of aluminum and aluminum oxide and having a rutile structure
JP2006518809A
Thermal protection glazing and method for manufacturing the same
JP2013543476A
Method of producing mask blank and method of producing phase shift mask
JP2014197190A