Manufacturing method of the joint

By applying a copper particle paste, drying, and staged heating/pressuring, the method addresses bonding strength issues at the fillet portion, enhancing the semiconductor device's structural integrity.

JP7955342B2Active Publication Date: 2026-11-24MITSUI MINING & SMELTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024512524
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-28
Publication Date
2026-11-24
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing manufacturing methods for semiconductor devices result in insufficient bonding strength between the semiconductor element and the substrate at the fillet portion, leading to delamination issues.

Method used

A method involving the application of a paste containing copper particles exceeding 100 nm, followed by drying the coating film, and then applying heat and pressure in multiple stages to form a bonding layer, ensuring improved adhesion and sintering of the copper particles.

Benefits of technology

Enhances bonding strength between the workpiece and the bonding layer, particularly at the fillet portion, reducing delamination and improving the integrity of the joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955342000002
    Figure 0007955342000002
  • Figure 0007955342000003
    Figure 0007955342000003
  • Figure 0007955342000001
    Figure 0007955342000001
Patent Text Reader

Abstract

The present invention is a method for manufacturing a joined body, formed by joining a first body to be joined and a second body to be joined with a joining layer therebetween, the method comprising: a step in which a paste is applied to the first body to be joined to form a coating film, the paste including copper particles having a cumulative-volume particle diameter D50 exceeding 100 nm at a cumulative volume of 50% by capacity according to a laser diffraction scattering particle size distribution measurement method; a step in which the coating film is dried at a first temperature; a step in which the second body to be joined is placed on the dried coating film to form a layered body; a step in which the layered body is heated to a first temperature that is at least as high as the first temperature and a first pressure is applied between the first body to be joined and the second body to be joined of the layered body; and a step in which the layered body is heated to a third temperature that is at least as high as the second temperature, a second pressure that is at least as high as the first pressure is applied between the first body to be joined and the second body to be joined of the layered body, and the coating film is sintered to form a joining layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a method for manufacturing a jointed body. [Background technology]

[0002] In recent years, manufacturing methods for semiconductor devices such as IGBTs, which generate significant heat when large currents are passed through them, have adopted a process of joining semiconductor elements and circuit boards using a bonding material containing sinterable metal particles.

[0003] As an example of such technology, Patent Document 1 discloses a technique in which a bonding layer containing sinterable metal particles with a particle size of 100 nm or less is used, a laminate is prepared in which a substrate, a bonding layer and a semiconductor element are sequentially stacked, a first pressure is applied between the semiconductor element and the substrate of the laminate which is at a first temperature below the sintering temperature of the sinterable metal particles of the bonding layer, and then a second pressure exceeding the first pressure is applied between the semiconductor element and the substrate of the laminate which is at a second temperature above the sintering temperature of the sinterable metal particles of the bonding layer to sinter the bonding layer, thereby bonding the semiconductor element to the substrate via the bonding layer. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2018-110149 [Overview of the Initiative]

[0005] According to the technology described above, when a semiconductor element is placed on the bonding layer, the portion of the bonding layer at the edge of the bonding layer where the semiconductor element is not placed (hereinafter also referred to as the "fillet portion") when viewed from above is not sufficiently bonded to the substrate (the object to be bonded), and delamination occurs in this portion. Therefore, the object of the present invention is to provide a method for manufacturing a bonded body that has excellent bonding strength between the body to be joined and the bonding layer, particularly in the fillet portion.

[0006] As a result of diligent research to solve the above problems, the present inventors have found that by pre-drying the coating film placed on the first workpiece before placing the second workpiece on the coating film, and then applying heat and pressure to the coating film at a predetermined timing after placing the second workpiece, the adhesion between the first workpiece and the coating film is improved, and as a result, the bonding strength between the first workpiece and the bonding layer formed from the coating film at the fillet portion can be improved.

[0007] In other words, the present invention is a method for manufacturing a bonded body in which a first body to be bonded and a second body to be bonded are bonded via a bonding layer, wherein the cumulative volume particle size D at 50% of the cumulative volume, as measured by laser diffraction scattering particle size distribution analysis, is 50 The present invention provides a method for manufacturing a bonded body, comprising the steps of: applying a paste containing copper particles exceeding 100 nm to the first body to be bonded to form a coating film; drying the coating film at a first temperature; placing the second body to be bonded on the dried coating film to form a laminate; heating the laminate to a second temperature above the first temperature and applying a first pressure between the first body to be bonded and the second body to be bonded in the laminate; and heating the laminate to a third temperature above the second temperature and applying a second pressure above the first pressure between the first body to be bonded and the second body to be bonded in the laminate, thereby sintering the coating film and forming the bonded layer. [Brief explanation of the drawing]

[0008] [Figure 1] Figure 1 is a schematic diagram showing the first step in the manufacturing method of the joint according to the present invention. [Figure 2] Figure 2 is a schematic diagram showing the next step in the process shown in Figure 1. [Modes for carrying out the invention]

[0009] The present invention will be described below based on its preferred embodiments. Figures 1 and 2 are process diagrams illustrating the joining method of the jointed body according to the present invention. First, as shown in Figure 1, a paste containing copper particles is applied to the first workpiece 11 to form a coating film 12X. The method of applying the paste is not particularly limited, but examples include screen printing, gravure printing, dispensing, reverse coating, and doctor blade methods.

[0010] The paste used in this invention appropriately contains copper particles, an organic solvent described later, and a conditioning agent. The copper particles contained in the paste are not particularly limited in shape, and both spherical and non-spherical particles can be used. Here, a copper particle is said to be spherical if its circularity coefficient, measured by the following method, is 0.85 or greater. The circularity coefficient is calculated as follows: A scanning electron microscope image of a primary copper particle is taken, and when the area of ​​the two-dimensional projection image of the copper particle is S and the perimeter is L, the circularity coefficient of the copper particle is 4πS / L. 2 It is calculated from the formula.

[0011] On the other hand, copper particles are said to be non-spherical if their circularity coefficient is less than 0.85. Specific examples of non-spherical shapes include flattened, polyhedral shapes such as hexahedrons and octahedrons, spindle shapes, and irregular shapes. In the present invention, it is preferable that one of the two or more types of copper powder be flattened copper particles, and it is more preferable that it contains both flattened copper particles and spherical copper particles, as will be described later. In this invention, "flattened" refers to a shape having a pair of plate-like surfaces that form the main surface of the particle, and sides perpendicular to these plate-like surfaces, and the plate-like surfaces and sides can each be independently flat, curved, or uneven.

[0012] The particle size of copper particles when they are spherical shall be determined by the following method: Specifically, 50 or more primary copper particles with clearly defined outlines are selected using a scanning electron microscope at a magnification of 10,000x to 150,000x, and the Heywood diameter of each particle is measured. Then, the volume is calculated from the obtained Heywood diameters assuming the particles are perfectly spherical, and the cumulative particle size at 50% of the cumulative volume is determined as D SEM50 It shall be determined by [the relevant law].

[0013] The D of the copper particles SEM50 is preferably greater than 0.1 μm, more preferably 0.11 μm or more, and even more preferably 0.12 μm or more. On the other hand, D SEM50 is preferably 0.55 μm or less, more preferably 0.5 μm or less. D SEM50 By setting the value to exceed 0.1 μm, shrinkage cracking is less likely to occur when the coating film 12X formed by applying the paste is fired to form a bonding layer, and sufficient bonding strength can be achieved between the fillet portion of the bonding layer and the first adherend 11. On the other hand, D SEM50 is set to 0.55 μm or less, sufficient sintering of the copper particles present in the coating film 12X can be achieved.

[0014] When the copper particles are non-spherical, the particle size is defined as the volume cumulative particle diameter D at a cumulative volume of 50% by volume as measured by a laser diffraction / scattering particle size distribution measurement method 50 . For example, the measurement can be performed by the following method. Specifically, 0.1 g of the measurement sample and an aqueous dispersant solution are mixed and dispersed for 1 minute using an ultrasonic homogenizer (US-300T, manufactured by Nihon Seiki Seisakusho Co., Ltd.). Thereafter, the particle size distribution is measured using, for example, MT3300 EXII manufactured by MicrotracBEL as a laser diffraction / scattering particle size distribution measuring apparatus, whereby D 50 is calculated.

[0015] The D of the copper particles 50 is preferably 0.3 μm or more and 50 μm or less, more preferably 0.5 μm or more and 40 μm or less, and even more preferably 1 μm or more and 20 μm or less. D 50 Within such a range, when combined with spherical copper particles, the coating film exhibits excellent sinterability while preventing cracking of the coating film due to excessive volume shrinkage of the coating film.

[0016] The content of copper particles in the paste is preferably 50% by mass or more, more preferably 60% by mass or more and 95% by mass or less, from the viewpoint of improving the filling property of copper particles and maintaining sufficient bonding strength as a bonding layer.

[0017] A surface treatment agent may be attached to the surface of the copper particles. By allowing the surface treatment agent to adhere to the surfaces of the copper particles, excessive aggregation of the copper particles can be suppressed.

[0018] The surface treatment agent is not particularly limited, and fatty acids, aliphatic amines, silane coupling agents, titanate-based coupling agents, aluminate-based coupling agents, and the like can be used. By using these, it is possible to interact with the surfaces of the particles, improve compatibility with the organic solvent contained in the paste, improve the fluidity of the paste, and prevent oxidation of the particle surfaces.

[0019] From the viewpoint of improving the coating property or printing property of the paste, the shear rate of 10s -1 is preferably 10 Pa·s or more and 200 Pa·s or less, more preferably 15 Pa·s or more and 200 Pa·s or less. The viscosity is measured using a rheometer (viscoelasticity measuring device). The measured value is obtained using a parallel sensor and a shear rate of 10s -1 . The viscosity of the paste can be measured using a rheometer MARS III manufactured by Thermo Scientific. The measurement conditions for the viscosity of the paste are as follows. Measurement mode: Shear rate dependence measurement Sensor: Parallel type (Φ20 mm) Measurement temperature: 25°C Gap: 0.300 mm Shear rate: 0.05 to 120.01 s -1 Measurement time: 2 minutes

[0020] The thickness of the coating film 12X is preferably 1 μm to 300 μm, and more preferably 5 μm to 250 μm, so that the bonding layer described later can ensure sufficient bonding strength.

[0021] Examples of organic solvents include monoalcohols, polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, esters, nitrogen-containing heterocyclic compounds, amides, amines, and saturated hydrocarbons. These organic solvents can be used individually or in combination of two or more.

[0022] The paste may contain modifiers as appropriate to adjust various properties, as described above. Examples of modifiers include reducing agents, viscosity modifiers, and surface tension modifiers.

[0023] Suitable reducing agents include those that promote the sintering of copper particles, such as monoalcohols, polyhydric alcohols, aminoalcohols, citric acid, oxalic acid, formic acid, ascorbic acid, aldehydes, hydrazines and their derivatives, hydroxylamines and their derivatives, dithiothreitol, phosphites, hydrophosphites, phosphorous acid and its derivatives, and the like.

[0024] Viscosity modifiers are preferably those that can adjust the viscosity of the paste to be within the above viscosity range, and examples include ketones, esters, alcohols, glycols, hydrocarbons, and polymers.

[0025] Suitable surface tension modifiers include those that can adjust the surface tension of the coating film 12X, such as polymers like acrylic surfactants, silicone surfactants, alkyl polyoxyethylene ethers, and fatty acid glycerol esters, as well as monomers like alcohols, hydrocarbons, esters, and glycols.

[0026] Next, the coating film 12X is dried at a first temperature. The first temperature is preferably a temperature at which the organic solvent and adjusting agents in the coating film 12X evaporate, but the copper particles do not sinter. Therefore, it is preferably 60°C to 150°C, and more preferably 80°C to 130°C. Furthermore, it is not necessary to remove the entire amount of the organic solvent; it is sufficient to remove the organic solvent to the extent that the coating film 12X loses its fluidity. Therefore, some organic solvent may remain in the coating film 12X, and its content may be, for example, 15% by mass or less, and particularly 10% by mass or less.

[0027] Furthermore, the drying of the coating film 12X can be carried out in an inert atmosphere or under atmospheric pressure. It may also be carried out under reduced pressure. The drying time is determined by allowing sufficient evaporation of organic solvents and adjusting agents in the coating film 12X, as described above. 50 The copper particles having the above characteristics are sintered to obtain a bonding layer of sufficient thickness and sufficient bonding strength, preferably dried for 1 minute or more, more preferably 5 minutes to 120 minutes, and even more preferably 10 minutes to 60 minutes.

[0028] Next, as shown in Figure 2, the second object to be bonded 13 is placed on the dried coating film 12X to form the laminate 15.

[0029] There are no particular restrictions on the types of the first to be joined 11 and the second to be joined 13. Generally, it is preferable that both the first to be joined 11 and the second to be joined 13 contain metal on their joining surfaces. For example, at least one of the first to be joined 11 and the second to be joined 13 can be a member having a metal surface. Here, "metal" refers to the metal itself that does not form a compound with other elements, or an alloy of two or more metals. Examples of such metals include copper, silver, gold, aluminum, palladium, nickel, or alloys consisting of two or more of these.

[0030] If at least one of the first joined body 11 and the second joined body 13 is a member having a surface made of metal, the metal surface may be made of one type of metal, or it may be made of two or more types of metals. If it is made of two or more types of metals, the surface may be an alloy. The metal surface is generally preferably flat, but it may be curved in some cases.

[0031] Specific examples of the first to be bonded 11 and the second to be bonded 13 include, independently, spacers or heat sinks made of the above-mentioned metals, semiconductor elements, and substrates having at least one of the above-mentioned metals on their surface. As a substrate, for example, an insulating substrate having a metal layer such as copper on the surface of a ceramic or aluminum nitride plate can be used. When a semiconductor element is used as the to be bonded, the semiconductor element contains one or more elements such as Si, Ga, Ge, C, N, and As. The first to be bonded 11 is preferably a substrate. The second to be bonded 13 is preferably a spacer, a heat sink, or a semiconductor element.

[0032] Furthermore, a dried paste containing metal fine particles and an organic solvent can be used as at least one of the first to be bonded body 11 and the second to be bonded body 13. Specifically, a member having a metal surface can be used as the first to be bonded body 11, and a dried paste containing metal fine particles and an organic solvent can be used as the second to be bonded body 13. When using a dried paste, it is preferable to apply the paste to a support substrate made of metal such as copper and dry it to produce the dried paste.

[0033] Next, as shown in Figure 2, the laminate 15 is held between predetermined jigs 16, 16, and the laminate 15 is heated to a second temperature higher than the first temperature, while a first pressure is applied between the first to be joined 11 and the second to be joined 13 of the laminate 15 using the jigs 16, 16. This process is a pre-baking process for the coating film 12X, and in this process, the viscosity of the coating film 12X acts on the first to be joined 11 and the second to be joined 13, maintaining the relative positions between the first to be joined 11 and the second to be joined 13, and increasing the bonding strength of the coating film 12X, which will later become the bonding layer 12.

[0034] The second temperature is preferably higher than the first temperature, specifically 100°C to 300°C, and more preferably 130°C to 280°C. Setting the second temperature within this range ensures good adhesion between the coating film 12X and the first workpiece 11, and reduces the likelihood of shrinkage cracks in the fillet portion when the coating film 12X is fired to form the bonding layer 12. The heating in this process may be carried out in an inert atmosphere or under atmospheric pressure.

[0035] The first pressure is preferably 0.001 MPa to 10 MPa, more preferably 1 MPa to 10 MPa, and even more preferably 2 MPa to 8 MPa, from the viewpoint of ensuring good adhesion between the coating film 12X and the first workpiece 11 and ensuring sufficient bonding strength between the bonding layer 12 of the fillet portion and the first workpiece.

[0036] Furthermore, the process between heating to the first temperature and heating to the second temperature includes the operation of placing the second workpiece 13 on the dried coating film 12X. This operation may be performed by first heating to the first temperature, then removing the first workpiece 11 with the coating film 12X formed on it from the heating furnace, and then placing the second workpiece 13 on the coating film 12X. In this case, heating to the first temperature and heating to the second temperature are performed independently. Alternatively, the second workpiece 13 may be placed directly on the coating film 12X without removing the first workpiece 11 with the coating film 12X formed on it from the heating furnace, and heating from the first temperature to the second temperature may be performed continuously. The timing of the temperature increase from the first temperature to the second temperature and the timing of the application of the first pressure may or may not coincide.

[0037] Next, in the state shown in Figure 2, the laminate 15 is heated to a third temperature of the second temperature or higher, and a second pressure of the first pressure or higher is applied between the first to be joined 11 and the second to be joined 13 of the laminate 15 using jigs 16, 16. This process is the main firing process for the coating film 12X, and in this process the coating film 12X is fired to become the bonding layer 12 for the first to be joined 11 and the second to be joined 13.

[0038] The third temperature is preferably higher than the second temperature, specifically 180°C to 350°C, more preferably 200°C to 300°C. By setting the third temperature within this range, the sintering of copper particles in the coating film 12X is promoted, and the bonding strength between the fillet portion of the bonding layer 12 and the first workpiece 11 can be made sufficient. Furthermore, by applying the second pressure described later within the temperature range of the third temperature, not only can the bonding strength between the fillet portion of the bonding layer 12 and the first workpiece 11 be made sufficient, but the bonding strength with the second workpiece 13 can also be made sufficient.

[0039] The second pressure is preferably 1 MPa to 40 MPa, and more preferably 10 MPa to 30 MPa, from the viewpoint of ensuring sufficient bonding strength with the first joined body 11 and the second joined body 13. The holding time for the second pressure is preferably 1 second to 60 minutes, and more preferably 1 minute to 30 minutes.

[0040] Heating to the third temperature may be performed immediately after heating to the second temperature, or it may be performed independently. Furthermore, the second and third temperatures may be the same as long as they do not hinder the effects of the present invention. Moreover, the timing of the rise from the second temperature to the third temperature and the timing of the application of the second pressure may or may not coincide. Furthermore, heating in this process may be carried out in an inert atmosphere or under atmospheric pressure.

[0041] In this invention, since there is a step of drying the coating film 12X at a first temperature before placing the second workpiece 13 on it, organic solvents and adjusting agents contained in the coating film 12X can be appropriately evaporated. Subsequently, by placing the second workpiece 13 on the coating film 12X and heating and applying a second temperature and a first pressure, the adhesion between the first workpiece 11 and the coating film 12X is improved, and a good bonding relationship is obtained without the coating film 12X peeling off from the first workpiece 11 even in the fillet portion. Furthermore, by heating and applying a third temperature and a second pressure, the sintering of copper particles present in the coating film 12X is promoted, and the bonding strength can be improved without the bonding layer 12 peeling off from the first workpiece 11 even in the fillet portion.

[0042] The rate at which the pressure is increased to the first pressure is preferably 0.2 MPa / second or more and 20 MPa / second or less, and more preferably 0.5 MPa / second or more and 7 MPa / second or less. This makes it possible to further improve the bonding strength between the coating film 12X and the first workpiece 11, and consequently the bonding strength of the bonding layer 12 to the first workpiece 11, and furthermore, the bonding strength with the second workpiece 13.

[0043] Furthermore, the rate of pressure increase to the second pressure is preferably 0.2 MPa / second or higher, and may be 1 MPa / second or higher. Moreover, the rate of pressure increase to the second pressure is preferably 20 MPa / second or lower, and more preferably 10 MPa / second or lower. This makes it possible to further improve the bonding strength of the coating film 12X with the first workpiece 11, and consequently the bonding strength of the bonding layer 12 with the first workpiece 11, and furthermore, the bonding strength with the second workpiece 13.

[0044] The ratio of the second temperature to the third temperature (second temperature / third temperature) is preferably 0.28 or more and 1.00 or less in Celsius, more preferably 0.36 or more and 0.95 or less, and even more preferably 0.50 or more and 0.90 or less. By strictly controlling the second and third temperatures as described above, and setting the second temperature lower than the third temperature, the bonding strength of the coating film 12X to the first workpiece 11, and consequently the bonding strength of the bonding layer 12 to the first workpiece 11, and furthermore, the bonding strength with the second workpiece 13 can be improved.

[0045] The ratio of the first pressure to the second pressure (first pressure / second pressure) is preferably 0.025 or more and 1.00 or less in Pa, more preferably 0.05 or more and 0.80 or less, and even more preferably 0.10 or more and 0.50 or less. By strictly controlling the first and second pressures as described above, the bonding strength of the coating film 12X to the first workpiece 11, and consequently the bonding strength of the bonding layer 12 to the first workpiece 11, and furthermore, the bonding strength with the second workpiece 13 can be improved.

[0046] The bonded structure obtained according to the present invention is suitable for use in applications such as automotive electronic circuits and electronic circuits on which power devices are mounted, taking advantage of the high bonding characteristics between the workpiece and the bonding layer in the fillet portion.

[0047] In addition, other than the drying process, the process of heating and applying the second temperature and first pressure, and the process of heating and applying the third temperature and second pressure described above, heating at a predetermined temperature or applying a predetermined pressure is permitted as long as it does not hinder the effects of the present invention.

[0048] Although the present invention has been described above based on its preferred embodiments, the present invention is not limited to the above embodiments.

[0049] With regard to the embodiments described above, the present invention further discloses the following method for manufacturing a joint. [1] A method for manufacturing a bonded body in which a first body to be bonded and a second body to be bonded are bonded via a bonding layer, A step of forming a coating film by applying a paste containing copper particles whose cumulative volume particle size D50 at a cumulative volume of 50% by laser diffraction scattering particle size distribution measurement method exceeds 100 nm to the first workpiece, A step of drying the coating film at a first temperature, A step of placing the second object to be bonded on the dried coating to form a laminate, A step of heating the laminate to a second temperature above the first temperature, and applying a first pressure between the first and second parts of the laminate, A method for manufacturing a bonded body, comprising the steps of: heating the laminate to a third temperature of the second temperature or higher; applying a second pressure of the first pressure or higher between the first and second bodies to be bonded in the laminate; and sintering the coating film to form the bonded layer. [2] The method for manufacturing a bonded body according to [1], wherein the second temperature is 100°C or more and 300°C or less. [3] The method for manufacturing a bond according to [1] or [2], wherein the third temperature is 180°C or higher and 350°C or lower. [4] A method for manufacturing a joint according to any one of [1] to [3], wherein the first pressure is 0.001 MPa or more and 10 MPa or less. [5] The method for manufacturing a joint according to any one of [1] to [4], wherein the second pressure is 1 MPa or more and 40 MPa or less. [6] A method for manufacturing a joint according to any one of claims [1] to [5], wherein the rate of increasing pressure to the first pressure is 0.2 MPa / second or more and 20 MPa / second or less. [7] A method for manufacturing a joint according to any one of [1] to [6], wherein the rate of increasing pressure to the second pressure is 0.2 MPa / second or more and 20 MPa / second or less. [8] A method for manufacturing a bond according to any one of [1] to [7], wherein the ratio of the second temperature to the third temperature (second temperature / third temperature) is 0.28 or more and 1 or less. [9] A method for manufacturing a joint according to any one of [1] to [8], wherein the ratio of the first pressure to the second pressure (first pressure / second pressure) is 0.025 or more and 1 or less.

[10] A method for manufacturing a bond according to any one of [1] to [9], wherein the viscosity of the coating film is 10 Pa·s or more and 200 Pa·s or less at 25°C. [Examples]

[0050] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to these examples. Also, unless otherwise specified, "%" means "mass%".

[0051] [Example 1] (1) Preparation of paste Copper particles (spherical, D) synthesized by wet process 50 A paste was prepared by mixing (0.16 μm) with hexylene glycol and polyethylene glycol 300 as organic solvents and bis(2-hydroxyethyl)iminotris(hydroxymethyl)methane as a reducing agent. The paste contained 82% copper particles, 17.9% organic solvent, and 0.1% reducing agent.

[0052] (2) Application of the paste to the first object to be joined A rectangular coating was formed on a copper substrate by applying a paste using a printing method with a metal mask having an opening of 0.55 cm × 0.55 cm and a thickness of 150 μm. This coating was dried in an air atmosphere at 110°C (first temperature) for 20 minutes to remove the organic solvent.

[0053] (3) Placing the second object to be bonded onto the dried coating (formation of a laminate) As the second substrate to be bonded, an Ag-plated alumina chip was prepared (0.5 cm x 0.5 cm, 0.5 mm thick), assuming a model component of a semiconductor power device. Next, the Ag-plated surface of this alumina chip was placed on the dried coating film, and a load of 0.8 MPa for 2 seconds was applied to form a laminate in which the first substrate, the coating film, and the second substrate were stacked in that order.

[0054] (4) Pre-firing of the laminate The laminate was initially heated to 40°C and unloaded (excluding its own weight). Pressure was then applied in a nitrogen atmosphere until a pressure of 6 MPa (first pressure) was reached between the first and second joined parts of the laminate. Subsequently, the laminate was heated to 150°C (second temperature). The holding time at the second temperature was 10 seconds, and the holding time at the first pressure was 8.8 seconds. The average heating rate from 40°C to the second temperature was 12.5°C / second, and the pressure increase rate to the first pressure was 1.2 MPa / second.

[0055] (5) Firing of the laminate (4) Following the pre-firing of the laminate, pressure was applied in a nitrogen atmosphere between the first and second joined parts of the laminate until a pressure of 20 MPa (second pressure) was reached. The laminate was then heated to 300°C (third temperature). The holding time at the third temperature was 10 minutes, and the holding time at the second pressure was 10 minutes and 10 seconds. The average heating rate from the second to the third temperature was 9.7°C / second, and the pressure increase rate from the first to the second pressure was 1.4 MPa / second. The ratio of the second temperature to the third temperature (second temperature / third temperature) was 0.50, and the ratio of the second pressure to the first pressure (first pressure / second pressure) was 0.30.

[0056] [Example 2] The steps from "(1) Preparation of paste" to "(3) Placement of the second object to be bonded onto the dried coating (formation of the laminate)" were carried out in the same manner as in Example 1.

[0057] (4) Pre-firing of the laminate The laminate was initially heated to 40°C and unloaded (excluding its own weight). Pressure was then applied in a nitrogen atmosphere until a pressure of 6 MPa (first pressure) was reached between the first and second joined parts of the laminate. Subsequently, the laminate was heated to 260°C (second temperature). The holding time at the second temperature was 10 seconds, and the holding time at the first pressure was 13.2 seconds. The average heating rate from 40°C to the second temperature was 16.7°C / second, and the pressure increase rate to the first pressure was 1.2 MPa / second.

[0058] (5) Firing of the laminate (4) Following the pre-firing of the laminate, pressure was applied in a nitrogen atmosphere between the first and second joined parts of the laminate until a pressure of 20 MPa (second pressure) was achieved. The laminate was then heated to 300°C (third temperature). The holding time at the third temperature was 10 minutes, and the holding time at the second pressure was 10 minutes and 6 seconds. The average heating rate from the second to the third temperature was 6.7°C / second, and the pressure increase rate from the first pressure to the second pressure was 1.4 MPa / second. The ratio of the second temperature to the third temperature (second temperature / third temperature) was 0.87, and the ratio of the first pressure to the second pressure (first pressure / second pressure) was 0.30.

[0059] [Example 3] The steps from "(1) Preparation of paste" to "(3) Placement of the second object to be bonded onto the dried coating (formation of the laminate)" were carried out in the same manner as in Example 1.

[0060] (4) Pre-firing of the laminate The laminate was initially heated to 40°C and unloaded (excluding its own weight). Pressure was then applied in a nitrogen atmosphere until a pressure of 6 MPa (first pressure) was reached between the first and second joined parts of the laminate. Subsequently, the laminate was heated to 150°C (second temperature). The holding time at the second temperature was 26.2 seconds, and the holding time at the first pressure was 8.8 seconds. The average heating rate from 40°C to the second temperature was 12.5°C / second, and the pressure increase rate to the first pressure was 1.2 MPa / second.

[0061] (5) Firing of the laminate (4) Following the pre-firing of the laminate, pressure was applied in a nitrogen atmosphere between the first and second joined parts of the laminate until a pressure of 20 MPa (second pressure) was achieved. The laminate was then heated to 300°C (third temperature). The holding time at the third temperature was 10 minutes, and the holding time at the second pressure was 10 minutes and 10 seconds. The average heating rate from the second to the third temperature was 14.4°C / second, and the pressure increase rate from the first to the second pressure was 0.53 MPa / second. The ratio of the second temperature to the third temperature (second temperature / third temperature) was 0.50, and the ratio of the first pressure to the second pressure (first pressure / second pressure) was 0.30.

[0062] [Example 4] The steps from "(1) Preparation of paste" to "(3) Placement of the second object to be bonded onto the dried coating (formation of the laminate)" were carried out in the same manner as in Example 1.

[0063] (4) Pre-firing of the laminate The laminate was initially heated to 40°C and unloaded (excluding its own weight). Pressure was then applied in a nitrogen atmosphere until a pressure of 6 MPa (first pressure) was reached between the first and second joined parts of the laminate. Subsequently, the laminate was heated to 150°C (second temperature). The holding time at the second temperature was 26.2 seconds, and the holding time at the first pressure was 8.8 seconds. The average heating rate from 40°C to the second temperature was 12.5°C / second, and the pressure increase rate to the first pressure was 0.6 MPa / second.

[0064] (5) Firing of the laminate (4) Following the pre-firing of the laminate, pressure was applied in a nitrogen atmosphere between the first and second joined parts of the laminate until a pressure of 20 MPa (second pressure) was achieved. The laminate was then heated to 300°C (third temperature). The holding time at the third temperature was 10 minutes, and the holding time at the second pressure was 10 minutes and 10 seconds. The average heating rate from the second to the third temperature was 14.4°C / second, and the pressure increase rate from the first to the second pressure was 0.55 MPa / second. The ratio of the second temperature to the third temperature (second temperature / third temperature) was 0.50, and the ratio of the first pressure to the second pressure (first pressure / second pressure) was 0.30.

[0065] [Example 5] The procedure for "(1) Preparation of the paste" was carried out in the same manner as in Example 1. The procedures for "(2) Application of the paste to the first substrate" to "(3) Placement of the second substrate on the dried coating (formation of the laminate)" were carried out in the same manner as in Example 1 for four sets.

[0066] (4) Pre-firing of the laminate The four sets mentioned above were pre-fired together. Starting from an initial temperature of 40°C and an unloaded state (excluding its own weight), pressure was applied in a nitrogen atmosphere until a pressure of 1 Pa (first pressure) was reached between the first and second joined parts of each laminate. Subsequently, the laminate was heated to 260°C (second temperature). The holding time at the second temperature was 10 seconds, and the holding time at the first pressure was 13.2 seconds. The average heating rate from 40°C to the second temperature was 16.7°C / second, and the pressure increase rate to the first pressure was 0.2 MPa / second.

[0067] (5) Firing of the laminate The four sets mentioned above were subjected to the main firing process together. (4) Following the pre-firing of the laminate, pressure was applied in a nitrogen atmosphere between the first and second joined parts of the laminate until a pressure of 20 MPa (second pressure) was reached. The laminate was then heated to 300°C (third temperature). The holding time at the third temperature was 10 minutes, and the holding time at the second pressure was 10 minutes and 6 seconds. The average heating rate from the second to the third temperature was 6.7°C / second, and the pressure increase rate from the first pressure to the second pressure was 1.9 Pa / second. The ratio of the second temperature to the third temperature (second temperature / third temperature) was 0.87, and the ratio of the first pressure to the second pressure (first pressure / second pressure) was 0.05.

[0068] [Comparative Example 1] In the same manner as in Example 1, (1) the paste was prepared, (2) the paste was applied to the first workpiece, and (3) the second workpiece was placed on the dried coating (forming a laminate). Then, (4) the laminate was not pre-fired, and (5') the laminate was fired.

[0069] (5') Firing of the laminated body The laminate was initially heated to 40°C and unloaded (excluding its own weight). Pressure was then applied in a nitrogen atmosphere until a pressure of 20 MPa was reached between the first and second joined layers of the laminate. Subsequently, the laminate was heated to 300°C. The holding time at 300°C was 10 minutes, and the holding time at 20 MPa was 10 minutes and 15 seconds. The average heating rate from 40°C to 300°C was 17.3°C / second, and the pressure increase rate to 20 MPa was 1.3 MPa / second.

[0070] [Comparative Example 2] In the same manner as in Example 1, (1) the paste was prepared, (2) the paste was applied to the first workpiece, and (3) the second workpiece was placed on the dried coating (forming a laminate). Then, (4) the laminate was not pre-fired, and (5') the laminate was fired.

[0071] (5') Firing of the laminated body Starting from an initial temperature of 40°C and an unloaded state (excluding its own weight), pressure was applied to the first and second joined layers of the laminate in a nitrogen atmosphere until it reached 6 MPa. The pressure increase rate to 6 MPa was 0.4 MPa / second. After applying 6 MPa for 10 seconds, the pressure was increased to 20 MPa. The pressure increase rate from 6 MPa to 20 MPa was 2.8 MPa / second. Subsequently, the laminate was heated from 40°C to 300°C. The holding time at 300°C was 10 minutes, and the holding time at 20 MPa was 10 minutes and 15 seconds. The average heating rate from 40°C to 300°C was 17.3°C / second.

[0072] [Evaluation of cracking in the fillet section] The fillet portions of the laminates fabricated in the examples and comparative examples were observed using a digital microscope (RH-2000, manufactured by Hirox Corporation) in a plan view. Specifically, the presence or absence of cracks was checked throughout the entire fillet portion, from the outer circumference of the chip (i.e., from the inner circumference to the outer circumference of the fillet portion). Laminates without cracks were rated "A," and those with cracks were rated "B." The evaluation results are shown in Table 1.

[0073] [Evaluation of peeling of the fillet area] The laminates prepared in the examples and comparative examples were examined using an ultrasonic flaw detection system (Hitachi Power Solutions, model number: FineSAT III) with a 75MHz probe, observing the fillet condition from the copper substrate side using the reflection method. With this system, areas with good bonding are observed as darker colors (black), while areas with delamination and poor bonding are observed as lighter colors (white). When observing the delamination state of the fillet, the gain value was set to 25-35 dB, and the delay and width of the S-gate were adjusted so that the peak position of the S-gate was on the surface of the copper plate. To specify the observation range of the bonding layer, the delay of the F-gate was adjusted and the width was set to a peak width of 1.5 wavelengths. The Z-axis coordinate of the probe was adjusted to maximize the amplitude of the observation peak, and observation was performed. The image brightness was automatically set using the device's operation software (FineSAT) to obtain image data for analysis. Next, the degree of peeling (%) of the fillet portion was calculated using this analysis image data and the image processing software imageJ. Fillet portions with a threshold of 201 or higher in imageJ were defined as peeled portions. The coated portion was defined as X, and the joint portion where the alumina chip was pressure-bonded was defined as Y (25mm). 2 ), with the delamination area of ​​the fillet portion (XY) as Z, the delamination percentage of the fillet portion (%) was calculated as Z / (XY) × 100. For Example 5, the delamination percentage of the fillet portion was calculated for four laminates, and the average value of the four was calculated. The calculation results of the delamination percentage of the fillet portion are shown in Table 1. If the delamination percentage of the fillet portion is 30% or less, it can be determined that the bonding strength between the joined material and the bonding layer at the fillet portion is high.

[0074] [Table 1] [Industrial applicability]

[0075] According to the present invention, it is possible to provide a manufacturing method that provides excellent bonding strength between the workpiece and the bonding layer in the fillet portion.

Claims

1. A method for manufacturing a joined body in which a first joined body and a second joined body are joined via a bonding layer, Volume cumulative particle size D at 50% cumulative volume, as measured by laser diffraction scattering particle size distribution analysis. 50 The process involves applying a paste containing copper particles exceeding 100 nm to the first object to be bonded to form a coating film, A step of drying the coating film at a first temperature, A lamination step in which the second object to be bonded is placed on the dried coating to form a laminate, A pre-firing step is performed in which the laminate is heated to a second temperature above the first temperature, and a first pressure is applied between the first and second parts of the laminate to be joined. The process includes heating the laminate to a third temperature of the second temperature or higher, and applying a second pressure of the first pressure or higher between the first and second parts of the laminate to sinter the coating film to form the bonding layer, The aforementioned main firing process is carried out without lowering the temperature after the aforementioned pre-firing process. A method for manufacturing a bonded body, comprising performing the lamination process such that, when the bonded layer is viewed in plan, there is a portion at the end of the bonded layer where the second body to be bonded is not placed.

2. The method for manufacturing a bonded body according to claim 1, wherein the second temperature is 100°C or more and 300°C or less.

3. The method for manufacturing a bonded body according to claim 1 or 2, wherein the third temperature is 180°C or higher and 350°C or lower.

4. The method for manufacturing a bonded body according to claim 1 or 2, wherein the first pressure is 0.001 MPa or more and 10 MPa or less.

5. The method for manufacturing a jointed body according to claim 1 or 2, wherein the second pressure is 1 MPa or more and 40 MPa or less.

6. A method for manufacturing a bonded body according to claim 1 or 2, wherein the rate of increasing pressure to the first pressure is 0.2 MPa / second or more and 20 MPa / second or less.

7. A method for manufacturing a bonded body according to claim 1 or 2, wherein the rate of increasing pressure up to the second pressure is 0.2 MPa / second or more and 20 MPa / second or less.

8. A method for manufacturing a bonded body according to claim 1 or 2, wherein the ratio of the second temperature to the third temperature (second temperature / third temperature) is 0.28 or more and 1 or less.

9. A method for manufacturing a jointed body according to claim 1 or 2, wherein the ratio of the first pressure to the second pressure (first pressure / second pressure) is 0.025 or more and 1 or less.

10. The method for manufacturing a bonded body according to claim 1 or 2, wherein the viscosity of the coating film is 10 Pa·s or more and 200 Pa·s or less at 25°C.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor device

    JP2018110149A

  • Bonding method by using conductive adhesive

    JP2020136580A

  • Bonding composition, bonding structure of electric conductor, and method for manufacturing same

    WO2020032161A1

  • Power semiconductor module and power conversion device

    WO2020208713A1

  • Conductive composition, conductive sintered part, and member having conductive sintered part

    WO2021235447A1