Improved castable magnesium alloy
A magnesium alloy with specific Gd:Nd ratio and composition achieves enhanced strength and mechanical properties in thicker castings, addressing the need for improved Mg-RE-Zr alloys in aerospace applications.
Patent Information
- Application Number
- JP2024502543
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-12
- Filing Date
- 2022-08-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-12
AI Technical Summary
There is a need for improved castable Mg-RE-Zr alloys with enhanced strength properties, particularly in aerospace applications, where existing alloys do not effectively achieve high strength-to-weight ratios in thicker castings using sand casting methods.
A magnesium alloy composition comprising 1.32-1.8 wt% Gd, 2-3.6 wt% Nd, 0.55-0.7 wt% Zr, 0.20-0.40 wt% Zn, and at least 85 wt% Mg, with a Gd:Nd ratio of 0.40-0.63, which when sand-cast and subjected to T6 aging treatment, achieves improved ultimate tensile strength (UTS) and maintains properties in thicker sections.
The alloy exhibits UTS of at least 310 MPa, with improved mechanical properties and finer grain size, achieving strength in thicker castings without requiring high solidification rate processes, suitable for aerospace components.
Smart Images

Figure 0007955334000005 
Figure 0007955334000006 
Figure 0007955334000007
Abstract
Description
Technical Field
[0001] The present invention relates to high-strength castable magnesium alloys, methods for producing such alloys, and articles containing the alloys.
Background Art
[0002] (Background Art)
[0003] Magnesium alloys containing rare earth metals and zirconium (Mg-RE-Zr alloys) are regularly used in aerospace and other specialized applications. In such applications, the strength-to-weight ratio is an important factor in material selection. Generally, a higher strength-to-weight ratio (i.e., higher strength for two materials of the same density) is desirable. Examples of applications where the strength-to-weight ratio is important include drivetrain components (gearboxes, housing covers, and similar items), engine components (cases, covers, moving component parts, etc.), and structural components (panels, body parts, etc.) in both conventional and electric aircraft. Similar material requirements apply to spacecraft and satellite applications, where the total weight of the spacecraft / satellite determines the cost of launching into space.
[0004] Even within the family of Mg-RE-Zr alloys, properties can vary significantly, and multiple subfamilies exist. By selecting specific rare earth elements and adding small amounts of other elements, certain aspects of alloy performance can be improved. There are many examples of alloys belonging to broader groups. The general benefits of various rare earth metals are covered in textbooks (e.g., "Light Alloys", 4th edition, Ian Polmear, p. 265, Fig. 5.17). It is generally recognized that rare earth metals increase strength up to the limit of solid solubility in the alloy, and further increases in content lead to reduced properties.
[0005] Examples of such alloys are disclosed in the applicant's earlier U.S. Patent No. 7,935,304, which describes alloys comprising 2–4.5 wt% neodymium, 0.2–7.0% at least one rare earth metal with atomic numbers 62–71, up to 1.3 wt% zinc, 0.2–0.7 wt% zirconium, and optionally one or more other trace components.
[0006] Alloys within this definition are defined as having the following composition in AMS4429B: [Table 1]
[0007] There is a need for improved castable Mg-RE-Zr alloys, particularly those with improved strength properties. [Overview of the project]
[0008] (Summary of the invention)
[0009] The present invention (a) 1.32-1.8 wt% of Gd, (b) 2-3.6 wt% Nd, (c) 0.55~0.7 wt% Zr and (d) 0.20~0.40 wt% Zn and (d) At least 85 wt% Mg, Includes, The Gd:Nd ratio (wt%) is 0.40-0.63 for magnesium alloys.
[0010] Surprisingly, the inventors have found that magnesium alloys having the above composition and a Gd:Nd(wt%) ratio of 0.40 to 0.63 exhibit improved strength, particularly improved ultimate tensile strength (UTS). In some embodiments, the alloy may be a cast magnesium alloy, more specifically a sand-cast alloy. In particular, the cast magnesium alloy may have a thickness of 5 to 350 mm. In some embodiments, the cast magnesium alloy may have a thickness of 25 to 350 mm, more specifically 100 to 350 mm, and even more specifically 200 to 350 mm. In other embodiments, the cast magnesium alloy may have a thickness of 5 to 100 mm, more specifically 10 to 100 mm. In the context of this invention, the term "thickness" is used to mean the minimum dimension of the cast magnesium alloy. Surprisingly, the inventors have found that the alloys of this invention exhibit improved retention of their properties in thicker castings. In some embodiments, the alloy may be a forged magnesium alloy. The forged alloy may be a forged alloy or an extruded alloy.
[0011] In particular, the ultimate tensile strength (UTS) of magnesium alloys can be at least 310 MPa when sand-cast in a 200 mm × 200 mm × 25.4 mm plate and subjected to T6 aging treatment, as measured according to ASTM B557M-15. More specifically, the UTS can be at least 315 MPa, even more specifically at least 316 MPa, and even more specifically at least 320 MPa. In particular, the UTS can be 350 MPa or less.
[0012] In relation to the present invention, the term “aging treatment” is used to refer to a process in which a magnesium alloy is heated to a temperature higher than room temperature, held at that temperature for a certain period of time, and then returned to room temperature (i.e., about 25°C). In particular, the aging treatment may be a T6 aging treatment. Such a process is known in the art and generally involves heating a magnesium alloy to a temperature of 515°C to 524°C, holding it at that temperature for a certain period of time (for solution treatment), quenching it as necessary (i.e., allowing it to cool to a temperature lower than the heated temperature, for example, room temperature (about 25°C)), and then reheating the magnesium alloy to a temperature of 200°C to 204°C and holding it at that temperature for a certain period of time (for precipitation heat treatment).
[0013] In connection with the present invention, the term "alloy" is used to mean a composition made by mixing and fusing two or more metallic elements by melting, mixing, and resolidifying them together. Therefore, in the context of alloys in the present invention, all elements mentioned exist in metallic form (not, for example, as salts).
[0014] In particular, the Gd:Nd ratio (wt%) can be between 0.40 and 0.61. More specifically, the Gd:Nd ratio (wt%) can be between 0.40 and 0.60. Even more specifically, the Gd:Nd ratio (wt%) can be between 0.40 and 0.57.
[0015] In particular, magnesium alloys may contain 1.35–1.8 wt% Gd, more specifically 1.40–1.75 wt% Gd, and even more specifically 1.40–1.70 wt% Gd.
[0016] More specifically, magnesium alloys may contain 2.2–3.4 wt% Nd, and even more specifically, 2.6–3.1 wt% Nd.
[0017] In particular, magnesium alloys may contain 0.6-0.7 wt% Zr, more specifically 0.60-0.70 wt% Zr.
[0018] More specifically, the magnesium alloy may contain at least 90 wt% Mg, and more specifically, at least 92 wt% Mg. In some embodiments, the remainder of the alloy may be magnesium and incidental impurities.
[0019] In particular, magnesium alloys may optionally contain (i) up to 0.4 wt% of rare earth metals other than Gd and Nd, (ii) up to 0.05 wt% of Ag, (iii) up to 0.01 wt% of Cu, (iv) up to 0.010 wt% of Fe, (v) up to 0.0020 wt% of Ni, and (vi) up to 0.01 wt% of other elements, with the remainder being magnesium. Examples of rare earth metals other than Gd and Nd include Ce, La, and Pr.
[0020] In connection with this invention, the term "rare earth metals" is used to refer to the 15 lanthanide elements, as well as Sc and Y.
[0021] In particular, when magnesium alloys are sand-cast into 200 mm × 200 mm × 25.4 mm plates and subjected to T6 aging treatment, they may have an average planar particle size of at least 10 μm, more specifically 10–100 μm, and even more specifically 20–80 μm. The average planar particle size was measured in a representative portion of the magnesium alloy using the Hein linear section method specified in ASTM E112-13. In this context, the term “representative section” is used to mean a section selected to represent the average state within the alloy. Typically, such sections should not be taken from areas affected by shearing, sintering, or other processes that alter the particle structure.
[0022] It is known in the art that particle size affects material properties. The Hall-Petch relationship shows that reducing particle size can increase UTS. There are other advantages to finer particle size. However, achieving particle sizes smaller than 10 μm (known as ultrafine) is generally difficult in large castings used industrially. Such large castings typically have complex shapes and average wall thicknesses exceeding 6 mm. Achieving ultrafine particle sizes in such materials requires employing processes such as material formation / processing or the use of high solidification rate processes (e.g., atomization, high-pressure die casting). However, these processes are not suitable for many industrial / aerospace components (i.e., the main applications of the alloys of the present invention) where sand casting is the preferred manufacturing method from a practical consideration. Therefore, for the alloys of the present invention, it is desirable to achieve the required properties (e.g., improved UTS) with materials having particle sizes greater than 20 μm and typically less than 100 μm. The grain size of many commercially available magnesium alloys, such as Mg-Al alloys, is highly dependent on the solidification rate, with grain size decreasing as the cooling rate increases (see, for example, LADBrzan'ski, M. Kro'l, T. Tan'ski, Effect of cooling rate and aluminum contents on the Mg-Al-Zn alloys' structure and mechanical properties, Journal of Achievements in Materials and Manufacturing Engineering 43 / 2(2010)613-633). The inventors have found that the alloy of the present invention can achieve improved (i.e., smaller) average grain size and mechanical properties when sand-cast (i.e., a method with a slow cooling rate) with a wall thickness of 25.4 mm (e.g., UTS).
[0023] More specifically, the magnesium alloy may include two or more crystalline phases, i.e., the magnesium alloy may be heterogeneous. In some embodiments, the alloy may include a first crystalline phase and a second crystalline phase. The first crystalline phase may differ from the second crystalline phase with respect to its crystal structure and / or its composition. In particular, the magnesium alloy may include at least 97%, more specifically at least 98%, particularly at least 98.5%, more particularly at least 99% of the first crystalline phase when sand-cast into a 200 mm × 200 mm × 25.4 mm plate and subjected to T6 aging treatment. In this context, percentages represent the area of two-dimensional scanning electron microscopy (SEM) microstructure images of the magnesium alloy.
[0024] Surprisingly, it has been found by the inventors that with the alloys of the present invention, having the relatively low Zn content specified herein, the content of the first phase is increased (and the content of the second phase is decreased). This improves the UTS of the alloy. This is contrary to the general knowledge in the art that a higher Zn content generally results in a higher UTS. Examples of this are given in the international standard ASTM B60-15, which describes ZK41A, ZK51A and ZK61A sand-casting alloys. These are Mg-Zn-Zr alloys that are nominally identical except for Zn levels of about 4.3, about 4.6 and about 6% (midpoints of the specification ranges), respectively. The minimum UTS specifications for these alloys are 200, 234 and 276 MPa, respectively, illustrating how increasing the Zn content increases the UTS value.
[0025] The present invention also relates to a component of an aircraft or spacecraft (e.g., a component of a conventional aircraft or an electric aircraft) comprising the above magnesium alloy. More specifically, the aircraft component may be an electric aircraft component. The term "aircraft" includes airplanes and helicopters. The term "spacecraft" also includes satellites. Including Gd in the alloy may provide a neutron absorption effect, which may be beneficial in environments with increased levels of neutrons (e.g., in space). In particular, the aircraft component may be a drivetrain component, an engine component, or a structural component. More specifically, the drivetrain component may be a gearbox, a housing, or a cover. In particular, the engine component may be a case, a cover, or a movable component. More specifically, the structural component may be a panel or a body part.
[0026] The present invention also (a) heating Mg, Gd, Nd, Zr and Zn to form a molten magnesium alloy comprising 1.32 to 1.8 wt% Gd, 2 to 3.6 wt% Nd, 0.55 to 0.7 wt% Zr, 0.20 to 0.40 wt% Zn and at least 85 wt% Mg, wherein the ratio (wt%) of Gd:Nd is 0.40 to 0.63; (b) mixing the resulting molten magnesium alloy; (c) casting the magnesium alloy; also relates to a method of manufacturing a magnesium alloy comprising
[0027] In particular, the method may be for manufacturing a magnesium alloy as defined above. Any other necessary ingredients in the resulting alloy (e.g., those listed in the preceding paragraph describing the alloy) may be added in the heating step (a). More specifically, the heating step may be performed at a temperature of at least 650°C (i.e., the melting point of pure magnesium), even more specifically less than 1090°C (the boiling point of pure magnesium). In particular, the temperature range may be 650°C to 850°C, more specifically 700°C to 800°C, even more specifically 750°C to 780°C. More specifically, in step (b), the resulting alloy may be completely melted and / or dissolved.
[0028] More specifically, in step (a), the resulting alloy can be completely melted. In particular, prior to melting in step (a), the alloy components may exist in elemental form or as one or more alloys.
[0029] In particular, step (c) may involve pouring molten magnesium alloy into a mold and then cooling and solidifying it. The mold may be a die mold, a permanent mold, a sand mold, an investment mold, a direct cooling (DC) mold, or other molds.
[0030] After step (c), the method may include one or more additional steps of (d) extrusion, (e) forging, (f) rolling, and (g) machining.
[0031] The present invention is further described with reference to the following drawings, which are not intended to limit the scope of the claimed invention. [Brief explanation of the drawing]
[0032] [Figure 1] This graph shows the ultimate tensile strength (UTS) of alloys from Examples 1 to 9 against the Gd:Nd ratio (wt%). [Figure 2] This graph shows the ultimate tensile strength (UTS) of alloys from Examples 10 to 16 against their Zn content (wt%). [Figure 3] This figure shows the microstructure of the alloy of Example 5 as measured by a scanning electron microscope (SEM). [Figure 4] Figure 3 shows an image after processing to distinguish between the first and second phases of the alloy. [Figure 5] This graph shows the ultimate tensile strength (UTS) as a percentage of the area of the second phase of the alloys in Examples 1 to 16. [Figure 6] This graph shows the area percentage of the second phase relative to the Gd:Nd ratio (wt%) of the alloys in Examples 1 to 16. [Examples]
[0033] (Examples)
[0034] Magnesium alloy compositions were prepared by combining the components in the amounts listed in Table 1 below. These compositions were then melted by heating to 750°C to 780°C. Next, the molten material was poured into a 200mm x 200mm x 25.4mm mold and subjected to T6 aging treatment. The ultimate tensile strength (UTS) of the alloy was then tested according to ASTM B557M-15.
[0035] [Table 2]
[0036] Figure 1 is a graph of UTS against the Gd:Nd ratio of the samples in Table 1. This clearly shows that the samples of the present invention, i.e., the samples having the Gd:Nd ratio (wt%) described in the claims, improved UTS.
[0037] Figure 3 is an SEM image of the optical microstructure of the magnesium alloy of Example 5 (i.e., cast in a 200 mm × 200 mm × 25.4 mm mold and subjected to T6 aging treatment). This shows that the alloy has a nearly equiaxed grain structure. This alloy is almost entirely single-phase, with only a few small regions of secondary phase present. An SEM image of the same alloy is shown in Figure 4. In Figure 4, a small amount of the second phase is shown as a white region.
[0038] Further magnesium alloy compositions were prepared by combining components in the amounts listed in Table 2 below. These compositions were prepared to demonstrate the effect of Zn content on the magnesium alloys of the present invention. The compositions were melted by heating to 750°C to 780°C. The molten material was then poured into a 200mm x 200mm x 25.4mm mold and subjected to T6 aging treatment. The ultimate tensile strength (UTS) of the alloy was then tested according to ASTM B557M-15.
[0039] [Table 3]
[0040] Figure 2 shows graphs of UTS against Zn content for Examples 10-16 in Table 2. This data shows that magnesium alloys with Zn content outside the claims exhibit reduced strength properties.
[0041] The percentage of the second phase was measured by generating two-dimensional optical SEM images of each alloy (i.e., cast in a 200mm x 200mm x 25.4mm mold and subjected to T6 heat treatment). The two phases have different atomic compositions and appear as contrast in the backscattered electron SEM image. By using image processing software, the initial SEM image can be converted to a grayscale image. The first phase is displayed as black, and the region of the second phase is displayed as white. Using the software, the area of the second phase (white) is measured as a percentage of the total area. This is the type of image shown in Figure 4. At least two images were taken for each alloy, and the average percentage was calculated. These results are shown in Table 3 below.
[0042] [Table 4]
[0043] Figure 5 shows the percentage values of the second phase in Table 3, compared to the UTS values of each alloy. The graph in Figure 5 shows a tendency for UTS to decrease as the amount of the second phase increases.
[0044] Further graphs are shown in Figure 6. These graphs plot the Gd:Nd ratio against the area percentage of the second phase for each example. For ease of reference, the data points are plotted as circles (Zn values less than 0.5, i.e., within the range of the alloy of the present invention) and squares (Zn values greater than 0.5, i.e., outside the range of the alloy of the present invention). For the circles (alloys with Zn content within the range of the alloy of the present invention), for alloys with a Gd:Nd ratio exceeding the value required for the alloy of the present invention, the percentage of the second phase is higher, and thus the UTS is lower. The data points in the squares (alloys with Zn content outside the range of the alloy of the present invention) show a higher percentage of the second phase and therefore a lower UTS for alloys that have a Gd:Nd ratio within the range required for the alloy of the present invention but with a Zn content exceeding the range required for the alloy of the present invention.
Claims
1. (a) 1.32 to 1.8 wt% of Gd, (b) 2-3.6 wt% Nd, (c) 0.55 to 0.7 wt% of Zr, (d) 0.20–0.40 wt% Zn, (e) at least 85 wt% Mg and Includes, The magnesium alloy has a Gd:Nd ratio (wt%) of 0.40 to 0.
63. The alloy is a magnesium alloy comprising (i) up to 0.4 wt% of rare earth metals other than Gd and Nd, (ii) up to 0.05 wt% of Ag, (iii) up to 0.01 wt% of Cu, (iv) up to 0.010 wt% of Fe, (v) up to 0.0020 wt% of Ni, and (vi) up to 0.01 wt% of other elements, with the remainder being magnesium.
2. The magnesium alloy according to claim 1, having an ultimate tensile strength of at least 310 MPa as measured according to ASTM B557M-15 when sand-cast into a 200 mm x 200 mm x 25.4 mm plate and subjected to T6 aging treatment.
3. The magnesium alloy according to claim 2, having an ultimate tensile strength of at least 315 MPa as measured according to ASTM B557M-15 when sand-cast into a 200 mm x 200 mm x 25.4 mm plate and subjected to T6 aging treatment.
4. The magnesium alloy according to claim 1, wherein the ratio of Gd:Nd (wt%) is 0.40 to 0.
61.
5. The magnesium alloy according to claim 4, wherein the ratio of Gd:Nd (wt%) is 0.40 to 0.
57.
6. The magnesium alloy according to claim 1, wherein the alloy contains 1.35 to 1.8 wt% of Gd.
7. The magnesium alloy according to claim 5, wherein the alloy contains 1.40 to 1.70 wt% of Gd.
8. The magnesium alloy according to claim 1, wherein the alloy contains 2.2 to 3.4 wt% Nd.
9. The magnesium alloy according to claim 8, wherein the alloy contains 2.6 to 3.1 wt% of Nd.
10. The magnesium alloy according to claim 1, wherein the alloy contains 0.6 to 0.7 wt% of Zr.
11. The magnesium alloy according to claim 1, wherein the alloy contains at least 90 wt% Mg.
12. The magnesium alloy according to claim 11, wherein the alloy contains at least 92 wt% Mg.
13. The magnesium alloy according to claim 1, wherein the alloy is sand-cast into a 200 mm × 200 mm × 25.4 mm plate and subjected to T6 aging treatment, and has an average planar particle size of 10 to 100 μm as measured according to ASTM E112-13.
14. The magnesium alloy according to claim 13, wherein the alloy is sand-cast into a 200 mm × 200 mm × 25.4 mm plate and subjected to T6 aging treatment, and has an average planar particle size of 20 to 80 μm as measured according to ASTM E112-13.
15. An aircraft component comprising the magnesium alloy according to any one of claims 1 to 14.
16. The aircraft component according to claim 15, wherein the aircraft component is a drive train component, an engine component, or a structural component.
17. The aircraft component according to claim 15, wherein the aircraft component is an electric aircraft component.
18. The aircraft component according to claim 16, wherein the aircraft component is an electric aircraft component.
19. (a) A step of heating Mg, Gd, Nd, Zr and Zn to form a molten magnesium alloy containing 1.32 to 1.8 wt% Gd, 2 to 3.6 wt% Nd, 0.55 to 0.7 wt% Zr, 0.20 to 0.40 wt% Zn and at least 85 wt% Mg, with a Gd:Nd ratio (wt%) of 0.40 to 0.63, (b) The step of mixing the obtained molten magnesium alloy, (c) A step of casting a magnesium alloy, A method for producing a magnesium alloy according to any one of claims 1 to 14, including the method described in any one of claims 1 to 14.
Citation Information
Patent Citations
High strength corrosion resistant rare earth cast magnesium alloy and preparation method thereof
CN101575683A
Heatproof magnesium alloy material with high strength and preparation method thereof
CN101603139A
Rare earth heat resistant magnesium alloy with high corrosion resistance
CN102304656A
castable magnesium alloy
JP2007508451A