Fatigue evaluation of fiber samples
The method addresses the inefficiency of fiber fatigue analysis by determining load energy and fatigue indices to predict fiber fracture, enhancing testing speed and accuracy in hair care product evaluation.
Patent Information
- Application Number
- JP2024501656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-16
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Statistically significant fatigue analysis of fiber samples, particularly human hair, is extremely time-consuming, making it impractical for screening active compositions in hair care products, and altering experimental parameters to accelerate fiber fracture can deviate from real-world conditions.
A method for evaluating fiber fatigue by determining load energy and an index of fatigue based on load energy changes over multiple cycles, allowing for predictive assessment of fiber fracture without waiting for actual breakage, using load energy integration and derivative analysis to identify fatigue indicators.
Enables efficient and practical formulation screening by significantly reducing the number of cycles required for fatigue testing, providing a predictive indicator of fiber failure and accounting for initial sample state, thus improving testing efficiency and accuracy.
Smart Images

Figure 0007955331000001 
Figure 0007955331000002 
Figure 0007955331000003
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for evaluating fatigue of a fiber sample, and related computer program codes and apparatuses. In particular, the method may relate to evaluating fatigue of a human hair sample. Background Art
[0002] Mechanical testing, particularly tensile testing and fatigue analysis, is used in various industries to analyze product and material properties, enabling engineers to improve designs and chemical formulations.
[0003] In the field of fast-moving consumer goods, in the development of hair care products, it is necessary to test the effect of a product on the properties of hair fibers so that the effect of the product as a chemical treatment agent can be evaluated and compared with the effect of existing formulations. Typically, such analysis can be performed by comparing the mechanical properties of fibers with and without product treatment. A common mechanical parameter used in these comparisons is Young's modulus. This can be measured using a simple tensile test (measurement of force versus strain, or stress versus strain). In some examples, the tensile test is repeated for approximately 50 fibers per type (treated vs. untreated). This type of test is sometimes referred to as a "classical tensile test". The entire experiment is relatively quick, and by using it for formulation screening, their effectiveness in influencing the physical properties of fiber samples in a desired manner can be determined.
[0004] However, fiber fatigue experiments are more relevant to the performance of some materials, including human hair, under real-world conditions than stress / strain measurements. In some cases, fatigue measurements can be performed by periodically repeating the straining and recovery of a sample. In hair care product testing, such analysis better represents the mechanical damage that hair fibers undergo during grooming than classical tensile tests. Typically, this periodic process may be repeated until the fiber breaks. This type of test is sometimes called a "single fiber fatigue test." The average number of "cycles to break" can be recorded for a large number of fibers (e.g., 30 or 50 fibers, or more). Furthermore, the literature reports that fatigue measurements can be far more sensitive to differences in hair type than conventional measurements.
[0005] However, statistically significant fatigue analysis is extremely time-consuming, making it currently impractical to screen active compositions using fatigue measurements. A limiting factor is the need to repeat measurements for each of multiple fibers until the fiber breaks (thousands of cycles). For example, a study requiring 30 fibers could take several weeks for the entire experiment.
[0006] It may be possible to accelerate fiber fracture by changing experimental parameters. This may include changing the amount of stress, force, or strain used in the experiment. Similarly, the humidity or other environmental parameters in which the experiment is conducted can be adjusted to affect the number of cycles required to fracture the fibers. However, significantly altering these physical parameters may cause the test to deviate substantially from real-world, consumer-relevant conditions, and thus reduce the probative value of the evaluation.
[0007] Some aspects of this disclosure relate to methods for accelerating hair fiber fatigue measurement within desired consumer-related conditions so that formulation screening becomes practical.
[0008] Another aspect of this disclosure relates to identifying the initial physical properties of a fiber sample under test. [Overview of the Initiative]
[0009] According to one embodiment of the present disclosure, a method for evaluating the fatigue of one or more fiber samples, We will receive fatigue test data of fiber samples for multiple load cycles, For at least one subset of cycles, determine the load energy based on data from fatigue tests, Determining an index of fatigue based on the load energy of at least one subset of the cycle, A method including this is provided.
[0010] The fatigue test may be a single-fiber fatigue test.
[0011] In one or more embodiments, determining an index of fatigue level includes determining the rate of change of load energy with respect to the number of cycles.
[0012] In one or more embodiments, the rate of change of load energy is based on the smoothed value of the load energy over multiple cycles.
[0013] In one or more embodiments, the fatigue level index is determined based on the initial load cycle.
[0014] In one or more embodiments, the fatigue test data includes fewer than one of 10,000, 20,000, or 50,000 cycles.
[0015] In one or more embodiments, the method further includes determining an index of the initial state of a fiber sample based on the number of maximum load energies relative to the number of cycles.
[0016] In one or more embodiments, fatigue test data include force or stress data with respect to displacement or strain. Furthermore, instead of using force or tensile displacement, fatigue test data may include bending or torsional force or stress as a function of displacement or strain.
[0017] In one or more embodiments, the load energy for one cycle is determined by integrating the force or stress with respect to the displacement or / strain of the load portion for that cycle.
[0018] In one or more embodiments, the load energy for a cycle is determined by integrating the force or stress against the displacement or strain within the load / unloading hysteresis of that cycle. The method may be a computer-implemented method.
[0019] In one or more embodiments, determining a fatigue index based on the load energy of a cycle includes determining it by integrating the force or stress with respect to the displacement or strain of the load portion during that cycle.
[0020] In one or more embodiments, determining an indicator of fatigue further includes integrating the forces or stresses with respect to the displacement or strain of the unloaded portion of the cycle to identify the energy lost within that cycle.
[0021] In one or more embodiments, the method further includes stopping the automated testing schedule of a sample in response to determining that a fatigue index meets a predetermined value.
[0022] In one or more embodiments, one or more fiber samples include human or animal hair fibers.
[0023] In one or more embodiments, the method further includes performing a fatigue test of multiple load cycles, which may be performed as an automated test schedule.
[0024] According to further embodiments of this disclosure, a method, receiving fatigue test data for a fiber sample for a plurality of load cycles; determining, based on data from the fatigue test for at least a subset of the cycles, a load energy; determining, based on a characteristic of the load energy as a function of cycle number, an indicator of an initial state of the fiber; and is provided.
[0025] According to another aspect, the present disclosure provides a computer program product comprising a computer program distributable by electronic data transmission and comprising computer program code means adapted to cause a computer to perform any of the method procedures described herein when the program is loaded onto the computer, or a computer-readable medium having computer program code means adapted to cause a computer to perform any one of the method procedures described herein when the program is loaded onto the computer.
[0026] According to further embodiments of the present disclosure, there is provided a fatigue testing apparatus comprising a controller configured, in use, to perform one or more of the methods described herein.
[0027] One or more embodiments will now be described, by way of example only, with reference to the accompanying drawings in which: BRIEF DESCRIPTION OF THE DRAWINGS
[0028] [Figure 1] is a diagram illustrating a method of assessing fatigue in a fiber sample; [Figure 2] is a plot of a force-strain hysteresis curve for a fiber load cycle; [Figure 3] is a plot of measured load energy as a function of cycle number; and [Figure 4]This is a plot of the measured load energy as a function of the number of cycles for a sample that has significantly more partial fracture points than the one in Figure 3. [Figure 5] This figure shows the results of the "cycle to fracture" experiment, comparing untreated hair samples with heat-treated hair samples. [Figure 6A] The figures 1 to 4 show the results of applying the aforementioned analytical method, comparing untreated hair samples with heat-treated hair samples. [Figure 6B] The figures 1 to 4 show the results of applying the aforementioned analytical method, comparing untreated hair samples with heat-treated hair samples. [Figure 6C] The figures 1 to 4 show the results of applying the aforementioned analytical method, comparing untreated hair samples with heat-treated hair samples. [Figure 7] This is a schematic block diagram of a system for performing a method to evaluate the fatigue of fiber samples. [Figure 8] This figure shows a computer-readable medium containing computer program code. [Modes for carrying out the invention]
[0029] This disclosure relates to an improved method for determining fatigue of a fiber sample. In some cases, the fiber sample may include human or animal hair fibers to enable efficient comparative testing of damaging treatments such as heat treatment or chemical treatments such as various shampoos or other consumer product formulations. Alternatively, the fiber sample may include synthetic or natural fibers.
[0030] Figure 1 outlines an exemplary method 100 for evaluating the fatigue of a fiber sample. The method includes receiving fatigue test data of the fiber sample for multiple load cycles 102. The fatigue test data may include force or stress data against displacement or strain. In some examples, the method may include performing fatigue tests and obtaining fatigue test data, and it will be understood that in practice, multiple different samples may be tested under various conditions, allowing for a comparison of the performance of one or more products.
[0031] For at least one subset of cycles, the load energy is determined based on data from fatigue tests (104).
[0032] Next, an index of fatigue is determined based on the load energy of at least one subgroup of the cycle (106).
[0033] The claimed method 100 provides a method for predicting fiber fracture during an experiment without having to wait for the actual fracture event to occur. This improves the efficiency of evaluating the effectiveness of various treatment formulations and allows for the screening of more formulations within a given period. In particular, it has been found that using load energy provides a predictor that allows for a useful comparison of fatigue performance between fiber samples without having to test the fiber samples until they break. Therefore, the fatigue test data described herein do not necessarily include fiber sample breakage tests.
[0034] Various aspects of this method, including the determination of fatigue indicators, are described in further detail below with reference to Figures 2 to 4. In particular, the first fatigue indicator is explained with reference to Figure 3, and the second fatigue indicator is explained with reference to Figure 4.
[0035] As can be seen from the following description, various aspects of this method make it possible to study the changes in specific parameters that vary with the number of fatigue cycles applied. In some examples, the results for each set of samples can be correlated with conventional evaluation indices for fatigue measurement based on the number of cycles to fracture.
[0036] Figure 2 shows an exemplary force-strain hysteresis curve for a single loading cycle, specifically for loading cycle 200. The X-axis represents the strain 210 generated in the fiber sample, and the Y-axis represents the force 208 applied to the sample. Alternatively, the Y-axis could represent stress and the X-axis could represent strain, yielding similar results. The force applied to the fiber sample induces stress in the material under test. The data captured for the selected cycle includes the entire loading portion 202 of cycle 200 (upper curve) and the entire unloading portion 204 of cycle 200 (lower curve) of the sample. The experiment was performed by stretching to a predetermined stress. The loading portion of the cycle ends when this stress is reached. In other embodiments of the experiment, a constant force or a constant strain can be used.
[0037] The region below the force / strain loading portion 202 in cycle 200 serves as a measure of the load energy. The load energy for a given cycle can be determined by integrating the force / stress against the displacement / strain of the loading portion 202 in that cycle. The load energy changes with the number of loading cycles applied to the fiber sample. Using the load energy parameter, the number of cycles required for the fiber sample to break can be determined. Therefore, by monitoring the load energy, a predictable assessment of the fatigue of the fiber sample can be obtained. For example, this analysis does not necessarily allow for predictions for each individual fiber that will break, but it allows for comparison of the fatigue performance between fiber samples based on the identified values. Fiber samples with a large rate of change in load energy with respect to the number of cycles show a higher degree of fatigue than fiber samples with a small rate of change.
[0038] Fatigue test data can be acquired using existing commercially available equipment and standard data acquisition parameters and techniques. Fatigue data may also be acquired using a Dia-Stron CYC801. In conventional experiments, only the number of cycles to fracture is recorded. In contrast, the method of this disclosure identifies the load energy based on data from the fatigue test for at least one subset of cycles. In the illustrated data, force / strain curves are recorded between selected cycles of the fatigue experiment (every 200 cycles in this example).
[0039] The region 206 between the loading section 202 and the unloading section 204 represents the amount of energy lost during the loading cycle 200. The energy loss represented by region 206 corresponds to the difference between the region below the loading curve 202 (load energy) and the region below the unloading curve 204 (unload energy).
[0040] Additional parameters derived from the load energy may be used to determine an index of fatigue. The region below the load portion 202 of cycle 200, or the region below the unload portion 204 of cycle 200, or the region 206 in the hysteresis curve can be used to identify the energy lost through the fiber sample during that cycle. The energy lost in a cycle can be used as a parameter that provides a predictive index of fiber breakage. More specifically, the changes in the shape of the load portion 202 of cycle 200, the unload portion 202 of cycle 200, and the region 206 in the hysteresis curve, measured for each selected cycle, can be used to determine an index of the likelihood of fiber breakage or fatigue.
[0041] A first aspect of the method for determining the indicator of fatigue is described below with reference to Figure 3.
[0042] Figure 3 shows a time-series graph 300 containing selected data samples 302 of physical specimens (i.e., fiber specimens). Graph 300 shows the load region 304 for each selected sample 302 for a number of cycles 306. Each point in Figure 3 represents the load energy for the selected cycle, which can be determined for each point using the measurements described above, for example, with reference to Figure 2. Alternatively, each point may correspond to a parameter derived from the load energy, such as the energy lost during the cycle (load energy minus unload energy).
[0043] Fatigue is known to be demonstrated by the change in the load curve with respect to the number of load cycles. When used herein, the term load cycle will be understood in its conventional sense, namely, the cycles in which a load is applied and removed. Therefore, the changes in the region below the load curve can be used as a predictive parameter for failure and as an indicator of fatigue. By using the data trends in Figure 3, it is possible to provide an indication / prediction of fiber fracture before the fiber is completely destroyed. For example, as shown in Figure 3, the load energy (indicated by the load region 304) initially decreases as the number of cycles 306 increases. In particular, the load energy decreases logarithmically with respect to the number of cycles 306.
[0044] As the number of cycles increases (306), the fibers weaken, and therefore the amount of energy lost during each cycle (i.e., the load region 304 below the load curve) also decreases. This is thought to be because the fiber sample becomes more easily deformed by the applied force.
[0045] An indicator of fatigue level includes determining the rate of change of load energy with respect to the number of cycles. In particular, the initial gradient of load energy with respect to the number of cycles has been shown to provide a useful indicator of fatigue. An indicator of fatigue level may also be determined based on the initial load cycle. This can be determined by comparing the energy lost to the initial state of the fiber sample, for example, when the load area has decreased by a threshold level such as 10% or 20%. Alternatively, the initial load cycle can include a fixed number of cycles, for example, 5,000, 10,000, 20,000, or 50,000 cycles. As a further alternative, the number of load cycles that constitute the initial load cycle may be based on determining the point at which the rate of change of the initial gradient of load energy with respect to the number of cycles reaches a threshold.
[0046] The rate of change of load energy may be based on the smoothed value of the load energy 304 over multiple cycles 306. Applying a conventional smoothing function is useful for removing inter-sample variability and improving the fit between the rate of change calculated based on the smoothing function and the overall trend. That is, the first derivative of the smoothed data gives the effective rate of decrease of the load region with respect to the number of cycles.
[0047] As shown in Figure 3, the data also includes unexpected protrusions 308 in the curve. These protrusions are understood to correspond to partial fiber break events.
[0048] To enable the prediction of fiber failure using the collected data, it is preferable to consider the temporal changes in the region below the load curve without interference from partial failure events. Data samples with outliers or those affected by partial fracture events can be excluded using conventional techniques, such as determining when the load region of a sample is greater than the load region of a preceding sample (or group of data samples) by a threshold level. Alternatively, outliers may be excluded by detecting the maximum value in the data and removing those data samples.
[0049] The analysis has also been shown that taking the mode of the first derivative of the data can reduce the impact of spikes associated with small / partial break events. Other mean values can also be used, but additional signal processing may be required to remove the effects of partial breaks.
[0050] Thus, the first derivative of the initial portion of the data shown in Figure 3 can be considered to provide an indicator of fatigue in the fiber sample being tested according to the first aspect of the method. This method was found to identify differences between fiber samples treated with different processes (e.g., untreated hair fibers and heat-treated hair fibers) after the 50th data sampling point (i.e., 50*200 cycles), which corresponds to the 10,000th cycle when data is captured every 200 cycles. Therefore, only a total of 20,000 cycles are required to compare the two types of treatments. In other words, in this example, only the first 10,000 cycles, which are the initial portion of the data, are considered for each of the two types of samples. This is about an order of magnitude less than the number of cycles required when using a method that tests until failure. Therefore, by using the above method, sample testing can be significantly improved, for example, by efficiently testing more processes to verify the results, or by testing the same process multiple times.
[0051] First-order derivatives have been shown to provide a substantially improved fatigue metric, including time series analysis (SARIMAX), log / linear fitting, and autocorrelation, which involve obtaining various integrals and derivatives of log / linear data, compared to several other candidate measurement metrics.
[0052] A specific example of the first aspect of this method is described below.
[0053] As explained with respect to Figure 1, in practice, this method may further include performing fatigue tests with multiple load cycles. In one specific example, the data processing required to predict fiber fracture includes the following steps:
[0054] For each fiber sample, 1. Data acquisition using commercially available fatigue testing machines such as the Dia-Stron CYC801 or other similar systems. 2. Data transfer to a suitable system such as a laptop computer. 3. Data processing using Python in Jupyter Notebook or any other data processing system. 3.1 Data visualization (optional; analysis can be performed in batch mode without visualization) and cleanup.
[0055] 3.2 Preparing data for each cycle: Determine the threshold value for force / strain data.
[0056] We determine the region below the load portion of the force / strain curve, which is called the "load region."
[0057] 3.3 Building a response: Load region vs. number of cycles 3.4 The response data is smoothed, and the damping constant is obtained using the local first derivative at each data point. This is done using the Savitsky-Golay filter (signal.savgol_filter Python package, version 1.6.3, The SciPy community, https: / / docs.scipy.org / doc / scipy / reference / signal.html).
[0058] 3.5 For the entire fiber data, calculate the mode of the attenuation constant (an example of mode calculation is described in more detail below with reference to Figure 6).
[0059] 3.6 For each set of data, For each fiber treatment, one set of data contains 40 values, and there are at least two types of fiber treatments. We compare data between pairs of fiber treatments using the Mann-Whitney U test (scipy.stats.mannwhitneyu Python package, version 1.6.3, The SciPy community, https: / / docs.scipy.org / doc / scipy / reference / generated / scipy.stats.mannwhitneyu.html).
[0060] The data analysis described above may include thousands of data points for thousands of cycles.
[0061] A second aspect of the method, which includes determining the initial state of a fiber sample, is described below with reference to Figure 4.
[0062] Figure 4 shows another exemplary time-series graph 400 of the load region 404 for cycle number 406, of the same type as described above with reference to Figure 3. In Figure 4, the data shows more unexpected protrusions 408 than in the sample test in Figure 3. As previously mentioned, these protrusions or outliers are understood to correspond to partial fiber fracture events.
[0063] Figure 4 also includes several erroneous data points 410 that are not physically important. These data points may be screened out of the analysis, for example, by thresholding.
[0064] In Graph 400, differences in the number of detected partial fracture events in fiber samples are understood to indicate that the fiber samples were in a different initial state or condition compared to other fiber samples. The initial state refers to the state of the fiber before the fatigue test. Therefore, the initial state includes the entire history of the fiber, including the effects of all grooming events and treatments prior to measurement. Aspects of the initial state may include, for example, fiber strength, integrity, physical damage (such as fiber splitting), and moisture content. The initial state can represent the degree of damage the fiber sample sustained before the fatigue test. Fibers that are closer to being intact initially can withstand partial fracture events longer before completely breaking. Therefore, a large number of unexpected protrusions 408 may represent fibers that were closer to being intact initially and were in a less damaged initial state than fibers that produce a small number of protrusions.
[0065] In other words, fibers exhibiting more protrusions 408 during data acquisition can be considered to be in a better initial state than fibers with fewer protrusions. Therefore, fibers in a better initial state can withstand smaller / partial fracture events during the experiment before overall fracture or before weakening to the point where the load energy reaches a threshold level.
[0066] Observing the number of partial fracture events in the fibers provides an indicator of the initial state of the fibers that is unavailable in conventional tests. In other words, conventional tests cannot take into account the initial state of the fiber sample, which can lead to overly broad measurements of fiber fatigue.
[0067] Therefore, by counting the number of partial fracture events (either until complete failure or up to a predetermined number of cycles, such as 100,000), a measure of existing fiber damage can be obtained that defines the initial state of the fiber sample.
[0068] Thus, the number of partial fracture events detected in the data of Figure 3 or Figure 4 can be considered to provide an indicator of the initial state of the fiber sample being tested according to the second aspect of the method.
[0069] Figures 5 and 6 compare data obtained using the conventional fatigue measurement experiment and the new method shown in Figure 1. The samples used in the experiment were collected from the following types of hair.
[0070] a) One lock of untreated, medium brown mixed hair from a Caucasian person, and b) One lock of Caucasian medium brown mixed hair, heat-treated (30 times at 450°F using a hair styling iron).
[0071] Untreated hair was supplied by International Hair Importers. Samples were taken from the tip of the fibers for both types of hair. Therefore, there are two types of samples.
[0072] Fatigue tests were conducted using a cycle testing machine (Dia-Stron CYC801) set to "constant stress mode" at a relative humidity of 80% (80%RH). The fatigue rate was set to 60 mm / s, and the number of cycles until fracture was measured at a target stress of 105 MPa and a relative humidity of 80%. In these experiments, both force and stress were recorded (stress = force / cross-sectional area). However, since the effective cross-sectional area of the fiber changes during the fatigue process (the effective cross-sectional area of the fiber decreases as a function of crack propagation), the analysis is performed with respect to the force / strain curve. This also eliminates the need to correct the data using the total fiber cross-sectional dimensions. This is justified in this application because we are studying the changes in parameters between cycles for the same fiber. To calculate the stress, the fiber dimensions were measured at 60%RH (at five points along the fiber).
[0073] Each experiment used approximately 40 fibers. Due to equipment limitations, some cells in the experiment had reduced datasets. Also, because there was a limit to the amount of data that could be saved during a single experiment, some fibers (those requiring a very large number of cycles to break) had to be rerun, resulting in more than two data files per fiber.
[0074] Figure 5 shows the results of a "cycle to breakage" experiment comparing untreated hair samples with heat-treated hair samples. In both cases, hair was collected from the tip of a hairpiece.
[0075] Figure 6 shows the results of applying the analysis method described above, with reference to Figures 1 to 4, to A) the entire dataset (all data from the cycle up to the break), B) the first 100 data points, and C) the first 50 data points.
[0076] As can be seen from the comparison between Figure 5 and Figure 6, similar qualitative changes in hair fatigue performance are observed under both heat-treated and non-heat-treated conditions, using both classical and new analytical methods.
[0077] The results in Figures 6A to 6C also demonstrate that good differentiation between samples can be achieved for all three datasets. Therefore, for example, good results can be obtained using only the first 50 data points. This means that the amount of data required to obtain the experimental results shown in Figure 6C is reduced to one-seventh of that required for conventional fatigue measurements, as explained with reference to Figure 5.
[0078] The data processing steps for creating Figure 6 are described below. As mentioned earlier, the first derivative is calculated for each time point. The obtained data is formed into a histogram of the count versus the first derivative value. In this example, 100 bins are used for the first derivative value, but this can be changed. The bin with the highest count is determined, and the midpoint of that bin is assigned to the damping constant. This process is performed for each fiber in the set, providing a distribution of the mode of the damping constant for each fiber set. The histogram is obtained using the Python package matplotlib.pyplot.hist (see https: / / matplotlib.org / stable / api / _as_gen / matplotlib.pyplot.hist.html). The maximum value of the histogram is obtained using the Python package numpy.argmax (see https: / / numpy.org / doc / stable / reference / generated / numpy.argmax.html).
[0079] Figure 7 shows a schematic block diagram of a system 700 that may be used to carry out the method described above. The system 700 comprises one or more processors 702 that communicate with memory 704, which is an example of a computer-readable storage medium. One or more processors 702 also communicate with one or more input devices 706 and one or more output devices 708. Various components of the system 700 may be implemented using common computing means known in the art. For example, the input device 706 may include a keyboard or mouse, and the output device 708 may include a monitor or display and an audio output device such as a speaker. Furthermore, the system 700 comprises a fatigue testing apparatus that may be conventional, and the fatigue testing apparatus 710 is at least partially controlled by one or more processors 702.
[0080] Figure 8 discloses a non-temporary computer-readable storage medium 800. The non-temporary computer-readable storage medium includes computer program code configured to cause a processor to perform the methods disclosed herein.
[0081] By performing calculations using a computer, calculations can be performed more quickly than the corresponding cycle experiments leading to fracture, thereby allowing for faster testing of fiber samples. This also opens up the possibility of immediate processing, i.e., processing immediately after obtaining data from each fatigue cycle. This enables quality control during the experiment. Furthermore, it allows for the possibility of automatically stopping the experiment when data indicates that a predetermined quality and conformance level has been reached. This technique can lead to further time savings. For example, the method may further include stopping the automated test schedule for a particular sample in response to determining that the fatigue index meets a predetermined value. In some examples, stopping the test schedule includes preventing any additional load cycles from being applied to the fiber sample.
Claims
1. A method for evaluating the fatigue of hair fiber samples, A system comprising memory and a processor receives fatigue test data relating to a fatigue test of the hair fiber sample for a plurality of load cycles in which a load is applied to and removed from the hair fiber sample, wherein the fatigue test data includes force or stress data for displacement or strain. The system identifies the load energy for at least one subgroup including a portion of the plurality of load cycles, based on data from the fatigue test data. The system determines an index of fatigue of the fiber sample based on the load energy of the at least one subgroup, A method that includes this.
2. The method according to claim 1, wherein determining an index of fatigue level includes determining the rate of change of the load energy with respect to the number of cycles.
3. The method according to claim 2, wherein the rate of change of the load energy is based on the smoothed value of the load energy for the plurality of cycles.
4. The method according to claim 2, wherein the fatigue index is determined based on an initial load cycle, and the initial load cycle includes fewer than one of 10,000 cycles, 20,000 cycles, or 50,000 cycles.
5. The method according to claim 2, wherein the fatigue index is determined based on the initial load cycle, and the number of load cycles that constitute the initial load cycle is determined when the rate of change of the initial gradient of the load energy with respect to the number of cycles reaches a threshold.
6. The method according to claim 1, further comprising determining an index of the initial state, which means the state of the fiber sample before the fatigue test, based on the number of maximum load energies relative to the number of cycles.
7. The method according to claim 1, wherein the load energy of the cycle is determined by integrating the force / stress with respect to the displacement / strain of the load portion of the cycle.
8. The method according to claim 1, wherein determining the fatigue index based on the load energy of the cycle includes determining it by integrating the force or stress with respect to the displacement or strain of the load portion of the cycle.
9. The method according to claim 8, further comprising determining the fatigue index by integrating the force or stress with respect to the displacement or strain of the unloaded portion of the cycle to identify the energy lost within the cycle.
10. The method according to claim 1, comprising stopping the application of an additional load cycle to the fiber sample in response to the determination that the fatigue index meets a predetermined value.
11. The method according to claim 1, wherein the hair fiber sample comprises human or animal hair fibers.
12. The method according to claim 1, further comprising performing a fatigue test of the plurality of load cycles.
13. A computer-readable storage medium comprising computer program code configured to cause a processor to execute the method according to any one of claims 1 to 10 when in use.
14. A fatigue testing apparatus comprising a controller configured to perform the method described in claim 12 when in use.
Citation Information
Patent Citations
Method for evaluating flexibility of hair
JP2010276558A
Quantitative evaluation method and device of hair damage degree
JP2015224961A
Method of evaluating hair
JP2017040578A
Evaluation of applications using digital image correlation techniques