Method and apparatus for etching a carbon-containing layer

A boron-containing passivant gas and oxygen-containing gas plasma etching process addresses bowing and clogging issues in carbon-containing masks, enhancing ellipticity and CD uniformity without degrading throughput.

JP7955345B2Active Publication Date: 2026-11-24LAM RES CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024513890
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-02
Filing Date
2022-09-01
Publication Date
2026-11-24
Estimated Expiration
2042-09-01

AI Technical Summary

Technical Problem

Current plasma etching techniques for carbon-containing masks in semiconductor devices face challenges with bowing, clogging, critical dimension (CD) uniformity, and throughput when etching high aspect ratio features, as improving one characteristic often degrades another.

Method used

A simultaneous etch and passivation process using a boron-containing passivant gas and an oxygen-containing gas in a plasma etching system, which etches features into the carbon-containing layer, improving ellipticity and reducing bowing and clogging without increasing CD variation.

Benefits of technology

The process achieves improved ellipticity and local CD uniformity while maintaining throughput, reducing bowing and clogging, and optimizing etching parameters in a single step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955345000002
    Figure 0007955345000002
  • Figure 0007955345000003
    Figure 0007955345000003
  • Figure 0007955345000004
    Figure 0007955345000004
Patent Text Reader

Abstract

A method for etching features in a carbon-containing layer beneath a mask is provided, comprising flowing an etching gas comprised of a boron-containing passivant gas and an oxygen-containing gas, wherein a plasma is generated from the etching gas, and the plasma etches the features into the carbon-containing layer.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Cross-Reference to Related Applications This application claims the benefit of priority from U.S. Patent Application No. 63 / 240,224, filed on September 2, 2021, which is incorporated herein by reference in its entirety for all purposes.

[0002] The background description provided herein is for the purpose of generally presenting the context of the disclosure. The information described in this Background section, as well as aspects of the description that may not otherwise qualify as prior art at the time of filing, are neither expressly nor impliedly admitted as prior art against the present disclosure.

[0003] The present disclosure relates to a method of forming a semiconductor device on a semiconductor wafer. More specifically, the present disclosure relates to etching a carbon-containing layer during the formation of a semiconductor device.

[0004] In forming semiconductor devices, holes or other features are etched. A carbon-containing layer, such as an amorphous carbon layer mask, may be used as a mask for etching features. When forming high aspect ratio channel features in an amorphous carbon layer mask, the etch process has bowing, clogging, critical dimension (CD), ellipticity, local critical dimension uniformity (LCDU), and throughput characteristics. Various processes attempt to optimize these various characteristics. However, improving one characteristic may degrade another characteristic. Summary of the Invention

[0005] To achieve the foregoing, and in accordance with the purposes of the present disclosure, a method of etching features into a carbon-containing layer under a mask is provided. A simultaneous etch and passivation step is provided that includes flowing an etch gas comprising a boron-containing passivant gas and an oxygen-containing gas. A plasma is generated from the etch gas, and the plasma etches features into the carbon-containing layer.

[0006] Another feature provides an apparatus for processing wafers having a carbon-containing layer. A processing chamber is provided. A substrate support holds the substrate inside the processing chamber. A coil supplies RF power to the processing chamber. A gas system for simultaneously supplying boron-containing passive and oxygen into the processing chamber includes a boron-containing passive source and an oxygen source.

[0007] These and other features of this disclosure are described in further detail below in conjunction with the detailed description and the following drawings. [Brief explanation of the drawing]

[0008] This disclosure is illustrated in the figures of the attached drawings for illustrative purposes only and is not intended to be limiting. In this disclosure, similar reference figures refer to similar elements.

[0009] [Figure 1A] Figure 1A is a schematic cross-sectional view of a stack processed according to one embodiment. [Figure 1B] Figure 1B is a schematic cross-sectional view of a stack processed according to one embodiment.

[0010] [Figure 2A] Figure 2A is a top view of the stack shown in Figures 1A and 1B. [Figure 2B] Figure 2B is a top view of the stack shown in Figures 1A and 1B.

[0011] [Figure 3] Figure 3 is a high-level flowchart of one embodiment.

[0012] [Figure 4A] Figure 4A is a cross-sectional view of a stack processed in various embodiments. [Figure 4B] Figure 4B is a cross-sectional view of a stack processed in various embodiments. [Figure 4C]FIG. 4C is a cross-sectional view of a stack processed in various embodiments. [Figure 4D] FIG. 4D is a cross-sectional view of a stack processed in various embodiments.

[0013] [Figure 5] FIG. 5 is a schematic diagram of a semiconductor processing chamber that may be used in one embodiment.

[0014] [Figure 6] FIG. 6 is a schematic diagram of a computer system that may be used in implementing one embodiment.

[0015] [Figure 7] FIG. 7 is a schematic diagram of a semiconductor processing chamber that may be used in another embodiment. DETAILED DESCRIPTION

[0016] Embodiments will now be described in detail with reference to some preferred embodiments thereof, as illustrated in the accompanying drawings. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present disclosure. It will be apparent, however, to one skilled in the art that the present disclosure may be practiced without some or all of these specific details. In other instances, well known process steps and / or structures have not been described in detail in order to not unnecessarily obscure the present disclosure.

[0017] Carbon-containing masks are sometimes used during the formation of semiconductor devices. In the formation of memory, such as three-dimensional NAND (3D NAND) devices and dynamic random access memory (DRAM) devices, alternating layers of memory stacks may be etched to form features. To increase chip density and reduce bit cost, 3D NAND devices continue to increase the number of alternating layers in the mold stack. The increase in the number of stack layers presents more serious challenges in pattern transfer from the lithography level to the mold stack level. For NAND with more than 90 layers, current plasma etching techniques are challenged by the need to continue etching with a larger aspect ratio. As the device size decreases while the amount of memory increases, more alternating layers are required, which can result in a thicker memory stack. Carbon-containing masks, such as amorphous carbon, may be used as masks to etch features into memory devices. As the stack thickness increases, the thickness of the carbon-containing mask also increases. As the thickness of the carbon-containing mask increases and the size of the features decreases, the depth-to-width aspect ratio increases. When etching high aspect ratio features, the etching process can be plagued by bowing and clogging. It is desirable to minimize local CD uniformity (LCDU) while maximizing throughput and bringing the ellipticity close to 1. Furthermore, it is desirable to achieve the target CD. Various processes attempt to optimize these various properties. However, improving one property often degrades another.

[0018] For ease of understanding, in one embodiment a stack comprised of ONON (silicon oxide (SiO2), silicon nitride (SiN), silicon oxide, silicon nitride, and repetition) with a multilayer mask is provided. FIG. 1A is a schematic cross-sectional view of a stack 100 comprising a substrate 104 below a memory stack 108 comprised of a plurality of bilayers where a layer 116 of silicon oxide (SiO2) is over a top surface of a layer 112 of silicon nitride. A carbon containing mask 120 is over the memory stack 108. In one embodiment, the carbon containing mask 120 comprises an amorphous carbon layer (ACL). In one embodiment, amorphous carbon is an amorphous carbon material. A patterned mask 124 is over the carbon containing mask 120. In one embodiment, the patterned mask 124 comprises silicon oxynitride (SiON). In other embodiments, the patterned mask 124 may comprise other materials.

[0019] FIG. 2A is a top view of a portion of the stack 100 showing the top of the patterned mask 124 and mask features 136. The mask features 136 are cylindrical holes with a circular cross section as shown.

[0020] FIG. 3 is a high level flowchart of one embodiment. In one embodiment, the stack is placed in a process chamber (step 304). The carbon containing mask 120 is opened (step 308) by etching features in the carbon containing mask 120, using the patterned mask 124. In one embodiment, the carbon containing mask 120 is etched (step 312) by flowing an etch gas in the process chamber. In one embodiment, the etch gas comprises a passivation gas and an opening gas. In one embodiment, the passivation gas is B x H y where x and y are positive integers, such as BCl3, BF3, BBr3, B2H6 or B2H2, and one or more of BD x Hy The etched gas is composed of boron-containing gases, such as (where D is a halogen and x and y are positive integers). In this embodiment, the etched gas is composed of oxygen-containing gases, such as one or more of oxygen (O2), sulfur dioxide (SO2), carbonyl sulfide (COS), carbon dioxide (CO2), and ozone (O3). In one example, the etching gas is composed of BCl3 and SO2.

[0021] An etching gas is formed in the plasma (step 316). In this embodiment, the plasma is formed by supplying radio frequency (RF) power between approximately 50 watts and approximately 10,000 watts at approximately 13.56 MHz to the processing chamber by a TCP coil. Other embodiments may provide other RF frequencies. A pulsed bias having an amplitude of 50 volts to 3,000 volts is supplied to the stack 100. In this embodiment, the bias has an RF frequency of 13.56 MHz, 27 MHz, 2 MHz, 1 MHz, or 400 kHz, with either a continuous wave or a pulse frequency between approximately 1 Hz and approximately 10,000 Hz and a duty cycle between approximately 3% and approximately 99%. After approximately 5 seconds to approximately 2,000 seconds, the flow of etching gas into the processing chamber is stopped. The duration of the etching process in this embodiment is sufficient to etch the features through the carbon-containing mask 120. A substrate temperature of -60°C to 120°C is provided.

[0022] Figure 1B is a schematic cross-sectional view of stack 100 after etching the carbon-containing mask 120 (step 308). Figure 2B is a top view of a portion of stack 100, showing the top surfaces of the patterned mask 124 and mask features 136 after etching the carbon-containing mask 120 (step 308). Etching the carbon-containing mask 120 may make the circular cross-section of the mask features 136 more elongated, as shown in the figure. Ellipticity is measured by the ellipticity ratio obtained by dividing the major axis of the feature by the minor axis of the feature, and vice versa. The major axis may be the widest dimension of the feature, and the minor axis may be the narrowest dimension of the feature. In Figure 2B, for one of the mask features 136, the major axis is shown as dimension J and the minor axis is shown as dimension N. Experiments have shown that for mask features 136, the ellipticity is improved (closer to a perfect circle, closer to 1.0) than the prior art method, without increasing the variation in CD between features or increasing bowing. The mask thus obtained can improve defect performance when etching features onto the memory stack 108 using the obtained carbon-containing mask 120. By etching the mask features 136 using a plasma formed from an etching gas composed of a boron-containing passive gas and an oxygen-containing gas, an improved ellipticity can be obtained without increasing the variation in CD between features and without increasing bowing.

[0023] Plasma sputters a portion of the patterned mask 124. The sputtered patterned mask 124 is redeposited to form a silicon-containing redeposited hard mask. The redeposited hard mask may alter the CD and circular cross-section of the mask features 136. Non-circular cross-sections can also occur using sulfur-based passivation. Sulfur-based passivation may be deposited on etching fronts in non-uniform patterns where ellipticity is increased. Adding sulfur-based passivation has been shown to reduce ellipticity but help protect the CD. Sputtering and faceting of the patterned mask 124 may also cause clogging or reduction in the size of the mask features 136, bowing of the mask features 136, and a decrease in LCDU. Increasing the temperature has been shown to improve ellipticity but increase the CD. Because the SiON in the patterned mask 124 is non-volatile, the sputtered SiON adheres to portions of the features, causing clogging.

[0024] Boron-containing passivation gases were found to improve the protection of the sidewalls of the mask features 136 of the patterned mask 124 and the carbon-containing mask 120. The improved protection of the patterned mask 124 reduces sputtering and redeposition of the patterned mask 124 compared to processes using carbon or sulfur-containing passivation. Boron-containing passivation was also found to reduce clogging. Furthermore, boron-containing passivation gases were unexpectedly found to reduce bowing. Oxygen-containing gases facilitate etching of the carbon-containing mask 120. In some embodiments, supplying BCl3 passivation gas reduces clogging and consumption of the patterned mask 124. Bowing is also eliminated. As a result, LCDU is improved. These improvements are achieved without increasing CD, while reducing ellipticity. Using a boron-containing passivation gas eliminates the need for a sulfur passivant due to the presence of a boron passivant, reducing ellipticity and allowing the etching gas to be sulfur-free. In some embodiments, the etching gas is sulfur-free, carbon-free, and halogen-free. In some embodiments, the etching gas further comprises a sulfur-containing component.

[0025] Previously, a two-step periodic process was used to improve etching parameters. Such a two-step process may include a passivation step and an etching step. Such a periodic process increases etching time and decreases throughput. In this embodiment, a single step is used to etch 90% to 100% of the depth of the features etched into the carbon-containing mask 120. By providing a single step to etch 90% to 100% of the depth of the features, etching time is reduced and throughput is increased. In this single step, etching and passivation are performed simultaneously in a single step. [Table 1]

[0026] Table 1 compares the results of etching the carbon-containing mask 120 using a sulfur-containing passive bunt with the results using a BCl3 passive bunt. Bow CD is the maximum CD after the mask feature 136 has been etched into the carbon-containing mask 120. Dimple CD is the average CD after the dimples have been etched into the layer below the carbon-containing mask 120. LCDU is local CD uniformity, meaning 3 sigma of the entire CD. Etching rate is the average number of nanometers (nm) etched per second. Ellipticity is calculated by dividing the major axis J by the minor axis N, as shown in Figure 2B. Since the ellipticity of the BCl3 passive bunt is closer to 1 than that of the sulfur passive bunt, the BCl3 passive bunt provides a more circular feature cross-section. In one embodiment, the mask feature 136 forms a channel feature with a CD in the range of 60 nm to 80 nm or a contact feature with a CD in the range of 150 nm to 200 nm. In other embodiments, the mask feature 136 may be a linear slit having a width with a CD in the range of 150 nm to 200 nm. For hard mask aperture patterning applications, the CD is in the range of 5 nm to 25 nm. Embodiments provide features having a width of less than 80 nm with a depth-to-width aspect ratio greater than 50.

[0027] After opening the carbon-containing mask (step 308), additional process steps may be provided (step 320). In this embodiment, features are etched within the stack 108 beneath the carbon-containing mask 120. In such a step, the carbon-containing mask 120 is used as a mask for etching the stack 108 beneath the carbon-containing mask 120 in the formation of DRAM or NAND. In various embodiments, the carbon-containing mask 120 may be located on other types of logic stacks and next-generation memory device stacks. In some embodiments, the carbon-containing mask 120 is removed after the stack 108 has been etched. The stack 108 is removed from the processing chamber (step 324).

[0028] In another embodiment, to provide profile engineering, the concentration of the boron-containing passive gas may be varied or a periodic process may be provided. In some embodiments, a periodic or two-step process having a step in which the boron passive gas is stopped includes the addition of a sulfur-containing component during that step. Figure 4A is a schematic cross-sectional view of a stack 400 consisting of a carbon-containing mask 420 beneath a patterned mask 424 having slot-shaped features 436. In this embodiment, the patterned mask 424 is made of silicon oxynitride (SiON) and the carbon-containing mask 420 is ACL. In this example, the sidewalls of the carbon-containing mask 420 are arc-shaped. Such arc-shaped features result from an etching process using oxygen gas without a passive gas. Because this process does not have a passive gas, the sidewalls of the carbon-containing mask 420 are etched, resulting in the arc shape.

[0029] Figure 4B is a schematic cross-sectional view of a stack 400 comprising a carbon-containing mask 420 beneath a patterned mask 424 having slot-shaped features 436. In this embodiment, the patterned mask 424 is made of silicon oxynitride (SiON), and the carbon-containing mask 420 is ACL. In this example, the sidewalls of the carbon-containing mask 420 form a taper. Such tapered features result from an etching process using oxygen gas and an excess of boron-containing passive gas. The excess boron-containing passive gas protects the sidewalls of the carbon-containing mask 420, resulting in the tapered shape.

[0030] Figure 4C is a schematic cross-sectional view of a stack 400 consisting of a carbon-containing mask 420 beneath a patterned mask 424 having a slot-shaped feature 436. In this embodiment, the patterned mask 424 is made of silicon oxynitride (SiON), and the carbon-containing mask 420 is ACL. In this example, the sidewalls of the carbon-containing mask 420 form vertical sidewalls. Such vertical sidewalls result from an etching process with a controlled gas mixture of oxygen and boron-containing passive gas. Proper control of the oxygen-containing gas and boron-containing passive gas protects the sidewalls of the carbon-containing mask 420 and prevents bowing or taper of the sidewalls. Thus, with proper control, vertical sidewalls are produced by combining tapered etching and bowing. In slit-shaped features, preventing bowing is important. If the sidewalls of the slit become bow-shaped, the width of the slit in the center of the feature becomes significantly larger than the width of the slit at the top or bottom of the feature. Various embodiments provide a ratio of the width of the slit at the center of the feature to the width of the slit at the bottom of the feature, ranging from 2:1 to 1:1.

[0031] In various embodiments, the preparation of the mixture of oxygen-containing gas and boron-containing passivation gas may be achieved by other means. In the embodiment shown in Figure 3, the oxygen-containing gas and boron-containing passivation gas are mixed at a constant flow rate to provide a single step using a constant etching gas. As mentioned above, such a process provides high throughput. In another embodiment, the ratio of oxygen-containing gas to boron-containing passivation gas is changed over time. For example, the flow rate of the oxygen-containing gas may be constant, while the flow rate of the boron-containing passivation gas is varied, such as by creating a gradient. In another embodiment, the flow rate of the oxygen-containing gas may be constant, while the flow rate of the boron-containing passivation gas is pulsed. Pulsing the boron-containing passivation gas provides temporal adjustment. In another example, either or both of the oxygen-containing gas and boron-containing passivation gas are gradient. Such ramping may be continuously increased, continuously decreased, or alternating between increase and decrease.

[0032] In other embodiments, the preparation of the mixture of oxygen-containing gas and boron-containing passive gas may be varied over time to provide a specially prepared sidewall profile. Figure 4D is a schematic cross-sectional view of a stack 400 comprising a carbon-containing mask 420 beneath a patterned mask 424 having a slot-shaped feature 436. In this embodiment, the patterned mask 424 is made of silicon oxynitride (SiON), and the carbon-containing mask 420 is ACL. In this example, the sidewalls of the carbon-containing mask 420 form an inverted bottle-shaped sidewall. In this example, the preparation provides a sidewall that is vertical near the top and bottom and tapers towards the middle, as shown. The vertical sidewalls near the top and bottom of the feature result from a prepared etching process of the mixture of oxygen-containing gas and boron-containing passive gas. In this embodiment, a bowing process and a taper process are used alternately to achieve a straight profile with vertical sidewalls. Alternating between bowing and taper processes may be achieved by alternating between having more boron-containing passive gas and more oxygen gas as a function of time. By appropriately adjusting the oxygen-containing gas and boron-containing passive gas, the sidewalls of the carbon-containing mask 420 are protected and bowing and taper are prevented. The tapered sidewalls in the central part of the feature result from the etching process with an excess of boron-containing passive gas. In other embodiments, other adjusted sidewall shapes may be provided.

[0033] Figure 5 schematically shows an example of a plasma processing system 500 that may be used to process the stack 100 according to an embodiment. The plasma processing system 500 includes a plasma reactor 502 having a plasma processing chamber 504 enclosed by chamber walls 576. Coordinated by a matched network 508, a plasma power supply 506 powers a transformer-coupled power (TCP) coil 510 located near a power window 512 to generate plasma 514 in the plasma processing chamber 504 by supplying inductively coupled power. The TCP coil (upper power supply) 510 may be configured to generate a uniform diffusion profile within the plasma processing chamber 504. For example, the TCP coil 510 may be configured to generate a toroidal power distribution in the plasma 514. A power window 512 is provided to isolate the TCP coil 510 from the plasma processing chamber 504, but energy can still pass from the TCP coil 510 to the plasma processing chamber 504. The wafer bias voltage power supply 516, coordinated by the matching network 518, powers the electrode 520 to set a bias voltage on the stack 100 supported on the electrode 520. The electrode 520 is also a substrate support. The controller 524 sets the points between the plasma power supply 506 and the wafer bias voltage power supply 516.

[0034] The plasma power supply 506 and the wafer bias voltage power supply 516 may be configured to operate at specific radio frequencies such as 13.56 megahertz (MHz), 27 MHz, 2 MHz, 1 MHz, 400 kilohertz (kHz), or a combination thereof. The plasma power supply 506 and the wafer bias voltage power supply 516 may be sized appropriately to supply a range of power to achieve desired process performance. For example, in one embodiment, the plasma power supply 506 may supply power in the range of 50 to 10,000 watts, and the wafer bias voltage power supply 516 may supply a bias voltage in the range of 50 to 3,000 volts (V). Furthermore, the TCP coil 510 and / or electrode 520 may consist of two or more subcoils or subelectrodes, and these subcoils or subelectrodes may be powered by a single power supply or by multiple power supplies.

[0035] As shown in Figure 5, the plasma processing system 500 further includes a gas source / gas supply mechanism 530 (gas system). The gas source / gas supply mechanism 530 supplies gas to the gas supply unit 540 in the form of nozzles. In this embodiment, the gas source / gas supply mechanism 530 comprises a boron-containing passive source and heater 532, an oxygen source 534, and other gas sources 536. The boron-containing passive source and heater 532, the oxygen source 534, and the other gas sources 536 supply gas to a mixing manifold 538 that provides a plenum from which the gas can be mixed before going to the gas supply unit 540. If the boron-containing passive source is BCl3, the heater 532 is positioned to heat and vaporize the BCl3. In one embodiment, the controller 524 has computer-readable code for simultaneously supplying oxygen from the oxygen source 534 and BCl3 from the boron-containing passive source and heater to the mixing manifold 538. Oxygen and BCl3 are mixed in a mixing manifold before flowing through the gas supply unit 540 into the plasma processing chamber 504. Process gases and by-products are removed from the plasma processing chamber 504 via a pressure control valve 542 and a pump 544. The pressure control valve 542 and pump 544 may also function to maintain a specific pressure within the plasma processing chamber 504. The gas source / gas supply mechanism 530 is controlled by a controller 524. Kiyo from Lam Research Corp., Fremont, California may be used to carry out the embodiment.

[0036] In some embodiments, the plasma wetted surfaces of the plasma processing system 500 have a protective coating to protect the plasma wetted surfaces from plasma generated from BCl3 at high bias power ranging from 50 to 3000 volts. In some embodiments, the coating may further provide protection from plasma generated from a mixture of BCl3 and oxygen at high bias power. In some embodiments, the protective coating is at least one of rare earth oxides, rare earth fluorides, or rare earth oxyfluorides. For example, the protective coating may be a coating of yttria, yttrium fluoride, or yttrium oxyfluoride. In some embodiments, the protective coating is applied using a thermal spraying process. In other embodiments, the protective coating may be deposited using other processes, such as aerosol deposition or atomic layer deposition. In some embodiments, the protective coating is provided on an electrode 520 that functions as an electrostatic chuck, or on the chamber wall 576. In some embodiments, a liner is provided inside the chamber wall 576, and the protective coating is placed on the plasma wetted surface of the liner. In Figure 5, a protective coating 583 is shown on the plasma-contacting surface of the chamber wall 576. In this embodiment, the chamber wall 576 is aluminum or an aluminum alloy. In this embodiment, an anodic oxide layer is formed over the plasma-facing surface of the chamber wall 576. Plasma generated from BCl3 with a high bias may damage the anodic oxide layer. Therefore, the protective coating 583 can protect the anodic oxide layer in the presence of plasma generated from BCl3 with a high bias. In another embodiment, a ceramic plate of aluminum oxide may be placed between the electrode 520 and the stack 100. Plasma generated from BCl3 with a high bias may damage the ceramic plate of aluminum oxide. The protective coating can reduce or eliminate such damage. Plasma damage may generate contaminants. Such contaminants increase defects. Therefore, the protective coating can reduce defects.

[0037] Figure 6 is a high-level block diagram showing a computer system 600 suitable for implementing the controller 524 used in the embodiment. The computer system may have many physical forms, ranging from integrated circuits, printed circuit boards, and small handheld devices to massive supercomputers. The computer system 600 includes one or more processors 602, an electronic display device 604 (for displaying graphics, text, and other data), main memory 606 (e.g., random access memory (RAM)), storage device 608 (e.g., hard disk drive), removable storage device 610 (e.g., optical disc drive), user interface device 612 (e.g., keyboard, touchscreen, keypad, mouse, or other pointing device, etc.), and a communication interface 614 (e.g., wireless network interface). The communication interface 614 allows software and data to be transferred between the computer system 600 and external devices via a link. The system may also include a communication infrastructure 616 (e.g., communication bus, crossover bar, or network) to which the aforementioned devices / modules are connected.

[0038] The information transferred via the communication interface 614 may be in the form of signals such as electronic signals, electromagnetic signals, optical signals, or other signals that can be received by the communication interface 614 via a signal-transmitting communication link, and may be implemented using wires or cables, optical fibers, telephone lines, mobile phone links, radio frequency links, and / or other communication channels. Using such a communication interface, it is intended that one or more processors 602 may receive information from or output information to the network in the process of performing the method steps described above. Furthermore, embodiments of the method may be performed by a single processor or in conjunction with a remote processor that shares part of the processing, and may be performed over a network, such as the Internet.

[0039] The term “non-transient computer-readable medium” is generally used to refer to media such as main memory, secondary memory, removable storage devices, and storage devices such as hard disks, flash memory, disk drive memory, CD-ROMs, and other forms of persistent memory, and should not be interpreted to cover transient subjects such as carrier waves or signals. Examples of computer code include files containing machine code, such as those generated by a compiler, and high-level code executed by a computer using an interpreter. Computer-readable medium may also be computer code transmitted by computer data signals, which are embodied in carrier waves and represent sequences of instructions executable by a processor.

[0040] Figure 7 schematically shows an example of a plasma processing system 700 that may be used to process the stack 100 according to another embodiment. The plasma processing system 700 includes a plasma reactor 702 having a plasma processing chamber 704 enclosed by a chamber wall 776. Coordinated by a matched network 708, a plasma power supply 706 powers a transformer-coupled power (TCP) coil 710 located near a power window 712 to generate plasma 714 in the plasma processing chamber 704 by supplying inductively coupled power. The TCP coil (upper power supply) 710 may be configured to generate a uniform diffusion profile within the plasma processing chamber 704. For example, the TCP coil 710 may be configured to generate a toroidal power distribution in the plasma 714. A power window 712 is provided to isolate the TCP coil 710 from the plasma processing chamber 704, but energy can still pass from the TCP coil 710 to the plasma processing chamber 704. The wafer bias voltage power supply 716, coordinated by the matching network 718, powers the electrode 720 to set a bias voltage on the stack 100 supported above the electrode 720. The controller 724 sets the points between the plasma power supply 706 and the wafer bias voltage power supply 716.

[0041] The plasma power supply 706 and the wafer bias voltage power supply 716 may be configured to operate at specific radio frequencies such as 13.56 megahertz (MHz), 27 MHz, 2 MHz, 1 MHz, 400 kilohertz (kHz), or a combination thereof. The plasma power supply 706 and the wafer bias voltage power supply 716 may be sized appropriately to supply a range of power to achieve desired process performance. For example, in one embodiment, the plasma power supply 706 may supply power in the range of 50 to 5000 watts, and the wafer bias voltage power supply 716 may supply a bias voltage in the range of 0 to 3000 volts (V). Furthermore, the TCP coil 710 and / or electrode 720 may consist of two or more subcoils or subelectrodes, and these subcoils or subelectrodes may be powered by a single power supply or by multiple power supplies.

[0042] As shown in Figure 7, the plasma processing system 700 further includes a gas source / gas supply mechanism including a boron-containing passive source 732, an oxygen source 734, and other gas sources 736. The oxygen source 734 and other gas sources 736 supply gas to a first gas supply unit 740. If the boron-containing passive source is BCl3, a line heater 733 is provided to heat the line to vaporize the BCl3. In this embodiment, the boron-containing passive source 732 is connected to a second gas supply unit 741 via the line heater 733. In this embodiment, the controller 724 includes computer-readable code for simultaneously flowing oxygen from the oxygen source 734 and boron-containing passive source 732 and mixing them in the plasma processing chamber 704. Process gases and by-products are removed from the plasma processing chamber 704 via a pressure control valve 742 and a pump 744. Additionally, the pressure control valve 742 and pump 744 may function to maintain a specific pressure within the plasma processing chamber 704. The gas source / gas supply mechanism 730 is controlled by the controller 724. The positions of the first gas supply unit 740 and the second gas supply unit 741 may be arranged in various positions depending on the desired gas distribution and mixing.

[0043] While this disclosure has been described in terms of several preferred embodiments, there are variations, modifications, permutations, and various alternative equivalents that fall within the scope of this disclosure. It should also be noted that there are many alternative ways of carrying out the methods and apparatus of this disclosure. Therefore, the following appended claims are intended to be interpreted as including all variations, modifications, permutations, and various alternative equivalents that fall within the true intent and scope of this disclosure. This disclosure includes the following examples of applications. [Application Example 1] A method for etching a feature into a carbon-containing layer beneath a mask, comprising the simultaneous steps of etching and passivation, The aforementioned simultaneous step is, The process involves flowing a boron-containing passive gas and an etching gas containing an oxygen-containing gas, The process involves generating a plasma from the etching gas, wherein the plasma etches features into the carbon-containing layer. Methods that include... [Application Example 2] The method described in Application Example 1, The boron-containing passive gas is BCl 3 (BF 3 ), BBr 3 , where x and y are positive integers, B x H y , as well as BD where D is a halogen and x and y are positive integers. x H y A method which is at least one of the following. [Application Example 3] The method described in Application Example 1, The aforementioned feature is a method in which the CD is less than 80 nm and the aspect ratio is greater than 50. [Application Example 4] The method described in Application Example 1, A method further comprising etching the stack beneath the carbon-containing layer, wherein the carbon-containing layer functions as a mask. [Application Example 5] The method described in Application Example 4, The method wherein the aforementioned stack is a 3D NAND stack, or a DRAM stack, or another logic stack, or a memory stack. [Application Example 6] The method described in Application Example 1, Further includes etching without the use of passivation gas, The etching described above is The etching gas is flowed through which an oxygen-containing gas is not present, and the etching without passivation is performed without boron. Generating plasma from the etching gas that does not contain passivation gas and Methods that include... [Application Example 7] The method described in Application Example 6, A method comprising flowing the etching gas, which does not contain a passivation gas, together with a sulfur-containing component. [Application Example 8] The method described in Application Example 1, The etching gas is sulfur-free. [Application Example 9] The method described in Application Example 1, The etching gas is halogen-free. [Application Example 10] The method described in Application Example 1, The carbon-containing layer comprises amorphous carbon, in a method. [Application Example 11] The method described in Application Example 10, The method for the mask comprising OCN. [Application Example 12] The method described in Application Example 1, The feature is a method for forming a slit having a width CD in the range of 150 nm to 200 nm. [Application Example 13] The method described in Application Example 1, A method wherein the boron-containing passive gas and the oxygen-containing gas are mixed before being introduced into the processing chamber. [Application Example 14] The method described in Application Example 1, A method wherein the boron-containing passive gas and the oxygen-containing gas are mixed in a processing chamber before the plasma is generated from the etching gas. [Application Example 15] The method described in Application Example 1, The aforementioned feature has a CD in the range of 150 nm to 200 nm. [Application Example 16] An apparatus for processing wafers having a carbon-containing layer, Processing chamber and A substrate support that supports the substrate inside the processing chamber, A coil that supplies RF power inside the processing chamber, A gas system that simultaneously supplies boron-containing passive fumes and oxygen into the processing chamber, Boron-containing passive source, Oxygen source and gas systems including A device equipped with the following features. [Application Example 17] The apparatus described in Application Example 16, The apparatus further comprises a plenum connected to the boron-containing passivebant source and the oxygen source, wherein the boron-containing passivebant and the oxygen are mixed in the plenum before being introduced into the processing chamber. [Application Example 18] The apparatus described in Application Example 16, The gas system further comprises a controller controllably connected to the boron-containing passive source and the oxygen source, the controller including computer-readable code for simultaneously flowing the boron-containing passive source and the oxygen into the processing chamber. [Application Example 19] The apparatus described in Application Example 16, The apparatus further comprises a heater positioned to heat the boron-containing passive tandem from the boron-containing passive tandem source. [Application Example 20] The apparatus described in Application Example 16, The apparatus comprises a processing chamber equipped with a protective coating containing at least one of rare earth oxides, rare earth fluorides, or rare earth acid fluorides.

Claims

1. A method for etching features into a carbon-containing layer beneath a mask, The process includes simultaneous etching and passivation steps, The aforementioned simultaneous step is, The process involves flowing a boron-containing passive gas and an etching gas containing an oxygen-containing gas, The process involves generating a plasma from the etching gas, wherein the plasma etches features into the carbon-containing layer. Methods that include...

2. The method according to claim 1, The boron-containing passive gas is BCl 3 BF3, BBr 3 , where x and y are positive integers, B x H y , and BD where D is a halogen and x and y are positive integers. x H y A method which is at least one of the following.

3. The method according to claim 1, The aforementioned feature is a method having an aperture width of less than 80 nm and an aspect ratio greater than 50.

4. The method according to claim 1, A method further comprising etching the stack beneath the carbon-containing layer, wherein the carbon-containing layer functions as a mask.

5. The method according to claim 4, The method wherein the aforementioned stack is a 3D NAND stack, or a DRAM stack, or another logic stack, or a memory stack.

6. The method according to claim 1, Further includes etching without the use of passivation gas, The etching described above is The etching gas is flowed through which an oxygen-containing gas is not present, and the etching without passivation is performed without boron. Generating plasma from the etching gas that does not contain passivation gas and Methods that include...

7. The method according to claim 6, A method comprising flowing the etching gas, which does not contain a passivation gas, together with a sulfur-containing component.

8. The method according to claim 1, The etching gas is sulfur-free.

9. The method according to claim 1, The etching gas is halogen-free.

10. The method according to claim 1, The carbon-containing layer comprises amorphous carbon, in a method.

11. The method according to claim 10, The aforementioned mask includes a method comprising SiON.

12. The method according to claim 1, The feature is a method for forming a slit having a width in the range of 150 nm to 200 nm.

13. The method according to claim 1, A method wherein the boron-containing passive gas and the oxygen-containing gas are mixed before being introduced into the processing chamber.

14. The method according to claim 1, A method wherein the boron-containing passive gas and the oxygen-containing gas are mixed in a processing chamber before the plasma is generated from the etching gas.

15. The method according to claim 1, The method wherein the feature is a contact feature having a width in the range of 150 nm to 200 nm.

16. An apparatus for processing wafers having a carbon-containing layer, Processing chamber and A substrate support that supports the substrate inside the processing chamber, A coil that supplies RF power inside the processing chamber, A gas system that simultaneously supplies boron-containing passive fumes and oxygen into the processing chamber, Boron-containing passive source, Oxygen source and gas systems including Equipped with, The gas system is configured to supply the etching gas containing the boron-containing passive bant and the oxygen into the processing chamber. The coil is configured to generate plasma from the etching gas, The plasma simultaneously etches and passivates the features in the carbon-containing layer. Device.

17. The apparatus according to claim 16, The apparatus further comprises a plenum connected to the boron-containing passivebant source and the oxygen source, wherein the boron-containing passivebant and the oxygen are mixed in the plenum before being introduced into the processing chamber.

18. The apparatus according to claim 16, The gas system further comprises a controller controllably connected to the boron-containing passive source and the oxygen source, the controller including computer-readable code for simultaneously flowing the boron-containing passive source and the oxygen into the processing chamber.

19. The apparatus according to claim 16, The apparatus further comprises a heater positioned to heat the boron-containing passive tandem from the boron-containing passive tandem source.

20. The apparatus according to claim 16, The apparatus comprises a processing chamber equipped with a protective coating containing at least one of rare earth oxides, rare earth fluorides, or rare earth acid fluorides.

Citation Information

Patent Citations

  • Formation of fine pattern

    JP1994214402A

  • Manufacturing apparatus of semiconductor device

    JP1997232295A

  • Module block for integrated type gas supply unit

    JP2001280595A

  • Method for manufacturing semiconductor integrated circuit

    JP2003297745A

  • Method of etching carbon-containing film and method of fabricating semiconductor device using same

    JP2007110112A